A fermentation-based graded porous biomass carbon and its preparation method
By using fermentation to form directional macropores and mesopores from Aspergillus niger hyphae and cellulase, combined with the self-activated micropores of the biomass matrix, the environmental pollution and pore structure connectivity problems in the preparation of porous carbon from biomass in existing technologies have been solved, achieving efficient ion transport and stable electrochemical performance.
Patent Information
- Application Number
- CN202611558410.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for preparing porous carbon from biomass rely on the addition of external chemical activators, which poses an environmental pollution risk. The pore structure lacks directional connectivity, making it difficult to accurately control the gradation relationship between macropores, mesopores, and micropores. Furthermore, they fail to fully utilize the template and etching effects of microbial hyphae and enzyme systems in the construction of hierarchical pore structures.
A three-level interconnected hierarchical pore structure was constructed by using fermentation to form a tubular macroporous network of Aspergillus niger hyphae, cellulase etching mesoporous channels, and self-activation of potassium and sodium ash in the biomass matrix to form micropores, thus avoiding the need for external activators.
It achieves efficient ion transport pathways and abundant active sites, avoiding environmental pollution and high-temperature energy consumption caused by chemical activators. It is suitable for lithium-ion batteries, sodium-ion batteries and supercapacitor anode materials, maintaining high specific capacity and cycle stability under high current density.
Smart Images

Figure CN123120728A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of carbon materials technology, and in particular to a fermentation-based graded porous biomass carbon and its preparation method. Background Technology
[0002] Porous carbon materials have wide applications in energy storage, catalysis, and adsorption due to their high specific surface area, abundant pore structure, good chemical stability, and conductivity. In electrochemical energy storage devices such as lithium-ion batteries, sodium-ion batteries, and supercapacitors, porous carbon serves as a negative electrode or electrode material, and its pore structure directly affects key electrochemical performance indicators such as ion diffusion rate, charge transfer impedance, and specific capacity.
[0003] In existing technologies, the preparation of porous carbon from biomass typically employs chemical activation methods (such as activators like KOH, ZnCl2, and H3PO4) or physical activation methods (such as activating gases like water vapor and CO2). While chemical activation can achieve high specific surface areas, it suffers from problems such as large activator usage, equipment corrosion, and environmental pollution from washing wastewater. Furthermore, the pore structure formed by chemical activation is usually dominated by micropores, with a low proportion of mesopores and macropores, which is not conducive to rapid ion transport under high current densities. In addition, chemical activation makes it difficult to precisely control the distribution ratio of pore sizes at different levels, resulting in pore morphologies that are mostly irregular and fissure-like, lacking directional connectivity.
[0004] To address these issues, researchers have proposed various hierarchical pore structure design schemes. However, existing design methods still present different problems with the carbon materials obtained. For example, they still require the use of activating pore-forming agents, and the macropore structure is non-directional and randomly distributed; or they rely on external template agents and high-temperature treatment, making the process complex; or they use alkaline activators such as KOH, and the silicon content needs to be controlled below 0.6 wt%.
[0005] Microbial fermentation for the preparation of porous carbon is a relatively new approach that has emerged in recent years. Other methods utilize microbial fermentation to prepare carbon materials, such as fermentation with Aspergillus niger followed by carbonization and high-temperature activation with KOH to obtain a hierarchical porous structure. However, this method still requires secondary activation with KOH after carbonization, and the pore structure formation primarily relies on chemical activation rather than the microbial action itself. Other methods utilize PHA accumulated within bacterial cells to carbonize and form a microporous-mesoporous bilevel structure, but these do not involve the formation of macroporous structures.
[0006] Another approach uses the residue from fermenting corn stalks to produce alcohol as raw material, extracts lignin through alkali dissolution, and activates it by mixing with potassium hydroxide to form a lignin-based porous carbon route (publication number 202411300308.8). This route still relies on the addition of an inorganic alkaline activator and requires dissolution-precipitation-separation steps. It is fundamentally different from the route of this invention, which uses the whole components of distiller's grains, ferments with a single mold and controls hierarchical pores through cellulase hydrolysis, and utilizes the inherent potassium and sodium ash to self-activate and create pores, in terms of biomass matrix selection, pore formation mechanism, and process route.
[0007] In summary, the existing technologies have the following shortcomings: (1) They rely on external chemical activators, activating gases or template agents, which are complex processes and pose a high risk of environmental pollution; (2) The pore structure lacks directional connectivity, and the gradation relationship between macropores, mesopores and micropores is difficult to control precisely; (3) Microbial fermentation methods mostly stay at the pretreatment stage, and the final pore formation still relies on external activation methods, failing to give full play to the template and etching effects of microbial hyphae and enzyme systems in the construction of hierarchical pore structures; (4) They avoid macropore structures, and the process route of external activation gas combined with water washing to neutrality determines that their products do not have self-activated ash residue markings; (5) They lack structural designs that utilize the inherent ash components of biomass to achieve self-activated pore formation.
[0008] In view of this, the present invention is hereby proposed. Summary of the Invention
[0009] One of the objectives of this invention is to provide a fermentation-based graded porous biomass carbon, so as to at least solve one of the technical problems existing in the prior art.
[0010] The second objective of this invention is to provide a method for preparing the above-mentioned porous carbon from biomass.
[0011] The third objective of this invention is to provide a battery electrode material.
[0012] The fourth objective of this invention is to provide a battery.
[0013] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted: In a first aspect, the present invention provides a fermentation-based hierarchical porous carbon from biomass, wherein the biomass porous carbon has a three-level interconnected hierarchical pore structure, the three-level interconnected hierarchical pore structure comprising: (a) Macroporous network, which is a tubular interconnected channel formed by the growth and penetration of fungal hyphae in a biomass matrix and the removal of the hyphae by carbonization, wherein the pore size of the macroporous network is 2~5 μm; (b) Mesoporous channels, formed by the enzymatic etching of biomass cellulose components in the biomass matrix by cellulase, wherein the pore size of the mesopores is 2~50 nm, and the mesopores are oriented along the wall of the macropores and communicate with the macropores. (c) Micropore array, formed by the self-activation and pore formation of potassium and sodium components contained in the inherent ash of the biomass matrix during carbonization, wherein the pore size of the micropores is less than 2 nm, and the micropores are densely distributed on the mesopore wall and communicate with the mesopore; The macropore network, mesopore channels, and micropore array form a hierarchical interconnected pore system from macropores to mesopores to micropores.
[0014] Furthermore, the mold is Aspergillus niger (… Aspergillus niger ); The biomass matrix includes distiller's grains.
[0015] Furthermore, the biomass porous carbon includes at least one of the following characteristics A1 to A4: A1. The pore volume of the macroporous network accounts for 15% to 35% of the total pore volume; the pore volume of the mesoporous channels accounts for 20% to 45% of the total pore volume; and the pore volume of the microporous array accounts for 25% to 55% of the total pore volume. A2. The macropores in the macropore network are tubular in shape, with a smoothness Ra value of less than 200 nm on the inner surface of the tube wall, and there are connecting windows with a diameter of 0.5~2 μm between adjacent macropores; A3. The pore size distribution of the mesoporous channel exhibits a bimodal characteristic, with the first peak located in the 2~10 nm range and the second peak located in the 20~50 nm range. A4. The biomass porous carbon has a BET specific surface area of 500~2000 m² / g and a total pore volume of 0.5~1.5 cm³. 3 / g, with an average pore size of 1.5~8.0 nm.
[0016] Furthermore, the total potassium and sodium content in the inherent ash of the biomass matrix is 0.05~2.0 wt%.
[0017] Furthermore, the biomass porous carbon contains inherent nitrogen doping derived from biomass protein components and inherent oxygen doping derived from biomass oxygen-containing functional groups, wherein the nitrogen content is 1.0~4.0 at%, and the oxygen content is 5.0~15.0 at%.
[0018] Furthermore, the biomass porous carbon includes at least one of the following characteristics B1 to B3: B1. The carbon framework of the biomass porous carbon is a composite structure consisting of a disordered carbon matrix and locally graphitized microregions. In the XRD pattern, the broadened diffraction peaks corresponding to the (002) crystal plane of the disordered carbon matrix are located at 2θ = 24°~25.5°, and the interlayer spacing d 002The intensity is 0.35~0.37 nm; and there is a weak diffraction peak corresponding to the crystal plane of the local graphitized micro-region (002) at 2θ=26.4°~26.6°, the peak area of the weak diffraction peak accounts for 5%~30% of the total peak area of the crystal plane diffraction; the intensity ratio ID / IG of the D peak to the G peak in the Raman spectrum is 0.8~1.2; B2. The biomass porous carbon has an irregular lamellar morphology with a lamellar thickness of 0.5~5μm, and the lamellar surface is distributed with an array of pores formed by the macroporous network. B3. The silicon content of the biomass porous carbon does not exceed 0.5 wt%.
[0019] Secondly, the present invention provides a method for preparing the above-mentioned porous carbon from biomass, comprising the following steps: S1. Pretreatment: The biomass matrix is dried to a moisture content of ≤10 wt% and then pulverized to obtain a pretreated biomass matrix; S2. Fermentation of a single mold strain: A single mold is inoculated into the pretreated biomass matrix at an inoculation amount of 5% to 15% of the dry mass of the pretreated biomass matrix. The moisture content of the material is adjusted to 50% to 65%, and solid-state fermentation is carried out at 25 to 40°C for 3 to 7 days until the mycelial coverage reaches more than 60%, and the fermented material is obtained. S3. Cellulase hydrolysis: Add cellulase to the fermentation material at a dosage of 20-60 FPU / g dry basis, and hydrolyze for 12-48 h at pH 4.5-5.5 and 45-55℃ to obtain hydrolyzed material; S4. Pre-carbonization: The enzymatically hydrolyzed material is pre-carbonized at 200~500℃ for 1~3 h under an inert atmosphere to obtain the pre-carbonized product; S5. Acid washing and desiliconization: The pre-carbonized product is washed with dilute acid to remove ash and silicon components, then washed with water until neutral and dried to obtain the acid-washed material. S6. High-temperature carbonization self-activation: The pickled material is carbonized at 700~1000℃ for 1~3 h in an inert atmosphere. The inherent potassium and sodium ash groups in the biomass matrix are self-activated and form pores during the carbonization process. After cooling, porous biomass carbon is obtained.
[0020] Further, in step S1, the total inherent potassium and sodium content in the biomass matrix is 0.05~2.0 wt%; the total inherent potassium and sodium content in the biomass matrix is tested, and when the total potassium and sodium content of the tested batch is not between 0.05~2.0 wt%, different batches of distiller's grains are blended in proportion to ensure that the potassium and sodium content in the blended raw material is between 0.05~2.0 wt%, before proceeding to subsequent steps; and / or, In step S2, the inoculum amount of *Aspergillus niger* is 5%–15% of the dry weight of the pretreated distiller's grains, the solid-state fermentation temperature is 25–40°C, and the solid-state fermentation time is 3–7 days; and / or, In step S3, the amount of cellulase added is 20-60 FPU / g dry basis, the hydrolysis temperature is 45-55℃, and the hydrolysis time is 12-48 h; and / or, The carbonization temperature in step S6 is 700~900℃, and the carbonization time is 1~3 h.
[0021] Thirdly, the present invention provides a battery electrode material, wherein the active material of the electrode sheet comprises the above-mentioned biomass porous carbon or biomass porous carbon prepared by the above-mentioned preparation method.
[0022] Fourthly, the present invention provides a battery comprising the aforementioned electrode plates.
[0023] The biomass porous carbon provided by this invention features a macroporous network formed by directional template formation using a single fungal species, exhibiting a tubular interconnected network. This differs from the irregular, fissured macropores formed by chemical activation and the amorphous channels formed by composting and mixed fermentation. Mesoporous channels are directionally distributed along the macropore walls, formed by enzymatic etching with cellulase, exhibiting a bimodal pore size distribution. Micropore arrays are densely distributed on the mesopore walls, formed by the self-activation of inherent ash. This tertiary porosity system, from macropores to mesopores to micropores, achieves efficient ion transport from macroscopic to microscopic levels: macropores act as ion buffer reservoirs, mesopores as ion transport channels, and micropores provide high specific surface area and active sites. The micropores are formed by the self-activation effect of inherent potassium and sodium ash components in the biomass matrix during carbonization, avoiding equipment corrosion, environmental pollution, and wastewater problems associated with external activators such as KOH and ZnCl2, as well as the high-temperature energy consumption required for external water vapor and CO2 activation gases. Attached Figure Description
[0024] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0025] Figure 1 A schematic diagram of the three-level interconnected hierarchical pore structure of porous carbon in fermentation-based hierarchical biomass provided in an embodiment of the present invention; Figure 2 This is a SEM image of porous carbon from fermentation-based graded-pore biomass provided in Example 1 of the present invention. Figure 3 The XRD patterns of porous carbon from biomass provided in Example 1 and Comparative Example 1 of this invention are shown in comparison. Figure 4 ICP-OES ash residue comparison chart of fermentation-based graded porous carbon from biomass provided in this embodiment of the invention. Figure 5 This is a schematic diagram illustrating the formation mechanism of locally graphitized microregions in porous carbon of fermentation-based hierarchical biomass provided in an embodiment of the present invention, where A represents K. + Intercalation promotes the rearrangement and stacking of carbon network surfaces. B represents the removal of amorphous regions of cellulose and the inheritance of crystal orientation. C represents the ordered stacking of aromatic rings in fused ring structures. Detailed Implementation
[0026] Unless otherwise defined herein, the scientific and technical terms used in conjunction with this invention shall have the meanings commonly understood by one of ordinary skill in the art. The meaning and scope of terms shall be clear; however, in any case of potential ambiguity, the definitions provided herein shall prevail over any dictionary or foreign definitions. In this application, unless otherwise stated, the use of "or" means "and / or". Furthermore, the use of the term "comprising" and other forms is non-limiting.
[0027] Unless otherwise stated, the methods and techniques of the present invention are generally carried out according to conventional methods well known in the art and as described in various general and more specific references, which are cited and discussed throughout this specification.
[0028] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0029] This invention provides a fermentation-based hierarchical porous biomass carbon, wherein the biomass porous carbon has a three-level interconnected hierarchical pore structure, the three-level interconnected hierarchical pore structure comprising: Macroporous networks are tubular interconnected channels formed by the growth and penetration of fungal hyphae in a biomass matrix and their removal through carbonization. The pore size of the macroporous network is 2~5 μm. Mesoporous channels are formed by the enzymatic etching of biomass cellulose components in the biomass matrix by cellulase. The pore size of the mesopores is 2~50 nm. The mesopores are oriented along the walls of the macropores and communicate with the macropores. The micropore array is formed by the self-activation and pore formation of potassium and sodium components contained in the inherent ash of the biomass matrix during the carbonization process. The pore size of the micropores is less than 2 nm, and the micropores are densely distributed on the wall of the mesopore and connected to the mesopore. The macropore network, mesopore channels, and micropore array form a hierarchical interconnected pore system from macropores to mesopores to micropores.
[0030] The macroporous network of this invention is formed by directional template formation using a single fungal species, presenting as a tubular interconnected network. This differs from the irregular, slit-like macropores formed by chemical activation, and also from the amorphous channels formed by composting-based mixed fermentation. Mesoporous channels are directionally distributed along the macropore walls, formed by enzymatic etching with cellulase, exhibiting a bimodal pore size distribution. Micropore arrays are densely distributed on the mesopore walls, formed by the self-activation of inherent ash. This tertiary porosity system, from macropores to mesopores to micropores, achieves highly efficient ion transport from the macroscopic to the microscopic level: macropores act as ion buffer reservoirs, mesopores as ion transport channels, and micropores provide high specific surface area and active sites.
[0031] By utilizing the self-activation effect of the inherent potassium and sodium ash components in the biomass matrix during the carbonization process to form micropores, the problems of equipment corrosion, environmental pollution and washing wastewater caused by the addition of activators such as KOH and ZnCl2 are avoided. It also avoids the high-temperature energy consumption required by adding water vapor and CO2 activation gas.
[0032] The "self-activation" mentioned in this article refers to the process of directly forming micropores in the carbon matrix by using only the inherent potassium and sodium ash components of the biomass matrix as endogenous activators, without the addition of chemical activators such as KOH, NaOH, ZnCl2, and H3PO4, or activating salts such as K2CO3 and KHCO3, or activating gases such as water vapor, CO2, and NH3, during high-temperature carbonization. In this process, the inherent potassium and sodium components have the dual role of catalyzing pore formation and catalyzing graphitization, and are retained in the final product as residual potassium and sodium, constituting the structural markers of the self-activation process route.
[0033] In some specific embodiments, the mold is Aspergillus niger. The diameter of the Aspergillus niger hyphae matches the target macropore size. When growing in the biomass matrix, the hyphae penetrate the gaps between the fiber bundles in a directional manner. The morphology of the channels left after carbonization is highly consistent with the hyphae morphology, making it a preferred species for constructing a 2-5 μm tubular macroporous network.
[0034] In some specific embodiments, the biomass porous carbon includes at least one of the following features A1 to A4: A1. The pore volume of the macroporous network accounts for 15% to 35% of the total pore volume; the pore volume of the mesoporous channels accounts for 20% to 45% of the total pore volume; and the pore volume of the microporous array accounts for 25% to 55% of the total pore volume. A2. The macropores in the macropore network are tubular in shape, with a smoothness Ra value of less than 200 nm on the inner surface of the tube wall, and there are connecting windows with a diameter of 0.5~2 μm between adjacent macropores; A3. The pore size distribution of the mesoporous channel exhibits a bimodal characteristic, with the first peak located in the 2~10 nm range and the second peak located in the 20~50 nm range; the enzymatic hydrolysis rate in the shaping zone is fast, forming smaller mesopores (2~10 nm); the enzymatic hydrolysis rate in the crystallization zone is slow, leaving larger mesopores (20~50 nm) after enzymatic digestion.
[0035] A4. The BET specific surface area of the biomass porous carbon is 500~2000 m². 2 / g, total pore volume is 0.5~1.5 cm³ 3 / g, with an average pore size of 1.5~8.0 nm.
[0036] In some specific implementations, the total potassium and sodium content in the inherent ash of the biomass matrix is 0.05~2.0 wt%.
[0037] The potassium and sodium residues originate from the inherent ash components in the biomass matrix (raw material). During carbonization, potassium and sodium act as endogenous activators, catalyzing the etching of the carbon framework to create pores, thus achieving self-activation pore formation. They remain in the final product, constituting a structural marker of the self-activation process. Their content and ratio can distinguish the product of this invention from products activated by external activators and products washed to neutrality after activation. The potassium-sodium mass ratio reflects the ash composition characteristics of the biomass raw material and is a key structural parameter distinguishing it from products activated by external activators (such as products activated by external KOH, which typically have a potassium content higher than 4 wt% and a potassium-sodium mass ratio greater than 10:1) and products washed to neutrality after activation (with potassium and sodium residues both below 0.1 wt%).
[0038] It should be noted that the inherent potassium and sodium content in biomass raw materials such as distiller's grains can fluctuate depending on the origin, batch, and brewing process, resulting in uncertainty in the potassium-to-sodium mass ratio. To ensure that the residual potassium and sodium content in the product is 0.05–2.0 wt%, this invention tests the ash composition of each batch of distiller's grains before feeding (e.g., using ICP-OES or flame photometry to determine potassium and sodium content), and selects batches of raw materials with a target potassium-to-sodium content falling within the range of 0.05–2.0 wt%. When the potassium-to-sodium mass ratio of the batch used deviates from the above range, batches of raw materials with different potassium and sodium contents are mixed and blended in proportion to ensure that the total potassium and sodium content of the blended raw material falls within the range of 0.05–2.0 wt%, before proceeding with subsequent fermentation, enzymatic hydrolysis, and carbonization steps. In this way, those skilled in the art can reliably obtain the above-mentioned residual potassium and sodium characteristics through conventional batch screening and blending operations based on the raw material test results. The principle is that the fermentation process disperses the potassium and sodium inherent in the raw material in the form of molecules or ions. After pre-carbonization, they are retained in the form of potassium carbonate and organic potassium. During the high-temperature carbonization stage, they participate in self-activation and pore formation and are partially retained in the product. Therefore, the potassium and sodium residues in the product and their mass ratio correspond to the potassium and sodium composition of the raw material and can be directly detected in the product, forming a structural marker for the self-activation process route.
[0039] In some specific embodiments, the biomass porous carbon contains inherent nitrogen doping derived from biomass protein components and inherent oxygen doping derived from biomass oxygen-containing functional groups, wherein the nitrogen content is 1.0~4.0 at%, and the oxygen content is 5.0~15.0 at%.
[0040] The inherent nitrogen doping originates from the protein and amino acid components abundant in biomass raw materials, which are converted into nitrogen-containing carbon structures during the carbonization process, without the need for external nitrogen sources or nitrogen-containing reagents.
[0041] In some specific embodiments, the biomass porous carbon includes at least one of the following features B1 to B3: B1. The carbon framework of the biomass porous carbon is a composite structure consisting of a disordered carbon matrix and locally graphitized microregions. In the XRD pattern, the broadened diffraction peaks corresponding to the (002) crystal plane of the disordered carbon matrix are located at 2θ = 24°~25.5°, and the interlayer spacing d 002 The interlayer spacing is 0.35~0.37 nm, which is greater than the standard interlayer spacing of graphite (0.335 nm), which is beneficial for ion insertion and extraction; and there is also a weak diffraction peak at 2θ=26.4°~26.6° corresponding to the crystal plane of the locally graphitized micro-region (002) (corresponding to the interlayer spacing of 0.335~0.337 nm), and the peak area of the weak diffraction peak accounts for 5%~30% of the total peak area of the crystal plane diffraction; the intensity ratio of D peak to G peak in the Raman spectrum ID / IG is 0.8~1.2, which proves the existence of the locally graphitized micro-region.
[0042] It should be noted that the local graphitized micro-region (002) crystal plane and the disordered carbon matrix (002) crystal plane mentioned in this article refer to the same crystal plane, which corresponds to a weak diffraction peak located at 2θ=26.4°~26.6° and interlayer spacing of 0.335~0.337 nm in the XRD spectrum. For the sake of consistency, this diffraction peak is referred to as "local graphitized micro-region (002)" throughout the article. It has the same meaning as the disordered carbon matrix (002) crystal plane, both referring to the locally ordered stacked structure of sp2 carbon skeleton formed in situ during carbonization, rather than an independently existing crystalline graphite phase.
[0043] It is worth noting that the aforementioned locally graphitized microregions are formed at a carbonization temperature of 700~1000℃, far lower than the temperature required for conventional graphitization (2500~3000℃). This is due to the dual synergistic mechanism employed in this invention: Firstly, the inherent potassium components in the biomass matrix act as catalysts for graphitization during the carbonization process. The inherent potassium, which is molecularly dispersed in the carbon matrix in the form of potassium carbonate and organic potassium after pre-carbonization, reacts with carbon at temperatures above 700℃ to generate potassium vapor in situ. The potassium vapor then intercalates between the disordered carbon layers to form potassium-graphite intercalation compounds. The repeated intercalation and deintercalation promote the rearrangement of carbon network surfaces into more regular graphite stacks. Due to the moderate inherent potassium concentration, graphitization only occurs locally in potassium-rich micro-regions, forming nanoscale graphitized micro-regions dispersed in the disordered carbon matrix. Secondly, fungal fermentation and cellulase hydrolysis preferentially degrade amorphous components, significantly increasing the crystallinity of crystalline cellulose in the residual solid phase. The lattice orientation of highly crystalline cellulose is inherited by the newly formed sp² carbon network surface through the biological template memory effect during carbonization and aromatization, forming locally parallel stacked graphite-like aromatic carbon domains. Therefore, the characteristic peaks of the (002) crystal surface of this locally graphitized micro-region can serve as structural markers for the detection of fermentation, enzymatic hydrolysis, and self-activation technical routes. At the same time, the dispersed graphitized micro-regions construct fast electron conduction channels in the disordered carbon matrix, which is beneficial to improving the rate performance of the material.
[0044] B2. The biomass porous carbon has an irregular lamellar morphology with a lamellar thickness of 0.5~5μm. The lamellar surface is distributed with an array of pores formed by the macroporous network. The lamellar morphology originates from the natural fibrous structure of the biomass matrix (raw material). After fermentation and carbonization, it retains the macroscopic lamellar characteristics, which is different from the spherical particles obtained by spray drying spheroidization process.
[0045] B3. The silicon content of the biomass porous carbon does not exceed 0.5 wt%. The low silicon content is a structural feature achieved through acid elution and silicon removal treatment before carbonization, which helps to improve the electrochemical cycling stability of the material.
[0046] In some specific embodiments, the biomass matrix is selected from distiller's grains, that is, the residue after solid-state fermentation and distillation of grains as raw materials. In some specific embodiments, the distiller's grains include at least one of baijiu (Chinese white liquor) brewing distiller's grains, beer brewing distiller's grains, or huangjiu (yellow wine) brewing distiller's grains; preferably, the distiller's grains are baijiu brewing distiller's grains, including at least one of strong-aroma baijiu distiller's grains, sauce-aroma baijiu distiller's grains, or light-aroma baijiu distiller's grains. The distiller's grains inherently contain potassium, sodium ash, protein, cellulose, and lignin components, with a dry basis content of 0.5-2.0 wt%, sodium 0.2-0.6 wt%, protein 8-15 wt%, cellulose 20-35 wt%, and lignin 15-25 wt%. Using the above-mentioned distiller's grains as a biomass matrix can provide inherent potassium and sodium ash to achieve carbonization self-activation and pore formation. On the other hand, its rich protein and cellulose can provide the material basis for inherent nitrogen doping and enzymatic hydrolysis mesopore formation, respectively. After the distiller's grains are treated by the above steps S1 to S6, the fermentation method graded pore biomass porous carbon of the present invention is obtained.
[0047] According to another aspect of the present invention, a method for preparing the above-mentioned porous carbon from biomass is also provided, comprising the following steps: S1. Raw material pretreatment: The biomass matrix is dried to a moisture content of ≤10 wt% and then pulverized to obtain pretreated biomass matrix; S2. Fermentation of a single mold strain: A single mold strain is inoculated into the pretreated biomass matrix at an inoculation amount of 5% to 15% of the dry mass of the pretreated biomass matrix. The moisture content of the material is adjusted to 50% to 65%, and solid-state fermentation is carried out at 25 to 40°C for 3 to 7 days until the mycelial coverage reaches more than 60%, and the fermented material is obtained. S3. Cellulase hydrolysis: Add cellulase to the fermentation material at a dosage of 20-60 FPU / g dry basis, and hydrolyze for 12-48 h at pH 4.5-5.5 and 45-55℃ to obtain hydrolyzed material; S4. Pre-carbonization: The enzymatically hydrolyzed material is pre-carbonized at 200~300℃ for 1~3 h under an inert atmosphere to obtain the pre-carbonized product; S5. Acid washing and desiliconization: The pre-carbonized product is washed with dilute acid to remove ash and silicon components, then washed with water until neutral and dried to obtain the acid-washed material. S6. High-temperature carbonization self-activation: The pickled material is carbonized at 700~1000℃ for 1~3 h in an inert atmosphere. The inherent potassium and sodium ash groups in the biomass matrix are self-activated and form pores during the carbonization process. After cooling, porous biomass carbon is obtained.
[0048] In the three-level interconnected hierarchical pore structure of the present invention, the pore size and pore volume ratio of each level can be independently controlled by fermentation conditions (strain selection, inoculum amount, fermentation time), enzymatic hydrolysis conditions (enzyme type, enzymatic hydrolysis time) and carbonization conditions (temperature, heating rate), thus realizing the precise design of the hierarchical pore structure. The pore size and connectivity of the macroporous network are mainly determined by the single mold species and fermentation time: Using *Aspergillus niger* as the sole fermentation species, with an inoculum size of 5%–15% of the pretreated dry lees, solid-state fermentation at 25–40℃ for 3–7 days, and a mycelial coverage rate exceeding 60%, leaves a tubular interconnected macroporous network with pore sizes of 2–5 μm after the mycelium grows through the biomass matrix and is removed by carbonization. There are connecting windows with pore sizes of 0.5–2 μm between adjacent macropores. The pore size distribution of the mesoporous channels is regulated by the amount of cellulase added, the enzymatic hydrolysis temperature, and the time: with an enzyme addition of 20–60 FPU / g dry lees, and enzymatic hydrolysis at pH 4.5–5.5 and 45–55℃ for 12–48 h, the amorphous cellulose regions are preferentially hydrolyzed to form smaller mesopores of 2–10 nm, while the crystalline regions are hydrolyzed more slowly, forming smaller mesopores of 20–50 nm. Larger mesopores (nm) are formed, resulting in a bimodal pore size distribution. The pore volume ratio of the micropore array is determined by both the carbonization temperature and the inherent potassium and sodium content of the raw material: under the conditions of carbonization temperature of 700~1000℃, carbonization time of 1~3 h, and residual potassium in the product of 0.1~2.0 wt%, the micropore volume formed by the self-activation of inherent potassium and sodium ash accounts for 25%~55% of the total pore volume. Accordingly, those skilled in the art can adjust the above fermentation, enzymatic hydrolysis, and carbonization conditions according to the target pore structure parameters to obtain the corresponding hierarchical pore structure.
[0049] It should be noted that the preparation method does not add an activator, and the product is not washed with water to remove ash after carbonization, so as to retain the inherent self-activation residual characteristics of potassium and sodium ash.
[0050] In some specific embodiments, in step S1, the total content of inherent potassium and sodium in the biomass matrix is 0.05~2.0 wt%; the total content of inherent potassium and sodium in the biomass matrix is tested, and when the total content of potassium and sodium in the tested batch is not between 0.05~2.0 wt%, different batches of distiller's grains are blended in proportion so that the content of potassium and sodium in the blended raw material is between 0.05~2.0 wt%, and then the subsequent steps are carried out.
[0051] In some specific embodiments, the inoculum amount of *Aspergillus niger* in step S2 is 5% to 15% of the dry weight of the pretreated distiller's grains, the solid-state fermentation temperature is 25 to 40°C, and the solid-state fermentation time is 3 to 7 days; and / or, In some specific embodiments, the amount of cellulase added in step S3 is 20~60 FPU / g dry basis, the hydrolysis temperature is 45~55℃, and the hydrolysis time is 12~48 h.
[0052] In some specific embodiments, the carbonization temperature in step S6 is 700~900℃, and the carbonization time is 1~3 h.
[0053] The hierarchical pore structure of this invention provides an efficient ion transport path and abundant active sites, making it suitable for lithium-ion batteries, sodium-ion batteries, and supercapacitor anode materials, while maintaining high specific capacity and cycle stability even at high current densities.
[0054] According to another aspect of the present invention, a battery electrode material is also provided, wherein the active material of the electrode sheet comprises the above-described biomass porous carbon or the biomass porous carbon prepared by the preparation method described in claim 7 or 8.
[0055] Specifically, the battery electrode includes at least one of a lithium-ion battery negative electrode, a sodium-ion battery negative electrode, or a supercapacitor electrode.
[0056] According to another aspect of the present invention, a battery comprising the above-described electrode plates is also provided.
[0057] The present invention will be further illustrated below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or purchased directly from the market.
[0058] In the following examples and comparative examples, the structural characteristics of biomass porous carbon were detected using the following methods: Particle morphology and macroporous network morphology were observed using scanning electron microscopy (SEM). Macropore diameter, connectivity window size, and inner surface roughness Ra value of the tube wall were obtained statistically from SEM images. Specific surface area, total pore volume, and pore size distribution were determined using nitrogen adsorption-desorption (-196℃). Specific surface area was calculated using the BET model, total pore volume was converted from nitrogen adsorption at a relative pressure P / P0 = 0.99, and pore size distribution was calculated using nonlocal density functional theory (NLDFT). The pore volume percentages were statistically analyzed, with pores less than 2 nm classified as micropores, 2–50 nm as mesopores, and greater than 50 nm as macropores. X-ray diffraction (Current X-ray diffraction) was used to determine the pore size distribution. XRD spectra were acquired using Kα radiation (2θ scan range 10°~80°). The diffraction peaks in the 2θ = 20°~30° range were fitted to determine the peak positions and interlayer spacing d002 of the broadened diffraction peaks of the (002) crystal plane of the disordered carbon matrix, as well as the peak positions and peak areas of the weak diffraction peaks of the (002) crystal plane in the local graphitized micro-regions, and the percentage of the total peak area of the (002) crystal plane diffraction. The intensity ratio ID / IG of the D peak and G peak was determined using a laser Raman spectrometer (excitation wavelength 532 nm), and the 2D peak at approximately 2690 cm⁻¹ was examined. The contents of potassium, sodium and silicon in the sample were determined using an inductively coupled plasma optical emission spectrometer (ICP-OES) after microwave digestion. The atomic contents of nitrogen and oxygen in the sample were determined using X-ray photoelectron spectroscopy (XPS).
[0059] Example 1 1. Raw materials: The biomass raw material is the lees from baijiu brewing, which has an inherent potassium content of 1.2 wt%, sodium content of 0.4 wt%, protein content of 12 wt%, cellulose content of 28 wt%, and lignin content of 18 wt%.
[0060] 2. Preparation of porous carbon from fermented graded biomass: (1) The lees from the brewing of baijiu (with an inherent potassium content of 1.2 wt%, a sodium content of 0.4 wt%, and a total potassium and sodium content of 1.6 wt%) are dried to a moisture content of less than 10 wt% and then crushed through a 40-mesh sieve to obtain pretreated lees; (2) Inoculate 8% of the dry weight of pretreated distiller's grains with Aspergillus niger bran starter, add water to adjust the moisture content of the material to 55 wt%, and ferment in solid state at 30℃ and 90% relative humidity for 4 days. At the end of fermentation, the mycelial coverage rate is 70% and the weight loss rate is 22%, and the fermented material is obtained. (3) Cellulase was added to the fermentation material at 40 FPU / g dry basis, the pH was adjusted to 4.8 with citrate-sodium citrate buffer, and the material was enzymatically hydrolyzed at 50℃ for 24 h. Then the enzyme was inactivated at 80℃ for 10 min and dried to obtain the enzymatically hydrolyzed material. (4) The enzymatic hydrolysate was pre-carbonized at 250°C for 2 h under a nitrogen atmosphere at a rate of 5°C / min to obtain the pre-carbonized product; (5) The pre-carbonized product was washed with 1 mol / L hydrochloric acid at 70°C for 2 h, then washed with deionized water until neutral and dried to obtain the pickled material. (6) The temperature was raised to 750℃ at 5℃ / min under a nitrogen atmosphere and held for 2 h for carbonization. The carbon was then cooled to room temperature in the furnace to obtain porous carbon of fermentation-based graded pore biomass.
[0061] In this embodiment, no external activator is added, and the product is not washed with water to remove ash after carbonization, so as to retain the inherent self-activation residual characteristics of potassium and sodium ash.
[0062] 3. Structural characteristics detection of porous carbon in fermentation-based graded-pore biomass: (1) Macropore network: The pore size is 2~5 μm, distributed in a tubular interconnected network, the smoothness Ra value of the inner surface of the tube wall is 120 nm, and there are interconnecting windows with a pore size of 0.5~1.5 μm between adjacent macropores. The macropore volume accounts for 25% of the total pore volume.
[0063] (2) Mesoporous channels: The pore size distribution exhibits a bimodal characteristic, with the first peak located in the 3~8 nm range and the second peak located in the 25~40 nm range. Mesopores are oriented along the walls of macropores and communicate with them. The volume of mesopores accounts for 35% of the total pore volume.
[0064] (3) Micropore array: The pore size is less than 2 nm and it is densely distributed on the wall of the mesopore. The micropore volume accounts for 40% of the total pore volume.
[0065] (4) The specific surface area of BET is 1280 m². 2 / g, total pore volume is 0.85 cm³ 3 / g, with an average pore size of 3.2 nm.
[0066] (5) The residual potassium content was determined to be 0.8 wt% and the residual sodium content was 0.25 wt% by ICP-OES.
[0067] (6) The nitrogen content determined by XPS was 2.5 at and the oxygen content was 8.7 at.
[0068] (7) In the XRD pattern, the broadening diffraction peak of the (002) crystal plane of the disordered carbon matrix is located at 2θ=24.8°, corresponding to the interlayer spacing d 002 =0.358 nm; a weak diffraction peak of the (002) crystal plane exists in a local graphitized micro-region at 2θ=26.5°, and its peak area accounts for 15% of the total peak area of the (002) crystal plane diffraction after peak fitting; the Raman ID / IG is 0.95, and it is ~2690 cm⁻¹. - A faint 2D peak was observed at point ¹.
[0069] (8) The silicon content is 0.15 wt%.
[0070] (9) The particle morphology is irregular lamellar, and the lamellar thickness is 1~3 μm.
[0071] Example 2 1. Raw materials: The biomass raw material is the lees from baijiu brewing, which has an inherent potassium content of 1.5 wt% and a sodium content of 0.3 wt%.
[0072] 2. Preparation of porous carbon from fermented graded biomass: (1) Dry the lees from the brewing of baijiu (with an inherent potassium content of 1.5 wt%, a sodium content of 0.3 wt%, and a total potassium and sodium content of 1.8 wt%) to a moisture content of less than 10 wt% and crush them through a 40-mesh sieve to obtain pretreated lees; (2) Inoculate 10% of the dry weight of pretreated distiller's grains with Aspergillus niger bran starter, add water to adjust the moisture content of the material to 60 wt%, and ferment in solid state at 32℃ and 90% relative humidity for 5 days. At the end of fermentation, the mycelial coverage rate is 75% and the weight loss rate is 26%, and the fermented material is obtained. (3) Cellulase was added to the fermentation material at 50 FPU / g dry basis, the pH was adjusted to 5.0 with citrate-sodium citrate buffer, and the material was enzymatically hydrolyzed at 52℃ for 36 h. Then the enzyme was inactivated at 80℃ for 10 min and dried to obtain the enzymatically hydrolyzed material. (4) The enzymatic hydrolysate was pre-carbonized at 250°C for 2 h under a nitrogen atmosphere at a rate of 5°C / min to obtain the pre-carbonized product; (5) The pre-carbonized product was washed with 1 mol / L hydrochloric acid at 70°C for 2 h, then washed with deionized water until neutral and dried to obtain the pickled material. (6) The temperature was raised to 800℃ at 5℃ / min under a nitrogen atmosphere and held for 2 h for carbonization. The carbon was then cooled to room temperature in the furnace to obtain porous carbon of fermentation-based graded pore biomass.
[0073] In this embodiment, no activator is added, and the product is not washed with water to remove ash after carbonization.
[0074] 3. Structural characteristics detection of porous carbon in fermentation-based graded-pore biomass: (1) Macropore network: The pore size is 2~4 μm, distributed in a tubular interconnected network, the smoothness Ra value of the inner surface of the tube wall is 95nm, and there are interconnecting windows with a pore size of 0.8~2 μm between adjacent macropores. The macropore volume accounts for 20% of the total pore volume.
[0075] (2) Mesoporous channels: The pore size distribution exhibits a bimodal characteristic, with the first peak located in the 2~6 nm range and the second peak located in the 20~35 nm range. Mesoporous pore volume accounts for 30% of the total pore volume.
[0076] (3) Micropore array: pore size is less than 2 nm, and the micropore volume accounts for 50% of the total pore volume.
[0077] (4) The specific surface area of BET is 1560 m². 2 / g, total pore volume is 1.12 cm³ 3 / g, with an average pore size of 2.8 nm.
[0078] (5) The residual potassium content was determined to be 1.1 wt% and the residual sodium content was 0.2 wt% by ICP-OES.
[0079] (6) The nitrogen content determined by XPS was 3.1 at% and the oxygen content was 10.2 at%.
[0080] (7) In the XRD pattern, the broadening diffraction peak of the (002) crystal plane of the disordered carbon matrix is located at 2θ=25.3°, corresponding to the interlayer spacing d 002 =0.352 nm; a weak diffraction peak of the (002) crystal plane exists in the local graphitized micro-region at 2θ=26.5°, and the peak area accounts for 22% of the total peak area of the (002) crystal plane diffraction, which is the highest among the three examples, corresponding to its highest potassium residue (1.1 wt%); Raman ID / IG is 1.05.
[0081] (8) The silicon content is 0.08 wt%.
[0082] (9) The particle morphology is irregular lamellar, and the lamellar thickness is 1~2 μm.
[0083] Example 3 1. Raw materials: The biomass raw material is the lees from baijiu brewing, which has an inherent potassium content of 0.9 wt% and a sodium content of 0.5 wt%.
[0084] 2. Preparation of porous carbon from fermented graded biomass: (1) The lees from the brewing of baijiu (with an inherent potassium content of 0.9 wt%, a sodium content of 0.5 wt%, and a total potassium and sodium content of 1.4 wt%) are dried to a moisture content of less than 10 wt% and then crushed through a 40-mesh sieve to obtain pretreated lees; (2) Inoculate 6% of the dry weight of pretreated distiller's grains with Aspergillus niger bran starter, add water to adjust the moisture content of the material to 52 wt%, and ferment in solid state at 28℃ and 90% relative humidity for 3 days. At the end of fermentation, the mycelial coverage rate is 62% and the weight loss rate is 16%, and the fermented material is obtained. (3) Cellulase was added to the fermentation material at 25 FPU / g dry basis, the pH was adjusted to 4.6 with citrate-sodium citrate buffer, and the material was enzymatically hydrolyzed at 48℃ for 18 h. Then the enzyme was inactivated at 80℃ for 10 min and dried to obtain the enzymatically hydrolyzed material. (4) The enzymatic hydrolysate was pre-carbonized at 250°C for 2 h under a nitrogen atmosphere at a rate of 5°C / min to obtain the pre-carbonized product; (5) The pre-carbonized product was washed with 1 mol / L hydrochloric acid at 70°C for 2 h, then washed with deionized water until neutral and dried to obtain the pickled material. (6) The temperature was raised to 700℃ at 5℃ / min under a nitrogen atmosphere and carbonized for 2 h. The carbon was then cooled to room temperature in the furnace to obtain porous carbon of fermentation-based graded pore biomass.
[0085] In this embodiment, no activator is added, and the product is not washed with water to remove ash after carbonization.
[0086] 3. Structural characteristics detection of porous carbon in fermentation-based graded-pore biomass: (1) Macropore network: The pore size is 3~5 μm, distributed in a tubular interconnected network, the smoothness Ra value of the inner surface of the tube wall is 165nm, and there are interconnecting windows with a pore size of 0.5~1.2 μm between adjacent macropores. The macropore volume accounts for 30% of the total pore volume.
[0087] (2) Mesoporous channels: The pore size distribution exhibits a bimodal characteristic, with the first peak located in the 4~10 nm range and the second peak located in the 30~50 nm range. Mesoporous pore volume accounts for 40% of the total pore volume.
[0088] (3) Micropore array: pore size is less than 2 nm, and the micropore volume accounts for 30% of the total pore volume.
[0089] (4) The specific surface area of BET is 920 m². 2 / g, total pore volume is 0.62 cm³ 3 / g, with an average pore size of 4.5 nm.
[0090] (5) The residual potassium content was determined to be 0.5 wt% and the residual sodium content was 0.3 wt% by ICP-OES.
[0091] (6) The nitrogen content determined by XPS was 1.8 at% and the oxygen content was 7.3 at%.
[0092] (7) In the XRD pattern, the broadening diffraction peak of the (002) crystal plane of the disordered carbon matrix is located at 2θ=24.4°, corresponding to the interlayer spacing d 002=0.365 nm; a weak diffraction peak of the (002) crystal plane with local graphitization micro-region exists at 2θ=26.5°, and the peak area accounts for 8% of the total peak area of the (002) crystal plane diffraction, which is the lowest among the three examples, corresponding to its lowest potassium residue (0.5 wt%); Raman ID / IG is 0.88.
[0093] (8) The silicon content is 0.22 wt%.
[0094] (9) The particle morphology is irregular lamellar, and the lamellar thickness is 2~4 μm.
[0095] Comparative Example 1 Using the same batch of baijiu brewing lees as in Example 1 as raw material (its inherent potassium content is 1.2 wt%, sodium content is 0.4 wt%, and total potassium and sodium content is 1.6 wt%), without mold fermentation and enzymatic hydrolysis, it is directly subjected to pre-carbonization and high-temperature carbonization (without the addition of an activator). Specifically, it includes: The above-mentioned lees were dried to a moisture content of less than 10 wt% and pulverized through a 40-mesh sieve. Without inoculation with any microorganisms or enzymatic hydrolysis, they were directly pre-carbonized at 250°C for 2 h under a nitrogen atmosphere at a rate of 5°C / min. The pre-carbonized product was washed with 1 mol / L hydrochloric acid at 70°C with stirring for 2 h, then washed with deionized water until neutral and dried. Finally, it was carbonized at 750°C under a nitrogen atmosphere at a rate of 5°C / min for 2 h and cooled in the furnace to obtain the control sample.
[0096] Structural characteristics detection of porous carbon in fermentation-based graded-pore biomass: BET has a specific surface area of 180 m² 2 / g, total pore volume is 0.12 cm³ 3 The macroporous network structure was absent, and the mesoporous ratio was less than 5%. ICP-OES analysis showed that the residual potassium was 0.15 wt% and the residual sodium was 0.06 wt%. In the XRD pattern, only the broadened disordered carbon (002) crystal plane appeared at 2θ≈23°, and there were no characteristic peaks of local graphitized micro-regions (002) crystal planes in the 2θ=26.4°~26.6° range. This indicates that the lack of fungal hyphae template formation and enzymatic etching prevented the formation of a three-level interconnected hierarchical pore structure, and the lack of interconnected macropores contributed by hyphae templates hindered ion transport. At the same time, the lack of the biological template memory effect brought about by enzymatic hydrolysis and concentration of crystalline cellulose, and the low effective catalytic concentration of potassium component due to the lack of homogenized dispersion without fermentation and enzymatic hydrolysis, resulted in the absence of local graphitized micro-regions (002) diffraction peaks in the carbonized product.
[0097] Comparative Example 2 Using the same batch of baijiu brewing lees as in Example 1 as raw material (its inherent potassium content is 1.2 wt%, sodium content is 0.4 wt%, and total potassium and sodium content is 1.6 wt%), the mixture underwent Aspergillus niger fermentation and cellulase enzymatic hydrolysis treatment as in Example 1, followed by high-temperature activation with added KOH (alkali-to-carbon ratio 2:1). Specifically, this included: Aspergillus niger fermentation and cellulase hydrolysis were performed according to the same steps as in Example 1 to obtain enzymatic hydrolysate. The enzymatic hydrolysate was pre-carbonized at 250°C for 2 h under a nitrogen atmosphere by heating at 5°C / min. The pre-carbonized product was ground and mixed with KOH at an alkali-to-carbon mass ratio of 2:1, and then activated at 800°C for 1 h under a nitrogen atmosphere by heating at 5°C / min. The activated product was then cooled in the furnace. The activated product was washed with deionized water until neutral and dried to obtain a control sample.
[0098] Structural characteristics detection of porous carbon in fermentation-based graded-pore biomass: BET has a specific surface area of 2150 m². 2 / g, total pore volume is 1.35 cm³ 3 / g. However, its macropore morphology is irregular fissure rather than tubular, and the wall roughness Ra value is greater than 500 nm; the mesopore distribution is unimodal rather than bimodal; ICP-OES analysis shows that the potassium content is as high as 4.8 wt%, the sodium content is 0.08 wt%, and the total potassium and sodium content is 4.88 wt%, far exceeding the 0.5~2 wt% range specified in this invention. In its XRD pattern, the broadened peak of disordered carbon (002) shifts to a lower angle (d 002 The peak width was >0.38 nm and the peak width was increased. There were no local graphitized micro-regions (002) crystal plane characteristic peaks in the 2θ=26.4°~26.6° range. This indicates that although the addition of KOH activation increased the specific surface area, it destroyed the tubular macropore morphology of hyphal template and the bimodal distribution characteristics of enzymatic hydrolysis mesopores. Moreover, the potassium-sodium mass ratio deviated significantly from the characteristic range of the self-activated product, and the product did not have the self-activated structure marker of the present invention. When the alkali-to-carbon ratio of the added KOH was 2:1, the activation reaction was dominated by carbon skeleton vaporization etching. The ordered structure was formed and consumed at the same time. It can be seen that the formation of catalytic graphitization depends on the molecular-level dispersion and moderate concentration of potassium. High concentration of added activator inhibits the formation and retention of graphitized micro-regions.
[0099] Comparative Example 3 Using the same batch of baijiu brewing lees as in Example 1 as raw material (with an inherent potassium content of 1.2 wt%, a sodium content of 0.4 wt%, and a total potassium and sodium content of 1.6 wt%), the same Aspergillus niger fermentation and cellulase enzymatic hydrolysis treatment as in Example 1 was employed. Instead of relying on inherent ash for self-activation, physical activation with steam (800℃, steam flow rate 50 mL / min, activation time 2 h) was used. Specifically, this included: Following the same steps as in Example 1, Aspergillus niger fermentation, cellulase hydrolysis, pre-carbonization at 250°C, and acid washing and desilication were performed to obtain the acid-washed material. The acid-washed material was heated to 800°C at 5°C / min under a nitrogen atmosphere, and then activated by introducing steam (flow rate 50 mL / min) for 2 h. It was then cooled and dried in the furnace to obtain the comparative sample.
[0100] Structural characteristics detection of porous carbon in fermentation-based graded-pore biomass: BET has a specific surface area of 680 m² 2 / g, total pore volume is 0.45 cm³ 3 / g. ICP-OES analysis showed that the potassium content was 0.05 wt% and the sodium content was 0.03 wt%, both lower than the self-activated structure marker content range defined in this invention. The macroporous and mesoporous structures were similar to those in Example 1, but the micropore volume accounted for only 15% of the total pore volume, far lower than the 25%~55% range of this invention. Its XRD pattern also lacked the characteristic peak of the (002) crystal plane in the 2θ=26.4°~26.6° region—the water vapor activation gas flow carried away the potassium component (potassium residue was only 0.05 wt%), losing the catalytic graphitization conditions, and physical activation etching introduced additional structural disorder. The results indicate that even when water vapor activation is used instead of self-activation, the micropore formation efficiency is still significantly lower than the inherent ash self-activation route, and the residual potassium and sodium content is also lower than the characteristic range of the self-activated structure marker.
[0101] Comparative Example 4 Using the same batch of baijiu brewing lees as in Example 1 as raw material (with an inherent potassium content of 1.2 wt%, a sodium content of 0.4 wt%, and a total potassium and sodium content of 1.6 wt%), the product was processed according to the same Aspergillus niger fermentation, cellulase hydrolysis, and high-temperature carbonization process as in Example 1. After carbonization, the product was thoroughly washed with water until neutral to investigate the binding relationship between potassium and sodium residues and the self-activated microporous structure. Specifically, this included: The same steps as in Example 1 were followed for Aspergillus niger fermentation, cellulase hydrolysis, pre-carbonization, acid washing and desilication, and high-temperature carbonization at 750°C to obtain the carbonized product. The carbonized product was then repeatedly washed with deionized water at 80°C until the washing solution was neutral (pH approximately 7), and dried to obtain the comparative sample. The only difference between this comparative sample and Example 1 was whether or not the product was washed with water after carbonization.
[0102] Structural characteristics detection of porous carbon in fermentation-based graded-pore biomass: BET has a specific surface area of 760 m² 2 / g, compared to 1280 m in Example 1 2 / g decreased by 40.6%; total pore volume was 0.52 cm³. 3 / g; ICP-OES analysis showed that potassium residue was 0.06 wt% and sodium residue was 0.02 wt%, both lower than the self-activation structure labeling limit specified in this invention (potassium 0.1 wt%, sodium 0.05 wt%); the proportion of micropore volume to total pore volume decreased from 40% in Example 1 to 18%. In the XRD pattern, the weak diffraction peak of the (002) crystal plane of the local graphitized micro-region at 2θ=26.5° was still retained, with a peak area ratio of 14%, which is basically consistent with 15% in Example 1, while the potassium residue decreased from 0.8 wt% to 0.06 wt%.
[0103] In this comparative example, washing to neutrality only removed residual potassium and sodium ash, without touching the hyphal templated macropores and enzymatically hydrolyzed mesopores (whose tubular morphology and bimodal distribution were retained). However, the micropore volume ratio dropped sharply from 40% to 18%, and the specific surface area decreased by more than 40%. This indicates that the formation of the micropore array in this invention is indeed dominated by the self-activation effect of inherent potassium and sodium ash, and the residual potassium and sodium content is positively correlated with the degree of micropore development, with the potassium and sodium residue serving as a marker of self-activated structure. Simultaneously, the potassium and sodium residue in this comparative example product is lower than the potassium content (0.1~2.0 wt%) specified in this invention, demonstrating the function of potassium and sodium residue markers as a distinguishing marker for the biomass porous carbon prepared in this invention. Furthermore, the weak diffraction peak of the (002) crystal plane in the locally graphitized micro-region was still retained after washing to remove potassium, proving that this peak belongs to the sp peak formed in situ during the carbonization process. 2 The diffraction contribution is from the ordered carbon framework structure (locally graphitized micro-regions), rather than from the residual potassium salt crystals—water washing removes potassium and sodium ash, but the formed graphitized micro-regions, as stable framework structures, remain unaffected. The diffraction peaks of the locally graphitized micro-regions (002) and the residual potassium and sodium crystals thus constitute a dual structural marker originating from the self-activation process but independently detectable.
[0104] Comparative Example 5 Using the same batch of baijiu brewing lees as in Example 1 as raw material (with an inherent potassium content of 1.2 wt%, a sodium content of 0.4 wt%, and a total potassium and sodium content of 1.6 wt%), the preparation was carried out according to the route disclosed in the patent with publication number CN122166772A: the raw material was mixed with urea (urea accounted for 10% of the dry weight), inoculated with a natural compound fermentation agent (compost-type mixed agent, accounting for 3% of the dry weight), and aerobic fermentation was carried out in a pile for 8 days (the temperature at the center of the pile was maintained at 50~60℃). After drying, it was carbonized at 500℃ for 3 h in a nitrogen atmosphere, and then activated at 800℃ for 1.5 h by introducing steam. The activated product was washed with water until neutral.
[0105] Structural characteristics detection of porous carbon in fermentation-based graded-pore biomass: BET has a specific surface area of 1720 m² / g and a total pore volume of 1.58 cm³. 3 / g, mesoporous pore volume is 0.91 cm³ 3 / g (accounting for 57.6% of the total pore volume), with a micropore volume of 0.63 cm³. 3 / g. However: (1) SEM observation showed that its pore morphology was a mixture of amorphous channels and activated etched holes, without tubular interconnected macropore network, rough pore walls, and no 0.5~2 μm interconnected window structure.
[0106] (2) The mesopore size distribution shows a single-peak broadening characteristic (concentrated in 30~60 nm), and there is no bimodal distribution corresponding to the enzymatic hydrolysis of cellulose partitions; (3) ICP-OES analysis showed that the potassium residue was 0.04 wt% and the sodium residue was 0.02 wt%, which is far below the range of the self-activated structure labeling of this invention.
[0107] (4) Its mesoporous pore volume ratio is 57.6%, which exceeds the upper limit of 20%~45% specified in this invention.
[0108] (5) In the XRD pattern, only the broadened disordered carbon (002) halo appears at 2θ≈23°. There are no local graphitized micro-regions (002) crystal plane characteristic peaks in the 2θ=26.4°~26.6° range. This is mainly because the composting mixed fermentation has no directional concentration effect on the crystallinity of cellulose, the water vapor activation introduces structural disorder, and the washing to neutral removes potassium components. These three factors together cause the product to not have local graphitized micro-regions.
[0109] The results showed that composting fermentation does not produce hyphal templated tubular macropores; the product mainly formed by the addition of activating gas does not have potassium and sodium self-activation residual markers; its pore size distribution, mesopore ratio, and composition fingerprint all have detectable substantial differences from the three-level interconnected hierarchical pore structure of the present invention.
[0110] Characterization of the (002) diffraction peaks in the locally graphitized micro-regions of the carbonization products: In the XRD patterns of the high-temperature carbonization products (carbonization temperature 700~800℃) of Examples 1~3 of this invention, except for those located at 2θ=24°~25.5°, corresponding to interlayer spacing d 002 Apart from the broadened diffraction peaks of the (002) crystal plane in the disordered carbon matrix at 0.35~0.37 nm, there are reproducible weak diffraction peaks at 2θ=26.4°~26.6°. Peak fitting confirmed that the corresponding interlayer spacing is 0.335~0.337 nm, which corresponds to the (002) crystal plane of the locally graphitized micro-regions; Raman spectra at ~2690 cm⁻¹. -The weak 2D peak at ¹ corroborates this, indicating the presence of locally graphitized micro-regions dispersed within the disordered carbon matrix. Control experiments show that no (002) diffraction peaks were observed in the pre-carbonization intermediates (200–300 °C); products with carbonization temperatures below 650 °C only exhibited broadened disordered carbon halos; this diffraction peak appeared only when the carbonization temperature reached 700 °C or higher, and its intensity increased with increasing carbonization temperature and potassium residue. This temperature threshold coincides with the initial temperature (approximately 700 °C) of the reaction where potassium carbonate is reduced by carbon to generate potassium vapor. It should be noted that this peak can exclude interference from crystalline silicon dioxide (quartz (101) crystal plane is located at 2θ≈26.6°): the silicon content of the product of this invention after acid elution and desiliconization does not exceed 0.5 wt%, and the other characteristic peak positions of the quartz (101) crystal plane in the XRD spectrum (2θ≈20.9°, 36.5°, 50.1°) do not diffract. In addition, this diffraction peak only appears above 700℃, while the quartz in the raw material should exist at any carbonization temperature.
[0111] Combination Figure 5 (Schematic diagram of the formation mechanism of local graphitized micro-regions, where A is the K+ intercalation promoting the rearrangement and stacking of carbon network surfaces, B is the removal of amorphous regions of cellulose and the inheritance of crystal orientation, and C is the ordered stacking of π-π aromatic rings in the aromatic structure), explaining the cause of the diffraction peak of the (002) local graphitized micro-regions in the carbonization product: First, the inherent potassium in the distiller's grains used in this invention exists as potassium carbonate and organic potassium after pre-carbonization. Due to the disruption of the dense structure of the biomass by fermentation and enzymatic hydrolysis pretreatment, it is dispersed at the molecular level within the carbon matrix, unlike the activator that interacts with carbon through particle accumulation and localized contact when KOH is added. When the carbonization temperature rises above 700℃, the reaction K₂CO₃ + 2C → 2K↑ + 3CO↑ occurs, and the in-situ generated potassium vapor inserts into the disordered carbon layers to form potassium-graphite intercalation compounds (such as KC8). The repeated intercalation and deintercalation gradually flattens the coiled, disordered carbon network and rearranges it into a more regular graphite stacking structure (corresponding to...). Figure 5(A). Due to the moderate inherent potassium concentration (potassium residue in the product is 0.5~1.1 wt%), catalytic graphitization only occurs locally in potassium-enriched micro-regions, forming nanoscale graphitized micro-regions dispersed in the disordered carbon matrix. Macroscopically, this manifests as weak local graphitized micro-region (002) diffraction peaks rather than overall graphitization. The area ratio of local graphitized micro-region (002) diffraction peaks in Examples 1-3 (15%, 22%, 8%) is positively correlated with the potassium residue (0.8, 1.1, 0.5 wt%). Comparative Example 3 (potassium is removed by steam activation gas flow, potassium residue is 0.05 wt%) and Comparative Example 5 (washed to neutral depotassium, potassium residue is 0.04 wt%) have no local graphitized micro-region (002) diffraction peaks, which jointly confirms the cause of potassium-catalyzed graphitization. Comparative Example 2 (with added KOH, alkali-to-carbon ratio 2:1) showed no local graphitized micro-region (002) diffraction peak, indicating that catalytic graphitization requires molecular-level dispersion and moderate concentration of potassium. Under high concentration of added activator, the carbon skeleton vaporization etching reaction is dominant, and the ordered structure is consumed as it is formed, making it impossible to retain the graphitized micro-region.
[0112] Second, cellulase preferentially hydrolyzes the amorphous region of cellulose, while mold fermentation simultaneously consumes easily degradable components. The synergistic effect of both significantly increases the crystallinity index of the residual solid phase of cellulose (from approximately 45% in the raw material to approximately 65% after fermentation). The molecular chains of cellulose type I crystals are highly parallel and oriented within the crystal region, with an interplanar spacing of approximately 0.39 nm for the (200) crystal planes. During carbonization, crystalline cellulose undergoes a sequence transformation involving dehydration, furanose intermediate formation, and aromatization. The stacking orientation of the newly formed sp² carbon network inherits the orientation information of the original cellulose crystal region (structural memory effect), forming locally parallel stacked aromatic carbon domains. The interplanar spacing shrinks from approximately 0.39 nm to 0.335~0.34 nm, contributing to the diffraction peaks of the (002) diffraction peaks in the locally graphitized microregions (corresponding to...). Figure 5 (B). Comparative Example 1 (without fermentation and enzymatic hydrolysis, direct carbonization) showed no local graphitized micro-region (002) diffraction peak, indicating that the formation of this biological template memory effect requires the concentration of crystalline components by fermentation and enzymatic hydrolysis as a necessary condition.
[0113] Third, the condensation of aromatic domains after fermentation to remove non-aromatic components, and the elimination of interference. The carbonization of aliphatic components such as hemicellulose tends to form disordered glassy carbon. The mold fermentation and enzymatic hydrolysis processes remove most of the hemicellulose, resulting in a relatively higher proportion of lignin-derived aromatic structures in the residual solid phase. During carbonization at 700-1000℃, these pre-aromaticated domains undergo dealkylation and condensation reactions to form larger fused-ring aromatic flat plates, with localized π-π stacking and ordering, contributing to the (002) diffraction peaks of the local graphitized micro-regions (corresponding to...). Figure 5 (C)
[0114] Furthermore, in Comparative Example 4, after the carbonized product was washed with water to neutrality, the potassium residue decreased to 0.06 wt%, while the diffraction peak of the local graphitized micro-region (002) at 2θ=26.5° was still retained (peak area ratio of 14%, comparable to 15% in Example 1), indicating that the peak belongs to the ordered structure of the sp² carbon skeleton itself rather than potassium salt crystals; the product of this invention was desiliconized by acid elution, and the silicon content did not exceed 0.5 wt%, and the other characteristic peak positions of the quartz (101) crystal plane in the XRD spectrum (2θ≈20.9°, 36.5°, 50.1°) did not diffract. In addition, the diffraction peak only appears above 700°C, while the quartz in the raw material should exist at any carbonization temperature, which can eliminate the interference of crystalline silicon dioxide (quartz (101) crystal plane is located at 2θ≈26.6°); Raman spectrum ~2690 cm⁻¹ - The weak 2D peak at ¹ is direct evidence of long-range ordering of sp2 carbons. In summary, this diffraction peak is the result of the synergistic effect of three factors: intrinsic potassium-catalyzed graphitization, the template memory effect of enzymatic hydrolysis and concentration of crystalline cellulose, and the condensation of aromatic domains.
[0115] It should be noted that (101) in the quartz (101) crystal plane marked in the text is the crystal plane index (Miller index) of quartz crystal, which is used to identify a family of crystal planes with a specific orientation in quartz crystal, and does not represent other process numbers or operation steps.
[0116] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A fermentation-based graded porous biomass carbon, characterized in that, The biomass porous carbon has a three-level interconnected hierarchical pore structure, which includes: Macroporous networks are tubular interconnected channels formed by the growth and penetration of fungal hyphae in a biomass matrix and their removal through carbonization. The pore size of the macroporous network is 2~5 μm. Mesoporous channels are formed by the enzymatic etching of biomass cellulose components in the biomass matrix by cellulase. The pore size of the mesopores is 2~50 nm. The mesopores are oriented along the walls of the macropores and communicate with the macropores. The micropore array is formed by the self-activation and pore formation of potassium and sodium components contained in the inherent ash of the biomass matrix during the carbonization process. The pore size of the micropores is less than 2 nm, and the micropores are densely distributed on the wall of the mesopore and connected to the mesopore. The macropore network, mesopore channels, and micropore array form a hierarchical interconnected pore system from macropores to mesopores to micropores.
2. The biomass porous carbon according to claim 1, characterized in that, The mold is Aspergillus niger ( Aspergillus niger ); The biomass matrix includes distiller's grains.
3. The biomass porous carbon according to claim 1, characterized in that, The biomass porous carbon includes at least one of the following characteristics A1 to A4: A1. The pore volume of the macroporous network accounts for 15% to 35% of the total pore volume; the pore volume of the mesoporous channels accounts for 20% to 45% of the total pore volume; and the pore volume of the microporous array accounts for 25% to 55% of the total pore volume. A2. The macropores in the macropore network are tubular in shape, with a smoothness Ra value of less than 200 nm on the inner surface of the tube wall, and there are connecting windows with a diameter of 0.5~2 μm between adjacent macropores; A3. The pore size distribution of the mesoporous channel exhibits a bimodal characteristic, with the first peak located in the 2~10 nm range and the second peak located in the 20~50 nm range. A4. The biomass porous carbon has a BET specific surface area of 500~2000 m² / g and a total pore volume of 0.5~1.5 cm³. 3 / g, with an average pore size of 1.5~8.0 nm.
4. The biomass porous carbon according to claim 1, characterized in that, The total potassium and sodium content in the inherent ash of the biomass matrix is 0.05~2.0 wt%.
5. The biomass porous carbon according to claim 1, characterized in that, The biomass porous carbon contains inherent nitrogen doping derived from biomass protein components and inherent oxygen doping derived from biomass oxygen-containing functional groups, wherein the nitrogen content is 1.0~4.0 at%, and the oxygen content is 5.0~15.0 at%.
6. The biomass porous carbon according to claim 1, characterized in that, The biomass porous carbon includes at least one of the following characteristics B1 to B3: B1. The carbon framework of the biomass porous carbon is a composite structure consisting of a disordered carbon matrix and locally graphitized microregions. In the XRD pattern, the broadened diffraction peaks corresponding to the (002) crystal plane of the disordered carbon matrix are located at 2θ = 24°~25.5°, and the interlayer spacing d 002 The intensity is 0.35~0.37 nm; and there is a weak diffraction peak corresponding to the crystal plane of the local graphitized micro-region (002) at 2θ=26.4°~26.6°, the peak area of the weak diffraction peak accounts for 5%~30% of the total peak area of the crystal plane diffraction; the intensity ratio ID / IG of the D peak to the G peak in the Raman spectrum is 0.8~1.2; B2. The biomass porous carbon has an irregular lamellar morphology with a lamellar thickness of 0.5~5μm, and the lamellar surface is distributed with an array of pores formed by the macroporous network. B3. The silicon content of the biomass porous carbon does not exceed 0.5 wt%.
7. The method for preparing porous biomass carbon according to any one of claims 1 to 6, characterized in that, Includes the following steps: S1. Pretreatment: The biomass matrix is dried to a moisture content of ≤10 wt% and then pulverized to obtain a pretreated biomass matrix; S2. Fermentation of a single mold strain: A single mold is inoculated into the pretreated biomass matrix at an inoculation amount of 5% to 15% of the dry mass of the pretreated biomass matrix. The moisture content of the material is adjusted to 50% to 65%, and solid-state fermentation is carried out at 25 to 40°C for 3 to 7 days until the mycelial coverage reaches more than 60%, and the fermented material is obtained. S3. Cellulase hydrolysis: Add cellulase to the fermentation material at a dosage of 20-60 FPU / g dry basis, and hydrolyze for 12-48 h at pH 4.5-5.5 and 45-55℃ to obtain hydrolyzed material; S4. Pre-carbonization: The enzymatically hydrolyzed material is pre-carbonized at 200~500℃ for 1~3 h under an inert atmosphere to obtain the pre-carbonized product; S5. Acid washing and desiliconization: The pre-carbonized product is washed with dilute acid to remove ash and silicon components, then washed with water until neutral and dried to obtain the acid-washed material. S6. High-temperature carbonization self-activation: The pickled material is carbonized at 700~1000℃ for 1~3 h in an inert atmosphere. The inherent potassium and sodium ash groups in the biomass matrix are self-activated and form pores during the carbonization process. After cooling, porous biomass carbon is obtained.
8. The preparation method according to claim 7, characterized in that, In step S1, the total inherent potassium and sodium content in the biomass matrix is 0.05~2.0 wt%; the total inherent potassium and sodium content in the biomass matrix is tested, and when the total potassium and sodium content of the tested batch is not between 0.05~2.0 wt%, different batches of distiller's grains are blended in a certain proportion to make the potassium and sodium content in the blended raw material between 0.05~2.0 wt%, before proceeding to subsequent steps; and / or, In step S2, the inoculum amount of *Aspergillus niger* is 5%–15% of the dry weight of the pretreated distiller's grains, the solid-state fermentation temperature is 25–40°C, and the solid-state fermentation time is 3–7 days; and / or, In step S3, the amount of cellulase added is 20-60 FPU / g dry basis, the hydrolysis temperature is 45-55℃, and the hydrolysis time is 12-48 h; and / or, The carbonization temperature in step S6 is 700~900℃, and the carbonization time is 1~3 h.
9. A battery electrode material, characterized in that, The active material of the electrode sheet comprises the biomass porous carbon as described in any one of claims 1 to 6 or the biomass porous carbon prepared by the preparation method described in claim 7 or 8.
10. A battery, characterized in that, It includes the electrode sheet as described in claim 9.
Citation Information
Patent Citations
Lignin-based porous carbon material for supercapacitor electrode and preparation method and application thereof
CN119170425A
Biomass-based porous carbon and preparation method thereof, and silicon-carbon negative electrode material and preparation method thereof
CN122166772A