Composite lithium supplementation materials and their preparation methods, cathode sheets, batteries, and electronic devices.
By coating the surface of the lithium-rich compound core with a LiyAlzPO4-xF1+x layer, the problem of lithium-rich compounds readily reacting with air is solved, improving the battery's charging capacity and stability, and extending its lifespan.
Patent Information
- Application Number
- CN202510625980.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-14
- Publication Date
- 2026-11-17
AI Technical Summary
Lithium-rich compounds readily react with H2O and CO2 in the air, leading to reduced electrochemical activity and safety hazards. Existing modified materials have failed to effectively improve the specific capacity of batteries.
A lithium-rich compound core is coated with a LiyAlzPO4-xF1+x coating layer to form a composite lithium replenishment material. The coating layer is calcined in a high-temperature oxygen atmosphere to ensure its stability and lithium-ion conductivity.
It improves the battery's charging capacity and structural stability, reduces side reactions, and extends the battery's lifespan.
Smart Images

Figure CN123120656A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, and in particular to a composite lithium replenishment material and its preparation method, a positive electrode, a battery, and electronic equipment. Background Technology
[0002] Lithium-rich compounds possess high theoretical specific capacity and can be used as positive electrode lithium replenishment materials in lithium-ion batteries to compensate for irreversible capacity loss during the first cycle and improve battery cycle life. However, lithium-rich compounds readily react with H2O and CO2 in the air, which not only reduces their electrochemical activity but also generates residual alkali that can lead to gas production in the battery, posing a safety hazard.
[0003] To address these issues, existing technologies employ methods such as coating and doping to modify lithium-rich compounds, with TiO2 and Li3PO4 being common modifying materials. However, the modified lithium-rich compound materials have not achieved the expected improvement in battery specific capacity. Summary of the Invention
[0004] The first aspect of this invention provides a composite lithium replenishment material with a stable structure, which is beneficial for improving the charging capacity of the battery.
[0005] The second aspect of the present invention provides a method for preparing a composite lithium replenishment material. The composite lithium replenishment material prepared by the method has a stable structure, which is beneficial to improving the charging capacity of the battery.
[0006] A third aspect of the present invention provides a positive electrode sheet, which, since it is made of the above-mentioned composite lithium-replenishing material, is beneficial to improving the charging capacity of the battery.
[0007] A fourth aspect of the present invention provides a battery that, since it is made from the above-mentioned positive electrode sheet, has a high charge capacity.
[0008] The fifth aspect of the present invention provides an electronic device that, since the electronic device is made from the aforementioned battery, has a long standby time.
[0009] The first aspect of this invention provides a composite lithium supplementation material, comprising:
[0010] A lithium-rich compound core and a coating layer covering at least a portion of the surface of the lithium-rich compound core, the coating layer comprising Li y Al z PO 4-x F 1+x Where 0 ≤ x < 4, y > 0, z > 0.
[0011] The composite lithium replenishment material as described above, wherein the lithium-rich compound core comprises a core layer and a transition layer covering at least a portion of the surface of the core layer, the core layer comprising a lithium-rich compound, and the transition layer comprising an element-doped lithium-rich compound, wherein the element comprises at least one of P, Al, and F.
[0012] The composite lithium supplementation material described above, wherein y:z = 1-10:1.
[0013] The composite lithium supplementation material as described above, wherein 0.02≤x≤0.1; and / or 0.5≤y≤3; and / or 0.1≤z≤1.
[0014] In the composite lithium-replenishing material described above, the mass of the coating layer accounts for 0.1-2% of the mass of the lithium-rich compound core; and / or, the thickness of the coating layer is 1-500 nm.
[0015] The composite lithium supplementation material as described above, wherein the Li y Al z PO 4-x F 1+x The particle size Dn50 satisfies: 1nm≤Dn50≤50nm.
[0016] The composite lithium-rich material described above, wherein the element-doped lithium-rich compound has at least one of a layered structure, a rock-salt-like structure, and a spinel-like structure.
[0017] In the composite lithium supplementation material described above, the mass percentage of P element in the transition layer is 0.1-20.8% of the mass of the transition layer; and / or, the mass percentage of Al element in the transition layer is 0.1-18.2% of the mass of the transition layer; and / or, the mass percentage of F element in the transition layer is 0.1-12.8% of the mass of the transition layer.
[0018] In the composite lithium replenishment material described above, the thickness of the transition layer is 2-499 nm.
[0019] The composite lithium-rich material as described above, wherein the lithium-rich compound includes at least one of Li2NiO2, Li6CoO4, and Li5FeO4.
[0020] In the composite lithium supplementation material described above, the particle size Dn50 of the lithium-rich compound satisfies: 500nm≤Dn50≤15μm.
[0021] A second aspect of the present invention provides a method for preparing a composite lithium supplement material, comprising:
[0022] In an oxygen atmosphere, lithium-rich compounds, Li y Al zPO 4-x F 1+x The mixture is calcined to obtain the composite lithium supplement material.
[0023] In the preparation method described above, the lithium-rich compound, Li y Al z PO 4-x F 1+x The mass ratio is 100:0.1-2.
[0024] In the preparation method described above, the calcination temperature is 200-800℃ and the calcination time is 0.5-6h.
[0025] In the preparation method described above, the calcination temperature is 300-600℃ and the calcination time is 2-6h.
[0026] The composite lithium-supplementing material described above, wherein, prior to calcination, further includes: reacting the lithium-rich compound with Li... y Al z PO 4-x F 1+x The solvent is mixed and then spray-dried to obtain the mixture; the spray-drying conditions include:
[0027] The pressure is 0.2-1 MPa; and / or the inlet temperature is 100-300℃; and / or the outlet temperature is 80-100℃; and / or the feed rate is 0.5-2 L / h.
[0028] A third aspect of the present invention provides a positive electrode sheet comprising the above-described composite lithium-replenishing material, or the composite lithium-replenishing material prepared by the above-described preparation method.
[0029] A fourth aspect of the present invention provides a battery comprising the above-described positive electrode.
[0030] A fifth aspect of the present invention provides an electronic device comprising the battery described above.
[0031] The composite lithium-rich material of the present invention comprises a lithium-rich compound core and a coating layer (Li y Al z PO 4-x F 1+x The coating layer not only acts as a physical barrier to isolate water and carbon dioxide from the lithium-rich compound core, but also provides structural stability, suppressing side reactions and ensuring the core's structural stability. Furthermore, the coating layer enables efficient lithium-ion conduction. Therefore, the composite lithium replenishment material of this invention can effectively improve the battery's specific charging capacity. Attached Figure Description
[0032] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.
[0033] Figure 1 This is a schematic diagram of the structure of the composite lithium replenishment material provided in Embodiment 1 of the present invention.
[0034] Figure label:
[0035] 1-Core layer; 2-Transition layer; 3-Covering layer.
[0036] The accompanying drawings have illustrated specific embodiments of this application, which will be described in more detail below. These drawings and descriptions are not intended to limit the scope of the concept in any way, but rather to illustrate the concept of this application to those skilled in the art through reference to specific embodiments. Detailed Implementation
[0037] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some embodiments of this invention, not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0038] Lithium-rich compounds, such as Li₂NiO₂, are suitable as cathode materials for lithium-ion batteries due to their high theoretical capacity ratio. However, Li₂NiO₂ readily reacts with H₂O and CO₂ in the air, reducing its activity. To address this issue, those skilled in the art have modified Li₂NiO₂ using TiO₂ or ZrO₂ through coating or doping. However, test results show that the battery structure made from this modified Li₂NiO₂ material has unsatisfactory stability, and the improvement in battery specific capacity has not met expectations.
[0039] The inventors analyzed that the above reasons are as follows: the Ti and Zr elements in TiO2 or ZrO2 have a high valence state of +4, making it difficult to achieve deep and uniform doping, thus reducing the doping effect. Furthermore, after calcination, TiO2 oxide may have oxygen vacancies, causing Ti to appear in the coating layer. 3+ / Ti 4+ Electron pair oxidation of the electrolyte reduces the stability of the battery system, thus preventing it from achieving the expected results.
[0040] Based on this, the first aspect of the present invention provides a composite lithium replenishment material, such as... Figure 1 As shown, it includes:
[0041] The lithium-rich compound core and the coating layer 3 covering at least a portion of the surface of the lithium-rich compound core, the coating layer 3 comprising Li y Al z PO 4-x F 1+x Where 0 ≤ x < 4, y > 0, z > 0.
[0042] It should be explained that in the composite lithium replenishment material of this invention, the lithium-rich compound core provides active lithium ions to replenish the lithium ions consumed during battery charging and discharging, either through the formation of the SEI film or lithium dendrites. This invention does not limit the selection of the lithium-rich compound core, as long as it can release lithium ions during the first charge.
[0043] The composite lithium replenishment material of this invention can significantly improve the charging capacity of batteries. Besides the coating layer acting as a physical barrier to isolate water and carbon dioxide to a certain extent, the inventors believe the main reason is: firstly, the Li in the coating layer... y Al z PO 4-x F 1+x Lithium has high ionic and electronic conductivity, and can act as a "dual conductor" to improve the interfacial dynamics of lithium-rich transition metal oxides, thereby enhancing lithium-ion transport efficiency and diffusion performance, and thus increasing the battery's charge capacity. On the other hand, Li... y Al z PO 4-x F 1+x Li exhibits strong chemical stability and a low probability of side reactions with water and carbon dioxide, significantly reducing the formation of residual alkali, avoiding electrolyte side reactions, and lowering the lithium demand for SEI film reconstruction in the system. This allows more lithium ions to participate in the insertion / extraction of the positive and negative electrodes. Furthermore, the suitable ionic radii and low valence states of the P, Al, and F elements in the coating layer may contribute to the high lithium content of the coating. y Al z PO 4-x F 1+x It is easier to coat the surface of lithium-rich transition metal oxides, thus making the connection between the lithium-rich transition metal oxides and the coating layer more stable, extending the lifespan of the coating structure, and thus enabling a more long-lasting and significant coating effect. This further improves the stability and electronic and ionic conductivity of the composite lithium replenishment material. Therefore, this composite lithium replenishment material has both good structural stability and electronic and ionic conductivity, thereby further improving the battery's charging capacity and stability.
[0044] In one specific implementation, such as Figure 1As shown, the lithium-rich compound core includes a core layer 1 and a transition layer 2 covering at least a portion of the surface of the core layer 1. The core layer 1 includes a lithium-rich compound, and the transition layer 2 includes an element-doped lithium-rich compound, wherein the element includes at least one of P, Al, and F.
[0045] like Figure 1 As shown, the composite lithium replenishment material comprises, from the inside out, a core layer 1, a transition layer 2, and a coating layer 3. The core layer is a lithium-rich compound; the coating layer is Li. y Al z PO 4-x F 1+x The transition layer is formed when at least one of the P, Al, and F elements provided in the coating layer enters the lithium-rich compound. Because the P, Al, and F elements in the coating layer have suitable ionic radii and low valence states, they are more easily incorporated into the bulk phase of the lithium-rich compound core, resulting in a higher and more uniform doping depth. This leads to a transition layer with good structural stability and minimal impact on the theoretical capacity of the lithium-rich compound, further enhancing the structural stability and lithium replenishment performance of the composite lithium replenishment material.
[0046] In one specific embodiment, y:z = 1-10:1. At this ratio, the doping effect of P, Al, and F elements is better, the transition layer is more stable, and the composite lithium replenishment material has stronger chemical stability and better ionic and electronic conductivity, thereby further improving the specific charging capacity of the battery.
[0047] For example, y:z = 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1, or a range consisting of any two of these values.
[0048] In one specific implementation, 0.02 ≤ x ≤ 0.1. By controlling the range of values for x, the amount of F element replacing O element can be controlled, thereby allowing Li... y Al z PO 4-x F 1+x It has a stronger ability to conduct electrons and ions.
[0049] For example, x is 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09 or 0.1, or a range of any two of these values.
[0050] In one specific implementation, 0.5 ≤ y ≤ 3. Within this range, Li... y Al z PO 4-x F 1+x The structure is more stable.
[0051] For example, y can be 0.5, 1, 1.5, 2, 2.5 or 3, or a range of any two of these values.
[0052] In one specific implementation, 0.1 ≤ z ≤ 1. Within this range, Li y Al z PO 4-x F 1+x The structure is more stable.
[0053] For example, z can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 1, or a range of any two of these values.
[0054] When the following conditions are met simultaneously: 0.02≤x≤0.1, 0.5≤y≤3, and 0.1≤z≤1, Li y Al z PO 4-x F 1+x It has the best electron-ion conduction ability.
[0055] In one specific implementation, such as Figure 1 As shown, the mass of the coating layer 3 accounts for 0.1-2% of the mass of the lithium-rich compound core. Within this range, it is more conducive to the efficient transport of lithium ions in the lithium-rich compound.
[0056] For example, the mass of the coating layer accounts for 0.1%, 0.7%, 0.9%, 1.1%, 1.3%, 1.5%, 1.7%, 1.9% or 2% of the mass of the lithium-rich compound core, or a range of any two of these values.
[0057] In one specific implementation, such as Figure 1 As shown, the thickness of the coating layer 3 is 1-500 nm. Within this range, the impedance is lower and the lithium-ion transport efficiency is higher.
[0058] For example, the thickness of the coating layer is 1 nm, 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm or 500 nm, or a range of any two of these values.
[0059] In one specific implementation, Li y Al z PO 4-x F 1+x The particle size Dn50 satisfies: 1nm ≤ Dn50 ≤ 50nm. Within this range, the coating layer can more uniformly and completely coat the core layer.
[0060] For example, Li y Alz PO 4-x F 1+x The particle size Dn50 is 1nm, 2nm, 5nm, 10nm, 20nm, 30nm, 40nm or 50nm, or a range of any two of these values.
[0061] In one specific implementation, such as Figure 1 As shown, transition layer 2, i.e., the element-doped lithium-rich compound, has at least one of the following structures: layered structure, rock-salt-like structure, and spinel-like structure. The rock-salt-like structure includes a disordered rock-salt-like structure. The structure of the transition layer is determined by the specific structure of the core layer; different core layers (lithium-rich compounds) result in different transition layer structures. The crystal phase structure described above is more stable, less prone to collapse, and more conducive to lithium-ion conduction, thus having a more significant effect on improving the battery's specific capacity.
[0062] In one specific implementation, such as Figure 1 As shown, the mass of element P in transition layer 2 accounts for 0.1-20.8% of the mass of transition layer 2. For example, the mass of element P in the transition layer accounts for 0.1%, 0.5%, 0.8%, 12.5%, 14.6%, 15.8% or 20.8% of the mass of the transition layer, or a range consisting of any two of these values.
[0063] In one specific embodiment, the mass of Al element in transition layer 2 accounts for 0.1-18.2% of the mass of transition layer 2. Exemplarily, the mass of Al element in transition layer accounts for 0.1%, 4.2%, 9.3%, 13.6%, 15.5%, 17.3% or 18.2% of the mass of transition layer, or a range consisting of any two of these values.
[0064] In one specific embodiment, the mass of element F in transition layer 2 accounts for 0.1-12.8% of the mass of transition layer 2. Exemplarily, the mass of element F in the transition layer accounts for 0.1%, 0.4%, 0.7%, 1.8%, 3.2%, 6.4%, 9.3%, or 12.8% of the mass of the transition layer, or a range consisting of any two of these values.
[0065] When the mass contents of P, Al, and F elements in the transition layer are all within the above ranges, the stability of the transition layer is better.
[0066] In one specific implementation, such as Figure 1 As shown, the thickness of transition layer 2 is 2-499 nm. Within this range, the thickness of the transition layer can further reduce the interface impedance, ensure higher utilization of lithium ions released from the core layer, and have little impact on the theoretical capacity of lithium-rich compounds.
[0067] For example, the thickness of the transition layer is 2nm, 50nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm or 499nm, or a range of any two of these values.
[0068] In one specific embodiment, the lithium-rich compound includes at least one of Li2NiO2, Li6CoO4, and Li5FeO4.
[0069] Specifically, when the core layer is Li2NiO2, Li5FeO4, or a mixture of Li2NiO2 and Li5FeO4, it is conducive to the formation of a disordered rock-salt-like phase structure doped with P, Al, and F in the transition layer; when the core layer is Li6CoO4, it is conducive to the formation of a mixed disordered structure of layered structure, rock-salt-like structure, and spinel-like structure doped with P, Al, and F in the transition layer.
[0070] In one specific embodiment, the particle size Dn50 of the lithium-rich compound satisfies: 500 nm ≤ Dn50 ≤ 15 μm. Within this range, the diffusion path of lithium ions is shortened, the diffusion efficiency is improved, thereby improving the specific charge capacity of the battery.
[0071] For example, the particle size Dn50 of the lithium-rich compound is 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1 μm, 3 μm, 6 μm, 9 μm, 12 μm or 15 μm, or a range of any two of these values.
[0072] In this embodiment of the invention, particle size Dn50 (or Dn50) is the median particle size of the material, that is, in the particle sample, 50% of the particles have a particle size less than or equal to this value, and the other 50% of the particles have a particle size greater than this value.
[0073] A second aspect of the present invention provides a method for preparing the composite lithium-supplementing material of the first aspect, comprising:
[0074] In an oxygen atmosphere, lithium-rich compounds, Li y Al z PO 4-x F 1+x The mixture is calcined to obtain a composite lithium supplement material.
[0075] It should be noted that the oxygen atmosphere in this invention refers to a pure oxygen atmosphere. Calcination in this invention is performed under an oxygen atmosphere to avoid the formation of oxygen vacancies, thereby improving the performance of the composite lithium-supplementing material. Calcination of the above mixture can enhance the performance of Li-... y Al z PO 4-x F 1+xBy coating the surface of lithium-rich compounds, a composite lithium supplement material is obtained.
[0076] This invention does not specifically limit the calcination temperature and time, as long as it can reduce the temperature of Li y Al z PO 4-x F 1+x It can be coated onto the surface of lithium-rich compounds.
[0077] This invention relates to lithium-rich compounds, Li y Al z PO 4-x F 1+x The source is not specifically limited; any product prepared using commercially available products or conventional preparation methods known to those skilled in the art is acceptable.
[0078] The present invention does not specifically limit the equipment used for calcination. In one embodiment, a sintering furnace is used.
[0079] In one specific embodiment, lithium-rich compounds, Li y Al z PO 4-x F 1+x The mass ratio is 100:0.1-2. Within this mass ratio range, lithium-ion transport in lithium-rich compounds becomes more efficient.
[0080] The resulting composite lithium supplement material exhibits better structural stability and ionic and electronic conductivity.
[0081] For example, lithium-rich compounds, Li y Al z PO 4-x F 1+x The mass ratio is 100:0.1, 100:0.5, 100:1, 100:1.5 or 100:2, or a range of any two of these values.
[0082] To improve the stability of the resulting composite lithium supplement material, the calcination temperature and time were further controlled.
[0083] In one specific embodiment, the calcination temperature is 200-800℃, and the calcination time is 0.5-6 hours. Within this calcination temperature and time range, the obtained composite lithium-supplementing material exhibits better stability.
[0084] For example, the calcination temperature is 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, or 800°C, or a range of any two of these values.
[0085] For example, the calcination time is 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h, or a range of any two of these values.
[0086] Preferably, the calcination temperature is 300-600℃, and the calcination time is 2-6 hours. Within this calcination time and temperature range, the prepared composite lithium replenishment material exhibits good structural stability and electronic and ionic conductivity, thereby further improving the specific charging capacity of the battery.
[0087] In one specific embodiment, prior to calcination, the process further includes: reacting a lithium-rich compound with Li... y Al z PO 4-x F 1+x After mixing with solvent, the mixture is spray-dried to obtain a mixture; the spray-drying conditions include at least one of the following:
[0088] In one embodiment, the spray drying pressure is 0.2-1 MPa. Within this pressure range, a uniform pre-coating layer can be achieved.
[0089] In one embodiment, the inlet air temperature for spray drying is 100-300°C. Within this temperature range, the drying rate of each raw material is increased.
[0090] In one embodiment, the outlet temperature of the spray dryer is 80-100°C. This outlet temperature range further ensures more thorough drying of the raw materials.
[0091] In one embodiment, the feed rate for spray drying is 0.5-2 L / h. Within this range, the efficiency of spray drying is higher.
[0092] When the above-mentioned spray drying pressure, inlet air temperature, outlet air temperature, and feed rate are simultaneously satisfied, the spray drying method is as follows:
[0093] In a protective atmosphere, lithium-rich compounds and Li y Al z PO 4-x F 1+x The mixture is dispersed in a solvent and spray-dried; the protective atmosphere pressure is 0.2-1 MPa, the inlet temperature is 100-300℃, the outlet temperature is 80-100℃, and the feed rate is 0.5-2 L / h. First, lithium-rich compounds and Li... y Al z PO 4-x F 1+x Spray drying is performed to ensure that the coating layer covers the core layer more evenly and completely after calcination.
[0094] For example, the protective atmosphere pressure is 0.2 MPa, 0.3 MPa, 0.4 MPa, 0.5 MPa, 0.6 MPa, 0.7 MPa, 0.9 MPa, or 1 MPa, or a range of any two of these values.
[0095] For example, the intake temperature is 100°C, 130°C, 160°C, 190°C, 210°C, 240°C, 270°C, or 300°C, or a range of any two of these values.
[0096] For example, the outlet temperature is 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C, 98°C or 100°C, or a range of any two of these values.
[0097] For example, the feed rate is 0.5L / h, 0.7L / h, 0.9L / h, 1.1L / h, 1.3L / h, 1.5L / h, 1.7L / h, 1.9L / h or 2L / h, or a range of any two of these values.
[0098] The present invention does not specifically limit the type of protective atmosphere; for example, it can be an inert atmosphere.
[0099] This invention is effective for dispersing lithium-rich compounds, Li y Al z PO 4-x F 1+x The solvent is not specifically limited. In one embodiment, the solvent includes at least one of N-methylpyrrolidone (NMP), ethanol, isopropanol, and ethylene glycol dimethyl ether.
[0100] The present invention does not specifically limit the equipment used for spray drying. In one embodiment, a spray dryer is used.
[0101] A third aspect of the present invention provides a positive electrode sheet comprising the composite lithium replenishing material of the first aspect above, or the composite lithium replenishing material prepared by the preparation method of the second aspect.
[0102] The positive electrode sheet of the present invention specifically includes a positive current collector and a positive active layer formed of a positive active material (the composite lithium supplementation material of the present invention) disposed on the surface of the positive current collector.
[0103] In the specific preparation of the positive electrode sheet, for example, the composite lithium-supplementing material of the present invention can be dispersed with a conductive agent and a binder in an appropriate amount of N-methylpyrrolidone (NMP) solvent, and thoroughly stirred and mixed to form a uniform positive electrode slurry; the positive electrode slurry is uniformly coated on the positive electrode current collector, and after drying, rolling and slitting, the positive electrode sheet is obtained. In one specific embodiment, the positive electrode active layer comprises, by weight percentage, 70-99 wt% of positive electrode active material, 0.5-15 wt% of conductive agent, and 0.5-15 wt% of binder, and further comprises 80-98 wt% of positive electrode active material, 1-10 wt% of conductive agent, and 1-10 wt% of binder.
[0104] The positive electrode current collector can be made of at least one of aluminum foil and nickel foil; the conductive agent can be made of at least one of carbon black, acetylene black, graphene, Ketjen black, and carbon fiber; and the binder can be made of at least one of polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl fluoride, polyethylene, polypropylene, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, ethylene oxide-containing polymers, polyvinylpyrrolidone, and polyurethane.
[0105] A fourth aspect of the present invention provides a battery comprising the above-described positive electrode.
[0106] In addition to the aforementioned positive electrode, the battery of this invention also includes a negative electrode, a separator, and an electrolyte. The following example uses a lithium-ion battery preparation method:
[0107] This invention does not strictly limit the negative electrode active material in the negative electrode sheet. It can be at least one of the negative electrode active materials commonly used in lithium-ion batteries, such as graphite, hard carbon, soft carbon, mesophase carbon microspheres, silicon-based negative electrode materials (mainly including silicon suboxide and silicon-carbon negative electrode), and tin-based negative electrode materials (mainly including tin and tin alloy).
[0108] This invention does not strictly limit the choice of electrolyte, and may include one or more of the solvents commonly used in lithium-ion battery electrolytes, as well as the electrolyte lithium salts commonly used in lithium-ion electrolytes. For example, the solvent may be one or more of ethylene carbonate, propylene carbonate, butene carbonate, fluoroethylene carbonate (FEC), dimethyl carbonate (DMC), diethyl carbonate (DEC), difluoroethylene carbonate (DFEC), dipropyl carbonate, methyl ethyl carbonate (EMC), ethyl acetate, ethyl propionate, propyl acetate, propyl propionate, sulfolane, and γ-butyrolactone; the lithium salt may be one or more of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).
[0109] This invention does not strictly limit the choice of separator material. It can be one of the separator materials commonly used in lithium-ion batteries, such as polypropylene separator (PP), polyethylene separator (PE), polypropylene / polyethylene double-layer composite membrane (PP / PE), polyimide electrospun separator (PI), polypropylene / polyethylene / polypropylene triple-layer composite membrane (PP / PE / PP), cellulose nonwoven separator, and separator with ceramic coating.
[0110] In the preparation of lithium-ion batteries, the positive electrode, separator, and negative electrode are wound or stacked to obtain a bare cell, which is then packaged into a pre-stamped aluminum-plastic film bag. After the packaged battery is dried at 85°C, the electrolyte is injected into the dried battery. The battery undergoes resting, formation, and secondary sealing to complete the preparation of the lithium-ion battery.
[0111] The battery of this application may be in the form of a battery cell, a battery module, or a battery pack. In some embodiments, battery cells may be assembled into a battery module, and the number of battery cells contained in a battery module may be one or more, the specific number of which can be selected by those skilled in the art based on the application and capacity of the battery module. In some embodiments, battery modules may also be assembled into a battery pack, and the number of battery modules contained in a battery pack may be one or more, the specific number of which can be selected by those skilled in the art based on the application and capacity of the battery pack.
[0112] The specific type of battery described in this application is not particularly limited. For example, from a shape perspective, the battery includes, but is not limited to, prismatic batteries, pouch batteries, and cylindrical batteries, etc., and this application does not impose any particular restrictions. From the perspective of the core structure, the battery core can be a wound core (i.e., a core formed by stacking positive electrode sheets, negative electrode sheets, and separators and then winding them) or a stacked core (i.e., multiple positive electrode sheets, negative electrode sheets, and separators are stacked to form a core). The outer casing can be a hard casing (such as a steel casing, a hard plastic casing, etc.) or a soft casing (such as an aluminum-plastic film casing, a pouch-type soft casing, etc.), etc., and this application does not impose any particular restrictions.
[0113] A fifth aspect of this invention provides an electronic device comprising the battery described in the fourth aspect. This electronic device has the advantage of a long standby time. The electronic device provided by this invention can be any conventional electrical device in the art, such as power equipment (e.g., electric vehicles), electrical devices (e.g., mobile phones, tablets, laptops, digital cameras, etc.), wearable devices (e.g., watches, bracelets, VR glasses, etc.), energy storage power stations, etc., without particular limitation.
[0114] The present invention will be further described below through specific embodiments.
[0115] Example 1
[0116] The preparation method of the composite lithium supplementation material in this embodiment includes the following steps:
[0117] 1) Fluorinated phosphate LiAlPO 3.94 F 1.06 High-energy ball milling was performed to control the particle size Dn50 to 10 nm; the grinding balls were zirconia grinding balls with a diameter of 1–8 mm; LiAlPO4 was used. 3.94 F 1.06 The mass ratio of grinding balls to the ball mill is 1:30; the inert atmosphere is nitrogen and / or argon; the ball milling jar speed is 1200 rpm; the ball milling time is 24 hours.
[0118] 2) Under an argon atmosphere, the ball-milled LiAlPO4 was processed. 3.94 F 1.06 A solid material was obtained by mixing lithium-rich compound Li2NiO2 at a mass ratio of 100:1. The solid material was then added to an NMP solution and stirred until homogeneous to obtain a mixture. The volume ratio of the solid material to the NMP solution was 1:1.1.
[0119] 3) Under an argon atmosphere, the mixture is fed into a spray dryer for spray drying to obtain a pretreated mixture; the heating argon pressure is 0.6 MPa, the inlet temperature is 250℃, the outlet temperature is 95℃, and the feed rate is 1.6 L / h.
[0120] 4) The pretreated mixture was fed into a sintering furnace and calcined at 600°C for 2 hours in an oxygen atmosphere to obtain LiAlPO4. 3.94 F 1.06 The coated Li2NiO2 material is a composite lithium supplement material.
[0121] The coating layer of the composite lithium-rich material accounts for 0.9% of the mass of the lithium-rich compound core.
[0122] Example 2
[0123] This embodiment is basically the same as embodiment 1, except that in step 4), the calcination temperature of the sintering furnace is 200℃.
[0124] Example 3
[0125] This embodiment is basically the same as embodiment 1, except that in step 4), the calcination temperature of the sintering furnace is 150°C.
[0126] Example 4
[0127] This embodiment is basically the same as embodiment 1, except that in step 4), the calcination temperature of the sintering furnace is 300℃.
[0128] Example 5
[0129] This embodiment is basically the same as embodiment 1, except that in step 4), the calcination temperature of the sintering furnace is 800℃.
[0130] Example 6
[0131] This embodiment is basically the same as embodiment 1, except that in step 4), the calcination temperature of the sintering furnace is 900℃.
[0132] Example 7
[0133] This embodiment is basically the same as Example 1, except that: lithium-rich compound, Li y Al z PO 4-x F 1+x The mass ratio is 100:2.
[0134] Example 8
[0135] This embodiment is basically the same as Example 1, except that: lithium-rich compound, Li y Al z PO 4-x F 1+x The mass ratio is 100:0.1.
[0136] Example 9
[0137] This embodiment is basically the same as Example 1, except that: lithium-rich compound, Li y Al z PO 4-x F 1+x The mass ratio is 100:0.08.
[0138] Example 10
[0139] This embodiment is basically the same as embodiment 1, except that in step 4), the calcination time in the sintering furnace is 4 hours.
[0140] Example 11
[0141] This embodiment is basically the same as embodiment 1, except that in step 4), the calcination time in the sintering furnace is 6 hours.
[0142] Example 12
[0143] This embodiment is basically the same as embodiment 1, except that in step 4), the calcination time in the sintering furnace is 0.5h.
[0144] Example 13
[0145] This embodiment is basically the same as Embodiment 1, except that in step 1), the fluorinated phosphate is LiAlPO4. 3.9F 1.1 .
[0146] Example 14
[0147] This embodiment is basically the same as Embodiment 1, except that in step 1), the fluorinated phosphate is LiAlPO4. 3.92 F 1.08 .
[0148] Example 15
[0149] This embodiment is basically the same as Embodiment 1, except that in step 1), the fluorinated phosphate is LiAlPO4. 3.96 F 1.04 .
[0150] Example 16
[0151] This embodiment is basically the same as Embodiment 1, except that in step 1), the fluorinated phosphate is LiAlPO4. 3.98 F 1.02 .
[0152] Example 17
[0153] This embodiment is basically the same as that of Embodiment 1, except that in step 1), the fluorinated phosphate is LiAlPO4F.
[0154] Example 18
[0155] This embodiment is basically the same as embodiment 1, except that in step 2), Li2NiO2 is replaced with Li5FeO4.
[0156] Example 19
[0157] This embodiment is basically the same as embodiment 1, except that in step 2), Li2NiO2 is replaced with Li6CoO4.
[0158] Example 20
[0159] This embodiment is basically the same as Embodiment 1, except that: LiAlPO 3.94 F 1.06 The particle size Dn50 is 60 nm.
[0160] Example 21
[0161] This embodiment is basically the same as Embodiment 1, except that: LiAlPO 3.94 F 1.06 The particle size Dn50 is 50 nm.
[0162] Example 22
[0163] This embodiment is basically the same as Embodiment 1, except that: LiAlPO 3.94 F 1.06 The particle size Dn50 is 1 nm.
[0164] Example 23
[0165] This embodiment is basically the same as Example 1, except that the particle size Dn50 of the lithium-rich compound is 17 μm.
[0166] Example 24
[0167] This embodiment is basically the same as Example 1, except that: lithium-rich compound, Li y Al z PO 4-x F 1+x The mass ratio is 100:2.5.
[0168] Example 25
[0169] This embodiment is basically the same as Example 1, except that: lithium-rich compound, Li y Al z PO 4-x F 1+x The mass ratio is 100:0.4.
[0170] Example 26
[0171] This embodiment is basically the same as Embodiment 1, except that: x = 0.01, that is, the coating layer is LiAlPO 3.99 F 1.01 .
[0172] Example 27
[0173] This embodiment is basically the same as Embodiment 1, except that: x = 0.11, that is, the coating layer is LiAlPO 3.89 F 1.11 .
[0174] Comparative Example 1
[0175] This embodiment is basically the same as Embodiment 1, except that: the core layer lithium-rich compound Li2NiO2 is not modified, that is, Li2NiO2 is directly used as the lithium supplement material.
[0176] Comparative Example 2
[0177] This embodiment is basically the same as embodiment 1, except that: the LiAlPO4 in step 1) is removed. 3.94 F 1.06 Replace with Al2O3, that is, modify Li2NiO2 with Al2O3.
[0178] Comparative Example 3
[0179] This embodiment is basically the same as embodiment 1, except that: the LiAlPO4 in step 1) is removed. 3.94 F 1.06 Replace with TiO2, that is, modify Li2NiO2 with TiO2.
[0180] Comparative Example 4
[0181] This embodiment is basically the same as embodiment 1, except that: the LiAlPO4 in step 1) is removed. 3.94 F 1.06 Replace with Li3PO4, that is, modify Li2NiO2 with Li3PO4.
[0182] Comparative Example 5
[0183] This embodiment is basically the same as embodiment 1, except that: the LiAlPO4 in step 1) is removed. 3.94 F 1.06 Replace it with Al-doped ZnO, that is, modify Li2NiO2 with Al-doped ZnO.
[0184] Comparative Example 6
[0185] This embodiment is basically the same as Embodiment 18, except that: the core layer lithium-rich compound Li5FeO4 is not modified, that is, Li5FeO4 is directly used as the lithium supplement material.
[0186] Comparative Example 7
[0187] This embodiment is basically the same as Embodiment 19, except that: the core layer lithium-rich compound Li6CoO4 is not modified, that is, Li6CoO4 is directly used as the lithium supplement material.
[0188] The implementation conditions for different embodiments and comparative examples are shown in Table 1.
[0189] Test method:
[0190] The percentage of the mass of the coating layer relative to the mass of the lithium-rich compound core (abbreviated as coating amount).
[0191] Table 1
[0192]
[0193]
[0194] Test case
[0195] (1) The composite lithium replenishing materials prepared in the above embodiments and comparative examples were subjected to the following tests. The thickness of the transition layer of the composite lithium replenishing materials and the percentage of P, Al and F elements in the transition layer by mass are shown in Table 2.
[0196] Test method:
[0197] 1) Transition layer thickness
[0198] The FIB is used to process the target particles to obtain a cross-section, which is then characterized by STEM to observe the surface crystal structure of the particle cross-section. The thickness of the transition layer and the surface fluorinated phosphate modified layer can be measured.
[0199] 2) The mass ratio of P, Al, and F elements in the transition layer
[0200] By using the EELS equipped with STEM for statistical characterization of surface element distribution, the mass ratios of P, Al, and F in the transition layer can be measured.
[0201] Table 2
[0202]
[0203]
[0204] (2) Battery manufacturing
[0205] The modified Li2NiO2 materials and the unmodified Li2NiO2 materials in the examples and comparative examples were exposed to air at a temperature of 25°C and a humidity of 40% for 24 hours.
[0206] The materials that were not placed in a humid environment and the materials that were placed in a humid environment were used as positive electrode materials to make button cells.
[0207] In the fabrication of coin cells, positive electrode material, conductive carbon black, and PVDF are dispersed in NMP at a mass ratio of 8:1:1. The positive electrode is obtained through slurry preparation, coating, drying, and rolling. A lithium metal sheet is used as the negative electrode, a Celgard 2400 polypropylene membrane as the separator, and a mixed solution of EC and DMC containing 1 mol / L lithium hexafluorophosphate (volume ratio 1:1) is used as the electrolyte. The battery is assembled with the aforementioned positive electrode in an argon-filled glove box.
[0208] Using the LAND battery testing system, the batteries were charged to 4.2V at constant current rates of 0.05C and 0.33C, respectively, and then charged at constant voltage at 4.2V until the current equals 0.03C. The charge capacity at 0.05C and the charge capacity at 0.33C were recorded respectively.
[0209] After the lithium replenishing agent powder is left to stand for 24 hours at 25°C and 40% humidity, the battery is made according to the above steps and charged at a constant current rate of 0.05C to 4.2V. Then, it is charged at a constant voltage rate of 4.2V to a current of 0.03C. The charging capacity at this time is recorded as the gram capacity of the powder after standing for 24 hours and charging at 0.05C.
[0210] The test results are shown in Table 3.
[0211] Table 3
[0212]
[0213]
[0214] As can be seen from Table 3, compared with the comparative example, the battery made from the composite lithium replenishment material of the present invention has a higher charging capacity.
[0215] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A composite lithium supplementation material, characterized in that, It includes a lithium-rich compound core and a coating layer covering at least a portion of the surface of the lithium-rich compound core, the coating layer comprising Li y Al z PO 4-x F 1+x Where 0 ≤ x < 4, y > 0, z > 0.
2. The composite lithium replenishment material according to claim 1, characterized in that, The lithium-rich compound core includes a core layer and a transition layer covering at least a portion of the surface of the core layer. The core layer includes a lithium-rich compound, and the transition layer includes an element-doped lithium-rich compound, wherein the element includes at least one of P, Al, and F.
3. The composite lithium replenishment material according to claim 1 or 2, characterized in that, y:z = 1-10:
1.
4. The composite lithium supplementation material according to any one of claims 1-3, characterized in that, 0.02≤x≤0.1; and / or, 0.5≤y≤3; and / or, 0.1≤z≤1.
5. The composite lithium supplementation material according to any one of claims 1-4, characterized in that, The mass of the coating layer accounts for 0.1-2% of the mass of the lithium-rich compound core; and / or, the thickness of the coating layer is 1-500 nm.
6. The composite lithium supplementation material according to any one of claims 1-5, characterized in that, The Li y Al z PO 4-x F 1+x The particle size Dn50 satisfies: 1nm≤Dn50≤50nm.
7. The composite lithium replenishment material according to claim 2, characterized in that, The element-doped lithium-rich compound has at least one of the following structures: layered structure, rock salt-like structure, and spinel-like structure.
8. The composite lithium replenishment material according to claim 7, characterized in that, The mass of P element in the transition layer accounts for 0.1-20.8% of the mass of the transition layer; and / or, the mass of Al element in the transition layer accounts for 0.1-18.2% of the mass of the transition layer; and / or, the mass of F element in the transition layer accounts for 0.1-12.8% of the mass of the transition layer.
9. The composite lithium replenishment material according to claim 7 or 8, characterized in that, The thickness of the transition layer is 2-499 nm.
10. The composite lithium supplementation material according to any one of claims 7-9, characterized in that, The lithium-rich compound includes at least one of Li2NiO2, Li6CoO4, and Li5FeO4.
11. The composite lithium supplementation material according to any one of claims 7-10, characterized in that, The particle size Dn50 of the lithium-rich compound satisfies: 500nm≤Dn50≤15μm.
12. A method for preparing the composite lithium-supplementing material according to any one of claims 1-11, characterized in that, include: In an oxygen atmosphere, lithium-rich compounds, Li y Al z PO 4-x F 1+x The mixture is calcined to obtain the composite lithium supplement material.
13. The preparation method according to claim 12, characterized in that, The lithium-rich compound, Li y Al z PO 4-x F 1+x The mass ratio is 100:0.1-2.
14. The preparation method according to claim 12 or 13, characterized in that, The calcination treatment temperature is 200-800℃, and the calcination treatment time is 0.5-6h.
15. The preparation method according to any one of claims 12-14, characterized in that, The calcination temperature is 300-600℃, and the calcination time is 2-6 hours.
16. The preparation method according to any one of claims 12-15, characterized in that, Prior to the calcination, the process further includes: reacting the lithium-rich compound with Li... y Al z PO 4-x F 1+x The solvent is mixed and then spray-dried to obtain the mixture; the spray-drying conditions include: The pressure is 0.2-1 MPa; and / or the inlet temperature is 100-300℃; and / or the outlet temperature is 80-100℃; and / or the feed rate is 0.5-2 L / h.
17. A positive electrode plate, characterized in that, Includes the composite lithium replenishing material according to any one of claims 1-11, or the composite lithium replenishing material prepared by the preparation method according to any one of claims 12-16.
18. A battery, characterized in that, Includes the positive electrode sheet as described in claim 17.
19. An electronic device, characterized in that, Includes the battery as described in claim 18.