Anode materials and their preparation methods, anode sheets and secondary batteries

By coating the surface of a silicon-carbon composite material with uncarbonized polyhedral oligomeric silsesquioxane (POSS) while retaining its cage-like structure, the interface can be actively controlled in silicon-based anode materials to form a dense SEI film. This solves the stability and capacity decay problems caused by volume changes in silicon-based materials during charge and discharge, and improves the cycle performance of the electrode.

CN123120699APending Publication Date: 2026-11-17SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611434314.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, silicon-based anode materials suffer from repeated SEI cracking and capacity decay due to volume changes during charging and discharging. This problem cannot be effectively addressed by using conventional carbon or silicon source coating layers to improve interface stability and cycle life.

Method used

Polyhedral oligomeric silsesquioxane (POSS) is used as the shell to coat silicon-carbon composite material, preserving its complete cage structure. By utilizing the weak Li+ coordination and strong solvent affinity of POSS, the Li+ solvation structure is actively reconstructed at the electrode/electrolyte interface to form a thin and dense SEI film, which suppresses SEI rupture caused by volume expansion.

Benefits of technology

It significantly improves the cycle stability and coulombic efficiency of the anode material. Through the active regulation of POSS molecules at the interface, an inorganic-rich SEI film is formed, reducing electrolyte consumption and loss of active materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of battery technology, specifically to a negative electrode material and its preparation method, a negative electrode sheet, and a secondary battery. The disclosed negative electrode material includes: active particles; the active particles include a core and a shell covering the surface of the core; the core comprises a silicon-carbon composite material, and the shell comprises a polyhedral oligomeric silsesquioxane. The negative electrode material of this invention utilizes the complete cage-like structure of the polyhedral oligomeric silsesquioxane and its weak Li-linked structure. + Electronic effects such as coordination and strong solvent affinity can actively modulate Li at the electrode / electrolyte interface. + The solvation structure induces the formation of a thin, dense, inorganic-rich SEI film, thereby effectively suppressing repeated SEI rupture and capacity decay caused by silicon volume expansion, and improving the cycle stability and coulombic efficiency of the anode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, specifically to a negative electrode material and its preparation method, a negative electrode sheet, and a secondary battery. Background Technology

[0002] In recent years, silicon-based materials have become a research hotspot due to their ultra-high theoretical specific capacity. However, silicon undergoes significant volume changes during charging and discharging, which can easily lead to electrode material pulverization and repeated rupture and regeneration of the solid electrolyte interphase (SEI), resulting in irreversible capacity loss. Therefore, combining silicon with carbon materials to buffer volume expansion and construct a conductive network has become a commonly used method. To further improve the interfacial stability and cycle life of silicon-carbon composite anodes, surface coating treatments are often applied to silicon-carbon particles, such as carbon coating, conductive polymer coating, and inorganic oxide coating. However, the carbon or silicon sources in these coating layers cannot effectively regulate the electrode / electrolyte interface.

[0003] Therefore, how to obtain a negative electrode material that can fully utilize its interface regulation function has become an important research topic. Summary of the Invention

[0004] In view of this, the present invention aims to at least partially solve one of the technical problems in the related art. To this end, the present invention provides a negative electrode material and its preparation method, a negative electrode sheet, and a secondary battery. The shell of the active particles comprises a polyhedral oligomeric silsesquioxane, and the POSS molecules in the shell are not carbonized and remain in their complete cage-like structure, retaining their intrinsic organic structural characteristics, and enabling weak Li-ionization. + Electronic effects such as coordination and strong solvent affinity can actively modulate Li at the electrode / electrolyte interface. + The solvation structure induces the formation of a thin, dense, inorganic-rich SEI film, thereby effectively suppressing repeated SEI rupture and capacity decay caused by silicon volume expansion, and improving the cycle stability and coulombic efficiency of the anode material.

[0005] To solve the above-mentioned technical problems, the present invention is implemented as follows: According to one aspect of the present invention, the present invention provides a negative electrode material, comprising: active particles, said active particles comprising a core and a shell covering the surface of said core; The core comprises a silicon-carbon composite material, and the shell comprises a polyhedral oligomeric silsesquioxane.

[0006] In some embodiments, the silicon-carbon composite material includes at least one of nano-silicon / graphite composite, nano-silicon / amorphous carbon composite, and porous silicon-carbon spheres.

[0007] In some of these embodiments, the polyhedral oligomeric silsesquioxane is a cage-type polysilsesquioxane.

[0008] In some embodiments, the cage-like polysilsesquioxane has the general chemical formula (RSiO). 1.5 ) n Where n = 6, 8, 10 or 12; preferably, n = 8; R is selected from hydrogen, alkyl, aryl, epoxy, amino, vinyl, mercapto, or acryloyloxy.

[0009] In some of these embodiments, the thickness of the housing is 2 nm to 50 nm.

[0010] In some of these embodiments, the median particle size D of the active particles 50 The size ranges from 1 μm to 28 μm, preferably from 3 μm to 22 μm, and more preferably from 5 μm to 13 μm.

[0011] In some of these embodiments, the median particle size D of the nucleus 50 The micrometer size is 0.8μm to 5μm, preferably 0.8μm to 3μm.

[0012] In some embodiments, the porous silicon carbide spheres have a pore size of 1 nm to 100 nm, preferably 5 nm to 50 nm, and more preferably 10 nm to 25 nm.

[0013] According to another aspect of the present invention, the present invention also provides a method for preparing a negative electrode material, comprising the following steps: Pretreatment of silicon-carbon composite materials; The polyhedral oligomeric silsesquioxane is coated onto the surface of the silicon-carbon composite material to obtain active particles.

[0014] In some embodiments, the pretreatment of the silicon-carbon composite material to coat the surface of the silicon-carbon composite material with the polyhedral oligomeric silsesquioxane includes: The silicon-carbon composite material was dispersed in a first solvent, and an oxidant was added to obtain activated particles; The polyhedral oligomeric silsesquioxane is dissolved in a second solvent, and the activated particles are added. The mixture is stirred under the first reaction conditions to obtain the activated particles.

[0015] In some of these embodiments, the first solvent includes at least one of an alcohol solvent, a ketone solvent, an ether solvent, an amide solvent, and water; Preferably, the first solvent includes at least one of ethanol, isopropanol, and tetrahydrofuran.

[0016] In some embodiments, the oxidation treatment includes adding an oxidant to the reaction solution, the oxidant including at least one of hydrogen peroxide, nitric acid, sulfuric acid, ozone, and piranha solution.

[0017] In some of these embodiments, the second solvent includes one or more of aromatic hydrocarbon solvents, ether solvents, halogenated hydrocarbon solvents, ketone solvents, and ester solvents; Preferably, the second solvent includes one or more of toluene, xylene, tetrahydrofuran, and chloroform.

[0018] In some of these embodiments, the reaction temperature in the first reaction conditions is 20°C to 80°C, and the reaction time is 1 hour to 24 hours.

[0019] In some embodiments, the mass ratio of the silicon-carbon composite material, the oxidant, and the polyhedral oligomeric silsesquioxane is 1:(0.1-0.3):(0.03-0.10).

[0020] In some embodiments, the pretreatment of the silicon-carbon composite material to coat the surface of the silicon-carbon composite material with the polyhedral oligomeric silsesquioxane includes: The silicon-carbon composite material is dispersed in a third solvent, and then the polyhedral oligomeric silsesquioxane is added. A fourth solvent is added dropwise during stirring to obtain the active particles.

[0021] In some embodiments, the third solvent includes at least one of ether solvents, ketone solvents, ester solvents, aromatic hydrocarbon solvents, halogenated hydrocarbon solvents, and amide solvents; Preferably, the third solvent includes at least one of tetrahydrofuran, acetone, and toluene.

[0022] In some embodiments, the method further includes adding an auxiliary agent to the reaction solution and carrying out a crosslinking reaction under a second reaction condition; Preferably, the additives include photoinitiators, thermal initiators, curing agents, or crosslinking agents; Preferably, the reaction temperature in the second reaction condition is 40℃~80℃; Preferably, the mass ratio of the silicon-carbon composite material, the additive, and the polyhedral oligomeric silsesquioxane is 1:(0.01-0.03):(0.03-0.10).

[0023] In some embodiments, the fourth solvent includes at least one of alcohol solvents, water, alkane solvents, and nitrile solvents.

[0024] According to another aspect of the present invention, the present invention also provides a negative electrode sheet, comprising: a current collector, and a negative electrode active material layer on at least one surface of the current collector in the thickness direction; The negative electrode active material layer includes the negative electrode material described in any of the above embodiments, or the negative electrode material prepared by the preparation method described in any of the above embodiments.

[0025] According to another aspect of the present invention, the present invention also provides a secondary battery, comprising: the negative electrode sheet described in any of the above embodiments.

[0026] Implementing the technical solution of the present invention has at least the following beneficial effects: The negative electrode material of this invention effectively preserves the complete cage structure of the POSS molecule and its weak Li-linked structure by directly setting a shell of polyhedral oligomeric silsesquioxane containing a complete cage structure on the core surface of a silicon-carbon composite material. + Interfacial electronic effects involving coordination and strong solvent affinity; among which, the shell can actively reconstruct Li at the electrode / electrolyte interface. + The solvation structure induces the formation of a thin and dense SEI film rich in inorganic substances such as LiF, thereby significantly suppressing the repeated SEI rupture and rapid capacity decay caused by silicon volume expansion, and achieving a significant improvement in cycle stability and coulombic efficiency.

[0027] Additional aspects and advantages of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Detailed Implementation

[0028] The technical solution of the present invention and how the technical solution of the present invention solves the above-mentioned technical problems are described in detail below with specific embodiments. These specific embodiments can be combined with each other, and the same or similar concepts or processes may not be described again in some embodiments. The embodiments of the present invention will be described below in conjunction with the embodiments.

[0029] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges or individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0030] Unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form new technical solutions.

[0031] Unless otherwise specified, all technical features and optional technical features of this invention can be combined to form new technical solutions.

[0032] Currently, in related technologies, silicon-carbon anode materials for lithium-ion batteries typically involve surface modification with polyhedral oligomeric silsesquioxanes. This is usually achieved by using the polyhedral oligomeric silsesquioxanes as precursors and subjecting them to high-temperature carbonization to transform them into SiOC ceramic or carbon material coatings. However, the inventors of this invention, through in-depth research and analysis, discovered that this treatment method completely destroys the intact cage-like structure of the polyhedral oligomeric silsesquioxanes, causing them to lose their weak Li-linked properties. + Intrinsic interface modulation functions such as coordination and strong solvent affinity cannot actively induce the formation of a thin, dense SEI film rich in inorganic substances at the electrode / electrolyte interface. Furthermore, the carbonization-formed coating only provides a physical barrier and does not protect Li. + Solvated structures lack the ability to be actively controlled, making it difficult to fundamentally solve the problems of repeated SEI rupture and rapid capacity decay caused by silicon volume expansion.

[0033] In view of the technical problems existing in the prior art, the present invention proposes a negative electrode material and its preparation method, a negative electrode sheet, and a secondary battery. The negative electrode material includes active particles, which are composed of a core and a shell covering the surface of the core. The core comprises a silicon-carbon composite material, and the shell comprises a polyhedral oligomeric silsesquioxane, wherein the polyhedral oligomeric silsesquioxane exists with its complete cage structure, that is, the shell is a non-carbonized, non-destructive POSS (polyhedral oligomeric silsesquioxane) bulk layer. By retaining the complete cage structure of the POSS and utilizing its intrinsic weak Li- ionization... + Coordination and strong solvent affinity electron effects can actively reconstruct Li at the electrode / electrolyte interface. + The solvation structure induces preferential decomposition of anions, thereby forming a thin, dense SEI film rich in inorganic substances such as LiF on the silicon-carbon surface. The SEI film is not easily broken during silicon volume expansion, effectively suppressing the continuous decomposition of the electrolyte and rapid capacity decay, thus improving the cycling stability and coulombic efficiency of the electrode.

[0034] The specific technical solution of the present invention is as follows: [Anode Material] In some embodiments of the present invention, a negative electrode material is provided, comprising: active particles, the active particles comprising a core and a shell covering the surface of the core; the core comprises a silicon-carbon composite material, and the shell comprises a polyhedral oligomeric silsesquioxane.

[0035] As examples, silicon-carbon composite materials include, but are not limited to, silicon-intercalated mesoporous carbon, Si@C, and Si / C@graphene composite materials. Polyhedral oligomeric silsesquioxanes (POSS) are inorganic cage-like frameworks formed by alternating silicon (Si) and oxygen (O) atoms, with chemical properties similar to siloxanes. The core of active particles includes silicon-carbon composite materials, and the shell includes POSS, giving the active particles a core-shell structure.

[0036] The researchers of this invention discovered that when POSS is modified by coating it onto the surface of a silicon-carbon anode material after high-temperature carbonization, although it can transform POSS into silicon-oxygen-carbon ceramics or carbonaceous materials and utilize its derived network framework as a physical barrier, it completely destroys the original complete organic-inorganic hybrid cage structure of POSS. This structural destruction means that the atomically symmetrical and hollow cage of the POSS molecule no longer exists, and its series of intrinsic functions are lost. For example, the original complete cage structure has unique electronic effects, enabling it to generate weak coordination with lithium ions and exhibit strong affinity for electrolyte solvent molecules. Thus, it can actively participate in the solvation structure of lithium ions at the interface between the electrode and the electrolyte, performing interface regulation and inducing the formation of a thin, dense solid electrolyte interphase (SEI) film rich in inorganic components such as lithium fluoride. However, once the cage structure is carbonized and thermally decomposed, the above-mentioned active interface regulation function is completely lost, and POSS merely functions as a structural framework for a carbon or silicon source. Therefore, the potential of POSS in interfacial chemical regulation cannot be fully utilized, and the resulting SEI film is often non-uniform and has poor stability. It is prone to repeated rupture during the huge volume expansion and contraction of the silicon anode, resulting in continuous consumption of electrolyte and loss of active material, which in turn adversely affects the cycle stability and coulombic efficiency of the electrode.

[0037] Furthermore, this invention forms a complete POSS molecular coating layer, i.e., a shell, on the surface of silicon-carbon composite material particles, with an intact cage-like structure. This shell is not an inorganic ceramic layer obtained through high-temperature conversion, but rather an organic-inorganic hybrid layer composed of a POSS matrix with a complete molecular structure. Thus, the shell on the resulting active particles provides both physical isolation and protection while retaining the electronic effects of weak lithium-ion coordination and strong solvent affinity of the POSS molecules. Consequently, when the active particles are used as a negative electrode material in a battery, the POSS coating layer on their surface can actively reconstruct the lithium-ion solvation structure at the interface, attracting anions (such as hexafluorophosphate) from the electrolyte to accumulate on the electrode surface, preferentially decomposing them before solvent molecules, thereby forming a thin and dense SEI film rich in inorganic substances (especially lithium fluoride). Moreover, the SEI film has excellent mechanical strength and ionic conductivity, which can adapt to the volume changes of silicon particles during cycling and is not easily broken. This effectively suppresses the continuous consumption of active lithium and electrolyte caused by repeated SEI repair, and significantly improves the cycle stability and coulombic efficiency of the battery.

[0038] In some embodiments, the silicon-carbon composite material includes, but is not limited to, one or more of nano-silicon / graphite composites, nano-silicon / amorphous carbon composites, and porous silicon-carbon spheres.

[0039] In some embodiments, the polyhedral oligomeric silsesquioxane is a cage-type polysilsesquioxane.

[0040] In some embodiments, the general chemical formula of the cage-like polysilsesquioxane is (RSiO 1.5 ) n Wherein, n = 6, 8, 10 or 12; preferably, n = 8; R is selected from hydrogen, alkyl, aryl, epoxy, amino, vinyl, mercapto or acryloyloxy.

[0041] For example, n represents the number of silicon atoms in the cage structure, i.e., the degree of polymerization, reflecting the size of the cage. n can be 6, 8, 10, or 12, corresponding to T6, T8, T10, or T12 cage structures, respectively. Among them, the T8 cage with n=8 has the best structural symmetry, and it has advantages in both synthesis and structural stability. R reflects the solubility, reactivity, and interaction mode of the POSS molecule with the silicon-carbon core surface. The R group can be an inert group, such as hydrogen, alkyl (e.g., methyl, ethyl, isobutyl, isooctyl, etc.), aryl (e.g., phenyl), etc. POSS with such groups mainly attaches to the core surface through non-covalent physical forces.

[0042] Optionally, to enhance the bonding force between the POSS coating layer, i.e., the shell and the silicon-carbon core, the R group preferably contains reactive functional groups. Reactive functional groups can provide anchor points for subsequent chemical bonding. When the POSS molecule carries such groups, it can chemically react with the active sites on the surface of the silicon-carbon core to form covalent bonds, achieving chemical grafting or cross-linking networks. For example, the R group can be selected from epoxy, amino, vinyl, mercapto, or acryloyloxy groups. Taking amino POSS as an example, the -NH2 group on its molecule can undergo a condensation reaction with the carboxyl or hydroxyl groups generated after activation treatment on the silicon-carbon surface, forming stable amide bonds or hydrogen bonds followed by further dehydration and covalent bonding. Or, taking vinyl POSS as an example, the C=C double bond on its molecule can undergo free radical polymerization under the action of an initiator or cross-link with other compounds containing unsaturated bonds, forming a continuous, network-structured POSS molecular film in situ on the silicon-carbon surface, firmly encapsulating the particles within it. Taking epoxy-based POSS as an example, its epoxy groups can undergo ring-opening addition reactions with hydroxyl or amino groups on the silicon-carbon surface to achieve grafting. Compared with simple physical adsorption, the above-mentioned chemical reaction anchoring method can provide stronger binding force and has a greater advantage in resisting the stress generated by silicon volume expansion, effectively preventing the coating layer from peeling off during long-term cycling.

[0043] In some embodiments, the thickness of the shell is 2nm to 50nm.

[0044] For example, the thickness of the shell can be any value or any value between any two of the following: 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, 12nm, 14nm, 16nm, 18nm, 20nm, 22nm, 24nm, 26nm, 28nm, 30nm, 35nm, 40nm, 45nm, or 50nm. In this way, the POSS shell provides sufficient physical isolation and complete interface control while keeping the resistance to lithium-ion cross-layer transport at a low level. The thickness and uniformity of the POSS coating layer affect the resistance to lithium-ion transport across the shell and the shell's protective effect on the core. If the thickness is less than the above range, i.e., the POSS shell is too thin, it may not be able to form a continuous and complete coverage of the silicon-carbon core, resulting in unprotected exposed areas. This prevents the effective interface control function, leading to localized overgrowth of the SEI film at these defects and affecting electrochemical performance. If the thickness exceeds the above range, i.e., the POSS casing is too thick, it will increase the solid-phase diffusion path length of lithium ions, increase the interface impedance, and lead to a decrease in the battery's rate performance and reversible capacity. In addition, an excessively thick non-conductive organic coating layer may also reduce the electronic conductivity of the electrodes.

[0045] In some embodiments, the median particle size D of the active particles 50The size ranges from 1 μm to 28 μm, preferably from 3 μm to 22 μm, and more preferably from 5 μm to 13 μm.

[0046] For example, the median particle size D of the active particles 50 The particle size can be any value within the range of 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 12μm, 14μm, 16μm, 20μm, 24μm, or 28μm, or any value between any two points. A particle size within this range balances electrode processing performance, compaction density, and electrolyte wettability. If the particle size is too large, the silicon material at the center of the active particle may not be effectively utilized due to its distance from the conductive network, and a large stress difference will be generated inside the particle during charging and discharging, easily leading to particle cracking. If the particle size is too small, the specific surface area is too large, which increases side reactions with the electrolyte, resulting in a decrease in the first-cycle coulombic efficiency, and excessive interparticle contact interfaces will reduce the electrode compaction density.

[0047] In some embodiments, the median particle size D of the nucleus 50 The particle size is 0.8 μm to 5 μm, preferably 0.8 μm to 3 μm. For example, the median particle size D of the nucleus... 50 It can be any point value among 0.8μm, 1.0μm, 1.2μm, 1.4μm, 1.6μm, 1.8μm, 2.0μm, 2.2μm, 2.4μm, 2.6μm, 2.8μm, 3.0μm, 3.5μm, 4.0μm, 4.5μm or 5.0μm, or any point value between any two points.

[0048] In some embodiments, the pore size of the porous silicon carbide spheres is 1 nm to 100 nm, preferably 5 nm to 50 nm, and more preferably 10 nm to 25 nm.

[0049] For example, the pore size of the porous silicon carbide spheres can be any value among 1nm, 2nm, 3nm, 4nm, 5nm, 6nm, 8nm, 10nm, 12nm, 15nm, 20nm, 25nm, 30nm, 50nm, 75nm, or 100nm, or any value between any two points. When using porous silicon carbide spheres as the core, the pore size inside the porous silicon carbide spheres is within the above range, which can effectively achieve efficient ion transport and effective volume buffering. The pore structure not only provides a near-end buffer space for the volume expansion of silicon, but also serves as a channel for the electrolyte to enter the interior of the particles, ensuring a rapid supply of lithium ions.

[0050] [Preparation methods for negative electrode materials] In some embodiments of the present invention, a method for preparing a negative electrode material is also provided, comprising the following steps: S101. Pretreatment of silicon-carbon composite material is performed to coat the surface of silicon-carbon composite material with polyhedral oligomeric silsesquioxane to obtain active particles.

[0051] As an example, silicon-carbon composite particles serve as the core, supporting electrochemical lithium storage. Silicon provides a high theoretical specific capacity, enhancing energy density, while the carbon matrix acts as a buffer against the drastic volume changes of silicon during charging and discharging, and provides a conductive network for the entire particle. There are various ways to combine the carbon matrix with silicon. For instance, silicon-carbon composites can be a combination of nano-silicon and graphite. The layered structure of graphite provides excellent conductivity and structural stability, allowing nano-silicon particles to be embedded or attached between or to the surface of graphite layers. The graphite matrix effectively disperses the silicon particles and buffers their volume expansion, while providing excellent electron transport channels. Alternatively, silicon-carbon composites can also be a combination of nano-silicon and amorphous carbon. Amorphous carbon typically exhibits isotropy and high porosity, enabling more comprehensive encapsulation and isolation of silicon particles, providing a balanced stress buffering effect. Alternatively, the silicon-carbon composite material can also be a porous silicon-carbon sphere, where silicon and carbon are constructed into a spherical particle with internal pores. These pores provide buffer space for the volume expansion of silicon, reducing the extent of outward expansion and thus helping to maintain the overall structural stability of the electrode. It is understood that the aforementioned core can be obtained through ball milling, spray drying, chemical vapor deposition, or liquid-phase solidification. This invention is not specifically limited in its application.

[0052] Furthermore, after obtaining the core containing the silicon-carbon composite material, the core is further pretreated to coat its surface with a shell. To ensure the integrity of the POSS molecular cage structure, the coating layer formation step needs to be carried out at a temperature that does not cause thermal decomposition of the molecular cage structure. Researchers of this invention have discovered that although the cage structure of POSS possesses a certain degree of thermal stability, above a certain temperature, its organic groups will break and rearrange, and the inorganic silicon-oxygen framework will collapse, ultimately transforming into amorphous silicon dioxide or silicon-oxygen-carbon materials. Thermal decomposition typically occurs at high temperatures and is related to conditions such as the type of R groups on the POSS molecule and the atmospheric environment. To completely avoid structural damage, the temperature of the entire coating step is controlled under mild conditions far below its decomposition temperature, for example, a reaction temperature not exceeding 100°C. Under these conditions, the organic-inorganic hybrid cage framework of the POSS molecule is absolutely stable, its molecular structure is not destroyed, and the functional groups are well preserved. Achieving POSS coating through liquid-phase reaction or mild heating assistance, rather than high-temperature pyrolysis, is key to ensuring the structural integrity of POSS from a process perspective.

[0053] The above steps yielded active particles with a core-shell structure, consisting of a core of silicon-carbon composite particles and a shell of POSS molecules with their complete cage-like structure. The shell, or POSS coating layer, exists as a non-carbonized, non-destructive POSS body layer. The adhesion between the POSS coating layer and the silicon-carbon core can take various forms. For example, POSS molecules can adhere to the silicon-carbon core surface through physical adsorption and intermolecular forces; or through van der Waals forces, hydrogen bonds, or strong electrostatic interactions. This method typically occurs during the self-assembly and precipitation of POSS molecules on the core surface using unsuitable solvents. Alternatively, POSS molecules can adhere to the silicon-carbon core surface through a more robust chemical grafting method. The reactive functional groups on the POSS molecules can chemically react with pre-introduced or inherent active sites (such as hydroxyl and carboxyl groups) on the silicon-carbon core surface, forming stable covalent bonds. This results in extremely strong bonding between the POSS coating layer and the core, ensuring that the coating layer does not easily detach even under cyclic stress caused by the large volume expansion and contraction of the silicon material, thus guaranteeing the durability of the interface protection function.

[0054] In some embodiments, the silicon-carbon composite material is pretreated to coat the surface of the silicon-carbon composite material with polyhedral oligomeric silsesquioxane, including: S201. Disperse the silicon-carbon composite material in a first solvent, add an oxidant, and obtain activated particles.

[0055] S201. Dissolve the polyhedral oligomeric silsesquioxane in the second solvent, add the activated particles, and stir under the first reaction conditions to obtain the activated particles.

[0056] For example, the active particles are prepared using a chemical grafting method. In step S201, the silicon-carbon composite material particles are first oxidized and activated, and the oxidant can be hydrogen peroxide, nitric acid, etc. Then, the activated particles and POSS are added to the second solvent, and after reacting for a period of time within a certain temperature range, the active particles are obtained after precipitation, filtration, washing, and drying.

[0057] In some embodiments, the silicon-carbon composite material is pretreated to coat the surface of the silicon-carbon composite material with polyhedral oligomeric silsesquioxane, including: S301. The silicon-carbon composite material is dispersed in a third solvent, and then polyhedral oligomeric silsesquioxane is added. A fourth solvent is added dropwise during stirring to obtain active particles.

[0058] For example, the active particles are prepared by a self-assembly cross-linking coating method. The silicon-carbon composite material is dispersed in a third solvent, and then POSS is added. The third solvent is a good solvent for POSS and can dissolve POSS well. Then a fourth solvent is added. The fourth solvent is a poor solvent for POSS. With the addition of the fourth solvent, the polarity of the system increases. Due to the decrease in solubility, the polyhedral oligomeric silsesquioxane gradually precipitates on the surface of the silicon-carbon spheres and self-assembles into a uniform coating layer, i.e., the shell.

[0059] In some embodiments, the first solvent includes, but is not limited to, alcohol solvents (such as ethanol, methanol, isopropanol), ketone solvents (such as acetone), ether solvents (such as tetrahydrofuran), amide solvents (such as N,N-dimethylformamide, N-methylpyrrolidone), water, or any combination thereof.

[0060] In some embodiments, the oxidant includes, but is not limited to, hydrogen peroxide, nitric acid, sulfuric acid, ozone, piranha solution, or any combination thereof.

[0061] In some embodiments, the second solvent includes, but is not limited to, one or more of aromatic hydrocarbon solvents, ether solvents, halogenated hydrocarbon solvents, ketone solvents, and ester solvents.

[0062] In some embodiments, the reaction temperature in the first reaction conditions is 20°C to 80°C, and the reaction time is 1 hour to 24 hours. Exemplarily, the reaction temperature can be any value among 20°C, 40°C, 60°C, and / or 80°C, or any value between any two of these values; the reaction time can be any value among 1 hour, 1 hour, 3 hours, 8 hours, 15 hours, 18 hours, 21 hours, or 24 hours, or any value between any two of these values.

[0063] In some embodiments, the third solvent includes, but is not limited to, solvents selected from ether solvents (such as tetrahydrofuran, 1,4-dioxane), ketone solvents (such as acetone, butanone), ester solvents (such as ethyl acetate, butyl acetate), aromatic hydrocarbon solvents (such as toluene, xylene), halogenated hydrocarbon solvents (such as chloroform, dichloromethane), amide solvents (such as N,N-dimethylformamide, N-methylpyrrolidone), or any combination thereof.

[0064] In some embodiments, the additives include photoinitiators, thermal initiators, curing agents, or crosslinking agents. It is understood that the additives can be photoinitiators, crosslinking agents, etc., and can be selected based on the different R groups in the POSS.

[0065] For example, the photoinitiator can be 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzophenone, etc.; the thermal initiator can be azobisisobutyronitrile, benzoyl peroxide, ammonium persulfate, etc.; the curing agent can be ethylenediamine, m-phenylenediamine, phthalic anhydride, etc.; and the crosslinking agent can be hexamethylene diisocyanate, vinyltriethoxysilane, etc.

[0066] In some embodiments, the fourth solvent includes, but is not limited to, one or more of water, n-pentane, n-hexane, cyclohexane, and cyclopentane.

[0067] In some embodiments, the reaction temperature in the second reaction condition is 40°C to 80°C. Exemplarily, the reaction temperature can be any value among 40°C, 50°C, 60°C, and / or 80°C, or any value between any two of these values.

[0068] In some embodiments, the mass ratio of the silicon-carbon composite material, the oxidant, and the polyhedral oligomeric silsesquioxane is 1:(0.1–0.3):(0.03–0.10). Exemplarily, the mass ratio of the silicon-carbon composite material, the oxidant, and the polyhedral oligomeric silsesquioxane can be any value from 1:0.1:0.03, 1:0.2:0.065, 1:0.1:0.10, 1:0.3:0.03, or 1:0.3:0.10, or any ratio between any two values.

[0069] [Negative electrode plate] In some embodiments of the present invention, a negative electrode sheet is also provided, comprising: a current collector, and a negative electrode active material layer on at least one side surface of the current collector in the thickness direction; the negative electrode active material layer comprises the negative electrode material in any of the above embodiments, or the negative electrode material prepared by the preparation method in any of the above embodiments.

[0070] Optionally, the current collector can be a metal foil such as copper or copper alloy, and the negative electrode active material layer is disposed on one or both sides of the surface of the current collector in the thickness direction. The negative electrode active material layer includes a negative electrode material, binder, conductive agent, etc. The negative electrode material is the negative electrode material in any embodiment of the present invention.

[0071] [Rechargeable Battery] In some embodiments of the present invention, a secondary battery is also provided, comprising: the negative electrode sheet in any of the above embodiments.

[0072] Optionally, the secondary battery may further include a positive electrode, a negative electrode, and a separator. As an example, the positive electrode includes a positive current collector and an active coating disposed on at least one surface of the positive current collector along its thickness direction. The aforementioned "active coating disposed on at least one surface of the positive current collector" means that the positive active layer can be disposed on one surface of the positive current collector along its thickness direction, or on two surfaces of the positive current collector along its thickness direction. Here, "surface" can be the entire area of ​​the positive current collector or a portion of the positive current collector; this application does not have any particular limitation, as long as the purpose of this application is achieved. In this invention, the separator is not particularly limited, as long as the purpose of this invention is achieved. Optionally, the separator includes, but is not limited to, a polymer separator of at least one selected from polyethylene, polypropylene, polyacrylonitrile, polysulfonyl, polyarylethersulfone, polyvinyl alcohol, and polyvinylidene fluoride.

[0073] Optionally, the secondary battery may include an outer packaging that can be used to encapsulate the aforementioned electrode assembly and electrolyte. The outer packaging of the secondary battery may be a rigid shell, such as a hard plastic shell, aluminum shell, steel shell, etc. Specifically, the rigid shell may include a housing and a cover plate, wherein the housing may include a bottom plate and a side plate connected to the bottom plate, the bottom plate and the side plate forming a receiving cavity, the housing having an opening communicating with the receiving cavity, and the cover plate being able to cover the opening to close the receiving cavity, the electrode assembly being encapsulated in the aforementioned receiving cavity, and the electrolyte in any of the above embodiments being immersed in the electrode assembly; it may also be a soft package, such as a pouch-type soft package; the material of the soft package may be plastic, and examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0074] The diaphragm used in this embodiment is a diaphragm used in the art and is not particularly limited herein. All solvents and substances in this invention are commercially available.

[0075] Since the battery provided in this embodiment of the invention adopts all the technical solutions of the above embodiments, it has at least all the beneficial effects brought about by the technical solutions of the above embodiments, and will not be described in detail here.

[0076] The present invention will be specifically described below with reference to the embodiments, but the implementation and protection of the present invention are not limited thereto. The following embodiments are only some embodiments of the present invention and are not intended to limit the present invention.

[0077] Example 1 S11. Take 10g of nano-silicon / graphite composite powder (silicon content 30%), disperse it in 100mL of ethanol, add 5mL of hydrogen peroxide (30%), stir at 60℃ for 2 hours, filter, wash, and vacuum dry to obtain surface-hydroxylated silicon-carbon particles.

[0078] S12. Dissolve 2g of aminopropyl isobutyl POSS (containing -NH2 group) in 50mL of toluene, add the above-mentioned hydroxylated silicon carbon particles, and reflux at 80℃ for 12 hours.

[0079] S13. After the reaction is complete, filter the mixture, wash it three times alternately with toluene and ethanol, and dry it under vacuum at 60°C to obtain a silicon-carbon composite material with amino POSS bulk coating.

[0080] Example 2 S21. Take 5g of porous silicon carbide spheres (pore size ~10nm) and disperse them in 50mL of tetrahydrofuran.

[0081] S22. Dissolve 1g of octavinylPOSS in 20mL of tetrahydrofuran, and slowly add it dropwise into the above dispersion while stirring for 30 minutes.

[0082] S23. Slowly add 100 mL of deionized water while stirring to allow POSS to precipitate and self-assemble on the surface of silicon carbide spheres. Add 0.1 g of photoinitiator (such as 1173) and irradiate under a UV lamp (365 nm) for 30 minutes to induce crosslinking of the vinyl groups.

[0083] S24. Centrifuge, wash three times with ethanol, and vacuum dry at 60°C to obtain a porous silicon-carbon composite material coated with cross-linked POSS.

[0084] Example 3 S31. Take 10g of nano-silicon / graphite composite powder (silicon content 30%), disperse it in 100g of nitric acid aqueous solution with a mass fraction of 40%, stir at 60℃ for 2 hours, filter, wash until pH is 7, and vacuum dry to obtain surface hydroxylated silicon carbon particles.

[0085] S32. Dissolve 2g of aminopropyl isobutyl POSS (containing -NH2 group) in 50mL of toluene, add the above-mentioned hydroxylated silicon carbon particles, and reflux at 80℃ for 12 hours.

[0086] S33. After the reaction is complete, filter the mixture, wash it three times alternately with toluene and ethanol, and dry it under vacuum at 60°C to obtain a silicon-carbon composite material with amino POSS bulk coating.

[0087] Example 4 Replace the aminopropyl isobutyl POSS (containing -NH2 group) in Example 1 with monoepoxy heptaisobutylsiloxane (epoxy POSS).

[0088] Example 5 S51. Ten parts by weight of silicon-carbon composite material (D50=8μm) were dispersed in 100 parts by weight of ethanol / water mixed solution (ethanol:water = 9:1, volume ratio). One part by weight of γ-methacryloyloxypropyltrimethoxysilane (KH-570) was added, and the pH was adjusted to 4-5 with acetic acid. The mixture was stirred at 60°C for 6 hours. After the reaction was completed, the mixture was washed three times with ethanol and dried under vacuum at 60°C for 12 hours to obtain silicon-carbon particles with double bonds on their surface.

[0089] S52. Dissolve 1.0 parts by weight of monothiol heptaisobutyl POSS and 0.05 parts by weight of photoinitiator 1173 in 50 parts by weight of tetrahydrofuran, and add the aforementioned silicon-carbon particles with double bonds on their surface. Under irradiation with a 365 nm ultraviolet lamp (light intensity 100 mW / cm²), stir at room temperature for 30 minutes.

[0090] S53. After the reaction is complete, the mixture is filtered, washed three times alternately with tetrahydrofuran and ethanol, and dried under vacuum at 60°C for 12 hours to obtain a silicon-carbon composite material with mercapto-POSS bulk coating.

[0091] Example 6 S61, 10g of silicon-carbon composite material (D) 50 A silicon-carbon particle with a surface carboxylation level of 8 μm was added to a mixed solution of 60 mL concentrated sulfuric acid (98 wt%) and 20 mL concentrated nitric acid (68 wt%) (volume ratio of concentrated sulfuric acid to concentrated nitric acid 3:1). The reaction was stirred at 60–70 °C for 2–4 hours. The nitric acid in the mixed acid provides oxidizing power, while the sulfuric acid provides a strongly acidic environment. The synergistic effect of the two can introduce oxygen-containing functional groups such as carboxyl groups (-COOH) onto the surface of the silicon-carbon material. After the reaction was completed, the material was allowed to cool naturally to room temperature, washed repeatedly with a large amount of deionized water until the pH reached 6–7, filtered, and then vacuum dried at 60 °C for 12 hours to obtain surface carboxylated silicon-carbon particles.

[0092] S62. Dissolve 1.0 g of aminoPOSS (aminopropyl isobutylPOSS) and 0.05–0.10 g of catalyst (DCC or EDC·HCl) in 50 mL of anhydrous toluene, and add the above-mentioned carboxylated silicon carbon particles. Reflux at 80 °C for 12 hours. Under the action of the catalyst, the -NH2 group of aminoPOSS undergoes an amidation reaction with the -COOH group on the surface of silicon carbon, forming a stable amide bond (-CO-NH-) covalently linked.

[0093] S63. After the reaction is complete, filter the mixture, wash it three times alternately with toluene and ethanol, and dry it under vacuum at 60°C for 12 hours to obtain a silicon-carbon composite material with amino POSS bulk coating.

[0094] Comparative Example 1 The composite material prepared in Example 1 was calcined at 800°C in an inert gas environment for 12 hours.

[0095] Comparative Example 2 Only silicon-carbon composite materials are used as the negative electrode.

[0096] Battery assembly: 1. Positive electrode sheet: NCM811 positive electrode active material, acetylene black conductive agent, and PVDF binder are mixed in a mass ratio of 95:2.5:2.5. An appropriate amount of NMP solvent is added and stirred evenly. The mixture is coated onto a 15μm thick aluminum foil, dried at 95℃, rolled and cut to obtain the positive electrode sheet.

[0097] 2. Negative electrode sheet: The prepared POSS body coated with silicon-carbon composite material, SuperP conductive agent, and CMC / SBR binder are mixed in a mass ratio of 8:1:1, deionized water is added and stirred evenly, coated on copper foil, dried and cut into round sheets with a diameter of 12mm to obtain the negative electrode sheet.

[0098] 3. Separator: The separator is a Celgard2400 polypropylene microporous membrane. The separator is stamped into small round pieces with a diameter of about 16 to 19 mm. The diameter needs to be slightly larger than the positive and negative electrode pieces to ensure complete isolation between the positive and negative electrodes and avoid short circuits.

[0099] 4. Electrolyte: In an argon glove box, dissolve LiPF6 in a mixed solvent of EC / EMC / DMC (volume ratio 1:1:1) to prepare a 1.0 mol / L solution. Add 10 wt% FEC and 1.0 wt% VC, stir well, and seal for storage.

[0100] Assembly: In an argon-filled glove box (H2O<0.1ppm, O2<0.1ppm), assemble the CR2032 coin cell in the following order: positive electrode shell, silicon-carbon negative electrode sheet, 50μL electrolyte, separator (Celgard2400, diameter 18mm), 50μL electrolyte, lithium sheet (diameter 16mm), gasket, spring sheet, and negative electrode shell. After sealing and compacting, let it stand for 12 hours.

[0101] Test case 1. Particle Size: The sample to be tested (e.g., silicon-carbon composite powder) is dispersed in a solvent containing a small amount of dispersant (e.g., 0.2 wt% aqueous solution of polyoxyethylene (20) sorbitan monolaurate). The dispersion is achieved by ultrasonic vibration, forming a uniform suspension. Then, a laser diffraction particle size analyzer (e.g., similar equipment manufactured by HORIBA, Malvern Panalytical, Shimadzu, etc.) is used for measurement. Based on the recorded scattered light intensity distribution, the instrument calculates the volumetric particle size distribution of the sample using an optical model. The particle size value corresponding to a cumulative volume distribution reaching 50% is the median particle size D. 50 .

[0102] 2. Cycling performance: After the initial charge and discharge cycle, it is charged at a constant current rate of 0.2C to 0.005V (vsLi). + / Li), then discharge at a constant current rate of 0.2C to 1.5V (vsLi). + (Li) was subjected to long-term cycle testing. Discharge capacity and coulombic efficiency were recorded after each cycle. The test was terminated when the battery discharge capacity dropped to 80% of the initial discharge capacity, and the number of cycles was recorded. Capacity retention was calculated using the following formula: Capacity retention (%) = (Discharge capacity of Nth cycle / Discharge capacity of 1st cycle) × 100%. Three parallel samples were tested in each group, and the average result was taken.

[0103] 3. Coulombic Efficiency: After the assembled CR2032 coin cells were placed in a constant temperature chamber at 25±1℃ for 12 hours, constant current charge-discharge tests were performed using the Blue Battery Testing System. The first charge (lithium intercalation) was performed at a constant current rate of 0.1C to 0.005V (vsLi). + / Li), then discharged at a constant current rate of 0.1C to 1.5V (vsLi). + / Li). The initial coulombic efficiency is calculated using the following formula: Initial coulombic efficiency (%) = (Initial discharge capacity / Initial charge capacity) × 100%.

[0104] The test results are shown in Table 1.

[0105] Table 1 As can be seen from Table 1, the battery capacity retention rate and coulombic efficiency of the negative electrode assembly in Examples 1 to 6 are better than those of the batteries in the comparative examples.

[0106] The parts of this invention not described in detail are techniques known to those skilled in the art.

[0107] In the above embodiments, the descriptions of each embodiment have their own emphasis. For parts not described in detail in a certain embodiment, please refer to the relevant descriptions of other embodiments. The technical features of the above embodiments can be combined arbitrarily. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as the combination of these technical features does not contradict each other, it should be considered within the scope of this specification.

[0108] Other embodiments of the invention will readily occur to those skilled in the art upon consideration of the specification and practice of the invention disclosed herein. This invention is intended to cover any variations, uses, or adaptations of the invention that follow the general principles of the invention and include common knowledge or customary techniques in the art not disclosed herein. The specification and examples are to be considered exemplary only, and the true scope and spirit of the invention are indicated by the following claims.

[0109] It should be noted that the terms "and / or" or " / " used herein are merely descriptions of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. The singular forms "a," "described," and "the" used in the embodiments of the invention and the appended claims are also intended to include the plural forms, unless the context clearly indicates otherwise.

[0110] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, then the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, then the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single element or multiple elements. Item B may contain a single element or multiple elements. Item C may contain a single element or multiple elements.

[0111] It should be understood that the present invention is not limited to the precise structure described above, and various modifications and changes can be made without departing from its scope. The scope of the invention is limited only by the appended claims.

Claims

1. A negative electrode material, characterized in that, include: Active particles, the active particles comprising a core and a shell covering the surface of the core; The core comprises a silicon-carbon composite material, and the shell comprises a polyhedral oligomeric silsesquioxane.

2. The negative electrode material according to claim 1, characterized in that, The silicon-carbon composite material includes at least one of nano-silicon / graphite composite, nano-silicon / amorphous carbon composite, and porous silicon-carbon spheres; And / or, the polyhedral oligomeric silsesquioxane is a cage-type polysilsesquioxane.

3. The negative electrode material according to claim 2, characterized in that, The general chemical formula of the cage-like polysilsesquioxane is (RSiO 1.5 ) n Where n = 6, 8, 10 or 12; preferably, n = 8; R is selected from hydrogen, alkyl, aryl, epoxy, amino, vinyl, mercapto, or acryloyloxy.

4. The negative electrode material according to any one of claims 1 to 3, characterized in that, Satisfying at least one of features (1) to (4): (1) The thickness of the shell is 2nm~50nm; (2) The median particle size D of the active particles 50 The micrometer size is 1μm to 28μm, preferably 3μm to 22μm, and more preferably 5μm to 13μm. (3) The median particle size D of the nucleus 50 The micrometer size is 0.8μm to 5μm, preferably 0.8μm to 3μm; (4) The pore size of the porous silicon carbide sphere is 1 nm to 100 nm, preferably 5 nm to 50 nm, and more preferably 10 nm to 25 nm.

5. A method for preparing a negative electrode material, characterized in that, Includes the following steps: Pretreatment of silicon-carbon composite materials; The polyhedral oligomeric silsesquioxane is coated onto the surface of the silicon-carbon composite material to obtain active particles.

6. The method for preparing the negative electrode material according to claim 5, characterized in that, The pretreatment of the silicon-carbon composite material to coat the surface of the silicon-carbon composite material with the polyhedral oligomeric silsesquioxane includes: The silicon-carbon composite material is dispersed in a first solvent and subjected to oxidation or plasma treatment to obtain activated particles. The polyhedral oligomeric silsesquioxane is dissolved in a second solvent, and the activated particles are added. The mixture is stirred under the first reaction conditions to obtain the activated particles.

7. The method for preparing the negative electrode material according to claim 6, characterized in that, Satisfying at least one of features (1) to (5): (1) The first solvent includes at least one of alcohol solvents, ketone solvents, ether solvents, amide solvents and water; Preferably, the first solvent includes at least one of ethanol, isopropanol, and tetrahydrofuran; (2) The oxidation treatment includes adding an oxidant to the reaction solution, wherein the oxidant includes at least one of hydrogen peroxide, nitric acid, sulfuric acid, ozone and piranha solution; (3) The second solvent includes one or more of aromatic hydrocarbon solvents, ether solvents, halogenated hydrocarbon solvents, ketone solvents, and ester solvents; Preferably, the second solvent includes one or more of toluene, xylene, tetrahydrofuran, and chloroform; (4) The reaction temperature in the first reaction condition is 20℃~80℃, and the reaction time is 1h~24h; (5) The mass ratio of the silicon-carbon composite material, the oxidant and the polyhedral oligomeric silsesquioxane is 1:(0.1-0.3):(0.03-0.10).

8. The method for preparing the negative electrode material according to claim 5, characterized in that, The pretreatment of the silicon-carbon composite material to coat the surface of the silicon-carbon composite material with the polyhedral oligomeric silsesquioxane includes: The silicon-carbon composite material is dispersed in a third solvent, and then the polyhedral oligomeric silsesquioxane is added. A fourth solvent is added dropwise during stirring to obtain the active particles.

9. The method for preparing the negative electrode material according to claim 8, characterized in that, Satisfying at least one of features (1) to (3): (1) The third solvent includes at least one of ether solvents, ketone solvents, ester solvents, aromatic hydrocarbon solvents, halogenated hydrocarbon solvents and amide solvents; Preferably, the third solvent includes at least one of tetrahydrofuran, acetone, and toluene; (2) The method further includes adding an auxiliary agent to the reaction solution and carrying out a crosslinking reaction under the second reaction conditions; Preferably, the additives include photoinitiators, thermal initiators, curing agents, or crosslinking agents; Preferably, the reaction temperature in the second reaction condition is 40℃~80℃; Preferably, the mass ratio of the silicon-carbon composite material, the additive, and the polyhedral oligomeric silsesquioxane is 1:(0.01-0.03):(0.03-0.10). (3) The fourth solvent includes at least one of alcohol solvents, water, alkane solvents and nitrile solvents.

10. A negative electrode sheet, characterized in that, include: A current collector, and a negative electrode active material layer on at least one side surface of the current collector in the thickness direction; The negative electrode active material layer includes the negative electrode material according to any one of claims 1 to 4, or the negative electrode material prepared by the preparation method according to any one of claims 5 to 9.