A production process for low-quality corrugated cardboard

By sequentially strengthening the fiber through fiber grading, xylanase treatment, cationic starch and amphoteric polyacrylamide, and directional application of microfibrillated cellulose, the problems of fiber shortening and low interlayer bonding strength in low-quality waste paperboard were solved, achieving efficient production and performance improvement of the paperboard.

CN123108981APending Publication Date: 2026-11-17SHANYING INT HLDG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611324439.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing low-quality waste paperboard production processes suffer from problems such as short fibers, insufficient surface activity, loose paper structure, low interlayer bonding strength, and low utilization rate of reinforcing agents. These issues fail to effectively address the spatial distribution of fibers in multilayer linerboard and the uniformity of reinforcing agent application.

Method used

By sequentially reinforcing fiber grade, xylanase treatment, cationic starch and amphoteric polyacrylamide, and directional application of microfibrillated cellulose, an interdependent process relationship is formed. This controls the storage of enzymes and the stability of the dispersion, ensuring effective adsorption of reinforcing agents on the fiber surface and uniform application between layers.

Benefits of technology

Without significantly increasing the paper basis weight, it improves the overall strength and interlayer bonding performance of linerboard, enhances the compressive strength and transportation safety of paperboard, and reduces the consumption of reinforcing agents and performance fluctuations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108981A_ABST
    Figure CN123108981A_ABST
Patent Text Reader

Abstract

This invention discloses a production process for low-quality corrugated paperboard, relating to the fields of papermaking and waste paper resource utilization. S1: Low-quality waste paper raw materials are crushed, deslag-removed, and coarsely screened to obtain recycled fiber pulp with a mass concentration of 2.0–4.5%. S2: The recycled fiber pulp is graded using a pressure screen with a sieve opening of 0.15–0.30 mm to obtain a skeleton fiber pulp and a short fiber fine fraction pulp, with an oven-dry mass ratio of 35:65–60:40. S3: The skeleton fiber pulp is refined to a freeness of 28–38°SR. Through fiber grading, long fibers are concentrated for the surface and bottom layers, improving the continuity and load-bearing capacity of the outer skeleton of the paperboard and reducing the ineffective dispersion of high-quality long fibers in the core layer. Controlled activation of the short fiber component using xylanase improves fiber fibrillation rate, water retention value, and surface hydroxyl accessibility while maintaining fiber length, thus improving the binding performance of short fibers from recycled waste paper.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of papermaking and waste paper resource utilization technology, specifically to a production process for low-quality corrugated paperboard. Background Technology

[0002] Corrugated cardboard is an important component of corrugated boxes. Its ring crush strength, short-distance compression strength, bursting strength, tensile strength, and interlayer bond strength directly affect the compressive load-bearing capacity, stacking stability, and transportation safety of corrugated boxes.

[0003] As the number of times waste paper is recycled increases, the fibers in the waste paper pulp continuously undergo keratinization, shortening, and fine fibrosis, resulting in a decrease in average fiber length, reduced accessibility of hydroxyl groups on the fiber surface, and weakened fiber water absorption and swelling capacity as well as interfiber bonding ability. Simultaneously, low-quality mixed waste paper pulp typically contains a high proportion of ash, adhesives, ink particles, and inorganic fillers, which can easily lead to loose paper sheet structure, insufficient interlayer bonding, and reduced utilization of wet-end additives.

[0004] Current low-quality waste paperboard production processes typically improve paperboard strength by increasing beating degree, adding cationic starch, or increasing paper basis weight. However, over-beating can easily lead to the cutting of long fibers, an increase in fine fibers, deterioration of water filtration performance, and increased drying energy consumption. Simply increasing the amount of reinforcing agents such as cationic starch is easily affected by anionic waste in the waste paper pulp, resulting in problems such as high consumption of additives, low retention rate, and unstable reinforcing effect. Simply increasing paper basis weight will increase fiber raw material consumption and cannot fundamentally improve the strength per unit mass of paperboard.

[0005] Existing technologies have also proposed methods to improve the properties of recycled pulp, such as fiber grading, cellulase treatment, polyacrylamide reinforcement, or microfibrillated cellulose reinforcement. However, most of these technologies are used as independent processing steps, failing to fully consider the spatial distribution of fibers of different lengths in multilayer linerboard, and also failing to address the problems of insufficient surface activity of short fibers, competitive adsorption of wet-end reinforcing agents, and disordered dispersion of microfibrillated cellulose in the pulp leading to deterioration of filtration.

[0006] In particular, if microfibrillated cellulose is added directly to the entire pulp, it is easily dispersed into the paper layers. Its high specific surface area significantly increases the pulp's water retention and the resistance to dewatering of wet paper sheets, while the proportion of microfibrillated cellulose actually located at the paper layer interface and capable of participating in interlayer bridging is limited. If the reinforcing agent is added in an unreasonable order, cationic starch and polyacrylamide may also prematurely form aggregates in the pulp, reducing their effective adsorption on the fiber surface.

[0007] Furthermore, xylanase is a bioactive preparation, and its enzyme activity is easily affected by storage temperature, light exposure, repeated freeze-thaw cycles, and opening time. If the storage or use conditions of the enzyme preparation are not properly controlled, the enzyme activity will decrease, causing fluctuations in the activation level of short fibers.

[0008] Microfibrillated cellulose has a high specific surface area and surface energy, and is prone to sedimentation, flocculation, and reagglomeration when left to stand for a long time in an aqueous dispersion system. If the dispersion is stored for too long or is not redispersed before use, it may lead to uneven interlayer application, discontinuity in the reinforced zone, and local fluctuations in the properties of the paperboard.

[0009] Meanwhile, the uniformity of the microfibrillated cellulose dispersion applied to the surface of the wet paper layer in both the transverse and longitudinal directions directly affects the continuity of the interlayer reinforcement zone. If the nozzle flow rate, coating gap, liquid supply pressure, or paper machine speed is unstable, it is easy to form local areas of excessive or insufficient application, which in turn affects the consistency of the interlayer bonding strength of the paperboard.

[0010] Therefore, there is a need to provide a low-quality linerboard production process with a clear process synergy, which allows recycled fibers of different lengths to be graded and utilized according to their structural functions, and controls the storage and use of xylanase, the stability of microfibrillated cellulose dispersions, and the uniformity of interlayer application. Through enzymatic activation, sequential reinforcement, and interlayer directional construction, the overall strength of low-quality linerboard can be improved without significantly increasing the basis weight of the paper. Summary of the Invention

[0011] The purpose of this invention is to solve the problems of short fibers, insufficient surface activity, loose paper structure, low interlayer bonding strength, and low utilization rate of conventional reinforcing agents in low-quality waste paper pulp, and to provide a production process for low-quality linerboard.

[0012] To achieve the above objectives, the present invention provides the following technical solution: a production process for low-quality corrugated paperboard, comprising the following steps.

[0013] S1. Add low-quality mixed waste paper raw materials into the pulping equipment, add water for pulping, control the pulp concentration to be 3.0% to 6.0%, the pulping temperature to be 40 to 60℃, and the pulping time to be 20 to 45 minutes.

[0014] The pulp after disintegration is passed through a coarse sieve, a slag remover, and a fine sieve to remove plastic flakes, sand particles, metal particles, adhesive clumps, and insufficiently disintegrated paper pieces, thus obtaining purified waste paper pulp.

[0015] The purified waste paper pulp, by oven-dry fiber weight, includes waste corrugated cardboard fiber, mixed office waste paper fiber, waste packaging paper fiber, or a combination thereof.

[0016] The low-quality waste paper pulp preferably has at least two of the following characteristics: 1. The mass percentage of fine fibers with a length of less than 0.20 mm is 25% to 55%; 2. The length-weighted average fiber length is 0.55 to 1.00 mm; 3. The ash content is 8% to 22%; 4. It has been recycled more than three times; 5. The interlayer bonding strength of the 160 g / m² linerboard obtained without treatment is not higher than 210 J / m².

[0017] The mass concentration of the purified waste paper pulp is adjusted to 1.5% to 3.5% and then fed into the fiber grading system.

[0018] S2. The purified waste paper pulp is fed into a slotted pressure screen for fiber classification.

[0019] The width of the pressure screen slit is 0.15-0.30 mm, preferably 0.18-0.25 mm; the feed pressure is 0.15-0.35 MPa; the inlet and outlet pressure difference is 20-80 kPa; and the slurry mass concentration is 1.5%-3.5%.

[0020] The pressure screen retains long fiber components on the truncated side and passes through the pressure screen on the short fiber side.

[0021] The oven-dry mass ratio of the long fiber component to the short fiber component is 35:65 to 60:40, preferably 42:58 to 55:45.

[0022] The length-weighted average fiber length of the long fiber component is preferably 1.10 to 1.60 mm, and the proportion of fibers with a length greater than 1.00 mm is preferably not less than 45%.

[0023] The length-weighted average fiber length of the short fiber component is preferably 0.30 to 0.70 mm, and the mass percentage of fine fibers with a length of less than 0.20 mm is preferably 35% to 65%.

[0024] Long fiber components are used as the main skeleton fibers in the surface layer, bottom layer, or surface layer and bottom layer of linerboard; short fiber components are used in the core layer or interlayer bonding area after subsequent enzymatic activation and sequential reinforcement treatment.

[0025] S3. The long fiber component is fed into a disc mill for light beating, with the beating concentration controlled at 3.0% to 5.0%, the beating temperature at 30 to 50°C, and the freeness after beating at 28 to 38°SR, preferably 30 to 35°SR.

[0026] Light beating is mainly used to promote the fine fibrillation of the long fibers on the outside and to avoid excessive cutting of the long fibers.

[0027] The treated long fiber components are used to formulate the top layer slurry and the bottom layer slurry.

[0028] In the top and bottom pulps, long fiber components account for 55% to 90% of the oven-dry fiber mass of each layer, with the remainder being treated short fiber components, damaged pulp, or other recycled fiber pulp.

[0029] S4. Adjust the mass concentration of the short fiber component to 2.0%–8.0%, adjust the pulp temperature to 35–60℃, and adjust the pH to 5.0–8.0.

[0030] Xylanase is added to the short fiber component. The amount of xylanase added is 20-200 U / g based on the oven-dry weight of the short fiber, preferably 60-150 U / g.

[0031] Enzymatic treatment is carried out under stirring conditions of 100–500 r / min for 20–90 min, preferably 35–70 min.

[0032] The xylanase is preferably an endo-xylanase.

[0033] Xylanase hydrolyzes some xylan and related hemicellulose on the fiber surface and in the outer layer of the cell wall in a controlled manner, exposing cellulose microfibrils and promoting microfibrillation on the fiber surface, thereby increasing the fiber's water retention value and the number of accessible hydroxyl groups.

[0034] The xylanase preparation used should be stored according to the manufacturer's storage conditions before use. In a preferred embodiment, the xylanase is packaged in a sealed container and stored at 2–8°C in a dark and dry environment, avoiding prolonged exposure to high temperatures, freezing, repeated freeze-thaw cycles, and storage with strong acids, strong alkalis, or oxidizing substances.

[0035] Unopened xylanase should preferably be used within the expiration date indicated on the product label. Under sealed and light-protected conditions at 2–8°C, its shelf life is preferably no more than 12 months. Once opened, xylanase should be resealed and stored, and preferably used within 30 days. If the expiration date specified in the xylanase product instructions is shorter than the above-mentioned period, the period specified in the product instructions shall prevail.

[0036] Before using xylanase, check the packaging integrity, product batch number, production date, and expiration date. Enzyme preparations that exhibit obvious turbidity, abnormal precipitation, abnormal color or odor, or have exceeded their expiration date should not be used directly in production.

[0037] Before use, liquid xylanase should be equilibrated at room temperature for 10–30 minutes, and then gently inverted or stirred at low speed to ensure homogeneity, avoiding vigorous shaking. The xylanase dilution should preferably be prepared and used immediately, and added to the pulp system within 4 hours of preparation; it should not be stored for extended periods.

[0038] For xylanases that have been stored for a long time, have experienced abnormal storage temperatures, or whose enzyme activity is questionable, the actual enzyme activity should be measured before use, and the amount added should be adjusted according to the actual enzyme activity value so that the effective enzyme activity added is within the specified range of 20-200 U / g.

[0039] After the enzymatic treatment is completed, the slurry can be heated to 65-80℃ and kept at that temperature for 5-15 minutes to inactivate the enzyme. Alternatively, the enzymatic reaction can be terminated by dilution, washing, or changing the pH.

[0040] The reduction in the length-weighted average fiber length of the short fiber component after enzymatic treatment relative to the untreated fiber length is preferably no more than 8%, the increase in fiber fibrillation rate is preferably no less than 15%, and the increase in water retention value is preferably no less than 8%.

[0041] S5. Adjust the mass concentration of the enzymatically activated short fiber slurry to 1.0%–4.0% and the temperature to 25–45℃.

[0042] First, cationic starch is added to the enzyme-activated short fiber slurry.

[0043] The degree of substitution of cationic starch is 0.015 to 0.060, and the amount added is 5 to 20 kg / t based on the oven-dry weight of short fibers, preferably 8 to 16 kg / t.

[0044] After adding cationic starch, mix at 300–1000 r / min for 3–15 min to allow the cationic starch to preferentially adsorb onto the negatively charged fiber surface and fine fiber surface.

[0045] Then amphoteric polyacrylamide was added.

[0046] The amount of amphoteric polyacrylamide added is 0.20-1.20 kg / t based on the oven-dry weight of short fibers, preferably 0.40-0.90 kg / t; the relative molecular mass is preferably 3 million to 15 million.

[0047] After the addition of amphoteric polyacrylamide, the mixture is stirred at 200-800 r / min for 30-180 s to form a sequentially reinforced short fiber slurry.

[0048] The oven-dry mass ratio of cationic starch to amphoteric polyacrylamide is 8:1 to 60:1, preferably 15:1 to 35:1.

[0049] By first adding cationic starch and then adding amphoteric polyacrylamide, the cationic starch forms a primary adsorption reinforcing layer on the fiber surface. Then, the amphoteric polyacrylamide is used to bridge the fiber, the starch adsorption layer, and the fine fibers, reducing the premature formation of ineffective aggregates by the two reinforcing agents in the slurry.

[0050] S6. Take microfibrillated cellulose raw material and add water to prepare a microfibrillated cellulose predispersant with a solid content of 0.3% to 2.0%.

[0051] The microfibrillated cellulose has an average diameter of 10–500 nm, a length of 1–100 μm, and a specific surface area of ​​not less than 20 m² / g.

[0052] The microfibrillated cellulose predispersant was sheared at 1000–5000 r / min for 5–30 min, followed by cyclic homogenization or ultrasonic dispersion.

[0053] The homogenization pressure during circulation was 10–80 MPa, the number of cycles was 1–5, the ultrasonic frequency was 18–30 kHz, and the ultrasonic time was 3–20 min.

[0054] In the dispersed microfibrillated cellulose dispersion, the number of aggregates with an equivalent diameter greater than 100 μm is preferably no more than 10 per mm².

[0055] The amount of microfibrillated cellulose added is 0.20% to 1.50% based on the total oven-dry fiber mass of the linerboard, preferably 0.50% to 1.20%.

[0056] Since microfibrillated cellulose dispersions may re-agglomerate during standing, this invention preferably adopts a fresh-preparation-and-use method. After preparation, the dispersion should preferably be used within 8 hours, and more preferably within 4 hours.

[0057] After the dispersion is prepared and before application, a low-speed stirring device or a circulating conveying device is installed in the storage tank. The preferred low-speed stirring speed is 50-150 r / min to maintain the suspension and uniform dispersion of microfibrillated cellulose, while avoiding the introduction of excessive air bubbles by high-speed stirring.

[0058] When the dispersion cannot be used immediately, it should be placed in a sealed container and stored for a short period at 4–10°C, preferably not exceeding 24 hours. During storage, freezing, high-temperature exposure, strong light exposure, and prolonged complete stagnation should be avoided.

[0059] Before use, microfibrillated cellulose dispersions that have been stored for a short period of time should be redispersed by high-speed shearing at 1000-3000 r / min for 3-10 min, or treated again by circulating homogenization.

[0060] After redispersion, the dispersion should be checked for obvious stratification, flocculent formation, sedimentation, or abnormal viscosity. It can continue to be used only if the following conditions are met: 1. The number of agglomerates with an equivalent diameter greater than 100 μm is no higher than 10 agglomerates / mm²; 2. The relative deviation of the solid content between the upper and lower layers of the dispersion does not exceed 5%; 3. The dispersion is free of large, visible gel particles or precipitates; 4. The dispersion can flow continuously and stably in the delivery pipeline and application device.

[0061] Dispersions that do not meet the above requirements should be subjected to high-speed shearing or homogenization again. If they still do not meet the requirements after reprocessing, they should not be used for interlayer application.

[0062] S7. The treated long fiber component and sequentially reinforced short fiber slurry are respectively formulated as surface slurry, core slurry and bottom slurry.

[0063] The oven-dry weight ratio of each layer of the linerboard is as follows: top layer: 20%–35%; core layer: 35%–60%; bottom layer: 20%–35%.

[0064] The surface and bottom layers are mainly composed of long fiber components as the backbone fibers, while the core layer is mainly composed of short fiber components that have been activated by xylanase and sequentially reinforced.

[0065] In a preferred embodiment, the oven-dry mass ratio of the top layer, core layer, and bottom layer is 25–30: 40–50: 25–30.

[0066] S8. Layered forming is performed using a multi-layer headbox, stacked mesh forming device, circular mesh forming device, or multi-layer inclined mesh forming device.

[0067] First, a first wet paper layer is formed. Then, a partial microfibrillated cellulose dispersion is applied to the surface of the first wet paper layer, and a second wet paper layer is formed on top of it.

[0068] The remaining microfibrillated cellulose dispersion is applied to the surface of the second wet paper layer to form a third wet paper layer, resulting in a multilayer wet paper web.

[0069] Microfibrillated cellulose dispersions are applied between adjacent wet paper layers by spraying, curtain coating, slot coating, or flow delivery.

[0070] When applying the spray, it is preferable to use multiple fan-shaped nozzles or atomizing nozzles arranged transversely along the paper web. The nozzle spacing is set according to the spray coverage width, the overlap rate of the spray areas of adjacent nozzles is preferably 30% to 60%, and the spray pressure is preferably 0.10 to 0.40 MPa.

[0071] A filter with a filtration accuracy of 80-200 mesh is installed before the nozzle to reduce clogging by fiber agglomerates or impurities. Each nozzle can be equipped with a flow regulating valve or use a zoned liquid supply pipeline, allowing the flow rate of each transverse zone to be adjusted independently.

[0072] When applying the coating using a curtain coating method, the curtain should be continuous, without interruption, and without significant lateral thickness differences. The liquid supply flow rate should be adjusted according to the paper machine running speed.

[0073] When applying the coating using the slotted spray method, the consistency of the slotted gap and the lateral hydraulic pressure should be controlled, and the coating head should be checked regularly for local blockage.

[0074] The preferred pipeline for transporting the microfibrillated cellulose dispersion is a circulating supply structure, with the storage tank continuously stirred at a low speed of 50–150 r / min to prevent the dispersion from settling or re-agglomerating in the storage tank and pipeline.

[0075] The dispersion supply flow rate should be linked to the paper machine speed, paper width, and target oven-dry application amount. When the paper machine speed changes, the supply flow rate should be adjusted synchronously via a metering pump or a variable frequency pump to keep the application amount per unit area stable.

[0076] The amount of microfibrillated cellulose applied at oven-dry depth between the surface layer and the core layer, and between the core layer and the bottom layer, is 0.10–1.50 g / m², respectively. The amount of microfibrillated cellulose applied at the two interfaces can be the same or different.

[0077] When microfibrillated cellulose is applied, the solid content of the first wet paper layer or the second wet paper layer is 4% to 18%, preferably 6% to 14%.

[0078] To control the uniformity of transverse application, multiple detection zones can be set along the transverse direction of the paper web, and the actual amount applied in each zone can be detected by flow meter, weighing method, fluorescence tracer method, image grayscale method or solid content determination method.

[0079] The coefficient of variation of the amount of microfibrillated cellulose applied in each transverse detection area is preferably no more than 8%, and more preferably no more than 6%; the relative deviation between the actual amount applied in any local area and the average amount applied in the transverse direction is preferably no more than ±10%.

[0080] When the coefficient of variation of the lateral application amount exceeds 8%, or the deviation of the local application amount exceeds ±10%, the nozzle blockage, liquid supply pressure, curtain continuity, slit gap, filter device and dispersion agglomeration should be checked, and the flow rate of each zone should be readjusted.

[0081] During production, it is recommended to check the operating status of the application device every 30 to 120 minutes. After shutdown, the storage tank, delivery pipeline, nozzle or coating head should be rinsed with clean water in time to avoid blockage caused by residual microfibrillated cellulose drying.

[0082] By applying microfibrillated cellulose in a directional and uniform manner before bonding adjacent wet paper layers, the microfibrillated cellulose is concentrated at the paper layer interface and forms an interlayer reinforcement zone with a thickness of 20–150 μm during wet pressing and drying.

[0083] The continuity rate of the interlayer reinforcement zone along the transverse direction of the paper web is preferably not less than 70%, and more preferably not less than 85%.

[0084] S9. Press and dewater the multi-layer wet paper web, with a press line pressure of 40-180 kN / m, and the solid content of the wet paper web after pressing is 38%-52%.

[0085] The pressed wet paper web is sent to the drying section and dried at 80-130°C to reduce the moisture content of the paperboard to 5%-10%.

[0086] Surface sizing can be applied to dried cardboard. Surface sizing agents include oxidized starch, enzyme-converted starch, polyvinyl alcohol, styrene-acrylate emulsion, or combinations thereof.

[0087] The oven-dry application rate of the surface sizing agent is 1.0–5.0 g / m².

[0088] The sizing of the cardboard is dried again, and then calendered, wound, and slit to obtain low-quality linerboard.

[0089] The basis weight of the obtained linerboard is preferably 100-250 g / m², and more preferably 130-200 g / m².

[0090] Technical Principles This invention does not simply superimpose fiber grading, xylanase, wet end reinforcing agent, and microfibrillated cellulose, but rather establishes an interdependent process relationship among the various processing steps in terms of raw material targets, location of action, and processing sequence.

[0091] Pressure screening first separates long fibers from short fibers, allowing long fibers to be concentrated in the top and bottom layers of the paperboard, forming a continuous skeleton that bears the compression load, and preventing long fibers from being over-pulped or covered by a large number of fine fibers.

[0092] Xylanase treatment targets the graded short fiber components. Due to the large specific surface area and high degree of surface keratinization of short fibers, controlled xylanase treatment can increase the accessibility of surface microfibers and hydroxyl groups, but will not cause significant strength damage to the long fibers that play a skeletal role.

[0093] By controlling the storage temperature, sealing condition, shelf life, and actual enzyme activity of xylanase, fluctuations in the activation level of short fibers caused by enzyme activity decay can be reduced, thereby improving the consistency between different production batches.

[0094] Cationic starch is first adsorbed onto the surface of short fibers after enzymatic activation, and then amphoteric polyacrylamide is added for bridging, so that the reinforcing agent mainly acts on short and fine fibers that have exposed more active sites, thereby improving the effective utilization rate of wet-end reinforcing agent.

[0095] Microfibrillated cellulose is not directly mixed into the pulp in large quantities, but is applied directionally between adjacent wet paper layers, forming a continuous network at the paper layer interface. This network can fill the interlayer pores and form hydrogen bonds and mechanical entanglements with the surface, core, and bottom fibers, improving the interlayer stress transfer capability.

[0096] By preparing and using the mixture immediately, stirring at low speed, circulating and conveying it, storing it at low temperature for a short period of time, and redispersing it before use, the re-agglomeration of microfibrillated cellulose during storage and transportation can be reduced.

[0097] By controlling the nozzle overlap rate, liquid supply pressure, transverse zone flow rate, paper machine speed linkage, and application amount variation coefficient, microfibrillated cellulose can form a uniform and continuous interlayer reinforcement area on the surface of the wet paper layer, avoiding local under-application or over-application.

[0098] Therefore, fiber grading determines the spatial distribution of different fibers, enzymatic treatment determines the reactivity of short fiber surfaces, sequential reinforcement determines the adsorption and bridging mechanisms of reinforcing agents, dispersion stability control determines the dispersion state of microfibrillated cellulose, and uniform application control determines the spatial distribution of reinforcing materials. These steps together form a multi-level reinforcement structure from the fiber scale, paper layer scale to the overall paperboard scale.

[0099] Compared with existing technologies, this invention provides a production process for low-quality corrugated paperboard, which has the following beneficial effects: By grading fibers, long fibers are concentrated for use in the surface and bottom layers, improving the continuity and load-bearing capacity of the outer skeleton of the paperboard and reducing the ineffective dispersion of high-quality long fibers in the core layer. Controlled activation of the short fiber components using xylanase improves fiber fissuring rate, water retention value, and surface hydroxyl accessibility while essentially maintaining fiber length, thus improving the binding performance of short fibers from recycled waste paper.

[0100] By specifying the low-temperature, sealed, and light-protected storage requirements for xylanase and its shelf life after opening, the impact of enzyme activity decay and batch fluctuations on the enzymatic treatment effect can be reduced. A sequential reinforcement method, adding cationic starch first and then amphoteric polyacrylamide, allows the cationic starch to first form an adsorption layer on the fiber surface, followed by bridging with amphoteric polyacrylamide, improving the retention rate of the reinforcing agent and reducing ineffective flocculation within the pulp. Orienting microfibrillated cellulose between adjacent wet paper layers to form a continuous interlayer reinforcement zone allows for a more significant interlayer reinforcement effect with a lower amount of microfibrillated cellulose compared to directly mixing it into all the pulp, while also reducing the adverse effects on pulp dewatering performance.

[0101] By adopting measures such as preparing and using immediately, low-speed stirring, short-term storage at low temperature, and redispersing before use, the sedimentation and reagglomeration of microfibrillated cellulose dispersions can be reduced, thereby improving their storage and use stability. Attached Figure Description

[0102] Figure 1 This is a SEM image of the surface of short fibers after xylanase activation in Example 2 of the present invention. Figure 2 This is a TEM image of the microfibrillated cellulose dispersion from Example 2 of the present invention. Figure 3 This is a confocal laser fluorescence micrograph of the interlayer distribution of microfibrillated cellulose in Example 2 of the present invention. Figure 4 This is a SEM image of the interface between the cardboard surface layer and the core layer in Embodiment 2 of the present invention; Figure 5 This is a SEM image of the fracture surface after the interlayer bonding strength test of the linerboard in Embodiment 2 of the present invention. Detailed Implementation

[0103] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0104] Please see Figures 1-5 This invention provides a technical solution for the production process of low-quality corrugated paperboard: Unless otherwise specified, all parts and percentages below are based on oven-dry weight, pulp concentration is mass concentration, and enzyme activity units U / g are based on oven-dry fiber weight.

[0105] Raw materials and equipment Low-quality waste paper raw materials are mixed waste paper, which, by oven-dry weight, include 55% waste corrugated cardboard boxes, 30% mixed packaging waste paper, and 15% office waste paper and other miscellaneous paper.

[0106] After pulping, coarse screening, slag removal, and fine screening, the main indicators of the purified waste paper pulp obtained from the waste paper raw materials are as follows: the length-weighted average fiber length is 0.82 mm; the mass percentage of fine fibers with a length less than 0.20 mm is 34.6%; the ash content is 14.2%; the initial freeness is 22°SR; and when the process of this invention is not used, the interlayer bonding strength of the 160 g / m² three-layer linerboard is 185 J / m².

[0107] Xylanase is an endo-xylanase, packaged in sealed containers and stored at 2–8°C in the dark. Unopened products should be used within the stated expiration date; once opened, the package should be resealed and used within 30 days.

[0108] The degree of substitution of cationic starch is 0.035.

[0109] The relative molecular mass of amphoteric polyacrylamide is approximately 8 million.

[0110] Microfibrillated cellulose has an average diameter of 50–200 nm, a length of 5–40 μm, and a specific surface area of ​​45 m² / g.

[0111] The low-quality waste paper raw material referred to in this invention refers to recycled waste paper raw material with an ash content of 8 to 18 wt% after shredding and purification, and whose short fiber and fine component content reaches the specified range.

[0112] Unless otherwise specified, the basis weight of the linerboard obtained in each embodiment and comparative example is controlled at 160±3g / m², and the oven-dry weight ratio of the surface layer, core layer and bottom layer is 28∶44∶28.

[0113] Preparation of microfibrillated cellulose dispersion Microfibrillated cellulose was added to deionized water to prepare a pre-dispersion with a solid content of 1.0%.

[0114] The cellulose was dispersed for 15 minutes at 3000 r / min using a high-speed disperser, and then homogenized twice at 40 MPa using a high-pressure homogenizer to obtain a microfibrillated cellulose dispersion.

[0115] Microscopic observation results showed that the number of microfibrillated cellulose aggregates with an equivalent diameter greater than 100 μm in the dispersion was 4 per mm².

[0116] The prepared microfibrillated cellulose dispersion was stored in a sealed storage tank equipped with a low-speed stirring device at a stirring speed of 80 r / min and was used up within 4 hours after preparation.

[0117] Example 1 A production process for low-quality corrugated board includes the following steps.

[0118] The mass concentration of the purified waste paper pulp was adjusted to 2.0%, and it was classified using a pressure screen with a sieve opening width of 0.18 mm to obtain long fiber components and short fiber components with an oven-dry mass ratio of 53:47.

[0119] The long fiber component was lightly pulped at a concentration of 4.0% to 30°SR and used to prepare the top layer slurry and the bottom layer slurry.

[0120] Adjust the concentration of the short fiber component to 4.0%, the temperature to 40℃, and the pH to 6.0. Before use, equilibrate the xylanase at room temperature for 20 min and mix gently. Add 20 U / g to the short fiber slurry and react at 250 rpm for 35 min. After the reaction, raise the temperature to 70℃ and hold for 10 min.

[0121] Adjust the concentration of the enzymatically treated short fiber slurry to 2.0%, first add 5 kg / t of cationic starch and stir for 5 min, then add 0.20 kg / t of amphoteric polyacrylamide and stir for 60 s.

[0122] A three-layer forming device is used for layer forming. The total amount of microfibrillated cellulose added is 0.20% of the oven-dry fiber mass of the linerboard, and it is applied between the surface layer and the core layer, and between the core layer and the bottom layer.

[0123] The microfibrillated cellulose dispersion was applied by a transverse multi-nozzle spray method, with an overlap rate of 40% between adjacent nozzle coverage areas, a spray pressure of 0.18 MPa, and a coefficient of variation of transverse application amount of 6.8%.

[0124] After pressing, drying and surface sizing, wet paper webs are used to obtain linerboard with a basis weight of 160 g / m².

[0125] Example 2 A production process for low-quality corrugated board includes the following steps.

[0126] The mass concentration of the purified waste paper pulp was adjusted to 2.5%, and it was classified using a pressure screen with a sieve opening width of 0.22 mm. The pulp inlet pressure was 0.25 MPa, and the inlet and outlet pressure difference was 45 kPa, resulting in long fiber components and short fiber components with an oven-dry mass ratio of 48:52.

[0127] The length-weighted average fiber length of the long fiber component is 1.36 mm, and the length-weighted average fiber length of the short fiber component is 0.50 mm.

[0128] The long fiber component is lightly pulped to 33°SR and used in both the top and bottom layer slurries.

[0129] Before using xylanase, check the packaging and expiration date, and equilibrate at room temperature for 20 minutes. Adjust the concentration of the short fiber component to 5.0%, the temperature to 50℃, and the pH to 6.5. Add 100 U / g of xylanase and react at 300 rpm for 50 minutes. After the reaction, raise the temperature to 72℃ and hold for 10 minutes.

[0130] The concentration of the enzymatically treated short fiber slurry was adjusted to 2.5%. First, 12 kg / t of cationic starch was added and mixed at 600 r / min for 8 min. Then, 0.60 kg / t of amphoteric polyacrylamide was added and mixed at 400 r / min for 90 s to obtain sequentially reinforced short fiber slurry.

[0131] In the surface and bottom layers of the slurry, the long fiber component accounts for 75% of the oven-dry fiber mass of each layer, while in the core layer, the sequentially reinforced short fiber slurry accounts for 85% of the oven-dry fiber mass of the core layer.

[0132] After the microfibrillated cellulose dispersion is prepared, it is placed in a sealed storage tank and stirred continuously at a low speed of 80 r / min, and used up within 4 hours.

[0133] The three-layer forming process is employed. The amount of microfibrillated cellulose added is 0.80% of the oven-dry fiber mass of the linerboard, with 50% applied between the surface layer and the core layer, and 50% applied between the core layer and the bottom layer.

[0134] The spray is applied using a transverse zone spraying device, with a 120-mesh filter installed before the nozzle. The spray coverage overlap between adjacent nozzles is 50%, and the spray pressure is 0.20 MPa. The liquid supply pump flow rate is linked to the paper machine running speed for control. The coefficient of variation for the transverse application amount is 5.8%, and the maximum local deviation is 8.5%.

[0135] When microfibrillated cellulose is applied, the corresponding wet paper layer solids content is 10%.

[0136] The wet paper web was pressed under a linear pressure of 110 kN / m, and the solid content after pressing was 46%; it was then dried to a moisture content of 7%.

[0137] Oxidized starch was used for surface sizing, with an oven-dry sizing amount of 3.0 g / m². After further drying, calendering, and winding, linerboard was obtained.

[0138] Example 3 Production was carried out according to Example 2, with the following differences: the width of the pressure screen slits was 0.25 mm; the amount of xylanase added was 200 U / g, the enzymatic treatment temperature was 55℃, and the time was 70 min; the amount of cationic starch added was 20 kg / t; the amount of amphoteric polyacrylamide added was 1.20 kg / t; and the amount of microfibrillated cellulose added was 1.50% of the oven-dry fiber mass of the linerboard. The remaining process conditions were the same as in Example 2.

[0139] Example 4 Production was carried out according to Example 2, with the following differences: the width of the pressure screen slits was 0.20 mm; the amount of xylanase added was 60 U / g, and the enzymatic treatment time was 40 min; the amount of cationic starch added was 8 kg / t; the amount of amphoteric polyacrylamide added was 0.40 kg / t; and the amount of microfibrillated cellulose added was 0.50% of the oven-dry fiber mass of the linerboard. The remaining process conditions were the same as in Example 2.

[0140] Example 5 Production was carried out according to Example 2, with the following differences: the width of the pressure screen slits was 0.24 mm; the amount of xylanase added was 150 U / g, and the enzymatic treatment time was 60 min; the amount of cationic starch added was 16 kg / t; the amount of amphoteric polyacrylamide added was 0.90 kg / t; and the amount of microfibrillated cellulose added was 1.20% of the oven-dry fiber mass of the linerboard. The remaining process conditions were the same as in Example 2.

[0141] Comparative Example 1 was produced according to Example 2, except that a pressure screen was not used to separate the purified waste paper pulp into long-fiber and short-fiber components; instead, all the purified waste paper pulp was mixed together. Xylanase, cationic starch, and amphoteric polyacrylamide were added to all the pulp in the amounts specified in Example 2, and the remaining process conditions were the same as in Example 2.

[0142] Comparative Example 2 was produced in accordance with Example 2, except that the width of the pressure screen slit was 0.10 mm, and the other process conditions were the same as in Example 2.

[0143] Comparative Example 3 was produced in accordance with Example 2, except that the width of the pressure screen slit was 0.35 mm, and the other process conditions were the same as in Example 2.

[0144] Comparative Example 4 was produced in accordance with Example 2, except that xylanase was not added to the short fiber component, while the other process conditions were the same as in Example 2.

[0145] Comparative Example 5 was produced in accordance with Example 2, except that the amount of xylanase added was 10 U / g, and the other process conditions were the same as in Example 2.

[0146] Comparative Example 6 was produced in accordance with Example 2, except that the amount of xylanase added was 300 U / g, and the other process conditions were the same as in Example 2.

[0147] Comparative Example 7 was produced in accordance with Example 2, except that amphoteric polyacrylamide was first added to the enzymatically treated short fiber slurry, mixed for 90 seconds, and then cationic starch was added and mixed for 8 minutes. The remaining process conditions were the same as in Example 2.

[0148] Comparative Example 8 was produced in accordance with Example 2, except that cationic starch and amphoteric polyacrylamide were premixed and then added to the short fiber slurry. The remaining process conditions were the same as in Example 2.

[0149] Comparative Example 9 was produced in accordance with Example 2, except that cationic starch was not added to the short fiber slurry, while the other process conditions were the same as in Example 2.

[0150] Comparative Example 10 was produced in accordance with Example 2, except that amphoteric polyacrylamide was not added to the short fiber slurry, while the other process conditions were the same as in Example 2.

[0151] Comparative Example 11 was produced in accordance with Example 2, except that no microfibrillated cellulose dispersion was applied between adjacent paper layers, while the other process conditions were the same as in Example 2.

[0152] Comparative Example 12 was produced in accordance with Example 2, except that all the microfibrillated cellulose dispersion was directly added to the core layer slurry, and was not applied directionally between the surface layer and the core layer or between the core layer and the bottom layer. The remaining process conditions were the same as in Example 2.

[0153] Comparative Example 13 was produced in accordance with Example 2, except that the microfibrillated cellulose was simply stirred at 500 r / min for 10 min without high-speed shearing and high-pressure homogenization, while the other process conditions were the same as in Example 2.

[0154] In the poorly dispersed microfibrillated cellulose dispersion, the number of aggregates with an equivalent diameter greater than 100 μm was 46 per mm².

[0155] Comparative Example 14 did not involve fiber grading, xylanase activation treatment, sequential reinforcement with cationic starch and amphoteric polyacrylamide, or the application of microfibrillated cellulose between paper layers.

[0156] The purified waste paper pulp undergoes only conventional beating and is formed into a surface layer, core layer, and bottom layer in a ratio of 28:44:28. After pressing, drying, and surface sizing, a linerboard with a basis weight of 160 g / m² is obtained.

[0157] Comparative Example 15 was produced in accordance with Example 2, except that after the microfibrillated cellulose dispersion was prepared, it was allowed to stand completely at room temperature for 24 hours and was not redispersed before use.

[0158] Comparative Example 16 was produced in accordance with Example 2, except that the microfibrillated cellulose dispersion was applied using a spray device without lateral zoning flow regulation, resulting in uneven nozzle coverage and a decrease in flow rate in some nozzles.

[0159] Performance testing 1. Fiber length test The fiber lengths of ungraded waste paper pulp, long fiber components, and short fiber components were determined according to GB / T 28218—2011 "Determination of Pulp Fiber Length - Image Analysis Method".

[0160] The length-weighted average fiber length was calculated based on the results of instrumental analysis.

[0161] 2. Fiber brooming rate test The fiber fibrillation rate of short fiber components before and after xylanase treatment was determined according to GB / T 22836—2008 "Determination of fiber fibrillation rate of pulp".

[0162] 3. Pulp water retention value test The water retention value of short fiber pulp before and after xylanase treatment was determined according to GB / T 29286—2012 "Determination of Water Retention Value of Pulp".

[0163] 4. Dispersion state test of microfibrillated cellulose Take 1 mL of microfibrillated cellulose dispersion, dilute it 100 times with deionized water, drop it onto a glass slide and cover it with a coverslip.

[0164] Ten random fields of view were observed using an optical microscope. The number of aggregates with an equivalent diameter greater than 100 μm was counted and converted into the number of aggregates per unit area.

[0165] 5. Interlayer reinforcement zone continuity test To facilitate the identification of the interlayer distribution of microfibrillated cellulose, in the verification experiment, a microfibrillated cellulose dispersion containing a small amount of cellulose-affinity fluorescent tracer was used instead of a regular microfibrillated cellulose dispersion, while other process conditions remained unchanged.

[0166] The obtained linerboard was cut into samples in the transverse direction, and then embedded in epoxy resin to prepare cross-sectional slices with a thickness of 10-30 μm.

[0167] Fluorescence microscopy was used to observe the interface between the surface layer and the core layer, as well as the interface between the core layer and the bottom layer.

[0168] Fluorescent bands that are continuously distributed along the paper layer interface and have a thickness of not less than 20 μm are identified as effective interlayer enhancement regions.

[0169] The continuity of the interlayer reinforcement zone is calculated using the following formula: Interlayer reinforcement zone continuity rate / % = Lc / L × 100%.

[0170] In the formula: Lc is the cumulative length of the effective continuous enhancement region on the detection interface, in mm; L represents the total length of the detection interface, in mm.

[0171] Five cross-sections were selected for each sample, with a test length of no less than 20 mm for each cross-section, and the average value was taken as the test result.

[0172] 6. Paperboard basis weight and sample preparation The basis weight of the paperboard was determined in accordance with GB / T 451.2—2023.

[0173] All physical property test specimens were equilibrated under standard atmospheric conditions as specified in GB / T 10739—2023.

[0174] 7. Short-range compressive strength test The transverse short-distance compressive strength of linerboard was determined according to GB / T 2679.10—1993, and the results are expressed in kN / m.

[0175] 8. Ring crush strength test Ring crush strength was determined according to GB / T 2679.8—2016, and the ring crush index was calculated quantitatively. The results are expressed in N·m / g.

[0176] 9. Bursting strength test The bursting strength of paperboard was determined according to GB / T 1539—2007, and the bursting index was calculated. The results are expressed as kPa·m² / g.

[0177] 10. Tensile strength test The tensile strength of linerboard was determined according to GB / T 12914—2018, and the tensile index was calculated. The results are expressed in N·m / g.

[0178] 11. Interlayer bond strength test According to GB / T 26203—2023, the internal bond strength of linerboard is determined using the Scott type interlayer bond strength test method, and the results are expressed in J / m².

[0179] 12. Water Absorption Test The Cobb water absorption of the front side of the linerboard was determined according to GB / T 1540—2002 over 60 seconds, and the result is expressed in g / m².

[0180] 13. Storage stability test of microfibrillated cellulose dispersion The same batch of microfibrillated cellulose dispersions were stored at different times and temperatures.

[0181] After storage, samples were taken from the top and bottom of the container to determine the solid content, and the relative deviation of the solid content between the upper and lower layers was calculated using the following formula: Relative deviation of solid content / % = |Cu-Cl| ÷ [(Cu+Cl) / 2] × 100%.

[0182] In the formula: Cu represents the solid content of the upper layer of the dispersion. Cl represents the solid content of the lower layer of the dispersion.

[0183] Meanwhile, the number of aggregates with an equivalent diameter greater than 100 μm was determined according to the aforementioned microscopic testing method, and the interlayer bonding strength was determined using the corresponding dispersion to prepare linerboard.

[0184] 14. Test on uniformity of application between microfibrillated cellulose layers A small amount of cellulose affinity fluorescent tracer was added to the microfibrillated cellulose dispersion.

[0185] The paper was divided into 10 detection areas at equal intervals along the transverse direction. The fluorescence intensity per unit area of ​​each area was measured, and the actual amount applied to each area was calculated based on the pre-established standard curve between fluorescence intensity and the amount of microfibrillated cellulose applied.

[0186] The coefficient of variation of the lateral application amount is calculated according to the following formula:

[0187] In the formula: s is the standard deviation of the amount applied in each lateral region; The average amount applied to each horizontal region.

[0188] The maximum local deviation is calculated using the following formula:

[0189] In the formula: This represents the actual amount applied to the i-th horizontal region.

[0190] For each application method, at least three paper rolls should be tested consecutively, and the average value should be taken as the test result.

[0191] Test Results 1. The effect of sieve slot width on fiber grading effect Table 1. Fiber grading results for different sieve slot widths

[0192] As shown in Table 1, when the screen opening width is too small, a large number of medium-length fibers are trapped in the long fiber component, resulting in an excessively high yield of the long fiber component and a significant increase in the pressure screen clogging rate. When the screen opening width is too large, more long fibers enter the short fiber component, leading to a decrease in the fiber length difference between the long and short fiber components and a decline in classification selectivity. When the screen opening width is 0.18–0.25 mm, a good balance can be achieved between the operational stability of the pressure screen and the fiber classification selectivity.

[0193] Table 2 Effect of xylanase dosage on short fiber properties

[0194] Table 2 shows that within the range of 20–200 U / g, the fibrillation rate and water retention value of short fibers significantly increased with increasing xylanase dosage, indicating moderate activation of the fiber surface. When the xylanase dosage was 10 U / g, the degree of fiber activation was limited; however, when the dosage reached 300 U / g, the fibrillation rate no longer increased significantly, while the pulp yield decreased significantly, indicating that excessive enzyme treatment may cause excessive hydrolysis of hemicellulose and dissolution of fine components. Therefore, the xylanase dosage should be controlled at 20–200 U / g, preferably 60–150 U / g.

[0195] Table 3 Test results of different reinforcing agent addition methods

[0196] Table 3 shows that both cationic starch and amphoteric polyacrylamide can improve the retention rate of fine molecules and the interlayer bonding strength to a certain extent. When both are added simultaneously or when amphoteric polyacrylamide is added first, some polymers tend to form flocs in the slurry prematurely, resulting in insufficient and uniform adsorption onto the fiber surface. Adding cationic starch first, allowing it to form an adsorption layer on the surface of the enzymatically activated short fibers, followed by adding amphoteric polyacrylamide for bridging, can achieve a higher retention rate of fine molecules and a stronger interlayer bonding strength.

[0197] Table 4. Effect of microfibrillated cellulose dosage on interlayer structure and dehydration performance.

[0198] Table 4 shows that a microfibrillated cellulose content of 0.20% is sufficient to form a partially continuous interlayer reinforcement zone. With increasing microfibrillated cellulose content, the continuity of the reinforcement zone and the interlayer bonding strength gradually improve; when the content reaches 0.80%–1.20%, the interlayer reinforcement zone exhibits good continuity. When the microfibrillated cellulose content exceeds 1.50%, the continuity of the reinforcement zone no longer increases significantly, the dewatering time of the wet paper sheet is significantly prolonged, and the interlayer bonding strength slightly decreases. This may be because excessive microfibrillated cellulose causes uneven local shrinkage, agglomeration, and excessively dense paper layer structure. Therefore, the optimal microfibrillated cellulose content is 0.20%–1.50% of the oven-dry fiber mass of the linerboard, preferably 0.50%–1.20%.

[0199] Table 5. Stability of microfibrillated cellulose dispersions under different storage conditions

[0200] Table 5 shows that when the microfibrillated cellulose dispersion is used immediately after preparation, or within 8 hours under low-speed stirring, the number of agglomerates and the deviation in solid content between the upper and lower layers are both low. After standing completely at room temperature for 24 hours, the number of large agglomerates in the dispersion increases significantly, resulting in a decrease in the interlayer bonding strength of the paperboard. Sealing the dispersion at 4–10°C for 24 hours and then redispersing it before use can maintain dispersion stability to some extent, but its interlayer strengthening effect is still slightly lower than that of a freshly prepared dispersion. When the low-temperature storage time is extended to 48 hours, even with redispersing, the number of large agglomerates still increases significantly. Therefore, microfibrillated cellulose dispersions are best prepared and used immediately; if immediate use is not possible, the low-temperature storage time should not exceed 24 hours.

[0201] Table 6. Uniformity and enhancement effect of different interlayer application methods

[0202] Table 6 shows that without lateral zoning flow control, the coefficient of variation of lateral application amount and the maximum local deviation are relatively large in ordinary spraying devices, resulting in a low continuity rate of the interlayer reinforcement zone. After adopting zoning spraying and linking the liquid supply flow rate with the paper machine running speed, the coefficient of variation of lateral application amount is reduced to 5.8%, and the continuity rate of the reinforcement zone is increased to 94%. Curtain coating and slot coating offer better lateral application uniformity, but the appropriate application method needs to be selected based on the paper machine structure, running speed, and wet paper layer strength. Considering equipment adaptability, operational flexibility, and application uniformity, the coefficient of variation of lateral application amount should ideally be controlled below 8%, preferably below 6%, and the maximum local deviation should ideally be controlled within ±10%.

[0203] Table 7. Properties of Corrugated Boards Obtained from Each Example and Comparative Example

[0204] As shown in Table 7, the short-range compression strength, ring crush index, bursting strength index, tensile strength index and interlayer bond strength of the linerboard obtained in Examples 1 to 5 are significantly higher than those of Comparative Example 14, which uses conventional production processes.

[0205] Example 2 uses a 0.22mm sieve, 100U / g xylanase, 12kg / t cationic starch, 0.60kg / t amphoteric polyacrylamide, and 0.80% microfibrillated cellulose, which has the most balanced overall performance.

[0206] Comparative Example 1 did not undergo fiber grading. Although enzymatic treatment, sequential reinforcement, and microfibrillated cellulose reinforcement were used, long fibers failed to concentrate in the top and bottom layers, resulting in lower short-pitch compression strength and ring crush strength compared to Example 2. Comparative Examples 2 and 3 demonstrate that both excessively small and excessively large sieve openings in the pressure screen are detrimental to the formation of long and short fiber components with significant length differences.

[0207] Comparative Examples 4-6 show that the strengthening effect of Example 2 cannot be obtained without enzyme treatment, with too low an enzyme dosage, or with too high an enzyme dosage. Excessive enzyme dosage may also cause excessive hydrolysis of fiber surface components, reducing pulp yield and the stability of the fiber bonding structure. Comparative Examples 7-10 show that the order of addition of cationic starch and amphoteric polyacrylamide has a significant impact on the strengthening effect. The absence of either reinforcing agent, or the simultaneous or reverse addition of both, will reduce interlayer bonding strength. Comparative Example 11 did not use microfibrillated cellulose for interlayer reinforcement, resulting in a significant decrease in interlayer bonding strength. Comparative Example 12 directly added microfibrillated cellulose to the core pulp, which improved some paper strength, but the microfibrillated cellulose failed to form a continuous reinforcing zone between adjacent paper layers, and its interlayer reinforcement effect was lower than that of the directional application method. In Comparative Example 13, the microfibrillated cellulose was not sufficiently dispersed, forming more agglomerates, leading to discontinuous reinforcing zones and causing local structural defects. In Comparative Example 15, the microfibrillated cellulose dispersion, after standing at room temperature for 24 hours, showed increased re-agglomeration and lower interlayer bonding strength compared to Example 2, indicating that the dispersion is not suitable for prolonged standing storage. In Comparative Example 16, the coefficient of variation for the transverse application amount of microfibrillated cellulose reached 14.2%, and the insufficient application in certain areas led to a decrease in the continuity of the interlayer reinforcement zone, indicating that the uniformity of application has a significant impact on the interlayer reinforcement effect.

[0208] Figure 1 In the image, the main structure of the short fibers remains intact, but the surface exhibits obvious longitudinal grooves, exposed fine fibers, and localized loosening and peeling of the surface layer. Arrow A indicates exposed fine fibers or microfibrillated areas on the surface, and arrow B indicates areas of loose or locally peeled fiber surface. The scale bar is 20 μm.

[0209] Figure 2 In the images, microfibrillated cellulose is mainly observed as long, thin filaments that interweave to form a loose network, with no obvious large-sized dense aggregates. Arrow A represents relatively independent and dispersed microfibrils, and arrow B represents local fiber bundles or overlapping areas. The scale bar is 500 nm.

[0210] Figure 3 In the diagram, green fluorescent signals represent microfibrillated cellulose, and gray areas represent pulp fibers. The dashed line L1 represents the interface between the surface layer and the core layer. Arrow A indicates a continuously distributed microfibrillated cellulose reinforcement band along the interface, and arrow B indicates the area that penetrates into and overlaps with the core layer fiber network. The scale bar is 100 μm.

[0211] Figure 4 In the diagram, the upper part is the surface layer, and the lower part is the core layer. The dashed line L1 represents the interface between the two. Arrow A indicates the fiber bridging structure across the interface, arrow B indicates the fine fiber network and pore-filling region at the interface, and arrow C indicates the tight overlap structure between adjacent fibers. The scale bar is 100 μm.

[0212] Figure 5 In the image, the fracture surface exhibits a rough and irregular morphology, with obvious fiber pulling, fiber wall tearing, and fine fiber residue visible. Arrow A indicates pulled-out fibers, arrow B indicates the fiber tearing area, and arrow C indicates the residual fine fiber network or cross-fiber overlapping structure. The scale bar is 50 μm.

[0213] In summary, controlling the storage and usage period of xylanase ensures the stability of the short fiber activation treatment; controlling the storage and redispersion of the microfibrillated cellulose dispersion ensures its dispersion state when it enters the interlayer application device; and adjusting the transverse application amount by region ensures the continuity and uniformity of the interlayer reinforcement structure.

Claims

1. A production process for low-quality corrugated cardboard, characterized in that, Includes the following steps: S1. Low-quality waste paper raw materials are crushed, slag removed, and coarsely screened to obtain recycled fiber pulp with a mass concentration of 2.0-4.5%; S2. The regenerated fiber pulp is classified using a pressure screen with a sieve opening of 0.15 to 0.30 mm to obtain a skeleton fiber pulp and a short fiber fine particle pulp, with an oven-dry mass ratio of 35:65 to 60:

40. S3. The skeleton fiber pulp is milled to a freeness of 28-38°SR; S4. The short fiber fine pulp is separated and reacted with endo-xylanase at 20-200 U / g oven-dry pulp at 40-55℃ and pH 5.0-7.0 for 20-90 min. After enzyme inactivation, 0.5-2.0% cationic starch and 0.02-0.15% amphoteric polyacrylamide relative to the oven-dry pulp mass are added sequentially to obtain cemented fiber pulp. S5. Prepare the surface layer slurry and bottom layer slurry with the skeleton fiber slurry, and prepare the core layer slurry with the binder fiber slurry. Sequentially form the surface layer, core layer and bottom layer in layers, and spray microfibrillated cellulose dispersion on each layer before bonding adjacent wet paper layers. The total oven-dry amount of the microfibrillated cellulose is 0.20-1.50% of the total oven-dry fiber mass of the linerboard. S6. The formed wet paper web is sequentially pressed, dried in sections, sizing the surface, and calendered to obtain the low-quality linerboard.

2. The production process for low-quality corrugated board according to claim 1, characterized in that, The low-quality waste paper raw materials include one or more of waste corrugated cardboard boxes, waste linerboard, and waste corrugated core paper; the pulp after the raw materials are crushed has an ash content of 8 to 18 wt%, a length-weighted average fiber length of 0.55 to 1.00 mm, and fine particles that can pass through a 200-mesh sieve account for 15 to 40% of the oven-dry pulp mass.

3. The production process for low-quality corrugated board according to claim 1, characterized in that, In step S2, the screen opening of the pressure screen is 0.18-0.25 mm. The retained component of the pressure screen is used as the skeleton fiber pulp, and the passed component of the pressure screen is used as the short fiber fine fraction pulp. In the skeleton fiber pulp, fibers with a length of not less than 1.5 mm account for 55-80% of the oven-dry fiber mass, and in the short fiber fine fraction pulp, fibers with a length of not more than 1.0 mm and the fine fraction together account for 60-85% of the oven-dry pulp mass.

4. The production process for low-quality corrugated board according to claim 1, characterized in that, The endoglucanase is a cellulase preparation obtained by fermentation of microorganisms of the genus Trichoderma, Aspergillus, or Bacillus; one enzyme activity unit U of the endoglucanase is defined as: the amount of enzyme required to catalyze the production of reducing sugar equivalent to 1 μmol of glucose per minute using sodium carboxymethyl cellulose as a substrate at 50°C and pH 4.

8. In step S4, 20-200 U / g of oven-dried pulp xylanase is added. The xylanase is an enzyme preparation obtained by fermentation of microorganisms of the genus Trichoderma, Aspergillus, or Bacillus. One enzyme activity unit U of xylanase is defined as the amount of enzyme required to catalyze the production of reducing sugar equivalent to 1 μmol xylose per minute using xylan as a substrate at 50°C and pH 5.

0.

5. The production process for low-quality corrugated board according to claim 1, characterized in that, In step S4, a cationic starch dispersion with a solid content of 2-8 wt% is first gelatinized at 90-98°C for 20-40 min, cooled to 45-60°C, and then added to the enzyme-inactivated short fiber fine slurry. The mixture is then stirred at 300-800 r / min for 5-20 min. Next, amphoteric polyacrylamide is diluted to a mass concentration of 0.05-0.20%, and added continuously and uniformly over 30-180 s, while continuing to mix at 200-500 r / min for 3-10 min. The degree of substitution of the cationic starch is 0.025-0.045, and the cationic degree of the amphoteric polyacrylamide is 5-20%, while the anionic degree is 2-10%.

6. The production process for low-quality corrugated board according to claim 1, characterized in that, In step S5, the surface layer slurry and the bottom layer slurry each contain skeletal fiber slurry accounting for 65-90% of their respective oven-dry fiber mass, and the core layer slurry contains cementing fiber slurry accounting for 60-85% of its oven-dry fiber mass; the oven-dry weight ratio of the surface layer, core layer and bottom layer is 20-30:40-60:20-30.

7. The production process for low-quality corrugated board according to claim 1, characterized in that, The interlayer reinforcing liquid comprises oxidized starch at a mass concentration of 6-12% and microfibrillated cellulose at a mass concentration of 0.5-5.0% relative to the oven-dry mass of oxidized starch; Before mixing with oxidized starch, the microfibrillated cellulose is first diluted with water to a solid content of 0.2-1.0%, sheared and dispersed at 3000-8000 r / min for 10-30 min, and then added to an oxidized starch solution at a temperature of 45-65℃ and mixed at 500-1500 r / min for 10-20 min to obtain an interlayer reinforcing liquid with a viscosity of 20-80 mPa·s. The interlayer reinforcing liquid is sprayed through a dual-fluid nozzle with an atomization pressure of 0.15–0.35 MPa, an overlap rate of 20–50% between adjacent nozzles, and a coefficient of variation of the amount of the sprayed horizontal strip that is dry to the touch not greater than 10%.

8. The production process for low-quality corrugated board according to claim 1, characterized in that, In step S6, the wet paper web passes sequentially through a first pressing zone with a linear pressure of 40-90 kN / m and a second pressing zone with a linear pressure of 100-220 kN / m, and the dryness of the paper web after pressing is 42-50%. The segmented drying process sequentially employs a pre-drying section at a temperature of 75–95°C, a main drying section at a temperature of 105–125°C, and a balance drying section at a temperature of 85–100°C. The surface sizing uses an oxidized starch sizing solution with a solid content of 6-14%, the single-sided oven-dry sizing amount is 0.5-2.0 g / m², and the calendering pressure is 30-90 kN / m.