A high-sealing, heat-insulating, and energy-saving door and window and its manufacturing process.

By combining a five-cavity, three-thermal-bridge profile and a four-layer gradient sealing system with dynamic double-network sealing materials, the problem of insufficient sealing and heat insulation performance of building doors and windows is solved, achieving high sealing, heat insulation, energy saving and sound insulation effects, and significantly improving the heat transfer coefficient and sealing performance of the entire window.

CN123109525APending Publication Date: 2026-11-17SHANDONG YUEYANG DOOR & WINDOW CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611531679.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing building doors and windows have deficiencies in sealing and heat insulation performance. The sealing strips are prone to aging and deformation, resulting in decreased air tightness and water tightness, and limited heat insulation efficiency, making it difficult to meet the requirements for long-term use.

Method used

It adopts a five-cavity, three-break bridge profile structure, a four-stage gradient sealing system, and a dynamic double-network sealing material. Combined with a three-layer insulated glass assembly, it forms an active compensation-mechanical throttling-low-pressure auxiliary gradient pressure reduction system through the combination of inflatable expansion sealing strips, labyrinth sealing strips, and low-pressure airbag sealing strips.

Benefits of technology

It achieves high sealing, heat insulation, energy saving and sound insulation performance, with a whole window heat transfer coefficient as low as 0.72~0.77 W/(m2·K), excellent sealing performance, low compression permanent deformation rate, high rebound recovery rate, long inflation and deflation cycle life, and a weighted sound insulation of 43 dB.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123109525A_ABST
    Figure CN123109525A_ABST
Patent Text Reader

Abstract

This invention discloses a high-sealing, heat-insulating, and energy-saving door and window and its manufacturing process, belonging to the field of building door and window technology. The window frame and sash profiles adopt a five-cavity, three-break structure consisting of a five-cavity body and three PA66 nylon thermal insulation strips. The second, fourth, and thermal insulation cavities are filled with polyurethane foam material. Four seals are installed between the window frame and sash: an inflatable expansion sealing strip, a soft-hard composite sealing strip, a labyrinth-type sealing strip, and a low-pressure airbag sealing strip. The first and fourth seals form a double-inflatable dynamic compensation system and, together with the labyrinth-type seal, form a gradient pressure-reducing sealing system. The sealing strips are made of dynamically double-network modified EPDM rubber. The insulated glass assembly is a triple-glazed Low-E glass. The door and window of this invention possess high sealing, heat insulation, energy-saving, and sound insulation characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building door and window technology, and in particular to a high-sealing, heat-insulating, and energy-saving door and window and its manufacturing process. Background Technology

[0002] Building doors and windows, being the weakest link in the building envelope in terms of thermal performance, account for 25% to 35% of the total building energy consumption, with heat transfer loss accounting for approximately 60% and air infiltration accounting for approximately 40%. Passive ultra-low energy buildings require the overall window heat transfer coefficient to be controlled at 0.8 W / (m²). 2 ·K) or below, to reduce building heating and cooling loads by more than 50%.

[0003] Aluminum alloy windows and doors, with their advantages of lightweight, high strength, and corrosion resistance, have rapidly replaced traditional steel windows since the 1990s and are widely used in residential, office, and high-rise buildings. However, the high thermal conductivity of aluminum alloys results in inherent deficiencies in their thermal insulation performance, which needs to be compensated for through "thermal break" technology, embedding thermal break strips in the profiles. In existing technologies, some windows and doors use double-cavity thermal break strips combined with a triple-sealing structure, reducing the overall window heat transfer coefficient to 1.1 W / (m²). 2 Approximately ·K); some high-end products can achieve a heat transfer coefficient as low as 0.8 W / (m²) through a five-chamber insulation system. 2 For example, CN 207553922 U discloses a four-sealed plastic profile door and window, in which the door and window frame and the door and window sash are seamlessly connected and spliced ​​again by four sealing strips, so that the cavity interior forms a triple sealed space, which greatly improves the airtightness, sound insulation and heat preservation performance.

[0004] However, the above-mentioned technical solutions still have the following shortcomings: In terms of sealing, the existing sealing structures of doors and windows are mostly single or double seals. After long-term use, the sealing strips are prone to aging and deformation, and the air tightness and water tightness are significantly reduced. Under repeated compression and temperature changes, the permanent compression deformation of the sealing strips gradually increases, and the resilience performance is weakened, resulting in an increase in the sealing gap, which makes it difficult to meet the requirements of long-term use of building doors and windows. In terms of thermal insulation, the existing thermal insulation strips mostly adopt a single-cavity or double-cavity "I"-shaped structure, which has a short thermal insulation path. Moreover, the thermal insulation cavity of the profile is mostly a hollow structure, which only uses the air gap for thermal insulation and does not fill with high-efficiency thermal insulation materials, resulting in limited thermal insulation efficiency.

[0005] In conclusion, the existing technology obviously has inconveniences and defects in practical use, so it is necessary to improve it. Summary of the Invention

[0006] To address the aforementioned shortcomings, the present invention aims to provide a high-sealing, heat-insulating, and energy-saving door and window and its manufacturing process. Through the comprehensive design of a five-cavity, three-thermal-bridge profile structure, a four-gradient sealing system, a dual-inflation dynamic compensation mechanism, and a dynamic dual-network sealing material, it achieves high sealing, heat insulation, energy saving, and sound insulation characteristics.

[0007] To achieve the above objectives, the present invention provides a high-sealing, heat-insulating, and energy-saving door and window, including a window frame, a window sash, and an insulated glass assembly installed inside the window sash;

[0008] Both the window frame and the window sash adopt a five-cavity, three-thermal-break profile structure.

[0009] The window frame is provided with a first sealing groove, a third sealing groove and a fourth sealing groove in sequence from the outside to the inside. The first sealing groove, the third sealing groove and the fourth sealing groove are respectively provided with an inflatable sealing strip, a labyrinth sealing strip and a low-pressure airbag sealing strip.

[0010] The window sash is provided with a second sealing groove, and a soft and hard composite sealing strip is provided in the second sealing groove;

[0011] The inflatable sealing strip, soft-hard composite sealing strip, labyrinth sealing strip, and low-pressure airbag sealing strip are made of a dynamic dual-network modified EPDM rubber composition.

[0012] Preferably, the dynamic dual-network modified EPDM rubber composition comprises, by weight: 100 parts maleic anhydride-grafted EPDM rubber, 3-10 parts furfurylamine, 2-8 parts bismaleimide crosslinking agent, 5-12 parts zinc methacrylate, 15-25 parts core-shell structured nanofiller, 2-8 parts modified graphene oxide, 1-3 parts ionic liquid functional additive, 3-6 parts modified nano lanthanum oxide particles, 1.5-3 parts sulfur, 1-2 parts accelerator CZ, 3-8 parts zinc oxide, and 1-2 parts stearic acid.

[0013] Preferably, the inflatable sealing strip has an inflatable cavity extending along its length, which is connected to the outside through a micro air valve, and the inflation pressure is 0.15~0.30 MPa; the ratio of the inflation pressure of the inflatable sealing strip to the inflation pressure of the low-pressure airbag sealing strip is 2~3:1.

[0014] Preferably, the insulating glass assembly is a three-layer insulating Low-E glass structure, with a hollow layer formed between adjacent glass panes, and the hollow layer is filled with argon gas.

[0015] Preferably, the five-cavity, three-thermal-bridge profile structure includes a first cavity, a second cavity, a third cavity, a fourth cavity, and a fifth cavity arranged sequentially from the outside to the inside. Thermal insulation cavities for installing thermal insulation strips are provided between the first cavity and the second cavity, the second cavity and the third cavity, and the third cavity and the fourth cavity profile. PA66 nylon thermal insulation strips are installed within each thermal insulation cavity, consisting of an outdoor C-shaped thermal insulation strip, a central flat multi-cavity thermal insulation strip, and an indoor irregularly shaped multi-cavity thermal insulation strip, forming three thermal breaks. The second cavity, the fourth cavity, and the thermal insulation cavity are also filled with B1-grade polyurethane foam material.

[0016] Preferably, in the dynamic dual-network modified EPDM rubber composition, the core-shell structured nanofiller is a composite material with porous nano-silica as the core, an organosiloxane network, and embedded nano-tungsten disulfide as the shell; the modified graphene oxide is graphene oxide modified with furfuryl alcohol, barium sulfate, and salicylic acid, with a sheet thickness of 1~5 nm and a sheet diameter of 0.5~5 μm; the modified nano-lanthanum oxide particles have nano-lanthanum oxide as the core, and the surface of the nano-lanthanum oxide is modified with an ionic liquid to form a modification layer, the modification layer thickness is 2~10 nm, the ionic liquid is 1-hexyl-3-methylimidazolium hexafluorophosphate, and the particle size of the modified nano-lanthanum oxide particles is 20~100 nm.

[0017] Preferably, in the dynamic dual-network modified EPDM rubber composition, the maleic anhydride-grafted EPDM rubber has a Mooney viscosity ML(1+4) of 40~80 at 100°C and a grafting rate of 0.5~2.0%; the ionic liquid functional additive is 1-butyl-3-methylimidazolium tetrafluoroborate or 1-hexyl-3-methylimidazolium hexafluorophosphate.

[0018] This invention also proposes a manufacturing process for highly sealed, heat-insulating, and energy-saving doors and windows, comprising the following steps:

[0019] S1 profile processing: Aluminum alloy is extruded into a five-cavity profile at an extrusion temperature of 480~520℃ and an extrusion speed of 5~8 m / min. After extrusion, the profile is quenched and stretched, then cut and milled to obtain profile components.

[0020] S2 Thermal Insulation Strip Installation and Cavity Filling: Install PA66 nylon thermal insulation strips on the profile assembly to form a thermal insulation cavity; inject polyurethane foam material into the second cavity, fourth cavity and thermal insulation cavity, and cure to obtain a five-cavity three-break bridge structure profile;

[0021] S3 sealing strip installation: Install the inflatable expansion sealing strip, soft and hard composite sealing strip, labyrinth sealing strip and low-pressure airbag sealing strip in the five-cavity three-break bridge structural profile respectively, and connect the inflation connector and miniature air valve to obtain the window frame profile and window sash profile.

[0022] S4 Insulating Glass Assembly Manufacturing: After cutting, grinding, cleaning and drying the glass, three layers of glass are stacked and assembled using stainless steel composite warm edge spacers to form an insulating layer between adjacent glass. Argon gas is then injected into the insulating layer, and the edges are sealed using a double-sealing process to obtain the insulating glass assembly.

[0023] S5 Assembly: Cut and assemble the window frame and sash profiles to form the window frame and sash, fix the insulated glass assembly inside the sash, install hardware, and inflate the inflatable expansion sealing strip and low-pressure airbag sealing strip to the predetermined pressure to obtain a highly sealed, heat-insulating, and energy-saving door and window.

[0024] Preferably, in step S3, the preparation method of the inflatable sealing strip, the soft-hard composite sealing strip, the labyrinth sealing strip, and the low-pressure airbag sealing strip includes the following steps:

[0025] S3-1: Maleic anhydride-grafted EPDM rubber and furfurylamine are mixed in an internal mixer at 60-80°C for 8-12 minutes to obtain furan-functionalized EPDM rubber.

[0026] S3-2: Cool furan-functionalized EPDM rubber to 60-90℃, add bismaleimide crosslinking agent, zinc methacrylate, core-shell structured nanofiller, modified graphene oxide, ionic liquid functional additives, and modified nano-lanthanum oxide particles, and mix for 8-12 minutes; cool to 50-60℃, add sulfur, accelerator CZ, zinc oxide, and stearic acid, and pass through a thin sheet 3-5 times to obtain unvulcanized compound;

[0027] S3-3: Uncured rubber compound is extruded at 120~140℃ into inflatable expansion sealing strips, soft-hard composite sealing strips, labyrinth sealing strips and low-pressure airbag sealing strips, and then continuously vulcanized in stages to obtain inflatable expansion sealing strips, soft-hard composite sealing strips, labyrinth sealing strips and low-pressure airbag sealing strips.

[0028] Preferably, in S3-3, the continuous segmented vulcanization process is as follows: hot air setting section, temperature 180~250℃, length 3m, time 18~22 s; microwave vulcanization section, microwave power 2.8 kW, temperature 220~250℃, length 10 m, time 60~75 s; hot air post-vulcanization section, temperature 220~260℃, length 9 m, time 54~67 s; cooling annealing section, temperature 50~70℃, length 6m, time 5~10 min.

[0029] In this invention's sealing system, the first (outdoor side) inflatable sealing strip and the fourth (indoor side) low-pressure airbag sealing strip form a dual-inflation dynamic compensation system. The pressure ratio between the two is set to 2-3:1. The first seal actively expands under high pressure to compensate for the gap between the frame and sash and aging shrinkage, while the fourth seal flexibly adheres under low pressure to ensure easy opening and closing and rapid retraction after deflation. The third labyrinthine sealing strip is located in the middle, with multi-stage folds in its cross-section, extending the path of permeating air and progressively throttling and dissipating kinetic energy of the leaking air, forming an intermediate pressure buffer zone.

[0030] The overall structure forms a gradient pressure reduction system of active compensation, mechanical throttling, and low-pressure assistance: when outdoor wind and rain intrude, they are first blocked by the first seal, and a small amount of infiltrated air is gradually depressurized through the labyrinth seal. The fourth seal forms the final airtight barrier on the indoor side, significantly reducing the pressure difference borne by each seal. In the four-seal structure, the first inflatable expansion seal strip is mainly on the outside, and the fourth low-pressure airbag seal strip is mainly on the inside, forming redundancy compensation; the labyrinth seal and double inflation work together to form pressure staged dissipation, avoiding a single seal bearing the entire pressure difference; the first seal can be replenished with air to restore its condition, and the fourth seal maintains the airtightness on the indoor side, thus actively extending the seal life.

[0031] In this invention, the inflatable sealing strip, the soft-hard composite sealing strip, the labyrinth sealing strip, and the low-pressure airbag sealing strip are all made of a dynamic dual-network modified EPDM rubber composition. The dynamic dual network is an interpenetrating dual-network structure constructed by Diels-Alder (DA) reversible covalent crosslinking bonds and ion cluster coordination crosslinking bonds. The DA reversible covalent crosslinking bonds are formed by the furan side groups on furan-functionalized EPDM rubber and the bismaleimide crosslinking agent through a [4+2] cycloaddition reaction. They are stable at room temperature, reversibly break above 120°C, and reform after cooling. When the sealing strip is subjected to alternating stress, the DA bonds break preferentially in the stress concentration area, dispersing the local stress to the surrounding molecular chains and preventing the initiation of microcracks. After the stress is released, the DA bonds reform, restoring the network integrity. This mechanism endows the material with thermally induced self-healing ability and stress relaxation ability, so that the local stress concentration generated during inflation can be dissipated through the reversible exchange of crosslinking bonds. The ionic cluster coordination crosslinking bonds consist of zinc ion-carboxylate ion clusters formed by zinc methacrylate with zinc oxide, stearic acid, and carboxyl groups generated from the ring opening of maleic anhydride in the system. These ion clusters are enriched into nanoscale ion cluster domains and serve as dynamic physical crosslinking points. During vulcanization, zinc ions preferentially form ion clusters with carboxylate groups. A small amount of zinc ions may participate in the activation of sulfur vulcanization, but this does not change the primary role of the ion clusters as dynamic physical crosslinking points. The ion clusters are stable at room temperature and can reversibly dissociate and recombine under stress.

[0032] When the DA bonds break, the ion clusters continue to bear the load as a second line of defense, preventing permanent deformation and insufficient springback caused by excessive relaxation of the network after the stress is completely unloaded. When the ion clusters dissociate, the DA bonds maintain the integrity of the network, and the material does not undergo macroscopic flow. The two types of dynamic cross-linking bonds complement each other, enabling the material to achieve both high elasticity and low permanent deformation.

[0033] The DA reaction is a thermally reversible reaction. Its forward reaction (crosslinking) proceeds spontaneously at lower temperatures (60–90 °C), while the reverse reaction (dissociation) occurs at higher temperatures (120–150 °C). At the vulcanization temperature, DA crosslinking is predominantly dissociative, and its forward crosslinking is inhibited. Therefore, sulfur vulcanization is preferentially completed, forming a permanent network. After vulcanization, as the system cools to room temperature, the furan side groups and maleimide groups re-approach within the free volume allowed by the sulfur crosslinking network and undergo partial DA recombination, forming an interpenetrating structure with sulfur crosslinking as the main network and reversible DA crosslinking and ionic cluster physical crosslinking as the dynamic network.

[0034] Meanwhile, the core-shell structured nanofiller in the composition provides mechanical reinforcement, while the shell improves compatibility with the EPDM rubber matrix and inhibits filler agglomeration. The interlayer slip effect of nano-tungsten disulfide reduces internal frictional heat generation during repeated deformation, improving fatigue life. The modified graphene oxide sheet structure effectively blocks ultraviolet light and ozone from penetrating into the rubber, and the interlayer slip effect helps to disperse stress, improving weather resistance and fatigue resistance. The ionic liquid functional additive acts as a lubricant between rubber molecular chains, reducing hysteresis and stress softening under alternating stress, allowing the material to maintain high resilience and fatigue resistance during repeated charge-discharge cycles. The rare earth elements in the modified nano-lanthanum oxide particles have a unique electronic structure that can effectively capture free radicals generated during aging and decompose hydrogen peroxide, delaying the thermo-oxidative aging process. Through the above composition design, the material simultaneously possesses excellent hydrolysis resistance, acid and alkali resistance, low-temperature flexibility, resilience, aging resistance, weather resistance, fatigue resistance, and airtightness.

[0035] In summary, the beneficial effects of the present invention are as follows:

[0036] 1. Excellent thermal insulation and energy-saving performance. The five-cavity structure plus three thermal break strips form a "five-cavity, three-thermal-bridge" structure, combined with polyurethane foam filling and triple-glazed Low-E glass, resulting in a window heat transfer coefficient as low as 0.72~0.77 W / (m²). 2 ·K).

[0037] 2. Excellent sealing performance and dynamic compensation capability. The four-seal structure, combined with the "dual inflation" dynamic compensation mechanism and labyrinth mechanical seal, forms a complete gradient pressure reduction sealing system. The first and fourth dual inflation seals provide redundant compensation, and the gradient configuration with a pressure ratio of 2 to 3:1 significantly reduces the pressure difference borne by each seal.

[0038] 3. Significantly improved sealing material performance. Dynamic dual-network modified EPDM rubber, through its interpenetrating network structure of reversible covalent bonds of DA and coordinated crosslinking bonds of ion clusters, combined with core-shell structured nanofillers, modified graphene oxide, and ionic liquid functional additives, achieves excellent comprehensive performance with compression set ≤11%, rebound recovery ≥90%, charge-discharge cycle life ≥100,000 cycles, and airtightness retention ≥95%.

[0039] 4. Extended service life. The inflatable sealing strip can dynamically compensate for sealing gaps caused by aging. The double-inflatable design of the first and fourth layers forms redundant compensation, extending the effective sealing life of the entire window.

[0040] 5. Excellent sound insulation performance. The triple-glazed windows, combined with a four-seal system, create multiple sound wave reflection and absorption interfaces, achieving a weighted sound insulation of 43 dB. Attached Figure Description

[0041] Figure 1 This is a horizontal cross-sectional assembly diagram of the high-sealing, heat-insulating, and energy-saving doors and windows of the present invention;

[0042] Figure 2 This is a partially enlarged schematic diagram of the four-seal structure for doors and windows of the present invention;

[0043] Figure 3 This is a partially enlarged view of the double-sealed edge of the door and window glass according to the present invention.

[0044] In the diagram: 1-Window frame; 2-Window sash; 3-Insulating glass assembly; 11-First cavity; 12-Second cavity; 13-Third cavity; 14-Fourth cavity; 15-Fifth cavity; 16-Polyurethane foam material; 17-PA66 nylon thermal insulation strip; 21-Inflatable expansion sealing strip; 22-Soft and hard composite sealing strip; 23-Labyrinth sealing strip; 24-Low-pressure airbag sealing strip; 31-Outdoor glass; 32-Intermediate glass; 33-Indoor glass; 34-First insulating layer; 35-Second insulating layer; 36-Stainless steel composite warm edge spacer; 37-Double seal. Detailed Implementation

[0045] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0046] Example 1 This example provides a high-sealing, heat-insulating, and energy-saving door and window, specifically a casement inward-opening window, the structure of which is shown in the attached diagram. Figures 1-3 The details are as follows:

[0047] Both the window frame 1 and the window sash 2 adopt a five-cavity, three-thermal-bridge profile structure, that is, five cavities are arranged sequentially from the outside to the inside: first cavity 11, second cavity 12, third cavity 13, fourth cavity 14, and fifth cavity 15; thermal insulation cavities for installing thermal insulation strips are provided between the profiles of the first cavity 11 and the second cavity 12, the second cavity 12 and the third cavity 13, and the third cavity 13 and the fourth cavity 14. PA66 nylon thermal insulation strips 17 are installed in the thermal insulation cavities, which are in the following order: an outdoor C-shaped thermal insulation strip, a central flat multi-cavity thermal insulation strip, and an indoor irregularly shaped multi-cavity thermal insulation strip, forming three thermal breaks; the second cavity 12, the fourth cavity 14, and the thermal insulation cavities are filled with B1 grade polyurethane foam material 16;

[0048] The window frame 1 is provided with a first sealing groove, a third sealing groove and a fourth sealing groove in sequence from the outside to the inside. The first sealing groove, the third sealing groove and the fourth sealing groove are respectively provided with an inflatable sealing strip 21, a labyrinth sealing strip 23 and a low-pressure airbag sealing strip 24.

[0049] The window sash 2 is provided with a second sealing groove, and a soft and hard composite sealing strip 22 is provided in the second sealing groove;

[0050] The window sash 2 is equipped with an insulated glass assembly 3, which is a triple-glazed Low-E glass structure: the insulated glass assembly includes an outdoor tempered glass 31, a middle tempered glass 32, and an indoor Low-E laminated safety glass 33. A first hollow layer 34 and a second hollow layer 35 are formed between the outdoor tempered glass 31, the middle tempered glass 32, and the indoor Low-E laminated safety glass 33; both the first hollow layer 34 and the second hollow layer 35 are filled with argon gas; the edges of the insulated glass assembly 3 are sealed with a stainless steel composite warm edge spacer 36 and a double seal 37.

[0051] In this embodiment, the first cavity 11 is 25 mm wide, the second cavity 12 is 15 mm wide, the third cavity 13 is 26 mm wide, the fourth cavity 14 is 15 mm wide, and the fifth cavity 15 is 25 mm wide, with a profile wall thickness of 2.0 mm; the PA66 nylon thermal insulation strip 17 consists of an outdoor C-shaped thermal insulation strip, a central flat multi-cavity thermal insulation strip, and an indoor irregular multi-cavity thermal insulation strip, all with a width of 6 mm;

[0052] The inflatable expansion sealing strip 21 has an inflation pressure of 0.25 MPa, and the low-pressure airbag sealing strip 24 has an inflation pressure of 0.10 MPa, with a pressure ratio of 2.5:1.

[0053] The outdoor tempered glass 31 is 5 mm tempered glass, the middle tempered glass 32 is 5 mm tempered glass, the indoor Low-E laminated safety glass 33 is two layers of 5 mm Low-E glass sandwiched with 0.76 mm PVB, the first hollow layer 34 is 14 mm wide, the second hollow layer 35 is 14 mm wide, and the hollow layer is filled with argon gas with a concentration of 94%.

[0054] Those skilled in the art should understand that the specific specifications of the above-mentioned parts (such as width, wall thickness, etc.) can be selected and adjusted according to relevant standards (GB / T 24498-2025, GB / T 8478, JG / T 174-2014, GB / T 11944-2025, etc.) and actual engineering needs.

[0055] Example 2 This example provides the manufacturing process of the above-mentioned high-sealing, heat-insulating, and energy-saving doors and windows. The specific steps are as follows:

[0056] S1 Profile Processing: Aluminum alloy is extruded into a five-cavity cross-section profile at an extrusion temperature of 500℃ and an extrusion speed of 6 m / min. After extrusion, the profile is quenched and stretched, then cut and milled to obtain the profile assembly. The specific implementation method of this step is existing technology.

[0057] S2 Thermal Insulation Strip Installation and Cavity Filling: Install PA66 nylon thermal insulation strips on the profile assembly to form a thermal insulation cavity; inject polyurethane foam material into the second cavity, fourth cavity and thermal insulation cavity, and cure for 36 hours to obtain a five-cavity three-break bridge structure profile.

[0058] S3 sealing strip installation: Install the inflatable expansion sealing strip, soft and hard composite sealing strip, labyrinth sealing strip and low-pressure airbag sealing strip in the five-cavity three-break bridge structural profile respectively, and connect the inflation connector and miniature air valve to obtain the window frame profile and window sash profile.

[0059] S4 Insulating Glass Assembly Manufacturing: After cutting, grinding, cleaning and drying the glass, three layers of glass are stacked and assembled using stainless steel composite warm edge spacers to form an insulated layer between adjacent glass. Argon gas is filled into the insulated layer, and a double-sealing process is used for edge sealing. The first layer is butyl rubber, and the second layer is polysulfide rubber, thus obtaining the insulating glass assembly.

[0060] S5 Assembly: Cut and assemble the window frame and sash profiles separately to form the window frame and sash. Fix the insulated glass assembly inside the sash, install the hardware, and inflate the inflatable expansion sealing strip and the low-pressure airbag sealing strip to the predetermined pressure (inflatable expansion sealing strip inflation pressure 0.25 MPa, low-pressure airbag sealing strip inflation pressure 0.10 MPa, pressure ratio 2.5:1) to obtain a highly sealed, heat-insulating, and energy-saving door and window.

[0061] In step S3, the formulation of the dynamically dual-network modified EPDM rubber composition comprises, by weight parts:

[0062] 100 parts of maleic anhydride-grafted EPDM rubber (grafting rate 1.0%, Mooney viscosity ML(1+4) 60 at 100℃), 6 parts of furfurylamine, 5 parts of bismaleimide crosslinking agent, 8 parts of zinc methacrylate, 20 parts of core-shell structured nanofiller (core particle size 50 nm, shell thickness 50 nm, nano tungsten disulfide particle size 25 nm), 5 parts of modified graphene oxide (sheet thickness 2 nm, sheet diameter 2 μm), 2 parts of ionic liquid functional additive (1-butyl-3-methylimidazolium tetrafluoroborate), 4 parts of modified nano lanthanum oxide particles (particle size 60 nm, modification layer thickness 6 nm), 2.2 parts of sulfur vulcanization system, 1.5 parts of accelerator CZ, 5 parts of zinc oxide, and 1.5 parts of stearic acid.

[0063] Preparation of core-shell structured nanofillers

[0064] Tetraethyl orthosilicate, anhydrous ethanol, deionized water, and ammonia were mixed in a volume ratio of 1:20:1:1 and stirred at 20°C for 6 hours. After centrifugation, the precipitate was washed three times with anhydrous ethanol and dried under vacuum at 60°C for 12 hours to obtain porous nano-silica cores. The porous nano-silica cores were redispersed in deionized water, and nano-tungsten disulfide and the organosiloxane precursor methyltrimethoxysilane were added, wherein the mass ratio of porous nano-silica cores, nano-tungsten disulfide, and methyltrimethoxysilane was 1:0.5:2. After ultrasonic dispersion at room temperature for 30 minutes, the mixture was stirred at 60°C for 4 hours, centrifuged, and the product was washed three times each with deionized water and anhydrous ethanol, and dried under vacuum at 80°C for 12 hours to obtain core-shell structured nanofillers.

[0065] Preparation of modified graphene oxide

[0066] Weigh out 118 parts of nano-graphene oxide, 12 parts of furfuryl alcohol, 9 parts of barium sulfate, and 6 parts of salicylic acid. Mix the nano-graphene oxide, furfuryl alcohol, and barium sulfate, and sonicate for 20 minutes. Then add salicylic acid and stir at room temperature for 55 minutes. After the reaction is complete, wash the product three times with deionized water and dry it under vacuum at 60°C for 24 hours to obtain modified graphene oxide.

[0067] Preparation of modified lanthanum oxide nanoparticles

[0068] Lanthanum carbonate was dissolved in deionized water to prepare a 0.1 mol / L solution, and sodium hydroxide was prepared to prepare a 0.2 mol / L solution. Under the conditions of a reaction temperature of 90℃ and a mass ratio of 1-hexyl-3-methylimidazolium hexafluorophosphate to lanthanum hydroxide of 2:3, the sodium hydroxide solution was slowly added dropwise to the lanthanum carbonate solution. The reaction was stirred until precipitation was complete, and the precipitate was separated by centrifugation. The precipitate was washed three times each with deionized water and anhydrous ethanol, dried at 100℃ for 12 hours, and then calcined at 720℃ for 1.5 hours to obtain modified nano-lanthanum oxide particles.

[0069] The preparation methods for inflatable expansion sealing strips, soft-hard composite sealing strips, labyrinth sealing strips, and low-pressure airbag sealing strips include the following steps:

[0070] S3-1: Maleic anhydride-grafted EPDM rubber and furfurylamine are mixed in a mixer at 70°C for 10 minutes to obtain furan-functionalized EPDM rubber.

[0071] S3-2: Cool furan-functionalized EPDM rubber to 75°C, add bismaleimide crosslinking agent, zinc methacrylate, core-shell structured nanofiller, modified graphene oxide, ionic liquid functional additives, and modified nano-lanthanum oxide particles, and mix for 10 minutes; cool to 55°C, add sulfur, accelerator CZ, zinc oxide, and stearic acid, pass through a thin filter 4 times, and sheet out to obtain unvulcanized compound;

[0072] S3-3: Uncured rubber compound was extruded at 130℃ into inflatable expansion sealing strips, soft-hard composite sealing strips, labyrinth sealing strips, and low-pressure airbag sealing strips, respectively. The process involved continuous segmented vulcanization: a hot air setting section (215℃, 3 m length, 20 s); a microwave vulcanization section (2.8 kW microwave power, 235℃, 10 m length, 67 s); a hot air post-vulcanization section (240℃, 9 m length, 60 s); and a cooling annealing section (60℃, 6 m length, 8 min). This process yielded inflatable expansion sealing strips, soft-hard composite sealing strips, labyrinth sealing strips, and low-pressure airbag sealing strips.

[0073] Example 3 This example provides the manufacturing process of the above-mentioned high-sealing, heat-insulating, and energy-saving doors and windows. The specific steps are as follows:

[0074] S1 Profile Processing: Aluminum alloy is extruded into a five-cavity cross-section profile at an extrusion temperature of 520℃ and an extrusion speed of 8 m / min. After extrusion, the profile is quenched and stretched, then cut and milled to obtain a profile assembly. The specific implementation method of this step is existing technology.

[0075] S2 Thermal Insulation Strip Installation and Cavity Filling: Install PA66 nylon thermal insulation strips on the profile assembly to form a thermal insulation cavity; inject polyurethane foam material into the second cavity, fourth cavity and thermal insulation cavity, and cure for 36 hours to obtain a five-cavity three-break bridge structure profile.

[0076] S3 sealing strip installation: Install the inflatable expansion sealing strip, soft and hard composite sealing strip, labyrinth sealing strip and low-pressure airbag sealing strip in the five-cavity three-break bridge structural profile respectively, and connect the inflation connector and miniature air valve to obtain the window frame profile and window sash profile.

[0077] S4 Insulating Glass Assembly Fabrication: After cutting, grinding, cleaning, and drying the glass, three layers of glass are stacked and assembled using stainless steel composite warm edge spacers to form an insulating layer between adjacent glass panes. Argon gas is then injected into the insulating layer, and a double-sealing process is used for edge sealing. The first layer is butyl rubber with a coating thickness of 2 mm and a width of 4 mm; the second layer is polysulfide rubber with a coating amount of 6 g / m per unit length along the glass edge, resulting in the insulating glass assembly.

[0078] S5 Assembly: Cut and assemble the window frame and sash profiles separately to form the window frame and sash. Fix the insulated glass assembly inside the sash, install the hardware, and inflate the inflatable expansion sealing strip and the low-pressure airbag sealing strip to the predetermined pressure (inflatable expansion sealing strip inflation pressure 0.30 MPa, low-pressure airbag sealing strip inflation pressure 0.15 MPa, pressure ratio 2:1) to obtain a highly sealed, heat-insulating, and energy-saving door and window.

[0079] In step S3, the formulation of the dynamically dual-network modified EPDM rubber composition comprises, by weight parts:

[0080] 100 parts of maleic anhydride-grafted EPDM rubber (grafting rate 2.0%, Mooney viscosity ML(1+4) 80 at 100℃), 10 parts of furfurylamine, 8 parts of bismaleimide crosslinking agent, 12 parts of zinc methacrylate, 25 parts of core-shell structured nanofiller (core particle size 80 nm, shell thickness 80 nm, nano tungsten disulfide particle size 40 nm), 8 parts of modified graphene oxide (sheet thickness 5 nm, sheet diameter 5 μm), 3 parts of ionic liquid functional additive (1-hexyl-3-methylimidazolium hexafluorophosphate), 6 parts of modified nano lanthanum oxide particles (particle size 100 nm, modification layer thickness 10 nm), 3 parts of sulfur, 2 parts of accelerator CZ, 8 parts of zinc oxide, and 2 parts of stearic acid.

[0081] Preparation of core-shell structured nanofillers

[0082] Tetraethyl orthosilicate, anhydrous ethanol, deionized water, and ammonia were mixed in a volume ratio of 1:15:1.5:1.5 and stirred at 30°C for 8 hours. After centrifugation, the precipitate was washed three times with anhydrous ethanol and dried under vacuum at 60°C for 12 hours to obtain porous nano-silica cores. The porous nano-silica cores were redispersed in deionized water, and nano-tungsten disulfide and the organosiloxane precursor methyltrimethoxysilane were added. The mass ratio of porous nano-silica cores, nano-tungsten disulfide, and methyltrimethoxysilane was 1:0.8:3. After ultrasonic dispersion at room temperature for 30 minutes, the mixture was stirred at 70°C for 6 hours and centrifuged. The product was washed three times each with deionized water and anhydrous ethanol, and dried under vacuum at 80°C for 12 hours to obtain core-shell structured nanofillers with a shell thickness of 20–80 nm.

[0083] Preparation of modified graphene oxide

[0084] Weigh out 135 parts of nano-graphene oxide, 13 parts of furfuryl alcohol, 11 parts of barium sulfate, and 8 parts of salicylic acid. Mix the nano-graphene oxide, furfuryl alcohol, and barium sulfate, and sonicate for 30 minutes. Then add salicylic acid and stir at room temperature for 65 minutes. After the reaction is complete, wash the product three times with deionized water and dry it under vacuum at 60°C for 24 hours to obtain modified graphene oxide.

[0085] Preparation of modified lanthanum oxide nanoparticles

[0086] Lanthanum carbonate was dissolved in deionized water to prepare a 0.15 mol / L solution, and sodium hydroxide was prepared to prepare a 0.3 mol / L solution. Under the conditions of a reaction temperature of 100℃ and a mass ratio of 1-hexyl-3-methylimidazolium hexafluorophosphate to lanthanum hydroxide of 1:1, the sodium hydroxide solution was slowly added dropwise to the lanthanum carbonate solution. The reaction was stirred until precipitation was complete, and the precipitate was separated by centrifugation. The precipitate was washed three times each with deionized water and anhydrous ethanol, dried at 120℃ for 10 hours, and then calcined at 800℃ for 2 hours to obtain modified nano-lanthanum oxide particles.

[0087] The preparation methods for inflatable expansion sealing strips, soft-hard composite sealing strips, labyrinth sealing strips, and low-pressure airbag sealing strips include the following steps:

[0088] S3-1: Maleic anhydride-grafted EPDM rubber and furfurylamine are mixed in a mixer at 80°C for 12 minutes to obtain furan-functionalized EPDM rubber.

[0089] S3-2: Cool furan-functionalized EPDM rubber to 90°C, add bismaleimide crosslinking agent, zinc methacrylate, core-shell structured nanofiller, modified graphene oxide, ionic liquid functional additives, and modified nano-lanthanum oxide particles, and mix for 12 minutes; cool to 60°C, add sulfur, accelerator CZ, zinc oxide, and stearic acid, pass through a thin filter 5 times, and sheet out to obtain unvulcanized compound;

[0090] S3-3: Uncured rubber compound is extruded at 140℃ into inflatable expansion sealing strips, soft-hard composite sealing strips, labyrinth sealing strips, and low-pressure airbag sealing strips, respectively. The mixture is then continuously vulcanized in stages, passing through a hot air setting stage (250℃, 3 m length, 18 s); a microwave vulcanization stage (2.8 kW microwave power, 250℃, 10 m length, 75 s); a hot air post-vulcanization stage (260℃, 9 m length, 67 s); and a cooling annealing stage (70℃, 6 m length, 10 min). This process yields inflatable expansion sealing strips, soft-hard composite sealing strips, labyrinth sealing strips, and low-pressure airbag sealing strips.

[0091] Example 4 This example provides the manufacturing process of the above-mentioned high-sealing, heat-insulating, and energy-saving doors and windows. The specific steps are as follows:

[0092] S1 Profile Processing: Aluminum alloy is extruded into a five-cavity profile at an extrusion temperature of 480℃ and an extrusion speed of 5 m / min. After extrusion, the profile is quenched and stretched, then cut and milled to obtain the profile assembly. The specific implementation method of this step is existing technology.

[0093] S2 Thermal Insulation Strip Installation and Cavity Filling: Install PA66 nylon thermal insulation strips on the profile assembly to form a thermal insulation cavity; inject polyurethane foam material into the second cavity, fourth cavity and thermal insulation cavity, and cure for 36 hours to obtain a five-cavity three-break bridge structure profile.

[0094] S3 sealing strip installation: Install the inflatable expansion sealing strip, soft and hard composite sealing strip, labyrinth sealing strip and low-pressure airbag sealing strip in the five-cavity three-break bridge structural profile respectively, and connect the inflation connector and miniature air valve to obtain the window frame profile and window sash profile.

[0095] S4 Insulating Glass Assembly Fabrication: After cutting, grinding, cleaning, and drying the glass, three layers of glass are stacked and assembled using stainless steel composite warm edge spacers to form an insulating layer between adjacent glass panes. Argon gas is then injected into the insulating layer, and a double-sealing process is used for edge sealing. The first layer is butyl rubber with a coating thickness of 2 mm and a width of 4 mm; the second layer is polysulfide rubber with a coating amount of 6 g / m per unit length along the glass edge, resulting in the insulating glass assembly.

[0096] S5 Assembly: Cut and assemble the window frame and sash profiles separately to form the window frame and sash. Fix the insulated glass assembly inside the sash, install the hardware, and inflate the inflatable expansion sealing strip and the low-pressure airbag sealing strip to the predetermined pressure (inflatable expansion sealing strip inflation pressure 0.15 MPa, low-pressure airbag sealing strip inflation pressure 0.05 MPa, pressure ratio 3:1) to obtain a highly sealed, heat-insulating, and energy-saving door and window.

[0097] In step S3, the formulation of the dynamically dual-network modified EPDM rubber composition comprises, by weight parts:

[0098] 100 parts of maleic anhydride-grafted EPDM rubber (grafting rate 0.5%, Mooney viscosity ML(1+4) 40 at 100℃), 3 parts of furfurylamine, 2 parts of bismaleimide crosslinking agent, 5 parts of zinc methacrylate, 15 parts of core-shell structured nanofiller (core particle size 20 nm, shell thickness 20 nm, nano tungsten disulfide particle size 10 nm), 2 parts of modified graphene oxide (sheet thickness 1 nm, sheet diameter 0.5 μm), 1 part of ionic liquid functional additive (1-butyl-3-methylimidazolium tetrafluoroborate), 3 parts of modified nano lanthanum oxide particles (particle size 20 nm, modification layer thickness 2 nm), 1.5 parts of sulfur, 1 part of accelerator CZ, 3 parts of zinc oxide, and 1 part of stearic acid.

[0099] Preparation of core-shell structured nanofillers

[0100] Tetraethyl orthosilicate, anhydrous ethanol, deionized water, and ammonia were mixed in a volume ratio of 1:25:0.8:0.8 and reacted at 15°C for 4 hours. After centrifugation, the precipitate was washed three times with anhydrous ethanol and dried under vacuum at 60°C for 12 hours to obtain porous nano-silica cores. The porous nano-silica cores were redispersed in deionized water, and nano-tungsten disulfide and the organosiloxane precursor methyltrimethoxysilane were added. The mass ratio of porous nano-silica cores, nano-tungsten disulfide, and methyltrimethoxysilane was 1:0.3:1.5. After ultrasonic dispersion at room temperature for 30 minutes, the mixture was stirred at 50°C for 3 hours and centrifuged. The product was washed three times each with deionized water and anhydrous ethanol, and dried under vacuum at 80°C for 12 hours to obtain core-shell structured nanofillers with a shell thickness of 20–80 nm.

[0101] Preparation of modified graphene oxide

[0102] Weigh out 102 parts of nano-graphene oxide, 11 parts of furfuryl alcohol, 7 parts of barium sulfate, and 5 parts of salicylic acid. Mix the nano-graphene oxide, furfuryl alcohol, and barium sulfate, and sonicate for 15 minutes. Then add salicylic acid and stir at room temperature for 45 minutes. After the reaction is complete, wash the product three times with deionized water and dry it under vacuum at 60°C for 24 hours to obtain modified graphene oxide.

[0103] Preparation of modified lanthanum oxide nanoparticles

[0104] Lanthanum carbonate was dissolved in deionized water to prepare a 0.05 mol / L solution, and sodium hydroxide was prepared to prepare a 0.1 mol / L solution. Under the conditions of a reaction temperature of 80℃ and a mass ratio of 1-hexyl-3-methylimidazolium hexafluorophosphate to lanthanum hydroxide of 1:2, the sodium hydroxide solution was slowly added dropwise to the lanthanum carbonate solution. The reaction was stirred until precipitation was complete, and the precipitate was separated by centrifugation. The precipitate was washed three times each with deionized water and anhydrous ethanol, dried at 80℃ for 16 hours, and then calcined at 600℃ for 1 hour to obtain modified nano-lanthanum oxide particles.

[0105] The preparation methods for inflatable expansion sealing strips, soft-hard composite sealing strips, labyrinth sealing strips, and low-pressure airbag sealing strips include the following steps:

[0106] S3-1: Maleic anhydride-grafted EPDM rubber and furfurylamine are mixed in a mixer at 60°C for 8 minutes to obtain furan-functionalized EPDM rubber.

[0107] S3-2: Cool furan-functionalized EPDM rubber to 60°C, add bismaleimide crosslinking agent, zinc methacrylate, core-shell structured nanofiller, modified graphene oxide, ionic liquid functional additives, and nano-modified lanthanum oxide particles, and mix for 8 minutes; cool to 50°C, add sulfur, accelerator CZ, zinc oxide, and stearic acid, pass through a thin filter 3 times, and sheet out to obtain unvulcanized compound;

[0108] S3-3: Uncured rubber compound is extruded at 120℃ into inflatable expansion sealing strips, soft-hard composite sealing strips, labyrinth sealing strips, and low-pressure airbag sealing strips, respectively. The mixture is then continuously vulcanized in stages, passing through a hot air setting stage (180℃, 3 m length, 22 s); a microwave vulcanization stage (2.8 kW microwave power, 220℃, 10 m length, 60 s); a hot air post-vulcanization stage (220℃, 9 m length, 54 s); and a cooling annealing stage (50℃, 6 m length, 5 min), resulting in inflatable expansion sealing strips, soft-hard composite sealing strips, labyrinth sealing strips, and low-pressure airbag sealing strips.

[0109] Comparative Example 1: The difference between this comparative example and Example 2 is that zinc methacrylate is not added to the dynamic dual-network modified EPDM rubber composition in this comparative example.

[0110] Comparative Example 2: The difference between this comparative example and Example 2 is that the dynamic dual-network modified EPDM rubber composition in this comparative example does not contain furfurylamine and bismaleimide crosslinking agents.

[0111] Comparative Example 3 differs from Example 2 in that the dynamic dual-network modified EPDM rubber composition in this comparative example does not contain furfurylamine, bismaleimide crosslinking agent, zinc methacrylate, core-shell structured nanofiller, modified graphene oxide, ionic liquid functional additive, or modified nano-lanthanum oxide particles. The composition is 100 parts maleic anhydride-grafted EPDM rubber, 2.2 parts sulfur, 1.5 parts accelerator CZ, 5 parts zinc oxide, and 1.5 parts stearic acid.

[0112] Comparative Example 4: The difference between this comparative example and Example 2 is that the inflatable expansion sealing strip, soft-hard composite sealing strip, labyrinth sealing strip, and low-pressure airbag sealing strip in this comparative example are prepared by mixing the modified EPDM rubber obtained by steps S3-1 to S3-2 of the dynamic dual-network modified EPDM rubber composition of Comparative Example 1 and the dynamic dual-network modified EPDM rubber composition of Comparative Example 2 at a mass ratio of 1:1 at 60°C for 10 minutes, and then proceeding to step S3-3.

[0113] Comparative Example 5: The difference between this comparative example and Example 2 is that the inflation pressure of the first and fourth sealing strips in this comparative example is 0.15 MPa, and the pressure ratio is 1:1.

[0114] Comparative Example 6: The difference between this comparative example and Example 2 is that this comparative example does not have a third labyrinth seal.

[0115] Comparative Example 7: The difference between this comparative example and Example 2 is that the profile in this comparative example adopts a conventional three-cavity structure, with two PA66 nylon thermal insulation strips (C-shaped thermal insulation strips) installed between the profiles, and no polyurethane foam material is filled in the cavities.

[0116] Performance testing

[0117] The sealing strip performance was tested on the sealing strip samples prepared in Examples 2-4 and Comparative Examples 1-4. The test methods are as follows:

[0118] Tensile strength and elongation at break: Tested according to GB / T 528-2009. Dumbbell-shaped specimens were used, the tensile speed was 500 mm / min, and the test temperature was 23±2℃. Tensile strength (MPa) and elongation at break (%) were recorded. Five specimens were tested in each group, and the arithmetic mean was taken.

[0119] Compression set: Tested according to GB / T 7759.1-2017. Test conditions: 70℃ × 22 h, compression rate 25%. Compression set is calculated using the following formula:

[0120] Compression permanent deformation rate = (h0 - h1) / (h0 - h2) × 100%;

[0121] In the formula: h0 is the initial height of the sample; h1 is the height of the sample after recovery; h2 is the height of the limiter. Three samples are tested in each group, and the arithmetic mean is taken.

[0122] Rebound rate: The test was conducted according to the test apparatus and procedures specified in GB / T 1683-2018. A standard cylindrical specimen (Φ29±0.5 mm × 12.5±0.5 mm) was used and equilibrated for at least 24 hours at 23±2℃ / 50±5% RH. The specimen was placed between two parallel compression plates and compressed to 25% compression using a restrainer, then held at 70℃ for 22 hours. After releasing the compression, the specimen was allowed to recover at standard laboratory temperature for 30 minutes, and the height h1 of the recovered specimen was measured. The rebound rate was calculated using the following formula:

[0123] Springback recovery rate = h1 / h0 × 100%;

[0124] In the formula: h0 is the initial height of the sample; h1 is the height of the sample after releasing the compression and recovering for 30 minutes. Three samples are tested in each group, and the arithmetic mean is taken.

[0125] Inflation / deflation cycle life: The inflatable expansion sealing strip and low-pressure airbag sealing strip samples were installed in a fixture simulating the gap between the frame and the sash. The pressure was inflated to 0.3 MPa and held for 30 s, then deflated to 0 MPa and held for 30 s. This constitutes one cycle. The number of cycles when the sample expansion decayed by more than 20% of the initial value was recorded. The test frequency was 10 cycles / min.

[0126] Air tightness retention rate: A self-made air tightness testing device was used for testing. The inflatable expansion sealing strip and low-pressure airbag sealing strip samples were inflated to 0.15 MPa and placed at 23±2℃ for 90 days. Pressure changes were measured, and the air tightness retention rate was calculated.

[0127] Air tightness retention rate = P 90 / P0 × 100%;

[0128] In the formula: P0 is the initial pressure; P 90 The pressure after 90 days. Three samples were tested in each group, and the arithmetic mean was taken.

[0129] The test data above are shown in Table 1.

[0130] Table 1. Performance test results of sealing strips

[0131]

[0132] The compression set of Comparative Example 1 was 15.8%, and that of Comparative Example 2 was 18.3%. If the two are simply superimposed, the expected value for a 1:1 weighted average by volume fraction is approximately 17.05%. The measured value of Comparative Example 4 was 17.2%, consistent with the expected weighted average, indicating that physical blending did not produce a synergistic effect. However, the compression set of Example 2 was 8.5%, significantly lower than the 17.2% of the physical blend system, a reduction of 50.6%, indicating a nonlinear synergistic gain effect between the DA reversible covalent bonds and the ionic cluster coordination bonds.

[0133] Example 2 achieved a charge-discharge cycle life of 125,000 cycles, which is 5 times that of Comparative Example 3 and 2.1 times that of Comparative Example 4. This indicates that the interpenetrating double network structure, through the synergistic stress dissipation of DA bonds and ion clusters, enables the sealing strip to maintain high resilience and low compression set during repeated charge-discharge cycles, significantly extending the effective service life of the sealing strip.

[0134] The airtightness retention rate of Example 2 was 96.5%, significantly higher than that of Comparative Example 4 (86.0%) and Comparative Example 3 (78.0%). The interpenetrating double network structure ensures that the sealing strip maintains high elasticity and low permanent deformation under long-term compression, and the inner wall of the airbag and the frame always maintain a tight fit, effectively reducing the permeability of the inflation medium.

[0135] The performance of the doors and windows was tested on the samples from Examples 2-4 and Comparative Examples 3, 5-7. The test methods are as follows:

[0136] Heat transfer coefficient: Tested according to GB / T 8484-2020. The calibration chamber method was used, with test conditions of indoor temperature 20℃, outdoor temperature -20℃, and window opening size of 1500 mm × 1500 mm. The heat transfer coefficient U-value (W / (m³)) of the entire window was recorded. 2 ·K)).

[0137] Air tightness: Tested according to GB / T 7106-2019. Under a pressure difference of ±300 Pa, the air permeation rate q1 (m) per unit seam length was measured. 3 / (m·h)) and air permeability per unit area q2 (m 3 / (m 2 ·h), determine the airtightness level.

[0138] Water tightness: Tested according to GB / T 7106-2019. The steady pressurization method is used, and the pressure is gradually increased until leakage occurs. The highest pressure value (Pa) without leakage is recorded to determine the water tightness level.

[0139] Sound insulation performance: Tested according to GB / T 8485-2008. The reverberation chamber method was used to measure the weighted sound insulation Rw (dB) and the traffic noise spectral correction Ctr (dB).

[0140] Expansion attenuation rate after inflation and deflation: Install doors and windows in a standard test opening, and perform 200 inflation-deflation cycles (0→0.3 MPa→0) on the inflatable sealing strip. Measure the expansion of the sealing strip before and after each cycle and calculate the attenuation rate.

[0141] Expansion decay rate = (L0 - L) 200 ) / L0 × 100%;

[0142] In the formula: L0 is the initial expansion amount; L 200 This represents the expansion amount after 200 cycles.

[0143] The test data above are shown in Table 2.

[0144] Table 2. Results of Door and Window Performance Tests

[0145]

[0146] Comparative Example 3 used a conventional EPDM rubber sealing strip with an air tightness rating of 6, a water tightness rating of 580 Pa, and a sound insulation rating of 38 dB, all of which were significantly lower than the ratings of Example 2 (8, 750 Pa, and 43 dB), indicating that the dynamic dual-network sealing strip makes a key contribution to the overall window sealing performance.

[0147] In Comparative Example 5, the inflation pressure of the first and fourth sealing strips was 0.15 MPa, which did not constitute a gradient pressure configuration. The air tightness was grade 7 and the water tightness was 650 Pa, both lower than those in Example 2. This indicates that in the dual-inflation dynamic compensation mechanism, the gradient configuration with a pressure ratio of 2 to 3:1 allows the first sealing strip to actively expand and compensate for the gap between the frame and the sash. The fourth sealing strip maintains flexible fit and rapid retraction under low pressure. The two form a pressure gradient in space, which significantly reduces the pressure difference borne by each seal, thereby extending the service life of the overall sealing system.

[0148] Comparative Example 6 eliminated the third labyrinth-type sealing strip, retaining only a three-layer sealing structure. Its air tightness was grade 7, and its water tightness was 670 Pa, both lower than Example 2. This indicates that the multi-stage folding channels of the labyrinth-type sealing strip dissipate the kinetic energy of the permeating air step by step, effectively extending the air permeation distance. It has a significant throttling effect in the gradient pressure reduction sealing system, and together with the double-inflated sealing strip, forms a complete gradient pressure reduction sealing system.

[0149] The expansion decay rate of Comparative Example 3 after 200 inflation and deflation cycles was 16.5%, while that of Example 2 was only 2.8%. This demonstrates that the dynamically modified EPDM rubber sealing strip exhibits excellent fatigue resistance and shape recovery ability during repeated inflation and deflation cycles, effectively extending the service life of the sealing system.

[0150] Comparative Example 7, employing a three-cavity, two-broken-bridge profile structure without polyurethane foam filling, has a heat transfer coefficient U of 1.05 W / (m²). 2 ·K), higher than 0.74 W / (m²) in Example 2. 2 ·K). This indicates that the five-cavity, three-break bridge + polyurethane foam filling structure forms a complete gradient insulation system. The multi-cavity structure effectively extends the heat transfer path and increases the thermal resistance of the profile cross-section by increasing the number of air gaps. The polyurethane foam material not only has a low thermal conductivity, but also effectively inhibits the natural convection of air in the insulation cavity, further reducing the equivalent thermal conductivity. The heat transfer path is blocked step by step by multiple insulation strips and foam materials.

[0151] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art should be able to make corresponding changes and modifications according to the present invention, but these corresponding changes and modifications should all fall within the protection scope of the appended claims.

Claims

1. A high-sealing, heat-insulating, and energy-saving door and window, comprising a window frame, a window sash, and an insulated glass assembly installed within the window sash, characterized in that: Both the window frame and the window sash adopt a five-cavity, three-thermal-break profile structure. The window frame is provided with a first sealing groove, a third sealing groove and a fourth sealing groove in sequence from the outside to the inside. The first sealing groove, the third sealing groove and the fourth sealing groove are respectively provided with an inflatable sealing strip, a labyrinth sealing strip and a low-pressure airbag sealing strip. The window sash is provided with a second sealing groove, and a soft and hard composite sealing strip is provided in the second sealing groove; The inflatable sealing strip, soft-hard composite sealing strip, labyrinth sealing strip, and low-pressure airbag sealing strip are made of a dynamic dual-network modified EPDM rubber composition.

2. The high-sealing, heat-insulating, and energy-saving door and window according to claim 1, characterized in that, The dynamically modified dual-network EPDM rubber composition comprises, by weight: 100 parts maleic anhydride-grafted EPDM rubber, 3-10 parts furfurylamine, 2-8 parts bismaleimide crosslinking agent, 5-12 parts zinc methacrylate, 15-25 parts core-shell structured nanofiller, 2-8 parts modified graphene oxide, 1-3 parts ionic liquid functional additive, 3-6 parts modified nano lanthanum oxide particles, 1.5-3 parts sulfur, 1-2 parts accelerator CZ, 3-8 parts zinc oxide, and 1-2 parts stearic acid.

3. The high-sealing, heat-insulating, and energy-saving door and window according to claim 1, characterized in that, The inflatable sealing strip has an inflatable cavity extending along its length, which is connected to the outside through a micro air valve. The inflation pressure is 0.15~0.30MPa. The ratio of the inflation pressure of the inflatable sealing strip to that of the low-pressure airbag sealing strip is 2~3:

1.

4. The high-sealing, heat-insulating, and energy-saving door and window according to claim 1, characterized in that, The hollow glass assembly is a three-layer hollow Low-E glass structure, with a hollow layer formed between adjacent glass panes, and the hollow layer is filled with argon gas.

5. The high-sealing, heat-insulating, and energy-saving door and window according to claim 1, characterized in that, The five-cavity, three-thermal-bridge profile structure includes a first cavity, a second cavity, a third cavity, a fourth cavity, and a fifth cavity arranged sequentially from the outside to the inside. Thermal insulation cavities for installing thermal insulation strips are provided between the first cavity and the second cavity, the second cavity and the third cavity, and the third cavity and the fourth cavity profile. PA66 nylon thermal insulation strips are installed within each thermal insulation cavity, consisting of an outdoor C-shaped thermal insulation strip, a central flat multi-cavity thermal insulation strip, and an indoor irregularly shaped multi-cavity thermal insulation strip, forming three thermal breaks. The second cavity, the fourth cavity, and the thermal insulation cavity are also filled with B1-grade polyurethane foam material.

6. The high-sealing, heat-insulating, and energy-saving door and window according to claim 1, characterized in that, In the dynamic dual-network modified EPDM rubber composition, the core-shell structured nanofiller is a composite material with porous nano-silica as the core, an organosiloxane network, and embedded nano-tungsten disulfide as the shell; the modified graphene oxide is graphene oxide modified with furfuryl alcohol, barium sulfate, and salicylic acid, with a sheet thickness of 1~5 nm and a sheet diameter of 0.5~5 μm; the modified nano-lanthanum oxide particles have nano-lanthanum oxide as the core, and the surface of the nano-lanthanum oxide is modified with an ionic liquid to form a modification layer with a thickness of 2~10 nm, the ionic liquid being 1-hexyl-3-methylimidazolium hexafluorophosphate, and the particle size of the modified nano-lanthanum oxide particles being 20~100 nm.

7. The high-sealing, heat-insulating, and energy-saving door and window according to claim 1, characterized in that, In the dynamic dual-network modified EPDM rubber composition, the maleic anhydride-grafted EPDM rubber has a Mooney viscosity ML(1+4) of 40~80 at 100℃ and a grafting rate of 0.5~2.0%; the ionic liquid functional additive is 1-butyl-3-methylimidazolium tetrafluoroborate or 1-hexyl-3-methylimidazolium hexafluorophosphate.

8. A manufacturing process for high-sealing, heat-insulating, and energy-saving doors and windows as described in any one of claims 1 to 7, characterized in that, Includes the following steps: S1 profile processing: Aluminum alloy is extruded into a five-cavity profile at an extrusion temperature of 480~520℃ and an extrusion speed of 5~8 m / min. After extrusion, the profile is quenched and stretched, then cut and milled to obtain profile components. S2 Thermal Insulation Strip Installation and Cavity Filling: Install PA66 nylon thermal insulation strips on the profile assembly to form a thermal insulation cavity; inject polyurethane foam material into the second cavity, fourth cavity and thermal insulation cavity, and cure to obtain a five-cavity three-break bridge structure profile; S3 sealing strip installation: Install the inflatable expansion sealing strip, soft and hard composite sealing strip, labyrinth sealing strip and low-pressure airbag sealing strip in the five-cavity three-break bridge structural profile respectively, and connect the inflation connector and miniature air valve to obtain the window frame profile and window sash profile. S4 Insulating Glass Assembly Manufacturing: After cutting, grinding, cleaning and drying the glass, three layers of glass are stacked and assembled using stainless steel composite warm edge spacers to form an insulating layer between adjacent glass. Argon gas is then injected into the insulating layer, and the edges are sealed using a double-sealing process to obtain the insulating glass assembly. S5 Assembly: Cut and assemble the window frame and sash profiles to form the window frame and sash, fix the insulated glass assembly inside the sash, install hardware, and inflate the inflatable expansion sealing strip and low-pressure airbag sealing strip to the predetermined pressure to obtain a highly sealed, heat-insulating, and energy-saving door and window.

9. The manufacturing process of high-sealing, heat-insulating, and energy-saving doors and windows according to claim 8, characterized in that, In step S3, the preparation methods for the inflatable sealing strip, the soft-hard composite sealing strip, the labyrinth sealing strip, and the low-pressure airbag sealing strip include the following steps: S3-1: Maleic anhydride-grafted EPDM rubber and furfurylamine are mixed in an internal mixer at 60-80°C for 8-12 minutes to obtain furan-functionalized EPDM rubber. S3-2: Cool furan-functionalized EPDM rubber to 60-90℃, add bismaleimide crosslinking agent, zinc methacrylate, core-shell structured nanofiller, modified graphene oxide, ionic liquid functional additives, and modified nano-lanthanum oxide particles, and mix for 8-12 minutes; cool to 50-60℃, add sulfur, accelerator CZ, zinc oxide, and stearic acid, and pass through a thin sheet 3-5 times to obtain unvulcanized compound; S3-3: Uncured rubber compound is extruded at 120~140℃ into inflatable expansion sealing strips, soft-hard composite sealing strips, labyrinth sealing strips and low-pressure airbag sealing strips, and then continuously vulcanized in stages to obtain inflatable expansion sealing strips, soft-hard composite sealing strips, labyrinth sealing strips and low-pressure airbag sealing strips.

10. The manufacturing process of high-sealing, heat-insulating, and energy-saving doors and windows according to claim 9, characterized in that, In S3-3, the continuous segmented vulcanization process is as follows: hot air setting section, temperature 180~250℃, length 3 m, time 18~22 s; microwave vulcanization section, microwave power 2.8 kW, temperature 220~250℃, length 10 m, time 60~75 s; hot air post-vulcanization section, temperature 220~260℃, length 9 m, time 54~67 s; Cooling annealing section, temperature 50~70℃, length 6 m, time 5~10 min.

Citation Information

Patent Citations

  • Four sealed plastic profile shapes door and window

    CN207553922U