Preparation method and application of low-temperature profibrillated membrane electrode with carboxyl carbon-induced MnO2 elastic crystalline phase and Mn-OC interfacial electron bridge co-evolution

By reacting carboxylated single-walled carbon nanotubes with a manganese source to form an Mn-OC electron bridge, and combining this with a low-temperature protofibrillation process, a high-capacity, high-energy-density, and cycle-stable self-supporting membrane electrode was prepared. This solved the problems of MnO2 crystal phase structure degradation and irreversible dissolution in existing technologies, and achieved highly efficient electrochemical performance in the zinc ion storage process.

CN123120522APending Publication Date: 2026-11-17JIANGSU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611610257.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing wet electrode processes suffer from solvent contamination and weak interfacial bonding, while dry electrode processes suffer from high fiberization temperatures, which easily damage MnO2 active materials. Furthermore, the degradation of the MnO2 crystal phase structure and irreversible dissolution are difficult to suppress, resulting in insufficient capacity utilization and cycle stability during zinc ion storage.

Method used

Carboxylated single-walled carbon nanotubes were used as crystal phase inducers and interface building units to react with manganese sources to form Mn-OC electron bridges. Combined with polytetrafluoroethylene emulsion and polymer additives with low-temperature mobility, a three-dimensional interconnected network structure self-supporting membrane electrode was prepared through a low-temperature fibrillation film formation process.

Benefits of technology

It improves the specific capacitance and energy density of zinc ion hybrid capacitors, enhances the structural stability and cycle life of electrodes, reduces the preparation cost, and is suitable for gel-based or all-solid-state electrolytes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120522A_ABST
    Figure CN123120522A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of energy storage materials and devices, and discloses a method for preparing a low-temperature protofibrillated membrane electrode by carboxyl-induced MnO2 elastic crystalline phase and the synergistic evolution of Mn-O-C electron bridges: Single-walled carbon nanotubes are oxidized with mixed acid to obtain SCNT-c, which is then hydrothermally reacted with potassium permanganate, manganese chloride tetrahydrate, and nitric acid to prepare ε-MnO2@SCNT-c powder; this powder is then slurried with PTFE emulsion and low-temperature dynamic polymer additives, and subjected to roll forming, rapid cooling, stretching activation, and low-temperature curing to obtain a self-supporting membrane electrode. The carboxyl-induced evolution of α-MnO2 into ε-MnO2 and the formation of Mn-O-C electron bridges, synergistically with low-temperature protofibrillated membrane formation, improves capacity, energy density, and cycle stability. The membrane electrode is used as the positive electrode of an aqueous zinc-ion hybrid capacitor, which is safe, low-cost, and environmentally friendly; it requires no current collector, is customizable, and adaptable to gel or all-solid-state electrolytes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of energy storage materials and devices, and relates to membrane electrodes, particularly to a method for preparing a low-temperature profibrillated membrane electrode with carboxyl carbon-induced MnO2 elastic crystalline phase and Mn-OC interfacial electron bridge synergistic evolution, and its application. Background Technology

[0002] Aqueous zinc-ion hybrid capacitors combine the high power density of aqueous capacitors with the high energy density of zinc-ion batteries, offering advantages such as high safety and low cost, making them an important development direction for next-generation high-safety energy storage devices. Among membrane capacitor cathode materials, manganese dioxide (MnO2) has been widely studied due to its high theoretical capacity, abundant reserves, and environmental friendliness. However, MnO2 suffers from problems such as lattice distortion, structural degradation, and irreversible dissolution during zinc-ion storage, and the improvement of its reversibility is limited by the insufficient reversibility of reaction intermediates, thus restricting the capacity utilization and cycle stability of manganese-based cathodes.

[0003] In electrode fabrication, the wet process has long been used in this field. This process requires dispersing active materials, conductive agents, and binders (such as PVDF) in an organic solvent (such as NMP) to form a slurry, which is then coated, dried, and rolled to form the electrode. However, the wet process has significant drawbacks: the use of organic solvents leads to higher costs (e.g., NMP is expensive), drying energy consumption is high (drying time accounts for more than 40% of the production line), a solvent recovery system is required, and problems such as active material shedding, poor dispersibility, and insufficient structural stability are prone to occur during the recycling process, thus limiting the application of highly active solid electrolytes.

[0004] The core breakthrough of dry electrode technology lies in completely eliminating solvents: by directly fiberizing and bonding dry powder materials (active material, conductive agent, binder), a self-supporting electrode film is formed through hot pressing. This technology has significant advantages: eliminating coating and drying steps, reducing energy consumption by more than 50%; avoiding solvent pollution, making it more environmentally friendly; compatible with water and oxygen-sensitive materials, accelerating the industrialization of solid-state capacitors / batteries; and simultaneously improving electrode compaction density and mechanical strength. However, for MnO2 matrix capacitor electrodes, the dry process still faces difficulties: firstly, conventional binders require high temperatures to achieve fiberization, and high temperatures can cause phase transformation and structural damage to the MnO2 active material; secondly, under solvent-free conditions, it is difficult to simultaneously ensure the dispersibility of the active material, the flexibility of the membrane electrode, and the permeability of ion transport channels, and the prepared membrane electrodes often suffer from problems such as high brittleness, easy cracking, and hindered ion diffusion after compaction.

[0005] Hydrothermally induced ε-MnO2@SCNT-c from carboxylated single-walled carbon nanotubes (SCNT-c) was used as the active material, with polytetrafluoroethylene (PTFE) emulsion and polydimethylsiloxane (PDMS) as the mixed binders. Through the fibrillation effect of PTFE, the prepared film exhibits a three-dimensional interconnected network, eliminating the need for solvent mixing and current collector coating, which is beneficial for the efficient transport of Zn ions in the electrolyte. PDMS facilitates the fibrillation and curing of the mixture at low temperatures, effectively reducing electrode fabrication costs and preventing powder shedding at high temperatures, thus further enhancing the electrode structural stability. Simultaneously, the compaction thickness of the self-supporting film electrode is controllable, preventing drying cracking and making it suitable for gel-type or all-solid-state electrolytes. Single-walled carbon nanotubes (SCNTs) possess a single-layer outer wall structure, exhibiting ultra-high conductivity and a large specific surface area. After SCNT carboxylation (-COOH), it can coordinate with α-MnO2 during hydrothermal processes, forming an interfacial Mn-OC electron bridge. The -COOH group can continuously supply protons to lower the local pH. Simultaneously, the single-channel α-MnO2 evolves into the three-dimensional channel elastic crystalline phase ε-MnO2. The synergistic effect of interfacial electronic structure regulation and crystal phase optimization enhances the adsorption / diffusion capacity and electron / ion migration efficiency of the electrolyte, shortening the MnO2 transition time. 3+ The residence time and suppression of Jahn-Teller distortion can effectively enhance the reversibility of the reaction intermediate Zn(MnO4)2 during MnO2 storage, reduce the irreversible dissolution of MnO2, and improve the stability and rate performance of the pseudocapacitive self-supporting membrane electrode structure. Simultaneously, ultra-high capacitance can be achieved based on the excellent double-layer capacitance of SCNT-c. Therefore, the prepared ε-MnO2@SCNT-c can achieve high capacity, high energy density, and long cycling stability.

[0006] Furthermore, while the composite of MnO2 and carbon nanotubes can improve conductivity, existing composite methods generally fail to simultaneously regulate the crystal phase structure and interfacial electronic structure of MnO2. The crystal phase of MnO2 remains predominantly tunnel or layered, limiting its ability to inhibit intrinsic structural degradation and irreversible dissolution. Simultaneously, conventional multi-walled carbon nanotubes have a large number of wall layers, limiting their specific surface area and double-layer contribution. Therefore, how to simultaneously induce the evolution of the MnO2 crystal phase towards an elastic crystal phase and construct electron bridges at the interface during hydrothermal processes using the surface functional groups of carbon nanotubes, and how to match this with low-temperature fibrillation film formation processes, thereby obtaining a self-supporting membrane electrode that balances high capacity, high energy density, and long-term cycling stability, remains a technical challenge in this field. Summary of the Invention

[0007] To address the problems of solvent contamination, solvent residue, and weak interfacial bonding in existing wet electrode processes, and the high fiberization temperature, easy damage to MnO2 active materials, and difficulty in suppressing the degradation and irreversible dissolution of MnO2 crystal phase structure in dry electrode processes, one objective of this invention is to disclose a low-temperature profibrillated membrane electrode preparation method that induces the co-evolution of MnO2 elastic crystal phase and interfacial Mn-OC electron bridge by carboxyl carbon.

[0008] The technical concept of this invention lies in using carboxylated single-walled carbon nanotubes (SCNT-c) as crystal phase inducers, interface building units, and conductive frameworks. Under hydrothermal conditions, the carboxyl groups on their surface continuously supply protons and lower the local pH environment, while simultaneously coordinating with α-MnO2 generated from a manganese source, forming Mn-OC electron bridges at the interface. This induces the evolution of the single-channel α-MnO2 crystal phase into a three-dimensional channel structure with a certain degree of elasticity, ε-MnO2 crystal phase, and constructs Mn-OC electron bridges at the interface between ε-MnO2 and carboxylated single-walled carbon nanotubes. Furthermore, a mixed bonding system is composed of polytetrafluoroethylene emulsion and polymer additives with low-temperature mobility. The reduction of the polymer molecular chain kinetic energy barrier enables low-temperature fibrillation film formation. Through temperature-controlled rolling, rapid cooling, stretching activation, and low-temperature curing, a self-supporting membrane electrode with a three-dimensional interconnected network structure is obtained. The crystal phase evolution, interface electronic structure regulation, and low-temperature fibrillation film formation process work synergistically to achieve high capacity, high energy density, and long-term structural stability. The aforementioned "polymer additive with low-temperature mobility" refers to a polymer with a glass transition temperature (Tg) below room temperature (25°C) or a melting point below 100°C, which retains the segment mobility of the molecular chain under low-temperature conditions and can assist polytetrafluoroethylene in achieving fibrillation at temperatures below 100°C.

[0009] Technical solution

[0010] A method for preparing a low-temperature protofibrous film electrode that induces the co-evolution of the carboxyl carbon-induced MnO2 elastic crystalline phase and the Mn-OC interfacial electron bridge includes the following steps:

[0011] A. Single-walled carbon nanotubes were ultrasonically dispersed in ethanol, centrifuged, and dried to remove impurities, thus obtaining purified single-walled carbon nanotubes. The purified single-walled carbon nanotubes were added to a mixed acid composed of concentrated sulfuric acid and concentrated nitric acid, and refluxed at 70-90℃ for 4-8 hours. After the reaction was completed, the mixture was cooled, diluted with water, centrifuged, washed, and dried to obtain carboxylated single-walled carbon nanotubes SCNT-c.

[0012] B. Dissolve potassium permanganate, manganese chloride tetrahydrate, and nitric acid in deionized water, mix thoroughly, and then add the carboxylated single-walled carbon nanotubes (SCNT-c). Perform a hydrothermal reaction at 130-180℃ for 4-8 hours. After the reaction, cool, centrifuge, wash, and dry to obtain a powder material ε-MnO2@SCNT-c, which is a composite of elastic crystalline phase ε-MnO2 and carboxylated single-walled carbon nanotubes. The mass ratio of carboxylated single-walled carbon nanotubes (SCNT-c) to potassium permanganate is 1:150-1:500, and the amount of carboxylated single-walled carbon nanotubes (SCNT-c) used is 3-12 mg.

[0013] C. Disperse the ε-MnO2@SCNT-c powder material in an organic solvent, sonicate for 30-60 min to form a suspension, then add a binder and a polymer additive with low-temperature mobility, continue sonicating for 30-60 min and stirring for 1-3 h, dry to remove the organic solvent, and obtain a fibrous slurry; wherein, the binder is a polytetrafluoroethylene emulsion, and the polymer additive is one or more of polydimethylsiloxane, perfluoropolyether, polyethylene glycol, polyoxyethylene, trifluoropropylsilane, and diethylsiloxane; based on 100 parts by weight of the ε-MnO2@SCNT-c powder material, the amount of polytetrafluoroethylene emulsion is 60-120 parts by weight, the amount of polymer additive is 4-10 parts by weight, and the amount of organic solvent is 500-2500 parts by weight;

[0014] D. The fiberized slurry is fed into a heated roller press and rolled into a film under the conditions of roller temperature 100-130℃, roller width 80-120mm, and roller pressure 80-130kg. The film thickness is 200-400μm. After film formation, it is rapidly cooled in an ice-water bath or liquid nitrogen environment for 1-10min, and then subjected to stretching activation treatment and low-temperature curing treatment. The stretching activation treatment has a stretching rate of 30-70%, and the low-temperature curing treatment has a temperature of -30~10℃ and a time of 1-12h to obtain the self-supporting film electrode M-ε-MnO2@SCNT-c.

[0015] In a preferred embodiment of the present invention, the SCNT-c can be replaced with carbon nanotubes modified with other functional groups, including but not limited to hydroxylated, aminolated, or sulfonated carbon nanotubes.

[0016] In a preferred embodiment of the present invention, in step A, the volume ratio of concentrated sulfuric acid to concentrated nitric acid in the mixed acid is 1:1-3:1, the reflux temperature is 70°C, and the reflux time is 5 hours; the dilution with water involves pouring the reaction solution into 8-12 times its volume of cold water for dilution; the washing involves alternating centrifugation with deionized water and ethanol; and the drying involves drying at 60°C for 12 hours.

[0017] In a preferred embodiment of the present invention, in step B, the temperature of the hydrothermal reaction is 150°C, the time of the hydrothermal reaction is 5 hours, the mass ratio of the carboxylated single-walled carbon nanotubes (SCNT-c) to potassium permanganate is 1:200-1:250, and the amount of carboxylated single-walled carbon nanotubes (SCNT-c) used is 6 mg.

[0018] In a preferred embodiment of the present invention, in step C, the organic solvent is one or more of anhydrous ethanol, isopropanol, and N-methylpyrrolidone; and the polymer additive is polydimethylsiloxane.

[0019] More preferably, the organic solvent is a mixture of anhydrous ethanol and isopropanol in a volume ratio of 1:1 to 2:1.

[0020] In a preferred embodiment of the present invention, in step D, the temperature of the roll is 100-125℃, the roll width is 80-120mm, the inter-roll pressure is 80-110kg, the film thickness is 200-300μm, the quenching time is 5min, the elongation is 30-60%, and the low-temperature curing temperature is -30 to -15℃ and the time is 6-10h.

[0021] The second objective of this invention is to provide a self-supporting membrane electrode M-ε-MnO2@SCNT-c prepared by the above-described method. This self-supporting membrane electrode comprises an elastic crystalline phase ε-MnO2, carboxylated single-walled carbon nanotubes, polytetrafluoroethylene (PTFE), and a polymer additive with low-temperature mobility. The elastic crystalline phase ε-MnO2 and the carboxylated single-walled carbon nanotubes interweave to form a three-dimensional interconnected network structure. The elastic crystalline phase ε-MnO2 is formed from a single-channel crystalline phase α-MnO2 through hydrothermal evolution induced by the carboxyl groups of the carboxylated single-walled carbon nanotubes. An interface Mn-OC electron bridge is formed between the elastic crystalline phase ε-MnO2 and the carboxylated single-walled carbon nanotubes. The electrode size can be arbitrarily cut according to actual needs.

[0022] Using PTFE emulsion and PDMS as a mixed binder, low-temperature (<100℃) fibrillation film formation is achieved by lowering the molecular chain motion energy barrier. The dry process effectively avoids the bottlenecks of current collector surface active material easy detachment, poor stability and dispersibility in electrodes prepared by wet process. The prepared membrane electrode exhibits a well-developed pore structure and has ultra-high specific surface area and ion transport capability.

[0023] The third objective of this invention is to apply the prepared M-ε-MnO2@SCNT-c membrane electrode to an aqueous zinc ion hybrid capacitor, that is, to use it as the positive electrode and assemble it with a zinc negative electrode, a separator and an aqueous electrolyte containing ZnSO4 and MnSO4 to form an aqueous zinc ion hybrid capacitor.

[0024] Specifically, the prepared M-ε-MnO2@SCNT-c film electrode was used as the positive electrode, with 0.5 mol L... -1 ZnSO4 and 0.2 mol L -1 MnSO4 is mixed at a volume ratio of 1:0.2 as the electrolyte solution, Zn sheet is used as the negative electrode, and glass fiber is used as the diaphragm to assemble a zinc ion mixed capacitor. The voltage window of the aqueous zinc ion mixed capacitor is 0.8-1.8V.

[0025] Capacity performance and cycle stability were tested using a Newway battery testing system and electrochemical workstation within a voltage window of 0.8-1.8V. Simultaneously, current densities of 0.1, 0.2, 0.5, 1.0, 2.0, 3.0, and 4.0 Ag were used for capacity performance testing. -1 Cyclic stability at a current density of 1.0 A g -1 Under these conditions, 2400 cycles were performed, and the rate performance and structural stability were evaluated in conjunction with capacity performance testing.

[0026] The M-ε-MnO2@SCNT-c self-supporting film material prepared in this invention was subjected to structural and performance analysis using instruments such as field emission scanning electron microscopy (SEM), X-ray diffraction (XRD), transmission electron microscopy (TEM), Xinwei Battery Testing System, and electrochemical workstation to evaluate its electrochemical activity.

[0027] Beneficial effects

[0028] This invention utilizes the carboxyl groups on the surface of carboxylated single-walled carbon nanotubes as proton donors and coordinating groups. During hydrothermal processes, these groups continuously supply protons and lower the local pH environment, causing the single-channel α-MnO2 phase to evolve into a three-dimensional channel structure with elasticity, ε-MnO2. This elastic crystalline structure is beneficial for enhancing Zn content. 2+ The diffusion efficiency and reversible storage capacity are improved, and the lattice distortion caused by volume expansion during charging and discharging is effectively mitigated. Carboxylated single-walled carbon nanotubes coordinate with α-MnO2 during hydrothermal processes, forming a Mn-OC electron bridge at the interface between ε-MnO2 and carbon nanotubes. This interfacial electron bridge can optimize the surface electronic structure of the material and weaken the interaction between MnO and Zn. 2+ Coordination between Mn significantly improves electron migration efficiency; the synergistic effect of crystal phase evolution and interface electronic structure regulation shortens the Mn transition time. 3+The residence time is extended and Jahn-Teller distortion is suppressed, thereby enhancing the reversibility of reaction intermediates, reducing the irreversible dissolution of MnO2, and enhancing the mass-capacitance properties. Carboxylated single-walled carbon nanotubes have a single-layer outer wall structure and a carboxylated surface, possessing excellent conductivity, electrolyte ion adsorption capacity, and double-layer capacitance contribution. Together with the mass-capacitance contribution of ε-MnO2, they enable the membrane electrode to obtain high specific capacity and high energy density. Using polytetrafluoroethylene emulsion and polymer additives with low-temperature mobility (such as polydimethylsiloxane) as a mixed binder system, low-temperature fibrillation film formation is achieved by reducing the kinetic energy barrier of polymer molecular chains. The film formation process does not require current collector coating, and the compaction thickness of the prepared membrane electrode is controllable, avoiding drying cracking and high-temperature powder shedding. The flexibility and structural stability of the membrane electrode are significantly improved, and it is suitable for gel electrolytes or all-solid-state electrolyte systems. Attached Figure Description

[0029] Figure 1 Photographs and cross-sectional scanning electron microscope (SEM) images of the M-ε-MnO2@SCNT-c self-supporting film electrode prepared in Example 1;

[0030] Figure 2 Transmission electron microscopy (TEM) images of α-MnO2 prepared in Example 1 evolving into ε-MnO2@SCNT-c, with α-MnO2 on the left and ε-MnO2@SCNT-c on the right;

[0031] Figure 3 X-ray diffraction (XRD) patterns of α-MnO2 and ε-MnO2@SCNT-c prepared in Example 1 are shown in the figure, along with the standard diffraction cards for ε-MnO2 (JCPDS 30-0820) and α-MnO2 (JCPDS 44-0141).

[0032] Figure 4 The hybrid zinc-ion capacitors assembled from the self-supported film electrodes M-α-MnO2, M-ε-MnO2@SCNT, M-ε-MnO2@MCNT-c, and M-ε-MnO2@SCNT-c prepared in Example 1, under different current densities (0.1, 0.2, 0.5, 1.0, 2.0, 3.0, 4.0 A g), showed performance at different current densities. -1 Capacity and rate performance analysis curves;

[0033] Figure 5 The power density-energy density comparison curve of the hybrid zinc-ion capacitor assembled by the M-α-MnO2 and Mε-MnO2@SCNT-c self-supporting film electrodes prepared in Example 1 is shown.

[0034] Figure 6The hybrid zinc-ion capacitor assembled from the self-supporting film electrodes M-α-MnO2, M-ε-MnO2@SCNT, M-ε-MnO2@MCNT-c, and M-ε-MnO2@SCNT-c prepared in Example 1, at a current density of 1.0 A g... -1 Curves showing the relationship between long-cycle operation and capacity / coulombic efficiency under certain conditions;

[0035] The M mentioned above represents a membrane electrode prepared using the prepared powder active material. Detailed Implementation

[0036] The present invention will be described in detail below with reference to embodiments, so that those skilled in the art can better understand the present invention, but the present invention is not limited to the following embodiments.

[0037] All reactants and reagents used in this invention are commercially available, including potassium permanganate (KMnO4), manganese chloride tetrahydrate (MnCl2·4H2O), single-walled carbon nanotubes (CNTs), multi-walled carbon nanotubes (MCNTs), concentrated sulfuric acid (H2SO4), concentrated nitric acid (HNO3), ethanol (C2H6O), isopropanol, N-methylpyrrolidone, polytetrafluoroethylene (PTFE), polydimethylsiloxane (PDMS), perfluoropolyether (PFPE), polyethylene glycol (PEG), polyethylene oxide (PEO), trifluoropropylsilane (TFPS), and diethylsiloxane (DESD). Both single-walled and multi-walled carbon nanotubes can be commercially available products, or the carboxylated products can be prepared by the mixed acid oxidation method described in this invention.

[0038] The SCNT-c and MCNT-c described in this invention can be commercially available or homemade. The homemade method includes: weighing 100 mg of carbon nanotubes and adding them to 50 mL of ethanol solution, ultrasonically dispersing for 30 minutes, centrifuging, and drying in a forced-air drying oven at 60 °C for 2 hours to obtain carbon nanotubes with impurities removed; then measuring concentrated H2SO4 (90 mL): concentrated HNO3 (30 mL) = 3:1 (volume ratio), pouring the mixed acid into a three-necked flask pre-cooled in an ice-water bath, and magnetically stirring for 30 minutes; slowly adding the treated nanotubes into the mixed acid, refluxing in an oil bath at 70 °C for 5 hours under continuous stirring, cooling, diluting with 500 mL of cold water, centrifuging, and drying at 60 °C for 12 hours to obtain high-purity carboxylated carbon nanotubes (SCNT-c, MCNT-c), wherein the single-walled carbon nanotubes (SCNT) and multi-walled carbon nanotubes (MCNT) used are commercially available.

[0039] Example 1

[0040] A method for preparing a low-temperature fibrillated film electrode with carboxylated single-walled CNT-induced MnO2 elastic crystalline phase and Mn-OC interfacial electron bridge includes the following steps:

[0041] Step 1: Weigh 100 mg of single-walled carbon nanotubes (SCNTs) and add them to 50 mL of ethanol solution. Disperse by sonication for 30 minutes, centrifuge, and then dry in a forced-air drying oven at 60 °C for 2 hours to obtain impurity-free single-walled CNTs. Then, measure concentrated H₂SO₄ (90 mL): concentrated HNO₃ (30 mL) = 3:1 (volume ratio), pour the mixed acid into a three-necked flask pre-cooled in an ice-water bath, and stir magnetically for 30 minutes. Slowly add the treated single-walled CNTs to the mixed acid, reflux in an oil bath at 70 °C for 5 hours with continuous stirring, cool, dilute with 500 mL of cold water, centrifuge, and dry at 60 °C for 12 hours to obtain high-purity carboxylated single-walled SCNT-c. Carboxylated multi-walled carbon nanotubes (MCNT-c) were prepared using the same method for comparative analysis.

[0042] Step 2: Weigh 1.25g KMnO4, 1.6g MnCl2·4H2O and 0.8 mL HNO3 and dissolve them in 40 mL deionized water. After uniform mixing, transfer the mixture to a 50 mL high-temperature reactor liner. At the same time, add 6 mg of the SCNT-c prepared above. Perform hydrothermal reaction at 150℃ for 5 hours. After the reaction is completed, cool to room temperature and wash 10 times each with deionized water and ethanol by alternating centrifugation. Dry in a forced-air drying oven at 60℃ for 12 hours to obtain ε-MnO2@SCNT-c powder. In the same way, adjust the type of carbon nanotubes added or not add carbon nanotubes to prepare α-MnO2, ε-MnO2@SCNT, and ε-MnO2@MCNT-c.

[0043] Step 3: Add 30 mg of ε-MnO2@SCNT-c powder to 5 mL of anhydrous ethanol and isopropanol (volume ratio 1:1), sonicate for 25 minutes to form a uniform suspension, then add 24 mg of polytetrafluoroethylene (PTFE) emulsion and 2 mg of polydimethylsiloxane (PDMS) with low-temperature mobility, continue sonicating for 40 min, finally magnetically stir for 2 h, dry at 60 °C for 7 h to remove anhydrous ethanol and isopropanol, and obtain black fibrous pulp;

[0044] Step 4: Place the fiberized slurry into the feed inlet of an electric heated roller press, roll it evenly to form a film. The roller temperature is 120℃, the roller width is 100mm, the roller pressure is 100kg, and the film thickness is 200μm. Transfer it to an ice-water bath for rapid cooling for 5 minutes, and then perform stretching activation (stretch rate 30%) and low-temperature curing (-20℃) for 6 hours to prepare a self-supporting film electrode (M-ε-MnO2@SCNT-c).

[0045] For comparative analysis, comparative samples were prepared using the same process: M-α-MnO2, M-ε-MnO2@SCNT, and M-ε-MnO2@MCNT-c.

[0046] Structure and performance analysis of the M-ε-MnO2@SCNT-c self-supporting film electrode material prepared in this embodiment

[0047] like Figure 1 As shown in the figure, M-ε-MnO2@SCNT-c exhibits a stable self-supporting membrane structure (left: actual photograph). Under microscopic conditions, the membrane cross-section shows a three-dimensional network structure (right: cross-sectional SEM image, scale bar 2μm), which contributes to the efficient transport of electrolyte ions and structural stability.

[0048] like Figure 2 As shown in the figure, it can be seen that in the microscopic state, the nanorod-shaped α-MnO2 successfully evolved into the sheet-like ε-MnO2 and was intercalated by SCNT to form a composite structure (the scale bar is 200 nm).

[0049] like Figure 3 As shown in the figure, the characteristic peaks of α-MnO2, ε-MnO2 and SCNT can be seen. The characteristic peaks of ε-MnO2 can be attributed to the (100), (101), (102) and (110) crystal planes, which correspond to the ε-MnO2 standard card JCPDS 30-0820. The characteristic peaks of α-MnO2 correspond to the α-MnO2 standard card JCPDS 44-0141, thus proving the composition and effective synthesis of the electrode material. It should be noted that, by comparing the XRD patterns of ε-MnO2@SCNT-c and α-MnO2, it can be seen that after the addition of carboxylated single-walled carbon nanotubes, the diffraction peaks of α-MnO2 at approximately 12.8° (corresponding to the (110) crystal plane) and approximately 18.1° (corresponding to the (200) crystal plane) at 2θ are significantly weakened or disappear, while the characteristic peaks of ε-MnO2 at approximately 22°, 37°, 42°, and 56° at 2θ appear and are enhanced, further confirming the phase transformation from α-MnO2 to ε-MnO2. In addition, the XRD pattern of ε-MnO2@SCNT-c shows the diffraction peak of the (002) crystal plane of carbon nanotubes at approximately 26° at 2θ, confirming the presence of carbon nanotubes in the composite powder.

[0050] like Figure 4 As shown, an aqueous zinc-ion hybrid capacitor assembled using the M-ε-MnO2@SCNT-c self-supporting film electrode prepared in this embodiment as the positive electrode was tested at different current densities (0.1, 0.2, 0.5, 1.0, 2.0, 3.0, 4.0 A g). -1 Under these conditions, the capacity reaches a maximum of 482.8 mAh g. -1 Comparative analysis shows that its capacitance performance is far superior to that of aqueous zinc-ion hybrid capacitors assembled from M-α-MnO2, M-ε-MnO2@SCNT, and M-ε-MnO2@MCNT-c.

[0051] like Figure 5 As shown, the aqueous zinc-ion hybrid capacitor assembled using the M-ε-MnO2@SCNT-c self-supporting film electrode prepared in this embodiment as the positive electrode can achieve a maximum energy density of 760 Wh / kg. -1 Comparative analysis shows that its energy density is much higher than that of the aqueous zinc ion mixed capacitor assembled by M-α-MnO2.

[0052] like Figure 6 As shown, the cycling stability test results of an aqueous zinc-ion hybrid capacitor assembled using the M-ε-MnO2@SCNT-c self-supporting film electrode prepared in this embodiment as the positive electrode are as follows: at a current density of 1 A g... -1 After 2400 cycles, the capacity retention rate was 80.4%, demonstrating good structural stability. This stability is significantly higher than that of α-MnO2, ε-MnO2@SCNT, and ε-MnO2@MCNT-c.

[0053] Example 2

[0054] A method for preparing a low-temperature protofibrous film electrode that induces the co-evolution of the carboxyl carbon-induced MnO2 elastic crystalline phase and the Mn-OC interfacial electron bridge includes the following steps:

[0055] Step 1: Weigh 90 mg of single-walled carbon nanotubes (SCNTs) and add them to 50 mL of ethanol solution. Disperse by sonication for 30 minutes, centrifuge, and then dry in a forced-air drying oven at 60 °C for 2 hours to obtain impurity-free single-walled CNTs. Then, measure concentrated H₂SO₄ (90 mL): concentrated HNO₃ (30 mL) = 3:1 (volume ratio), pour the mixed acid into a three-necked flask pre-cooled in an ice-water bath, and stir magnetically for 30 minutes. Slowly add the treated single-walled CNTs to the mixed acid, reflux in an oil bath at 70 °C for 5 hours with continuous stirring, cool, dilute with 500 mL of cold water, centrifuge, and dry at 60 °C for 12 hours to obtain high-purity carboxylated single-walled SCNT-c. Carboxylated multi-walled carbon nanotubes (MCNT-c) were prepared using the same method for comparative analysis.

[0056] Step 2: Weigh 1.2g KMnO4, 1.5g MnCl2·4H2O, and 0.8 mL HNO3, dissolve them in 40 mL of deionized water, mix thoroughly, and transfer to a 50 mL high-temperature reactor. Simultaneously add 6 mg of the prepared SCNT-c. Initiate a hydrothermal reaction at 130℃ for 5 hours. After the reaction, cool to room temperature and wash 10 times each with alternating centrifugation using deionized water and ethanol. Dry in a forced-air drying oven at 60℃ for 12 hours to obtain ε-MnO2@SCNT-c powder. Similarly, adjust the type of carbon nanotubes added or omit them to prepare α-MnO2, ε-MnO2@SCNT, and ε-MnO2@MCNT-c.

[0057] Step 3: Add 20 mg of ε-MnO2@SCNT-c powder to 6 mL of anhydrous ethanol and isopropanol (volume ratio 2:1), sonicate for 25 minutes to form a uniform suspension, then add 24 mg of polytetrafluoroethylene (PTFE) emulsion and 2 mg of polydimethylsiloxane (PDMS) with low-temperature mobility, continue sonicating for 30 minutes, finally magnetically stir for 1 hour, dry at 60°C for 7 hours to remove anhydrous ethanol and isopropanol to form a black fibrous slurry;

[0058] Step 4: Place the fiberized slurry into the feed inlet of an electric heated roller press and roll it evenly on the surface of the current collector to form a film. The roller temperature is 100℃, the roller width is 80mm, the roller pressure is 80kg, and the film thickness is 250μm. After film formation, transfer it to an ice-water bath for rapid cooling for 5 minutes. After stretching activation (stretch rate 40%) and low-temperature curing (-30℃) for 7 hours, a self-supporting film electrode (M-ε-MnO2@SCNT-c) is prepared.

[0059] For comparative analysis, comparative samples were prepared using the following process: M-α-MnO2, M-ε-MnO2@SCNT, and M-ε-MnO2@MCNT-c.

[0060] Using the M-ε-MnO2@SCNT-c self-supporting film electrode prepared in this embodiment as the positive electrode, an aqueous zinc-ion hybrid capacitor was assembled at a current density of 0.1 A g. -1 The maximum capacity reaches 480.5mAh g. -1 Its energy density can reach up to 752 Wh / kg. -1 At a current density of 1 A g -1 After 2400 cycles, the capacity retention rate was 80%. Its performance is far superior to M-α-MnO2, M-ε-MnO2@SCNT, and M-ε-MnO2@MCNT-c, proving that the prepared M-ε-MnO2@SCNT-c self-supporting film electrode has excellent charge storage capacity and stability.

[0061] Example 3

[0062] A method for preparing a low-temperature protofibrous film electrode that induces the co-evolution of the carboxyl carbon-induced MnO2 elastic crystalline phase and the Mn-OC interfacial electron bridge includes the following steps:

[0063] Step 1: Weigh 80 mg of single-walled carbon nanotubes (SCNTs) and add them to 50 mL of ethanol solution. Disperse by sonication for 30 minutes, centrifuge, and then dry in a forced-air drying oven at 60 °C for 2 hours to obtain impurity-free single-walled CNTs. Then, measure concentrated H₂SO₄ (80 mL): concentrated HNO₃ (40 mL) = 2:1 (volume ratio), pour the mixed acid into a three-necked flask pre-cooled in an ice-water bath, and stir magnetically for 30 minutes. Slowly add the treated single-walled CNTs to the mixed acid, reflux in an oil bath at 70 °C for 5 hours with continuous stirring, cool, dilute with 500 mL of cold water, centrifuge, and dry at 60 °C for 12 hours to obtain high-purity carboxylated single-walled SCNT-c. Carboxylated multi-walled carbon nanotubes (MCNT-c) were prepared using the same method for comparative analysis.

[0064] Step 2: Weigh 1.3g KMnO4, 1.7g MnCl2·4H2O, and 0.8 mL HNO3, dissolve them in 40 mL of deionized water, mix thoroughly, and transfer to a 50 mL high-temperature reactor. Simultaneously add 6 mg of the prepared SCNT-c. Initiate a hydrothermal reaction at 140℃ for 5 hours. After the reaction, cool to room temperature and wash 10 times each with alternating centrifugation using deionized water and ethanol. Dry in a forced-air drying oven at 60℃ for 12 hours to obtain ε-MnO2@SCNT-c powder. Similarly, adjust the type of carbon nanotubes added or omit them to prepare α-MnO2, ε-MnO2@SCNT, and ε-MnO2@MCNT-c.

[0065] Step 3: Add 25 mg of ε-MnO2@SCNT-c powder to 7 mL of anhydrous ethanol and isopropanol (volume ratio 1:1), sonicate for 25 minutes to form a uniform suspension, then add 24 mg of polytetrafluoroethylene (PTFE) emulsion and 2 mg of polydimethylsiloxane (PDMS) with low-temperature mobility, continue sonicating for 35 minutes, finally magnetically stir for 1.5 h, dry at 60 °C for 7 hours to remove anhydrous ethanol and isopropanol to form a black fibrous slurry;

[0066] Step 4: The fiberized slurry is placed into the feed port of an electric heated roller press and uniformly rolled into a film on the surface of the current collector. The roller temperature is 115℃, the roller width is 110mm, the roller pressure is 105kg, and the film thickness is 300μm. After film formation, it is transferred to an ice-water bath for rapid cooling for 5 minutes. After stretching activation (stretch rate 50%) and low-temperature curing (-25℃) for 8 hours, a self-supporting film electrode (M-ε-MnO2@SCNT-c) is prepared.

[0067] For comparative analysis, comparative samples were prepared using the following process: M-α-MnO2, M-ε-MnO2@SCNT, and M-ε-MnO2@MCNT-c.

[0068] Using the M-ε-MnO2@SCNT-c self-supporting film electrode prepared in this embodiment as the positive electrode, an aqueous zinc-ion hybrid capacitor was assembled at a current density of 0.1 A g. -1 The highest capacity reaches 479.3mAh g. -1 Its energy density can reach up to 750Wh / kg. -1 At a current density of 1 A g -1 At that time, the capacity retention rate was 79.2% after 2400 cycles. Its performance is far superior to M-α-MnO2, M-ε-MnO2@SCNT, and M-ε-MnO2@MCNT-c, proving that the prepared M-ε-MnO2@SCNT-c membrane electrode has outstanding energy output and stability.

[0069] Example 4

[0070] A method for preparing a low-temperature protofibrous film electrode that induces the co-evolution of the carboxyl carbon-induced MnO2 elastic crystalline phase and the Mn-OC interfacial electron bridge includes the following steps:

[0071] Step 1: Weigh 95 mg of single-walled carbon nanotubes (SCNTs) and add them to 50 mL of ethanol solution. Disperse by sonication for 30 minutes, centrifuge, and then dry in a forced-air drying oven at 60 °C for 2 hours to obtain impurity-free single-walled CNTs. Then, measure concentrated H₂SO₄ (90 mL): concentrated HNO₃ (45 mL) = 2:1 (volume ratio), pour the mixed acid into a three-necked flask pre-cooled in an ice-water bath, and stir magnetically for 30 minutes. Slowly add the treated single-walled CNTs to the mixed acid, reflux in an oil bath at 70 °C for 5 hours with continuous stirring, cool, dilute with 500 mL of cold water, centrifuge, and dry at 60 °C for 12 hours to obtain high-purity carboxylated single-walled SCNT-c. Carboxylated multi-walled carbon nanotubes (MCNT-c) were prepared using the same method for comparative analysis.

[0072] Step 2: Weigh 1.4g KMnO4, 1.8g MnCl2·4H2O, and 0.8 mL HNO3, dissolve them in 40 mL of deionized water, mix thoroughly, and transfer to a 50 mL high-temperature reactor. Simultaneously add 6 mg of the prepared SCNT-c. Initiate a hydrothermal reaction at 160℃ for 5 hours. After the reaction, cool to room temperature and wash 10 times each with alternating centrifugation using deionized water and ethanol. Dry in a forced-air drying oven at 60℃ for 12 hours to obtain ε-MnO2@SCNT-c powder. Similarly, adjust the type of carbon nanotubes added or omit them to prepare α-MnO2, ε-MnO2@SCNT, and ε-MnO2@MCNT-c.

[0073] Step 3: Add 35mg of ε-MnO2@SCNT-c powder to 10mL of anhydrous ethanol and isopropanol (volume ratio 1:1), sonicate for 25 minutes to form a uniform suspension, then add 24mg of polytetrafluoroethylene (PTFE) emulsion and 2mg of polydimethylsiloxane (PDMS) with low-temperature mobility, continue sonicating for 50 minutes, finally magnetically stir for 2.5h, dry at 60℃ for 6 hours to remove anhydrous ethanol and isopropanol to form a black fibrous slurry;

[0074] Step 4: The fiberized slurry is placed into the feed port of an electric heated roller press and uniformly rolled into a film on the surface of the current collector. The roller temperature is 125℃, the roller width is 120mm, the roller pressure is 110kg, and the film thickness is 300μm. After film formation, it is transferred to an ice-water bath for rapid cooling for 5 minutes. After stretching activation (stretch rate 60%) and low-temperature curing (-15℃) for 10 hours, a self-supporting film electrode (M-ε-MnO2@SCNT-c) is prepared.

[0075] For comparative analysis, comparative samples were prepared using the following process: M-α-MnO2, M-ε-MnO2@SCNT, and M-ε-MnO2@MCNT-c.

[0076] Using the M-ε-MnO2@SCNT-c self-supporting film electrode prepared in this embodiment as the positive electrode, an aqueous zinc-ion hybrid capacitor was assembled at a current density of 0.1 A g. -1 The highest capacity reaches 481.5mAh g. -1 Its energy density can reach up to 753 Wh / kg. -1 At a current density of 1 A g -1 After 2400 cycles, the capacity retention rate was 79.6%. Its performance is far superior to M-α-MnO2, M-ε-MnO2@SCNT, and M-ε-MnO2@MCNT-c, proving that the prepared M-ε-MnO2@SCNT-c self-supporting film electrode has outstanding energy storage efficiency.

[0077] Example 5

[0078] A method for preparing a low-temperature protofibrous film electrode that induces the co-evolution of the carboxyl carbon-induced MnO2 elastic crystalline phase and the Mn-OC interfacial electron bridge includes the following steps:

[0079] Step 1: Weigh 110 mg of single-walled carbon nanotubes (SCNTs) and add them to 50 mL of ethanol solution. Disperse by sonication for 30 minutes, centrifuge, and then dry in a forced-air drying oven at 60 °C for 2 hours to obtain impurity-free single-walled CNTs. Then, measure concentrated H₂SO₄ (100 mL): concentrated HNO₃ (30 mL) = 2:1 (volume ratio), pour the mixed acid into a three-necked flask pre-cooled in an ice-water bath, and stir magnetically for 30 minutes. Slowly add the treated single-walled CNTs to the mixed acid, reflux in an oil bath at 70 °C for 5 hours with continuous stirring, cool, dilute with 500 mL of cold water, centrifuge, and dry at 60 °C for 12 hours to obtain high-purity carboxylated single-walled SCNT-c. Carboxylated multi-walled carbon nanotubes (MCNT-c) were prepared using the same method for comparative analysis.

[0080] Step 2: Weigh 1.5g KMnO4, 2.0g MnCl2·4H2O, and 0.8 mL HNO3, dissolve them in 40 mL of deionized water, mix thoroughly, and transfer to a 50 mL high-temperature reactor. Simultaneously add 6 mg of the prepared SCNT-c. Initiate a hydrothermal reaction at 170℃ for 5 hours. After the reaction, cool to room temperature and wash 10 times each with alternating centrifugation using deionized water and ethanol. Dry in a forced-air drying oven at 60℃ for 12 hours to obtain ε-MnO2@SCNT-c powder. Similarly, adjust the type of carbon nanotubes added or omit them to prepare α-MnO2, ε-MnO2@SCNT, and ε-MnO2@MCNT-c.

[0081] Step 3: Add 40 mg of ε-MnO2@SCNT-c powder to 20 mL of anhydrous ethanol and isopropanol (volume ratio 2:1), sonicate for 30 minutes to form a uniform suspension, then add 30 mg of polytetrafluoroethylene (PTFE) emulsion and 2 mg of polydimethylsiloxane (PDMS) with low-temperature mobility, continue sonicating for 60 minutes, finally magnetically stir for 3 hours, dry at 60°C for 7 hours to remove anhydrous ethanol and isopropanol to form a black fibrous slurry;

[0082] Step 4: Place the fiberized slurry into the feed inlet of an electric heated roller press and roll it evenly on the surface of the current collector to form a film. The roller temperature is 130℃, the roller width is 120mm, the roller pressure is 130kg, and the film thickness is 400μm. After film formation, transfer it to an ice-water bath for rapid cooling for 5 minutes. After stretching activation (stretch rate 70%) and low-temperature curing (-10℃) for 12 hours, a self-supporting film electrode (M-ε-MnO2@SCNT-c) is prepared.

[0083] For comparative analysis, comparative samples were prepared using the following process: M-α-MnO2, M-ε-MnO2@SCNT, and M-ε-MnO2@MCNT-c.

[0084] An aqueous zinc-ion hybrid capacitor assembled using the M-ε-MnO2@SCNT-c self-supporting film electrode prepared in this embodiment as the positive electrode was tested at a current density of 0.1 A g. -1 The maximum capacity reaches 482mAh g -1 Its energy density can reach up to 758 Wh / kg. -1 At a current density of 1 A g -1 At that time, the capacity retention rate was 78.3% after 2400 cycles. Its performance is much higher than that of M-α-MnO2, M-ε-MnO2@SCNT, and M-ε-MnO2@MCNT-c, proving that the prepared M-ε-MnO2@SCNT-c self-supporting film electrode has outstanding electrochemical performance.

[0085] Comparative Example 1

[0086] Mixed zinc ion capacitors were assembled using uncarboxylated single-walled carbon nanotubes (SCNT), carboxylated multi-walled carbon nanotubes (MCNT-c), and no carbon nanotubes added, respectively, with the rest being the same as in Example 1.

[0087] Results: The maximum capacities of the aqueous zinc ion hybrid capacitors obtained by the three schemes were 249.7, 333.2 and 262 mAh / g, respectively, and the capacity retention rate after 2400 cycles was the highest at only 57.5%.

[0088] Comparative Example 2

[0089] Without adding PDMS, the rest is the same as in Example 1.

[0090] Results: The membrane electrode became more brittle, more prone to fracture under tension, and its cycle stability decreased.

[0091] Comparative Example 3

[0092] Electrodes with the same composition were prepared using a traditional wet process (PVDF+NMP coating).

[0093] Results: The capacity was 227 mAh / g, and the retention rate was 50.2% after 2400 cycles.

[0094] Table 1 lists the electrochemical performance of the M-ε-MnO2@MCNT-c self-supporting membrane electrodes prepared in Examples 1-5 and the electrodes obtained in Comparative Examples 1-3. As can be seen from Table 1, when the process parameters such as the ratio of carboxylated single-walled carbon nanotubes to potassium permanganate, hydrothermal temperature, rolling parameters, and curing conditions vary within the range defined by this invention, the performance of the obtained self-supporting membrane electrodes remains stable, indicating that the technical solution of this invention has a wide process window.

[0095] Table 1. Comparison of electrochemical performance of electrodes prepared in each example and the comparative example.

[0096]

[0097] Note: “—” in the table indicates that no corresponding test data was provided for the comparison scheme; “≤57.5” is the highest capacity retention rate among the three schemes in Comparative Example 1.

[0098] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made using the present invention specification, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.

Claims

1. A method for preparing a low-temperature fibrillated membrane electrode with carboxyl carbon-induced MnO2 elastic crystal phase and interface Mn-O-C electronic bridge synergistic evolution, characterized in that, Includes the following steps: A. Single-walled carbon nanotubes were ultrasonically dispersed in ethanol, centrifuged, and dried to remove impurities, thus obtaining purified single-walled carbon nanotubes. The purified single-walled carbon nanotubes were added to a mixed acid composed of concentrated sulfuric acid and concentrated nitric acid, and refluxed at 70-90℃ for 4-8 hours. After the reaction was completed, the mixture was cooled, diluted with water, centrifuged, washed, and dried to obtain carboxylated single-walled carbon nanotubes SCNT-c. B. Dissolve potassium permanganate, manganese chloride tetrahydrate, and nitric acid in deionized water, mix thoroughly, and then add the carboxylated single-walled carbon nanotubes (SCNT-c). Perform a hydrothermal reaction at 130-180℃ for 4-8 hours. After the reaction, cool, centrifuge, wash, and dry to obtain a powder material ε-MnO2@SCNT-c, which is a composite of elastic crystalline phase ε-MnO2 and carboxylated single-walled carbon nanotubes. The mass ratio of carboxylated single-walled carbon nanotubes (SCNT-c) to potassium permanganate is 1:150-1:500, and the amount of carboxylated single-walled carbon nanotubes (SCNT-c) used is 3-12 mg. C. Disperse the ε-MnO2@SCNT-c powder material in an organic solvent, sonicate for 30-60 min to form a suspension, then add a binder and a polymer additive with low-temperature mobility, continue sonicating for 30-60 min and stirring for 1-3 h, dry to remove the organic solvent, and obtain a fibrous slurry; wherein, the binder is a polytetrafluoroethylene emulsion, and the polymer additive is one or more of polydimethylsiloxane, perfluoropolyether, polyethylene glycol, polyoxyethylene, trifluoropropylsilane, and diethylsiloxane; based on 100 parts by weight of the ε-MnO2@SCNT-c powder material, the amount of polytetrafluoroethylene emulsion is 60-120 parts by weight, the amount of polymer additive is 4-10 parts by weight, and the amount of organic solvent is 500-2500 parts by weight; D. The fiberized slurry is fed into a heated roller press and rolled into a film under the conditions of roller temperature 100-130℃, roller width 80-120mm, and roller pressure 80-130kg. The film thickness is 200-400μm. After film formation, it is rapidly cooled in an ice-water bath or liquid nitrogen environment for 1-10min, and then subjected to stretching activation treatment and low-temperature curing treatment. The stretching activation treatment has a stretching rate of 30-70%, and the low-temperature curing treatment has a temperature of -30~10℃ and a time of 1-12h to obtain the self-supporting film electrode M-ε-MnO2@SCNT-c.

2. The method for preparing a low-temperature protofibrous film electrode based on the co-evolution of carboxyl carbon-induced MnO2 elastic crystalline phase and interfacial Mn-OC electron bridge according to claim 1, characterized in that: In step A, the volume ratio of concentrated sulfuric acid to concentrated nitric acid in the mixed acid is 1:1-3:1, the reflux temperature is 70°C, and the reflux time is 5 hours; the dilution with water involves pouring the reaction solution into 8-12 times its volume of cold water for dilution; the washing involves alternating centrifugation with deionized water and ethanol; and the drying involves drying at 60°C for 12 hours.

3. The method for preparing a low-temperature protofibrous film electrode based on the co-evolution of carboxyl carbon-induced MnO2 elastic crystalline phase and interfacial Mn-OC electron bridge according to claim 1, characterized in that: In step B, the hydrothermal reaction temperature is 150℃, the hydrothermal reaction time is 5h; the mass ratio of carboxylated single-walled carbon nanotubes (SCNT-c) to potassium permanganate is 1:200-1:250; and the amount of carboxylated single-walled carbon nanotubes (SCNT-c) used is 6mg.

4. The method for preparing a low-temperature protofibrous membrane electrode based on the co-evolution of carboxyl carbon-induced MnO2 elastic crystalline phase and interfacial Mn-OC electron bridge according to claim 1, characterized in that: In step C, the organic solvent is one or more of anhydrous ethanol, isopropanol, and N-methylpyrrolidone; the polymer additive is polydimethylsiloxane; preferably, the organic solvent is a mixture of anhydrous ethanol and isopropanol in a volume ratio of 1:1 to 2:

1.

5. The method for preparing a low-temperature protofibrous membrane electrode based on the carboxyl carbon-induced co-evolution of MnO2 elastic crystalline phase and interfacial Mn-OC electron bridge according to claim 1, characterized in that: In step D, the roll temperature is 100-125℃, the roll width is 80-120mm, the inter-roll pressure is 80-110kg, the film thickness is 200-300μm, the quenching time is 5min, the elongation is 30-60%, and the low-temperature curing temperature is -30 to -15℃ and the time is 6-10h.

6. A low-temperature protofibrotic membrane electrode prepared by the method according to any one of claims 1-5, which exhibits synergistic evolution of carboxylated carbon-induced MnO2 elastic crystalline phase and interfacial Mn-OC electron bridge.

7. The low-temperature protofibrous membrane electrode according to claim 6, characterized in that: The device comprises an elastic crystalline phase ε-MnO2, carboxylated single-walled carbon nanotubes, polytetrafluoroethylene, and polymer additives with low-temperature mobility. The elastic crystalline phase ε-MnO2 and the carboxylated single-walled carbon nanotubes intertwine to form a three-dimensional interconnected network structure. The elastic crystalline phase ε-MnO2 is formed from the single-channel crystalline phase α-MnO2 through hydrothermal evolution induced by the carboxyl groups of the carboxylated single-walled carbon nanotubes. An interface Mn-OC electron bridge is formed between the elastic crystalline phase ε-MnO2 and the carboxylated single-walled carbon nanotubes. The electrode size can be arbitrarily cut according to actual needs.

8. The application of a low-temperature protofibrous film electrode with carboxyl carbon-induced MnO2 elastic crystalline phase and interface Mn-OC electron bridge co-evolution as described in claim 6 or 7, characterized in that: Using the electrode as the positive electrode, an aqueous zinc ion mixed capacitor is assembled with a zinc negative electrode, a separator, and an aqueous electrolyte containing ZnSO4 and MnSO4.

9. The application of the low-temperature protofibrous film electrode according to claim 8, characterized in that: The electrolyte is prepared by mixing 0.5 mol L -1 of ZnSO4and 0.2 mol L -1 of MnSO4in a volume ratio of 1:0.

2.

10. The application of the low-temperature protofibrous film electrode according to claim 8, characterized in that: The voltage window of the aqueous zinc ion hybrid capacitor is 0.8-1.8V.