All-solid-state electrochromic devices and their fabrication methods

By introducing P-type transparent conductive interface modulation layers on both sides of the electrochromic layer, the problems of irreversible interface phase and electron leakage in all-solid-state electrochromic devices are solved, improving optical modulation performance and cycle stability, and extending device life.

CN123113205APending Publication Date: 2026-11-17SHANGHAI CENTAUR ENTERPRISE DEV GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611627769.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing inorganic all-solid-state electrochromic devices suffer from irreversible interface phase formation, parasitic electron leakage, and ion transport loss during long-term cycling, leading to attenuation of optical modulation amplitude and decrease in coulombic efficiency.

Method used

A nanometer-thick P-type transparent conductive interface control layer is introduced on both sides of the electrochromic layer to form a heterojunction, which can finely control electron injection and lithium-ion exchange, suppress interface phase formation and electron leakage, and optimize the electric field distribution.

Benefits of technology

It improves the optical modulation retention rate and cycle stability of electrochromic devices, enhances the overall water and oxygen resistance of the device packaging, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123113205A_ABST
    Figure CN123113205A_ABST
Patent Text Reader

Abstract

This invention provides an all-solid-state electrochromic device and its fabrication method, relating to the field of electrochromic materials and devices. The device comprises, from bottom to top, a first conductive layer, an electrochromic layer, a dielectric layer, an ion storage layer, a lithiation layer, and a second conductive layer. A first P-type transparent conductive interface control layer is disposed between the electrochromic layer and the first conductive layer, and / or a second P-type transparent conductive interface control layer is disposed between the electrochromic layer and the dielectric layer. This achieves electron-selective modulation, suppresses irreversible interface phase formation, and optimizes the device's operating potential distribution, resulting in an all-inorganic solid-state electrochromic device with high cyclic electrochemical stability and high light modulation range retention.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrochromic materials and devices, specifically to an all-solid-state electrochromic device comprising a P-type conductive interface control layer and its preparation method. Background Technology

[0002] All-solid-state electrochromic devices have become a research hotspot in novel functional materials due to their broad application prospects in fields such as intelligent dimming, displays, and energy-efficient buildings. The typical structure of existing inorganic all-solid-state electrochromic devices is "ITO conductive layer / electrochromic layer (e.g., WO3) / electrolyte layer / ion storage layer (e.g., NiO) / ITO conductive layer". This structure suffers from the following main problems during long-term cycling: 1. Irreversible interface phase formation: Irreversible interface phases such as lithium tungstate (Li2WO4) easily form at the direct contact between the color-changing functional layer and the dielectric layer, consuming reversible coloring active sites, leading to attenuation of optical modulation amplitude and a decrease in coulombic efficiency. 2. Parasitic electron leakage: Electrons from the color-changing functional layer leak into the ion-dielectric layer, participating in unfavorable side reactions, increasing the hold-state leakage current, and reducing the device's optical memory performance. 3. Ion transport loss: Li + Uneven concentration distribution at the interface creates deep traps, leading to irreversible Li₂ concentration loss. + Losses and a decline in available ion inventory.

[0003] The main problems with existing technical solutions that use wide bandgap oxides such as Ta2O5, HfO2, and ZrO2 as interfacial passivation layers are: 1. They are purely insulating barrier layers, lacking the ability to react with Li. + 1. It has no explicit control over the transport of holes; 2. It lacks hole-selective transport capabilities and cannot perform fine-tuning of the interface potential by matching the energy levels of the counter electrode material; 3. Its inhibition effect on the initial nucleation of Li2WO4 at the direct interface of the color-changing functional layer / dielectric layer is relatively limited. Summary of the Invention

[0004] To address the shortcomings of existing technologies, the purpose of this invention is to provide an all-solid-state electrochromic device.

[0005] According to the present invention, an all-solid-state electrochromic device includes a first conductive layer, an electrochromic layer, a dielectric layer, an ion storage layer, a lithiation layer, and a second conductive layer stacked from bottom to top. Wherein, a first P-type transparent conductive interface control layer is disposed between the electrochromic layer and the first conductive layer, and / or, a second P-type transparent conductive interface control layer is disposed between the electrochromic layer and the dielectric layer.

[0006] Furthermore, the substrate material of the first conductive layer and the second conductive layer is one of fluorine-doped tin oxide, indium tin oxide, and aluminum-doped zinc oxide glass; The thickness of the first conductive layer is 150-400 nm, and the sheet resistance is 3-40 Ω / cm. 2 .

[0007] Furthermore, the material of the first P-type transparent conductive interface control layer is CuI or a CuI-containing composite such as CuI / TiO2 composite. The thickness of the first P-type transparent conductive interface control layer is 5-20 nm, and the conductivity is 1-300. .

[0008] Furthermore, the electrochromic layer is made of tungsten. The tungsten layer material is tungsten oxide and tungsten oxide derivatives. The tungsten oxide derivatives are element-doped tungsten oxides, and the doping elements include one or more of Ti, Al, and Ni. The thickness of the electrochromic layer is 200-450 nm.

[0009] Furthermore, the material of the second P-type transparent conductive interface control layer is CuI or a composite containing CuI, such as a CuI / TiO2 composite. The thickness of the second P-type transparent conductive interface control layer is 3-10 nm, and the conductivity is 50-400. .

[0010] Furthermore, the dielectric layer is a transparent dielectric film with a thickness of 10-200 nm.

[0011] Furthermore, the ion storage layer is a Ni-based alloy oxide thin film with a thickness of 100-250 nm.

[0012] Furthermore, the lithium layer is prepared by Li metal target sputtering; The atmosphere is Ar, the sputtering pressure is 0.3-0.5 Pa, the sputtering power is 50-100 W, and the time is 3-20 min.

[0013] Furthermore, the first conductive layer and the second conductive layer are laser-scribed to form a transparent conductive electrode, which is exposed at the edge; A metal main electrode is connected to the transparent conductive electrode exposed at the edge, which is used to connect to the power controller.

[0014] A method for fabricating the all-solid-state electrochromic device according to the present invention includes: S1. Prepare a 5-10 nm first P-type transparent conductive interface control layer on the cleaned glass-based first conductive layer. S2. An electrochromic layer is prepared on the first P-type transparent conductive interface control layer; S3. Prepare a 3-5 nm second P-type transparent conductive interface control layer on the electrochromic layer; S4. A dielectric layer, an ion storage layer, a lithiation layer, and a second conductive layer are sequentially sputtered onto the second P-type transparent conductive interface control layer. S5. Perform laser scribing and fix the metal electrodes to obtain the all-solid-state electrochromic device.

[0015] Compared with the prior art, the present invention has the following beneficial effects: This invention introduces nanoscale-thick p-type transparent conductive ultrathin interface control layers on both sides of the electrochromic layer to form a heterojunction, achieving finer electron injection control, suppressing lithium ion deep migration to the transparent conductive layer, improving electrode structure stability, and simultaneously smoothing the peak lithium ion concentration. This also suppresses the formation of irreversible interface phases at the interface between the electrochromic layer and the dielectric layer, optimizes device potential, and improves cycle stability. Compared to traditional wide-bandgap oxide passivation layers, the CuI layer allows for more precise control of interface electron transfer and Li... + Exchange and electric field distribution.

[0016] Specifically, by appropriately regulating lithium-ion implantation, the formation of harmful phases at the electrochromic layer interface can be suppressed, thereby improving the optical modulation retention rate and cycling stability of electrochromic devices. Limiting electron over-implantation into the electrochromic layer reduces deep reduction of the electrochromic layer material and minimizes irreversible reactions. Furthermore, restricting lithium-ion entry into the transparent conductive layer during cycling improves the stability of the transparent conductive layer and enhances the overall device packaging's resistance to water and oxygen. Attached Figure Description

[0017] Other features, objects, and advantages of the present invention will become more apparent from the following detailed description of non-limiting embodiments with reference to the accompanying drawings: Figure 1 This is a schematic diagram of the electrochromic device of the present invention. Detailed Implementation

[0018] The present invention will now be described in detail with reference to specific embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the invention in any way. It should be noted that those skilled in the art can make several changes and improvements without departing from the concept of the present invention. These all fall within the protection scope of the present invention.

[0019] like Figure 1 As shown, the present invention provides an all-solid-state electrochromic device comprising, from bottom to top, a first conductive layer, an electrochromic layer, a dielectric layer, an ion storage layer, a lithiation layer, and a second conductive layer. A first P-type transparent conductive interface control layer is disposed between the electrochromic layer and the first conductive layer, and / or a second P-type transparent conductive interface control layer is disposed between the electrochromic layer and the dielectric layer. The first conductive layer is fabricated on a substrate.

[0020] The substrate material for both the first and second conductive layers is one of fluorine-doped tin oxide (FTO), indium tin oxide (ITO), or aluminum-doped zinc oxide (AZO) glass. The thickness of the first conductive layer is 150-400 nm, and its sheet resistance is 3-40 Ω / cm. 2 .

[0021] The first P-type transparent conductive interface control layer material is CuI or a CuI-containing composite such as a CuI / TiO2 composite; the thickness of the P-type transparent conductive ultrathin interface control layer is 5-20 nm; the conductivity is 1-300. The preparation methods include, but are not limited to, thermal evaporation, magnetron sputtering, atomic layer deposition, laser-assisted deposition, etc.

[0022] The electrochromic layer is made of tungsten; the tungsten layer material is tungsten oxide (WO3) and its derivatives, the tungsten oxide derivatives are element-doped tungsten oxide, and the doping elements include one or more of Ti, Al and Ni. The thickness of the electrochromic layer is 200-450 nm.

[0023] The second P-type transparent conductive interface control layer material is CuI or a CuI-containing composite such as CuI / TiO2 composite; the thickness of the P-type transparent conductive ultrathin interface control layer is 3-10 nm, and the conductivity is 50-400. The preparation methods include, but are not limited to, thermal evaporation, magnetron sputtering, atomic layer deposition, laser-assisted deposition, etc.

[0024] The dielectric layer refers to a conventional transparent dielectric film, including but not limited to films such as SiAlOx, Ta2O5, SiO2, Si3N4, ZrO2, and HfO2, with a thickness of 10-200 nm.

[0025] The ion storage layer refers to a Ni-based alloy oxide thin film, including but not limited to NiOx, NiWOx, NiVOx, etc., with a thickness of 100-250 nm. Preparation methods include, but are not limited to, thermal evaporation, magnetron sputtering, laser-assisted deposition, etc.

[0026] The lithiation layer refers to Li metal target sputtering in an Ar atmosphere; sputtering pressure 0.3-0.5 Pa, sputtering power 50-100 W, and time 3-20 min.

[0027] The first and second conductive layers are laser-etched to create transparent conductive electrodes, which are exposed at the edges. It should be noted that laser etching refers to electrochromic or a typical leakage current control technique in the photovoltaic industry. A metal main electrode is connected to the exposed transparent conductive electrode at the edges for connecting to the power controller, through methods including but not limited to pasting or screen-printing silver paste and curing.

[0028] This invention introduces a wide-bandgap, highly transparent, p-type conductive, and tunable work function interface layer material that simultaneously suppresses the nucleation and expansion of harmful (Li2WO4, etc.) interface phases and secondary phases. The thinner interface layer, coupled with an ultrathin protective layer, provides controlled interface trapping and migration rate limiting for lithium ions, allowing them to pass through I0 before over-lithiation. - Related coordination or restricted transformation preferentially captures a portion of excess Li. + To reduce the entry into W from a dynamic perspective 4+ —The probability of the irreversible reaction pathway of Li2WO4; In addition, applying a highly transparent p-type conductive layer to the transparent electrode side can reduce parasitic electron leakage, restrict electron injection and lithium ion migration to the transparent conductive electrode side, reduce local over-reduction and interfacial electrochemical damage of the color-changing functional layer (WOx) layer near the transparent conductive electrode, and appropriately block lithium ion diffusion to the transparent conductive electrode (ITO) electrode, prevent damage to the ITO layer, and improve the device cycle stability and service life.

[0029] In one embodiment, the all-solid-state electrochromic device includes, from bottom to top, a first conductive layer, an electrochromic layer, a second P-type transparent conductive interface control layer, a dielectric layer, an ion storage layer, a lithiation layer, and a second conductive layer stacked sequentially. The mechanism of the P-type transparent conductive interface control layer in this structure includes Li + Embedded WO x It first occupies the reversible intercalation site in the W–O framework, accompanied by W 6+ Restore to W 5+ As local lithiation and electron injection continue to enhance, the system further generates W. 4+ and deep trap-related structures such as Li₂WO₄ / Li₂O. Located in WO₄ x / SiAlO x The CuI at the interface can be converted to I before over-lithiation. - Related coordination or restricted transformation preferentially captures a portion of excess Li. + The conversion reaction preferentially consumes some lithium ions and electrons at the interface, forming an in-situ LiI / Cu composite interface layer with LiI as the ion-regulating phase and dispersed Cu as the electron-conducting phase. The generated Cu can also absorb SiAlO. x The reactive oxygen species in the WO3 layer are prevented from entering the color-changing functional layer. This composite interface layer reduces WO3 levels. x / SiAlO x The local electron-ion coupling reaction rate at the direct contact point, buffering the instantaneous lithium-ion flux and limiting the reaction depth under excessive reduction conditions, reduces WO3. x Localized over-lithiation of the surface layer and Li2WO4, W 4+The tendency for Li₂WO₄ and related irreversible ion traps to form or expand kinetically reduces entry into W₂WO₄. 4+ —Probability of the irreversible reaction pathway of Li2WO4.

[0030] In one embodiment, the all-solid-state electrochromic device includes, from bottom to top, a first conductive layer, a first P-type transparent conductive interface control layer, an electrochromic layer, a dielectric layer, an ion storage layer, a lithiation layer, and a second conductive layer, stacked sequentially. The mechanism of the P-type transparent conductive interface control layer in this structure is as follows: it controls the W0... x The coloring process employs gentle electron injection current limiting to avoid excessive electron injection, deep reduction, and associated excess Li during high-voltage pulses or long-term cycling. + Embedded.

[0031] In one embodiment, the all-solid-state electrochromic device includes, from bottom to top, a first conductive layer, a first P-type transparent conductive interface control layer, an electrochromic layer, a second P-type transparent conductive interface control layer, a dielectric layer, an ion storage layer, a lithiation layer, and a second conductive layer, stacked sequentially. P-type transparent conductive interface control layers are disposed on both sides of the electrochromic layer, providing the dual advantages of suppressing initial side reactions at the interface (on the color-changing functional layer side) and limiting excessive electron injection.

[0032] This invention also provides a method for fabricating an all-solid-state electrochromic device, comprising: S1. Prepare a 5-10 nm first P-type transparent conductive interface control layer on the cleaned glass-based first conductive layer.

[0033] S2. An electrochromic layer is prepared on the first P-type transparent conductive interface control layer.

[0034] S3. Prepare a 3-5 nm second P-type transparent conductive interface control layer on the electrochromic layer.

[0035] S4. A dielectric layer, an ion storage layer, a lithiation layer, and a second conductive layer are sequentially sputtered onto the second P-type transparent conductive interface control layer.

[0036] S5. Perform laser scribing and fix the metal electrodes to obtain the all-solid-state electrochromic device.

[0037] Example 1 This embodiment provides a method for fabricating an all-solid-state electrochromic device including a P-type conductive interface control layer, such as... Figure 1 As shown, the material comprises, in sequence, a first conductive layer, a first P-type transparent conductive interface control layer, an electrochromic layer, a second P-type transparent conductive interface control layer, a dielectric layer, an ion storage layer, a lithiation layer, and a second conductive layer deposited by sputtering; its preparation method includes the following steps: 1. A 5 nm thick CuI film was deposited on a 100 mm × 100 mm ITO conductive glass substrate (ITO thickness 2 mm) using magnetron sputtering, with an initial vacuum of 5 × 10⁻⁶. -6 Pa, using CuI target, pure Ar gas sputtering, gas pressure 0.5 Pa, sputtering power 50 W; time 400 s to form the first P-type transparent conductive interface control layer.

[0038] 2. Continue to sputter and deposit a 200-450nm WOx thin film in the chamber: WO3 target, Ar / O2 (volume ratio 6:1), sputtering power 150 W, gas pressure 1 Pa; time 40 min, to form a WO3 layer (400nm), forming an electrochromic layer.

[0039] 3. A 3 nm CuI thin film was sputtered onto the formed electrochromic layer. The sputtering target was CuI, pure Ar gas was used for sputtering, the gas pressure was 0.5 Pa, the sputtering power was 30 W, and the deposition time was 300 s.

[0040] 4. Continue sputtering to prepare a 30nm SiAlOx dielectric layer film, using Si9Al1 alloy as the target material, Ar / O2 mixed gas (3:1) as the working gas, sputtering pressure 1Pa, sputtering power 100W, substrate temperature 25℃, and time 5 min.

[0041] 5. Continue sputtering the ion storage layer: The substrate is placed in the Ni metal target reactive sputtering chamber, and reactive sputtering is performed using a medium frequency power supply. The Ar / O2 volume ratio is 1:1; the sputtering pressure is 1.2 Pa; the sputtering power is 150 W; the substrate temperature is 25 °C; the time is 30 min; and the deposition thickness is 155 nm. Then, annealing treatment is performed (270 °C, 2 h) to obtain the ion storage layer.

[0042] 6. After the substrate is cooled to 100°C, lithium metal is lithiated by sputtering a Li metal target in an Ar atmosphere; the sputtering pressure is 0.3 Pa, the sputtering power is 50 W, and the time is 5 min.

[0043] 7. Sputtering a transparent conductive layer: The substrate is placed in the ITO chamber and sputtered using a DC pulse power supply. The substrate is heated to 300°C and an Ar / O2 mixed gas (O2 volume content 1.83%) is introduced. The sputtering pressure is 0.3 Pa, the power is 100 W, and the time is 15 min to obtain a transparent conductive layer (thickness of 196 nm).

[0044] 8. Laser scribing and edge clearing: Using laser scribing P1, P2, P3, P4 and edge clearing process, a lower transparent conductive electrode is prepared; an electrochromic device is formed with electrodes exposed at the edge and separated at the upper and lower edge positions.

[0045] 9. Fix the main electrode: Apply conductive copper tape to the position where the lower transparent electrode is exposed and the corresponding upper electrode position on the other side.

[0046] 10. Performance testing: The test methods shall be in accordance with the test methods of ASTM E2141-21 and ISO18510:2017 standards.

[0047] Response time: At 2.5V, coloring time is 40s and fading time is 25s.

[0048] Cycle life: After 10,000 cycles of color change, the rate of change in optical transmittance is maintained at 85%.

[0049] Example 2 This embodiment provides a method for fabricating an all-solid-state electrochromic device including a P-type conductive interface control layer, comprising the following steps: 1. A 10 nm thick CuI film was deposited on a 100 mm × 100 mm ITO conductive glass substrate (ITO thickness 2 mm) using magnetron sputtering, with an initial vacuum of 5 × 10⁻⁶. -6 Pa, using CuI target, pure Ar gas sputtering, gas pressure 0.5 Pa, sputtering power 60 W; time 600 s to form the first P-type transparent conductive interface control layer.

[0050] 2. Continue to sputter and deposit a 200-450nm WOx thin film in the chamber: WO3 target, Ar / O2 (flow ratio 6:1), sputtering power 150 W, gas pressure 1 Pa; time 40 min, to form a WO3 layer (400nm), forming an electrochromic layer.

[0051] 3. A 5 nm CuI thin film was sputtered onto the formed electrochromic layer. The sputtering target was CuI, pure Ar gas was used for sputtering, the gas pressure was 0.5 Pa, the sputtering power was 50 W, and the deposition time was 400 s.

[0052] 4. Continue sputtering to prepare a 30nm SiAlOx dielectric layer film, using Si9Al1 alloy as the target material, Ar / O2 mixed gas (3:1) as the working gas, sputtering pressure 1Pa, sputtering power 100W, substrate temperature 25℃, and time 5 min.

[0053] 5. Continue sputtering the ion storage layer: The substrate is placed in the Ni metal target reactive sputtering chamber, and reactive sputtering is performed using a medium frequency power supply. The Ar / O2 volume ratio is 1:1; the sputtering pressure is 1.2 Pa; the sputtering power is 150 W; the substrate temperature is 25 °C; the time is 30 min; and the deposition thickness is 155 nm. Then, annealing treatment is performed (270 °C, 2 h) to obtain the ion storage layer.

[0054] 6. After the substrate is cooled to 100°C, lithium metal is lithiated by sputtering a Li metal target in an Ar atmosphere; the sputtering pressure is 0.3 Pa, the sputtering power is 50 W, and the time is 5 min.

[0055] 7. Sputtering a transparent conductive layer: The substrate is placed in the ITO chamber and sputtered using a DC pulse power supply. The substrate is heated to 300°C and an Ar / O2 mixed gas (O2 volume content 1.83%) is introduced. The sputtering pressure is 0.3 Pa, the power is 100 W, and the time is 15 min to obtain a transparent conductive layer (thickness of 196 nm).

[0056] 8. Laser scribing and edge clearing: Using laser scribing P1, P2, P3, P4 and edge clearing process, a lower transparent conductive electrode is prepared; an electrochromic device is formed with electrodes exposed at the edge and separated at the upper and lower edge positions.

[0057] 9. Fix the main electrode: Apply conductive copper tape to the position where the lower transparent electrode is exposed and the corresponding upper electrode position on the other side.

[0058] 10. Performance Testing: Test methods are conducted in accordance with ASTM E2141-21 and ISO18510:2017 standards. Response Time: At 3V, coloring time is 50s, and fading time is 35s.

[0059] Cycle life: After 10,000 cycles of color change, the rate of change in optical transmittance is maintained at 90%.

[0060] Transmittance adjustment range: transmittance variation in the visible light region (550nm) is 10%-65%, meeting the needs of smart window use.

[0061] Comparative Example This comparative example provides an all-solid-state electrochromic device and its fabrication method, which is basically the same as Example 1, except that a P-type conductive interface control layer is not used. The device comprises a first conductive layer, an electrochromic layer, a dielectric layer, an ion storage layer, a lithiation layer, and a second conductive layer, deposited sequentially by sputtering. The fabrication method includes the following steps: 1. A 200-450 nm WOx thin film was sputtered onto a 100 mm × 100 mm ITO conductive glass (ITO thickness 2 mm) in a chamber: WO3 target, Ar / O2 (volume ratio 6:1), sputtering power 150 W, gas pressure 1 Pa; time 40 min, forming a WO3 layer (400 nm), thus forming an electrochromic layer.

[0062] 2. On the formed electrochromic layer, a 30 nm SiAlOx dielectric layer film was prepared by sputtering. The target material was Si9Al1 alloy, the working gas was Ar / O2 mixture (3:1), the sputtering pressure was 1 Pa, the sputtering power was 100 W, the substrate temperature was 25 °C, and the time was 5 min.

[0063] 3. Continue sputtering the ion storage layer: The substrate is placed in the Ni metal target reactive sputtering chamber, and reactive sputtering is performed using a medium frequency power supply. The Ar / O2 volume ratio is 1:1; the sputtering pressure is 1.2 Pa; the sputtering power is 150 W; the substrate temperature is 25 °C; the time is 30 min; and the deposition thickness is 155 nm. Then, annealing treatment is performed (270 °C, 2 h) to obtain the ion storage layer.

[0064] 4. After the substrate is cooled to 100°C, lithium metal is lithiated by sputtering a Li metal target in an Ar atmosphere; the sputtering pressure is 0.3 Pa, the sputtering power is 50 W, and the time is 5 min.

[0065] 5. Sputtering a transparent conductive layer: The substrate is placed in the ITO chamber and sputtered using a DC pulse power supply. The substrate is heated to 300°C and an Ar / O2 mixed gas (O2 volume content 1.83%) is introduced. The sputtering pressure is 0.3 Pa, the power is 100 W, and the time is 15 min to obtain a transparent conductive layer (thickness of 196 nm).

[0066] 6. Laser scribing and edge clearing: Using laser scribing P1, P2, P3, P4 and edge clearing process, a lower transparent conductive electrode is prepared; an electrochromic device is formed with electrodes exposed at the edge and separated at the upper and lower edge positions.

[0067] 7. Fix the main electrode: Apply conductive copper tape to the position where the lower transparent electrode is exposed and the corresponding upper electrode position on the other side.

[0068] 8. Performance testing: The test methods shall be in accordance with the test methods of ASTM E2141-21 and ISO18510:2017 standards.

[0069] Response time: At 2.5V, coloring time is 40s and fading time is 25s.

[0070] Cycle life: After 10,000 cycles of color change, the rate of change in optical transmittance is maintained at 60%.

[0071] In the description of this application, it should be understood that the terms "upper", "lower", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.

[0072] Specific embodiments of the present invention have been described above. It should be understood that the present invention is not limited to the specific embodiments described above, and those skilled in the art can make various changes or modifications within the scope of the claims, which do not affect the essence of the present invention. Unless otherwise specified, the embodiments and features described in this application can be arbitrarily combined with each other.

Claims

1. A fully solid-state electrochromic device, characterized in that, It includes a first conductive layer, an electrochromic layer, a dielectric layer, an ion storage layer, a lithiation layer, and a second conductive layer, which are stacked sequentially from bottom to top; Wherein, a first P-type transparent conductive interface control layer is disposed between the electrochromic layer and the first conductive layer, and / or, a second P-type transparent conductive interface control layer is disposed between the electrochromic layer and the dielectric layer.

2. The all-solid-state electrochromic device according to claim 1, characterized in that, The substrate material of the first conductive layer and the second conductive layer is one of fluorine-doped tin oxide, indium tin oxide, and aluminum-doped zinc oxide glass; The thickness of the first conductive layer is 150-400 nm, and the sheet resistance is 3-40 Ω / cm. 2 .

3. The all-solid-state electrochromic device according to claim 1, characterized in that, The material of the first P-type transparent conductive interface control layer is CuI or a CuI-containing composite such as CuI / TiO2 composite. The thickness of the first P-type transparent conductive interface control layer is 5-20 nm, and the conductivity is 1-300. .

4. The all-solid-state electrochromic device according to claim 1, characterized in that, The electrochromic layer is made of tungsten material; The tungsten layer material is tungsten oxide and tungsten oxide derivatives. The tungsten oxide derivatives are element-doped tungsten oxides, and the doping elements include one or more of Ti, Al, and Ni. The thickness of the electrochromic layer is 200-450 nm.

5. The all-solid-state electrochromic device according to claim 1, characterized in that, The material of the second P-type transparent conductive interface control layer is CuI or a composite containing CuI, such as a CuI / TiO2 composite. The thickness of the second P-type transparent conductive interface control layer is 3-10 nm, and the conductivity is 50-400. .

6. The all-solid-state electrochromic device according to claim 1, characterized in that, The dielectric layer is a transparent dielectric film with a thickness of 10-200 nm.

7. The all-solid-state electrochromic device according to claim 1, characterized in that, The ion storage layer is a Ni-based alloy oxide thin film with a thickness of 100-250 nm.

8. The all-solid-state electrochromic device according to claim 1, characterized in that, The lithium-ion layer was prepared by Li metal target sputtering. The atmosphere is Ar, the sputtering pressure is 0.3-0.5 Pa, the sputtering power is 50-100 W, and the time is 3-20 min.

9. The all-solid-state electrochromic device according to claim 1, characterized in that, The first conductive layer and the second conductive layer are laser scribing to prepare a transparent conductive electrode, which is exposed at the edge. A metal main electrode is connected to the transparent conductive electrode exposed at the edge, which is used to connect to the power controller.

10. A method for preparing an all-solid-state electrochromic device according to any one of claims 1-9, characterized in that, include: S1. Prepare a 5-10 nm first P-type transparent conductive interface control layer on the cleaned glass-based first conductive layer. S2. An electrochromic layer is prepared on the first P-type transparent conductive interface control layer; S3. Prepare a 3-5 nm second P-type transparent conductive interface control layer on the electrochromic layer; S4. A dielectric layer, an ion storage layer, a lithiation layer, and a second conductive layer are sequentially sputtered onto the second P-type transparent conductive interface control layer. S5. Perform laser scribing and fix the metal electrodes to obtain the all-solid-state electrochromic device.