A method for preparing an aqueous metal tracer

The water-based metal tracer prepared by the hydrothermal method utilizes the spherical structure formed by the copolymer of acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid and metal salt to solve the problem of aggregation and adsorption of water-soluble tracers in high-salinity oil reservoirs, and realizes the application of tracers with high efficiency and low cost.

CN123109644APending Publication Date: 2026-11-17CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510628517.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing water-soluble tracers tend to aggregate and be adsorbed in high-salinity oil reservoirs, failing to meet the exploitation needs of high-salinity oil fields.

Method used

Aqueous metal tracers were prepared by using copolymers, binders and metal salts in a hydrothermal reaction. By introducing acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid copolymers and metal salts, spheres containing metal elements in the core were formed, and AMPS functional groups were combined to improve salt resistance.

Benefits of technology

The prepared aqueous metal tracer is not easily agglomerated or adsorbed under high salinity conditions, has high detection accuracy, low cost, and is suitable for mass spectrometry or spectrometry detection. It is also suitable for fracturing and exploitation of harsh oil reservoirs with high salinity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123109644A_ABST
    Figure CN123109644A_ABST
Patent Text Reader

Abstract

This invention provides a method for preparing an aqueous metal tracer, belonging to the field of oilfield development additives technology. The method includes the following steps: dissolving a copolymer, a binder, and a metal salt in a solvent to obtain a mixed solution; the copolymer is mainly composed of acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid; the binder contains hydroxyl and / or amino groups, wherein the total number of hydroxyl and amino functional groups is more than two; subjecting the mixed solution to a hydrothermal reaction at 160–200°C, followed by dialysis and freeze-drying to obtain the aqueous metal tracer. This invention significantly improves the tracer's tolerance to high salinity, making it suitable for harsh, high-salinity underground conditions. It provides a novel preparation route and strategy for high-salinity resistant tracers and has extremely broad application prospects in fracturing and exploitation of harsh, high-salinity oil reservoirs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of oilfield development additives technology, specifically relating to a method for preparing an aqueous metal tracer. Background Technology

[0002] In the petroleum industry, fracturing is the artificial creation of fractures in the formation to improve the underground flow environment of oil, thereby increasing well production. It plays a crucial role in improving bottomhole flow conditions, mitigating inter-layer flow, and enhancing reservoir activity. Oilfield tracers are substances that enter the reservoir along with the injected fluid during fracturing. By analyzing their content, the fluid's trajectory can be tracked, and its flow patterns within the reservoir can be determined. This allows for understanding reservoir properties and parameters, facilitating better evaluation of development effectiveness and optimization of treatment strategies.

[0003] Existing water-soluble tracers used in reservoir fracturing mainly include rare earth element complexes, fluorescent substances, and fluorobenzoic acid derivatives. They have good stability and compatibility with injected fluids, but they still have the following shortcomings in application: Existing tracers are often expensive, especially with limited tolerance to harsh reservoir conditions with high salinity. When applied to high salinity (salinity > 100,000 mg / L) reservoirs, tracers are prone to agglomeration and precipitation, thus losing their tracer function and failing to meet the needs of high salinity oilfield development.

[0004] Therefore, there is an urgent need to develop tracers that are low-cost and have high salinity tolerance to meet the demanding requirements of fracturing in oil reservoirs with high salinity. Summary of the Invention

[0005] The purpose of this invention is to provide a method for preparing an aqueous metal tracer, so as to solve the problem that aqueous metal tracers in the prior art are prone to agglomeration and adsorption, and cannot tolerate high mineralization.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing an aqueous metal tracer includes the following steps:

[0008] A mixed solution is obtained by dissolving the copolymer, the binder, and the metal salt in a solvent. The copolymer is mainly composed of acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid. The binder contains hydroxyl and / or amino groups, wherein the total number of hydroxyl and amino functional groups is more than two.

[0009] The mixed solution was subjected to a hydrothermal reaction at a temperature of 160–200°C, and the aqueous metal tracer was obtained by dialysis and freeze-drying.

[0010] This invention is a pioneering invention. The beneficial effects of the above technical solution are as follows: (1) The water-based metal tracer of this invention is obtained by reacting a copolymer containing acrylic acid (AA) and 2-acrylamide-2-methylpropanesulfonic acid (AMPS), a linker and a metal salt. The copolymer contains carboxyl groups. Some of the carboxyl groups and the linker undergo dehydration condensation at high temperature, and some of the carboxyl groups combine with metal ions to form spheres containing metal elements in the core. At the same time, the AMPS functional group contained in the copolymer gives the carbon sphere structure good resistance to high mineralization. The tracer of this invention is not easy to agglomerate, is not easy to be adsorbed, and has high tolerance to mineralization, and can withstand mineralization of 200,000 mg / L; (2) The raw materials for preparation of this invention (3) The tracer of the present invention can overcome the inability of traditional carbon dot tracers to withstand the high mineralization of the formation, and will not lose stability due to flocculation and agglomeration, and will not affect the detection accuracy; (4) The carbon ball tracer is prepared by hydrothermal method, which has the characteristics of being non-toxic and harmless, and has good compatibility with the injected fluid; (5) The tracer of the present invention is easy to detect with mass spectrometer or spectrometer, and can detect all metal elements at one time, with a detection limit of ppb level, and low detection cost; (6) The present invention can provide a novel preparation route and strategy for tracers resistant to high mineralization, and the tracer of the present invention has extremely broad application prospects in the fracturing and exploitation of harsh oil reservoirs with high mineralization.

[0011] Preferably, the copolymer is an acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer. The abbreviation for acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer is AA-AMPS. It contains carboxyl groups and AMPS groups. Introducing copolymers containing carboxyl groups and AMPS groups into the tracer synthesis can effectively improve the tracer's salt resistance.

[0012] Preferably, the linker is one or more selected from ethylenediamine, ethylene glycol, glycerol, and ethanolamine. The linker contains two hydroxyl groups and / or amino groups, enabling it to undergo dehydration and meet the requirements of hydrothermal reactions.

[0013] Preferably, the metal salt is one or more of the following: cerium salt, copper salt, zinc salt, strontium salt, zirconium salt, gallium salt, niobium salt, tin salt, lead salt, hafnium salt, cadmium salt, antimony salt, tantalum salt, indium salt, bismuth salt, lanthanum salt, praseodymium salt, neodymium salt, promethium salt, samarium salt, europium salt, gadolinium salt, terbium salt, dysprosium salt, holmium salt, erbium salt, thulium salt, ytterbium salt, lutetium salt, scandium salt, and yttrium salt. Before fracturing, technicians can conventionally select metal elements with low background concentrations and the ability to bind with carboxyl groups by analyzing groundwater samples. By introducing metal elements as composite tracers during the hydrothermal process, both temperature and oxidation resistance are retained, and the diverse selectivity of metal ions allows for the serialization of tracer varieties, resulting in tracers with different metal ions.

[0014] Preferably, the ratio of the copolymer, the binder and the metal salt is (100-150) g ​​: (0.2-0.6) mol : (0.01-0.15) mol.

[0015] More preferably, the solvent is water, and the concentration of the copolymer in the mixed solution is (100-150) g / L.

[0016] More preferably, the ratio of the copolymer, the binder and the metal salt is (120-130) g : (0.4-0.6) mol : (0.04-0.07) mol.

[0017] Preferably, the hydrothermal reaction time is 5-6 hours. Technicians can conventionally select a suitable hydrothermal reactor for the reaction; for example, the hydrothermal reactor can be a polytetrafluoroethylene hydrothermal reactor, a stainless steel hydrothermal reactor, a high-pressure hydrothermal reactor, etc.

[0018] Preferably, the dialysis method includes dialysis of the solution after hydrothermal reaction using a dialysis bag, wherein the dialysis bag has a molecular weight cutoff of 1000-1200 Da to remove unreacted raw materials. Attached Figure Description

[0019] Figure 1 Transmission electron microscopy image of the aqueous metal tracer prepared in Example 1 of this invention;

[0020] Figure 2 The particle size distribution diagram of the aqueous metal tracer prepared in Example 1 of this invention;

[0021] Figure 3 The surface elemental analysis results are for the aqueous metal tracer prepared in Example 1 of this invention. Detailed Implementation

[0022] This invention primarily addresses the limitations of existing technologies in preparing water-based metal tracers resistant to high salinity. By introducing metal elements as composite tracers during the hydrothermal process, this invention retains both temperature and oxidation resistance while leveraging the diverse selectivity of metal ions to create a series of tracer varieties. Furthermore, by introducing copolymers containing carboxyl and AMPS groups into the tracer synthesis, this invention effectively improves the tracer's salt resistance, addressing the problem that traditional tracers cannot withstand high salinity in formations and suffer from instability due to flocculation and agglomeration, thus affecting detection accuracy.

[0023] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described clearly and completely below in conjunction with specific embodiments. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0024] Unless otherwise specified, the test methods used in the following embodiments are conventional methods; the raw materials used are commercially available items commonly used in the art, unless otherwise specified. In the following embodiments, acrylic acid-2-acrylamido-2-methylpropanesulfonic acid copolymer (AA-AMPS) is from Jinan Shenghe Chemical Co., Ltd. (CAS 40623-75-4).

[0025] I. Specific Embodiments of the Preparation Method of the Aqueous Metal Tracer of the Present Invention

[0026] Example 1

[0027] This embodiment describes a method for preparing an aqueous metal tracer. The specific preparation steps are as follows:

[0028] AA-AMPS, ethylenediamine, and cerium nitrate were dissolved in deionized water at concentrations of 120 g / L, 0.4 mol / L, and 0.04 mol / L, respectively, to prepare 50 mL mixed solutions. These solutions were transferred to a polytetrafluoroethylene (PTFE) hydrothermal reactor and subjected to hydrothermal reaction at 180°C for 5 h, followed by natural cooling to room temperature. After cooling, the reacted solution was dialyzed for 48 h using a dialysis bag with a molecular weight cutoff of 1000 Da. The water was changed every 12 h during dialysis to remove unreacted raw materials. The resulting sample was freeze-dried after dialysis to obtain the aqueous metal tracer of Example 1, denoted as CS.

[0029] The Ce content in the aqueous metal tracer prepared in Example 1 was tested using an ICP spectrometer. The test results showed that the mass fraction of Ce in the tracer of this example was 2.77%.

[0030] In other embodiments, besides cerium nitrate, other types of metal salts can be selected. Before fracturing, technicians can analyze groundwater samples to select metal salts with low background concentrations that can bind to carboxyl groups for tracer preparation. Optional metal salts include, for example, copper, zinc, strontium, zirconium, gallium, niobium, tin, lead, hafnium, cadmium, antimony, tantalum, indium, bismuth, lanthanum, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium, and yttrium.

[0031] II. Comparative Example

[0032] Comparative Example 1

[0033] This comparative example is a carbon dot tracer, and its preparation method includes the following steps:

[0034] Citric acid, ethylenediamine, and cerium nitrate were prepared into 50 mL mixed solutions at concentrations of 0.2 mol / L, 0.4 mol / L, and 0.01 mol / L, respectively. The mixed solutions were transferred to a polytetrafluoroethylene hydrothermal reactor and subjected to a hydrothermal reaction at 180 °C for 5 h. After natural cooling to room temperature, the reaction solution was dialyzed for 48 h using a dialysis bag with a molecular weight cutoff of 1000 Da. The water was changed every 12 h during the dialysis process to remove unreacted raw materials. After dialysis, the obtained sample was freeze-dried to obtain the carbon dot tracer of Comparative Example 1, denoted as CD.

[0035] The Ce content in the carbon dot tracer prepared in Comparative Example 1 was tested using an ICP spectrometer. The test results showed that the mass percentage of Ce in the tracer of this comparative example was 0.18%.

[0036] III. Experimental Examples

[0037] Composition and structural analysis of the tracer in Experiment Example 1

[0038] The CS sample in the aqueous metal tracer prepared in Example 1 was analyzed using transmission electron microscopy, and the particle size distribution of the CS sample was tested. The results are as follows: Figure 1 and Figure 2 As shown. By Figure 1 As shown in the transmission electron microscope (TEM) images, this invention successfully prepared a tracer product with a relatively large size; from Figure 2 It can be seen that the average particle size of the CS sample prepared in Example 1 is 51.97 nm, which is larger than that of the carbon dot tracer in Comparative Example 1 (less than 10 nm).

[0039] In summary, this invention, by introducing a polymer as a precursor during tracer synthesis and then conducting a crosslinking reaction under hydrothermal conditions, can effectively prepare large-sized spherical structures.

[0040] Surface elemental analysis of the aqueous metal tracer CS prepared in Example 1 was performed using X-ray photoelectron spectroscopy (XPS), and the results are as follows: Figure 3 As shown, the CS sample prepared in Example 1 contains C, O, N, S, and Ce elements simultaneously. The N element originates from ethylenediamine, the S element from AA-AMPS, and the Ce element from cerium nitrate. This indicates that the Ce element has been successfully incorporated into the polymer carbon sphere structure, meeting the application requirements of the tracer.

[0041] Experimental Example 2: Tracer Mineralization Tolerance and Adsorption Test

[0042] 2.1 Mineralization tolerance test

[0043] ①Calculate the sample mass required to prepare 20 ml of salt solution with a mineralization of 200000 mg / L, based on the concentrations of NaCl, MgCl2 and CaCl2 being 181570 mg / L, 5940 mg / L and 12490 mg / L, respectively. That is, weigh 3.631 g of NaCl, 0.119 g of MgCl2 and 0.250 g of CaCl2 respectively.

[0044] ② Take 0.1g of the tracer sample CS prepared in Example 1, mix it with the three salts mentioned in step ① in a beaker, dilute it with water to make a 20ml solution, then transfer the solution to a hydrothermal reactor, place it in an oven at 150℃ for 2h, then cool it to room temperature, filter it with a 0.45μm filter, digest and dilute the filtrate, and test the Ce concentration using an inductively coupled plasma optical emission spectrometer (ICP-OES), which is recorded as C1; the tracer CD of Comparative Example 1 is operated in the same manner.

[0045] ③ Take another 0.1g of the tracer sample CS prepared in Example 1 and water to make a 20mL solution. Digest the solution and test the Ce concentration, which is recorded as C0. The tracer CD of Comparative Example 1 is operated in the same way.

[0046] ④ Calculate the Ce content retention rate before and after the mineralization experiment based on C1 / C0. Similarly, referring to the above-mentioned tracer sample mineralization tolerance test procedure, conduct tolerance tests on tracer samples CS and CD under a mineralization condition of 50000 mg / L. The calculated mineralization retention rates are shown in Table 1.

[0047] 2.2 Adsorption experiment:

[0048] The tracer sample CS prepared in Example 1 was used. 200 ml of a tracer solution with a Ce content of 200 mg / L was prepared with water, and its specific concentration C0 was measured. A rock sample was ground and passed through a 50-mesh sieve. 30 g of the ground rock fragments were placed in an Erlenmeyer flask, and 90 ml of the prepared tracer solution was added. The flask was sealed and shaken in a water bath at 150°C for 48 h. After cooling to room temperature, the supernatant was absorbed through a 0.45 μm filter for digestion. The Ce concentration was measured using ICP-OES and recorded as C1. The Ce retention rate before and after the adsorption experiment was calculated based on C1 / C0. The tracer CD of Comparative Example 1 was prepared using the same procedure. Similarly, following the above adsorption experiment procedure for tracer samples, quartz sand was used instead of rock fragments to conduct adsorption experiments on tracer samples CS and CD. The calculated adsorption retention rates are shown in Table 1.

[0049] Table 1 shows the mineralization retention rate and adsorption retention rate results for CD and CS.

[0050]

[0051] As shown in Table 1, the mineralization retention rates of both the CD tracer sample in Comparative Example 1 and the CS tracer sample in Example 1 decreased with increasing mineralization. However, the performance of the CS tracer was significantly better than that of the CD tracer, especially under high mineralization conditions of 200,000 mg / L, where the content loss was only 13.17%. This indicates that the carbon spheres synthesized by introducing the AMPS structure can meet the stringent requirements of high mineralization applications. Furthermore, the adsorption retention rates of both rock fragments and quartz sand were lower for the CD tracer than for the CS tracer, indicating that the introduction of the AMPS structure into the CS tracer can significantly suppress its adsorption ratio, which is more conducive to improving the stability and lifetime of the tracer.

[0052] Zeta potential analysis of tracers in Experiment Example 3

[0053] The particle size and zeta potential of the comparative CD tracer and the CS tracer of Example 1 at mineralizations of 50,000 mg / L and 200,000 mg / L were compared using a nanoparticle-scale zeta potential analyzer. The results are shown in Table 2.

[0054] Table 2 Comparison of average particle size and zeta potential of CD and CS

[0055]

[0056] As shown in Table 2, the average particle size of both the CD tracer in Comparative Example 1 and the CS tracer in Example 1 increases with increasing mineralization, indicating that increased mineralization causes tracer aggregation. In contrast, the average particle size of the CS tracer increases less, suggesting that the CS tracer has better tolerance to high mineralization.

[0057] A larger absolute value of the zeta potential indicates a stronger repulsive force during particle aggregation, making aggregation less likely. The zeta potential results show that the absolute values ​​of the zeta potentials for both the CD and CS tracers decrease with increasing mineralization, but the decrease for the CS tracer is relatively smaller. Therefore, the CS tracer in Example 1 of this invention exhibits better tolerance to high mineralization.

[0058] In summary, the aqueous metal tracer prepared by this invention is not prone to aggregation or adsorption, exhibits high tolerance to salinity (up to 200,000 mg / L), and is suitable for harsh, high-salinity underground fracturing operations. Therefore, this invention provides a novel preparation route and strategy for tracers resistant to high salinity, and has extremely broad application prospects in fracturing operations of harsh, high-salinity oil reservoirs.

[0059] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of their technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing an aqueous metal tracer, characterized in that, Includes the following steps: A mixed solution is obtained by dissolving the copolymer, the binder, and the metal salt in a solvent. The copolymer is mainly composed of acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid. The binder contains hydroxyl and / or amino groups, wherein the total number of hydroxyl and amino functional groups is more than two. The mixed solution was subjected to a hydrothermal reaction at a temperature of 160–200°C, and the aqueous metal tracer was obtained by dialysis and freeze-drying.

2. The method for preparing the aqueous metal tracer according to claim 1, characterized in that, The copolymer is an acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer.

3. The method for preparing the aqueous metal tracer according to claim 1, characterized in that, The binder is one or more of ethylenediamine, ethylene glycol, glycerol, and ethanolamine.

4. The method for preparing the aqueous metal tracer according to claim 1, characterized in that, The metal salt is one or more of the following: cerium salt, copper salt, zinc salt, strontium salt, zirconium salt, gallium salt, niobium salt, tin salt, lead salt, hafnium salt, cadmium salt, antimony salt, tantalum salt, indium salt, bismuth salt, lanthanum salt, praseodymium salt, neodymium salt, promethium salt, samarium salt, europium salt, gadolinium salt, terbium salt, dysprosium salt, holmium salt, erbium salt, thulium salt, ytterbium salt, lutetium salt, scandium salt, and yttrium salt.

5. The method for preparing the aqueous metal tracer according to claim 1, characterized in that, The ratio of the copolymer, binder and metal salt is (100-150) g ​​: (0.2-0.6) mol : (0.01-0.15) mol.

6. The method for preparing the aqueous metal tracer according to claim 5, characterized in that, The solvent is water, and the concentration of the copolymer in the mixed solution is (100-150) g / L.

7. The method for preparing the aqueous metal tracer according to claim 5, characterized in that, The ratio of the copolymer, binder and metal salt is (120-130) g : (0.4-0.6) mol : (0.04-0.07) mol.

8. The method for preparing the aqueous metal tracer according to claim 1, characterized in that, The hydrothermal reaction takes 5 to 6 hours.

9. The method for preparing the aqueous metal tracer according to claim 1, characterized in that, The dialysis method includes dialysis of the solution after hydrothermal reaction using a dialysis bag, wherein the molecular weight cutoff of the dialysis bag is 1000-1200 Da.