Negative current collector for sodium-ion batteries, negative electrode for sodium-ion batteries, and sodium-ion batteries

By employing a porous metal anode current collector in sodium-ion batteries and controlling the aspect ratio and porosity of the metal skeleton, the problem of reduced capacity retention caused by the expansion and contraction of the anode active material was solved, thereby improving the stability and charge/discharge performance of the battery.

CN123120750APending Publication Date: 2026-11-17TOYOTA JIDOSHA KK
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202610487361.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-04-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

During the charging and discharging process, the capacity retention rate of the negative electrode current collector in existing sodium-ion batteries decreases due to the expansion and contraction of the alloy-based negative electrode active material. In particular, the connection part of the structural unit of the metal porous body is cut off, which affects the movement of charge carrier ions.

Method used

A porous metal body is used as the negative electrode current collector. The ratio of the thickness of the metal skeleton to the average pore diameter is in the range of 0.8 to 1.5. The alloy-based negative electrode active material is formed on the metal skeleton. By controlling the aspect ratio of the metal skeleton to 0.8 to 1.2, multiple continuous structural units are formed, which suppresses the influence of the expansion and contraction of the negative electrode active material on the porous metal body.

Benefits of technology

It effectively suppressed the decrease in battery capacity retention, improved the stability of the negative electrode current collector and the charge and discharge performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120750A_ABST
    Figure CN123120750A_ABST
Patent Text Reader

Abstract

The negative electrode current collector for a sodium-ion battery comprises a porous metal body. The porous metal body has a plurality of continuous structural units. Each structural unit has a metal framework as a polyhedron and pores existing within the metal framework, and the thickness of the negative electrode current collector is in a ratio of 0.8 to 1.5 to the average pore diameter of the pores. The negative electrode for a sodium-ion battery comprises the negative electrode current collector of this disclosure and a negative electrode active material layer, and the negative electrode active material layer comprises an alloy-based negative electrode active material. The negative electrode active material layer comprises an alloy-based negative electrode active material and is formed on the metal framework. The sodium-ion battery has the negative electrode of this disclosure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to a negative current collector for sodium-ion batteries, a negative electrode for sodium-ion batteries, and sodium-ion batteries. Background Technology

[0002] As disclosed in Japanese Patent Application Publication Nos. 2016-134376 and 2015-041455, a negative electrode for sodium-ion batteries has been developed.

[0003] Japanese Patent Application Publication No. 2016-134376 discloses a porous metal body with a three-dimensional mesh-like structure and a hollow framework as a current collector for the negative electrode of a sodium-ion battery. In this patent application, the porous metal body has multiple unit-shaped pores surrounded by a metal framework. A large amount of negative electrode active material is retained within the porous metal body, and the pores are effectively maintained. Furthermore, these pores absorb the expansion and contraction of Sn, the negative electrode active material, during charging and discharging, thereby increasing capacity.

[0004] Furthermore, Japanese Patent Application Publication No. 7-111150 discloses a material in which carbon powder is filled in foamed metal as a negative electrode for alkali metal ion batteries such as sodium ion batteries. In Japanese Patent Application Publication No. 7-111150, foamed metal is used as the current collector of the carbon electrode. As a result, the carbon powder is supported in the three-dimensional network of foamed metal, and even if the volume change of carbon is caused by charging and discharging, it can be prevented from falling off or peeling off from the surface of the current collector. Summary of the Invention

[0005] It is known that phosphorus and other alloy-based negative electrode active materials used as negative electrode active materials in sodium-ion batteries expand and contract with the charging and discharging of the battery.

[0006] There is room for improvement in the negative electrode current collector for sodium-ion batteries containing metal porous bodies, from the viewpoint of suppressing the decrease in capacity retention caused by the expansion and contraction of the negative electrode active material during battery charging and discharging.

[0007] This disclosure provides a negative current collector for a sodium-ion battery capable of suppressing the reduction in battery capacity retention, a negative electrode comprising such a negative current collector, and a sodium-ion battery comprising such a negative electrode.

[0008] The negative electrode current collector for a sodium-ion battery in the first embodiment may comprise a metal porous body, the metal porous body may have a continuous plurality of structural units, the structural units may have a metal skeleton as a polyhedron and pores existing inside the metal skeleton, and the ratio of the thickness of the negative electrode current collector to the average pore diameter of the pores may be 0.8 to 1.5.

[0009] In the sodium-ion battery negative electrode current collector of the first embodiment, the aspect ratio of at least one face of the metal skeleton is 0.8 to 1.2.

[0010] The second type of sodium-ion battery negative electrode may include the sodium-ion battery negative electrode current collector and negative electrode active material layer described in the first type, and the negative electrode active material layer may include alloy-based negative electrode active material and be formed on the metal skeleton.

[0011] In the second type of sodium-ion battery negative electrode, the metal forming the metal framework can be nickel, and the alloy-based negative electrode active material can be phosphorus.

[0012] The third type of sodium-ion battery may include the negative electrode for sodium-ion batteries described in the second type.

[0013] According to this disclosure, it is possible to provide a negative electrode current collector for a sodium-ion battery that can suppress the reduction of battery capacity retention, a negative electrode comprising such a negative electrode current collector, and a sodium-ion battery comprising such a negative electrode. Attached Figure Description

[0014] The features, advantages, and technical and industrial significance of exemplary embodiments of the present invention will now be described with reference to the accompanying drawings, wherein like symbols denote like elements, wherein:

[0015] Figure 1A This is a schematic cross-sectional view showing an example of the negative electrode of the sodium-ion battery of this disclosure before charging;

[0016] Figure 1B This is a schematic cross-sectional view showing an example of the negative electrode of the sodium-ion battery of this disclosure after charging;

[0017] Figure 2 It is a schematic diagram illustrating the extent of volume change of a negative electrode for a sodium-ion battery during charging, within the scope of this disclosure, of the aspect ratio of at least one face of the metal skeleton.

[0018] Figure 3A This is a schematic cross-sectional view of an example of a conventional sodium-ion battery negative electrode before charging;

[0019] Figure 3B This is a schematic cross-sectional view showing an example of a conventional sodium-ion battery negative electrode after charging;

[0020] Figure 4 This is a schematic diagram illustrating the extent of volume change of a negative electrode for a sodium-ion battery during charging, outside the scope of this disclosure, representing the aspect ratio of at least one face of the metal skeleton; and

[0021] Figure 5This is a graph showing the relationship between the number of cycles and capacity retention in the batteries of Example 1 and Comparative Example 1. Detailed Implementation

[0022] The embodiments of this disclosure will now be described in detail. It should be noted that this disclosure is not limited to the embodiments described below, and various modifications can be made within the scope of the disclosure.

[0023] Negative current collector for sodium-ion batteries

[0024] The negative electrode current collector for sodium-ion batteries disclosed herein comprises a porous metal body. Here, the porous metal body has a plurality of continuous structural units. Each structural unit has a metal framework as a polyhedron and pores existing within the metal framework, and the thickness of the negative electrode current collector is in a ratio of 0.8 to 1.5 to the average pore diameter of the pores.

[0025] The inventors of this application have discovered that the capacity retention of batteries having a conventional metal porous negative electrode current collector, as disclosed in Japanese Patent Application Publication No. 2016-134376, is insufficient. As a reason, without intending to be bound by any theory, we speculate as follows: That is, when using an alloy-based negative electrode active material that expands and contracts with the charging and discharging of the battery as the negative electrode active material, such as… Figure 3B As illustrated, due to the expansion of the negative electrode active material, the connecting portions of the structural units in a porous metal mass are sometimes truncated. This is believed to be because, as will be explained later, the connecting portions have voids, and particularly because multiple consecutive structural units are layered, thus stress is easily applied in the direction in which the connecting portions are truncated. It should be noted that... Figure 3A This indicates the state before charging. Figure 3B This indicates the state after charging. It is believed that by trunculating the connection in this way, the movement of sodium ions, which are charge carriers, is suppressed, thus reducing the battery's capacity retention.

[0026] In contrast, the inventors of this application discovered that the negative current collector of this disclosure can suppress the truncation of the connecting portions of the structural units of the porous metal. As a reason, they are not intended to be bound by any theory, but rather speculate as follows: That is, in the negative current collector of this disclosure, the ratio of the thickness of the negative current collector to the average pore diameter is within a specified range. That is, as... Figure 1A and Figure 1B As illustrated, by assuming a single layer of continuous structural units 10a, even with gaps 11a at the connecting portions, it is difficult to apply stress in the direction of segmentation. Consequently, it is believed that the decrease in battery capacity retention can be suppressed. It should be noted that... Figure 1A This indicates the state before charging. Figure 1B This indicates the state after charging.

[0027] The following describes the elements that constitute the negative electrode current collector for sodium-ion batteries disclosed herein.

[0028] metal porous body

[0029] The negative electrode current collector for sodium-ion batteries disclosed herein comprises a metallic porous body 10. For example... Figure 1A As illustrated, the negative current collector can be made of a porous metal 10, in which case the same symbol "10" is sometimes used to denote both "negative current collector" and "porous metal".

[0030] Structural unit

[0031] like Figure 1A As illustrated, the porous metal 10 has a plurality of continuous structural units 10a. The number of structural units is not particularly limited.

[0032] Each structural unit 10a can be interconnected via the metal frame 11 described later. For example... Figure 1A As illustrated in the enlarged portion, the connecting portion caused by the metal skeleton 11 may have a gap 11a. The gap 11a can be formed by removing the foamed polyurethane as described later. The structural units 10a can be connected through at least one face of the metal skeleton 11, i.e., an opening formed by the metal skeleton 11.

[0033] Metal skeleton

[0034] like Figure 1A As illustrated, structural unit 10a has a metal framework 11 that serves as a polyhedron. The number of faces constituting the polyhedron is not particularly limited as long as there are holes of a specified size described later inside the metal framework.

[0035] The aspect ratio of at least one face of the metal frame can be 0.5 to 1.5 or 0.8 to 1.2. The aspect ratio can be 0.5 or more, 0.6 or more, 0.7 or more, 0.8 or more, 0.9 or more, or 1.0 or more, and can also be 1.5 or less, 1.4 or less, 1.3 or less, 1.2 or less, 1.1 or less.

[0036] Here, Figure 4 This is a schematic diagram illustrating the extent of volume change of a negative electrode for a sodium-ion battery with an aspect ratio outside the scope of this disclosure, as the battery is charged. Figure 4 The diagram to the left of the arrow shows the state of the negative electrode before charging, and the diagram to the right of the arrow shows the state of the negative electrode after charging. If the aspect ratio is outside the range described above, the stress accompanying the expansion of the negative electrode active material layer 20 (described later) in at least one face of the metal frame 11 will concentrate near the vertices of the polygon, thereby sometimes causing the negative electrode current collector 10 to increase in volume excessively.

[0037] Here, Figure 2 This is a schematic diagram illustrating the extent of volume change of a negative electrode for a sodium-ion battery with the aforementioned aspect ratio within the scope of this disclosure, as the battery is charged. Figure 2 The diagram to the left of the arrow shows the state of the negative electrode before charging, and the diagram to the right of the arrow shows the state of the negative electrode after charging. Compared to the aspect ratios described above, which are outside the scope of this disclosure, when the aspect ratio is within the aforementioned range, stress concentration as described above can be suppressed, thereby suppressing excessive volume increase of the negative electrode current collector 10. As a result, the decrease in battery capacity retention can be effectively suppressed.

[0038] Regarding this disclosure, "aspect ratio" refers to the ratio of the length of the negative current collector in the face direction to the length in the thickness direction of the negative current collector with respect to at least one face of the metal frame. Additionally, "aspect ratio" can refer to the value when the negative current collector is not pressed.

[0039] The aspect ratio can be measured using a VK-9700 laser microscope manufactured by KEYENCE.

[0040] The shape of at least one face of the metal frame is not particularly limited; for example, it can be a polygon. Examples of polygons include those with 3 to 10 vertices. The shape of this face can be the same or different across all faces.

[0041] There are no particular limitations on the metal that forms the metallic framework, as long as it is not alloyed with sodium. Examples of such metals include aluminum, aluminum alloys, copper, copper alloys, nickel, nickel alloys, iron, cobalt, chromium, and silver.

[0042] empty hole

[0043] like Figure 1A As illustrated, structural unit 10a has a cavity 12 inside the metal frame 11.

[0044] The average pore diameter can be 100μm–500μm, 100μm–400μm, 100μm–300μm, or 150μm–250μm. Alternatively, the average pore diameter can be greater than 100μm, greater than 150μm, or greater than 200μm, or less than 500μm, less than 400μm, less than 350μm, less than 300μm, less than 250μm, or less than 200μm. This facilitates the formation of a continuous series of multiple structural units forming a single-layer negative electrode current collector, effectively suppressing the decrease in battery capacity retention.

[0045] Regarding this disclosure, the average aperture diameter of the pore can refer to the value under conditions where the negative current collector is not suppressed.

[0046] The average pore diameter can be measured using a VK-9700 laser microscope manufactured by KEYENCE.

[0047] There is no specific limit to the porosity.

[0048] Thickness of negative current collector

[0049] The thickness of the negative current collector can be 80μm to 750μm, 100μm to 500μm, 100μm to 400μm, 100μm to 300μm, or 150μm to 250μm. This thickness can be 80μm or more, 100μm or more, 150μm or more, or 200μm or more; alternatively, it can be 750μm or less, 500μm or less, 400μm or less, 350μm or less, 300μm or less, 250μm or less, or 200μm or less. Therefore, the negative current collector can be easily manufactured without pressing. From the viewpoint of ensuring an appropriate amount of porosity and setting the aspect ratio of at least one face of the metal skeleton within the range of this disclosure, it is suitable not to press the negative current collector.

[0050] The value of the thickness of the negative current collector / the average pore diameter of the pore

[0051] The ratio of the thickness of the negative electrode current collector to the average pore diameter is 0.8 to 1.5. If this ratio is within the above range, multiple consecutive structural units can be set as a single layer, which can suppress the decrease in the capacity retention rate of the battery.

[0052] This ratio can be 0.8–1.3 or 0.9–1.2. It can also be above 0.8, 0.9, or 1.0, or below 1.4, 1.3, 1.2, 1.1, or 1.0. Therefore, it is easy to design multiple consecutive structural units as a single layer, effectively suppressing the decrease in battery capacity retention.

[0053] Other structures

[0054] like Figure 1A As illustrated, the current collector foil can also be configured to sandwich the negative current collector 10.

[0055] Manufacturing method of negative electrode current collector for sodium-ion batteries

[0056] The negative electrode current collector for sodium-ion batteries of the present invention can be manufactured by a method including the following steps:

[0057] Polyurethane foam is prepared by mixing polyols, polyisocyanates and water, wherein the polyurethane foam has polar functional groups derived from polyols.

[0058] The metal is attached to the polyurethane foam to form a metal skeleton; and

[0059] Remove the polyurethane foam.

[0060] Preparation of polyurethane foam

[0061] This method involves mixing a polyol, a polyisocyanate, and water, followed by foaming and curing to produce a foamed polyurethane. Here, the foamed polyurethane has polar functional groups derived from the polyol. This allows for adjustment of the surface tension of the foam, i.e., the gas-liquid interface, generated by the reaction of the polyisocyanate with water, thereby enabling control of the average pore size to a specified value. Examples of polar functional groups include ester groups, ketone groups, nitrile groups, nitro groups, or sulfonyl groups.

[0062] There are no particular restrictions on the conditions for mixing the components. For example, the mixing temperature can be 50℃~150℃ or 80℃~120℃.

[0063] As a polyol, there are no particular limitations as long as it has polar functional groups.

[0064] As a polyisocyanate, there are no particular limitations.

[0065] Formation of the metal framework

[0066] The method involves attaching metal to polyurethane foam to form a metal skeleton.

[0067] Regarding metals, please refer to the above records.

[0068] There are no particular limitations on the method for attaching metal to polyurethane foam; an example based on electroplating can be given.

[0069] Removal of polyurethane foam

[0070] This method involves removing the foamed polyurethane. This allows for the fabrication of a porous metal body with pores formed within a metal framework.

[0071] Heating can be cited as an example of a method for removing polyurethane foam. The heating temperature and time are not particularly limited as long as the polyurethane foam can be removed.

[0072] Negative electrode for sodium-ion batteries

[0073] like Figure 1A As illustrated, the negative electrode 1 for a sodium-ion battery includes the negative electrode current collector 10 and the negative electrode active material layer 20 of this disclosure. Here, the negative electrode active material layer 20 includes an alloy-based negative electrode active material and is formed on a metal framework 11.

[0074] Alloy-based negative electrode active materials expand and contract during battery charging and discharging. In contrast, such as... Figure 1A As illustrated, in the negative electrode 1 of this disclosure, a negative electrode active material layer 20 comprising an alloy-based negative electrode active material is formed on a metal framework 11 of a porous metal body 10 that serves as a negative electrode current collector. Thus, the pores 12 within the metal framework 11 can absorb the aforementioned expansion and contraction.

[0075] Negative current collector for sodium-ion batteries

[0076] Regarding the negative electrode current collector for sodium-ion batteries disclosed herein, please refer to the above description.

[0077] Negative electrode active material layer

[0078] like Figure 1A As illustrated, the negative electrode active material layer 20 contains an alloy-based negative electrode active material and is formed on the metal skeleton 11.

[0079] From the viewpoint of reducing the impact of expansion and contraction of the negative electrode active material during battery charging and discharging, the thickness of the negative electrode active material layer can be 0.1 μm to 10 μm, or 0.5 μm to 5 μm. This thickness can be greater than 0.1 μm, greater than 0.5 μm, or greater than 1 μm, and can also be less than 10 μm, less than 5 μm, or less than 1 μm.

[0080] Alloy-based negative electrode active materials

[0081] Regarding this disclosure, "alloy-based negative electrode active material" refers to a material capable of forming an alloy with sodium ions, which are charge carrier ions, and thereby expanding and contracting during battery charging. There are no particular limitations on the alloy-based negative electrode active material; for example, it can be phosphorus. Red phosphorus is exemplified as phosphorus. Red phosphorus can be appropriately ball-milled.

[0082] There is no particular limitation on the content of alloy-based negative electrode active material in the negative electrode active material layer; it can be appropriately set considering factors such as the desired battery capacity.

[0083] The negative electrode active material layer may include negative electrode active materials other than alloy-based negative electrode active materials, or it may not include them.

[0084] The negative electrode active material layer may further contain components other than the negative electrode active material. Examples of such components include conductive additives and binders.

[0085] Conductive additives

[0086] The conductive additive is not particularly limited and can be, for example, a carbon material or a metallic material. Examples of carbon materials include carbon black such as acetylene black, Ketjen black, furnace black, and thermal cracking carbon black; carbon fibers such as carbon nanotubes (CNTs) and vapor-grown carbon fibers (VGCF); graphite; hard carbon; and coke. Examples of metallic materials include Fe, Cu, Ni, and Al. The conductive additive can be one or more of the above-mentioned materials.

[0087] There is no particular limitation on the content of conductive additives in the negative electrode active material layer; it can be appropriately set considering the desired conductivity, etc.

[0088] adhesives

[0089] Examples of adhesives include fluorinated adhesives such as polyvinylidene fluoride (PVdF) adhesives and polytetrafluoroethylene (PTFE) adhesives; rubber-based adhesives such as styrene-butadiene rubber (SBR) adhesives; olefin-based adhesives such as polypropylene (PP) adhesives and polyethylene (PE) adhesives; cellulose-based adhesives such as carboxymethyl cellulose (CMC) adhesives; and polyacrylic acid (PAA) adhesives. The adhesive may be one or more of the above-mentioned materials.

[0090] There is no particular limitation on the content of binder in the negative electrode active material layer; it can be set appropriately considering the desired adhesion, etc.

[0091] Manufacturing method of negative electrode for sodium-ion battery

[0092] The negative electrode for sodium-ion batteries can be manufactured by a method including the following steps:

[0093] The negative electrode current collector for sodium-ion batteries is manufactured using the method described above.

[0094] Provides negative electrode slurry containing alloy-based negative electrode active material and dispersion medium; and

[0095] The negative electrode slurry is coated onto the negative electrode current collector, and then dried to remove the dispersion medium.

[0096] Manufacturing of negative electrode current collectors for sodium-ion batteries

[0097] The method includes manufacturing a negative electrode current collector for sodium-ion batteries using the method described above.

[0098] Supply of negative electrode mixture slurry

[0099] The method includes providing a negative electrode slurry containing an alloy-based negative electrode active material and a dispersion medium.

[0100] Regarding this disclosure, "negative electrode mixture" refers to a composition capable of forming a negative electrode active material layer by directly or further containing other components. Additionally, regarding this disclosure, "negative electrode mixture slurry" refers to a slurry that, in addition to the "negative electrode mixture," also contains a dispersion medium, thereby enabling coating and drying to form a negative electrode active material layer.

[0101] For information on alloy-based anode active materials, please refer to the above description.

[0102] As a dispersion medium, there are no particular limitations as long as it can disperse the active material of the alloy-based negative electrode.

[0103] The negative electrode slurry may further contain components other than the alloy-based negative electrode active material. For details regarding such components, please refer to the above description. In this case, there are no particular limitations on the dispersion medium, as long as it can disperse the negative electrode active material and the conductive additive, and disperse or dissolve the binder.

[0104] As a dispersion medium, it can be a material commonly used as a dispersion medium for negative electrode mixture slurries, such as N-methyl-2-pyrrolidone (NMP).

[0105] Drying and removal of dispersion media

[0106] The method involves coating a negative electrode slurry onto a negative electrode current collector and then drying and removing the dispersion medium.

[0107] There are no particular limitations on the method for drying and removing the dispersion medium; conventional methods can be used.

[0108] Sodium-ion batteries

[0109] The sodium-ion battery disclosed herein has a negative electrode for use in sodium-ion batteries as described above. Regarding the negative electrode for sodium-ion batteries as described above, please refer to the above description.

[0110] The sodium-ion battery disclosed herein may sequentially include a negative electrode, an electrolyte layer, a positive electrode active material layer, and a positive electrode current collector.

[0111] The sodium-ion battery disclosed herein can be a solid-state battery or a liquid battery, particularly a liquid battery.

[0112] The electrolyte layer of a liquid battery can contain an electrolyte containing sodium ions.

[0113] Regarding this disclosure, a "solid-state battery" refers to a battery that contains at least a solid electrolyte as an electrolyte; therefore, a solid-state battery can also contain a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. Furthermore, a solid-state battery can also be an all-solid-state battery, that is, a battery in which only a solid electrolyte is contained as an electrolyte. Therefore, in the case of the sodium-ion battery of this disclosure being a solid-state battery, the electrolyte layer can contain a solid electrolyte having sodium ions.

[0114] The sodium-ion battery disclosed herein can be a secondary battery.

[0115] Sodium-ion batteries can be shaped like coins, laminated (pouch), cylindrical, or square.

[0116] Sodium-ion batteries can be manufactured by molding the above layers using dry or wet methods.

[0117] The sodium-ion battery disclosed herein can be applied, for example, to at least one type of vehicle selected from hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), and battery electric vehicles (BEV).

[0118] The elements constituting the battery of this disclosure will now be described. The following examples illustrate the case where the battery of this disclosure is a liquid battery.

[0119] negative electrode

[0120] Regarding the negative electrode, please refer to the above description.

[0121] Electrolyte layer

[0122] The electrolyte layer can be formed by impregnating the insulating element with electrolyte.

[0123] Isolation component

[0124] As a separator, there are no particular limitations as long as it has the function of electrically separating the negative electrode active material layer from the positive electrode active material layer. Examples of separators include porous sheets made of resins such as polyethylene (PE), polypropylene (PP), polyester, cellulose, and polyamide, as well as porous insulating materials such as non-woven fabrics and glass fiber non-woven fabrics, or combinations thereof.

[0125] electrolyte

[0126] Electrolytes can contain sodium salts and non-aqueous solvents.

[0127] As a sodium salt, there are no particular limitations. For example, it can be inorganic sodium salts such as NaPF6, NaBF4, NaClO4, and NaAsF6; as well as organic sodium salts such as NaCF3SO3, NaN(CF3SO2)2, NaN(C2F5SO2)2, NaN(FSO2)2, and NaC(CF3SO2)3, or combinations thereof.

[0128] The non-aqueous solvent is not particularly limited as long as it is a solvent capable of dissolving sodium salts. The non-aqueous solvent may be a high dielectric constant solvent, a low dielectric constant solvent, or a combination thereof. Examples of the high dielectric constant solvent include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC); γ-butyrolactone; sulfolane; N-methyl-2-pyrrolidone (NMP); 1,3-dimethyl-2-imidazolidinone (DMI); or a combination thereof. Examples of the low dielectric constant solvent include chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC); acetates such as methyl acetate and ethyl acetate; ethers such as 2-methyltetrahydrofuran; or a combination thereof.

[0129] Positive electrode active material layer

[0130] The positive electrode active material layer contains a positive electrode active material, and may optionally contain a conductive auxiliary agent, a binder, and the like.

[0131] Positive electrode active material

[0132] The positive electrode active material is not particularly limited as long as it is a substance that exhibits a high potential relative to the negative electrode active material. Examples of such positive electrode active materials include Na-containing oxides such as layered active materials, spinel-type active materials, and olivine-type active materials. Specifically, NaFeO2, NaNiO2, NaCoO2, NaMnO2, NaVO2, Na(Ni X Mn 1-X )O2 (0<X<1), Na(Fe X Mn 1-X )O2 (0<X<1), NaVPO4F, Na2FePO4F, and Na3V2(PO4)3.

[0133] The content of the positive electrode active material in the positive electrode active material layer is not particularly limited, and can be appropriately set in consideration of the desired battery capacity and the like.

[0134] The shape and size of the positive electrode active material are not particularly limited.

[0135] Conductive auxiliary agent and binder

[0136] For the conductive auxiliary agent and the binder, reference may be made to the above description.

[0137] Positive electrode current collector layer

[0138] Examples of the material for the positive electrode current collector layer include SUS, aluminum, nickel, iron, titanium, and carbon.

[0139] Shape and thickness of each layer

[0140] The shape of each of the above layers is not particularly limited; for example, it can be a sheet with a generally flat surface.

[0141] The thickness of each of the above layers is not particularly limited and can be adjusted appropriately according to the battery structure.

[0142] Other components

[0143] The sodium-ion battery disclosed herein may include a battery casing housing the aforementioned layers, and terminals connected to the current collector layer, etc. These may be materials commonly used in sodium-ion batteries.

[0144] Example 1

[0145] Fabrication of negative current collector

[0146] Production of polyurethane foam

[0147] Polyurethane foam is prepared by mixing polyols with ester groups and polyisocyanates at 100°C.

[0148] Formation of the metal framework

[0149] A metallic skeleton is formed on the surface of the obtained polyurethane foam by electroplating nickel (Ni).

[0150] Removal of polyurethane foam

[0151] A Ni-coated polyurethane foam is heated and then removed to fabricate a porous metal body. The resulting porous metal body has an average pore size of 190 μm, comprises multiple continuous structural units in a single layer, and has a thickness of 200 μm. At least one face of the metal framework has an aspect ratio of 1.0. The resulting porous metal body is used as a negative electrode current collector.

[0152] The average pore diameter and aspect ratio were measured using a VK-9700 laser microscope manufactured by KEYENCE.

[0153] Negative electrode fabrication

[0154] For red phosphorus, ball milling was performed at 500 rpm for 24 hours. The ball-milled red phosphorus, CNTs, and PVdF were weighed sequentially at a mass ratio of 93:1:6 and dispersed in N-methyl-2-pyrrolidone (NMP) to prepare a negative electrode slurry. The resulting negative electrode slurry was coated onto a porous metal body, dried to remove NMP, forming a negative electrode active material layer on the metal framework of the porous metal body. The thickness of the negative electrode active material layer was 1 μm. Then, it was further vacuum dried overnight at 120 °C to prepare the sample electrode.

[0155] Evaluation of battery manufacturing

[0156] As the electrolyte, 1M NaPF6 (EC:DEC = 1:1 (volume ratio), FEC 3% by mass) was used. Sodium foil was used as the positive electrode. An evaluation battery was constructed from these and the resulting negative electrode.

[0157] evaluate

[0158] Capacity maintenance rate

[0159] The capacity retention rate was evaluated as follows: The evaluation battery was subjected to three charge-discharge cycles at a voltage range of 0.01–2.0V and a rate of 0.1C in a constant temperature bath at 25°C, followed by repeated fast charging at 2C. The initial capacity (before charging) and the capacity after the above charge-discharge cycle were measured respectively. The ratio of the capacity from the first to the tenth cycle to the initial capacity was calculated and used as the capacity retention rate. The results are presented below. Figure 5 .

[0160] Comparative Example 1

[0161] Except for using a polyol without ester groups, the negative electrode current collector was fabricated in the same manner as in Example 1. This negative electrode current collector has an average pore size of 65 μm, consists of multiple continuous structural units with a 3-layer structure, a thickness of 200 μm, and the thickness of the negative electrode current collector is in a ratio of 3.1 to the average pore size. Furthermore, following the same procedure as in Example 1, an evaluation battery was obtained and evaluated. The results are shown below. Figure 5 .

[0162] like Figure 5 As shown, the ratio of the thickness of the negative electrode current collector to the average aperture of the pores is within the scope of this disclosure, that is, in the battery of the embodiment of the negative electrode current collector of this disclosure having a single layer of continuous structural units, the capacity retention rate is high.

Claims

1. A negative electrode current collector for a sodium-ion battery, comprising a porous metal body, The porous metal body has multiple continuous structural units. The structural unit has a metal skeleton as a polyhedron and hollow spaces existing inside the metal skeleton, and The thickness of the negative current collector is in the ratio of 0.8 to 1.5 to the average diameter of the pore.

2. The negative electrode current collector for a sodium-ion battery according to claim 1, wherein, The aspect ratio of at least one face of the metal skeleton is 0.8 to 1.

2.

3. A negative electrode for a sodium-ion battery, comprising the negative electrode current collector and the negative electrode active material layer as described in claim 1 or 2, and The negative electrode active material layer contains an alloy-based negative electrode active material and is formed on the metal skeleton.

4. The negative electrode for a sodium-ion battery according to claim 3, wherein, The metal forming the metal skeleton is nickel, and the alloy system negative electrode active material is phosphorus.

5. A sodium-ion battery comprising the negative electrode for a sodium-ion battery as described in claim 3.

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery

    JP1995111150A

  • Negative electrode active material for sodium ion secondary battery, negative electrode for sodium ion secondary battery using the same, and sodium ion secondary battery

    JP2015041455A

  • Negative electrode for sodium ion secondary battery and sodium ion secondary battery

    JP2016134376A