Framework-accommodating silicon-carbon materials, their preparation methods and applications
The elastic network framework and silicon-carbon composite unit prepared by biomass nanofibers and microorganisms solve the problems of preparation complexity and safety of existing silicon-carbon anode technology, and improve the cycle life and dynamic performance of the battery.
Patent Information
- Application Number
- CN202611354346.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-17
AI Technical Summary
Existing silicon-carbon anode technology suffers from complex manufacturing processes, high costs, poor safety, and short cycle life, making it difficult to meet the demands of high-energy-density batteries.
Elastic network frameworks and silicon-carbon composite units are prepared using biomass nanofibers and silicon-rich microorganisms. Carbonization and reduction treatments are used to form a carbon matrix with internally dispersed nano-silicon particles. Combined with a carbon coating layer, a framework-accommodating silicon-carbon material is formed.
It improves the cycle life and kinetic performance of the material, reduces production costs, avoids the safety risks of silane vapor deposition, and achieves efficient lithium-ion conduction and volume expansion mitigation.
Smart Images

Figure CN123120691A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery materials technology, and in particular to a framework-accommodation type silicon-carbon material, its preparation method, and its application. Background Technology
[0002] Traditional graphite anodes for lithium-ion batteries have a theoretical specific capacity of only 372 mAh / g, and despite continuous development, their performance is nearing its ceiling, making it difficult to meet the ever-increasing energy density demands of power batteries and consumer electronics. Silicon, on the other hand, boasts a theoretical specific capacity of up to 4200 mAh / g, more than ten times that of graphite, making it the core candidate material for next-generation high-capacity anodes. However, silicon has a fatal inherent drawback: its volume expands by up to 280 mm during lithium intercalation. Repeated charging and discharging at 300% capacity can cause silicon particle pulverization, conductive network breakage, and continuous side reactions in the electrolyte, resulting in rapid degradation during cycling and making it difficult to use as a standalone anode. The core idea of existing silicon-carbon anode technology is to composite silicon with a carbon matrix, where carbon simultaneously assumes the triple roles of conductive network, stress buffer, and structural support, achieving both high capacity and cycle stability, making it the mainstream solution in the industry.
[0003] Current mainstream technologies employ a porous carbon matrix combined with CVD vapor deposition of silicon. Porous carbon is prepared using carbon sources such as resin and biomass. Through physical or chemical activation methods, a large number of micropores and mesopores are created in the carbon material. This process can utilize the rich pore structure inside the porous carbon to nanoscale silicon in situ and confine it within the pores of the carbon matrix. This can effectively disperse silicon particles, alleviate the volume expansion effect during silicon charging and discharging, and obtain silicon-carbon anode materials with excellent first-efficiency and cycle performance.
[0004] However, the CVD silicon-carbon technology route has significant engineering shortcomings: on the one hand, the preparation process of high-performance porous carbon precursors is complex, the product yield during carbonization is low, and the raw material loss is large, which increases the overall material cost; on the other hand, silane vapor deposition has stringent requirements for equipment airtightness, temperature control, and gas pressure control. Silane itself is a flammable and explosive high-risk gas, making safety management during the production process difficult and resulting in high equipment investment and maintenance costs; at the same time, the rigid porous carbon framework cannot withstand the periodic expansion and contraction stress caused by repeated lithium insertion and extraction from silicon. During long cycles, the framework is prone to cracking and damage, which in turn destroys the internal conductive network, restricting the actual service life of the material and the improvement of mass production yield.
[0005] In view of this, the present invention is hereby proposed. Summary of the Invention
[0006] The primary objective of this invention is to provide a framework-accommodating silicon-carbon material to solve the aforementioned technical problems.
[0007] A second objective of the present invention is to provide a method for preparing the above-mentioned framework-accommodation type silicon-carbon material.
[0008] A third objective of this invention is to provide the application of the above-mentioned framework-accommodation type silicon-carbon material as a negative electrode active material in the preparation of batteries.
[0009] To achieve the above objectives, the following technical solution is adopted: In a first aspect, the present invention provides a framework-accommodating silicon-carbon material, comprising an elastic network framework and silicon-carbon composite units; the silicon-carbon composite units are dispersed and loaded within the elastic network framework; the surface of the elastic network framework contains a carbon coating layer; The elastic network framework is obtained by impregnating biomass nanofibers with a transition metal salt solution and then graphitizing them. The silicon-carbon composite unit comprises a carbon matrix and nano-silicon particles dispersed within the carbon matrix, obtained by carbonization and reduction treatment of silicon-rich microorganisms.
[0010] As a further technical solution, the carbon matrix and the elastic network framework in the silicon-carbon composite unit are connected by C-C bonds; And / or, the mass ratio of the elastic network framework to the silicon-carbon composite unit is (3~97):(97~3).
[0011] As a further technical solution, the particle size of the silicon-carbon composite unit is 500nm~20μm; the number of silicon-carbon composite units in the framework-accommodation type silicon-carbon composite material is at least one; the size of the nano-silicon in the silicon-carbon composite unit is 2~500nm; And / or, the silicon content in the framework-accommodating silicon-carbon material is 10% to 80% by mass.
[0012] As a further technical solution, the specific surface area of the framework-accommodating silicon-carbon material is between 0.1 and 5 m². 2 / g; the Dv50 of the framework-accommodating silicon carbide material is 3~12μm.
[0013] As a further technical solution, the biomass nanofibers are selected from at least one of bacterial cellulose nanofibers, plant cellulose nanofibers, or chitin nanofibers; the diameter of the biomass nanofibers is 2~1000nm and the length is 2~200μm. And / or, the silicon-rich microorganism is one or more of the bacteria or fungi in the biological world that can decompose and absorb silicon; the silicon source decomposed and absorbed by the microorganism is one or more of silicates, silica sols, orthosilicic acid, montmorillonite, or mica.
[0014] As a further technical solution, the transition metal salt solution is a metal salt solution of Fe, Co, Ni, Mn or Ti.
[0015] As a further technical solution, the carbon coating layer is an organic carbon layer, and the organic carbon includes one or more of the following: asphalt, starch, glucose, polyaniline, polypyrrole, polydopamine, polythiophene, phenolic resin, epoxy resin, or polyacrylonitrile.
[0016] Secondly, the present invention provides a method for preparing the above-mentioned framework-accommodating silicon-carbon material, comprising the following steps: Biomass nanofibers were dispersed in a transition metal salt solution, then mixed with silicon-rich microorganisms, and after spray granulation, carbonized and graphitized, and then reduced to obtain a carbonized intermediate. The carbonized intermediate was then coated with carbon to prepare a framework-accommodating silicon-carbon material.
[0017] As a further technical solution, the transition metal salt solution comprises a nickel acetate aqueous solution with a mass fraction of 0.02% to 5%; The carbonization and graphitization processes are carried out at temperatures of 500~1000℃, with a heating rate of 0.1~10℃ / min. The reduction process includes a step of removing transition metal elements by acid washing.
[0018] Thirdly, the present invention provides the application of the above-mentioned framework-accommodation type silicon-carbon material as a negative electrode active material in the preparation of batteries.
[0019] Compared with the prior art, the present invention has the following beneficial effects: The framework-accommodation type silicon-carbon material provided by this invention has silicon-carbon composite units prepared by microorganisms through carbonization. Utilizing the ability of microorganisms to decompose silicon, silicon is enriched in the body to form a silicon-containing macromolecular framework. After carbonization and reduction, a carbon matrix with nano-silicon particles dispersed inside is obtained, avoiding the problems of high cost and harsh conditions of silane vapor deposition. At the same time, the elastic network framework layer serves as a conductive network and supporting structure to improve kinetics and cycle life. Attached Figure Description
[0020] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0021] Figure 1 This is a structural diagram of the framework-accommodating silicon-carbon material of the present invention.
[0022] Figure 2 This is an XRD data diagram of bacterial cellulose sample 4-1, which was carbonized without the addition of a catalyst in Comparative Example 4 of the present invention.
[0023] Figure 3 The image shows the XRD data of bacterial cellulose sample 4-2, which was carbonized with a catalyst in Comparative Example 4 of this invention. Detailed Implementation
[0024] The embodiments and examples of the present invention will be described in detail below. However, those skilled in the art will understand that the following embodiments and examples are for illustrative purposes only and should not be considered as limiting the scope of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention. Unless otherwise specified, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.
[0025] In a first aspect, the present invention provides a framework-accommodating silicon-carbon material, such as... Figure 1 (Where, 1 is a carbon coating layer, 2 is an elastic network framework, and 3 is a silicon-carbon composite unit) As shown, it includes an elastic network framework (the elastic network framework encloses a three-dimensional network structure to accommodate space, providing a transmission channel for lithium-ion migration and electron conduction) and silicon-carbon composite units; the silicon-carbon composite units are dispersed and loaded within the elastic network framework; the surface of the elastic network framework contains a carbon coating layer; The elastic network framework is obtained by impregnating biomass nanofibers with a transition metal salt solution and then graphitizing them. The silicon-carbon composite unit comprises a carbon matrix and nano-silicon particles dispersed within the carbon matrix, obtained by carbonization and reduction treatment of silicon-rich microorganisms (the purpose of the reduction treatment is to reduce silicon oxide to elemental silicon).
[0026] The framework-accommodation type silicon-carbon material provided by this invention has silicon-carbon composite units prepared by microorganisms through carbonization. Utilizing the ability of microorganisms to decompose silicon, silicon is enriched in the body to form a silicon-containing macromolecular framework. After carbonization and reduction, a carbon matrix with nano-silicon particles dispersed inside is obtained, avoiding the problems of high cost and harsh conditions of silane vapor deposition. At the same time, the elastic network framework serves as a conductive network and supporting structure to improve kinetics and cycle life.
[0027] In some optional embodiments, the carbon matrix and the elastic network framework in the silicon-carbon composite unit are connected by CC bonds. After high-temperature carbonization, the carbon matrix and the elastic network framework in the silicon-carbon composite unit will bond in situ to form CC bonds.
[0028] In some optional embodiments, the mass ratio of the elastic network framework to the silicon-carbon composite unit is (3~97):(97~3), for example, but not limited to 20:80, 40:40, 90:10 or 10:90; In some alternative embodiments, the elastic network framework obtained by the carbonization treatment has a graphitized structure, mainly composed of sp² hybrid carbon, providing deformation buffer space for the internal silicon-carbon composite units.
[0029] In some optional embodiments, the particle size of the silicon-carbon composite unit is 500 nm to 20 μm, for example, but not limited to 500 nm, 10 μm or 20 μm; the number of silicon-carbon composite units in the framework-accommodating silicon-carbon composite material is at least one; the size of the nano-silicon in the silicon-carbon composite unit is 2 to 500 nm, for example, but not limited to 2 nm, 100 nm or 500 nm.
[0030] In some optional embodiments, the silicon content in the framework-accommodating silicon-carbon material is 10% to 80% by mass, for example, but not limited to 10%, 30%, 50% or 70%.
[0031] In some optional embodiments, the specific surface area of the framework-accommodating silicon-carbon material is between 0.1 and 5 m². 2 / g; the Dv50 of the framework-accommodating silicon carbide material is 3~12μm.
[0032] In some optional embodiments, the elastic network framework is composed of nanofibers, wherein the biomass nanofibers are selected from at least one of bacterial cellulose nanofibers, plant cellulose nanofibers, or chitin nanofibers; the diameter of the biomass nanofibers is 2-1000 nm, and the length is 2-200 μm. The number of interlacing nodes formed by the interconnection of a single nanofiber and other nanofibers is 2-1000; the nanofibers are formed by the natural growth of microorganisms and have functional groups such as hydroxyl, carboxyl, and aldehyde groups. During the high-temperature treatment process, a large number of carbon free radicals at the interface are recoupled, generating interconnected branched structures at the fiber intersections, achieving "edge fusion" and physical locking.
[0033] In some optional embodiments, the silicon-rich microorganism is one or more of the bacteria or fungi in the biological world that decompose and absorb silicon; the silicon source decomposed and absorbed by the microorganism is one or more of silicates, silica sols, orthosilicic acid, montmorillonite, or mica.
[0034] In some alternative embodiments, the transition metal salt solution is a metal salt solution of Fe, Co, Ni, Mn or Ti.
[0035] In some alternative embodiments, the carbon coating layer is an organic carbon layer, which includes one or more of the following: asphalt, starch, glucose, polyaniline, polypyrrole, polydopamine, polythiophene, phenolic resin, epoxy resin, or polyacrylonitrile.
[0036] Secondly, the present invention provides a method for preparing the above-mentioned framework-accommodating silicon-carbon material, comprising the following steps: Biomass nanofibers were dispersed in a transition metal salt solution, then mixed with silicon-rich microorganisms, and after spray granulation, carbonized and graphitized, and then reduced to obtain a carbonized intermediate. The carbonized intermediate was then coated with carbon to prepare a framework-accommodating silicon-carbon material.
[0037] The preparation method is simple, and the prepared framework-accommodating silicon-carbon material can be used as the negative electrode active material of the battery to improve the cycle performance of the battery.
[0038] In some optional embodiments, the transition metal salt solution comprises an aqueous solution of nickel acetate with a mass fraction of 0.02% to 5%; The carbonization and graphitization processes (transition metals have the effect of lowering the graphitization temperature; graphitization can be achieved at 800℃ after the introduction of transition metals) are carried out at temperatures of 500~1000℃, for example, but not limited to 500℃, 800℃ or 1000℃; the temperature is increased to the carbonization temperature at a rate of 0.1~10℃ / min. The reduction process includes a step of removing transition metal elements by acid washing.
[0039] In some optional embodiments, the reducing agent for the reduction treatment includes magnesium powder; the magnesium powder reduction treatment further includes an acid washing step to remove magnesium.
[0040] Thirdly, the present invention provides the application of the above-mentioned framework-accommodation type silicon-carbon material as a negative electrode active material in the preparation of batteries.
[0041] The framework-accommodation type silicon-carbon material provided by this invention is used as the negative electrode active material to prepare batteries, and the prepared batteries have good cycle performance.
[0042] The present invention will be further illustrated below with specific embodiments and comparative examples. However, it should be understood that these embodiments are merely for the purpose of more detailed illustration and should not be construed as limiting the present invention in any way.
[0043] Example 1 Step 1: Take 20g of the purchased bacterial cellulose membrane and treat it in 0.2mol / L NaOH solution at 40℃ for 30 minutes. Then wash it with water several times until neutral. Then add 100g of nickel acetate by mass fraction and ultrasonically disperse it evenly.
[0044] Step 2: Magnetotactic bacteria were cultured in sterile water and nutrient solution for 10 days to prepare a bacterial suspension. Sodium silicate was added at a mass ratio of bacterial suspension to sodium silicate of 100:10. The suspension was cultured in an aerobic environment at 30 degrees Celsius for 15 days. Afterward, sodium silicate that had not entered the bacteria was washed away with pure water, and the silicon-containing fungi were obtained by filtration.
[0045] Step 3: The silica-containing fungal filtrate and the bacterial cellulose membrane solution containing nickel acetate were ultrasonically mixed at a mass ratio of 30:150 for 1 hour, followed by spray drying for granulation. The mixture was then carbonized (graphitized) at 850℃ for 2 hours under a nitrogen atmosphere. It was then washed twice with 500g of 1mol / L hydrochloric acid solution to remove nickel and sodium. 20nm magnesium powder and the hydrochloric acid-washed silicon-carbon composite material were mixed uniformly in a V-shaped mixer at a mass ratio of 1:1. The mixture was then heated to 650℃ at a rate of 5℃ / min under a nitrogen atmosphere and held for 2 hours. After cooling to room temperature, the mixture was removed and washed twice with 1mol / L hydrochloric acid solution to remove magnesium.
[0046] Step 4: Mix the treated silicon-carbon composite material with coated asphalt containing 5% solids (mass ratio 50:40) again until homogeneous, and then treat it at 600℃ for 3 hours under a nitrogen atmosphere to obtain a silicon-carbon composite material containing an elastic network skeleton and silicon-carbon composite units.
[0047] Example 2 Compared with Example 1, the mass ratio of bacterial suspension to sodium silicate in step 2 was adjusted to 200:10, and the carbonization temperature in step 3 was 1000℃, while other aspects remained unchanged.
[0048] Example 3 Compared with Example 1, the mass ratio of bacterial suspension to sodium silicate in step 2 was adjusted to 300:10, while other aspects remained unchanged.
[0049] Example 4 Compared with Example 1, the silica-containing fungal filtrate in step 3 was ultrasonically mixed with the bacterial cellulose membrane solution containing nickel acetate at a mass ratio of 10:150 for 1 hour, while other steps remained unchanged.
[0050] Example 5 Compared to Example 1, the silica-containing fungal filtrate and the nickel acetate-containing bacterial cellulose membrane solution in step 3 were ultrasonically mixed for 1 hour at a mass ratio of 80:150. The heating rate of the carbonization temperature after adding magnesium powder in step 3 was adjusted to 0.5 degrees Celsius per minute, while other steps remained unchanged.
[0051] Example 6 Compared to Example 1, the mass fraction of nickel acetate in step 1 was adjusted to 3%. The mass ratio of bacterial suspension to sodium silicate in step 2 was adjusted to 60:10. The silica-containing fungal filtrate and the nickel acetate-containing bacterial cellulose membrane solution in step 3 were ultrasonically mixed at a mass ratio of 130:150 for 1 hour, while other steps remained unchanged.
[0052] Example 7 Compared with Example 1, the heating rate of the carbonization temperature after adding magnesium powder in step 3 was adjusted to 0.5 degrees per minute, while other steps remained unchanged.
[0053] Comparative Example 1 Based on Example 1, step 1 was removed, and the silicon-containing fungi in step 2 were carbonized under the conditions of Example 1, subjected to magnesium thermal reduction, and carbon coating to obtain a silicon-carbon composite material without a network structure.
[0054] Comparative Example 2 Porous carbon with a pore volume of 0.75 ml / g was placed in a tube furnace and heated to 580 °C at 5 °C / min under a N2 atmosphere. A 25% SiH4-N2 mixture was then introduced and maintained for 18 hours. The atmosphere was changed to N2, and the substrate was placed back in the tube furnace and heated to 650 °C. Methane gas was introduced for carbon coating for 2 hours. The atmosphere was then changed back to N2, and the substrate was cooled to room temperature.
[0055] Comparative Example 3 Based on Example 1, the nickel-containing bacterial cellulose membrane solution from step 1 was spray-granulated and carbonized at 850°C for 2 hours under a nitrogen atmosphere. The nickel was removed by washing with 500g of 1mol / L hydrochloric acid solution, resulting in a near-spherical network structure. This substrate was placed in a tube furnace and heated to 580°C at 5°C / min under a N2 atmosphere, followed by a 18-hour period of purging with a 25% SiH4-N2 mixture. The atmosphere was then changed to N2, and the substrate was placed back in the tube furnace and heated to 650°C. Methane gas was then introduced for carbon coating for 0.5 hours. The atmosphere was then changed back to N2, and the substrate was cooled to room temperature. The process of asphalt coating and carbonization was repeated as described in Example 1.
[0056] Comparative Example 4 The difference from Example 1 is that the bacterial cellulose membrane was not impregnated with nickel acetate. In step 3 of this comparative example, the carbonized sample is designated as Sample 4-1; the carbonized sample in step 3 of Example 1 is designated as Sample 4-2. The XRD spectra of the two are compared as follows... Figure 2 and Figure 3 As shown.
[0057] Physical property testing of silicon-carbon composite materials: 1. Particle size test: The particle size of the silicon-carbon composite materials in each embodiment and comparative example was measured using a laser particle size analyzer MS3000. 0.5 ± 0.05 g of porous carbon powder was weighed using a 0.1% balance and poured into 100 ml of a 0.2% dispersant solution. The mixture was then stirred magnetically for 20 minutes at 500-550 rpm. The laser particle size analyzer was operated at 80% ultrasonic power and 3000 rpm. After background removal, the average value of three manually measured data points was obtained to calculate the volume distribution data (Dv10, Dv50, Dv90). The Span data was calculated using Span = (Dv90 - Dv50) / Dv10, and the results are shown in Table 2.
[0058] 2. Specific surface area test: BET data for the silicon-carbon composite materials in each embodiment and comparative example were obtained using a Bestech BSD-660M tester. 0.2 ± 0.02 g of silicon-carbon composite material powder was weighed into a sample tube. The empty sample tube was weighed (m0), and the sample + sample tube (m1) was weighed. The sample mass m = m0 - m1 was recorded. A purge head was attached to the end of each sample tube, and heating and purging were performed. Nitrogen purging was performed at 150°C for 30 minutes, followed by degassing at 300°C for 90 minutes. After cooling for 5-10 minutes, the sample + sample tube (m2) was weighed again. The degassed sample mass m3 = m2 - m0. The sample type was selected as "ultrafine ultralight powder (extremely easily dispersed)," and the degassing setting was selected as "non-in-situ degassing / no degassing." In the isotherm report, P is the pressure after adsorption equilibrium, and P0 is the saturated vapor pressure of the adsorbate at the adsorption temperature. The BET multi-point method automatic range P / P0 = 0.0149~0.1573 is selected as the specific surface area data, and the results are shown in Table 2.
[0059] Physical and electrochemical performance testing of silicon-carbon composite materials: 1. Test of Si content in silicon-carbon composite materials: 3.0 g of silicon-carbon composite material was dried in an oven at 150℃ until constant weight, and the mass m1 was recorded. The dried composite material was then placed in a muffle furnace, heated to 1100℃ and held for 2 hours, cooled, and weighed, and the mass m2 was recorded. The Si content calculation formula is as follows: .
[0060] 2. Nano-silicon size testing: Phase analysis of the sample was performed using an X-ray diffractometer. The test conditions were: Cu Kα rays (λ=0.15406 nm), operating voltage 40 kV, operating current 40 mA, scanning range 2θ from 10° to 90°, scanning step size 0.008°, and scanning time 12 s per step. The obtained X-ray diffraction patterns were analyzed, and the diffraction peaks near 2θ=28.4°±0.2°, belonging to the silicon (111) crystal plane, were selected. The full width at half maximum (FWHM) of these diffraction peaks was obtained by fitting (Lorentz function), and then the grain size of silicon was calculated using the Scherrer formula. The Scherrer formula is as follows: D = Kλ / (β cosθ).
[0061] in: D is the grain size of silicon (nm); K is Scherrer's constant (taken as 0.89); λ is the X-ray wavelength (Cu Kα, λ=0.15406 nm). β is the full width at half maximum (FWHM) value (in radians) of the measured diffraction peak of silicon (111) crystal plane. θ is the Bragg angle (°) corresponding to the diffraction peak of the silicon (111) crystal plane.
[0062] Using the silicon-carbon composite materials prepared in the above embodiments and comparative examples as negative electrode active materials, negative electrode sheets were prepared respectively. The negative electrode sheets were used to prepare CR2032 coin cells using conventional methods, and the electrical performance of the cells was tested.
[0063] Specific testing methods include: Half-cell assembly: Assemble CR2032 coin cells in a glove box, using lithium metal sheets as the counter electrode, polypropylene microporous membranes as the separator, and LiPF6 dissolved in a mixture of ethyl carbonate (EC) and diethyl carbonate (DEC) (volume ratio EC:DEC=1:1), with a LiPF6 concentration of 1 mol / L.
[0064] The battery was charged and discharged using the LAND battery testing system: (1) Specific capacity, initial efficiency and 1C rate test: After the CR2032 button cell was left to stand for 6 hours, it was discharged at 0.1C to 0.005V and the specific capacity was recorded as Q1; then it was discharged at a constant voltage of 0.005V to the current cutoff of 0.01C and the specific capacity was recorded as Q2; after standing for 5 minutes, it was charged at a constant current of 0.1C to 0.8V and the specific capacity was recorded as Q3; after standing for 5 minutes, it was charged at a constant current of 0.1C to 1.5V and the specific capacity was recorded as Q4; after standing for 5 minutes, it was discharged at a constant current of 1.0C to 0.005V and the specific capacity was recorded as Q5; after standing for 2 hours, the thickness of the negative electrode sheet was measured in sequence and the average value was recorded as h1. Another coated and dried electrode sheet was taken and the thickness of the negative electrode sheet at 5 points was measured and the average value was recorded as h2. The specific capacity of the first lithium delithiation is the specific capacity (or mass specific capacity) of the electrode material. The ratio of the first lithium delithiation capacity to the first lithium insertion capacity is the first coulombic efficiency of the battery.
[0065] 1.5V initial efficiency = (Q3 + Q4) / (Q1 + Q2) * 100%; 1C rate discharge retention rate = Q5 / (Q3 + Q4) * 100%; (2) Electrode expansion rate: After the CR2032 type button cell was left to stand for 6 hours, it was discharged to 0.005V at 0.05C and then discharged to 0.005V at 0.01C. Then the button cell was disassembled in the glove box, the electrode was cleaned with DMC and the thickness of the electrode was measured. The expansion rate was calculated as: (thickness of electrode in the first fully charged state - thickness of fresh electrode) / thickness of fresh electrode × 100%.
[0066] Using the silicon-based composite material or silicon-carbon composite material obtained in the above embodiments and comparative examples as the negative electrode active material, a pouch cell was prepared using conventional methods with an electrode containing the negative electrode active material, and its electrical performance was tested. The pouch cell was tested at the dew point. Prepared in a dehumidified room at 45℃. The battery underwent charge-discharge cycle testing using the LANBTS battery testing system. The specific test method is as follows: Preparation of positive electrode sheet: The positive electrode active material NCM811, conductive agent Super P, binder PVDF and solvent NMP are mixed evenly in a mass ratio of 92:3:5:150. The mixture is then evenly coated onto the positive electrode current collector and dried at 80℃ to obtain the positive electrode sheet.
[0067] Fabrication of the negative electrode sheet: The silicon-carbon composite material or silicon-carbon composite material obtained in the examples and comparative examples is mixed with graphite to obtain the negative electrode active material. The negative electrode active material, conductive agent Super P, binder polyacrylic acid and solvent deionized water are stirred and mixed evenly in a mass ratio of 95:1:4:120. The mixture is then evenly coated on the negative electrode current collector and dried at 100°C to obtain the negative electrode sheet.
[0068] The positive and negative electrode sheets are stacked in a square and separated by a polypropylene separator to form a battery cell, which is then packaged into an aluminum-plastic bag. An electrolyte of appropriate capacity is injected into the bag, and after vacuum sealing, a soft-pack battery is obtained. The electrolyte is a mixture of LiPF6 EC and DEC, where the LiPF6 concentration is 1 mol / L and the volume ratio of EC to DEC is 1:1.
[0069] Formation and Capacity Testing: After electrolyte injection and sealing, the battery begins formation. It is placed in a 25°C constant temperature chamber for 12 hours, then charged at a constant current of 0.02C to 3.3V, placed for 30 minutes, charged at a constant current of 0.025C to 3.8V, placed for 10 minutes, and charged at a constant current of 0.33C to 4.2V. After formation, the battery is vacuum-sealed and then subjected to capacity testing. It is charged at a constant current of 0.33C to 4.45V, placed for 10 minutes, discharged at a constant current of 1C to 3V, placed for 10 minutes, and discharged at a constant current of 0.33C to 3V. The capacity testing is then complete. The ratio of the discharge capacity to the charge capacity during the formation and capacity testing of the pouch battery is the battery's initial coulombic efficiency.
[0070] 25℃ Cyclic Test: The battery was placed in a 25℃ constant temperature chamber and charged at a constant current of 1C to 4.45V, then charged at a constant voltage of 4.45V to a current of 0.1C; after resting for 10 minutes, it was discharged at a constant current of 1C to 3.0V, and then rested for 10 minutes. The above charging and discharging steps were repeated until the discharge capacity was lower than 80% of the discharge capacity of the first cycle. The number of cycles obtained at this time is the cycle life of the soft pack battery; this record shows the capacity retention rate after 100 cycles.
[0071] The process parameters and data of each embodiment and comparative example are shown in Table 1; the physical property data of the silicon-carbon composite materials obtained in each embodiment and comparative example are shown in Table 2; and the electrochemical properties of the silicon-carbon composite materials obtained in each embodiment and comparative example are shown in Table 3.
[0072] Table 1 Process parameters and data
[0073] Table 2 Physical property data of silicon-carbon composite materials
[0074] Table 3 Electrochemical properties of silicon-carbon composite materials
[0075] The data in the table above shows that in Examples 1-3, the silicon content gradually decreased as the proportion of bacterial suspension increased. Under the same silicon source conditions, the increased number of fungi led to a decrease in the proportion of silicon in the body, and the specific capacity and first-efficiency also decreased. In Examples 4-5, by adjusting the proportion of silicon-containing fungi and bacterial cellulose, it was found that the silicon content further increased as the proportion of silicon-carbon composite units in the silicon-carbon composite particles increased. Comparing Example 7 with Comparative Examples 1, 2, and 3, Comparative Example 1, without the introduction of bacterial cellulose, showed a significant decrease in cycling performance compared to Example 7. This is because the bacterial cellulose network structure acts as a conductive communication channel, promoting electron transport, while the mesopores in the network structure provide pathways for ion transport, effectively accelerating the lithium insertion / extraction rate. Simultaneously, the carbonized bacterial cellulose acts as a framework, binding and accommodating the carbon composite units, thus mitigating the expansion of the silicon-carbon composite units in space. Compared to Comparative Example 2, Example 7 divides the individual particles into multiple small units and uses bacterial cellulose to physically fix these units. After high-temperature graphitization, the bacterial cellulose exhibits high mechanical strength and elasticity, making it less prone to loosening during battery fabrication. Furthermore, it elastically buffers expansion during excessive volume deformation after lithium insertion / extraction, while simultaneously fixing the particle structure, effectively improving cycle performance. Compared to Example 1, Example 7's magnesium thermal reduction reaction, with controlled heating rate, yields more uniformly dispersed silicon nanoparticles, while preventing silicon nanoparticle aggregation, further improving cycle performance. In Example 5, by further increasing the proportion of silicon-containing fungal filtrate and nickel acetate-containing fungal filtrate, the silicon content is simultaneously increased. By controlling the magnesium thermal reduction temperature, the size of silicon elements is reduced, improving the cycle performance of silicon-carbon materials and reducing the expansion effect caused by lithium insertion / extraction. Thanks to the small-sized silicon particles and high silicon content, the 1C rate reaches 56%, demonstrating excellent performance. This study demonstrates that high-strength conductive networks can be fabricated using the natural fibrous structures of microorganisms in nature. Furthermore, the presence of elements such as N, S, P, Fe, Co, Ni, and Mn in the microorganisms themselves can further enhance the kinetic performance. By utilizing the microorganisms' ability to absorb different elements, metallic or non-metallic elements can be evenly distributed, and high-performance lithium battery materials can be prepared through carbonization.
[0076] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A framework-occluding silicon-carbon material, characterized by, It includes an elastic network framework and silicon-carbon composite units; the silicon-carbon composite units are dispersed and loaded within the elastic network framework; the surface of the elastic network framework contains a carbon coating layer; The elastic network framework is obtained by impregnating biomass nanofibers with a transition metal salt solution and then graphitizing them. The silicon-carbon composite unit comprises a carbon matrix and nano-silicon particles dispersed within the carbon matrix, obtained by carbonization and reduction treatment of silicon-rich microorganisms.
2. The framework- hosting silicon-carbon material of claim 1, wherein, The carbon matrix and the elastic network framework in the silicon-carbon composite unit are connected by C-C bonds; And / or, the mass ratio of the elastic network framework to the silicon-carbon composite unit is (3~97):(97~3).
3. The framework-encased silicon-carbon material of claim 1, wherein, The particle size of the silicon-carbon composite unit is 500 nm to 20 μm; the number of silicon-carbon composite units in the framework-accommodating silicon-carbon composite material is at least one; the size of the nano-silicon in the silicon-carbon composite unit is 2 to 500 nm. And / or, the silicon content in the framework-accommodating silicon-carbon material is 10% to 80% by mass.
4. The framework-encased silicon-carbon material of claim 1, wherein, The specific surface area of the skeleton-containing silicon-carbon material is 0.1-5 m 2 / g; and the Dv50 of the skeleton-containing silicon-carbon material is 3-12 μm.
5. The framework-encased silicon-carbon material of claim 1, wherein, The biomass nanofibers are selected from at least one of bacterial cellulose nanofibers, plant cellulose nanofibers, or chitin nanofibers; the diameter of the biomass nanofibers is 2~1000nm and the length is 2~200μm. And / or, the silicon-rich microorganism is one or more of the bacteria or fungi in the biological world that can decompose and absorb silicon; the silicon source decomposed and absorbed by the microorganism is one or more of silicates, silica sols, orthosilicic acid, montmorillonite, or mica.
6. The framework-encased silicon-carbon material of claim 1, wherein, The transition metal salt solution is a metal salt solution of Fe, Co, Ni, Mn or Ti.
7. The framework-encased silicon-carbon material of claim 1, wherein, The carbon coating layer is an organic carbon layer, which includes one or more of the following: asphalt, starch, glucose, polyaniline, polypyrrole, polydopamine, polythiophene, phenolic resin, epoxy resin, or polyacrylonitrile.
8. The method of making a skeleton-hosting silicon-carbon material according to any one of claims 1 to 7, characterized in that, Includes the following steps: Biomass nanofibers were dispersed in a transition metal salt solution, then mixed with silicon-rich microorganisms, and after spray granulation, carbonized and graphitized, and then reduced to obtain a carbonized intermediate. The carbonized intermediate was then coated with carbon to prepare a framework-accommodating silicon-carbon material.
9. The preparation method according to claim 8, characterized in that, The transition metal salt solution comprises a nickel acetate aqueous solution with a mass fraction of 0.02% to 5%; The carbonization and graphitization processes are carried out at temperatures of 500~1000℃, with a heating rate of 0.1~10℃ / min. The reduction process includes a step of removing transition metal elements by acid washing.
10. The application of the framework-accommodating silicon-carbon material according to any one of claims 1 to 7 as a negative electrode active material in the preparation of batteries.