Current collectors and their preparation methods, lithium-ion batteries
By introducing a composite structure of polymer matrix and nano-copper powder particles into the current collector of lithium-ion batteries, combined with flame retardants, active power cut-off and chemical flame retardancy in the early stage of thermal runaway are achieved, solving the safety problem of existing current collectors during thermal runaway, and being compatible with existing battery manufacturing processes, thus realizing industrial application.
Patent Information
- Application Number
- CN202611047120.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing lithium-ion battery current collectors lack active safety intervention functions in the event of thermal runaway, and existing solutions for imparting safety characteristics are complex in process and have poor compatibility with battery manufacturing, making it difficult to achieve industrialization.
The composite structure of dispersed nano-copper powder particles in a polymer matrix is adopted. A conductive network is formed by sintering the neck and adding flame retardants to achieve high-temperature power-off and chemical flame retardancy. The preparation method is compatible with existing battery manufacturing processes.
It can actively cut off power in the early stage of thermal runaway to prevent the spread of thermal runaway. It has good conductivity at room temperature and high temperature safety protection capabilities, is compatible with existing battery manufacturing processes, and can be used for industrial applications.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery technology, specifically to current collectors and their preparation methods, and lithium-ion batteries. Background Technology
[0002] Thermal runaway is the most serious safety failure mode of lithium-ion batteries. It is often triggered by overcharging, internal short circuits, or mechanical abuse, causing a rapid increase in the internal temperature of the battery, initiating a chain of exothermic reactions, and potentially leading to fire or explosion. During thermal runaway, the copper foil only serves as a good conductor of heat and a pathway for current, without any active safety intervention function. Recent studies have attempted to endow current collectors with safety characteristics; however, these solutions are often complex in process, have poor compatibility with existing mature battery manufacturing processes, or adversely affect the initial conductivity and mechanical strength of the current collector, making industrial application difficult.
[0003] Therefore, there is an urgent need to develop a negative electrode current collector that has active safety intervention capabilities and good compatibility with battery manufacturing processes. Summary of the Invention
[0004] This invention aims to at least partially solve one of the technical problems in related technologies. To this end, this invention proposes a current collector, its preparation method, and a lithium-ion battery. This current collector exhibits stable performance at room temperature and, when the internal temperature of the battery abnormally rises, can actively cut off local conductive pathways and synergistically suppress combustion, thereby preventing the spread of thermal runaway.
[0005] A first aspect of this application provides a current collector. The current collector comprises a polymer matrix and nano-copper powder particles dispersed within the polymer matrix, with at least some adjacent nano-copper powder particles electrically connected. This current collector constructs a composite structure of a polymer matrix and a dispersed conductive network of nano-copper powder particles, enabling it to conduct electricity at room temperature and actively disconnect power in response to high temperatures, providing a safety protection capability.
[0006] According to an embodiment of this application, the electrical connection between adjacent copper nanoparticles satisfies at least one of the following conditions: there is a sintered neck between adjacent copper nanoparticles; the surfaces of adjacent copper nanoparticles are in contact.
[0007] According to an embodiment of this application, the nano-copper powder particles achieve effective electrical connection; the electrical connection refers to the sheet resistance of the current collector being less than 100mΩ / □.
[0008] According to embodiments of this application, the current collector further includes at least one of the following: a flame retardant dispersed in the polymer matrix; a leveling agent dispersed in the polymer matrix; and a dispersant dispersed in the polymer matrix.
[0009] According to embodiments of this application, the current collector further satisfies at least one of the following conditions: the nano-copper powder particles are spherical or flake-shaped; the polymer matrix includes at least one of polymethyl methacrylate, polycarbonate, polystyrene, ethyl cellulose, polyvinyl chloride, polyacrylamide, polyphosphazene, polysiloxane, polylactic acid, polyethylene terephthalate, polyethylene, polyurethane, polypropylene, acrylonitrile-butadiene-styrene, polyethylene oxide, polyaniline, polypyrrole, polythiophene, polyacetylene, and poly(3,4-ethylenedioxythiophene); the leveling agent includes BYK-333, BYK-306, BYK-307, BYK-310, BYK-354, BYK-3609, and Perenol. At least one of F40; the dispersant includes at least one of polyvinylpyrrolidone, sodium polyacrylate, Tween 80, cetyltrimethylammonium bromide, and butyl phosphate; the flame retardant includes unmodified inorganic flame retardant filler and inorganic flame retardant filler with surface modified by silane coupling agent and / or titanate coupling agent, wherein the unmodified inorganic flame retardant filler includes at least one of polyphosphazene, polycyclic phosphazene, aluminum hydroxide, magnesium hydroxide, and ammonium polyphosphate.
[0010] A second aspect of this application provides a method for preparing the aforementioned current collector. The method includes: preparing a copper paste containing nano-copper powder particles, a polymer, and a solvent; molding and solidifying the copper paste to form a green blank; sintering the green blank; and rolling the sintered green blank to obtain the current collector. This preparation method is simple in steps, highly compatible with various processes, and easily industrialized.
[0011] According to an embodiment of this application, the copper paste further includes at least one of a curing agent raw material, a leveling agent, a dispersant, and a flame retardant, wherein the curing agent raw material includes a monomer and an initiator.
[0012] According to embodiments of this application, at least one of the following conditions is satisfied: the monomer includes at least one selected from polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, pentaerythritol tetraacrylate, trimethylolpropane triacrylate, epoxy acrylate, 1,6-hexanediol diacrylate, and polyurethane acrylate; the initiator includes azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, benzoyl peroxide, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and 2,4,6-trimethyl... The sintering solution comprises at least one of the following: ethyl benzoylphenylphosphonate, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, (2,4,6-trimethylbenzoyl)di(p-tolyl)phosphine oxide, 2-hydroxy-2-methylphenylacetone, and camphorquinone; the solvent comprises at least one of ethylene glycol, diethylene glycol, glycerol, polyethylene glycol, ethanol, methanol, isopropanol, dipropylene glycol methyl ether acetate, terpineol, and glyceryl tripalmitate; the sintering temperature is 100℃-150℃; the sintering time is 0.5h-24h; and the rolling pressure is 1 MPa-50 MPa.
[0013] According to an embodiment of this application, the copper paste comprises, by weight: 70-95 parts by weight of the nano-copper powder particles; 1-10 parts by weight of the polymer; 1-10 parts by weight of the curing agent raw material, wherein the weight ratio of the initiator to the monomer is 0.5:100 to 4:100; 1-10 parts by weight of the solvent; 0.01-0.5 parts by weight of the leveling agent; 0.01-0.5 parts by weight of the dispersant; and 0.1-5 parts by weight of the flame retardant.
[0014] In a third aspect, this application provides a lithium-ion battery comprising a current collector as described above, or a current collector obtained by the above preparation method. This lithium-ion battery possesses all the features and advantages of the aforementioned current collector, which will not be elaborated further here. Detailed Implementation
[0015] The embodiments of the present invention described below are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0016] This application is based on the inventor’s discovery and understanding of the following facts and problems: As mentioned above, the related technologies have the following problems: (1) Traditional methods are mostly passive protection, that is, delaying or isolating when thermal runaway occurs or spreads, but it is difficult to actively and quickly interrupt the vicious cycle from the physical path of energy transfer in the early stage of thermal runaway; (2) The schemes that give the current collector safety are often complex in process, have poor compatibility with existing mature battery manufacturing processes, or have an adverse effect on the initial conductivity and mechanical strength of the current collector, making it difficult to achieve industrial application; (3) Existing safety design schemes are mostly concentrated on a single protection mechanism, lack synergistic effect, and cannot suppress combustion reaction while cutting off the heat source. After research and analysis, the inventor concluded that the reasons may be: (1) Traditional copper foil is only a good conductor of heat and a path for current, and does not have any active safety intervention function. When thermal runaway occurs, copper foil will accelerate the accumulation of heat and electrochemical reaction; (2) Existing composite current collectors mostly adopt a composite structure of "metal-polymer-metal". Although the circuit is broken due to the melting and shrinkage of polymer at high temperature, its conductive network depends on the continuous metal layer. Once short circuit occurs, it will lead to overall failure; (3) A single short circuit or flame retardant mechanism cannot cope with the complex electrochemical-thermal coupling chain reaction in thermal runaway.
[0017] In response to the above situation, the inventors have proposed a current collector, its preparation method, and a lithium-ion battery. This application transforms the current collector from a passive conductor into an intelligent safety component with "temperature sensing-power-off-flame retardant" functions, enabling proactive intervention in the early stages of thermal runaway and preventing a vicious cycle.
[0018] A first aspect of this application provides a current collector. According to an embodiment of this application, the current collector comprises: a polymer matrix; and nano-copper powder particles dispersed within the polymer matrix, with at least some adjacent nano-copper powder particles electrically connected. This current collector constructs a composite structure of a polymer matrix and a conductive network of dispersed nano-copper powder particles, enabling it to conduct electricity at room temperature and actively disconnect power in response to high temperatures, providing a safety protection capability.
[0019] According to an embodiment of this application, adjacent copper nanoparticles have sintered necks. These sintered necks form a metallurgical bond, providing a stable conductive path.
[0020] Sintered necks are neck-shaped metallurgical connections formed at the contact points of powder particles through mass migration mechanisms such as surface diffusion, volume diffusion, and evaporation-condensation at high temperatures. Essentially, it is a process of spontaneous reduction of free energy driven by the surface energy of the system—particles evolve from point contact to surface contact, the total surface area and surface energy drop sharply, and the density and strength increase accordingly.
[0021] According to an embodiment of this application, the surfaces of adjacent copper nanoparticles are in contact. The physical contact points of the surfaces form a mechanical overlap, supplementing the conductive path on the basis of the sintered neck. The two work together to ensure that the rate performance requirements of the battery are met at room temperature.
[0022] According to embodiments of this application, the nano-copper powder particles achieve effective electrical connectivity. This ensures that the vast majority of the nano-copper powder in the current collector participates in conductivity, forming a high-density, low-resistance conductive network.
[0023] According to an embodiment of this application, the electrical connection refers to the sheet resistance of the current collector being less than 100 mΩ / □. This ensures that the current collector has good basic conductivity.
[0024] Sheet resistance (SRR) is a key parameter describing the resistive characteristics of thin-film conductive materials. It represents the resistance of a square material with an arbitrary side length, and its unit is ohms per square (Ω). It reflects the combined effect of the material's conductivity and thickness, depending only on resistivity and thickness, and is independent of the square size. By quantifying the uniform conductivity of a material, sheet resistance can be used to optimize thin film thickness, evaluate process quality, control circuit performance, and guide material selection and design. It is a crucial indicator for ensuring the stable and efficient performance of electronic devices.
[0025] According to embodiments of this application, the polymer further includes at least one of the following: a flame retardant dispersed in the polymer matrix; a leveling agent dispersed in the polymer matrix; and a dispersant dispersed in the polymer matrix. The introduction of the flame retardant adds chemical flame-suppressing functionality to the current collector in addition to physical circuit breaking, improving safety and reliability. The leveling agent and dispersant ensure that the flame retardant and other components are uniformly distributed in the polymer.
[0026] According to embodiments of this application, the nano-copper powder particles are spherical or flake-shaped. Spherical copper powder forms point contacts, while flake-shaped copper powder forms surface / line contacts, resulting in denser conductive pathways, easier circuit breaking at high temperatures, and thus meeting the battery's safety protection requirements at high temperatures and suppressing thermal runaway.
[0027] According to embodiments of this application, the polymer matrix includes at least one selected from polymethyl methacrylate (PMMA), polycarbonate (PC), polystyrene (PS), ethyl cellulose (EC), polyvinyl chloride (PVC), polyacrylamide (PAM), polyphosphonitrile (PNP), polysiloxane (PDMS), polylactic acid (PLA), polyethylene terephthalate (PET), polyethylene (PE), polyurethane (PU), polypropylene (PP), acrylonitrile-butadiene-styrene (ABS), polyethylene oxide (PEO), polyaniline (PANI), polypyrrole (PPy), polythiophene (PTH), polyacetylene (PA), and poly(3,4-ethylenedioxythiophene) (PEDOT). The above polymers can effectively bond nano-copper powder particles and provide thermal responsiveness. Furthermore, thermoplastic polymers, such as PMMA and PS, soften and melt at high temperatures, expanding their volume to stretch the conductive network and achieve sensitive circuit breaking. Energetic polymers, such as PU, decompose at high temperatures to generate gas, utilizing gas stress to break the sintering neck and achieve physical circuit breaking. Phosphorus / silicon-containing polymers, such as PNP and PDMS, inherently possess flame-retardant elements, synergistically forming charcoal insulation with added flame retardants at high temperatures, improving chemical flame-suppressing efficiency and achieving dual protection. Flexible polymers can impart bending resistance to current collectors, meeting the requirements of winding processes; rigid polymers can improve the strength of the film layer, ensuring no deformation during active material coating. Therefore, different polymers can be selected according to needs, facilitating customized formulation development for different molding processes and performance requirements.
[0028] According to embodiments of this application, the leveling agent includes at least one of BYK-333, BYK-306, BYK-307, BYK-310, BYK-354, BYK-3609, and Perenol F40, wherein BYK-333, BYK-306, BYK-307, BYK-310, BYK-354, and BYK-3609 are commercial products manufactured by BYK Chemicals, and Perenol F40 is a commercial product manufactured by BASF. Selecting the above leveling agents can effectively reduce the surface tension of the paste, eliminate surface defects such as orange peel, pinholes, and streaks generated during coating or printing, and ensure uniform wet film spreading.
[0029] According to the embodiments of this application, the dispersant is at least one of polyvinylpyrrolidone (PVP), sodium polyacrylate, Tween 80 (polysorbate-80), cetyltrimethylammonium bromide (CTAB), and butyl phosphate. Selecting the above materials can ensure that each component is uniformly dispersed through steric hindrance or electrostatic repulsion, thus ensuring the uniformity of the current collector's microstructure.
[0030] According to embodiments of this application, the flame retardant includes unmodified inorganic flame retardant fillers and inorganic flame retardant fillers with surfaces modified by silane coupling agents and / or titanate coupling agents. The unmodified inorganic flame retardant fillers include at least one of polyphosphazene, polycyclic phosphazene, aluminum hydroxide, magnesium hydroxide, and ammonium polyphosphate. Selecting the above-mentioned flame retardant fillers can synergistically provide dual protection of "circuit breaking and flame retardancy." At high temperatures, ammonium polyphosphate (APP) decomposes to generate polyphosphoric acid and ammonia, absorbing heat and cooling, diluting oxygen, and forming a protective layer; aluminum hydroxide / magnesium hydroxide (ATH / MDH) decomposes, absorbing a large amount of heat and releasing water vapor; polyphosphazene (PNP) can capture free radicals and inhibit the combustion chain reaction. Furthermore, the gas pressure generated by the high-temperature decomposition of the flame retardant can synergistically expand the copper powder conductive network, accelerating the breakage of the sintering neck and the separation from the physical contact point, thus reducing the thermal response trigger threshold.
[0031] According to embodiments of this application, the nano-copper powder particles are spherical or flake-shaped, with a D50 of 50 nm to 500 nm. Specifically, the particle size is within the range of 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, or any combination thereof. Particle sizes within the above range can form effective sintering necks while retaining sufficient specific surface area to synergistically disrupt the polymer gas generation circuit.
[0032] A second aspect of this application provides a method for preparing the above-described current collector, comprising: S10: Prepare copper paste, wherein the copper paste contains nano-copper powder particles, polymer and solvent.
[0033] According to embodiments of this application, the copper paste further includes at least one of a curing agent, a leveling agent, a dispersant, and a flame retardant, wherein the curing agent includes a monomer and an initiator. By uniformly mixing and stably dispersing nano-copper powder particles, polymers, solvents, and optional functional additives (flame retardants, leveling agents, dispersants, etc.), a conductive network that conducts electricity at room temperature and de-energizes at high temperatures is constructed. This step ensures uniform distribution and interfacial compatibility of the components at the microscale, while the rheological properties of the paste are adaptable to various molding processes such as coating and printing.
[0034] According to embodiments of this application, the monomer includes at least one of polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, pentaerythritol tetraacrylate, trimethylolpropane triacrylate, epoxy acrylate, 1,6-hexanediol diacrylate, and polyurethane acrylate. Selecting the above monomers allows for the crosslinking and fixation of the nano-copper powder particles with the flame retardant. Furthermore, monomers containing multiple acrylate functional groups can crosslink into a three-dimensional network under the action of an initiator, ensuring uniform green strength and component distribution.
[0035] According to embodiments of this application, the initiator includes at least one selected from azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, benzoyl peroxide, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (TPO), ethyl 2,4,6-trimethylbenzoylphenylphosphonate (TPO-L), phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (819), (2,4,6-trimethylbenzoyl)bis(p-tolyl)phosphine oxide (TMO), 2-hydroxy-2-methylphenylacetone (HMPP), and camphorquinone. Selecting the above initiators allows for compatibility with low-temperature sintering processes, enabling efficient decomposition to generate free radicals within the low-temperature sintering range, and precise activation of monomer crosslinking.
[0036] According to embodiments of this application, the solvent includes at least one selected from ethylene glycol (EG), diethylene glycol (DEG), glycerol (G), polyethylene glycol (PEG300, PEG400), ethanol (EtOH), methanol (MeOH), isopropanol (IPA), dipropylene glycol methyl ether acetate (DPMA), terpineol derivatives, and glyceryl tripalmitate (GT). Terpineol derivatives are preferably α-terpineol, and polyethylene glycol is preferably polyethylene glycol 300 (PEG300) or polyethylene glycol 400 (PEG400). The selection of the above solvents effectively wets the nano-copper powder particles, polymer, and flame retardant, and, in conjunction with a dispersant, achieves uniform dispersion of each component. The solvent evaporates slowly during sintering, ensuring that it is substantially removed before the initiator decomposes, thus not interfering with the crosslinking reaction and the formation of the sintering neck.
[0037] According to an embodiment of this application, the copper paste comprises, by weight: 70-95 parts by weight of the nano-copper powder particles; 1-10 parts by weight of the polymer; 1-10 parts by weight of the curing agent raw material, wherein the weight ratio of the initiator to the monomer is 0.5:100 to 4:100; 1-10 parts by weight of the solvent; 0.01-0.5 parts by weight of the leveling agent; 0.01-0.5 parts by weight of the dispersant; and 0.1-5 parts by weight of the flame retardant.
[0038] According to embodiments of this application, the nano-copper powder particles are 70 parts by weight to 95 parts by weight, specifically 70 parts by weight, 75 parts by weight, 80 parts by weight, 85 parts by weight, 90 parts by weight, 95 parts by weight, or any range between two of these. Within this range, efficient conductivity at room temperature is ensured while also reserving sufficient space for other functional components. Furthermore, this range ensures the slurry has a suitable viscosity, guaranteeing green strength and compatibility with various molding processes.
[0039] According to the embodiments of this application, the polymer is 1 part by weight to 10 parts by weight, specifically 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight or any range between the two. Within the above range, it can be ensured that the polymer forms a continuous matrix after sintering, which serves as both a dispersion carrier for the flame retardant and a synergistic charring process with the flame retardant during high-temperature decomposition, thereby enhancing the chemical flame retardant effect. At the same time, it provides sufficient bonding strength and flexibility to the green body to meet the requirements of coating and winding processes.
[0040] According to the embodiments of this application, the curing agent raw material is 1 part by weight to 10 parts by weight, specifically 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight or any range between the two. Within the above range, the curing agent raw material can ensure that the cross-linked network has appropriate strength and toughness, which is sufficient to maintain the stability of the conductive network structure at room temperature. At high temperature, the constraint provided by the cross-linked network is just right, so that the stress generated by polymer decomposition can quickly destroy the sintering neck and physical contact point, and achieve sensitive circuit breaking.
[0041] According to embodiments of this application, the weight ratio of the initiator to the monomer is 0.5:100 to 4:100, specifically 0.5:100, 1:100, 1.5:100, 2:100, 2.5:100, 3:100, 3.5:100, 4:100, or any range between the two. Within the above range, sufficient cross-linking can be ensured, preventing excessive cross-linking from causing the network to become too dense, and ensuring that the polymer and flame retardant can effectively destroy the conductive network at high temperatures, thereby achieving sensitive circuit breaking.
[0042] According to the embodiments of this application, the solvent is 1 part by weight to 10 parts by weight, specifically 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight or any range between the two. Within the above range, a slurry with a suitable viscosity can be formed, while avoiding drying shrinkage, ensuring that the solvent evaporates completely during the sintering process, and meeting the performance requirements of the current collector.
[0043] According to the embodiments of this application, the leveling agent is 0.01 parts by weight to 0.5 parts by weight, specifically 0.01 parts by weight, 0.05 parts by weight, 0.1 parts by weight, 0.15 parts by weight, 0.2 parts by weight, 0.25 parts by weight, 0.3 parts by weight, 0.35 parts by weight, 0.4 parts by weight, 0.45 parts by weight, 0.5 parts by weight, or any range between the two. Within the above range, the leveling agent reduces the surface tension of the slurry, eliminates defects such as orange peel, pinholes, and streaks generated during coating or printing, and ensures uniform spreading of the wet film.
[0044] According to the embodiments of this application, the dispersant is 0.01 parts by weight to 0.5 parts by weight, specifically 0.01 parts by weight, 0.05 parts by weight, 0.1 parts by weight, 0.15 parts by weight, 0.2 parts by weight, 0.25 parts by weight, 0.3 parts by weight, 0.35 parts by weight, 0.4 parts by weight, 0.45 parts by weight, 0.5 parts by weight, or any range between the two. Within the above range, it can ensure that the surface of solid particles such as nano-copper powder particles and flame retardants is fully wetted and coated, and effectively prevent agglomeration through steric hindrance or electrostatic repulsion, forming a uniform and stable slurry system.
[0045] According to the embodiments of this application, the flame retardant is 0.1 parts by weight to 5 parts by weight, specifically 0.1 parts by weight, 0.5 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight, 5 parts by weight, or any range between the two. Within the above range, it can be ensured that the flame retardant decomposes and absorbs heat at high temperatures, releases inert gases, or captures free radicals, effectively inhibiting combustion.
[0046] S20: The copper paste is shaped and cured to form a green blank.
[0047] This step transforms the liquid slurry into a solid green body with a specific shape and thickness, providing a structural basis for subsequent sintering. The curing process prevents flow or sedimentation after molding, ensuring uniform distribution of each component within the film layer and guaranteeing consistent performance of the final current collector.
[0048] According to embodiments of this application, the molding method includes at least one of coating, screen printing, casting, and 3D printing. The above molding processes enable precise thickness control, and all molding methods are mature technologies in the battery industry, seamlessly integrating with existing electrode manufacturing lines without requiring additional equipment investment, thus having a low threshold for industrialization.
[0049] S30: Sinter the green blank.
[0050] This step, through sintering, simultaneously completes solvent removal, initiator decomposition, and the formation of sintered necks for the nano-copper powder particles. This allows for electronic conductivity between the copper powder particles while maintaining structural fragility. The decomposition stress of the polymer / flame retardant at high temperatures is sufficient to cause them to fracture, achieving a sensitive thermal response. At the same time, it provides a structurally complete and uniformly thick preform for subsequent rolling.
[0051] According to embodiments of this application, the sintering temperature is 100℃-150℃, specifically 100℃, 105℃, 110℃, 115℃, 120℃, 125℃, 130℃, 135℃, 140℃, 145℃, 150℃, or any range between two of these. Within the above temperature range, it is possible to ensure that the nano-copper powder particles undergo solid-state diffusion to form a sintering neck, while simultaneously activating the initiator decomposition, promoting monomer cross-linking and solidification, and ensuring the green strength and conductive network construction.
[0052] According to embodiments of this application, the sintering time is 0.5h-24h, specifically 0.5h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h, or any range between two of these. Within the above time range, complete solvent evaporation, full decomposition of the initiator, and thorough cross-linking of the monomers can be ensured, while simultaneously allowing the nano-copper powder particles to form an effective sintering neck. This time span can meet the needs of different scales of production.
[0053] S40: Roll pressing is performed on the sintered blank to obtain a current collector.
[0054] This step involves rolling the blank to create tight physical contact points between the loose copper particles after sintering, filling the insufficient area of the sintering neck and meeting the battery rate performance requirements.
[0055] According to embodiments of this application, the rolling pressure is 1 MPa-50 MPa, specifically 1 MPa, 5 MPa, 10 MPa, 15 MPa, 20 MPa, 25 MPa, 30 MPa, 35 MPa, 40 MPa, 45 MPa, 50 MPa, or any range between two of these. Within this pressure range, the loose copper particles after sintering can form tight physical contact points, filling the insufficient area of the sintering neck and meeting the rate performance requirements of the battery. This pressure range, combined with precision rolling equipment, can accurately control the thickness of the current collector within the required range, meeting the stringent requirements of thinness and consistency for battery electrodes.
[0056] In a third aspect, this application provides a lithium-ion battery comprising a current collector as described above, or a current collector obtained according to the preparation method described above. This lithium-ion battery possesses all the features and advantages of the aforementioned current collector and preparation method, which will not be elaborated upon here. In some embodiments, the specific structure and type of the lithium-ion battery are not limited, as long as the aforementioned current collector is required.
[0057] Lithium-ion batteries mainly consist of a positive electrode, a negative electrode, a separator, an electrolyte, and an outer casing. The positive electrode includes a positive current collector and a layer of positive active material coated on it. This active material layer typically contains lithium transition metal composite oxides (such as lithium iron phosphate, lithium cobalt oxide, or ternary materials), a conductive agent, and a binder. The negative electrode includes a negative current collector and a layer of negative active material coated on it. This active material layer typically contains carbon-based materials (such as artificial graphite, natural graphite, or mesophase carbon microspheres) and a binder. The separator is positioned between the positive and negative electrodes to isolate them and prevent short circuits while allowing ions to pass through. The separator is typically a polyolefin microporous membrane (such as a single-layer or multi-layer composite membrane of polyethylene or polypropylene). The electrolyte fills the outer casing, wetting the positive and negative electrode plates. It typically contains non-aqueous organic solvents (such as ethylene carbonate, dimethyl carbonate, etc.) and dissolved lithium salts (such as lithium hexafluorophosphate), and may optionally contain functional additives (such as fluoroethylene carbonate) to optimize battery performance. The outer casing is encapsulated with metal (such as aluminum or steel) or an aluminum-plastic composite film to seal the internal components and provide mechanical protection.
[0058] The security protection mechanism of this application is as follows: 1. Electrical Circuit Breaking Mechanism (Active Power-Off): When localized thermal runaway of the battery causes the current collector temperature to rise, the adhesion between the polymer matrix and the nano-copper powder particles decreases, and the polymer matrix and flame retardant decompose to generate gas. This gas accumulates within the relatively sealed porous membrane, generating internal stress. This stress is sufficient to cause the fragile sintering necks between the copper powder particles to fracture and the physical contact points to detach. This results in a catastrophic decrease in the electronic conductivity of the localized area within seconds, equivalent to forming a localized "micro-circuit," cutting off the current in that area from the heat source for further electrochemical reactions.
[0059] 2. Chemical flame retardant mechanism (synergistic fire suppression): Dispersed flame retardants are activated at high temperatures. For example, modified ammonium polyphosphate (APP) decomposes to generate polyphosphoric acid and ammonia, which can absorb heat and lower the temperature, and the formed polyphosphoric acid layer can provide a protective coating, while the ammonia can dilute oxygen; modified aluminum hydroxide (ATH) / magnesium hydroxide (MDH) with a silane coupling agent on its surface decomposes to absorb a large amount of heat and release water vapor. More importantly, some flame retardant components can effectively capture free radicals generated by the decomposition of the electrolyte, thereby inhibiting the chain reaction of combustion.
[0060] This application has at least the following beneficial effects: 1. Active safety: The current collector is creatively transformed from a passive conductor into an intelligent safety component with "temperature sensing-power cut-off-flame retardant" functions, which can actively intervene in the early stage of thermal runaway and prevent a vicious cycle.
[0061] 2. Strong process compatibility: The slurry preparation and coating / printing / sintering processes are highly compatible with existing battery electrode manufacturing processes, making industrialization easy.
[0062] 3. Excellent and adjustable performance: Through component and process design, a balance can be achieved between excellent room temperature conductivity, mechanical flexibility and keen thermal triggering response.
[0063] 4. Reliable dual protection mechanism: The synergistic effect of "electrical circuit breaking" and "chemical flame retardancy" provides more comprehensive safety protection.
[0064] The embodiments of this application are described in detail below: Example 1 A low-temperature sintering copper paste with thermal runaway self-protection function, its composition (by weight percentage) is as follows: Nano copper powder particles (D50 150nm, oleic acid coated): 83% Polymer matrix: Polymethyl methacrylate (PMMA): 5% Curing agent raw material: 6%, of which: monomer: pentaerythritol tetraacrylate 5.7%, initiator: 2-hydroxy-2-methylphenylacetone (HMPP) 0.3%. Solvent: α-terpineol: 4% Leveling agent: BYK-333: 0.05% Dispersant: Polyvinylpyrrolidone (PVP, K30): 0.05% Flame retardant: Ammonium polyphosphate (APP) microspheres with surface modified by KH-550 silane coupling agent: 1.9% Preparation method: Drying: Place the nano copper powder particles and modified APP in a vacuum oven at 60℃ and dry for 3 hours.
[0065] Mixing: In a room temperature planetary mixing jar, add α-terpineol, PVP and BYK-333 and mix at 300 rpm for 12 minutes.
[0066] Paste preparation: The dried nano-copper powder particles are slowly added at room temperature, first mixed at a low speed of 400 rpm, then increased to 900 rpm and stirred for 40 minutes to form a paste. The temperature is controlled to be below 40℃ throughout the process using water cooling.
[0067] Ingredients: Add modified APP, PMMA powder, pentaerythritol tetraacrylate and HMPP to the paste, and continue to stir and mix at room temperature to obtain the first intermediate slurry.
[0068] Dispersion: The first intermediate slurry was stirred at high speed of 1800 rpm for 25 minutes at room temperature and then degassed under vacuum for 15 minutes to obtain the second intermediate slurry.
[0069] Rolling and curing: The second intermediate slurry was rolled four times at room temperature using a three-roll mill, sealed, and cured at 25°C for 6 hours. The finished copper slurry was then sieved to obtain the final product.
[0070] Preparation of negative electrode current collector: Copper paste was coated onto a PI film (wet film thickness 100 μm) and placed in a hot air oven. The film was then processed as follows: the temperature was increased from room temperature to 120°C at a rate of 2°C / min, and held at 120°C for 8 hours to complete polymer curing and low-temperature solid-state diffusion / redox sintering of copper particles. After cooling, the film was peeled off and rolled at 30 MPa at room temperature to obtain a current collector with a thickness of approximately 9 ± 2 μm.
[0071] Example 2 A low-temperature sintering copper paste with thermal runaway self-protection function, the composition of which is as follows: Nano copper powder particles (D50 50nm, PAM coated): 88% Polymer matrix: Polycarbonate (PC) powder: 2.5% Curing agent raw material: 4%, of which: monomer: 1,6-hexanediol diacrylate 3.88%, initiator: benzoyl peroxide (BPO) 0.12%. Solvent: Polyethylene glycol 400 (PEG400): 4.5% Leveling agent: BYK-307: 0.1% Dispersant: Sodium polyacrylate: 0.1% Flame retardant: Polyphosphazene (PNP) powder with surface modified by titanate coupling agent: 0.8% Preparation and molding: The slurry preparation process at room temperature is the same as in Example 1. A blade coating green body is used. The green body is placed in a forced-air oven and heat-treated at 130°C for 12 hours to induce BPO decomposition, initiate curing, and achieve interparticle bonding. It is then rolled at 10 MPa at room temperature to obtain a current collector with a thickness of approximately 9 ± 2 μm.
[0072] Example 3 A low-temperature sintering copper paste with thermal runaway self-protection function, the composition of which is as follows: Nano-sheet copper powder (D50 70nm): 73% Polymer matrix: Polypyrrole (ppy): 8% Curing agent raw materials: 5%, of which: monomer: polyurethane acrylate 4.85%, initiator: camphorquinone (CQ) 0.15% Solvent: Ethanol / Diethylene Glycol (1:1 mixture): 10% Leveling agent: Perenol F40: 0.3% Dispersant: Tween 80: 0.2% Flame retardant: 3.5% composite flame retardant, of which modified aluminum hydroxide (ATH): 2.1% and modified magnesium hydroxide (MDH): 1.4%. Preparation and molding: The slurry was prepared at room temperature and ≤40°C, with the remaining preparation process the same as in Example 1. The cast green body (wet film thickness 200 μm) was placed in a UV lamp box and irradiated with 405 nm UV light for 30 seconds (triggering CQ-initiated pre-curing). It was then transferred to an oven and heat-treated at 140°C for 6 hours. Finally, it was rolled at 50 MPa high pressure at room temperature to obtain a current collector with a thickness of approximately 9 ± 2 μm.
[0073] Example 4 A low-temperature sintering copper paste with thermal runaway self-protection function, the composition of which is as follows: Nano copper powder particles (D50 of 300nm): 90% Polymer matrix: Polystyrene (PS) powder: 1.5% Curing agent raw materials: 3%, of which: monomer: trimethylolpropane triacrylate (TMPTA) 2.94%, initiator: azobisisobutyronitrile (AIBN) 0.06%. Solvent: Dipropylene glycol methyl ether acetate (DPMA): 4.9% Leveling agent: BYK-354: 0.08% Dispersant: Cetyltrimethylammonium bromide (CTAB): 0.02% Flame retardant: Modified aluminum hydroxide (ATH): 0.5% Preparation and molding: The slurry was prepared at room temperature as in Example 1. After 3D printing the green body, it was placed in an atmosphere oven (N2 protection) and heat-treated at 150°C for 5 hours (to fully decompose and solidify AIBN). It was then shaped by light pressure (5MPa) to obtain a high-porosity current collector with a thickness of approximately 9±2μm.
[0074] Example 5 A low-temperature sintering copper paste with thermal runaway self-protection function, the composition of which is as follows: Nano copper powder particles (D50 of 500nm): 68% Polymer matrix: Waterborne acrylic resin dispersion (50% solids content): 12% (equivalent to 6% solids content) Curing agent raw materials: 7%, of which: monomer: polyethylene glycol dimethacrylate (PEGDMA) 6.65%, initiator: ethyl 2,4,6-trimethylbenzoylphenylphosphonate (TPO-L) 0.35%. Solvent: Deionized water: 3% Leveling agent: BYK-310: 0.4% Dispersant: Butyl phosphate: 0.1% Flame retardant: 9.5% composite flame retardant, of which: modified polycyclic phosphonitrile microspheres: 6%, modified ammonium polyphosphate (APP): 3.5%. Preparation and molding: The slurry was prepared at room temperature as in Example 1, avoiding high temperatures. After coating and molding, it was pre-cured by UV light (395nm). Subsequently, it was continuously heat-treated in a circulating hot air oven at 120°C for 10 hours to thoroughly remove moisture, complete resin curing, and promote particle bonding. A roller pressing pressure of 15MPa was used to obtain a current collector with a thickness of approximately 9±2μm. Example 6 A low-temperature sintering copper paste with thermal runaway self-protection function, its composition (by weight percentage) is as follows: Nano-copper powder particles (D50 100nm, oleylamine coated): 71% Polymer matrix: Waterborne polyurethane (PU) dispersion (40% solids content): 12.5% (equivalent to 5% PU solids) Curing agent raw materials: 4.5%, of which: monomer: polyethylene glycol diacrylate (PEGDA, Mn=400) 4.275%, initiator: azobisisobutyronitrile (AIBN) 0.225%. Solvent: α-terpineol: 7% Leveling agent: BYK-333: 0.05% Dispersant: Tween 80: 0.15% Flame retardant: Magnesium hydroxide (MDH) modified with silane coupling agent: 4.8% Preparation and molding: Drying: The raw material is vacuum dried at 80℃.
[0075] Slurry preparation: All mixing, dispersing and rolling steps are completed at room temperature or ≤40℃ water cooling conditions, and maturation is carried out at 25℃.
[0076] Molding and Pre-curing: After slit coating, immediately pre-cur by irradiation with 385nm UV light for 10 seconds.
[0077] Low-temperature heat treatment: The green body undergoes segmented heat treatment in a forced-air oven: 80℃ / 12 hours + 100℃ / 8 hours. AIBN fully decomposes at this temperature, initiating curing / crosslinking.
[0078] Post-processing: room temperature cooling, peeling, and room temperature rolling at 20MPa to obtain a current collector with a thickness of approximately 9±2μm.
[0079] Comparative Example 1 A 9μm double-sided photoelectrolytic copper foil, commonly used in high-energy-density lithium-ion batteries, was used as a comparative example.
[0080] Test method: A. Shear resistance test (testing equipment: four-probe tester): (1) I. Sample preparation and environment. Cut the current collector into a sample with a side length of not less than 20 mm, clean the surface with alcohol, and control the ambient temperature at 25±2℃ and humidity at <60%.
[0081] (2) Set up the instrument. Turn on the power and warm up for 10 minutes. Select the sheet resistance mode, set the current (1-2mA for metal foil), and calibrate with a standard plate.
[0082] (3) Place the sample flat on the insulating stage, gently place the probe so that it makes perpendicular contact with the sample, and record the reading after it stabilizes. At least 3-5 different positions should be measured on the same sample.
[0083] (4) After the test, lift the probe, clean the tip, turn off the power and cover it with the protective cap. Calculate the average value of the sheet resistance at each measuring point as the final result.
[0084] B. Thermal Trigger Response Test (Test Equipment: Programmed Temperature Rise Stage with Resistance Tester): Monitored using a programmed temperature rise stage with a resistance tester.
[0085] (1) Connect the programmed heating stage to the resistance tester through the dedicated interface and ensure that the signal line is properly grounded. Turn on the system power and preheat the instrument for 15 to 30 minutes until it is in stable working condition.
[0086] (2) Cut the composite current collector sample to fit the sample stage size (e.g., 20×20mm) and place it flat in the center of the programmed heating stage. Adjust the probe holder so that the four probes are in vertical contact with the sample surface to ensure uniform and stable contact pressure.
[0087] In the host computer software, set the heating program: starting temperature (e.g., 25℃), ending temperature (e.g., 200℃), and heating rate (e.g., 1~5℃ / min). Select continuous measurement mode and synchronously set the acquisition interval of the resistance tester (once per second).
[0088] (3) Start the heating program and simultaneously turn on the resistance tester to begin recording. The system will automatically collect temperature and resistance data synchronously and plot the resistance-temperature curve in real time. When the temperature reaches the preset target or a sudden change in resistance is observed, the data collection will stop (a resistance growth rate greater than or equal to 30% is considered a triggered thermal response). 2. Based on a negative / positive electrode capacity ratio (N / P ratio) of 1.08, the electrode sheet was coated and cut to a size of 10.2 × 6.8 × 2.2 cm. The Li(Ni) alloy was then assembled. 0.9 Co 0.05 Mn 0.05 O2 / basic electrolyte / (SiO) x2Ah pouch battery ( / Graphite).
[0089] A. Use a battery charge / discharge tester to perform constant current charge / discharge cycle tests at 1C current (3-4.25V).
[0090] B. Assemble the same 2Ah soft-pack battery as the constant current charge-discharge test, charge it to 4.25V at 0.33C, and then conduct an overcharge test at 1C. The cutoff conditions are battery explosion and fire or charging for 1 hour.
[0091] C. Assemble the same 2Ah soft-pack battery as the constant current charge-discharge test, charge it to 4.25V with a current of 0.33C, and then place it in an explosion-proof oven. The heating rate is 5℃ / min, and the temperature is raised to 200℃. Keep it at this temperature for 1 hour and record the battery temperature when the battery thermally runs away. The standard for not running away is that the battery does not catch fire or explode.
[0092] D. Assemble the same 2Ah soft-pack battery as the constant current charge-discharge test, charge it to 4.25V at 0.33C, and then place it in an explosion-proof oven. Use a 5mm steel needle to pierce the center point of the battery at a speed of 0.1mm / s and leave it for 5 minutes.
[0093] Table 1
[0094] The thermal response thresholds of Examples 1-6 were concentrated in the range of 118-174℃, far lower than that of Comparative Example 1. In the early stage of thermal runaway (<200℃), the current collector actively cut off the local conductive path, blocking the continuous accumulation of current and heat. In the overcharge test, the batteries using the thermal runaway protection current collector only bulged and did not catch fire or explode; the highest temperature in the needle penetration test dropped significantly to 209-331℃, far lower than the >600℃ of the comparative example, and none of them caught fire. In the needle penetration test, Examples 3, 4, and 5 even reached the "smokeless" level, and in the oven heating test, Examples 1, 3, 4, 5, and 6 did not trigger thermal runaway. This indicates that the uniformly dispersed flame retardant decomposes and absorbs heat simultaneously at high temperatures, capturing free radicals and effectively inhibiting the combustion reaction of the electrolyte. Even after physical circuit breaking, a small amount of heat remains, and the flame retardant can suppress the consequences of an accident from fire and explosion to only bulging or smoke, or even smokeless, achieving excellent safety performance.
[0095] The initial sheet resistance of Examples 1-6 was 0.03-0.09 Ω / sq, and the capacity retention after 500 cycles at 1C was 88.5%-92.8%, which was basically the same as that of Comparative Example 1 (92.0%). The conductive network constructed by low-temperature sintering and rolling provided the same conductivity and cycle stability as conventional copper foil at room temperature, demonstrating that the introduction of safety features did not sacrifice the electrochemical performance of the battery.
[0096] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified.
[0097] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0098] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.
Claims
1. A current collector characterized by comprising: include: Polymer matrix; The nano-copper powder particles are dispersed in the polymer matrix and are electrically connected to at least some of the adjacent nano-copper powder particles.
2. The current collector of claim 1, wherein The electrical connection between adjacent copper nanoparticles satisfies at least one of the following conditions: There are sintered necks between adjacent copper nanoparticles; The surfaces of adjacent copper nanoparticles are in contact.
3. The current collector of claim 1, wherein The nano-copper powder particles achieve effective electrical connection; the electrical connection refers to the sheet resistance of the current collector being less than 100mΩ / □.
4. The current collector according to claim 1, characterized in that, It also includes at least one of the following: A flame retardant, wherein the flame retardant is dispersed in the polymer matrix; A leveling agent, wherein the leveling agent is dispersed in the polymer matrix; A dispersant, wherein the dispersant is dispersed in the polymer matrix.
5. The current collector according to claim 4, characterized in that, At least one of the following conditions must be met: The nano-copper powder particles are spherical or flake-shaped. The polymer matrix includes at least one of polymethyl methacrylate, polycarbonate, polystyrene, ethyl cellulose, polyvinyl chloride, polyacrylamide, polyphosphazene, polysiloxane, polylactic acid, polyethylene terephthalate, polyethylene, polyurethane, polypropylene, acrylonitrile-butadiene-styrene, polyethylene oxide, polyaniline, polypyrrole, polythiophene, polyacetylene, and poly(3,4-ethylenedioxythiophene). The leveling agent includes at least one of BYK-333, BYK-306, BYK-307, BYK-310, BYK-354, BYK-3609, and PerenolF40; The dispersant includes at least one of polyvinylpyrrolidone, sodium polyacrylate, Tween 80, cetyltrimethylammonium bromide, and butyl phosphate. The flame retardant includes unmodified inorganic flame retardant filler and inorganic flame retardant filler with surface modified by silane coupling agent and / or titanate coupling agent. The unmodified inorganic flame retardant filler includes at least one of polyphosphazene, polycyclic phosphazene, aluminum hydroxide, magnesium hydroxide, and ammonium polyphosphate.
6. A method for preparing the current collector according to any one of claims 1 to 5, characterized in that, include: A copper paste is prepared, wherein the copper paste contains nano-copper powder particles, a polymer, and a solvent; The copper paste is shaped and cured to form a green blank; The green blank is sintered; The sintered blank is rolled to obtain a current collector.
7. The preparation method according to claim 6, characterized in that, The copper paste also includes at least one of the following: curing agent raw material, leveling agent, dispersant, and flame retardant, wherein the curing agent raw material includes monomer and initiator.
8. The preparation method according to claim 7, characterized in that, At least one of the following conditions must be met: The monomers include at least one of polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, pentaerythritol tetraacrylate, trimethylolpropane triacrylate, epoxy acrylate, 1,6-hexanediol diacrylate, and polyurethane acrylate. The initiator includes at least one of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, benzoyl peroxide, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphine, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, (2,4,6-trimethylbenzoyl)bis(p-tolyl)phosphine oxide, 2-hydroxy-2-methylphenylacetone, and camphorquinone; The solvent includes at least one of ethylene glycol, diethylene glycol, glycerol, polyethylene glycol, ethanol, methanol, isopropanol, dipropylene glycol methyl ether acetate, terpineol derivatives, and glyceryl tripalmitate. The sintering temperature is 100℃-150℃; The sintering time is 0.5h - 24h; The pressure of the roller is 1 MPa-50 MPa.
9. The preparation method according to claim 7, characterized in that, The copper paste, by weight, comprises: The nano-copper powder particles are 70-95 parts by weight; The polymer is 1-10 parts by weight; The curing agent raw material is 1 part by weight to 10 parts by weight, wherein the weight ratio of the initiator to the monomer is 0.5:100 to 4:100; The solvent is 1 to 10 parts by weight; The leveling agent is used in amounts of 0.01 to 0.5 parts by weight. The dispersant is used in amounts of 0.01 to 0.5 parts by weight. The flame retardant is 0.1 to 5 parts by weight.
10. A lithium-ion battery, characterized in that, The current collector includes the current collector as described in any one of claims 1 to 5, or the current collector obtained by any one of the preparation methods according to claims 6 to 9.