An AlCr coating for emergency rescue equipment and its preparation method

By preparing an AlCr coating on the steel surface of well control and rescue equipment, the oxidation resistance of Al and Cr oxide films is improved, which solves the problem of insufficient oxidation resistance of well control and rescue equipment at high temperatures and enables stable use at high temperatures.

CN123108484APending Publication Date: 2026-11-17CHINA NAT PETROLEUM CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510619153.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing steel used for well control and emergency rescue has low oxidation resistance at high temperatures, making it unsuitable for long-term use. This results in thinner walls, lower yield strength, and an inability to bear loads.

Method used

An AlCr coating was prepared on a steel surface by magnetron sputtering. By controlling the current gradient deposition of Cr and Al, a dense Al2O3 and Cr2O3 oxide film was formed, which improved the antioxidant performance.

Benefits of technology

It forms a dense Al and Cr oxide film at high temperatures, which prevents the substrate material from oxidizing, enhances the coating adhesion, prevents peeling, and has good resistance to thermal cycling oxidation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108484A_ABST
    Figure CN123108484A_ABST
Patent Text Reader

Abstract

This invention relates to an AlCr coating for steel used in emergency rescue equipment and its preparation method, belonging to the field of oil and gas well control emergency rescue equipment manufacturing technology. The method includes the following steps: controlling the Cr target current to increase from 0A to 3A, depositing for 10-15 seconds; controlling the Cr target current to decrease from 3A-4A to 0.5A, depositing for 15-20 minutes; controlling the Cr target current to decrease from 0.5A to 0A, depositing for 10 seconds; controlling the aluminum target current to increase from 0A to 0.5A, depositing for 10 seconds; controlling the aluminum target current to increase from 0.5A to 3A-4A, depositing for 15-20 minutes; controlling the aluminum target current to decrease from 3A-4A to 0A, depositing for 10 seconds. In this invention, the Al and Cr alloy compositions in the AlCr coating form a gradient, ensuring coating adhesion and preventing peeling during the use of well control emergency rescue equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of oil and gas well control emergency rescue equipment manufacturing technology, specifically to an AlCr coating on steel for emergency rescue equipment and its preparation method. Background Technology

[0002] As exploration and development ventures into new areas, ultra-deep formations, and unconventional methods, well control risks in drilling are becoming increasingly intertwined and overlapping. High-temperature, high-volume, and high-pressure wells, horizontal wells, factory-type wells, and shallow gas wells present significant risks, posing new challenges to well control safety. Well control emergency rescue equipment mainly includes wellhead removal and reconstruction equipment. This equipment requires close proximity to the wellhead, facing high temperatures and flame environments, and involves long operation times. Currently, a "one-wrap, two-pack, three-spray" method is used to protect the equipment from fire and heat. During operation, the equipment endures a cyclic oxidation process of flame exposure, cold water spray, and then flame exposure again. Previously used carbon structural steel and new refractory steels in well control rescue equipment have insufficient resistance to cyclic oxidation. As temperatures rise, severe oxidation occurs, thinning the wall thickness and rapidly decreasing the yield strength, rendering it unable to bear loads at high temperatures. Therefore, this invention provides an AlCr coating for steel used in emergency rescue equipment and its preparation method. Summary of the Invention

[0003] The technical problem to be solved by this invention is to provide an AlCr coating for steel used in emergency rescue equipment and its preparation method. The aim is to address the issues of low oxidation resistance and inability to withstand prolonged use at high temperatures in existing well control and rescue steels.

[0004] The technical solution of the present invention to solve the above-mentioned technical problems is as follows:

[0005] In a first aspect, a method for preparing an AlCr coating on steel for emergency rescue equipment includes the following steps: preparing an AlCr coating on a workpiece to be processed using magnetron sputtering; the magnetron sputtering method is as follows:

[0006] The Cr target current was increased from 0A to 3A, with a deposition time of 10s to 15s; the Cr target current was decreased from 3A to 4A to 0.5A, with a deposition time of 15 to 20 minutes; the Cr target current was decreased from 0.5A to 0A, with a deposition time of 10s.

[0007] The aluminum target current was increased from 0A to 0.5A with a deposition time of 10s; the aluminum target current was increased from 0.5A to 3A-4A with a deposition time of 15-20 minutes; and the aluminum target current was decreased from 3A-4A to 0A with a deposition time of 10s to obtain an AlCr coating on steel for emergency rescue equipment.

[0008] For existing low-alloy structural steel workpieces, without coatings, a mixed oxide of multiple elements only forms at 600℃~700℃ to protect the substrate. However, these oxides undergo severe oxidation failure at low temperatures, thus failing to meet the requirements for high-temperature oxidation resistance. In the AlCr coating of this invention, the main elements playing a role in resisting high-temperature oxidation are Al and Cr. Al can form a dense Al2O3 film on the coating surface, thereby preventing O elements from the environment from further diffusing into the coating and oxidizing the inner coating. Cr elements can promote the formation of Al2O3 film, reducing the critical Al content required for Al2O3 formation, and can also react with O elements to form a Cr2O3 film, mainly playing a role in resisting hot corrosion. However, higher Al and Cr content in the coating is not always better: when the Al content is high, the coating exhibits extreme brittleness and a lower melting point; when the Cr content is high, it will damage the adhesion between the oxide film and the coating. Therefore, this invention strictly controls the content and distribution of Al and Cr in the coating, resulting in a higher Al content on the surface and a higher Cr content inside the coating. This avoids contact between the substrate material and oxygen, while ensuring the coating's adhesion, making it less prone to peeling off during the use of well control emergency rescue equipment.

[0009] The beneficial effects of this invention are:

[0010] (1) The present invention provides a high-temperature cyclic oxidation resistant AlCr coating for steel used in emergency rescue equipment. In terms of composition design, Al and Cr alloy composite is adopted, which can form a dense Al and Cr oxide film at high temperature, avoiding contact between the base material and oxygen.

[0011] (2) In the AlCr coating of the steel used in emergency rescue equipment of the present invention, the Al and Cr alloy components form a gradient to ensure the coating adhesion and it is not easy to peel off during the use of well control emergency rescue equipment.

[0012] Based on the above technical solution, the present invention can be further improved as follows.

[0013] Furthermore, the specific steps include the following:

[0014] (1) Place the workpiece to be processed into the cavity of the magnetron sputtering equipment, and install Cr target and Al target in the magnetron sputtering equipment respectively;

[0015] (2) Evacuate the inside of the magnetron sputtering equipment and then fill it with argon gas;

[0016] (3) Control the Cr target current to increase from 0A to 3A, and the deposition time is 10s to 15s; control the Cr target current to decrease from 3A to 4A to 0.5A, and the deposition time is 15 to 20 minutes; control the Cr target current to decrease from 0.5A to 0A, and the deposition time is 10s.

[0017] The aluminum target current was increased from 0A to 0.5A with a deposition time of 10s; the aluminum target current was increased from 0.5A to 3A-4A with a deposition time of 15-20 minutes; and the aluminum target current was decreased from 3A-4A to 0A with a deposition time of 10s to obtain an AlCr coating on steel for emergency rescue equipment.

[0018] The rise can be a uniform rise.

[0019] Furthermore, the workpiece to be processed in step (1) includes at least one of low alloy structural steel Q235 and fire-resistant steel FQ460.

[0020] Furthermore, in step (1), before the workpiece to be processed is placed into the cavity of the magnetron sputtering equipment, the surface of the workpiece to be processed is first subjected to wet sandblasting, and then cleaned and dried in sequence. Among them, the wet sandblasting medium is white corundum abrasive particles with a mesh size of 120-220, and the sandblasting pressure is controlled at 0.2-0.4MPa.

[0021] The beneficial effects of adopting the above-mentioned further solutions are: the workpiece surface is cleaned and decontaminated, while a rough surface structure is formed, providing more physical anchor points for coating and increasing the adhesion between the film and the substrate.

[0022] Furthermore, the installation of Cr and Al targets in step (1) includes the following specific steps: at least two Cr targets and at least two Al targets are installed in the magnetron sputtering equipment respectively; the purity of the Cr target is greater than 99.99%, and the purity of the Al target is greater than 99.99%.

[0023] The beneficial effect of adopting the above-mentioned further solution is to ensure the uniformity of the coating composition in each direction during the workpiece rotation process.

[0024] Furthermore, step (2) includes the following specific steps: evacuating the interior of the magnetron sputtering equipment to a vacuum pressure of 1–2 × 10⁻⁶. -5 Then fill the vacuum with argon gas, and the vacuum pressure after filling with argon gas is 3 to 5 × 10⁻⁶. -5 The preferred design, after being filled with argon gas, has a vacuum pressure of 4 × 10⁻⁶. -5 toor.

[0025] Furthermore, step (3) includes the following specific steps: controlling the Cr target current to increase linearly from 0A to 3A, with a deposition time of 10s to 15s; controlling the Cr target current to decrease linearly from 3A to 4A to 0.5A, with a deposition time of 15 to 20 minutes; controlling the Cr target current to decrease linearly from 0.5A to 0A, with a deposition time of 10s;

[0026] The aluminum target current was linearly increased from 0A to 0.5A with a deposition time of 10s; the aluminum target current was linearly increased from 0.5A to 3A-4A with a deposition time of 15-20 minutes; and the aluminum target current was linearly decreased from 3A-4A to 0A with a deposition time of 10s to obtain an AlCr coating on steel for emergency rescue equipment.

[0027] The beneficial effects of adopting the above-mentioned further scheme are as follows: In the initial stage of coating, the gradient increase of current can reduce the stress at the junction of the film layer and the substrate, and the Cr layer has a stronger bonding force with the steel substrate. Both steps can increase the bonding force between the film layer and the substrate. At the same time, the gradient increase of Cr target current and the gradient decrease of Al target current can maintain the comprehensive AlCr content in the film layer and maintain the corrosion resistance of the film layer.

[0028] Secondly, an AlCr coating on steel for emergency rescue equipment, wherein the AlCr coating on the steel for emergency rescue equipment is prepared by the aforementioned preparation method.

[0029] Furthermore, the AlCr coating of the steel used in the emergency rescue equipment has a thickness of 7μm to 15μm; between the workpiece to be processed and the AlCr coating interface, there is an intermediate oxide layer ((Al,Cr)2O3), the thickness of which is 80nm to 150nm.

[0030] The beneficial effects of adopting the above-mentioned further scheme are as follows: the intermediate oxide layer α-(Al,Cr)2O3 has certain covalent properties and a band gap of 5eV to 8eV; firstly, this intermediate oxide layer can act as a diffusion barrier between the coating and the substrate, maintaining the chemical stability of the coating-substrate interface; secondly, this intermediate oxide layer is a compound generated by the selective oxidation of residual oxygen and Al and Cr elements under low vacuum conditions in the early stage of coating deposition, which effectively improves the coating adhesion and gives the coating excellent thermal shock resistance; finally, due to the template effect, the AlCr coating is a nanocrystalline coating in the range of about 100nm to 200nm close to the α-(Al,Cr)2O3 layer, which further improves the toughness of the coating.

[0031] Furthermore, the AlCr coating of the steel used in the emergency rescue equipment has an Al content of 37%–48% and a Cr content of 52%–63% by mass; the intermediate oxide layer has an Al content of 35%–48% and a Cr content of 15%–25% by mass, with the remainder being O. Attached Figure Description

[0032] Figure 1 This is a scanning electron microscope image of Embodiment 1 of the present invention;

[0033] Figure 2 This is a scanning electron microscope image of Embodiment 2 of the present invention. Detailed Implementation

[0034] The principles and features of this invention are described below. The examples given are for illustrative purposes only and are not intended to limit the scope of the invention. Where specific techniques or conditions are not specified in the embodiments, they should be performed according to the techniques or conditions described in the literature in this field, or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased through legitimate channels.

[0035] Description of the source of materials and reagents:

[0036] Low-alloy structural steel Q235 is a common steel plate used for components of well control and rescue equipment procured through unified procurement; fire-resistant steel FQ460 is a fire-resistant steel plate for well control and rescue equipment developed by CNPC.

[0037] Before placing the low-alloy structural steel Q235 or refractory steel FQ460 into the cavity of the magnetron sputtering equipment, the surface of the workpiece to be processed is first subjected to wet sandblasting, followed by cleaning and drying to obtain the workpiece to be processed. The wet sandblasting medium is white corundum abrasive particles with a mesh size of 120-220, and the sandblasting pressure is controlled at 0.2-0.4 MPa.

[0038] Example 1:

[0039] This embodiment relates to a method for preparing a high-temperature cyclic oxidation resistant AlCr coating deposited on a low-alloy structural steel Q235 substrate, including the following steps:

[0040] Step 1: Place the workpiece to be processed into the UDP450 closed-field unbalanced magnetron sputtering chamber, and install two Cr targets and two Al targets facing each other in the UDP450 closed-field unbalanced magnetron sputtering equipment; the purity of the target materials is greater than 99.99%;

[0041] Step 2: The inside of the magnetron sputtering reactor is evacuated to a low vacuum, and then filled with argon gas; the vacuum pressure after filling with argon gas is 4×10⁻⁶. -5 toor.

[0042] Step 3: Control the Cr target current to increase linearly from 0A to 3A, with a deposition time of 10s; control the Cr target current to decrease from 3A to 0.5A, with a deposition time of 15 minutes; then control the Cr target current to decrease from 0.5A to 0A, with a deposition time of 10s.

[0043] The aluminum target current was linearly increased from 0 A to 0.5 A over a deposition time of 10 s, and then linearly increased from 0.5 A to 3 A over a deposition time of 15 minutes. The AlCr coating consisted of the following components by mass percentage: Al content 40 wt.%, Cr content 60 wt.%. Figure 1 ).

[0044] The AlCr coating on steel used in emergency rescue equipment, resistant to high-temperature cyclic oxidation, was subjected to 20 cycles of high-temperature cyclic oxidation, including holding at 700℃ for 40 minutes and cooling to room temperature for 20 minutes. After this process, the weight gain was 5 × 10⁻⁶ kg / m³. -6 g / mm 2 The test results demonstrate that the coating enables well control and rescue equipment to possess excellent resistance to thermal cycling oxidation under ventilated conditions. The AlCr coating for high-temperature cyclic oxidation resistance of this emergency rescue equipment steel was subjected to 10 cycles of thermal shock testing at 700℃ for 40 minutes followed by water quenching, resulting in a weight gain of 4 × 10⁻⁶. -6 g / mm 2 The test results show that the coating enables well control and rescue equipment to have excellent resistance to oxidation under water spray conditions.

[0045] Example 2:

[0046] This embodiment relates to a method for preparing a high-temperature cyclic oxidation resistant AlCr coating deposited on a refractory steel FQ460 substrate, including the following steps:

[0047] Step 1: Place the workpiece to be processed into the magnetron sputtering cavity, and install two Cr targets and two Al targets facing each other in the magnetron sputtering equipment; the purity of the target materials is greater than 99.99%;

[0048] Step 2: The inside of the magnetron sputtering reactor is evacuated to a low vacuum, and then filled with argon gas; the vacuum pressure after filling with argon gas is 4×10⁻⁶. -5 toor.

[0049] Step 3: Control the Cr target current to increase linearly from 0A to 3A, with a deposition time of 10s; control the Cr target current to decrease from 3A to 0.5A, with a deposition time of 20 minutes, and then control the Cr target current to decrease from 0.5A to 0A, with a deposition time of 10s.

[0050] The aluminum target current was linearly increased from 0 A to 0.5 A over a deposition time of 10 s, and then linearly increased from 0.5 A to 3 A over a deposition time of 20 minutes. The AlCr coating consisted of the following components by mass percentage: Al content 40 wt.%, Cr content 60 wt.%. Figure 2 ).

[0051] The AlCr coating on steel used in emergency rescue equipment, resistant to high-temperature cyclic oxidation, was subjected to 20 cycles of high-temperature cyclic oxidation, including holding at 700℃ for 40 minutes and cooling to room temperature for 20 minutes. After this process, the weight gain was 5 × 10⁻⁶ kg / m³. -6 g / mm 2 The test results show that the coating enables well control and rescue equipment to have excellent resistance to oxidation under cold and hot cycles when operating with ventilation.

[0052] The steel with a high-temperature cyclic oxidation-resistant AlCr coating for emergency rescue equipment was subjected to a thermal shock test of 10 cycles at 700℃ for 40 minutes followed by water quenching. The weight gain was 3 × 10⁻⁶. -6 g / mm 2 The test results show that the coating enables well control and rescue equipment to have excellent resistance to oxidation under water spray conditions.

[0053] Comparative Example 1:

[0054] Using uncoated low-alloy structural steel Q235 substrate, after holding at 700℃ for 40 minutes and cooling to room temperature, and undergoing 20 high-temperature oxidation cycles, the weight gain is 5×10. -5 g / mm 2 The uncoated low-alloy structural steel Q235 substrate was directly subjected to a 700℃ heat treatment for 40 minutes followed by water quenching. After 10 cycles of thermal shock testing, the weight gain was 3 × 10⁻⁶. -5 g / mm 2 The test results show that the coating enables well control and rescue equipment to have excellent resistance to oxidation under water spray conditions.

[0055] Comparative Example 2:

[0056] Using an uncoated fire-resistant steel FQ460 substrate, after holding at 700℃ for 40 minutes and cooling to room temperature, and undergoing 20 high-temperature oxidation cycles, the weight gain was 6×10⁻⁶. -5 g / mm 2 Using an uncoated fire-resistant steel FQ460 substrate, after holding at 700℃ for 40 minutes and water quenching, and undergoing 10 cycles of thermal shock testing, the weight gain was 2.5 × 10⁻⁶. -5 g / mm 2 The test results show that the coating enables well control and rescue equipment to have excellent resistance to oxidation under water spray conditions.

[0057] Comparative Example 3

[0058] This embodiment relates to a method for preparing a high-temperature cyclic oxidation resistant AlCr coating deposited on a low-alloy structural steel Q235 substrate, including the following steps:

[0059] Step 1: Place the workpiece to be processed into the magnetron sputtering cavity, and install two Cr targets and two Al targets facing each other in a UDP450 closed-field unbalanced magnetron sputtering device; the purity of the target materials is greater than 99.99%;

[0060] Step 2: The inside of the magnetron sputtering reactor is evacuated to a low vacuum, and then filled with argon gas; the vacuum pressure after filling with argon gas is 4×10⁻⁶. -5 toor.

[0061] Step 3: Control the Cr target current and aluminum target current to 2A, and the deposition time to 15 minutes.

[0062] The AlCr coating on steel used in emergency rescue equipment, resistant to high-temperature cyclic oxidation, was subjected to 20 cycles of high-temperature cyclic oxidation, including holding at 700℃ for 40 minutes and cooling to room temperature. The weight loss was 2 × 10⁻⁶. -6 g / mm 2 The test results indicate that the coating has poor adhesion and peels off after repeated oxidation.

[0063] Comparative Example 4

[0064] This embodiment relates to a method for preparing a high-temperature cyclic oxidation resistant AlCr coating deposited on a refractory steel FQ460 substrate, including the following steps:

[0065] Step 1: Place the workpiece to be processed into the magnetron sputtering cavity, and install two Cr targets and two Al targets facing each other in the magnetron sputtering equipment; the purity of the target materials is greater than 99.99%;

[0066] Step 2: The inside of the magnetron sputtering reactor is evacuated to a low vacuum, and then filled with argon gas; the vacuum pressure after filling with argon gas is 4×10⁻⁶. -5 toor.

[0067] Step 3: Control the current of Cr target and Al target to 2A and the deposition time to 15 minutes.

[0068] This type of steel with an AlCr coating resistant to high-temperature cyclic oxidation, used in emergency rescue equipment, exhibits a weight loss of 0.5 × 10⁻⁶ after 20 cycles of high-temperature cyclic oxidation, including holding at 700℃ for 40 minutes and cooling to room temperature. -6 g / mm 2 The test results indicate that the coating has poor adhesion and peels off after repeated oxidation.

[0069] In summary, the high-temperature cyclic oxidation resistant AlCr coating for emergency rescue equipment provided by this invention employs an Al and Cr alloy composite composition, which can form a dense Al and Cr oxide film at high temperatures, preventing the substrate material from contacting oxygen. Furthermore, the Al and Cr alloy components in the high-temperature cyclic oxidation resistant AlCr coating of this invention form a gradient, ensuring coating adhesion and preventing peeling during the use of well control emergency rescue equipment.

[0070] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.

Claims

1. A method for preparing an AlCr coating on steel for emergency rescue equipment, characterized in that, The process includes the following steps: preparing an AlCr coating on the workpiece to be processed using magnetron sputtering; the magnetron sputtering method is as follows: The Cr target current was increased from 0A to 3A, with a deposition time of 10s to 15s; the Cr target current was decreased from 3A to 4A to 0.5A, with a deposition time of 15 to 20 minutes; the Cr target current was decreased from 0.5A to 0A, with a deposition time of 10s. The aluminum target current was increased from 0A to 0.5A with a deposition time of 10s; the aluminum target current was increased from 0.5A to 3A-4A with a deposition time of 15-20 minutes; and the aluminum target current was decreased from 3A-4A to 0A with a deposition time of 10s to obtain an AlCr coating on steel for emergency rescue equipment.

2. The method for preparing an AlCr coating on steel for emergency rescue equipment according to claim 1, characterized in that, The specific steps include the following: (1) Place the workpiece to be processed into the cavity of the magnetron sputtering equipment, and install Cr target and Al target in the magnetron sputtering equipment respectively; (2) Evacuate the inside of the magnetron sputtering equipment and then fill it with argon gas; (3) Control the Cr target current to increase from 0A to 3A, and the deposition time is 10s to 15s; control the Cr target current to decrease from 3A to 4A to 0.5A, and the deposition time is 15 to 20 minutes; control the Cr target current to decrease from 0.5A to 0A, and the deposition time is 10s. The aluminum target current was increased from 0A to 0.5A with a deposition time of 10s; the aluminum target current was increased from 0.5A to 3A-4A with a deposition time of 15-20 minutes; and the aluminum target current was decreased from 3A-4A to 0A with a deposition time of 10s to obtain an AlCr coating on steel for emergency rescue equipment.

3. The method for preparing an AlCr coating on steel for emergency rescue equipment according to claim 2, characterized in that, The workpiece to be processed in step (1) includes at least one of low alloy structural steel Q235 and fire-resistant steel FQ460.

4. The method for preparing an AlCr coating on steel for emergency rescue equipment according to claim 2, characterized in that, In step (1), before the workpiece to be processed is placed into the cavity of the magnetron sputtering equipment, the surface of the workpiece to be processed is first wet sandblasted, and then cleaned and dried in sequence.

5. The method for preparing an AlCr coating on steel for emergency rescue equipment according to claim 2, characterized in that, The installation of Cr and Al targets in step (1) includes the following specific steps: at least two Cr targets and at least two Al targets are installed in the magnetron sputtering equipment respectively; the purity of the Cr target is greater than 99.99%, and the purity of the Al target is greater than 99.99%.

6. The method for preparing an AlCr coating on steel for emergency rescue equipment according to claim 2, characterized in that, Step (2) includes the following specific steps: evacuating the interior of the magnetron sputtering equipment to a vacuum pressure of 1–2 × 10⁻⁶. -5 Then fill the vacuum with argon gas, and the vacuum pressure after filling with argon gas is 3 to 5 × 10⁻⁶. -5 toor.

7. The method for preparing an AlCr coating on steel for emergency rescue equipment according to claim 2, characterized in that, Step (3) includes the following specific steps: controlling the Cr target current to increase linearly from 0A to 3A, with a deposition time of 10s to 15s; controlling the Cr target current to decrease linearly from 3A to 4A to 0.5A, with a deposition time of 15 to 20 minutes; controlling the Cr target current to decrease linearly from 0.5A to 0A, with a deposition time of 10s; The aluminum target current was linearly increased from 0A to 0.5A with a deposition time of 10s; the aluminum target current was linearly increased from 0.5A to 3A-4A with a deposition time of 15-20 minutes; and the aluminum target current was linearly decreased from 3A-4A to 0A with a deposition time of 10s to obtain an AlCr coating on steel for emergency rescue equipment.

8. An AlCr coating on steel for emergency rescue equipment, characterized in that, The AlCr coating on the steel used in the emergency rescue equipment is prepared by the preparation method described in any one of claims 1 to 7.

9. The AlCr coating on steel for emergency rescue equipment according to claim 8, characterized in that, The AlCr coating on the steel used in the emergency rescue equipment has a thickness of 7μm to 15μm; there is an intermediate oxide layer between the workpiece to be processed and the AlCr coating interface, and the thickness of the intermediate oxide layer is 80nm to 150nm.

10. The AlCr coating on steel for emergency rescue equipment according to claim 8, characterized in that, The AlCr coating of the steel used in the emergency rescue equipment has an Al content of 37%–48% and a Cr content of 52%–63% by mass; the intermediate oxide layer has an Al content of 35%–48% and a Cr content of 15%–25% by mass, with the remainder being O.