Magnetic field assisted isotropic proton exchange membrane, method of making and battery
By introducing polyvinylpyrrolidone to coat gadolinium oxide and perfluorosulfonic acid into the proton exchange membrane and combining it with magnetic field-assisted technology, a directional nanoframework network was constructed, which solved the problem of performance degradation of the proton exchange membrane at high temperatures, improved proton conduction efficiency and mechanical stability, and extended the service life of the fuel cell.
Patent Information
- Application Number
- CN202611280473.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing proton exchange membranes are prone to water loss at high temperatures, leading to performance degradation, insufficient strength, inadequate proton conductivity, and poor hydrolysis stability, which affects the service life and safety of fuel cells.
A magnetic field-assisted isotropic proton exchange membrane was prepared by introducing polyvinylpyrrolidone to coat gadolinium oxide and perfluorosulfonic acid into the proton exchange membrane to form an ordered structure. A directional nanoframework network was constructed using magnetic field-assisted drying and curing technology to optimize the structural design of the proton conduction channel.
It improves the proton conduction efficiency, mechanical stability, and hydrolytic stability of the proton exchange membrane, reduces transmission resistance, extends the service life of the fuel cell, and enhances safety.
Smart Images

Figure CN123120798A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, specifically to a magnetic field-assisted isotropic proton exchange membrane, its preparation method, and a battery. Background Technology
[0002] The development of proton exchange membranes (PEMs) has undergone several generations of evolution. The earliest fuel cells used polystyrene sulfonate membranes, but these had poor stability. It wasn't until the 1960s, with the successful application of DuPont's Nafion® perfluorosulfonate membrane in the aerospace field, that the practical application of PEM fuel cells truly began. These PEMs possess a polytetrafluoroethylene (PTFE) backbone providing mechanical and chemical stability, while the sulfonic acid groups at the end of the side chains are responsible for proton conduction. Their overall performance is excellent, and they remain the benchmark for research and application to this day. Continued in-depth research on PEMs is not only key to overcoming technological bottlenecks in fuel cells but also a crucial cornerstone for promoting the maturity of the entire hydrogen energy industry and ultimately achieving a green transformation of the energy structure.
[0003] However, the Nafion® perfluorosulfonic acid membrane developed by DuPont suffers from problems such as rapid water loss at high temperatures leading to a sharp decline in performance, which severely restricts the large-scale commercialization of fuel cells. Some proton exchange membranes also suffer from insufficient strength, insufficient proton conductivity, and poor hydrolytic stability. These defects not only cause microcracks and deformation of the proton exchange membrane, directly disrupting the continuity of the proton conduction channel, but also shorten the battery's lifespan, operational reliability, and pose safety hazards.
[0004] Therefore, it is essential to develop a proton exchange membrane with high strength, high proton conductivity, and good hydrolytic stability. Summary of the Invention
[0005] This invention proposes a magnetic field-assisted isotropic proton exchange membrane, its preparation method, and a battery, to solve or alleviate at least one of the above-mentioned problems.
[0006] The technical solution of the present invention is as follows: This invention proposes a magnetic field-assisted isotropic proton exchange membrane, comprising polyvinylpyrrolidone-coated gadolinium oxide and perfluorosulfonic acid. In the polyvinylpyrrolidone-coated gadolinium oxide, the gadolinium oxide is anisotropically distributed in the proton exchange membrane to form an ordered structure, and the perfluorosulfonic acid is adsorbed on the framework surface formed by the polyvinylpyrrolidone-coated gadolinium oxide in an isotropic distribution.
[0007] Preferably, the mass ratio of the polyvinylpyrrolidone-coated gadolinium oxide to the perfluorosulfonic acid is 0.5~2:98~99.5.
[0008] Preferably, the method for preparing the polyvinylpyrrolidone-coated gadolinium oxide includes the following steps: dispersing gadolinium oxide particles in water, adding polyvinylpyrrolidone, mixing, centrifuging, washing and drying to obtain the polyvinylpyrrolidone-coated gadolinium oxide.
[0009] Preferably, in the polyvinylpyrrolidone-coated gadolinium oxide, the weight-average molecular weight of the polyvinylpyrrolidone is 40,000 to 55,000.
[0010] Preferably, in the polyvinylpyrrolidone-coated gadolinium oxide, the gadolinium oxide particles have a particle size of 300~800nm.
[0011] This invention also proposes a method for preparing a magnetic field-assisted isotropic proton exchange membrane, comprising the following steps: S1. Disperse the perfluorosulfonic acid in an organic solution to obtain a perfluorosulfonic acid solution; S2. Mix the polyvinylpyrrolidone-coated gadolinium oxide and the perfluorosulfonic acid solution evenly to obtain a composite proton exchange membrane solution; S3. The composite proton exchange membrane solution is poured onto a glass plate and dried and cured with magnetic field assistance to obtain the magnetic field-assisted isotropic proton exchange membrane.
[0012] Preferably, the mass ratio of the perfluorosulfonic acid to the organic solvent is 2~5.5:94.5~98, and the organic solvent includes one or more of N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide, and acetonitrile.
[0013] Preferably, the magnetic field conditions for the magnetic field-assisted drying and curing are uniform superconducting magnetic fields with a magnetic induction intensity of 1~2T.
[0014] Preferably, after the magnetic field-assisted drying and curing, a post-processing step is further included, which includes the following steps: the dried proton exchange membrane is sequentially soaked in hydrogen peroxide, water, sulfuric acid and water and then dried to obtain the magnetic field-assisted isotropic proton exchange membrane.
[0015] The present invention also proposes a battery comprising the magnetic field-assisted isotropic proton exchange membrane described above or the magnetic field-assisted isotropic proton exchange membrane prepared by the preparation method described above.
[0016] The working principle and beneficial effects of this invention are as follows: In this invention, gadolinium oxide particles are coated and modified using polyvinylpyrrolidone (PVP). PVP is well-suited to the physicochemical properties of perfluorosulfonic acid (PFSA) systems, effectively improving the interfacial compatibility and dispersibility of nano-gadolinium oxide particles in PFSA solutions. The modified PVP-coated gadolinium oxide can construct a rigid one-dimensional nanoframework network spanning the thickness of the PFSA membrane. Under the synergistic effect of magnetic field-assisted curing and combined with the template-directing effect of the nanoframework, the arrangement of PFSA molecular chains can be controlled on a macroscopic scale, ensuring the ordered hydrophobic fluorocarbon backbone of PFSA along the surface of the oriented nanoframework. Adsorption and spreading enable an isotropic structural design of proton conduction channels within the membrane, optimizing ion transport paths and solving the problems of anisotropy and limited transport efficiency in traditional membrane proton conduction. The narrow confined spaces formed between the uniformly distributed one-dimensional nanoframework within the membrane can physically confine the microphase separation process of the perfluorosulfonic acid system, forcing the hydrophilic and hydrophobic phases within the system to undergo regular and controllable microphase separation along the orientation direction of the framework. This structural effect enhances the directionality, continuity, and regularity of the proton conduction channels, effectively reducing resistance and loss during proton transport and improving proton conduction efficiency. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 This is a diagram illustrating the experimental mechanism of the magnetic field-assisted isotropic proton exchange membrane of this invention. Figure 2 This is a scanning electron microscope image of the magnetic field-assisted isotropic proton exchange membrane prepared in Example 4 of the present invention. Detailed Implementation
[0019] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments. Various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0020] A specific embodiment of the first aspect of the present invention provides a magnetic field-assisted isotropic proton exchange membrane, comprising polyvinylpyrrolidone-coated gadolinium oxide and perfluorosulfonic acid. In the polyvinylpyrrolidone-coated gadolinium oxide, the gadolinium oxide is anisotropically distributed in the proton exchange membrane to form an ordered structure, and the perfluorosulfonic acid is adsorbed on the framework surface formed by the polyvinylpyrrolidone-coated gadolinium oxide in an isotropic distribution.
[0021] In one embodiment of the present invention, the mass ratio of polyvinylpyrrolidone-coated gadolinium oxide to perfluorosulfonic acid is 0.5~2:98~99.5, for example, it can be any ratio among 0.5:99.5, 0.8:99.2, 1:99, 1.2:98.8, 1.5:98.5, 1.8:98.2, 2:98, and any range between any two ratios.
[0022] In one embodiment of the present invention, the preparation method of polyvinylpyrrolidone-coated gadolinium oxide includes the following steps: dispersing gadolinium oxide particles in water, adding polyvinylpyrrolidone, mixing, centrifuging, washing and drying to obtain polyvinylpyrrolidone-coated gadolinium oxide.
[0023] In this invention, gadolinium oxide particles are dispersed in deionized water at a mass ratio of 0.3-0.7 mmol:100-300 mL, preferably 0.5 mmol:200 mL. Polyvinylpyrrolidone (PVP) is added, with a mass-to-volume ratio of PPVP to deionized water of 100-200 mg:100-300 mL, preferably 150 mg:200 mL. The centrifugation speed is 10000-14000 r / min, for example, any value from 10000 r / min, 11000 r / min, 12000 r / min, 13000 r / min, and 14000 r / min, or any range between any two values, preferably 12000 r / min. The centrifugation time is 10-30 min, for example, 10 min, 12 min... The time is any value from 14 min, 15 min, 16 min, 18 min, 20 min, 22 min, 24 min, 25 min, 26 min, 28 min, and 30 min, and the range between any two values, preferably 20 min. The washing is performed by alternating ethanol and water 2 to 5 times, for example, 2, 3, 4, or 5 times, preferably 3 times. The drying temperature is 60 to 80°C, for example, any value from 60°C, 62°C, 64°C, 65°C, 68°C, 70°C, 72°C, 74°C, 75°C, 76°C, 78°C, and 80°C, and the range between any two values, preferably 70°C. The drying time is 8 to 12 hours, for example, any value from 8 hours, 9 hours, 10 hours, 11 hours, and 12 hours, and the range between any two values, preferably 10 hours.
[0024] In this invention, the preparation method of gadolinium oxide particles includes the following steps: dissolving a gadolinium oxide precursor in ethylene glycol, stirring until clear to obtain a mixed solution, evaporating the mixed solution to obtain a gel-like precursor; heating the gel-like precursor to 700~900℃ in an air atmosphere, for example, any point value or range between any two points from 700℃, 710℃, 720℃, 750℃, 780℃, 800℃, 810℃, 820℃, 850℃, 880℃, and 900℃, preferably 800℃, and holding at this temperature to obtain gadolinium oxide nanoparticles.
[0025] In this invention, the gadolinium oxide precursor can be one or both of gadolinium nitrate hexahydrate and gadolinium chloride hexahydrate, preferably gadolinium nitrate hexahydrate; the molar concentration of the gadolinium oxide precursor in the mixed solution is 0.0015~0.14 mol / L; the evaporation temperature is 80~120℃, for example, any point value and any range between any two points from 80℃, 82℃, 85℃, 88℃, 90℃, 92℃, 95℃, 98℃, 100℃, 102℃, 105℃, 108℃, 110℃, 112℃, 115℃, 118℃, 120℃, preferably 90℃; the evaporation time is 12~16h, for example, 12h, 13h, 14h. The heating rate is 5~10℃ / min, for example, any value among 5℃ / min, 6℃ / min, 7℃ / min, 8℃ / min, 9℃ / min, 10℃ / min, for example, any value among 2h, 2.2h, 2.4h, 2.6h, 2.5h, 2.8h, 3h, 3.2h, 3.4h, 3.5h, 3.6h, 3.8h, 4h ...4h, for example, any value among 2h, 2.2h, 2.4h, 3.5h, 3.6h, 3.8h, 4h, for example, 3h.
[0026] In one embodiment of the present invention, the gadolinium oxide particles have a particle size of 300~800nm, for example, any point value or range between any two point values from 300nm, 350nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm, 750nm, and 800nm.
[0027] In one embodiment of the present invention, the weight-average molecular weight of polyvinylpyrrolidone is 40,000 to 55,000.
[0028] In this invention, the weight-average molecular weight of polyvinylpyrrolidone is 40,000 to 55,000. The molecular chain length of polyvinylpyrrolidone in this molecular range is moderate, which can effectively improve the dispersibility of gadolinium oxide particles in the aqueous phase and perfluorosulfonic acid slurry system and inhibit particle aggregation. On the other hand, the molecular chain is not excessively long, which can prevent a single polyvinylpyrrolidone molecule from bridging multiple gadolinium oxide particles at the same time, reduce local flocculation in the slurry, ensure the uniformity and stability of the perfluorosulfonic acid slurry, and make the film layer smooth during subsequent film formation, and less prone to defects such as particle aggregation spots and pinholes.
[0029] A second aspect of the present invention provides a method for preparing a magnetic field-assisted isotropic proton exchange membrane, used to prepare a magnetic field-assisted isotropic proton exchange membrane as provided in the first aspect of the present invention, comprising the following steps: S1. Disperse perfluorosulfonic acid in an organic solution to obtain a perfluorosulfonic acid solution; In this invention, the mass ratio of perfluorosulfonic acid to the organic solution is 2~5.5:94.5~98, for example, any ratio or range between any two ratios from 2:98, 2.5:97.5, 3:97, 3.5:96.5, 4:96, 4.5:95.5, 5:95, 5.5:94.5. The organic solvent includes one or more of N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide, and acetonitrile, preferably N-methylpyrrolidone. The dispersion temperature is 140~160℃, for example, any point value or any two of 140℃, 142℃, 145℃, 148℃, 150℃, 152℃, 155℃, 158℃, and 160℃. The range between point values is preferably 150°C, and the dispersion speed is 400~600 r / min, for example, any point value and the range between any two point values can be selected from 400 r / min, 420 r / min, 440 r / min, 450 r / min, 460 r / min, 480 r / min, 500 r / min, 520 r / min, 540 r / min, 550 r / min, 560 r / min, 580 r / min, and 600 r / min, preferably 500 r / min, and the dispersion time is 2~6 h, for example, any point value and the range between any two point values can be selected from 2 h, 3 h, 4 h, 5 h, and 6 h, preferably 4 h; S2. Mix polyvinylpyrrolidone-coated gadolinium oxide and perfluorosulfonic acid solution evenly to obtain a composite proton exchange membrane solution; In this invention, the mixing temperature is 60~100℃, for example, it can be any point value or any range between two points from 60℃, 65℃, 70℃, 75℃, 80℃, 85℃, 90℃, 95℃, 100℃, preferably 80℃; the mixing speed is 400~600 r / min, for example, it can be any point value or any range between two points from 400 r / min, 420 r / min, 450 r / min, 480 r / min, 500 r / min, 520 r / min, 550 r / min, 580 r / min, 600 r / min, preferably 500 r / min; the mixing time is 10~20h, for example, it can be any point value or any range between two points from 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, preferably 12h; S3. The composite proton exchange membrane solution is poured onto a glass plate, dried and cured with magnetic field assistance, and then post-processed to obtain a magnetic field-assisted isotropic proton exchange membrane.
[0030] In this invention, a composite proton exchange membrane solution is cast onto a glass plate, and the entire mold is immediately placed in a strong uniform magnetic field with a magnetic induction intensity of 1~2T. Under the condition of maintaining the magnetic field, it is placed in an oven for drying and curing. First, it is dried at 60~90℃ for 8~12h, preferably at 80℃ for 10h, and then the temperature is raised to 110~130℃ for 1~3h, preferably at 120℃ for 2h, so that the anisotropic structure of perfluorosulfonic acid is cured.
[0031] In one embodiment of the present invention, the post-processing includes the following steps: the dried proton exchange membrane is sequentially soaked in hydrogen peroxide, water, sulfuric acid and water and then dried to obtain a magnetic field-assisted isotropic proton exchange membrane.
[0032] In this invention, the temperature of the hydrogen peroxide is 60~100℃, for example, it can be any point value or the range between any two points from 60℃, 65℃, 70℃, 75℃, 80℃, 85℃, 90℃, 95℃, and 100℃, preferably 80℃. The concentration of the hydrogen peroxide is 2wt%~5wt%, for example, it can be 2wt%, 2.2wt%, 2.5wt%, 2.8wt%, 3wt%, 3.2wt%, 3.5wt%, 3.8wt%, 4wt%, 4.2wt%, and 4.5wt%. The concentration of sulfuric acid is 60-100°C, for example, any point value or range between any two points from 60°C, 4.8 wt%, 5 wt%, preferably 3 wt%; the water temperature is 60-100°C, for example, any point value or range between any two points from 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, preferably 80°C; the sulfuric acid temperature is 60-100°C, for example, 60°C, 62°C, 65°C, 68°C, 70°C, 72°C, 74°C, 76°C, 78°C, 80°C, 8... The temperature can be any point value among 2℃, 85℃, 88℃, 90℃, 95℃, and 100℃, and the range between any two points, preferably 80℃. The concentration of sulfuric acid is 0.5~2mol / L, for example, 0.5mol / L, 0.8mol / L, 1mol / L, 1.2mol / L, 1.4mol / L, 1.5mol / L, 1.8mol / L, and 2mol / L, preferably 1mol / L; the soaking time is 0.5~3h, for example, 0.5h, 1h, and 1h. The drying time is any value from 5h, 2h, 2.5h, 3h and any range between two values, preferably 1h. The drying temperature is 50~85℃, for example, any value from 50℃, 55℃, 60℃, 65℃, 70℃, 75℃, 80℃, 85℃ and any range between two values, preferably 80℃. The drying time is 10~15h, for example, any value from 10h, 11h, 12h, 13h, 14h, 15h and any range between two values, preferably 12h.
[0033] A specific embodiment of the third aspect of the present invention provides a battery, including a magnetic field-assisted isotropic proton exchange membrane provided by the specific embodiment of the first aspect of the present invention or a magnetic field-assisted isotropic proton exchange membrane prepared by the preparation method provided by the specific embodiment of the second aspect of the present invention.
[0034] The present invention will now be described in detail with reference to preferred embodiments and comparative examples. The preferred embodiments of the invention described below can be modified in various ways, and therefore the scope of the invention should not be construed as limited to the preferred embodiments described in detail below. Preferred embodiments are provided to help those skilled in the art to more readily understand the invention.
[0035] Unless otherwise specified, the following embodiments and comparative examples are as follows: Gadolinium oxide particles: 500 nm in diameter; Polyvinylpyrrolidone: weight average molecular weight is 40,000.
[0036] Example 1 The preparation method of polyvinylpyrrolidone-coated gadolinium oxide includes the following steps: 0.5 mmol of gadolinium nitrate hexahydrate was dissolved in 10 mL of ethylene glycol and stirred until clear to obtain a mixed solution. The mixed solution was evaporated at 90 °C for 14 h to obtain a gel-like precursor. The precursor was heated to 800 °C at a rate of 8 °C / min in air and kept at this temperature for 3 h to decompose nitrate and organic components, generating gadolinium oxide particles. The gadolinium oxide particles were dispersed in 200 mL of deionized water, and 150 mg of polyvinylpyrrolidone was added. After mixing, the mixture was centrifuged at 12000 r / min for 20 min, washed three times with alternating ethanol and water, and dried at 70 °C for 10 h to obtain polyvinylpyrrolidone-coated gadolinium oxide. A method for preparing a magnetic field-assisted isotropic proton exchange membrane includes the following steps: S1. Add perfluorosulfonic acid to N-methylpyrrolidone and stir at 150°C and 500 r / min for 4 h. The mass ratio of perfluorosulfonic acid to N-methylpyrrolidone is 5:95 to obtain a perfluorosulfonic acid solution. S2. Mix polyvinylpyrrolidone-coated gadolinium oxide and perfluorosulfonic acid solution, and stir at 500 r / min for 12 h at 80 °C to obtain composite proton exchange membrane solution; the mass ratio of polyvinylpyrrolidone-coated gadolinium oxide to perfluorosulfonic acid is 0.5:99.5. S3. Cast the composite proton exchange membrane solution onto a glass plate and immediately place the entire mold in a strong uniform magnetic field (magnetic induction intensity of 2T). While maintaining the magnetic field, place it in an oven and dry at 80℃ for 10 hours. Then, raise the temperature to 120℃ and dry for 2 hours to solidify the perfluorosulfonic acid anisotropic structure. Then, immerse it in hydrogen peroxide (concentration of 3wt%) at 80℃, water at 80℃, sulfuric acid (concentration of 1mol / L) at 80℃, and water at 80℃ for 1 hour each. Finally, dry it at 80℃ for 12 hours to obtain a magnetic field-assisted isotropic proton exchange membrane.
[0037] Example 2 The preparation method of polyvinylpyrrolidone-coated gadolinium oxide includes the following steps: 0.5 mmol of gadolinium nitrate hexahydrate was dissolved in 10 mL of ethylene glycol and stirred until clear to obtain a mixed solution. The mixed solution was evaporated at 100 °C for 15 h to obtain a gel-like precursor. The precursor was heated to 850 °C at a rate of 10 °C / min in air and held for 3.5 h to decompose nitrate and organic components, generating gadolinium oxide particles. The gadolinium oxide particles were dispersed in 200 mL of deionized water, and 150 mg of polyvinylpyrrolidone was added. After mixing, the mixture was centrifuged at 14000 r / min for 15 min, washed three times with alternating ethanol and water, and dried at 80 °C for 8 h to obtain polyvinylpyrrolidone-coated gadolinium oxide. A method for preparing a magnetic field-assisted isotropic proton exchange membrane includes the following steps: S1. Add perfluorosulfonic acid to N-methylpyrrolidone and stir at 160°C and 600 r / min for 2 h. The mass ratio of perfluorosulfonic acid to N-methylpyrrolidone is 5:95 to obtain a perfluorosulfonic acid solution. S2. A solution of polyvinylpyrrolidone-coated gadolinium oxide and perfluorosulfonic acid was mixed and stirred at 600 r / min for 10 h at 90 °C to obtain a composite proton exchange membrane solution; the mass ratio of polyvinylpyrrolidone-coated gadolinium oxide to perfluorosulfonic acid was 0.5:99.5. S3. Cast the composite proton exchange membrane solution onto a glass plate and immediately place the entire mold in a strong uniform magnetic field (magnetic induction intensity of 2T). While maintaining the magnetic field, place it in an oven and dry at 90℃ for 8 hours. Then, raise the temperature to 130℃ and dry for 1 hour to solidify the perfluorosulfonic acid anisotropic structure. Then, immerse it in hydrogen peroxide (concentration of 3wt%) at 90℃, water at 90℃, sulfuric acid (concentration of 1mol / L) at 90℃, and water at 90℃ for 0.8 hours each. Finally, dry it at 70℃ for 15 hours to obtain a magnetic field-assisted isotropic proton exchange membrane.
[0038] Example 3 The difference between Example 3 and Example 1 is that the mass ratio of polyvinylpyrrolidone-coated gadolinium oxide to perfluorosulfonic acid is 1:99.
[0039] Example 4 The difference between Example 4 and Example 1 is that the mass ratio of polyvinylpyrrolidone-coated gadolinium oxide to perfluorosulfonic acid is 1.5:98.5. Figure 2 This is a scanning electron microscope image of the magnetic field-assisted isotropic proton exchange membrane prepared in this embodiment. It can be seen from the vertical direction that the internal structure of the membrane has orientation.
[0040] Example 5 The difference between Example 1 and Example 5 is that the mass ratio of polyvinylpyrrolidone-coated gadolinium oxide to perfluorosulfonic acid is 2:98.
[0041] Example 6 The difference between Example 6 and Example 4 is that polyvinylpyrrolidone (weight average molecular weight of 40,000) was replaced with an equal amount of polyvinylpyrrolidone (weight average molecular weight of 55,000).
[0042] Example 7 The difference between Example 7 and Example 4 is that polyvinylpyrrolidone (weight average molecular weight of 40,000) was replaced with an equal amount of polyvinylpyrrolidone (weight average molecular weight of 30,000).
[0043] Example 8 The difference between Example 8 and Example 4 is that polyvinylpyrrolidone (weight average molecular weight of 40,000) was replaced with an equal amount of polyvinylpyrrolidone (weight average molecular weight of 60,000).
[0044] Comparative Example 1 Compared with Example 4, Comparative Example 1 differs in that the composite proton exchange membrane solution is only a perfluorosulfonic acid solution and does not contain polyvinylpyrrolidone-coated gadolinium oxide.
[0045] Comparative Example 2 Compared with Comparative Example 1, Comparative Example 2 differs in that 0.91g of trimethoxy(3,3,3-trifluoropropyl)silane was added to the perfluorosulfonic acid solution.
[0046] Comparative Example 3 The difference between Comparative Example 3 and Example 4 is that polyvinylpyrrolidone was replaced with an equal amount of dextran.
[0047] Comparative Example 4 The difference between Comparative Example 4 and Example 4 is that polyvinylpyrrolidone was replaced with an equal amount of oleic acid.
[0048] Comparative Example 5 Compared with Example 4, Comparative Example 5 differs in that, in the preparation method of polyvinylpyrrolidone-coated gadolinium oxide, 0.5 mmol of gadolinium nitrate hexahydrate is replaced with 0.2 mmol of tungsten hexachloride.
[0049] Experimental Example 1 The performance of the magnetic field-assisted isotropic proton exchange membranes prepared in Examples 1-8 and Comparative Examples 1-5 was tested according to the following test methods: 1. Tensile Strength: The proton exchange membrane was made into a rectangular strip with a length of 65 mm and a width of 15 mm. A universal tensile testing machine was used, with a tensile speed of 5 mm / min and an initial gauge length of 20 mm. The mechanical properties were calculated using the following formula:
[0050] In the formula, σ1 is the tensile strength (MPa), p is the maximum load (N), b is the width of the rectangular spline (mm), and d is the thickness of the rectangular spline (mm), which is measured by a thickness gauge.
[0051] 2. Proton conductivity (proton electrical conductivity): conducted at a temperature of 25℃ and a humidity of 100%RH; 3. Water Absorption Rate: The proton exchange membrane was dried in an oven at 80℃ for 24 hours. When the proton exchange membrane reached the ambient temperature, its mass was measured as m0 (g). Then, the proton exchange membrane was soaked in distilled water at 80℃ for 8 hours. The water on the surface of the proton exchange membrane was removed with filter paper, and its mass was measured as m1 (g) within 30 seconds. The water absorption rate Δm was calculated using the following formula:
[0052] 4. Hydrolytic stability: The mass of pre-dried material is W o (g) The proton exchange membrane was immersed in deionized water at 80℃ for 48 hours. After immersion, the proton exchange membrane was removed and dried at 80℃ for 8 hours. Its mass was measured to be W. t (g). The hydrolytic stability Wc value of the proton exchange membrane is calculated by the following formula:
[0053] The test results are shown in Table 1: Table 1 Performance test results of Examples 1-8 and Comparative Examples 1-5
[0054] In Comparative Example 3, after gadolinium oxide was coated with dextran and dispersed in N-methylpyrrolidone, precipitation and magnetic failure immediately occurred, making it unusable in this system and no further testing was conducted.
[0055] As shown in Table 1, comparing Comparative Examples 1-5 with Example 1, it can be seen that introducing polyvinylpyrrolidone-coated gadolinium oxide into the composite proton exchange membrane solution and reconstructing the proton conduction network topology of the perfluorosulfonic acid membrane through the magnetic field-induced nanotemplate effect achieves a synergistic improvement in proton conduction efficiency, mechanical stability, and dimensional stability. Among these improvements, the vertical conductivity is increased more than the horizontal proton conductivity.
[0056] A comparison of Examples 4 and 6-8 shows that when the weight-average molecular weight of polyvinylpyrrolidone is 40,000-55,000, the magnetic field-assisted isotropic proton exchange membrane has a stronger strength, higher proton conduction efficiency, and higher hydrolysis stability.
[0057] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A magnetic field-assisted isotropic proton exchange membrane, characterized in that: The invention comprises polyvinylpyrrolidone-coated gadolinium oxide and perfluorosulfonic acid. In the polyvinylpyrrolidone-coated gadolinium oxide, the gadolinium oxide is anisotropically distributed in a proton exchange membrane to form an ordered structure, and the perfluorosulfonic acid is isotropically adsorbed on the framework surface formed by the polyvinylpyrrolidone-coated gadolinium oxide.
2. The magnetic field-assisted isotropic proton exchange membrane according to claim 1, characterized in that, The mass ratio of the polyvinylpyrrolidone-coated gadolinium oxide to the perfluorosulfonic acid is 0.5~2:98~99.
5.
3. The magnetic field-assisted isotropic proton exchange membrane according to claim 1, characterized in that, The preparation method of the polyvinylpyrrolidone-coated gadolinium oxide includes the following steps: dispersing gadolinium oxide particles in water, adding polyvinylpyrrolidone, mixing, centrifuging, washing and drying to obtain the polyvinylpyrrolidone-coated gadolinium oxide.
4. The magnetic field-assisted isotropic proton exchange membrane according to claim 1, characterized in that, In the polyvinylpyrrolidone-coated gadolinium oxide, the weight-average molecular weight of the polyvinylpyrrolidone is 40,000 to 55,000.
5. A magnetic field-assisted isotropic proton exchange membrane according to claim 1, characterized in that, In the polyvinylpyrrolidone-coated gadolinium oxide, the gadolinium oxide particles have a particle size of 300~800nm.
6. A method for preparing a magnetic field-assisted isotropic proton exchange membrane, used to prepare the magnetic field-assisted isotropic proton exchange membrane according to any one of claims 1 to 5, characterized in that, Includes the following steps: S1. Disperse the perfluorosulfonic acid in an organic solution to obtain a perfluorosulfonic acid solution; S2. Mix the polyvinylpyrrolidone-coated gadolinium oxide and the perfluorosulfonic acid solution evenly to obtain a composite proton exchange membrane solution; S3. The composite proton exchange membrane solution is poured onto a glass plate and dried and cured with magnetic field assistance to obtain the magnetic field-assisted isotropic proton exchange membrane.
7. The method for preparing a magnetic field-assisted isotropic proton exchange membrane according to claim 6, characterized in that, The mass ratio of the perfluorosulfonic acid to the organic solvent is 2~5.5:94.5~98, and the organic solvent includes one or more of N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide, and acetonitrile.
8. The method for preparing a magnetic field-assisted isotropic proton exchange membrane according to claim 6, characterized in that, The magnetic field used for magnetic field-assisted drying and curing is a uniform superconducting magnetic field with a magnetic induction intensity of 1~2T.
9. The method for preparing a magnetic field-assisted isotropic proton exchange membrane according to claim 6, characterized in that, After the magnetic field-assisted drying and curing, a post-processing step is also included, which includes: soaking the dried proton exchange membrane in hydrogen peroxide, water, sulfuric acid and water in sequence and then drying it.
10. A battery, characterized in that, The magnetic field-assisted isotropic proton exchange membrane according to any one of claims 1 to 5 or the magnetic field-assisted isotropic proton exchange membrane prepared by the preparation method according to any one of claims 6 to 9 isotropic proton exchange membrane.