A high-strength, anti-corrosion seedling paper, its preparation method and application

By coating the surface of seedling paper with a nanocellulose-based mixed emulsifier, a hydrophobic cross-linked network and an antibacterial layer are formed, solving the strength and antibacterial problems of paper seedling containers in humid environments, and realizing the preparation of high-strength and corrosion-resistant seedling paper.

CN123108992APending Publication Date: 2026-11-17ZHEJIANG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610980205.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Conventional paper seedling containers have low strength and are easily deformed in humid environments, and lack antibacterial components, leading to seedling failure and increased management costs.

Method used

A nanocellulose-based mixed emulsifier, containing polyhexamethylene biguanide, Kathon, and azobisisobutyronitrile, is coated on the surface of the substrate paper. This process initiates the copolymerization of acrylic acid and methyl methacrylate to form a hydrophobic polyacrylate crosslinking network, thereby enhancing paper strength and imparting antibacterial properties.

Benefits of technology

It significantly improves the wet tensile strength and antibacterial properties of seedling paper, prevents paper from deforming and rotting in humid environments, increases seedling success rate, and reduces management costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108992A_ABST
    Figure CN123108992A_ABST
Patent Text Reader

Abstract

This invention provides a high-strength, anti-corrosion seedling paper, its preparation method, and its applications, relating to the field of functional paper-based materials technology. The high-strength, anti-corrosion seedling paper is prepared by coating a substrate paper surface with a coating solution containing nanocellulose, polyhexamethylene biguanide, Kathon, azobisisobutyronitrile, acrylic acid, and methyl methacrylate, followed by initiated polymerization. During the preparation process, the functional coating solution with excellent stability and uniformity is obtained by precisely controlling the proportions of each component. The synergistic effect between the components improves both the dry and wet tensile strength of the paper. The seedling paper prepared by this invention possesses both high strength and excellent antibacterial properties, and can be widely used in the seedling field, effectively ensuring the healthy growth of seedlings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of functional paper-based materials technology, and in particular to a high-strength, anti-corrosion seedling paper, its preparation method, and its application. Background Technology

[0002] In the entire agricultural industry chain, seedling cultivation, as the initial stage of production, directly determines the final yield and quality of the crop. Seedling containers, as the physical carriers for seedling growth, play a crucial role in the success or failure of the entire seedling cultivation process due to their material properties. Currently, while the widely used plastic seedling trays and nutrient pots in agricultural production meet the structural stability requirements of large-scale production to some extent, their non-degradable nature has led to a serious "white pollution" problem. Waste plastic, after breaking down in the soil, severely damages the soil's aggregate structure and hinders water transport, making it unsuitable for the current development direction of green and circular agriculture.

[0003] To address environmental pressures, biodegradable seedling containers made from virgin paper or recycled pulp are gradually becoming an alternative. However, in actual industrialized seedling cultivation scenarios, the adoption of conventional paper containers is limited due to inherent material defects. Specifically, the strength of paper-based materials mainly comes from the hydrogen bonds between fibers. Under continuous irrigation and high humidity, water molecules penetrate into the fibers, causing hydrogen bonds to break and resulting in fiber swelling and softening. Conventional seedling paper has low wet strength, making it prone to softening, deformation, and scattering during automated transplanting processes, severely damaging seedling roots and significantly reducing transplant survival rates. Simultaneously, the warm and humid seedling environment is a breeding ground for fungi and bacteria. Conventional plant fibers lack effective antibacterial components, easily becoming a nutrient substrate for microorganisms. This not only accelerates the physical damage to the container walls but also triggers seedling diseases such as damping-off, leading to seedling failure and significantly increasing management costs.

[0004] In view of this, it is necessary to design an improved high-strength anti-corrosion seedling paper, its preparation method, and its application to solve the above problems. Summary of the Invention

[0005] The purpose of this invention is to provide a high-strength, anti-corrosion seedling paper, its preparation method, and its application.

[0006] To achieve the above-mentioned objectives, in a first aspect, the present invention provides a method for preparing high-strength, anti-corrosion seedling paper, characterized by comprising the following steps:

[0007] S1. Polyhexamethylene biguanide, Kathon and azobisisobutyronitrile are added to a nano-cellulose suspension to prepare a nano-cellulose-based mixed emulsifier.

[0008] The coating solution contains 1-10 wt% polyhexamethylene biguanide, 1-5 wt% Kathon, and 5 wt% azobisisobutyronitrile.

[0009] S2. Add methyl methacrylate mixture to the nanocellulose-based mixed emulsifier obtained in step S1, emulsify, and obtain a coating liquid; coat the coating liquid onto the surface of the substrate paper to obtain high-strength anti-corrosion seedling paper.

[0010] Preferably, in step S2, the coating amount of the coating liquid is 1-15 g / m². 2 .

[0011] Preferably, in step S1, the mass percentage of the nanocellulose suspension is 0.25-1.0 wt%.

[0012] Preferably, in step S1, the mass percentage of the nanocellulose suspension is 1.0 wt%, the mass percentage of the polyhexamethylene biguanide in the coating solution is 10 wt%, and the mass percentage of Kathon in the coating solution is 5 wt%.

[0013] Preferably, in step S2, the methyl methacrylate mixture is composed of acrylic acid and methyl methacrylate, wherein the mass ratio of methyl methacrylate to acrylic acid is 9:1; and the volume ratio of the methyl methacrylate mixture to the nanocellulose-based mixed emulsifier is 1:4.

[0014] Preferably, in step S2, the emulsification process is carried out under ultrasonic conditions for 1-10 minutes.

[0015] Preferably, in step S2, the basis weight of the substrate paper is 50-60 g / m³. 2 .

[0016] Preferably, the ultrasound time is 5 minutes.

[0017] Secondly, the present invention provides a high-strength, corrosion-resistant seedling paper.

[0018] Thirdly, the present invention provides an application of high-strength anti-corrosion seedling paper in seedling cultivation.

[0019] The beneficial effects of this invention are:

[0020] 1. The high-strength anti-corrosion seedling paper provided by the present invention is prepared by coating a coating liquid containing nanocellulose, polyhexamethylene biguanide, Kathon, azobisisobutyronitrile, acrylic acid, and methyl methacrylate onto the surface of a substrate paper and then initiating polymerization. Azobisisobutyronitrile is used as a thermal initiator to initiate in-situ copolymerization of acrylic acid and methyl methacrylate on the surface of the cellulose fibers of the substrate paper, forming a hydrophobic polyacrylate crosslinking network. Polyhexamethylene biguanide and Kathon provide antibacterial properties, giving the paper antibacterial properties and preventing it from being degraded and damaged by microorganisms when used for seedling cultivation. This effectively solves the defects of traditional seedling paper base materials that deform when exposed to water and are damaged during the seedling cultivation process.

[0021] 2. The high-strength anti-corrosion seedling paper provided by the present invention is prepared by first mixing the antibacterial agents polyhexamethylene biguanide and Kathon with the remaining raw materials evenly before coating. This not only ensures that the polyhexamethylene biguanide and Kathon are evenly distributed in the coating layer, but also allows the polyhexamethylene biguanide and Kathon to be encapsulated in the crosslinked network formed by the copolymerization of acrylic acid and methyl methacrylate. This not only reduces the amount of antibacterial agent used, but also prevents the antibacterial agent from being lost and affecting the paper performance, thereby maximizing the effect of the antibacterial agent and ensuring the stable performance of the seedling paper. Attached Figure Description

[0022] Figure 1 This is a Leica microscope image of the coating liquid prepared in Example 1 of the present invention;

[0023] Figure 2 These are optical photographs of the coating solutions prepared in Examples 1-4 of this invention after standing for 1 week.

[0024] Figure 3 This is an optical photograph of the seedling paper prepared in Example 1 of the present invention after being buried in the soil for 40 days;

[0025] Figure 4 This is a Leica microscope image of the coating liquid prepared in Example 2 of the present invention;

[0026] Figure 5 This is an optical photograph of the seedling paper prepared in Example 2 of the present invention after being buried in the soil for 40 days;

[0027] Figure 6 This is a Leica microscope image of the coating liquid prepared in Example 3 of the present invention;

[0028] Figure 7 This is an optical photograph of the seedling paper prepared in Example 3 of the present invention after being buried in the soil for 40 days;

[0029] Figure 8 This is a Leica microscope image of the coating liquid prepared in Example 4 of the present invention;

[0030] Figure 9 This is an optical photograph of the seedling paper prepared in Example 4 of the present invention after being buried in the soil for 40 days;

[0031] Figure 10 This is an optical photograph of the substrate paper used in Example 4 of the present invention after being buried in the soil for 40 days.

[0032] Figure 11 An optical photograph of the seedling paper prepared in Comparative Example 1 of this invention after being buried in soil for 40 days;

[0033] Figure 12 This is a Leica microscope image of the coating liquid prepared in Comparative Example 2 of the present invention.

[0034] Figure 13 This is an optical photograph of the seedling paper prepared in Comparative Example 2 of the present invention after being buried in the soil for 40 days. Detailed Implementation

[0035] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in detail below with reference to the accompanying drawings and specific embodiments.

[0036] It should also be noted that, in order to avoid obscuring the present invention with unnecessary details, only the structures and / or processing steps closely related to the present invention are shown in the accompanying drawings, while other details that are not closely related to the present invention are omitted.

[0037] Additionally, it should be noted that the terms “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0038] This invention provides a method for preparing high-strength, anti-corrosion seedling paper, comprising the following steps:

[0039] S1. Add polyhexamethylene biguanide, Kathon and azobisisobutyronitrile to the nanocellulose suspension and mix evenly to obtain a nanocellulose-based mixed emulsifier.

[0040] S2. Add methyl methacrylate mixture to the nanocellulose-based mixed emulsifier obtained in step S1, emulsify, and obtain a coating liquid; coat the coating liquid onto the surface of the substrate paper to obtain high-strength anti-corrosion seedling paper.

[0041] The preparation mechanism of the above preparation method is as follows: Azobisisobutyronitrile (AIB) acts as a thermal initiator, which can decompose to generate free radicals, initiating in-situ copolymerization of acrylic acid and methyl methacrylate on the surface of cellulose fibers of the substrate paper to form a hydrophobic polyacrylate crosslinking network. This network not only significantly improves the wet tensile strength and burst strength of the paper by physically encapsulating and sealing the hydrophilic hydroxyl sites on the fiber surface, but also enhances the overall cohesiveness of the coating. Meanwhile, polyhexamethylene biguanide and Kathon can impart antibacterial and anti-corrosion properties to the seedling paper, preventing it from being degraded and damaged by microorganisms when used for seedling cultivation.

[0042] In some embodiments, in step S1, the mass percentage of the nanocellulose suspension is 0.25-1.0 wt%, preferably cellulose nanofibers (CNF), which are obtained by high-pressure homogenization or milling and defibrillation of plant cellulose, and have a Zeta potential of -32.4 mV. The mass percentage of polyhexamethylene biguanide in the coating solution is 1-10 wt%, the mass percentage of Kathon in the coating solution is 1-5 wt%, and the mass percentage of azobisisobutyronitrile (AIBN) in the coating solution is 5 wt%. Preferably, the mass percentage of the nanocellulose suspension is 1.0 wt%, the mass percentage of polyhexamethylene biguanide in the coating solution is 10 wt%, and the mass percentage of Kathon in the coating solution is 5 wt%.

[0043] In the above technical solution, by selecting nanocellulose as the main emulsifier, its amphiphilicity and nanoscale effect allow it to adsorb at the interface between the oil and water phases composed of methyl methacrylate and acrylic acid. Through steric hindrance, a dense solid particle barrier is formed, effectively inhibiting droplet aggregation and constructing a monomer emulsion with uniform particle size and stable dispersion. This interface structure anchored by nanocellulose not only ensures the uniform spreading and wetting of the coating liquid on the paper substrate surface but also provides a confined reaction site for initiator-induced in-situ free radical copolymerization, achieving a strong interlock between the polymer network and cellulose fibers. By using polyhexamethylene biguanide and Kathon as antibacterial agents in combination, Kathon's rapid bactericidal properties can compensate for the insufficient initial antibacterial rate of polyhexamethylene biguanide, while the durability of polyhexamethylene biguanide can offset the time-dependent decay of Kathon. This extends the overall antibacterial and preservative lifespan while significantly reducing the raw material cost pressure caused by using high-molecular-weight guanidine salts alone, achieving the best balance between performance and economy.

[0044] In some embodiments, in step S2, the methyl methacrylate mixture is obtained by mixing acrylic acid and methyl methacrylate. Preferably, the mass ratio of methyl methacrylate to acrylic acid is 9:1, that is, based on the total mass of monomers, the mass percentage of methyl methacrylate is 90 wt%, the mass percentage of acrylic acid is 10 wt%, and the volume ratio of the methyl methacrylate mixture to the nanocellulose-based mixed emulsifier is 1:4.

[0045] In some embodiments, in step S2, the emulsification process is carried out under ultrasonic conditions for 1-10 minutes. The ultrasonic process of the present invention does not have too many requirements for temperature and power, as long as emulsification can be achieved.

[0046] In some embodiments, in step S2, the coating amount of the coating liquid is 1-15 g / m². 2 .

[0047] The high-strength, anti-corrosion seedling paper, its preparation method, and its application provided by the present invention will be further explained below with reference to specific embodiments:

[0048] Example 1

[0049] This embodiment provides a method for preparing high-strength anti-corrosion seedling paper, including the following steps: adding polyhexamethylene biguanide, Kathon, and azobisisobutyronitrile to a CNF suspension with a mass percentage of 0.25 wt% to obtain a CNF-based mixed emulsifier, wherein the mass percentages of polyhexamethylene biguanide, Kathon, and azobisisobutyronitrile in the emulsifier are 1 wt%, 1 wt%, and 5 wt%, respectively;

[0050] Add methyl methacrylate mixture to the above CNF-based mixed emulsifier and ultrasonically emulsify for 5 min to obtain coating liquid; wherein, the methyl methacrylate mixture is obtained by mixing acrylic acid and methyl methacrylate, the mass percentage of methyl methacrylate in the mixture is 90 wt%, the mass percentage of acrylic acid is 10 wt%, and the volume ratio of methyl methacrylate mixture to CNF-based mixed emulsifier is 1:4.

[0051] The above coating solution was applied at a concentration of 10 g / m 2 The coating amount is 50 g / m². 2 The surface of the substrate paper is heated and dried at 60°C for 1 hour to obtain high-strength, anti-corrosion seedling paper. It should be noted that, unless otherwise specified, the reagents and raw materials used in the embodiments of this invention can be obtained commercially.

[0052] The morphology and structure of the coating liquid were observed using a Leica microscope, and the results were as follows: Figure 1 As shown, the average size of the oil phase droplets in the coating solution is 284 μm, and the size distribution is poor, with a large number of oil phase droplets exceeding 500 μm in size. Optical photographs of the coating solution after standing at room temperature (25℃) for one week are shown below. Figure 2 (correspond Figure 2As shown in the first image from left to right, the results show obvious stratification of the coating solution, indicating poor stability of the coating solution under these conditions. Further testing of the paper properties after coating revealed that the dry tensile strength increased from 2.1434 kN / m to 3.2883 kN / m of the uncoated substrate paper, and the wet tensile strength increased from 0.8172 kN / m to 1.0782 kN / m. The seedling paper prepared in this embodiment was buried in soil for 40 days. The burial process was carried out outdoors in soil with an average temperature of 30℃ and an ambient humidity of 70%RH. The soil was kept moist by watering every two days. Optical photographs of the seedling paper after 40 days of burial are shown below. Figure 3 As shown in the image, the paper exhibits obvious signs of decay and degradation.

[0053] Example 2

[0054] This embodiment provides a method for preparing high-strength, anti-corrosion seedling paper, including the following steps:

[0055] Polyhexamethylene biguanide, Kathon, and azobisisobutyronitrile were added to a CNF suspension with a mass percentage of 0.50 wt% to obtain a CNF-based mixed emulsifier. The mass percentages of polyhexamethylene biguanide, Kathon, and azobisisobutyronitrile in the emulsifier were 2 wt%, 2 wt%, and 5 wt%, respectively.

[0056] Add methyl methacrylate mixture to the above CNF-based mixed emulsifier and ultrasonically emulsify for 5 min to obtain coating liquid; wherein, the methyl methacrylate mixture is obtained by mixing acrylic acid and methyl methacrylate, the mass percentage of methyl methacrylate in the mixture is 90 wt%, the mass percentage of acrylic acid is 10 wt%, and the volume ratio of methyl methacrylate mixture to CNF-based mixed emulsifier is 1:4.

[0057] The above coating solution was applied at a concentration of 10 g / m 2 The coating amount is 50 g / m². 2 The surface of the substrate paper is heated and dried at 60℃ for 1 hour to obtain high-strength anti-corrosion seedling paper.

[0058] The morphology and structure of the coating liquid were observed using a Leica microscope, and the results were as follows: Figure 4 As shown, the average droplet size of the oil phase of the coating solution is 213 μm, and the size distribution is poor, with some droplets exceeding 500 μm in size. Optical photographs of the coating solution after one week of settling are shown below. Figure 2 (correspond Figure 2As shown in the second image from the left (from right), the results show that the coating solution exhibited obvious stratification, indicating poor stability under these conditions. Further testing of the paper properties after coating revealed that the dry tensile strength increased from 2.1434 kN / m to 3.4136 kN / m of the uncoated substrate paper, and the wet tensile strength increased from 0.8172 kN / m to 1.1811 kN / m. The seedling paper prepared in this embodiment was buried in soil for 40 days. The burial process was carried out outdoors in soil with an average temperature of 30°C and an ambient humidity of 70% RH. The soil was kept moist by watering every two days. Optical photographs of the seedling paper after 40 days of burial are shown below. Figure 5 As shown in the image, the paper exhibits a small amount of decay and degradation.

[0059] Example 3

[0060] This embodiment provides a method for preparing high-strength, anti-corrosion seedling paper, including the following steps:

[0061] Polyhexamethylene biguanide, Kathon, and azobisisobutyronitrile were added to a CNF suspension with a mass percentage of 0.75 wt% to obtain a CNF-based mixed emulsifier. The mass percentages of polyhexamethylene biguanide, Kathon, and azobisisobutyronitrile in the emulsifier were 5 wt%, 5 wt%, and 5 wt%, respectively.

[0062] Add methyl methacrylate mixture to the above CNF-based mixed emulsifier and ultrasonically emulsify for 5 min to obtain coating liquid; wherein, the methyl methacrylate mixture is obtained by mixing acrylic acid and methyl methacrylate, the mass percentage of methyl methacrylate in the mixture is 90 wt%, the mass percentage of acrylic acid is 10 wt%, and the volume ratio of methyl methacrylate mixture to CNF-based mixed emulsifier is 1:4.

[0063] The above coating solution was applied at a concentration of 10 g / m 2 The coating amount is 60 g / m². 2 The surface of the substrate paper is heated and dried at 60℃ for 1 hour to obtain high-strength anti-corrosion seedling paper.

[0064] The morphology and structure of the coating liquid were observed using a Leica microscope, and the results were as follows: Figure 6 As shown, the average size of the oil phase droplets in the coating solution is 164 μm, and the size distribution uniformity is poor; however, a small number of oil phase droplets with a size exceeding 500 μm still exist. Optical photographs of the coating solution after one week of settling are shown below. Figure 2 (correspond Figure 2As shown in the third image from the left (the third image from the right), the results show obvious stratification of the coating solution, indicating poor stability of the coating solution under these conditions. Further testing of the paper properties after coating revealed that the dry tensile strength increased from 2.8521 kN / m to 4.0924 kN / m of the uncoated substrate paper, and the wet tensile strength increased from 0.9558 kN / m to 1.2597 kN / m. The seedling paper prepared in this embodiment was buried in soil for 40 days. The burial process was carried out outdoors in soil with an average temperature of 30℃ and an ambient humidity of 70%RH. The soil was kept moist by watering every two days. Optical photographs of the seedling paper after 40 days of burial are shown below. Figure 7 As shown in the figure, the paper does not show obvious signs of decay or degradation.

[0065] Example 4

[0066] This embodiment provides a method for preparing high-strength, anti-corrosion seedling paper, including the following steps:

[0067] Polyhexamethylene biguanide, Kathon, and azobisisobutyronitrile were added to a CNF suspension with a mass percentage of 1.0 wt% to obtain a CNF-based mixed emulsifier. The mass percentages of polyhexamethylene biguanide, Kathon, and azobisisobutyronitrile in the emulsifier were 10 wt%, 5 wt%, and 5 wt%, respectively.

[0068] Add methyl methacrylate mixture to the above CNF-based mixed emulsifier and ultrasonically emulsify for 5 min to obtain coating liquid; wherein, the methyl methacrylate mixture is obtained by mixing acrylic acid and methyl methacrylate, the mass percentage of methyl methacrylate in the mixture is 90 wt%, the mass percentage of acrylic acid is 10 wt%, and the volume ratio of methyl methacrylate mixture to CNF-based mixed emulsifier is 1:4.

[0069] The above coating solution was applied at a concentration of 15 g / m 2 The coating amount is 60 g / m². 2 The surface of the substrate paper is heated and dried at 60℃ for 1 hour to obtain high-strength anti-corrosion seedling paper.

[0070] The morphology and structure of the coating liquid were observed using a Leica microscope, and the results were as follows: Figure 8 As shown, the average droplet size of the oil phase in the coating solution is 63 μm, and no stratification is observed, with an emulsion index of 100%. Optical photographs of the coating solution after one week of settling are shown below. Figure 2 (correspond Figure 2As shown in the fourth image from the left (fourth from the right), the results show that the coating solution exhibited obvious stratification, indicating poor stability under these conditions. Further testing of the paper properties after coating revealed that the dry tensile strength increased from 2.8521 kN / m to 4.3260 kN / m of the uncoated substrate paper, and the wet tensile strength increased from 0.9558 kN / m to 1.4381 kN / m. The seedling paper prepared in this embodiment was buried in soil for 40 days. The burial process was carried out outdoors in soil with an average temperature of 30°C and an ambient humidity of 70% RH. The soil was kept moist by watering every two days. Optical photographs of the seedling paper after 40 days of burial are shown below. Figure 9 As shown in the image, the paper does not exhibit obvious signs of decay or degradation. The basis weight is 60 g / m³. 2 Optical photographs of the substrate paper after being buried in soil for 40 days under the same conditions, such as... Figure 10 As shown, the results indicate that the seedling paper decomposes more fully than the coated seedling paper, which indirectly demonstrates that the seedling paper prepared in this embodiment has higher strength and corrosion resistance than the base paper.

[0071] Comparative Example 1

[0072] The only difference between this comparative example and Example 4 is that azobisisobutyronitrile and methyl methacrylate are not added. The specific preparation steps are as follows:

[0073] Polyhexamethylene biguanide and Kathon were added to a CNF suspension with a mass percentage of 1.0 wt% to obtain a CNF-based mixed emulsifier, wherein the mass percentages of polyhexamethylene biguanide and Kathon in the emulsifier were 10 wt% and 5 wt%, respectively.

[0074] Using the above CNF-based mixed emulsifier as the coating liquid, at a concentration of 15 g / m²... 2 The coating amount is 60 g / m². 2 The surface of the substrate paper is heated and dried at 60℃ for 1 hour to obtain high-strength anti-corrosion seedling paper.

[0075] The results showed that the dry tensile strength of the seedling paper increased from 2.8521 kN / m to 3.6826 kN / m of the uncoated substrate paper, and the wet tensile strength increased from 0.9558 kN / m to 1.1724 kN / m. Compared with Example 4, the strength of the seedling paper was significantly reduced. This is because Comparative Example 1 lacked the methyl methacrylate mixture, which prevented the formation of a dense and stable water-resistant reinforcing coating on the paper surface. Furthermore, the single CNF coating was easily damaged by water, resulting in a decrease in both dry and wet strength. The seedling paper prepared in this example was buried in soil for 40 days. The burial process was carried out outdoors in soil with an average temperature of 30°C and an ambient humidity of 70% RH. The soil was kept moist by watering every two days. The optical photographs of the seedling paper after 40 days of burial are shown below. Figure 11 As shown in the figure, the paper does not show obvious signs of decay or degradation.

[0076] Comparative Example 2

[0077] The only difference between this comparative example and Example 4 is that polyhexamethylene biguanide and Kathon are not added. The specific preparation steps are as follows:

[0078] Azobisisobutyronitrile (AIBN) was added to a CNF suspension with a mass percentage of 1.0 wt% to obtain a CNF-based mixed emulsifier, wherein the mass percentage of AIBN, the three components in the emulsifier was 5 wt%.

[0079] Add methyl methacrylate mixture to the above CNF-based mixed emulsifier and ultrasonically emulsify for 5 min to obtain coating liquid; wherein, the methyl methacrylate mixture is obtained by mixing acrylic acid and methyl methacrylate, the mass percentage of methyl methacrylate in the mixture is 90 wt%, the mass percentage of acrylic acid is 10 wt%, and the volume ratio of methyl methacrylate mixture to CNF-based mixed emulsifier is 1:4.

[0080] The above coating solution was applied at a concentration of 15 g / m 2 The coating amount is 60 g / m². 2 The surface of the substrate paper is heated and dried at 60℃ for 1 hour to obtain high-strength anti-corrosion seedling paper.

[0081] The morphology and structure of the coating liquid were observed using a Leica microscope, and the results were as follows: Figure 12 As shown, the average droplet size of the oil phase of the coating solution was 58 μm. The droplet size of the coating solution was significantly reduced and it exhibited good uniformity. After standing for one week, no stratification was observed in the coating solution, and the emulsion index was 100%, indicating that the coating solution had good stability under these conditions. Further testing of the paper properties after coating revealed that the dry tensile strength increased from 2.8521 kN / m of the uncoated substrate paper to 4.2478 kN / m, and the wet tensile strength increased from 0.9558 kN / m of the uncoated substrate paper to 1.3975 kN / m. Compared with the seedling paper prepared in Example 4, the strength was significantly reduced. This is because the coating solution in Comparative Example 2 lacked polyhexamethylene biguanide and Kathon, which prevented the formation of a dense and stable anti-corrosion reinforcing coating on the paper surface. In a humid and warm environment, the fibers rapidly degraded and rotted, affecting the use of the seedling paper. The seedling paper prepared in this embodiment was buried in soil for 40 days. The burial process was carried out outdoors in soil with an average temperature of 30°C and an ambient humidity of 70%RH. The soil was kept moist by watering every two days. The optical photograph of the seedling paper after 40 days of burial is shown below. Figure 13 As shown in the image, the paper exhibits obvious signs of decay and degradation.

[0082] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention.

Claims

1. A method for preparing high-strength, anti-corrosion seedling paper, characterized in that, Includes the following steps: S1. Polyhexamethylene biguanide, Kathon and azobisisobutyronitrile are added to the nanocellulose suspension to prepare a nanocellulose-based mixed emulsifier. The coating solution contains 1-10 wt% polyhexamethylene biguanide, 1-5 wt% Kathon, and 5 wt% azobisisobutyronitrile. S2. Add methyl methacrylate mixture to the nanocellulose-based mixed emulsifier obtained in step S1, emulsify, and obtain a coating liquid; coat the coating liquid onto the surface of the substrate paper to obtain high-strength anti-corrosion seedling paper.

2. The preparation method according to claim 1, characterized in that, In step S2, the coating amount of the coating liquid is 1-15 g / m². 2 .

3. The preparation method according to claim 1, characterized in that, In step S1, the mass percentage of the nanocellulose suspension is 0.25-1.0 wt%.

4. The preparation method according to claim 1, characterized in that, In step S1, the mass percentage of the nanocellulose suspension is 1.0 wt%, the mass percentage of the polyhexamethylene biguanide in the coating solution is 10 wt%, and the mass percentage of Kathon in the coating solution is 5 wt%.

5. The preparation method according to claim 1, characterized in that, In step S2, the methyl methacrylate mixture is composed of acrylic acid and methyl methacrylate, wherein the mass ratio of methyl methacrylate to acrylic acid is 9:1; and the volume ratio of the methyl methacrylate mixture to the nanocellulose-based mixed emulsifier is 1:

4.

6. The preparation method according to claim 1, characterized in that, In step S2, the emulsification process is carried out under ultrasonic conditions for 1-10 minutes.

7. The preparation method according to claim 1, characterized in that, In step S2, the basis weight of the substrate paper is 50-60 g / m³. 2 .

8. The preparation method according to claim 6, characterized in that, The ultrasound duration is 5 minutes.

9. A high-strength, anti-corrosion seedling paper prepared by the method described in claims 1-8.

10. The application of a high-strength anti-corrosion seedling paper prepared by the preparation method described in claims 1-8 or the high-strength anti-corrosion seedling paper described in claim 9 in seedling cultivation.