An electrode material, a battery electrode, and an energy storage device.

By introducing thermoelectric negative feedback control materials into the electrode materials and utilizing their positive temperature coefficient resistance characteristics, the current and temperature distribution can be dynamically adjusted, thus solving the problem of local overheating caused by uneven current density in power batteries and improving the cycle life and thermal stability of the batteries.

CN123120735APending Publication Date: 2026-11-17BEIJING CHEHEJIA AUTOMOBILE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611342866.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

During the charging and discharging process, uneven current density distribution in power batteries leads to excessive current and high temperature in some areas, triggering a vicious cycle. Existing external cooling systems cannot solve the problems of current accumulation and uneven heat generation at the microscale.

Method used

By introducing thermoelectric negative feedback control materials into electrode materials and utilizing their positive temperature coefficient resistance characteristics, the current and temperature distribution can be dynamically adjusted through a negative feedback mechanism to achieve adaptive current equalization at the electrode layer and improve temperature uniformity.

Benefits of technology

It effectively suppresses local hot spots and current accumulation, improves battery cycle life and thermal stability, simplifies the cooling system, is suitable for various battery systems and electrodes, and has a wide range of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120735A_ABST
    Figure CN123120735A_ABST
Patent Text Reader

Abstract

This invention discloses an electrode material, a battery electrode, and an energy storage device, belonging to the field of energy storage technology. The electrode material includes a thermoelectric negative feedback control material, which has a positive temperature coefficient resistivity. In this invention, by introducing a thermoelectric negative feedback control material into the electrode material as a thermoelectric negative feedback control unit, adaptive current equalization at the electrode layer is achieved during charging and discharging, thereby dynamically adjusting the current distribution. This negative feedback mechanism improves the uniformity of temperature distribution, avoids current accumulation and uneven heat generation, and simultaneously improves cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of energy storage technology, and more specifically, to an electrode material, a battery electrode, and an energy storage device. Background Technology

[0002] With the rapid development of the new energy vehicle industry, higher requirements have been placed on the cycle performance of power batteries. Currently, a significant reason for the degradation of power battery cycle life is internal non-uniformity. During charging and discharging, the uneven distribution of current density within the electrodes leads to excessively high current and temperature in some areas (hot spots), while other areas experience low current and temperature. This non-uniformity induces a vicious cycle: localized high temperatures enhance electrochemical activity and reduce impedance in those areas, increasing current density, further driving up temperature, exacerbating localized side reactions and material degradation, and ultimately leading to localized electrode material failure. Currently, conventional solutions mostly involve external macroscopic interventions, such as improving the cooling system to enhance external heat dissipation. However, this cannot solve the problems of current accumulation and uneven heat generation at the microscale. Summary of the Invention

[0003] This invention is based on the inventor's discovery and understanding of the following facts and problems: during the charging and discharging process, the uneven distribution of current density inside the electrodes leads to the degradation of the cycle life of the power battery.

[0004] This invention aims to at least partially solve one of the technical problems in related technologies. To this end, embodiments of this invention propose an electrode material, a battery electrode, and an energy storage device. By introducing a thermoelectric negative feedback control material into the electrode material as a thermoelectric negative feedback control unit, adaptive current equalization at the electrode layer level is achieved during charging and discharging, thereby dynamically adjusting the current distribution. This negative feedback mechanism improves the uniformity of temperature distribution, avoids current accumulation and uneven heat generation, and simultaneously improves cycle performance.

[0005] This invention provides an electrode material, including a thermoelectric negative feedback control material, wherein the thermoelectric negative feedback control material has a positive temperature coefficient resistance characteristic.

[0006] The advantages and technical effects of the electrode material in this invention embodiment are as follows: The thermoelectric negative feedback control material is a conductive material with a positive temperature coefficient (PTC) resistance characteristic (PTC material), and the resistance of the PTC material increases with increasing temperature. By introducing a material with a positive temperature coefficient resistance characteristic into the electrode material and the electrode active material layer as a thermoelectric negative feedback control unit, adaptive current equalization at the electrode layer level is achieved during charging and discharging, thereby dynamically adjusting the current distribution. This negative feedback mechanism improves the uniformity of temperature distribution.

[0007] In some embodiments, the thermoelectric negative feedback control material has a positive temperature coefficient resistance characteristic in a temperature range of 25~80°C.

[0008] In some embodiments, the resistivity of the thermoelectric negative feedback control material at 80°C is not less than 20 times the resistivity of the thermoelectric negative feedback control material at 30°C.

[0009] In some embodiments, the resistivity of the thermoelectric negative feedback control material at 50°C is not less than twice the resistivity of the thermoelectric negative feedback control material at 25°C.

[0010] In some embodiments, the thermoelectric negative feedback control material includes at least one of semiconductor materials and polymer PTC materials; And / or, the thermoelectric negative feedback control material is a micron-sized particle; And / or, the thermoelectric negative feedback control material is uniformly distributed in the electrode material; And / or, the thermoelectric negative feedback control material is 0.1% to 0.5% of the mass of the electrode material.

[0011] In some embodiments, the semiconductor material comprises BaTiO3-based ceramics; And / or, the polymeric PTC material comprises a composite material consisting of a polymer matrix and a conductive filler; preferably, the polymeric PTC material comprises at least one of a composite material of epoxy resin and carbon black, and a composite material of polyurethane and carbon black.

[0012] This invention provides a battery electrode, including an active material layer, wherein the active material layer comprises the electrode material described in this invention.

[0013] In this embodiment of the invention, a thermoelectric negative feedback control material with a positive temperature coefficient (PTC) resistance characteristic is introduced into the electrode active material layer as a thermoelectric negative feedback control unit. This enables adaptive current equalization at the electrode layer level during charging and discharging, thereby dynamically adjusting the current distribution, improving the current distribution at the electrode layer level, and further improving heat generation and temperature uniformity during charging. In other words, this negative feedback mechanism improves the uniformity of temperature distribution. A more uniform temperature distribution at the cell electrode layer level helps simplify the overall battery pack cooling system and improves cycle performance.

[0014] In this embodiment of the invention, after introducing PTC material into the electrode material formulation of the positive and negative electrodes, the working mechanism of the thermoelectric negative feedback control unit is as follows: When a local area of ​​the electrode becomes a "hot spot," the temperature is significantly higher than other areas; at this time, the resistance of the PTC material in the "hot spot" area increases significantly; for the local area of ​​the electrode sheet, it is in parallel with other areas, and according to the principle of current shunting, the current will preferentially and dynamically shun to the adjacent low-temperature area with lower impedance; the current density in the "hot spot" area decreases, and the Joule heat generation decreases accordingly (heat generation P=U^2 / R), and the temperature rise trend is suppressed; the whole process forms a negative feedback closed loop of "temperature increase → resistance increase → current decrease → heat generation decrease → temperature rise slowdown → temperature suppression," breaking the original positive feedback mechanism (deteriorating cycle). This invention improves the heat generation process at the microscopic level through electrode material composition optimization, changing the original positive feedback mechanism of the heat generation process to a negative feedback mechanism, thereby improving the temperature rise and cell temperature distribution uniformity during charging, and improving cycle performance.

[0015] In some embodiments, the thermoelectric negative feedback control material is 0.1% to 0.5% of the mass of the active material layer; And / or, the resistivity of the active material layer at 80°C is not less than twice the resistivity of the active material layer at 30°C; And / or, the resistivity of the active material layer at 50°C is not less than 1.2 times the resistivity of the active material layer at 25°C; And / or, the battery electrodes include a positive electrode or a negative electrode; And / or, the thermoelectric negative feedback control material is uniformly distributed in the active material layer.

[0016] This invention provides a method for preparing a battery electrode, comprising: coating a slurry of electrode material onto a current collector, drying it to form an active material layer, and obtaining a battery electrode.

[0017] This invention provides an energy storage device, including the electrode material described in this invention, or the battery electrode described in this invention.

[0018] In this embodiment of the invention, the energy storage device improves the heat generation process at the microscopic level by changing the original positive feedback mechanism of the heat generation process to a negative feedback mechanism, thereby improving the temperature rise and cell temperature distribution uniformity during the charging process, and improving cycle performance.

[0019] In this embodiment of the invention, by suppressing local hot spots and current accumulation, the local accelerated degradation is fundamentally slowed down, resulting in more uniform overall battery degradation and significantly improved cycle life, especially fast-charging life. It also reduces the risk of internal local overheating, improves battery thermal stability, and enhances battery safety. The regulation process is spontaneously completed based on the material's physical properties, with a rapid response and no need for additional algorithms in the battery management system (BMS). The system is simpler and more reliable, achieving adaptive regulation without complex external control. Only the addition of thermoelectric negative feedback regulation materials to the existing manufacturing process is required, resulting in minimal modifications, easy industrialization, and good process compatibility. It is applicable to various battery systems (e.g., lithium-ion batteries, sodium-ion batteries, etc.) and various electrodes (e.g., positive and negative electrodes), with a wide range of applications and strong universality.

[0020] In some embodiments, the energy storage device includes a lithium-ion battery or a sodium-ion battery; And / or, the energy storage device includes a positive electrode and a negative electrode, and the positive electrode and / or negative electrode includes a thermoelectric negative feedback control material. Attached Figure Description

[0021] Figure 1 This is a temperature cloud map of the battery cell during the charging process in Example 1.

[0022] Figure 2 This is a temperature cloud map of the battery cell during the charging process in Example 2.

[0023] Figure 3 This is a temperature cloud map of the battery cell during the charging process in Example 4.

[0024] Figure 4 This is a temperature cloud map of the battery cell during the charging process of Comparative Example 1. Detailed Implementation

[0025] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.

[0026] An electrode material according to an embodiment of the present invention includes a thermoelectric negative feedback control material, wherein the thermoelectric negative feedback control material has a positive temperature coefficient resistance characteristic.

[0027] The electrode material of this invention includes a thermoelectric negative feedback control material with a positive temperature coefficient of resistance, the resistance of which increases with increasing temperature. By introducing a material with a positive temperature coefficient of resistance into the electrode material and the electrode active material layer as a thermoelectric negative feedback control unit, adaptive current equalization at the electrode layer level is achieved during charging and discharging, thereby dynamically adjusting the current distribution and improving the uniformity of temperature distribution through this negative feedback mechanism.

[0028] In some embodiments, the thermoelectric negative feedback control material has a positive temperature coefficient resistance characteristic in a temperature range of 25~80℃ (e.g., 25℃, 30℃, 40℃, 50℃, 55℃, 60℃, 70℃, 80℃). Optionally, the resistivity of the thermoelectric negative feedback control material at 80°C is not less than 20 times the resistivity of the thermoelectric negative feedback control material at 30°C; Optionally, the resistivity of the thermoelectric negative feedback control material at 50°C is not less than twice the resistivity of the thermoelectric negative feedback control material at 25°C.

[0029] In this embodiment of the invention, the thermoelectric negative feedback control material refers to a conductive material with a positive temperature coefficient of resistance, meaning that the resistance of the material increases with increasing temperature. PTC materials with a resistivity at 80°C greater than or equal to 20 times their resistivity at 30°C exhibit a rapid increase in resistivity with increasing temperature. Their resistivity-temperature curve has a sufficiently steep upward slope within the typical operating temperature range of the battery to ensure a significant negative feedback effect. This further facilitates adaptive current equalization at the electrode level during charging and discharging, thereby dynamically adjusting the current distribution and improving the uniformity of temperature distribution through this negative feedback mechanism. When the resistivity at 80°C is less than 20 times that at 30°C—for example, 10 or 5 times the resistivity at 30°C—the resistance ratio is relatively low, the current control amplitude is limited, and the temperature control effect brought about by current adaptation will be significantly reduced.

[0030] In this embodiment of the invention, the resistivity at 50°C is further selected to be no less than twice the resistivity at 25°C, which is beneficial to further improve the uniformity of temperature distribution.

[0031] In some embodiments, the thermoelectric negative feedback control material includes at least one of semiconductor materials and polymer PTC materials; the present invention does not impose any special restrictions on the source of the thermoelectric negative feedback control material, for example, it can be obtained by purchase.

[0032] In some embodiments, the semiconductor material includes BaTiO3-based ceramics, that is, BaTiO3-based ceramics with positive temperature coefficient resistance characteristics; the BaTiO3-based ceramics are available by purchase. Optionally, the BaTiO3-based ceramic includes BaTi x M1 y M2 zO3, x+y+z=1, 1>x>0, 1>y≥0, 1>z≥0; M1 is a donor dopant element, and M2 is an acceptor dopant element; optionally, the (semiconductor) donor dopant element includes at least one of Sr, La, Sb, Y, and Nd; the donor dopant element is 0.1~0.5 at% relative to the Ti element in BaTiO3, i.e., 0.005≥y≥0.001; the acceptor dopant element includes at least one of Mn and Fe; the acceptor dopant element is 0.02~0.1 at% relative to the Ti element in BaTiO3, i.e., 0.001≥z≥0.0002; Optionally, the BaTiO3-based ceramic further includes an oxide; the oxide includes at least one of Si oxide and Ti oxide; the mass of the oxide is 0.5~2 wt% of the mass of the BaTiO3-based ceramic. Optionally, the room temperature (25°C) resistivity of the BaTiO3-based ceramic is 10~100 Ω·cm, with a jump range of 3~6 orders of magnitude (near Tc); the Curie temperature Tc can be adjusted by replacing Ba with Sr (e.g., adding 20 mol% Sr lowers Tc to 80°C). Optionally, the particle size range of the BaTiO3-based ceramic is 2~20 μm, specifically, for example, 2 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm.

[0033] In this embodiment of the invention, doping with BaTiO3-based ceramics improves the resistivity jump amplitude. Oxides form a grain boundary insulating layer. The jump amplitude refers to the change in the intrinsic resistivity of the PTC material near Tc. A jump amplitude that is too low cannot significantly alter the resistance of the electrode region, while a jump amplitude that is too high will affect the local overcurrent capacity of the electrode. The BaTiO3-based ceramics have a particle size range of 2–20 μm, which is beneficial for obtaining the optimal PTC effect.

[0034] In some embodiments, the polymeric PTC material comprises a composite material consisting of a polymer matrix and a conductive filler; Optionally, the polymeric PTC material includes at least one of a composite material of epoxy resin and carbon black, or a composite material of polyurethane and carbon black; the polymeric PTC material can be purchased.

[0035] In some embodiments, the polymeric PTC material comprises a composite material of epoxy resin and carbon black; Optionally, the abrupt change temperature of the epoxy resin and carbon black composite material is 60~80°C, specifically, for example, 60°C, 70°C, 80°C; Optionally, the carbon black includes acetylene black, for example, Denka Black, with a particle size of 35 nm; Optionally, in the composite material of epoxy resin and carbon black, the mass percentage of carbon black is 1-5%, specifically, for example, 1%, 2%, 3%, 4%, 5%. Optionally, the epoxy resin has a molecular weight of 400~700 g / mol, specifically, for example, 400 g / mol, 500 g / mol, 600 g / mol, 700 g / mol; the epoxy resin includes bisphenol A type epoxy resin; the bisphenol A type epoxy resin includes E-51 / DGEBA, and optionally, EEW (epoxy equivalent) ≈ 190 g / mol; Optionally, the raw materials for the epoxy resin and carbon black composite material, by mass parts, include: epoxy resin: 100 parts; Reactive diluent: 15-30 parts, for example, 15 parts, 20 parts, 30 parts; Hardener: 28-37 parts, for example, 28 parts, 30 parts, 35 parts, 37 parts; Carbon black: 2 to 6 parts, for example, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts; Optionally, with or without defoamer: 0.1 to 0.2 parts, for example, 0.1 parts or 0.2 parts; Optionally, with or without thickener: 1 to 2 parts, for example, 1 part, 1.5 parts, 2 parts; Optionally, the reactive diluent includes AGE (C 12 ~C 14 Alkyl glycidyl ether); the curing agent includes Jeffamine D-230 (active hydrogen equivalent ≈ 57.5 g / mol) and / or Jeffamine D-400 (active hydrogen equivalent ≈ 100 g / mol); the defoamer includes BYK-A530; the thickener includes fumed silica; Optionally, the present invention does not specifically limit the preparation method of the epoxy resin and carbon black composite material. Existing preparation methods or directly purchased materials can be used. For example, the preparation method of the epoxy resin and carbon black composite material includes: mixing bisphenol A type epoxy resin and an reactive diluent, then adding carbon black and mixing; then adding a curing agent and curing to obtain the epoxy resin and carbon black composite material; other components (e.g., defoamer and thickener) are added before the curing agent is added. Specifically, for example, the thickener is added at the same time as or after the addition of carbon black. Then add defoamer; in a specific embodiment, the temperature for mixing the bisphenol A epoxy resin and reactive diluent is 60°C, the mixing is carried out under stirring, and the mixture is cooled to room temperature after mixing; the mixture after adding carbon black is ground twice using a high-speed disperser (2000 rpm, 30 min) or a three-roll mill to ensure uniform dispersion of carbon black, and then vacuum degassed (0.08 MPa, 30 min); after adding curing agent, stir (e.g., manually stir for 3 minutes) to avoid introducing air bubbles, and then vacuum degassed again for 10 minutes; the curing conditions are 40°C / 4h → 60°C / 2h → 45°C / 12h (annealing), and then naturally cooled to room temperature; In a specific embodiment, the resistivity of the epoxy resin and carbon black composite material at 80°C is ~200 times that at 30°C, and the resistivity at 50°C is ~30 times that at 25°C. The raw materials for the epoxy resin and carbon black composite material, by mass parts, include: 100 parts of bisphenol A type epoxy resin E-51 (EEW≈190 g / mol); 16 parts of reactive diluent AGE; 28 parts of curing agent Jeffamine D-230; 4 parts of acetylene black (Denka Black, particle size 35 nm); and 1 part of fumed silica.

[0036] In some embodiments, the polymeric PTC material comprises a composite material of polyurethane and carbon black; Optionally, the abrupt change temperature of the polyurethane and carbon black composite material is 60~80°C, specifically, for example, 60°C, 70°C, 80°C; Optionally, in the polyurethane and carbon black composite material, the mass percentage of carbon black is 12-19%, specifically, for example, 12%, 15%, 17%, 18%, or 19%. Optionally, the molecular weight of the polyurethane is 20,000 to 80,000 g / mol, specifically, for example, 20,000 g / mol, 40,000 g / mol, 50,000 g / mol, 60,000 g / mol, or 80,000 g / mol; Optionally, the raw materials for the polyurethane and carbon black composite material, by mass parts, include: Polyols: 100 parts; Isocyanates: 25 to 38 parts (e.g., 25 parts, 30 parts, 35 parts, 38 parts); Chain extender: 5 to 8 parts (e.g., 5 parts, 6 parts, 7 parts, 8 parts); Carbon black: 12 to 40 parts (e.g., 12 parts, 14 parts, 16 parts, 20 parts, 30 parts, 40 parts). Catalyst: 0.02~0.05 parts (e.g., 0.02 parts, 0.03 parts, 0.04 parts, 0.05 parts); Optionally, the polyol comprises at least one of polycaprolactone diol or polyether polyol; the polycaprolactone diol comprises PCL-2000 (hydroxyl value 56 mg KOH / g, OH equivalent ≈ 1000 g / mol); the polyether polyol comprises PPG-2000 (hydroxyl value 56 mg KOH / g, Mn ≈ 2000); the isocyanate comprises MDI (4,4'-diphenylmethane diisocyanate); the chain extender comprises 1,4-butanediol; the carbon black comprises conductive carbon black; the conductive carbon black comprises Ketjen Black EC-300J or acetylene black; and the catalyst comprises dibutyltin dilaurate T-12. Optionally, the present invention does not specifically limit the preparation method of the polyurethane and carbon black composite material. Existing preparation methods or direct purchase can be used. For example, the preparation method of the polyurethane and carbon black composite material includes: performing a prepolymerization reaction of polyol and isocyanate to obtain a prepolymer; then adding carbon black for mixing; and then adding a chain extender and a catalyst for curing to obtain the polyurethane and carbon black composite material. In a specific embodiment, the polyol is dried (e.g., vacuum dried at 110°C for 1 hour) and the carbon black is dried (e.g., oven dried at 150°C for 2 hours) before preparation. The prepolymerization reaction is carried out at 80°C for 2 hours under nitrogen protection. A small amount of the prepolymer is taken to determine the NCO content (e.g., by di-n-butylamine titration) to ensure that the NCO% is close to the theoretical value. The prepolymer is cooled to 60°C and then carbon black is added. The carbon black is first ultrasonically dispersed in anhydrous THF for 5 minutes and then added to the prepolymer. The mixture is stirred at high speed (1000~2000 rpm, 15~30 minutes) and THF is removed under vacuum (rotary evaporator, 60°C, 0.08 MPa, 30 minutes). After adding the chain extender and catalyst, the mixture is stirred rapidly for 2 minutes. The curing includes curing at 80°C for 2 hours, followed by annealing in an oven at 50~60°C for 12 hours. Finally, the mixture is allowed to cool naturally for 24 hours.

[0037] In some embodiments, the thermoelectric negative feedback control material is micron-sized particles; optionally, the particle size of the thermoelectric negative feedback control material can be 5~50 μm, specifically, for example, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm. In these embodiments of the invention, using micron-sized particles for the thermoelectric negative feedback control material facilitates its uniform dispersion in the electrode slurry, which is beneficial for obtaining the optimal PTC effect.

[0038] In some embodiments, the thermoelectric negative feedback control material is uniformly distributed in the electrode material. In these embodiments, the uniform dispersion of the thermoelectric negative feedback control material in the electrode material is beneficial for obtaining the optimal PTC effect.

[0039] In some embodiments, the thermoelectric negative feedback control material is 0.1% to 0.5% of the mass of the electrode material, specifically, for example, 0.1%, 0.2%, 0.3%, 0.4%, or 0.5%. In this embodiment, using 0.1% to 0.5% of the mass of the thermoelectric negative feedback control material is beneficial for further dynamically adjusting the current distribution and improving the uniformity of the temperature distribution. The amount of PTC added is low to avoid affecting the overall conductivity and energy density of the electrode. However, if the amount of PTC added is too low, the control of local impedance is limited, thus affecting the current and temperature control effects.

[0040] In some embodiments, the electrode material includes an active substance, a conductive agent, a binder, and a thermoelectric negative feedback control material; optionally, it also includes a dispersant. The present invention does not impose any special limitation on the type of active material, and can be applied to a variety of active materials. For example, in a specific embodiment, for the negative electrode, the negative electrode active material may include at least one of graphite, silicon oxide, and silicon carbon. The present invention does not impose any special limitation on the content of the active material in the electrode material, and can adopt the usual content range of active materials in battery electrode materials. This invention does not impose any special restrictions on the types of conductive agents, binders, and dispersants. In specific embodiments, the binder may include at least one of sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), and polyacrylic acid (PAA); the dispersant may include at least one of sodium carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyethylene glycol (PEG), Triton X-100, and SDS; this invention does not impose any special restrictions on the content of conductive agents, binders, and dispersants in the electrode material, and the usual content range of conductive agents, binders, and dispersants in battery electrode materials can be used.

[0041] A battery electrode according to an embodiment of the present invention includes an active material layer, wherein the active material layer comprises the electrode material described in the embodiment of the present invention.

[0042] In this embodiment of the invention, the electrode material refers to the material of the active material layer, which includes the electrode material. The electrode material of this invention includes an active material, a conductive agent, a binder, and a thermoelectric negative feedback control material. The battery electrode achieves adaptive current equalization within the internal current based on thermoelectric negative feedback. By introducing a thermoelectric negative feedback control material with a positive temperature coefficient (PTC) resistance characteristic into the electrode active material layer as a thermoelectric negative feedback control unit, adaptive current equalization at the electrode layer level is achieved during charging and discharging, thereby dynamically adjusting the current distribution, improving the current distribution at the electrode layer level, and further improving heat generation and temperature uniformity during charging. In other words, this negative feedback mechanism improves the uniformity of temperature distribution. A more uniform temperature distribution at the cell electrode layer level helps simplify the overall cooling system and improves cycle performance.

[0043] In this embodiment of the invention, after introducing PTC material into the electrode material formulation of the positive and negative electrodes, the working mechanism of the thermoelectric negative feedback control unit is as follows: When a local area of ​​the electrode becomes a "hot spot," the temperature is significantly higher than other areas; at this time, the resistance of the PTC material in the "hot spot" area increases significantly; for the local area of ​​the electrode sheet, it is in parallel with other areas, and according to the principle of current shunting, the current will preferentially and dynamically shun to the adjacent low-temperature area with lower impedance; the current density in the "hot spot" area decreases, and the Joule heat generation decreases accordingly (heat generation P=U^2 / R), and the temperature rise trend is suppressed; the whole process forms a negative feedback closed loop of "temperature increase → resistance increase → current decrease → heat generation decrease → temperature rise slowdown → temperature suppression," breaking the original positive feedback mechanism (deteriorating cycle). This invention improves the heat generation process at the microscopic level through electrode material composition optimization, changing the original positive feedback mechanism of the heat generation process to a negative feedback mechanism, thereby improving the temperature rise and cell temperature distribution uniformity during charging, and improving cycle performance.

[0044] In some embodiments, the thermoelectric negative feedback control material is 0.1% to 0.5% of the mass of the active material layer, specifically, for example, 0.1%, 0.2%, 0.3%, 0.4%, or 0.5%.

[0045] In this embodiment of the invention, the thermoelectric negative feedback control material is 0.1% to 0.5% of the mass of the active material layer, which is beneficial for further dynamic adjustment of the current distribution and improvement of the uniformity of the temperature distribution. The amount of PTC added is low to avoid affecting the overall conductivity and energy density of the electrode. However, if the amount of PTC added is too low, the control of local impedance is limited, thus affecting the current and temperature control effect.

[0046] In some embodiments, the resistivity of the active material layer at 80°C is not less than twice the resistivity of the active material layer at 30°C; alternatively, the resistivity of the active material layer at 50°C is not less than 1.2 times the resistivity of the active material layer at 25°C.

[0047] In this embodiment of the invention, the resistivity of the active material layer at 80°C is greater than or equal to twice the resistivity at 30°C. The resistivity increases sharply with increasing temperature, and its resistivity-temperature curve has a sufficiently steep upward slope within the typical operating temperature range of the battery. This ensures a significant negative feedback effect and further facilitates adaptive current sharing at the electrode layer during charging and discharging, thereby dynamically adjusting the current distribution and improving the uniformity of temperature distribution through this negative feedback mechanism. When the resistivity at 80°C is less than twice the resistivity at 30°C, the resistance ratio is relatively low, the current regulation range is limited, and the temperature regulation effect brought about by current adaptation will be greatly reduced. Furthermore, a resistivity at 50°C not less than 1.2 times the resistivity at 25°C can be selected, which is beneficial for further improving the uniformity of temperature distribution.

[0048] In some embodiments, the thermoelectric negative feedback control material is uniformly distributed in the active material layer. In these embodiments, the uniform distribution of the thermoelectric negative feedback control material in the active material layer facilitates further dynamic adjustment of the current distribution and improves the uniformity of the temperature distribution.

[0049] In some embodiments, the battery electrode includes a positive electrode or a negative electrode. In these embodiments, the thermoelectric negative feedback control material is suitable for both positive and negative electrodes, exhibiting wide application and strong versatility.

[0050] In some embodiments, the battery electrode includes an active material layer and a current collector, the active material layer being disposed on both sides of the current collector along its thickness direction.

[0051] A method for preparing a battery electrode according to an embodiment of the present invention includes: coating a slurry of electrode material onto a current collector, drying it to form an active material layer, and obtaining a battery electrode.

[0052] In some embodiments, an active material, a conductive agent, a binder, a thermoelectric negative feedback control material, and a solvent are mixed to obtain a slurry of electrode material. The slurry of electrode material is then coated onto a current collector and dried to form an active material layer, thereby obtaining a battery electrode. Optionally, the mixing process may also include other optional components (e.g., a dispersant). The present invention does not impose any particular limitation on the solvent or its amount; any solvent and its amount range applicable to the preparation of battery electrodes may be used. For example, the solvent may include NMP.

[0053] In some embodiments, the coating includes applying a slurry of the electrode material to the surfaces of both sides of the current collector along its thickness direction.

[0054] In some embodiments, the present invention does not impose special restrictions on the drying parameters, and drying can be achieved as long as it is dry; in a specific embodiment, for example, vacuum drying is performed at 120°C.

[0055] An energy storage device according to an embodiment of the present invention includes the electrode material described in the embodiment of the present invention, or the battery electrode described in the embodiment of the present invention.

[0056] In this embodiment of the invention, the energy storage device improves the heat generation process at the microscopic level by changing the original positive feedback mechanism of the heat generation process to a negative feedback mechanism, thereby improving the temperature rise and cell temperature distribution uniformity during the charging process, and improving cycle performance.

[0057] In this embodiment of the invention, by suppressing local hot spots and current accumulation, the local accelerated degradation is fundamentally slowed down, resulting in more uniform overall battery degradation and significantly improved cycle life, especially fast-charging life. It also reduces the risk of internal local overheating, improves battery thermal stability, and enhances battery safety. The regulation process is spontaneously completed based on the material's physical properties, with a rapid response and no need for additional algorithms in the battery management system (BMS). The system is simpler and more reliable, achieving adaptive regulation without complex external control. Only the addition of thermoelectric negative feedback regulation materials to the existing manufacturing process is required, resulting in minimal modifications, easy industrialization, and good process compatibility. It is applicable to various battery systems (e.g., lithium-ion batteries, sodium-ion batteries, etc.) and various electrodes (e.g., positive and negative electrodes), with a wide range of applications and strong universality.

[0058] In some embodiments, the energy storage device includes a lithium-ion battery or a sodium-ion battery.

[0059] In some embodiments, the energy storage device includes a positive electrode and a negative electrode, wherein the positive electrode and / or the negative electrode includes the thermoelectric negative feedback control material described in the embodiments of the present invention.

[0060] The present invention will now be described with reference to specific embodiments. It should be noted that these embodiments are merely descriptive and do not limit the present invention in any way.

[0061] Example 1 A method for preparing a negative electrode sheet with PTC material includes the following steps: The components were mixed in the following mass percentages: graphite: silicon carbide: conductive carbon black: binder (PAA): dispersant (CMC): PTC material (BaTiO3-based ceramic) = 91.2%: 4.8%: 1.5%: 2.2%: 0.2%: 0.1%, and then mixed with a solvent to obtain the negative electrode slurry. The BaTiO3-based ceramic (particle size 2~20 μm) includes BaTiO3... 0.9975 Sb 0.002 Mn0.0005 O3, specifically Sb at 0.2 at% of Ti in BaTiO3 and Mn at 0.05 at% of Ti in BaTiO3, has a resistivity at 80℃ that is 44.5 times that at 30℃, and at 50℃ that is 5 times that at 25℃. After the negative electrode slurry stabilizes, it is directly coated onto a foil and vacuum dried at 120℃ to obtain the negative electrode sheet. The resistivity of the active material layer of the negative electrode sheet at 80℃ is 2.2 times that at 30℃; and at 50℃ it is 1.25 times that at 25℃.

[0062] The positive electrode uses NCM622 material and is assembled with the above-mentioned negative electrode sheet to form an NCM622 positive electrode / graphite lithium-ion battery.

[0063] Performance testing: The battery underwent overcharging: 10-20% SOC charging rate was 6C, 20-50% SOC charging rate was 3C, 50-70% SOC charging rate was 2C, and 70-80% SOC charging rate was 1C. Temperature cloud maps of the battery cells at 60% SOC were measured during the charging process. The results are as follows: Figure 1 As shown. Figure 1 This is a temperature cloud map of the battery cell during the charging process in Example 1. Figure 1 It can be seen that with the introduction of PTC material, the temperature uniformity increases and the temperature difference between different regions decreases significantly, thus improving the temperature uniformity.

[0064] In addition, supercharging cycles were performed: the supercharging strategy described above was used for charging, followed by 0.5C discharge, and after resting for 1 hour, the next round of supercharging was carried out. The battery cycle decay to 80% SOH in Example 1 corresponds to a cycle count of no less than 2500 cycles, and the cycle performance was improved.

[0065] Example 2 The preparation method is the same as that in Example 1, except that the components are mixed in the following mass percentages: graphite: silicon carbide: conductive carbon black: binder: dispersant: PTC material (BaTiO3-based ceramic) = 91.1%: 4.7%: 1.5%: 2.2%: 0.2%: 0.3%.

[0066] Figure 2 This is a cell temperature cloud map during the charging process in Example 2. (From...) Figure 2 It can be seen that with the introduction of PTC material, the temperature uniformity increases and the temperature difference between different regions decreases significantly, thus improving the temperature uniformity.

[0067] Example 3 The preparation method is the same as that in Example 1, except that the components are mixed in the following mass percentages: graphite: silicon carbide: conductive carbon black: binder: dispersant: PTC material (BaTiO3-based ceramic) = 91.0%: 4.6%: 1.5%: 2.2%: 0.2%: 0.5%.

[0068] Tests revealed that with the introduction of PTC material, the average temperature increased and the temperature difference between different regions decreased significantly, thus improving temperature uniformity.

[0069] Example 4 The preparation method is the same as in Example 1, except that the BaTiO3-based ceramic is replaced with a composite material of epoxy resin and carbon black. The resistivity of the epoxy resin and carbon black composite material at 80°C is ~200 times that at 30°C, and at 50°C it is ~30 times that at 25°C. The resistivity of the active material layer of the negative electrode at 80°C is 2.5 times that at 30°C; the resistivity of the active material layer at 50°C is 1.2 times that at 25°C.

[0070] Figure 3 This is a temperature cloud map of the battery cell during the charging process in Example 4. (From...) Figure 3 It can be seen that with the introduction of PTC material, the temperature uniformity increases and the temperature difference between different regions decreases, thus improving the temperature uniformity.

[0071] Example 5 The preparation method is the same as in Example 1, except that the PTC material in Example 1 is replaced with BaTiO3-based ceramic whose resistivity at 80°C is 20 times that at 30°C.

[0072] Tests revealed that with the introduction of PTC material, the average temperature increased and the temperature difference between different regions decreased, thus improving temperature uniformity.

[0073] Comparative Example 1 The preparation method is the same as in Example 1, except that PTC material is not added, and the relative proportions of the other components remain unchanged.

[0074] Figure 4 This is a temperature cloud map of the battery cell during the charging process of Comparative Example 1. From... Figure 4 It can be seen that the temperature uniformity is poor in the X direction (left and right directions in the figure) of the large surface of the cell.

[0075] Furthermore, the battery in Comparative Example 1, when cycle-degraded to 80% SOH, corresponds to approximately 2000 cycles, indicating relatively poor cycle performance.

[0076] Table 1 Electrochemical performance Group Number of cycles @ 80% SOH Comparative Example 1 2000 Example 1 2500 Example 2 2600 Example 3 2800 Example 4 2200 Comparative Example 2 The preparation method is the same as that in Example 1, except that the ratio of graphite:silicon carbide:conductive carbon black:binder:dispersant:PTC material is 90.8%:4.5%:1.5%:2.2%:0.2%:0.8%.

[0077] In Comparative Example 2, the content of thermoelectric negative feedback control material in the active material layer was too high, which affected the overall conductivity and energy density of the electrode.

[0078] In this invention, the terms "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0079] Although the above embodiments have been shown and described, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Any changes, modifications, substitutions and variations made to the above embodiments by those skilled in the art are within the protection scope of the present invention.

Claims

1. An electrode material, characterized in that, It includes thermoelectric negative feedback control materials, which have positive temperature coefficient resistance characteristics.

2. The electrode material according to claim 1, characterized in that, The thermoelectric negative feedback control material has a positive temperature coefficient resistance characteristic in the temperature range of 25~80℃.

3. The electrode material according to claim 2, characterized in that, The resistivity of the thermoelectric negative feedback control material at 80°C is not less than 20 times the resistivity of the thermoelectric negative feedback control material at 30°C. And / or, the resistivity of the thermoelectric negative feedback control material at 50°C is not less than twice the resistivity of the thermoelectric negative feedback control material at 25°C.

4. The electrode material according to any one of claims 1 to 3, characterized in that, The thermoelectric negative feedback control material includes at least one of semiconductor materials and polymer PTC materials; And / or, the thermoelectric negative feedback control material is a micron-sized particle; And / or, the thermoelectric negative feedback control material is uniformly distributed in the electrode material; And / or, the thermoelectric negative feedback control material is 0.1% to 0.5% of the mass of the electrode material.

5. The electrode material according to claim 4, characterized in that, The semiconductor material includes BaTiO3-based ceramics; And / or, the polymeric PTC material comprises a composite material consisting of a polymer matrix and a conductive filler; preferably, the polymeric PTC material comprises at least one of a composite material of epoxy resin and carbon black, and a composite material of polyurethane and carbon black.

6. A battery electrode, characterized in that, It includes an active material layer, wherein the active material layer comprises the electrode material according to any one of claims 1 to 5.

7. The battery electrode according to claim 6, characterized in that, The thermoelectric negative feedback control material constitutes 0.1% to 0.5% of the mass of the active material layer; And / or, the resistivity of the active material layer at 80°C is not less than twice the resistivity of the active material layer at 30°C; And / or, the resistivity of the active material layer at 50°C is not less than 1.2 times the resistivity of the active material layer at 25°C; And / or, the battery electrodes include a positive electrode or a negative electrode; And / or, the thermoelectric negative feedback control material is uniformly distributed in the active material layer.

8. A method for preparing a battery electrode according to claim 6 or 7, characterized in that, include: The electrode material slurry is coated onto the current collector and dried to form an active material layer, thus obtaining the battery electrode.

9. An energy storage device, characterized in that, It includes the electrode material according to any one of claims 1 to 5, or the battery electrode according to claim 6 or 7.

10. The energy storage device according to claim 9, characterized in that, The energy storage device includes a lithium-ion battery or a sodium-ion battery. And / or, the energy storage device includes a positive electrode and a negative electrode, and the positive electrode and / or negative electrode includes a thermoelectric negative feedback control material.