A high-pressure lithium iron phosphate cathode material, its preparation method, and a lithium-ion battery.

By controlling the number of small particles, agglomeration rate, and particle size on the surface of large particles, and combining carbon source coating and freeze treatment, the problems of low compaction density and high agglomeration rate of lithium iron phosphate cathode materials were solved, realizing lithium iron phosphate cathode materials with high compaction density and low agglomeration rate, thereby improving the energy density and production yield of batteries.

CN123120723APending Publication Date: 2026-11-17GUANGDONG BRUNP RECYCLING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611540962.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium iron phosphate cathode materials suffer from low powder compaction density and high powder agglomeration rate, which makes it difficult to improve battery energy density and reduces mass production yield.

Method used

By controlling the number of small particles T, agglomeration rate M, and median particle size D50 attached to the surface of large particles, high-pressure lithium iron phosphate cathode material was prepared. A carbon source was mixed with low-temperature lithium iron phosphate powder in a molten state to form a carbon layer coating, which was then frozen to avoid agglomeration. Subsequently, it was carbonized at high temperature.

Benefits of technology

This achieves high compaction density and low agglomeration rate, improving the volumetric energy density and specific capacity of the battery, and ensuring the compaction performance and production yield of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120723A_ABST
    Figure CN123120723A_ABST
Patent Text Reader

Abstract

This invention discloses a high-density lithium iron phosphate cathode material, its preparation method, and a lithium-ion battery, relating to the field of lithium-ion battery cathode material technology. The high-density lithium iron phosphate cathode material satisfies the following formula: [Formula omitted for brevity]; where 10≤T≤30; 1≤M≤4; 1≤Z≤50. The preparation method includes: heating a carbon source to melt it into a liquid and atomizing it to form hot carbon source droplets; mixing the hot carbon source droplets with cold lithium iron phosphate powder in opposite directions; freezing the resulting carbon source-coated lithium iron phosphate particles to destroy their melting characteristics, followed by calcination to obtain carbon-coated lithium iron phosphate. This invention utilizes T, D... 50 By synergistically satisfying the comprehensive index of 1≤Z≤50, the microstructure of the powder is controlled as a whole, resulting in lithium iron phosphate cathode materials with high compaction density, low agglomeration rate, and high specific capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery cathode material technology, and more specifically, to a high-pressure lithium iron phosphate cathode material, its preparation method, and a lithium-ion battery. Background Technology

[0002] Lithium iron phosphate (LFP) cathode materials are widely used in power lithium batteries and energy storage batteries due to their excellent safety performance, long cycle life, low cost, and environmental friendliness. However, existing commercial LFP materials generally suffer from two major technical defects that severely restrict battery energy density and mass production processing stability.

[0003] Firstly, the powder compaction density is relatively low. Conventional lithium iron phosphate (LFP) batteries mostly use single-size particles for packing, resulting in large secondary particles with large gaps and high porosity. If the process is not properly controlled, a large number of disordered and agglomerated ultrafine particles will adhere to the surface of the large particles. Excessive small particles will increase the specific surface area of ​​the powder and increase the frictional resistance between particles. During the pressing process, bridging and springback phenomena are prone to occur, making it impossible to achieve tight packing. Ultimately, this leads to insufficient electrode compaction density, making it difficult to improve the volumetric energy density of the battery. Existing particle size gradation technologies are mostly simple physical mixing, with small particles existing in a free state. They cannot accurately adhere to the surface of large particles, resulting in poor gap filling and limited improvement in compaction density.

[0004] Secondly, the powder agglomeration rate is high. Lithium iron phosphate ultrafine particles have high surface energy and strong electrostatic adsorption. In traditional manufacturing processes, these small particles easily agglomerate and clump together. Furthermore, the uneven distribution and stacking of small particles adhering to the surface of larger particles easily lead to moisture absorption and adhesion, resulting in severe agglomeration during room temperature storage and transportation. Powder agglomeration leads to poor slurry dispersibility, uneven coating, and inconsistent electrode thickness, significantly reducing battery mass production yield. Simultaneously, the internal voids within the agglomerates further deteriorate compaction performance.

[0005] Existing technologies cannot simultaneously solve the three coupled problems of disordered adhesion of small particles on the surface of large particles, high agglomeration rate of powder, and insufficient compaction density.

[0006] In view of this, the present invention is proposed. Summary of the Invention

[0007] The purpose of this invention is to provide a high-pressure lithium iron phosphate cathode material, its preparation method, and a lithium-ion battery.

[0008] This invention is implemented as follows: In a first aspect, the present invention provides a high-pressure lithium iron phosphate cathode material that satisfies the following formula: ; In the formula, T represents the number of small particles adhering to the surface of large particles under SEM testing; M represents the agglomeration rate of the cathode material, M = residual mass of lithium iron phosphate material on a 200-mesh sieve ÷ total mass of lithium iron phosphate material × 100%; D 50 The median particle size of lithium iron phosphate powder; Where T represents the value when the unit is 1, M represents the value when the unit is % and D 50 The value corresponding to the unit is μm. The obtained Z is dimensionless, 10≤T≤30; 1≤M≤4; 1≤Z≤50.

[0009] In an optional implementation, D 50 It is 2-3 μm; And / or, the compaction density of the high-pressure lithium iron phosphate cathode material is greater than 2.6 g / cm³. 3 ; And / or, the capacity of the high-pressure lithium iron phosphate cathode material is greater than 154 mAh / g.

[0010] In a second aspect, the present invention provides a method for preparing a high-pressure lithium iron phosphate cathode material as described in any of the foregoing embodiments, comprising: The carbon source is heated and melted into a liquid, which is then atomized to form thermal carbon source droplets. The hot carbon source droplets are mixed with cold lithium iron phosphate powder in opposite directions to form carbon source-coated lithium iron phosphate particles, wherein the temperature difference between the hot carbon source droplets and the cold lithium iron phosphate powder is greater than 140°C. The carbon-coated lithium iron phosphate particles are first frozen to destroy their melting characteristics, and then calcined to obtain carbon-coated lithium iron phosphate.

[0011] In an optional embodiment, the feed mass of the hot carbon source droplets is 5% to 15% of the feed mass of the cold lithium iron phosphate powder; And / or, the temperature of the thermal carbon source droplets is 120~150℃; And / or, the temperature of the cold lithium iron phosphate powder is -60 to -20°C.

[0012] In an optional embodiment, the heating and melting temperature is 150~200°C; And / or, the atomization includes atomization using a centrifugal atomizer.

[0013] In an optional embodiment, the carbon source includes at least one of xylitol, methylparaben, and resorcinol.

[0014] In an optional embodiment, the freezing includes freezing at -60 to -80°C for 5 to 10 hours; And / or, the calcination is carried out under an inert atmosphere, the calcination temperature is 600~750℃, and the time is 2~12h.

[0015] In an optional embodiment, the preparation method of the cold lithium iron phosphate powder includes: mixing iron phosphate and lithium carbonate and then calcining at low temperature, followed by cooling and grinding.

[0016] In an optional embodiment, the iron phosphate and the lithium carbonate are mixed in a molar ratio of 1:1.01~1.03; And / or, the low-temperature calcination is carried out under an inert atmosphere, and the temperature of the low-temperature calcination is 500~600℃, and the time is 4~8h; And / or, the cooling to a temperature of -30℃ to -10℃; And / or, the grinding is carried out to a particle size of 0.3~10μm.

[0017] Thirdly, the present invention provides a lithium-ion battery comprising a high-pressure lithium iron phosphate cathode material as described in any of the foregoing embodiments or a high-pressure lithium iron phosphate cathode material prepared by a method for preparing a high-pressure lithium iron phosphate cathode material as described in any of the foregoing embodiments.

[0018] The present invention has the following beneficial effects: The high-pressure lithium iron phosphate cathode material provided by this invention satisfies the following formula: In this invention, the number of small particles T adhering to the surface of large particles under SEM testing is kept between 10 and 30, the agglomeration rate M is kept between 1 and 4, and D is kept between 1 and 4. 50 By ensuring that T, D, and Z are within a suitable range and synergistically satisfy the comprehensive index of 1≤Z≤50, overall control of the powder microstructure is achieved. This simultaneously solves the two major problems of low compaction density and easy powder agglomeration at both physical and chemical levels, taking into account compaction performance and breaking through the bottleneck of existing technologies that cannot achieve both simultaneously. This results in lithium iron phosphate cathode materials with high compaction density, low agglomeration rate, and high specific capacity. Only when T, D, and Z are within a suitable range can this be achieved. 50 When T, M, and Z all fall within a suitable range, and Z satisfies 1≤Z≤50, the material can simultaneously possess high compaction density and low agglomeration rate. If Z is too high (T is too large, M is too low, or the particle size is unsuitable) or too low (T is too small, M is too high), the material will deviate from its optimal state, resulting in decreased compaction density or increased agglomeration.

[0019] The preparation method provided by this invention mixes a carbon source with low-temperature lithium iron phosphate powder in a molten state, achieving rapid coating and solidification of the carbon layer, thus preventing hydrogen bonding and agglomeration between different particles. Subsequently, the coated lithium iron phosphate is subjected to low-temperature (freezing) treatment, causing the carbon chains to form a dense and irreversible hydrogen bond network through numerous hydroxyl, amino, and ether bonds. The molecular chains are anchored and bound by microcrystals, and the thermal motion of the chain segments is locked, preventing the restoration of molten fluidity upon heating. Therefore, no agglomeration occurs during direct carbonization at high temperatures. The prepared lithium iron phosphate cathode material possesses characteristics such as high compaction density, low agglomeration rate, and high specific capacity. Attached Figure Description

[0020] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0021] Figure 1 The SEM image provided in Example 3. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0023] This invention provides a high-pressure lithium iron phosphate cathode material that satisfies the following formula: ; In the formula, T represents the number of small particles adhering to the surface of large particles under SEM testing. M represents the agglomeration rate of the positive electrode material, M = (residual mass of lithium iron phosphate material on a 200-mesh sieve) ÷ (total mass of lithium iron phosphate material) × 100%; D 50 The median particle size of lithium iron phosphate powder; Where T represents the value when the unit is 1, M represents the value when the unit is % and D 50 The value corresponding to the unit is μm. The obtained Z is dimensionless, 10≤T≤30; 1≤M≤4; 1≤Z≤50.

[0024] The terminology is explained below: "T" refers to the number of small particles (in units) that can be identified on the surface of a single large particle under scanning electron microscopy (SEM) testing, used to characterize the precise adhesion degree of small particles on the surface of large particles. In this invention, 10≤T≤30 ensures that there are enough small particles to fill the gaps between large particles to improve compaction density, while avoiding excessive small particles that would lead to an excessively large specific surface area, excessive frictional resistance, and cause bridging and rebound.

[0025] "Agglomeration rate M" refers to the percentage of the residual mass of lithium iron phosphate material on a 200-mesh sieve to the total mass of lithium iron phosphate material. That is, M = residual mass on a 200-mesh sieve ÷ total mass of material × 100%. It is used to characterize the degree of agglomeration / agglomeration of powder. The smaller M is, the better the powder dispersion and the less likely it is to agglomerate.

[0026] “D 50 "D" refers to the median particle size (volume basis) of lithium iron phosphate powder, in μm. 50 It is 2-3 μm.

[0027] "Z" is a comprehensive index determined by three parameters: T, D50, and M. It characterizes the coupling state of the cathode material in three dimensions: the number of attached small particles, particle size, and degree of agglomeration. Only when all three are within a suitable window, causing Z to fall within the range of 1 to 50, can the material simultaneously possess high compaction density and low agglomeration rate. To facilitate the calculation of Z, in this invention, T, M, and D... 50 All values ​​are dimensionless and have no unit restriction. Specifically, T represents the value when the unit is "one", M represents the value when the unit is "%", and D... 50 The value corresponding to the unit is μm, and the obtained Z is dimensionless.

[0028] In this invention, the number of small particles T adhering to the surface of large particles under SEM testing is kept between 10 and 30, the agglomeration rate M is kept between 1 and 4, and D is kept between 1 and 4. 50 By ensuring that the three factors are within a suitable range and work together to satisfy the comprehensive index of 1≤Z≤50, a lithium iron phosphate cathode material with high compaction density, low agglomeration rate, and high specific capacity can be obtained.

[0029] It should be noted that T represents the precise number of small particles attached to the surface of large particles. This invention achieves this by controllably ensuring that an appropriate amount of small particles are tightly and uniformly attached to the surface of large particles (rather than existing in a free state or being randomly stacked), thereby precisely filling the gaps between large particles during accumulation and achieving tight packing. If T is too small (e.g., less than 10), the number of small particles on the surface of large particles is insufficient to fully fill the gaps, resulting in a high gap ratio, limited increase in compaction density, and significant rebound. If T is too large (e.g., greater than 30), there are too many and too dense small particles on the surface of large particles, significantly increasing the specific surface area of ​​the powder, increasing the frictional resistance between particles, and easily causing bridging and rebound during compaction, which in turn leads to a decrease in compaction density. Furthermore, excessive small particles can easily thicken the pack and cause agglomeration. This invention controls T within the range of 10-30, ensuring sufficient gap filling without excessive attachment. For example, the dimensionless value of T can be any one of 10, 12, 15, 18, 20, 22, 25, 28, or 30, or a range between any two. More preferably, T is 12~28.

[0030] M characterizes the degree of powder agglomeration. This invention controls the agglomeration rate at a low level of 1% to 4%. A lower agglomeration rate results in better powder flowability, more uniform slurry dispersion, better consistency between coating and electrode thickness, higher mass production yield, and fewer internal voids in the agglomerates, thus minimizing their adverse impact on compaction performance. Exemplarily, the dimensionless value of M can be any one of 1, 1.5, 2, 2.5, 3, 3.5, or 4, or a range between any two. More preferably, M is 1.3 to 3.3.

[0031] D 50 The bulk particle size of the powder is determined. This invention will use D... 50 The particle size is controlled within the range of 2–3 μm. This particle size range retains sufficient ion / electron transport channels and good rate capability, while also forming an optimized multi-level particle size distribution with the small particles (T = 10–30) attached to the surface, allowing the small particles to efficiently fill the gaps between large particles. For example, D… 50 The dimensionless value can be any one of 2.0, 2.2, 2.4, 2.5, 2.6, 2.8, 3.0, or a range between any two. More preferably, it is 2.4 to 2.6.

[0032] Z is composed of T and D. 50 This is a comprehensive indicator jointly constructed by T, D, and M. It is important to emphasize that T and D... 50 The three parameters, M, and A, are not independent of each other, but rather exhibit a significant interaction: T is closely related to compaction density. If T is too high, there are too many tiny particles on the surface of large particles, which easily agglomerate, making it difficult for particles to move during compaction and reducing compaction density. If T is too low, there are too few tiny particles on the surface of large particles, making it difficult to fill the voids during compaction, resulting in low compaction density. Increasing T makes it easier for small particles to agglomerate, causing clumping, and more particles cannot pass through the sieve, thus increasing the M value. T and M are generally positively correlated. A high M value is due to agglomeration preventing sieving and resulting in low compaction density. A low M value means there is a lack of soft agglomerates to fill the voids of large particles, also reducing compaction density. Excessive M hinders flowability, while a low M value results in a high proportion of ultrafine particles, easily causing bridging and also affecting flowability. D 50 The larger the particle size, the more small particles it can hold, and the larger the T value; D 50 If the particle size is too small, the overall T will be too small, and it will be easier for small particles to accumulate excessively, resulting in an excessively large M.

[0033] Therefore, this invention couples the above three interactions into a quantifiable comprehensive criterion using Z: only when T, D 50 When T, M, and Z all fall within a suitable range, and Z satisfies 1 ≤ Z ≤ 50, the material can simultaneously possess high compaction density and low agglomeration rate. Excessive Z (total T too high, minimum M too low, or unsuitable particle size) or excessive Z (total T too low, minimum M too high) will cause the material to deviate from its optimal state, resulting in decreased compaction density or increased agglomeration. For example, Z can be any one of 1, 2, 5, 10, 15, 20, 25, 30, 40, or 50, or a range between any two. More preferably, Z is 3 to 38.

[0034] By using the above formula and its scope limitation, this invention incorporates the three key parameters T, M, and D50 into the protection scope under the comprehensive index Z, thereby achieving overall control of the microstructure of powder. This solves the two major problems of low compaction density and easy powder agglomeration at both the physical and chemical levels, breaking through the bottleneck that existing technologies cannot address simultaneously.

[0035] Specifically, in this invention, the compaction density of the high-compact lithium iron phosphate cathode material is greater than 2.6 g / cm³. 3 The capacity of the high-pressure lithium iron phosphate cathode material is greater than 154 mAh / g.

[0036] In particular, high compaction density directly increases the volumetric energy density of the electrode and the battery. For example, the compaction density can be 2.62 g / cm³. 3 2.63 g / cm 3 2.65 g / cm 3 2.7 g / cm 3 2.75 g / cm 3 2.8 g / cm 3 2.85 g / cm 32.9 g / cm 3 The value is any one of the values, or a range between any two. Preferably, it is 2.62 g / cm³. 3 ~2.63 g / cm 3 .

[0037] The thin and uniform carbon coating and monodisperse particle structure ensure a high discharge specific capacity. For example, the capacity can be any one of 155 mAh / g, 156 mAh / g, 158 mAh / g, 160 mAh / g, 162 mAh / g, 165 mAh / g, 168 mAh / g, 170 mAh / g, or a range between any two. Preferably, it is 155 mAh / g to 157 mAh / g.

[0038] Furthermore, the present invention provides a method for preparing the above-mentioned high-pressure lithium iron phosphate cathode material, which includes the following steps: The carbon source is heated and melted into a liquid and then atomized to form hot carbon source droplets. The hot carbon source droplets are mixed with cold lithium iron phosphate powder in opposite directions to form carbon source-coated lithium iron phosphate particles. The temperature difference between the hot carbon source droplets and the cold lithium iron phosphate powder is greater than 140°C. The carbon source-coated lithium iron phosphate particles are first frozen to destroy their melting characteristics, and then calcined to obtain carbon-coated lithium iron phosphate.

[0039] The principle of the preparation method of the present invention is as follows: the carbon source is mixed with low-temperature lithium iron phosphate powder in a molten state to achieve rapid coating and solidification of the carbon layer, so that hydrogen bonds are not formed between different particles and agglomeration is not generated; then the coated lithium iron phosphate is subjected to low-temperature (freezing) treatment, so that the carbon chain forms a dense and irreversible hydrogen bond network by a large number of hydroxyl, amino and ether bonds. The molecular chain is anchored and bound by microcrystals, and the thermal motion of the chain segments is locked, and the molten fluidity cannot be restored by heating; therefore, agglomeration will not occur when directly carbonized at high temperature.

[0040] Specifically, the present invention includes the following steps: S1. Prepare cold lithium iron phosphate powder.

[0041] Iron phosphate and lithium carbonate were mixed in a molar ratio of 1:1.01~1.03, and then calcined at a low temperature. After cooling, the mixture was ground.

[0042] The low-temperature calcination is carried out under an inert atmosphere at a temperature of 500~600℃ for 4~8h; the temperature is then lowered to -30℃~-10℃; and the particles are ground to a particle size of 0.3~10μm.

[0043] In this invention, lithium iron phosphate crystalline phase is generated by reacting an iron source with a lithium source through low-temperature calcination. The resulting powder is then cooled and ground to obtain lithium iron phosphate powder with controlled particle size, high crystalline phase purity, and a low-temperature state. The key point is that the powder is kept in a low-temperature state after cooling, thus creating a temperature difference greater than 140°C during subsequent antagonistic mixing with hot carbon source droplets, achieving rapid coating and rapid solidification. The low-temperature powder also helps retain fine grains and a highly active surface, promoting uniform coating.

[0044] For example, the calcination temperature can be any one of 500°C, 520°C, 540°C, 550°C, 560°C, 580°C, or 600°C, or a range between any two; the time can be any one of 4 h, 5 h, 6 h, 7 h, or 8 h, or a range between any two. These conditions allow the iron and lithium sources to react fully to form well-crystallized lithium iron phosphate, while avoiding excessively high temperatures that could cause grain growth, thus laying the foundation for obtaining a median particle size of 2–3 μm.

[0045] For example, the cooled temperature can be any one of -30°C, -25°C, -20°C, -15°C, -10°C, or a range between any two.

[0046] For example, the particle size after grinding can be any one of 1 μm, 2 μm, 2.5 μm, 3 μm, 4 μm, 5 μm, or any range between two; more preferably, it is ground to a D50 of 2~3 μm. The appropriate grinding particle size directly determines the median particle size of the final powder and the basis for the adhesion of small particles on the surface, which is the source of gradation efficiency.

[0047] S2. Prepare thermal carbon source droplets.

[0048] The carbon source is heated and melted into a liquid, which is then atomized to form thermal carbon source droplets.

[0049] In this invention, the carbon source includes at least one of xylitol, methylparaben, and resorcinol. These three types of carbon sources share the common characteristic of containing abundant and active functional groups in their molecules: xylitol is a five-carbon polyol rich in hydroxyl groups; resorcinol is a diphenol rich in phenolic hydroxyl groups and contains a benzene ring; and methylparaben contains phenolic hydroxyl groups, ester groups, and a benzene ring. During low-temperature processing, these functional groups can form a dense and irreversible hydrogen bond network through numerous hydrogen bonds and intermolecular forces, anchoring and binding the molecular chains to microcrystals. This locks the thermal motion of chain segments and disrupts melt flowability during heating, which is key to achieving "high-temperature carbonization without agglomeration." Simultaneously, conjugated structures such as the benzene ring exhibit high carbonization rates and good conductivity during carbonization, which is beneficial for forming a continuous and conductive carbon coating layer.

[0050] In this invention, by controlling the heating and melting temperature to 150~200℃, this melting temperature matches the melting point of the selected carbon source (xylitol, methylparaben, resorcinol, etc.), which enables the carbon source to be fully melted into a low-viscosity, atomizable liquid, while avoiding excessively high temperatures that could lead to thermal decomposition or carbonization of the carbon source, thereby ensuring the quality of the subsequent carbon coating layer.

[0051] For example, it can be any one of 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C, or a range between any two.

[0052] Atomization includes atomization using a centrifugal atomizer. Centrifugal atomization can obtain fine droplets with uniform particle size and narrow particle size distribution with high atomization efficiency, which is conducive to the formation of a thin and uniform carbon coating layer and is the preferred atomization method.

[0053] In this invention, by pre-preparing hot carbon source droplets, the contact area between the carbon source and lithium iron phosphate powder can be significantly increased, achieving uniform and thin-layer coating; it can also create conditions for subsequent rapid curing driven by temperature difference with cold powder.

[0054] S3. Mix hot carbon source droplets with cold lithium iron phosphate powder in opposite directions to form carbon source-coated lithium iron phosphate particles.

[0055] The feed mass of the hot carbon source droplets is 5% to 15% of the feed mass of the cold lithium iron phosphate powder. If the carbon source content is too low (below 5%), the carbon coating layer is incomplete, the conductive network is discontinuous, and the capacity and rate performance decrease. If the carbon source content is too high (above 15%), the carbon layer is too thick, and the residual carbon increases, which dilutes the active material, increases the specific surface area and interparticle friction, and is detrimental to compaction density. For example, this feed mass ratio can be any one of 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, or 15%, or a range between any two. More preferably, it is 6% to 10%.

[0056] In this invention, the temperature of the hot carbon source droplet is 120~150℃; the temperature of the cold lithium iron phosphate powder is -60~-20℃, and the temperature difference between the hot carbon source droplet and the cold lithium iron phosphate powder is greater than 140℃.

[0057] The settings for hot droplet temperature and cold powder temperature must be considered in conjunction to ensure that the temperature difference between the two is greater than 140℃: the higher the hot droplet temperature and the lower the cold powder temperature, the greater the temperature difference, the faster the melt cools and solidifies, and the better the anti-agglomeration and low-caking effect. A hot droplet temperature of 120~150℃ can ensure that the carbon source is in a fully molten and flowing state without causing the carbon source to decompose or oxidize due to excessive temperature.

[0058] This invention employs a counter-current mixing method for contact, ensuring that hot droplets collide with cold powder in a counter-current manner, enhancing momentum and heat transfer, and guaranteeing uniform coating without dead zones. A temperature difference greater than 140°C is crucial for rapid coating and solidification: hot molten carbon source droplets experience a rapid temperature drop upon contact with the low-temperature powder, quickly cooling and solidifying to rapidly spread and form a film on the particle surface, instantly locking in shape. Due to the extremely rapid cooling rate, the carbon source melt does not have time to form bonding necks or hydrogen bond bridges between different lithium iron phosphate particles, thus preventing particle adhesion and agglomeration at the source, and also preventing secondary agglomeration due to carbon source flow.

[0059] S4. The carbon-coated lithium iron phosphate particles are first frozen to destroy their melting characteristics, and then calcined to obtain carbon-coated lithium iron phosphate.

[0060] In this process, the freezing treatment transforms the hydrogen bond network between the carbon source molecular chains from a reversible to an irreversible microcrystalline anchoring structure, thus disrupting the melt flowability of the carbon source when it is reheated. As a result, during the subsequent high-temperature calcination and carbonization process, the carbon source will not remelt and flow, the particles remain monodisperse, the carbonization process proceeds in situ, and high-temperature agglomeration during the calcination stage is avoided.

[0061] Specifically, freezing includes freezing at -60 to -80°C for 5 to 10 hours; for example, the freezing temperature can be any one of -60°C, -65°C, -70°C, -75°C, and -80°C, or a range between any two; the freezing time can be any one of 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, and 10 hours, or a range between any two. Sufficient low temperature and freezing time ensure that the carbon source molecular chains completely form a dense irreversible hydrogen bond network and that the thermal motion of the chain segments is fully locked, thereby maximally destroying its remelting fluidity; if the temperature is too high or the time is too short, the hydrogen bond network will be insufficient, and local melting and adhesion may still occur during the calcination stage.

[0062] Calcination is carried out under an inert atmosphere at a temperature of 600–750°C for 2–12 hours. For example, the calcination temperature can be any one of 600°C, 620°C, 640°C, 650°C, 660°C, 680°C, 700°C, 720°C, or 750°C, or a range between any two; the calcination time can be any one of 2 hours, 4 hours, 6 hours, 8 hours, 10 hours, or 12 hours, or a range between any two. An inert atmosphere (such as nitrogen or argon) prevents the carbon layer from oxidizing at high temperatures. These calcination conditions allow the carbon source to carbonize completely, forming a thin, uniform, conductive, and dense carbon coating layer, while ensuring sufficient crystallization of the lithium iron phosphate phase without particle sintering and agglomeration. Because freezing destroys the remelting properties of the carbon source, this high-temperature carbonization process can be carried out in situ in a monodisperse state.

[0063] The various steps in this invention are interconnected and form an indispensable organic whole. Specifically, melting and atomizing the carbon source provides the prerequisite for rapid temperature-differential coating and solidification. Simultaneously, the temperature difference between the hot carbon source droplets and the cold lithium iron phosphate powder, as defined in this invention, is greater than 140°C. This temperature difference facilitates rapid solidification, achieving a low agglomeration rate. The greater the temperature difference, the faster the cooling, and the less likely hydrogen bonding and melt flow will form between particles, resulting in a lower agglomeration rate. In this invention, the lithium iron phosphate particles coated with the carbon source are first frozen to disrupt their melting characteristics before calcination. The freezing operation ensures that subsequent high-temperature calcination does not lead to agglomeration. If the freezing step is omitted, the carbon source will remelt and flow during the calcination heating process, causing adhesion and agglomeration between particles.

[0064] Furthermore, this invention also provides a lithium-ion battery comprising the aforementioned high-compaction lithium iron phosphate cathode material or the high-compaction lithium iron phosphate cathode material prepared by the aforementioned preparation method. Because the high-compaction lithium iron phosphate cathode material possesses high compaction density, low agglomeration rate, and high capacity, using this material as the cathode material in lithium-ion batteries can yield lithium-ion batteries with high electrode compaction density, high volumetric energy density, uniform slurry dispersion, good coating consistency, and high batch yield, demonstrating significant application value in the fields of power batteries and energy storage batteries.

[0065] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0066] Example 1 This embodiment provides a high-pressure lithium iron phosphate cathode material, the preparation method of which includes: S1. Iron phosphate and lithium carbonate are calcined at a molar ratio of 1:1.02, kept at 500℃ for 6 hours under an inert atmosphere, cooled to -30℃ and then ground to obtain lithium iron phosphate powder at -20℃.

[0067] S2. Xylitol is heated to 150°C to form a liquid, and then centrifuged to form hot carbon source droplets at 120°C.

[0068] S3. The hot carbon source droplets are sprayed onto lithium iron phosphate powder in an opposing direction, and the amount of xylitol used is 5% of the mass of lithium iron phosphate, to obtain carbon source-coated lithium iron phosphate particles.

[0069] S4. The carbon-coated lithium iron phosphate particles are kept at -60℃ for 2 hours, and then the treated material is calcined at a heating rate of 5℃ / min, and kept at 650℃ for 10 hours. The entire calcination process is protected by inert gas to obtain carbon-coated lithium iron phosphate.

[0070] Example 2 This embodiment provides a high-pressure lithium iron phosphate cathode material, the preparation method of which includes: S1. Iron phosphate and lithium carbonate are calcined at a molar ratio of 1:1.02, kept at 500℃ for 6 hours under an inert atmosphere, cooled to -60℃ and then ground to obtain lithium iron phosphate powder at -40℃.

[0071] S2. Methylparaben is heated to 180°C to form a liquid, and then centrifuged to form hot carbon source droplets at 150°C.

[0072] S3. The hot carbon source droplets are sprayed onto lithium iron phosphate powder in an opposing direction. The amount of methylparaben used is 8% of the mass of lithium iron phosphate, to obtain carbon source-coated lithium iron phosphate particles.

[0073] S4. The carbon-coated lithium iron phosphate particles are kept at -80℃ for 3 hours, and then the treated material is calcined at a heating rate of 5℃ / min. The temperature is raised to 700℃ and kept for 10 hours. The entire calcination process is protected by inert gas to obtain carbon-coated lithium iron phosphate.

[0074] Example 3 This embodiment provides a high-pressure lithium iron phosphate cathode material, the preparation method of which includes: S1. Iron phosphate and lithium carbonate are calcined at a molar ratio of 1:1.02, kept at 600℃ for 6 hours under an inert atmosphere, cooled to -60℃ and then ground to obtain lithium iron phosphate powder at -40℃.

[0075] S2. Resorcinol is heated to 180°C to form a liquid, and then centrifuged to form hot carbon source droplets at 150°C.

[0076] S3. The hot carbon source droplets are sprayed onto lithium iron phosphate powder in an opposing direction. The amount of resorcinol used is 15% of the mass of lithium iron phosphate, to obtain carbon source-coated lithium iron phosphate particles.

[0077] S4. The carbon-coated lithium iron phosphate particles are treated at -80℃ for 3 hours, and then calcined at a heating rate of 5℃ / min until they reach 750℃ and are held for 8 hours. The entire calcination process is carried out under inert gas protection to obtain carbon-coated lithium iron phosphate (see [reference]). Figure 1 ).

[0078] Example 4 This embodiment provides a high-pressure lithium iron phosphate cathode material, the preparation method of which includes: S1. Iron phosphate and lithium carbonate are calcined at a molar ratio of 1:1.02, kept at 500℃ for 6 hours under an inert atmosphere, cooled to -40℃ and then ground to obtain lithium iron phosphate powder at -20℃.

[0079] S2. Methylparaben is heated to 200°C to form a liquid, and then centrifuged to form hot carbon source droplets at 150°C.

[0080] S3. The hot carbon source droplets are sprayed onto lithium iron phosphate powder in an opposing direction. The amount of methylparaben used is 8% of the mass of lithium iron phosphate, to obtain carbon source-coated lithium iron phosphate particles.

[0081] S4. The carbon-coated lithium iron phosphate particles are kept at -80℃ for 3 hours, and then the treated material is calcined at a heating rate of 5℃ / min, and kept at 700℃ for 8 hours. The entire calcination process is protected by inert gas to obtain carbon-coated lithium iron phosphate.

[0082] Comparative Example 1 This comparative example provides a carbon-coated lithium iron phosphate, which includes the following steps: S1. Iron phosphate and lithium carbonate were calcined at a molar ratio of 1:1.02, kept at 500℃ for 6 hours under an inert atmosphere, cooled to room temperature, and then ground and crushed to obtain lithium iron phosphate powder at 25℃.

[0083] S2. Add methylparaben and mix. The amount of methylparaben is 8% of the mass of lithium iron phosphate to obtain carbon source-coated lithium iron phosphate particles.

[0084] S3. The carbon-coated lithium iron phosphate particles are calcined at a heating rate of 5℃ / min, and held at 700℃ for 8 hours. The entire calcination process is protected by inert gas to obtain carbon-coated lithium iron phosphate.

[0085] Comparative Example 2 This comparative example is basically the same as Example 4, the main difference being that in this comparative example, the cooling to -40°C in step S1 is omitted, and grinding is only performed after cooling to room temperature. At this time, the temperature difference between the hot carbon source droplets and the lithium iron phosphate powder is 125°C. Specifically, the steps are as follows: S1. Iron phosphate and lithium carbonate are calcined at a molar ratio of 1:1.02, kept at 500℃ for 6 hours under an inert atmosphere, cooled to room temperature, and then ground to obtain lithium iron phosphate powder at 25℃.

[0086] S2. Methylparaben is heated to 200°C to form a liquid, and then centrifuged to form hot carbon source droplets at 150°C.

[0087] S3. The hot carbon source droplets are sprayed onto lithium iron phosphate powder in an opposing direction. The amount of methylparaben used is 8% of the mass of lithium iron phosphate, to obtain carbon source-coated lithium iron phosphate particles.

[0088] S4. The carbon-coated lithium iron phosphate particles are kept at -80℃ for 3 hours, and then the treated material is calcined at a heating rate of 5℃ / min, and kept at 700℃ for 8 hours. The entire calcination process is protected by inert gas to obtain carbon-coated lithium iron phosphate.

[0089] Comparative Example 3 This comparative example is basically the same as Example 4, except that in this comparative example, methylparaben, after being heated to 200°C to form a liquid, is directly mixed with lithium iron phosphate powder at -20°C without atomization. The specific steps include the following: S1. Iron phosphate and lithium carbonate are calcined at a molar ratio of 1:1.02, kept at 500℃ for 6 hours under an inert atmosphere, cooled to -40℃ and then ground to obtain lithium iron phosphate powder at -20℃.

[0090] S2. Add methylparaben and mix. The amount of methylparaben is 8% of the mass of lithium iron phosphate to obtain carbon source-coated lithium iron phosphate particles.

[0091] S4. The carbon-coated lithium iron phosphate particles are calcined at a heating rate of 5℃ / min, and held at 700℃ for 8 hours. The entire calcination process is protected by inert gas to obtain carbon-coated lithium iron phosphate.

[0092] Comparative Example 4 This comparative example provides a carbon-coated lithium iron phosphate, the preparation method of which includes: Ferric phosphate and lithium carbonate were mixed at a molar ratio of 1:1.02, and then 5% glucose by mass of the mixture was added. The mixture was then kept at -60℃ for 2 hours, and then calcined at a heating rate of 5℃ / min until it reached 650℃ and was kept at that temperature for 10 hours. Inert gas protection was used throughout the calcination process.

[0093] Comparative Example 5 This comparative example is basically the same as Example 4, except that in this comparative example, iron phosphate, lithium carbonate and methylparaben are mixed together. The specific operation is as follows: iron phosphate and lithium carbonate are mixed at a molar ratio of 1:1.02, and then 8% of the mass of the mixture of methylparaben is added. The mixture is kept at -80°C for 3 hours, and then the treated material is calcined at a heating rate of 5°C / min. The temperature is raised to 700°C and kept for 8 hours. The entire calcination process is protected by inert gas to obtain carbon-coated lithium iron phosphate.

[0094] Comparative Example 6 This comparative example is basically the same as Example 4, the main difference being that the low-temperature -80℃ holding treatment for 3 hours in step S4 is omitted in this comparative example, and the carbon source-coated lithium iron phosphate particles are directly calcined. The specific steps are as follows: S1. Iron phosphate and lithium carbonate are calcined at a molar ratio of 1:1.02, kept at 500℃ for 6 hours under an inert atmosphere, cooled to -40℃ and then ground to obtain lithium iron phosphate powder at -20℃.

[0095] S2. Methylparaben is heated to 200°C to form a liquid, and then centrifuged to form hot carbon source droplets at 150°C.

[0096] S3. The hot carbon source droplets are sprayed onto lithium iron phosphate powder in an opposing direction. The amount of methylparaben used is 8% of the mass of lithium iron phosphate, to obtain carbon source-coated lithium iron phosphate particles.

[0097] S4. The carbon-coated lithium iron phosphate particles are calcined at a heating rate of 5℃ / min, and held at 700℃ for 8 hours. The entire calcination process is protected by inert gas to obtain carbon-coated lithium iron phosphate.

[0098] Experimental Example The carbon-coated lithium iron phosphate prepared in the above examples and comparative examples were tested, and the test items and methods are as follows: (1) Detection method for the number of small particles attached: SEM images were taken using a NanoSEM 450 electron microscope in accordance with the general rules of scanning electron microscopy analysis method JY / T 0584-2020. The number of small particles attached to large particles was calculated based on the average value of the small particles loaded by the four largest particles in the field of view. (2) D 50 The testing method was as follows: laser particle size analyzer was used for testing according to the GB / T 19077-2016 standard. (3) Method for detecting agglomeration rate: Dry the sample at 100℃ for 2 h and cool it to room temperature; accurately weigh 100g of lithium iron phosphate powder and place it on a 200-mesh sieve, with matching sieve bottom and sieve cover; set a fixed vibration frequency of 24Hz, amplitude of 0.5mm, and sieving time of 10min; after sieving, collect the residual powder on the sieve and weigh it m. The agglomeration rate is m / 500g. 100%; (4) The method for calculating Z is as follows: ; (5) Test method for compaction density: The compaction density was tested according to GB / T 24533-2009 using the Sansi longitudinal and transverse compaction density tester; (6) Capacity testing method: Lithium iron phosphate, acetylene black and PVDF are mixed in a ratio of 0.95:0.02:0.03, NMP is used as solvent to prepare the slurry to make the positive electrode, and lithium metal sheet is used as the negative electrode to make the coin cell. The capacity of the coin cell is tested using the Blue Battery Test System.

[0099] The test results are as follows:

[0100] As can be seen from the table above, T and D in Embodiments 1-4 of the present invention 50 The values ​​of M are all within the range of this application, and the final obtained Z is also within the range of this application. At this time, the cathode material prepared has good compaction density, which is significantly higher than that of comparative examples 1-6. Meanwhile, the battery prepared has good melting, which is significantly higher than that of comparative examples 1-6.

[0101] In Comparative Example 1, the room temperature lithium iron phosphate powder was directly mixed with room temperature methyl paraben. It can be seen that the number of small particles attached increased significantly, and D50 and agglomeration rate M were significantly improved, which in turn led to a significant increase in Z. The final compaction density and volume were reduced.

[0102] In Comparative Example 2, room temperature lithium iron phosphate powder was directly mixed with high temperature hot carbon source droplets. Compared with Comparative Example 1, the number of small particles attached, D50 and agglomeration rate M were significantly reduced, but still significantly higher than Examples 1-4. This proves that the temperature difference between lithium iron phosphate powder and hot carbon source droplets has a significant impact on the above parameters, and it is necessary to strictly control the temperature of both and the mixing method.

[0103] In Comparative Example 3, methylparaben, heated to 200°C to form a liquid, was directly mixed with lithium iron phosphate powder at -20°C without atomization. Its effect was better than Comparative Examples 1 and 2, but still inferior to Examples 1-4. Comparative Example 3, due to the lack of atomization, resulted in higher temperatures (T and D). 50 Too small, D 50 The smaller T is smaller overall and more likely to cause excessive accumulation of small particles, resulting in an excessively large M, which in turn leads to a significantly lower Z, which is below the range of this application, and the final compaction density and volume are reduced.

[0104] In Comparative Example 4, all raw materials were mixed together and then calcined after low-temperature treatment. The low-temperature conditions could not change the melting point of glucose. During the calcination stage, glucose melted, causing agglomeration on the particle surface, which significantly increased the Z value and exceeded the range defined in this application. As a result, the compaction density and volume of the material decreased.

[0105] In Comparative Example 5, all raw materials were mixed together and then calcined after low-temperature treatment. The low-temperature treatment prevented methylparaben from melting during the sintering process, resulting in poor coating of lithium iron phosphate. This caused a significant increase in the number of small particles, D50, and agglomeration rate M. This was mainly due to incomplete carbon coating. During calcination, the particles grew, and surface carbon appeared on the surface, ultimately leading to a significant increase in Z, which exceeded the scope of this application. The final compaction density and capacity were both reduced.

[0106] In Comparative Example 6, the low-temperature -80℃ heat treatment for 3 hours in step S4 was omitted, and the lithium iron phosphate particles coated with carbon source were directly calcined. At this time, the number of small particles attached, D50 and agglomeration rate M all increased significantly. This is because without freezing to destroy the melting characteristics, the carbon source will remelt and flow during the subsequent high-temperature calcination and carbonization process, and the particles are prone to high-temperature agglomeration, which leads to Z significantly increasing and exceeding the scope of this application. The final compaction density and capacity are reduced.

[0107] In summary, the high-pressure lithium iron phosphate cathode material provided by this invention satisfies the following formula: This invention achieves overall control of the powder's microstructure by ensuring that the number of small particles (T) adhering to the surface of large particles (as measured by SEM) is between 10 and 30, the agglomeration rate (M) is between 1 and 4, and the D50 is within a suitable range. Furthermore, it ensures that these three factors synergistically satisfy the comprehensive index of 1 ≤ Z ≤ 50. This achieves simultaneous control of the two major problems of low compaction density and easy powder agglomeration at both physical and chemical levels, overcoming the bottleneck of existing technologies that cannot simultaneously address these issues. This results in a lithium iron phosphate cathode material with high compaction density, low agglomeration rate, and high specific capacity. Only when T and D50 are within a suitable range can the overall microstructure of the powder be controlled. 50 When T, M, and Z all fall within a suitable range, and Z satisfies 1≤Z≤50, the material can simultaneously possess high compaction density and low agglomeration rate. If Z is too high (T is too large, M is too low, or the particle size is unsuitable) or too low (T is too small, M is too high), the material will deviate from its optimal state, resulting in decreased compaction density or increased agglomeration.

[0108] The preparation method provided by this invention mixes a carbon source with low-temperature lithium iron phosphate powder in a molten state, achieving rapid coating and solidification of the carbon layer, thus preventing hydrogen bonding and agglomeration between different particles. Subsequently, the coated lithium iron phosphate is subjected to low-temperature (freezing) treatment, causing the carbon chains to form a dense and irreversible hydrogen bond network through numerous hydroxyl, amino, and ether bonds. The molecular chains are anchored and bound by microcrystals, and the thermal motion of the chain segments is locked, preventing the restoration of molten fluidity upon heating. Therefore, no agglomeration occurs during direct carbonization at high temperatures. The prepared lithium iron phosphate cathode material possesses characteristics such as high compaction density, low agglomeration rate, and high specific capacity.

[0109] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A high-pressure lithium iron phosphate cathode material, characterized in that, It satisfies the following formula: ; In the formula, T represents the number of small particles adhering to the surface of large particles under SEM testing; M represents the agglomeration rate of the cathode material, M = residual mass of lithium iron phosphate material on a 200-mesh sieve ÷ total mass of lithium iron phosphate material × 100%; D 50 The median particle size of lithium iron phosphate powder; Where T represents the value when the unit is 1, M represents the value when the unit is % and D 50 The value corresponding to the unit is μm. The obtained Z is dimensionless, 10≤T≤30; 1≤M≤4; 1≤Z≤50.

2. The high-pressure lithium iron phosphate cathode material according to claim 1, characterized in that, D 50 It is 2-3 μm; And / or, the compaction density of the high-pressure lithium iron phosphate cathode material is greater than 2.6 g / cm³. 3 ; And / or, the capacity of the high-pressure lithium iron phosphate cathode material is greater than 154 mAh / g.

3. A method for preparing a high-pressure lithium iron phosphate cathode material as described in any one of claims 1-2, characterized in that, It includes: The carbon source is heated and melted into a liquid, which is then atomized to form thermal carbon source droplets. The hot carbon source droplets are mixed with cold lithium iron phosphate powder in opposite directions to form carbon source-coated lithium iron phosphate particles, wherein the temperature difference between the hot carbon source droplets and the cold lithium iron phosphate powder is greater than 140°C. The carbon-coated lithium iron phosphate particles are first frozen to destroy their melting characteristics, and then calcined to obtain carbon-coated lithium iron phosphate.

4. The method for preparing high-pressure lithium iron phosphate cathode material according to claim 3, characterized in that, The feed mass of the hot carbon source droplets is 5% to 15% of the feed mass of the cold lithium iron phosphate powder; And / or, the temperature of the thermal carbon source droplet is 120~150℃; And / or, the temperature of the cold lithium iron phosphate powder is -60~-20℃; And / or, the particle size of the thermal carbon source droplets is 3~10μm; And / or, the particle size of the cold lithium iron phosphate powder is 0.3~10μm.

5. The method for preparing high-pressure lithium iron phosphate cathode material according to claim 3, characterized in that, The heating and melting temperature is 150~200℃; And / or, the atomization includes atomization using a centrifugal atomizer.

6. The method for preparing high-pressure lithium iron phosphate cathode material according to claim 3, characterized in that, The carbon source includes at least one of xylitol, methylparaben, and resorcinol.

7. The method for preparing high-pressure lithium iron phosphate cathode material according to claim 3, characterized in that, The freezing process includes freezing at -80 to -60°C for 5 to 10 hours. And / or, the calcination is carried out under an inert atmosphere, the calcination temperature is 600~750℃, and the time is 2~12h.

8. The method for preparing high-pressure lithium iron phosphate cathode material according to any one of claims 3-7, characterized in that, The preparation method of the cold lithium iron phosphate powder includes: mixing iron phosphate and lithium carbonate and then calcining at low temperature, followed by cooling and grinding.

9. The method for preparing high-pressure lithium iron phosphate cathode material according to claim 8, characterized in that, The iron phosphate and the lithium carbonate are mixed in a molar ratio of 1:1.01~1.03; And / or, the low-temperature calcination is carried out under an inert atmosphere, and the temperature of the low-temperature calcination is 500~600℃, and the time is 4~8h; And / or, the cooling to a temperature of -30℃ to -10℃; And / or, the grinding is carried out to a particle size of 0.3~10μm.

10. A lithium-ion battery, characterized in that, It includes high-density lithium iron phosphate cathode materials as described in any one of claims 1-2 or high-density lithium iron phosphate cathode materials prepared by the preparation method of high-density lithium iron phosphate cathode materials as described in any one of claims 3-9.