Carrier for Lithium Metal Anode and its Manufacturing Method

By introducing a porous structure with a lithium affinity gradient into the lithium battery anode material, the problems of lithium dendrite growth and volume expansion were solved, and internal electrodeposition of lithium was achieved, thereby improving the stability and energy density of the battery.

CN123120739APending Publication Date: 2026-11-17HYUNDAI MOTOR CO LTD +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610249902.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-03-03
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium battery anode materials suffer from lithium dendrite growth, volume expansion, and safety issues. Conventional porous structures, when electrodeposited on surfaces with low lithium-ion diffusion resistance, fail to suppress dendrite formation, and excessive thickness and weight negatively impact energy density.

Method used

By introducing lithium-affinity silver at the bottom of the conductive metal nanoparticle layer to form a lithium affinity gradient, an electrochemical displacement reaction is used to introduce a lithium affinity gradient into the porous structure, promoting lithium electrodeposition from the bottom of the structure, inhibiting dendrite growth, and reducing volume expansion.

Benefits of technology

It achieves internal lithium electrodeposition, improves battery stability and cycle life, maintains high capacity per unit weight and volume, and is suitable for large-area electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120739A_ABST
    Figure CN123120739A_ABST
Patent Text Reader

Abstract

This invention relates to a carrier for lithium metal anodes and a method for manufacturing the same. A carrier for a lithium metal anode includes: a separator; a layer on the separator comprising conductive metal nanoparticles; and a lithium affinity layer on the layer comprising the conductive metal nanoparticles, wherein the layer comprising the conductive metal nanoparticles further includes pores.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-references to related applications This application claims priority and benefit to Korean Patent Application No. 10-2025-0062293, filed with the Korean Intellectual Property Office on May 14, 2025, the entire contents of which are incorporated herein by reference. Technical Field

[0002] This invention relates to a carrier for lithium metal anodes and a method for manufacturing the same. Background Technology

[0003] Climate change, caused by environmental pollution and global warming, is triggering environmental disasters and threatening lives. Therefore, alternatives to internal combustion engines that can perform environmentally friendly energy storage / transmission processes are being researched. Among these, rechargeable lithium batteries (which emit no carbon during storage / transmission and have high energy and output densities) are attracting attention not only as a power source for small electronic devices but also as a power source for environmentally friendly electric vehicles.

[0004] Lithium metal, which has a high theoretical capacity (3862 mAh g⁻¹), is a next-generation anode material for rechargeable lithium batteries. -1 2046 mA h cm -3 ) and low standard redox potential (-3.03 V) SHE(标准氢电极) It can replace conventional graphite anodes and significantly improve the energy density and output density of batteries. However, there are safety and stability issues, such as decreased cycle life due to lithium dendrite deposition during charging / discharging, and fires and explosions due to battery short circuits.

[0005] Therefore, a method has been proposed to suppress dendrite formation by using structurally porous structures with large electrochemically active surface areas to reduce the effective current density. However, in actual lithium electrodeposition processes, lithium is not electrodeposited inside the structure due to the diffusion resistance of lithium ions, but rather on the outside of the structure where the lithium ion diffusion resistance is lower. To improve this phenomenon, a method has been developed to coat structures such as copper (Cu) foam or carbon paper with lithium-affinity materials. In this case, lithium can be induced to undergo internal electrodeposition, but this method has the following problems: it is not suitable for large-area electrodes, and the high thickness and weight significantly reduce the capacity per unit weight / capacity per unit volume, making it unsuitable for manufacturing batteries with commercially desirable energy and output densities. Summary of the Invention

[0006] To maintain a high capacity per unit weight / volume ratio, a porous structure with a thin thickness but high porosity and low weight should be manufactured. Furthermore, it should be achieved in a simple manner suitable for manufacturing large-area electrodes. In one embodiment, a carrier for a lithium metal anode and a method for manufacturing the same are provided.

[0007] The technical problem solved by one or more embodiments of the present invention is that by introducing lithium-affinity silver (a conductive metal element) at the bottom of a layer containing conductive metal nanoparticles, such as a copper structure, a lithium affinity gradient is formed, thereby inducing lithium to be electrodeposited from the bottom of the structure, thereby suppressing the growth of lithium dendrites and reducing volume expansion during charging / discharging, and thus improving the stability of the battery.

[0008] A lithium metal anode support with a lithium affinity gradient according to an embodiment may include: a separator; a layer on the separator and comprising conductive metal nanoparticles; and a lithium affinity layer on the layer comprising conductive metal nanoparticles, wherein the layer comprising conductive metal nanoparticles further comprises pores.

[0009] A method for manufacturing a support for a lithium metal anode with a lithium affinity gradient, according to another embodiment, may include: adding a mixture of a conductive metal element, conductive carbon fibers, and a binder to a solvent; adding a pore-forming agent to the solvent to which the mixture was added to prepare a slurry; casting the slurry onto a separator; drying the slurry cast on the separator; etching the dried slurry to obtain a support for a lithium metal anode in a first state (e.g., a state in which the support does not have a lithium affinity gradient); and reacting the support in the first state with a solution containing a lithium ion affinity element.

[0010] This invention relates to a high-performance lithium metal anode carrier with a lithium affinity gradient and a method for manufacturing the same. According to an embodiment, the carrier for the lithium metal anode can be a copper (conductive metal element) structure with a lithium affinity gradient, and during plating, lithium plating can occur from the bottom of this structure, thereby reducing volume expansion during charging / discharging and simultaneously improving the cycle life and capacity of the battery.

[0011] Specifically, the lithium metal carrier according to embodiments of the present invention can have a structure in which a lithium-affinity material, such as silver, is readily introduced into the structure via an electrochemical substitution reaction based on a reduction potential difference to form a lithium affinity gradient, and can be applied using a float coating technique not reported in other patents or articles. This method can utilize the hydrophobicity of the separator and amorphous carbon to modify only the surface of the carbon layer with a conductive metal element such as silver (Ag), and this portion can serve as the bottom of the lithium metal anode during battery manufacturing. Therefore, unlike lithium electrodeposition on the surface of conventional conductive porous structures, lithium-affinity silver can react with lithium first, allowing lithium to be electrodeposited from the bottom. Furthermore, this technique has the advantage of being able to coat a large area of ​​conductive metal elements such as Ag in a short time. By using the above structure in the lithium metal anode, internal electrodeposition of lithium can be achieved, thereby suppressing the growth of lithium dendrites during charging / discharging and reducing the volume expansion of lithium metal. Attached Figure Description

[0012] Figure 1 To illustrate a method for manufacturing a carrier according to Comparative Example 2 and Example 1, wherein, Figure 1 The upper portion (up to the step of removing NaCl by etching the etching material in water) is a schematic diagram of a method for manufacturing a carrier for a lithium metal anode without a lithium affinity gradient, while Figure 1 The lower part (up to the step of electrochemical displacement reaction after etching) is a schematic diagram of a method for manufacturing a carrier for a lithium metal anode with a lithium affinity gradient.

[0013] Figure 2 Photograph of a carrier for a lithium metal anode without a lithium affinity gradient according to Comparative Example 2.

[0014] Figure 3 Photograph of a carrier with a lithium affinity gradient for a lithium metal anode according to Example 1.

[0015] Figure 4 A graph showing the proportion of copper (Cu) replaced by silver (Ag) as the silver nitrate coating time increases, according to one embodiment.

[0016] Figure 5 This is half-cell data used to confirm the optimal value of Ag content according to one implementation scheme.

[0017] Figure 6 The images show cross-sectional scanning electron microscope (SEM) images and energy-dispersive X-ray spectroscopy (EDS) analysis data based on the silver nitrate coating time, according to one embodiment.

[0018] Figure 7Data are shown according to one embodiment, using a two-terminal DC resistance measurement method based on the proportion of conductive material (graphite nanofibers (GNF)).

[0019] Figure 8 Electrochemical evaluation data of a half-cell based on the proportion of conductive material (GNF) according to one embodiment are shown.

[0020] Figure 9 A cross-sectional image of the carrier after lithium electrode deposition is shown according to Comparative Example 1.

[0021] Figure 10 A cross-sectional image of the carrier after lithium electrode deposition is shown according to Comparative Example 2.

[0022] Figure 11 A cross-sectional image of the carrier after lithium electrode deposition, according to Example 1, is shown.

[0023] Figure 12 The graph shows the differences in nucleation overvoltage during lithium deposition on the carrier according to Comparative Example 1, Comparative Example 2, and Example 1.

[0024] Figure 13 Cycle life evaluation data of half-cells including carriers according to Comparative Example 1, Comparative Example 2 and Example 1 are shown.

[0025] Figure 14A and Figure 14B The symmetric battery cycle life and output evaluation data are shown, including the carriers according to Comparative Example 1, Comparative Example 2 and Example 1.

[0026] Figure 15A and Figure 15B The full battery cycle life and output evaluation data include the carriers according to Comparative Example 1, Comparative Example 2 and Example 1. Detailed Implementation

[0027] The specific terminology used herein is for the purpose of describing embodiments only and is not intended to limit the invention. The singular forms used herein should also be considered to include the plural forms, unless the wording expressly indicates the opposite. The terms “comprising” or “including” as used herein mean embodying a particular feature, region, integer, step, operation, element, and / or component, and do not exclude other particular features, regions, integers, steps, operations, elements, and / or components.

[0028] Unless otherwise defined, all terms used herein (including technical and scientific terms) shall have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. Unless otherwise defined, commonly used predefined terms shall be further interpreted as having a meaning consistent with relevant technical literature and this invention, and shall not be construed as having an ideal or highly formal meaning.

[0029] The terms "first," "second," and "third" are used to describe various technologies, components, regions, layers, and / or portions, but are not limited thereto. These terms are used only to distinguish any part, component, region, layer, or portion from other parts, components, regions, layers, or portions. Therefore, a first part, component, region, layer, or portion described below may be referred to as a second part, component, region, layer, or portion within the scope of this invention without departing from the scope of this invention.

[0030] In addition, unless otherwise specified, % refers to weight%, and weight-based units are omitted unless otherwise specified.

[0031] As used herein, the term "combination thereof" as described in Markush format means one or more mixtures or combinations of components selected from those described in Markush format, and means including at least one selected from said components. In this invention, each of the phrases such as "A or B," "at least one of A and B," "at least one of A or B," "A, B or C," "at least one of A, B and C," "at least one of A, B or C," and "at least one of A, B or C or a combination thereof" may include any one or all possible combinations of a commonly listed item in the respective phrase.

[0032] The embodiments are described in detail below. However, these embodiments are examples, and the invention is not limited thereto.

[0033] Carrier for lithium metal anodes In recent years, with growing concerns about fossil fuel shortages and environmental pollution, the demand for environmentally friendly energy storage / conversion devices has been increasing. Among them, rechargeable lithium batteries, due to their high power density, high energy density, long cycle life, and environmental friendliness, are used as core components in environmentally friendly electric vehicles and small electronic devices, and therefore have the potential to replace conventional internal combustion engines.

[0034] Lithium metal has a high capacity (3862 mAh·g) -1 2046mAh·cm -3With its low reduction potential, lithium dendrites are considered suitable anode materials for next-generation rechargeable lithium batteries, and can generate high energy and electrical power. However, due to the formation of lithium dendrites during charging / discharging, problems such as battery short circuits, dead lithium formation, and volume expansion exist.

[0035] To address these issues, a solution has been proposed using conductive porous structures with high electrochemically active surface areas to reduce local current density and thus suppress dendrite formation. However, when using conductive porous structures, dendrite formation is not suppressed because most lithium is deposited on the surface of the structure with short lithium-ion diffusion distances. As a method to improve such lithium metal anode supports, it is necessary to fabricate porous structures with lithium affinity gradients. However, conventional supports with lithium affinity gradients (where the lithium affinity gradient is formed by stacking multiple layers containing and not containing lithium affinity materials after introducing lithium affinity materials into the structure) suffer from complex processes and low cost-effectiveness. Furthermore, conventional porous structures in foam form are very thick, leading to reduced energy density and making them unsuitable for commercial use. Therefore, to address this problem, embodiments of the present invention provide a structure with an appropriate thickness that allows for internal lithium electrodeposition by introducing a lithium affinity gradient into the structure rather than forming multiple layers.

[0036] The embodiments of the present invention achieve the following technical tasks: lithium affinity gradients can be easily introduced into porous structures through electrochemical substitution reactions based on reduction potential differences without stacking multiple layers; the slurry casting method ensures that the structure has an appropriate thickness to induce internal electrodeposition of lithium, thereby reducing volume expansion during repeated charging / discharging processes, thus ensuring battery stability and improving performance.

[0037] Conventional research on lithium metal anode supports, both domestically and internationally, has focused on fabricating conductive porous structures. These structures are designed to allow lithium-ion batteries to deposit into their pores, thereby mitigating volume expansion during charging / discharging. Furthermore, the structure possesses a large electrochemically active surface area, which reduces local current density and thus inhibits dendrite growth.

[0038] However, in conventional conductive porous structures studied to date, most lithium is deposited on the surface of the structure due to the short diffusion distance of lithium ions. This renders the pores of the structure unusable during charging / discharging, resulting in volume expansion and an increased risk of battery short circuits. Therefore, there is a growing demand for novel structures capable of internal lithium electrodeposition.

[0039] The lithium metal carrier according to an embodiment of the present invention has a conductive porous structure, but it differs significantly from conventional conductive porous structures in that lithium is not electrodeposited on the surface of the structure but is electrodeposited from the interior of the structure, and the structure is not too thick to minimize or reduce the energy density loss of the battery using the structure.

[0040] A lithium metal anode support with a lithium affinity gradient according to an embodiment includes: a separator; a layer on the separator comprising conductive metal nanoparticles; and a lithium affinity layer on the layer comprising the conductive metal nanoparticles. The layer comprising the conductive metal nanoparticles further includes pores.

[0041] For example, since the substrate used as a separator serves as a simple coating substrate, there are no particular restrictions, as long as it is used as a separator for general rechargeable lithium batteries. For example, porous polymer membranes (such as polyethylene (PE) or polypropylene (PP)), nonwoven membranes composed of oriented or random fibers, inorganic composite membranes made by complexing inorganic nanoparticles with polymers, ceramic separators made of ceramic materials (such as alumina (Al2O3) or lithium aluminum titanium phosphate (LATP)), glass fiber separators formed by extruding fine glass fibers to form a porous structure, nonwoven separators formed by entanglement of fibers to form a porous structure, PP / PE / PP three-layer composite membranes, fluorinated separators, etc.

[0042] For example, the porosity of a support for a lithium metal anode with a lithium affinity gradient can range from 60% to 97%, such as 60% to 95%, 70% to 95%, 70% to 90%, or 75% to 85%. The support for a lithium metal anode according to the embodiment has a very high porosity within the above range, making it easy to achieve a lithium affinity gradient suitable for large-area electrodes, preventing lithium deposition on the upper portion of the support, and inducing internal lithium electrodeposition. A pore-forming agent can be used to form pores. As a pore-forming agent, sodium chloride (NaCl), sucrose, or combinations thereof that are harmless to humans can be used. Alternatively, silica, polymethyl methacrylate (PMMA), styrene, iron oxide (Fe2O3), nickel(II) oxide (NiO), aluminum oxide (Al2O3), or combinations thereof can also be used. The porosity of a lithium metal anode support with a lithium affinity gradient can be controlled by the volume ratio of conductive metal nanoparticles to an etchable pore-forming agent, and the pore size of the lithium metal anode support with a lithium affinity gradient can be controlled by the size of the pore-forming agent (e.g., NaCl). In other words, according to the embodiments, porosity and pore size can be easily controlled, thereby enabling the fabrication of lithium metal batteries with various specifications.

[0043] For example, the lithium affinity layer may also contain lithium ion affinity elements.

[0044] In other words, the lithium affinity gradient according to the embodiment can be achieved using a lithium affinity layer, and the lithium affinity gradient can be a gradient in which the lithium concentration gradually decreases along the direction of the lithium affinity layer, the layer containing conductive metal nanoparticles, and the separator. In the embodiment, since lithium affinity is provided to some of the conductive nanoparticles by electroless plating after coating the conductive nanoparticles (the part where electroless plating occurs plays the role of lithium affinity), the coating floats on the solution where electroless plating occurs and only partially reacts, so that a lithium affinity gradient is formed by electroless plating, and the proportion of the affinity layer gradually decreases from the lithium anode layer to the separator.

[0045] Lithium-ion affinity elements are elements that exhibit a strong affinity for lithium ions. They can include both metallic / nonmetallic elements that form alloys with lithium and elements containing functional groups that have a strong affinity for lithium ions. They can include, for example, silver (Ag), zinc (Zn), gold (Au), aluminum (Al), carbon (C), or combinations thereof.

[0046] For example, a layer containing conductive metal nanoparticles may include conductive metal elements and conductive carbon fibers. The conductive metal elements may include copper (Cu), iron (Fe), nickel (Ni), or combinations thereof, and the conductive carbon fibers may include carbon nanotubes (CNTs), graphite nanofibers (GNFs), or combinations thereof.

[0047] Supports for lithium metal anodes with lithium affinity gradients may also contain binders.

[0048] The adhesive is used to improve the adhesion between the conductive carbon fibers and the pore-forming agent, as well as the adhesion strength to the membrane. Examples may include: polyvinylidene fluoride (PVDF), PVDF-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene-butadiene rubber (SBR), fluorinated elastomers, or various copolymers thereof, and may be used alone or in mixtures of two or more thereof. More specifically, in one embodiment, it may be polyvinylidene fluoride (PVDF).

[0049] Based on the total weight (100 wt%) of the conductive metal element, conductive carbon fiber, and binder, the content of conductive carbon fiber can range from 1 wt% to 5 wt%, for example, greater than 1 wt% and less than 5 wt%, for example, 2 wt% to 4 wt%, for example, 3 wt%. When the content of conductive carbon fiber is less than 1 wt% based on the total weight of the carrier for the lithium metal anode with a lithium affinity gradient, the amount of conductive carbon fiber is too small to reduce the conductivity, and the reduction is too great for electrical connections to be formed between structures, thus the structure cannot function. When the content of conductive carbon fiber is greater than 5 wt% based on the total weight of the carrier for the lithium metal anode, the conductivity is too high for lithium to be electrodeposited on the structure. In one embodiment, the conductive carbon fiber can be graphite nanofibers (GNF) instead of carbon nanotubes (CNTs).

[0050] For example, the thickness of the support for lithium metal anodes with a lithium affinity gradient can range from 10 μm to 100 μm, such as 20 μm to 80 μm, 20 μm to 60 μm, 20 μm to 50 μm, or even 35 μm. The thickness of the support for lithium metal anodes can be easily controlled by adjusting the casting thickness as described below. In other words, since the support for lithium metal anodes with a lithium affinity gradient according to the embodiment can be controlled by producing the electrode using a casting method, lithium metal batteries with various specifications can be manufactured using this support.

[0051] Method for manufacturing carbon fiber carriers for lithium metal anodes A method for manufacturing a support for a lithium metal anode with a lithium affinity gradient, according to an embodiment, includes: adding a mixture of a conductive metal element, conductive carbon fiber, and a binder to a solvent; adding a pore-forming agent to the solvent to which the mixture was added to prepare a slurry; casting the slurry onto a separator; drying the slurry cast on the separator; etching the slurry cast on the separator after drying to obtain a support for a lithium metal anode in a first state (e.g., a state in which the support does not have a lithium affinity gradient); and reacting the support for a lithium metal anode in the first state with a solution containing a lithium ion affinity element.

[0052] The porous structure (lithium metal support) of the embodiment can be prepared by mixing conductive carbon fibers, conductive metal elements, and binders constituting the structure in a specific mass ratio, and adding the mixture to a solvent; adding an etching material (pore-forming agent) that can be etched with deionized (DI) water, and ball milling them to prepare a slurry; casting the slurry onto a separator using a doctor blade; drying it; and etching it with deionized water to create a support with high porosity for a lithium metal anode. However, the support for a lithium metal anode obtained in this step does not yet have a lithium affinity gradient. Subsequently, the lithium metal anode support that does not yet have a lithium affinity gradient is reacted with a solution containing elements with lithium ion affinity to achieve a lithium affinity gradient and obtain a support in a second state (where the support for a lithium metal anode includes a lithium affinity gradient). With this lithium affinity gradient, internal electrodeposition of lithium can be easily induced, making it suitable for large-area applications.

[0053] A lithium affinity treatment method is introduced by float coating a lithium metal anode support without a lithium affinity gradient in a solution containing lithium-ion affinity elements. When using the float coating method, lithium-ion affinity elements can be easily formed only on the surface of the structure. Specifically, a lithium metal anode support without a lithium affinity gradient can be floated in an aqueous silver nitrate (AgNO3) solution for a predetermined time, and a conductive porous structure with a silver-rich lithium affinity gradient on its surface can be created through an electrochemical displacement reaction (see [link to relevant documentation]). Figure 4 The concentration of silver nitrate (AgNO3) aqueous solution can be adjusted to a specific level to control the Ag content. Pore-forming agents can be added to porous structures to reduce the aggregation of conductive carbon fibers. The weight of the porous structure can be reduced to 0.12 mg / cm³. 2 / 10 μm or smaller, enabling the realization of batteries with high energy per unit weight / energy per unit volume.

[0054] For example, pore-forming agents may include NaCl, sucrose, silica, PMMA, styrene, iron oxide (Fe2O3), nickel(II) oxide (NiO), aluminum oxide (Al2O3), or combinations thereof. In particular, in one embodiment, NaCl and / or sucrose may be etched with water alone, thus greatly improving processability when manufacturing porous structures (lithium metal carriers) according to embodiments of the present invention.

[0055] According to the implementation scheme, the porous structure (for a lithium metal anode support) with a lithium affinity gradient can be easily controlled in terms of microstructure using micron-sized particles and etching and casting methods, and the macrostructure can also be easily controlled by using casting to produce the electrode. In other words, the method for manufacturing a lithium metal anode support with a lithium affinity gradient according to the implementation scheme can easily control the microstructure and macrostructure simultaneously or selectively, thereby enabling the manufacture of lithium metal batteries with various specifications.

[0056] The step of reacting a lithium metal anode support without a lithium affinity gradient with a solution containing a lithium-ion affinity element can be carried out for more than 1 minute and less than 10 minutes, for example, 1 minute to 10 minutes, 1 minute to 5 minutes, 2 minutes to 4 minutes, or 3 minutes. This is a process in which a lithium-ion affinity element (e.g., Ag) replaces a conductive metal element (e.g., Cu) in an electroless plating method. Where the lithium metal anode support without a lithium affinity gradient reacts with a solution containing a lithium-ion affinity element within a certain time range, the lithium-ion affinity element (e.g., Ag) can be present in a higher proportion due to the higher proportion of lithium-ion affinity elements, while maintaining excellent battery performance. If the reaction time is less than 1 minute, it is too short, and there is almost no amount of lithium-ion affinity element; however, if the reaction time is greater than 10 minutes, the battery performance may deteriorate.

[0057] In the method for manufacturing a lithium metal anode carrier with a lithium affinity gradient according to the embodiment, conductive carbon fibers, pore-forming agents, binders, etc. are as described above, and other components may also be as described above.

[0058] As described above, the lithium metal battery according to embodiments of the present invention can have excellent cycle life and excellent electrochemical performance, and therefore can be used in portable devices such as mobile phones, laptops and digital cameras, as well as electric vehicles such as hybrid electric vehicles (HEVs).

[0059] The following embodiments illustrate one or more embodiments of the present invention in more detail. However, the following embodiments are merely embodiments of the present invention, and the present invention is not limited to the following embodiments.

[0060] Comparative Example 1: Copper Foil As a control group, copper foil (Cu foil) was used.

[0061] Comparative Example 2: Fabrication of a conductive porous structure without a lithium affinity gradient Copper particles, conductive material, and binder (PVDF) in a mass ratio of 87:3:10 were added to NMP (N-methyl-2-pyrrolidone) solvent, and an etching material, NaCl, was added to achieve a porosity of 80%. The mixture was ball-milled and then cast onto a diaphragm using a scraper. After drying, the etching material was etched with water to remove the NaCl, thereby obtaining a conductive porous structure.

[0062] Example 1: Fabrication of a conductive porous structure with lithium affinity gradient Copper particles, conductive material, and binder (PVDF) in a mass ratio of 87:3:10 were added to an NMP (N-methyl-2-pyrrolidone) solvent, and an etching material, NaCl, was added to achieve a porosity of 80%. The mixture was ball-milled and then cast onto a diaphragm using a scraper. After drying, the etching material was etched with water to remove the NaCl, thereby obtaining the conductive porous structure of Comparative Example 2. This structure was floated in an aqueous silver nitrate solution for 3 minutes, and a conductive porous structure with a silver-rich lithium affinity gradient on the surface was obtained through an electrochemical displacement reaction.

[0063] Conditions for the following evaluation - A 170 μm thick lithium layer was stacked on a conductive porous structure and used as both a counter electrode and a reference electrode. The conductive porous structure was then used as the working electrode to test the electrochemical performance at different current densities and electrodeposition times.

[0064] - In electrochemical analysis, the electrolyte is prepared as follows: lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) salt is dissolved at a concentration of 1 M in a solvent containing DOL (1,3-dioxolane) / DME (1,2-dimethoxyethane) in a 1:1 volume ratio and 1% (wt%) LiNO3. (Symmetric cell test, full cell test) - In this electrochemical analysis, an electrolyte prepared by means of L... i TFSI salt was dissolved at a concentration of 1 M in a solvent containing DOL (1,3-dioxolane) / DME (1,2-dimethoxyethane) in a 1:1 volume ratio and 2% (wt%) LiNO3. (Half-cell test) Evaluation 1: Control of reaction time of silver nitrate solution in the structure In the electroless plating method of replacing Cu with Ag (Cu→Ag), the proportion of Ag increases as the reaction time of the structure in silver nitrate solution increases.

[0065] The Ag and Cu ratios were examined at each reaction time of 1 minute, 3 minutes, 5 minutes, and 10 minutes, and the results are shown in Table 1 and... Figure 4In the middle. Button half-cell tests showed that peak performance was achieved at a response time of 3 minutes (see...). Figure 5 ).

[0066] The shortest reaction time, 1 minute, showed an Ag content of 0.007 mg, meaning almost no Ag. Therefore, reaction times of less than 3 minutes have been proven insufficient for silver formation in electroless plating (see [link to relevant documentation]). Figure 4 (and Table 1).

[0067] Cross-sectional scanning electron microscopy (SEM) and energy-dispersive X-ray spectroscopy (EDS) analyses of the structure confirmed that it retains its shape due to the Ag reaction. Furthermore, when the float coating method was applied, it was confirmed that Ag forms only on the surface of the structure (see [link to relevant documentation]). Figure 6 ).

[0068] Table 1 Evaluation 2: Controlling the proportion of graphite nanofibers (GNF) Conductivity was measured using a two-terminal DC resistance method, which confirmed that a higher GNF ratio leads to greater Cu ion connectivity and thus a higher overall conductivity of the structure (see [link to relevant documentation]). Figure 7 (and Table 2).

[0069] By testing at GNF ratios of 1%, 3%, and 5%, the results confirmed that higher ratios resulted in higher conductivity and lower resistance (see [reference]). Figure 7 (and Table 2). The results shown in Table 2 are obtained from Equation 1: ρ = (R·S) / L = (U·S) / (I·L) U: Average voltage increases S: Electrode area (r=5 mm) I: Applied current (5 mA) L: Electrode thickness.

[0070] When the conductivity is low, the structure loses its electrical connection with other structures and cannot function properly. However, when the conductivity is high, lithium batteries are deposited on the structure. This confirms that the conductivity needs to be at an appropriate level, and that structures manufactured at a 3% weight ratio exhibit the highest performance (see [link to relevant documentation]). Figure 8 ).

[0071] Table 2 Evaluation 3: Lithium-ion battery deposition on conductive porous structures Comparative Example 1 (in which copper foil was used) exhibited non-uniform electrodeposition with a curved shape (see Example 2). Figure 9 ).

[0072] Comparative Example 2 confirms that lithium is deposited on top of the structure. This indicates that, when no lithium-affinity material is applied, lithium is deposited on top of the structure rather than inside. The lithium electrodeposited on top of the structure results in a total thickness of 62.54 μm for both the structure and the electrodeposited lithium (see [link to example]). Figure 10 ).

[0073] Example 1 demonstrated lithium electrodeposition within the structure. This was achieved by applying a lithium-affinity metal to electrodeposit lithium by filling the structure from the bottom. The lithium electrodeposition within the structure reduces the thickness of the electrodeposited lithium within the structure to a very thin 34.32 μm (see [link to example 1]). Figure 11 ).

[0074] Evaluation 4: Differences in nucleation overvoltage Comparative Examples 1 and 2, using copper as the main component, do not exhibit lithium affinity. Therefore, a high nucleation overvoltage of 100 mV or higher occurs (see...). Figure 12 ).

[0075] Due to the presence of silver (a lithium-affinity metal), Example 1 exhibited a low nucleation overvoltage. This indicates that lithium reacts with silver at the start of lithium deposition (see [link to example 1]). Figure 12 ).

[0076] Evaluation 5: Battery Cell Test (1) The reversibility of lithium-ion is evaluated by half-cell cycle life evaluation using a conductive porous structure made without the use of lithium-affinity silver.

[0077] Example 1, which applied silver, exhibited the highest performance, followed by Comparative Example 2, which did not apply silver to the structure. Comparative Example 1 (copper foil), which did not apply silver to the structure, exhibited the lowest performance (see [link]). Figure 13 ).

[0078] (2) Electrochemical testing of battery cells with conductive porous structures made without the use of lithium-affinity silver.

[0079] Symmetrical battery cycle life test (see) Figure 14A ) and output tests (see Figure 14B () also exhibited the same performance as (1), with Example 1 exhibiting the highest performance.

[0080] (3) Full cell test of conductive porous structure without the use of lithium-affinity silver.

[0081] Full battery cycle life test (see) Figure 15A ) and cycle life testing (see Figure 15B (1) exhibits the same performance as (1), with Example 1 exhibiting the highest performance.

[0082] Although the invention has been described in conjunction with exemplary embodiments now considered practical, it should be understood that the invention is not limited to the disclosed embodiments, but rather is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims. Therefore, the foregoing embodiments should be understood as examples and not as limiting the invention in any way.

Claims

1. A support for a lithium metal anode with a lithium affinity gradient, the support comprising: Diaphragm; A layer located on the diaphragm and containing conductive metal nanoparticles; and A lithium affinity layer located on a layer containing conductive metal nanoparticles. The layer containing conductive metal nanoparticles also includes pores.

2. The support for a lithium metal negative electrode with a gradient of lithium affinity according to claim 1, wherein, The porosity of the carrier used for lithium metal anodes ranges from 60% to 97%.

3. The support for a lithium metal negative electrode with a gradient of lithium affinity according to claim 1, wherein, The lithium affinity layer contains lithium ion affinity elements.

4. The support for a lithium metal negative electrode with a gradient of lithium affinity according to claim 3, wherein, The lithium-ion affinity elements include silver, zinc, gold, aluminum, carbon, or combinations thereof.

5. The support for a lithium metal negative electrode with a gradient of lithium affinity according to claim 1, wherein, The layer containing conductive metal nanoparticles includes conductive metal elements and conductive carbon fibers.

6. The support for a lithium metal negative electrode with a gradient of lithium affinity according to claim 5, wherein, The conductive metal element includes copper, iron, nickel, or a combination thereof.

7. The support for a lithium metal negative electrode with a gradient of lithium affinity according to claim 5, wherein, The conductive carbon fiber includes carbon nanotubes, graphite nanofibers, or a combination thereof.

8. The support for a lithium metal negative electrode having a gradient of lithium affinity according to claim 5, wherein, The carrier used for lithium metal anodes also includes a binder.

9. The support for a lithium metal negative electrode with a gradient of lithium affinity according to claim 8, wherein, The content of the conductive carbon fiber ranges from 1% to 5% by weight, based on a total weight of 100% by weight of the conductive metal element, conductive carbon fiber, and binder.

10. The support for a lithium metal negative electrode having a gradient of lithium affinity according to claim 1, wherein, The thickness of the carrier used for lithium metal anodes ranges from 10 μm to 100 μm.

11. A method for manufacturing a carrier for a lithium metal anode, comprising: A mixture of conductive metal elements, conductive carbon fibers, and adhesives is added to a solvent; A pore-forming agent is added to a solvent containing the mixture to prepare a slurry; The slurry is cast onto the diaphragm; The slurry cast on the diaphragm is dried; After drying the slurry cast on the separator, etching is performed to obtain a carrier for the lithium metal anode in a first state; and The carrier in its first state is reacted with a solution containing an element with lithium ion affinity.

12. The method of manufacturing a carrier for a lithium metal anode of claim 11, wherein, The carrier in the first state does not have a lithium affinity gradient.

13. The method of manufacturing a carrier for a lithium metal anode of claim 11, wherein, Reacting a carrier in its first state with a solution containing a lithium-ion affinity element involves float-coating the carrier in its first state in a solution containing a lithium-ion affinity element.

14. The method of manufacturing a carrier for a lithium metal anode of claim 11, wherein, The pore-forming agent includes sodium chloride, sucrose, silicon dioxide, polymethyl methacrylate, styrene, iron oxide, nickel oxide, aluminum oxide, or a combination thereof.

15. The method of manufacturing a carrier for a lithium metal anode of claim 11, wherein, The reaction time between the carrier in its first state and the solution containing lithium-ion-affinity elements is more than 1 minute and less than 10 minutes.

16. The method of manufacturing a carrier for a lithium metal anode of claim 11, wherein, The conductive carbon fiber content ranges from 1% to 5% by weight, based on 100% by weight of the total weight of the mixture of conductive metal elements, conductive carbon fibers, and binders.

17. The method of manufacturing a carrier for a lithium metal anode of claim 11, further comprising: A support in a second state is obtained by reacting a support in a first state with a solution containing a lithium-ion affinity element, wherein the support in the second state comprises a lithium affinity gradient.

18. The method of manufacturing a carrier for a lithium metal anode of claim 11, wherein, The lithium-ion affinity elements include silver, zinc, gold, aluminum, carbon, or combinations thereof.

19. The method of manufacturing a carrier for a lithium metal anode of claim 11, wherein, The conductive metal element includes copper, iron, nickel, or a combination thereof.

20. The method of manufacturing a carrier for a lithium metal anode of claim 11, wherein, The conductive carbon fiber includes carbon nanotubes, graphite nanofibers, or a combination thereof.

Citation Information

Patent Citations

  • Controlling method of heat balance using adjusting pattern shape of spot welding electrode

    KR1020250062293A