Secondary batteries and their preparation methods, and electrical equipment

By incorporating porous materials into the binder and combining them with acrylate copolymers to form secondary particles, the problem of low ionic conductivity of the binder is solved, thereby improving the rate performance of the secondary battery.

CN123120822APending Publication Date: 2026-11-17CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510637006.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing binders have low ionic conductivity in secondary batteries, which affects the rate performance of the batteries.

Method used

Porous materials are added to the binder and combined with acrylate copolymers to form secondary particles. The porous materials are located inside and/or on the surface of the particles, increasing transport channels and storage space.

Benefits of technology

This improved the ionic conductivity of the binder and the adhesion of the separator, thereby enhancing the rate performance of the secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120822A_ABST
    Figure CN123120822A_ABST
Patent Text Reader

Abstract

This application relates to the field of secondary battery technology. This application provides a secondary battery and its preparation method, as well as an electrical device. The secondary battery includes a positive electrode, an electrolyte, a separator, and a negative electrode. The separator includes a base film and an adhesive layer disposed on at least one side of the base film. The adhesive layer includes an adhesive, which comprises a polymer and a porous material. The polymer includes an acrylate copolymer. The acrylate copolymer and the porous material together form secondary particles, with the porous material located inside and / or on the surface of the secondary particles. The secondary battery proposed in this application exhibits excellent rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of secondary battery technology, specifically to a secondary battery and its preparation method and electrical equipment. Background Technology

[0002] In recent years, rechargeable batteries have been widely used in energy storage systems such as hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric cars, military equipment, aerospace, and many other fields. While binders account for a relatively small percentage of the total usage and cost in rechargeable batteries, they effectively improve battery performance and are an indispensable component. As a non-active material in the battery, binders hold the various components and adjacent parts together, reducing the expansion and shedding of active materials during charging and discharging, and lowering the battery's internal resistance. However, current binders still present several challenges in practical applications and require further improvement. Summary of the Invention

[0003] This application aims to at least partially solve one of the technical problems in the related art. Therefore, one objective of this application is to provide a secondary battery and its preparation method, as well as an electrical device thereof, wherein the separator containing a binder has high ionic conductivity, and the secondary battery has superior rate performance.

[0004] Therefore, in a first aspect, this application provides a secondary battery, the secondary battery comprising a positive electrode, an electrolyte, a separator, and a negative electrode, the separator comprising a base film and an adhesive layer disposed on at least one side of the base film, the adhesive layer comprising an adhesive comprising a polymer and a porous material, the acrylate copolymer and the porous material together forming secondary particles, the porous material being located inside and / or on the surface of the secondary particles.

[0005] Therefore, the secondary battery proposed in this application incorporates a porous material into the binder, and the two are combined to form secondary particles. The porous material is located inside and / or on the surface of the secondary particles, which significantly increases the overall pore size of the binder, providing more transport channels for metal active ions and more storage space and transport channels for the electrolyte. The pores of the porous material can also serve as channels for conducting metal active ions, improving the ionic conductivity of the binder and resulting in high adhesion of the separator, thus giving the secondary battery excellent rate performance.

[0006] In some embodiments of this application, the mass ratio of the polymer to the porous material is (60:40) to (95:5). This improves the rate performance of the secondary battery.

[0007] In some embodiments of this application, the mass ratio of the polymer to the porous material is (80:20) to (95:5). This improves the rate performance of the secondary battery.

[0008] In some embodiments of this application, the areal density of the adhesive layer on the base film is 1 g / m³. 2 -1.8g / m 2 This can improve the rate performance of secondary batteries.

[0009] In some embodiments of this application, at least some of the pores in the porous material extend through the porous material. This can improve the rate performance of the secondary battery.

[0010] In some embodiments of this application, the porous material includes one or more of the following: molecular sieves, zeolites, mesoporous silica, halloysite nanotubes, diatomaceous earth, porous titanium dioxide, porous boron nitride, porous graphene, carbon nanotubes, hydrated aluminum silicate, and activated carbon. This can improve the rate performance of secondary batteries.

[0011] In some embodiments of this application, the binder has a Dv50 particle size of 1μm-20μm. This can improve the rate performance of the secondary battery.

[0012] In some embodiments of this application, the acrylate copolymer is formed by monomer polymerization, wherein the monomer of the polymer includes one or more of a first monomer, a second monomer, and a third monomer, and the structure of the first monomer is shown in Formula 1:

[0013]

[0014] Wherein, R1 includes a hydrogen atom or a C1-C6 alkyl group, and R2 includes a substituted or unsubstituted C1-C6 alkyl group. 15 Alkyl, substituted or unsubstituted C3-C6 isobornyl, wherein the C1-C 15 The alkyl substituents include hydroxyl groups or C1-C6 alkyl groups;

[0015] The structure of the second monomer is shown in Equation 2, and / or Equation 3:

[0016]

[0017] R3 includes hydrogen atoms or C1-C atoms. 18 The alkyl group, where R4 includes a hydrogen atom or a C1-C6 alkyl group;

[0018] The structure of the third monomer is shown in Equation 4:

[0019]

[0020] R5 includes a hydrogen atom, a hydroxyl-substituted C1-C6 alkyl group, or a C1-C6 alkoxy group, and R6 includes a hydrogen atom or a C1-C6 alkyl group. This improves the rate performance of the secondary battery.

[0021] In some embodiments of this application, the first monomer includes at least one of ethyl acrylate, n-butyl acrylate, n-propyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, cyclohexyl acrylate, isooctyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, vinyl acetate, trimethylolpropane triacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate. This can improve the rate performance of the secondary battery.

[0022] In some embodiments of this application, the second monomer includes at least one selected from acrylonitrile, methacrylonitrile, ethyl acrylonitrile, acrylic acid, methacrylic acid, butenoic acid, and heptenoic acid. This can improve the rate performance of the secondary battery.

[0023] In some embodiments of this application, the third monomer includes at least one of acrylamide, N-hydroxymethylacrylamide, and N-butoxymethylacrylamide. This can improve the rate performance of the secondary battery.

[0024] In some embodiments of this application, the monomers of the polymer include a first monomer, a second monomer, and a third monomer, wherein the mass ratio of the first monomer, the second monomer, and the third monomer is 100:(1-70):(5-20).

[0025] In a second aspect, this application proposes a method for preparing a secondary battery, including a method for preparing a separator membrane, comprising: blending and stirring an emulsifier, an initiator, and a monomer of a polymer, and heating to react to obtain a polymer emulsion; mixing and stirring a porous material with the polymer emulsion, and spray drying to obtain a binder; and disposing the binder on at least one side of a base membrane to obtain a separator membrane; wherein the separator membrane comprises a base membrane and an binder layer disposed on at least one side of the base membrane, the binder layer comprising a binder, the binder comprising a polymer and a porous material, the polymer comprising an acrylate copolymer, the acrylate copolymer and the porous material together forming secondary particles, the porous material being located inside and / or on the surface of the secondary particles. Therefore, the separator membrane prepared in this application, and the secondary battery containing it, exhibits excellent rate performance.

[0026] In some embodiments of this application, the binder is dispersed in a solvent and sprayed onto at least one side of the base film to obtain a separator. This can improve the rate performance of the secondary battery.

[0027] In some embodiments of this application, the porosity of the porous material is 5%-85%. This can improve the rate performance of the secondary battery.

[0028] In some embodiments of this application, the specific surface area of ​​the porous material is 10 m². 2 / g-2000m 2 / g. This can improve the rate performance of secondary batteries.

[0029] In some embodiments of this application, the Dv50 particle size of the porous material is less than or equal to 3 μm. This can improve the rate performance of the secondary battery.

[0030] In a third aspect of this application, this application proposes an electrical device comprising the secondary battery described in the first aspect of this application, or the secondary battery prepared by the method described in the second aspect of this application.

[0031] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description

[0032] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which:

[0033] Figure 1 This is a schematic diagram of a secondary battery according to one embodiment of this application.

[0034] Figure 2 yes Figure 1 An exploded view of a secondary battery according to an embodiment of this application is shown.

[0035] Figure 3 This is a schematic diagram of a battery module according to one embodiment of this application.

[0036] Figure 4 This is a schematic diagram of a battery pack according to one embodiment of this application.

[0037] Figure 5 yes Figure 4 An exploded view of a battery pack according to one embodiment of this application is shown.

[0038] Figure 6 This is a schematic diagram of an electrical device using a secondary battery as a power source according to an embodiment of this application.

[0039] Figure 7This is a SEM image of the adhesive prepared in Example 4 of this application.

[0040] Figure 8 yes Figure 7 Enlarged image.

[0041] Figure 9 This is a SEM image of the adhesive prepared in Comparative Example 1 of this application.

[0042] Explanation of reference numerals in the attached figures:

[0043] 1 Battery pack; 2 Upper housing; 3 Lower housing; 4 Battery module; 5 Secondary battery; 51 Housing; 52 Electrode assembly; 53 Top cover assembly. Detailed Implementation

[0044] The following detailed description, with appropriate reference to the accompanying drawings, discloses the lithium secondary battery and its preparation method, as well as embodiments of the electrical device thereof. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0045] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0046] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0047] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.

[0048] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0049] Typically, a battery consists of a positive electrode, a negative electrode, and a separator. The separator and the electrode need to be tightly bonded together with an adhesive. The bonded positive and negative electrodes and separator support each other, giving the secondary battery a certain degree of compressive strength. The negative electrode expands and contracts during charging and discharging. When the adhesion between the separator and the electrode is weak, the separator cannot maintain a good fit on the surface of the negative electrode after it shrinks, creating gaps between the positive and negative electrodes and the separator. This results in a loose and less rigid secondary battery, significantly increasing its internal resistance. Adding an adhesive layer to the surface of the separator's base film can effectively improve the separator's adhesion performance and enhance the bonding effect between the separator and the electrode. Furthermore, during the charging and discharging process of the battery, active metal ions (such as lithium ions and sodium ions) migrate between the positive and negative electrodes and pass through the binder on the surface of the base film. The conduction of active metal ions in the binder mainly includes electrolyte conduction and binder bulk conduction. The electrolyte conduction rate depends on the swelling capacity of the polymer for the electrolyte and electrolyte solution, and its conduction rate is relatively fixed, while the binder bulk conduction rate is relatively slow. Therefore, in order to further improve the conduction rate of active metal ions, the binder should not only have good adhesion but also high ionic conductivity.

[0050] Acrylic copolymers are a general term for polymers produced by copolymerizing acrylate monomers with other comonomers. Acrylic copolymers exhibit good adhesion and a low glass transition temperature, making them suitable as binders on the base film surface for improved adhesion between the separator and the electrode after cold or hot pressing. However, their ionic conductivity still needs improvement.

[0051] It can be understood that cold pressing refers to shaping the wound battery cell at a lower ambient temperature than hot pressing, which reduces the elasticity of the battery cell and improves the core assembly qualification rate and the consistency of the thickness of the finished battery cell.

[0052] In this application, by adding a porous material to an acrylate copolymer, the two are combined to form secondary particles. The porous material is located inside and / or on the surface of the secondary particles, which significantly increases the pores of the binder, providing more transport channels for metal active ions. The porous material provides more storage space and transport channels for the electrolyte. The pores of the porous material can also serve as channels for conducting metal active ions, so that metal active ions can be transported not only through the acrylate copolymer swollen with electrolyte and electrolyte solution, but also through the porous material. The combined effect of the two can improve the rate performance of the secondary battery.

[0053] The secondary battery disclosed in this application can be used in electrical devices that use batteries as a power source or in various energy storage systems that use batteries as energy storage elements. Electrical devices may include, but are not limited to, mobile phones, tablets, laptops, electric toys, power tools, electric vehicles, electric cars, ships, spacecraft, etc. Electric toys may include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Spacecraft may include airplanes, rockets, space shuttles, and spacecraft, etc.

[0054] The first aspect of this application discloses a secondary battery, the secondary battery comprising a positive electrode, an electrolyte, a separator, and a negative electrode. The separator comprises a base film and an adhesive layer disposed on at least one side of the base film. The adhesive layer comprises an adhesive, the adhesive comprising a polymer and a porous material. The polymer comprises an acrylate copolymer. The acrylate copolymer and the porous material together form secondary particles, the porous material being located inside and / or on the surface of the secondary particles.

[0055] In this application, by adding a porous material to an acrylate copolymer, the two are combined to form secondary particles. The porous material is located inside and / or on the surface of the secondary particles, which significantly increases the number of pores in the binder, providing more transport channels for metal active ions. The porous material also provides more storage space and transport channels for the electrolyte. The pores of the porous material can also serve as channels for conducting metal active ions. This means that metal active ions can be transported not only through the acrylate copolymer swollen with electrolyte and electrolyte solution, but also through the porous material. The combined effect of both can improve the rate performance of the secondary battery.

[0056] For example, please refer to Figure 7 and Figure 8 , Figure 7This is a scanning electron microscope image of multiple secondary adhesive particles according to one embodiment of this application. Figure 8 for Figure 7 The image shows an enlarged view. As can be seen, the porous material is located inside (not shown) and on the surface of the secondary particles. The porous material consists of linear particles, while the polymer particles are spherical primary particles. The porous material and polymer particles together form the binder secondary particles.

[0057] In some embodiments of this application, the mass ratio of the polymer to the porous material is (60:40)-(95:5). As examples, the mass ratio of the polymer to the porous material can be 60:40, 70:30, 80:20, 90:10, 95:5, etc. In other embodiments of this application, the mass ratio of the polymer to the porous material is (80:20)-(95:5). Controlling the mass ratio within the above range effectively improves the ionic conductivity of the binder without causing excessive porous material content that could affect the binder's bonding performance, thereby further improving the rate performance of the secondary battery.

[0058] It is understood that "the mass ratio of the polymer to the porous material" is a well-known definition in the art and can be determined using methods known in the art, such as the following methods:

[0059] The battery is disassembled, the separator is removed, and after cleaning and drying, the powder is scraped off to obtain the binder. The binder is subjected to XRD to determine the composition of the porous material, and infrared spectroscopy is performed to determine the composition of the polymer.

[0060] Take another binder and perform elemental analysis to determine the content of each element, and convert it into the mass ratio of porous material to polymer.

[0061] In some embodiments of this application, the areal density of the adhesive layer on the base film is 1 g / m³. 2 -1.8g / m 2 For example, the areal density of the adhesive layer on the base film can be 1 g / m³. 2 -1.7g / m 2 1.1g / m 2 -1.6g / m 2 1.2g / m 2 -1.5g / m 2 1.3g / m 2 -1.4g / m 2 By controlling the areal density of the adhesive layer on the base film within the above range, it is sufficient to bond the separator to the positive and negative electrode sheets, without causing excessive adhesive content that would affect lithium-ion transport. This reduces the probability of adhesive clogging the pores of the separator and further improves the rate performance of the secondary battery.

[0062] It can be understood that "the areal density of the adhesive layer on the base film" refers to the mass of the adhesive layer coated on a unit area (i.e., 1 square meter) of the base film surface, expressed in g / m². 2 The areal density can be determined using conventional testing methods in the field. For example, the areal density testing method includes: cutting three 100mm × 100mm samples from the left, middle, and right portions, perpendicular to the coating direction of the release liner; weighing these samples on an analytical balance with an accuracy of 0.0001 (m1); scraping off the adhesive layer and weighing it again (m2); calculating the average areal density of the three samples, which is recorded as the areal density of the adhesive layer, in g / m³. 2 The formula is as follows:

[0063] areal density (g / m³) 2 )=(m1-m2) / 0.01m1.

[0064] In some embodiments of this application, the porosity of the porous material is 5%-85%, for example, the porosity of the porous material can be 5%-84%, 10%-80%, 20%-70%, 30%-60%, 40%-50%, etc. Controlling the porosity of the porous material within the above range provides more storage space and transport channels for the electrolyte. The pores can also serve as channels for conducting active metal ions, further improving the rate performance of the secondary battery. In other embodiments of this application, the porosity of the porous material is 30%-70%.

[0065] It is understood that "porosity of porous materials" is a well-known definition in the art and can be determined using methods known in the art, such as the following methods:

[0066] Gas adsorption method

[0067] Principle: Based on the adsorption characteristics of gases on the surface of porous materials, the specific surface area is calculated by measuring the amount of adsorbed gas, and then the porosity is estimated by combining it with other parameters. Commonly used gases include nitrogen and argon.

[0068] Procedure: Place the sample in the adsorption apparatus at a specific temperature for degassing. Then, measure the amount of gas adsorbed under different relative pressures to obtain adsorption isotherms. Calculate the specific surface area and porosity based on adsorption theoretical models, such as the BET equation.

[0069] In some embodiments of this application, the specific surface area of ​​the porous material is 10 m². 2 / g-2000m 2 / g. For example, the specific surface area of ​​porous materials can be 10m². 2 / g-1900m 2 / g, 50m2 / g-1500m 2 / g, 100m 2 / g-1000m 2 / g, 150m 2 / g-500m 2 / g, 200m 2 / g-300m 2 By controlling the specific surface area of ​​the porous material within the above range (e.g., g), the liquid retention capacity of the binder can be improved, providing more storage space and transport channels for the electrolyte, thereby further enhancing the rate performance of the secondary battery. In some other embodiments of this application, the specific surface area of ​​the porous material is 30 m² / g. 2 / g-700m 2 / g.

[0070] It is understood that "specific surface area of ​​porous materials" is a well-known definition in the art and can be measured using methods known in the art, such as the following methods:

[0071] Gas adsorption method

[0072] Principle: At constant low temperature, after measuring the amount of gas adsorbed on the solid surface at different relative pressures, the amount of monolayer adsorption of the sample is obtained based on the Brown-Etter-Taylor (BET) multilayer adsorption theory and its formula, thereby calculating the specific surface area of ​​the solid.

[0073] Procedure: Place the sample in the adsorption apparatus and degas it first to remove surface impurities and adsorbed gas. Then, introduce nitrogen gas under different relative pressures, measure the adsorption amount, obtain the adsorption isotherm, and calculate the specific surface area by fitting the data according to the BET equation.

[0074] In some embodiments of this application, the Dv50 particle size of the porous material is less than or equal to 3 μm, for example, it can be 0.01 μm-3 μm, 0.05 μm-2 μm, 0.1 μm-1.5 μm, 0.5 μm-1 μm, 0.7 μm-0.8 μm, etc. Controlling the Dv50 particle size of the porous material within the above range results in higher uniformity of distribution in the binder and a better effect on improving the ionic conductivity of the binder. In other embodiments of this application, the Dv50 particle size of the porous material is 0.05 μm-1 μm, for example, 0.1 μm-0.8 μm.

[0075] It is understood that the Dv50 particle size is the particle size corresponding to a cumulative particle size distribution percentage of 50%. As an example, the Dv50 particle size in this application can be measured using a laser particle size analyzer (Malvin 3000, MasterSizer 3000), with a helium-neon red light source as the main light source. Take a clean small beaker, add 1g of the sample to be tested, add one drop of surfactant, add 20ml of deionized water, and sonicate at 53kHz / 120W for 5 minutes to ensure complete dispersion of the sample. Turn on the laser particle size analyzer, clean the optical path system, and automatically test the background. Stir the sonicated solution to be tested to ensure uniform dispersion, place it in the sample cell as required, and begin measuring the particle size. The measurement results can be read from the instrument.

[0076] In some embodiments of this application, at least some of the channels of the porous material penetrate through the porous material, that is, at least some of the channels of the porous material are through holes, and the channels are not all blind holes. This further facilitates the transport of metal active ions and the flow of electrolyte, further improves the ionic conductivity of the binder, and enhances the rate performance of the secondary battery.

[0077] In some embodiments of this application, the porous material includes one or more of the following: molecular sieves, zeolites, mesoporous silica, halloysite nanotubes, diatomaceous earth, porous titanium dioxide, porous boron nitride, porous graphene, carbon nanotubes, hydrated aluminum silicate, and activated carbon. These porous materials possess abundant pore structures, providing more storage space and transport channels for the electrolyte. The pores of the porous material can also serve as channels for conducting active metal ions, allowing these ions to be transported through the porous material, effectively improving the ionic conductivity of the binder and thus enhancing the rate performance of the secondary battery.

[0078] Halloysite nanotubes are naturally occurring aluminosilicate nanotubes. Halloysite nanotubes (Al2Si2O5(OH)4·2H2O) are a two-layer aluminosilicate with a hollow tubular structure in the submicron range and chemical properties similar to kaolin.

[0079] In some embodiments of this application, the Dv50 particle size of the binder is 1μm-20μm, for example, it can be 1μm-19μm, 5μm-15μm, 8μm-10μm, etc. Controlling the Dv50 particle size of the binder within the above range can reduce the clogging of the base film pores by the binder and help form an binder coating of appropriate thickness. In other embodiments of this application, the Dv50 particle size of the binder is 3μm-15μm.

[0080] In some embodiments of this application, the acrylate copolymer is formed by monomer polymerization, wherein the monomer of the polymer includes one or more of a first monomer, a second monomer, and a third monomer, and the structure of the first monomer is shown in Formula 1:

[0081]

[0082] Wherein, R1 includes a hydrogen atom or a C1-C6 alkyl group, and R2 includes a substituted or unsubstituted C1-C6 alkyl group. 15 Alkyl, substituted or unsubstituted C3-C6 isobornyl, wherein the C1-C 15 The alkyl substituents include hydroxyl groups or C1-C6 alkyl groups;

[0083] The structure of the second monomer is shown in Equation 2, and / or Equation 3:

[0084]

[0085] R3 includes hydrogen atoms or C1-C atoms. 18 The alkyl group, where R4 includes a hydrogen atom or a C1-C6 alkyl group;

[0086] The structure of the third monomer is shown in Equation 4:

[0087]

[0088] R5 includes a hydrogen atom, a hydroxyl-substituted C1-C6 alkyl group or a C1-C6 alkoxy group, and R6 includes a hydrogen atom or a C1-C6 alkyl group.

[0089] In the battery manufacturing process, hot pressing or cold pressing is required to ensure a tight bond between the separator and the electrode. When the first monomer satisfies the aforementioned structural formula, the soft and hard monomers in the first monomer can polymerize to form the backbone of the polymer molecular chain segments, giving the polymer excellent stability and good adhesion, while also helping to improve the polymer's anti-swelling properties.

[0090] In some embodiments of this application, the first monomer includes at least one of ethyl acrylate, n-butyl acrylate, n-propyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, cyclohexyl acrylate, isooctyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, vinyl acetate, trimethylolpropane triacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate. Using any one or more of the above first monomers can adjust the polymer's adhesive properties and anti-swelling properties.

[0091] The second monomer contains unsaturated double bonds, which is beneficial to monomer polymerization. It also has carboxyl and / or cyano functional groups. The carboxyl and cyano groups can combine with the functional groups on the base membrane of the separator to improve the adhesion between the polymer and the base membrane, and can also increase the crosslinking active sites of the polymer, thereby improving the polymer's creep resistance and cohesive strength.

[0092] In some embodiments of this application, the second monomer includes at least one selected from acrylonitrile, methacrylonitrile, ethylacrylonitrile, acrylic acid, methacrylic acid, butenoic acid, and heptenoic acid. This can further improve the ionic conductivity and adhesive properties of the polymer. Using any one or more of the above-mentioned second monomers can adjust the adhesive properties of the polymer; wherein, monomers containing cyano groups can also improve the ionic conductivity of the polymer.

[0093] The third monomer contains unsaturated amide groups, which is beneficial to the polymerization of the monomer. This type of monomer can play a role in regulating the molecular weight, and at the same time, it can also improve the adhesion and anti-swelling properties of the polymer.

[0094] In some embodiments, the third monomer includes at least one of acrylamide, N-hydroxymethylacrylamide, and N-butoxymethylacrylamide. This can further improve the adhesive properties of the polymer.

[0095] Using any one or more of the aforementioned third monomers can help adjust the molecular weight of the polymer. Within a certain range, the molecular weight of the polymer can help improve its adhesiveness.

[0096] The presence of fluorinated groups, ester groups, carboxyl groups, acrylamide groups, carbonyl groups, amide groups, and cyano groups in the polymer structure can be tested according to the general rules of infrared spectroscopy analysis methods in the national standard GB / T 6040-2002. Specifically, the sample is pressed into a KBr pellet using the transmission method, and the KBr background blank is subtracted by the transmission method to obtain the sample test spectrum (resolution: 4 cm⁻¹). -1 Wavenumber range: 400cm -1 -4000cm -1 ).

[0097] In some embodiments of this application, the polymer monomers include a first monomer, a second monomer, and a third monomer, wherein the mass ratio of the first monomer, the second monomer, and the third monomer is 100:(1-70):(5-20). For example, the mass ratio of the three monomers can be 100:(1-69):(5-20), 100:(10-60):(5-20), 100:(20-50):(5-20), 100:(30-40):(5-20), 100:(1-70):(5-15), 100:(1-70):(10-15), etc. By controlling the mass percentage of the three polymer monomers within the above range, the adhesive properties, anti-swelling properties, and anti-creep properties of the adhesive can be considered.

[0098] The aforementioned acrylate copolymers can be prepared by combining different proportions of functional monomers. On the one hand, the prepared acrylate copolymers have a low glass transition temperature, which allows them to effectively wet the gaps in the electrode at room temperature, resulting in a strong mechanical linkage between the acrylate copolymers and the electrode, thus improving the adhesion to the electrode. On the other hand, by selecting the appropriate monomer combination, reactive groups can be introduced into the acrylate copolymers, giving them better hydrophilicity, improving the surface wettability of the copolymer particles in the polymer emulsion, reducing irregular aggregation, and improving the mixing uniformity between the solid electrolyte and the polymer.

[0099] In some embodiments of this application, the base film may include at least one of polyethylene, polypropylene, polyvinylidene fluoride, polytetrafluoroethylene, and nonwoven fabric. Using a base film made of the above materials can effectively improve the adhesion of the polymer to the base film and enhance the structural stability of the separator.

[0100] In a second aspect, this application proposes a method for preparing a secondary battery, including a method for preparing a separator membrane, the method comprising:

[0101] S1. The emulsifier, initiator, and polymer monomers are blended and stirred, and then heated to react to obtain a polymer emulsion.

[0102] S2. The porous material and the polymer emulsion are mixed and stirred, and then spray-dried to obtain an adhesive, wherein the polymer includes acrylate copolymers;

[0103] S3. The adhesive is disposed on at least one side of the base film to obtain a release film;

[0104] The isolation membrane includes a base membrane and an adhesive layer disposed on at least one side of the base membrane. The adhesive layer includes an adhesive, which includes a polymer and a porous material. The polymer includes an acrylate copolymer. The acrylate copolymer and the porous material together form secondary particles, and the porous material is located inside and / or on the surface of the secondary particles.

[0105] The monomer polymerization method described above is emulsion polymerization. In emulsion polymerization, the monomers are dispersed in water to form an emulsion with the help of emulsifiers and mechanical stirring, and then an initiator is added to initiate the polymerization of the monomers.

[0106] Emulsifiers are substances that can transform immiscible oils and water into emulsions that are difficult to separate. Emulsifiers are usually surfactants that combine the properties of both hydrophilic polar groups and hydrophobic (lipophilic) nonpolar groups.

[0107] An initiator is a substance that can initiate a polymerization reaction of monomers. For example, a free radical initiator refers to a class of compounds that are easily decomposed into free radicals (i.e., primary free radicals) by heat, and can be used to initiate free radical polymerization and copolymerization reactions of alkene and diene monomers.

[0108] In some embodiments of this application, the emulsifier includes at least one of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, sodium dodecylbenzene sulfate, sodium laurate, sodium stearate, and sodium palmitate.

[0109] In some embodiments of this application, the initiator includes at least one selected from persulfate initiators, acyl peroxide initiators, and azo initiators. Specifically, persulfate initiators include at least one selected from potassium persulfate and ammonium persulfate; acyl peroxide initiators include at least one selected from benzoyl peroxide and dioctanoyl peroxide; and azo initiators include at least one selected from azobisisobutyronitrile and dimethyl azobisisobutyrate.

[0110] In some embodiments of this application, the adhesive can be disposed on at least one side of the base film by the following methods:

[0111] The adhesive and glue (such as polyacrylic acid, polyacrylate, styrene-butadiene latex) prepared as described above are stirred and mixed evenly in deionized water to obtain an adhesive slurry. The adhesive slurry is sprayed onto one or both sides of the base film, dried to remove the solvent, and a release film is obtained.

[0112] The prepared binder needs to be in full contact with the electrode after the battery is cold-pressed or hot-pressed in order to play its role. Therefore, additional glue needs to be added when preparing the binder layer.

[0113] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During charging and discharging, active ions move back and forth between the positive and negative electrodes, inserting and releasing. The electrolyte acts as a conductor between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits while allowing ions to pass through.

[0114] [Positive electrode plate]

[0115] The positive electrode includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector.

[0116] As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive active material layer is disposed on either or both of the two opposite surfaces of the positive current collector.

[0117] In some embodiments of this application, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0118] In some embodiments of this application, when the battery is a lithium-ion battery, the positive electrode active material may be a positive electrode active material known in the art for lithium-ion batteries.

[0119] In some embodiments of this application, the positive electrode active material may be a known positive electrode active material for lithium-ion batteries. As an example, the positive electrode active material may include at least one of the following materials: lithium phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as battery positive electrode active materials may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides include, but are not limited to, lithium cobalt oxides (such as LiCoO2), lithium nickel oxides (such as LiNiO2), lithium manganese oxides (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, and lithium nickel cobalt manganese oxides (such as LiNi). 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also known as NCM) 333 LiNi0.5 Co 0.2 Mn 0.3 O2 (also known as NCM) 523 LiNi 0.5 Co 0.25 Mn 0.25 O2 (also known as NCM) 211 LiNi 0.6 Co 0.2 Mn 0.2 O2 (also known as NCM) 622 LiNi 0.8 Co 0.1 Mn 0.1 O2 (also known as NCM) 811 ), lithium nickel cobalt aluminum oxide (such as LiNi) 0.8 Co 0.15 Al 0.05 At least one of O2 and its modified compounds. Examples of lithium phosphates with an olivine structure include, but are not limited to, lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), lithium iron phosphate and carbon composites, lithium manganese phosphate (such as LiMnPO4), lithium manganese phosphate and carbon composites, lithium manganese iron phosphate, and lithium manganese iron phosphate and carbon composites.

[0120] During the charging and discharging process of a battery, Li undergoes insertion / extraction and consumption, resulting in varying molar Li content at different discharge states. In the examples of positive electrode active materials in this application, the molar Li content refers to the initial state of the material, i.e., the state before material addition. After charge-discharge cycles, the molar Li content changes when the positive electrode active material is applied to the battery system.

[0121] In the examples of positive electrode active materials for lithium-ion batteries in this application, the molar content of O is only a theoretical state value. Oxygen release from the crystal lattice will cause changes in the molar content of oxygen, and the actual molar content of O will fluctuate.

[0122] In some embodiments, when the battery is a sodium-ion battery, the positive electrode active material may be a positive electrode active material known in the art for sodium-ion batteries.

[0123] As an example, the positive electrode active material may include at least one of the following materials: sodium transition metal oxides, polyanionic compounds, and Prussian blue sodium compounds, and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may also be used. The modified compounds of the above materials may be for doping modification and / or surface coating modification of the materials.

[0124] In some embodiments, the transition metal in the sodium transition metal oxide can be at least one selected from Ti, V, Mn, Co, Ni, Fe, Zn, V, Zr, Ce, Cr, and Cu. The chemical formula of the sodium transition metal oxide can satisfy Na x MO2, wherein M includes at least one of Ti, V, Mn, Co, Ni, Fe, Zn, V, Zr, Ce, Cr, and Cu, and 0 < x ≤ 1.

[0125] In some embodiments, the polyanionic compound may be a compound containing sodium ions, transition metal ions, or a tetrahedral (YO4) structure. n- A class of compounds with anionic units. The transition metal may include at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce; Y may include at least one of P, S, and Si; n represents (YO4). n- The price state.

[0126] In some embodiments, the polyanionic compound may also be a sodium ion, transition metal ion, or tetrahedral (YO4) compound. n- A class of compounds containing anionic units and halide anions. Transition metals may include at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce; Y may include at least one of P, S, and Si, where n represents (YO4). n- The valence state of halogens can include at least one of F, Cl, and Br.

[0127] In some embodiments, the polyanionic compound may also be a tetrahedral compound containing sodium ions (YO4). n- Anionic unit, polyhedral unit (ZO) y ) m+ And a class of compounds with optional halide anions. M may include at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce, Y may include at least one of P, S and Si, and n represents (YO4). n- The valence state, Z represents transition metal, m represents (ZO) y ) m+ The valence state of halogens can include at least one of F, Cl, and Br.

[0128] As an example, polyanionic compounds can satisfy the chemical formulas NaFePO4, Na3V2(PO4)3 (sodium vanadium phosphate, abbreviated as NVP), Na4Fe3(PO4)2(P2O7), NaM'PO4F (M' includes at least one of V, Fe, Mn and Ni), and Na3(VO y )2(PO4)2F 3-2yAt least one of (0≤y≤1).

[0129] In some embodiments, Prussian blue compounds may be compounds containing sodium ions, transition metal ions, and cyanide ions (CN). - A class of compounds. Transition metals may include at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce.

[0130] As an example, Prussian blue compounds can satisfy the chemical formula Na a Me b Me' c (CN)6, wherein Me and Me' each independently include at least one of Ni, Cu, Fe, Mn, Co, and Zn, 0 < a ≤ 2, 0 < b < 1, and 0 < c < 1.

[0131] During the charging and discharging process of a battery, sodium (Na) undergoes insertion / extraction and consumption, resulting in varying molar Na content at different discharge states. In the examples of positive electrode active materials in this application, the molar Na content refers to the initial state of the material, i.e., the state before material addition. After charge-discharge cycles, the molar Na content changes when the positive electrode active material is applied to the battery system.

[0132] In the examples of positive electrode active materials in this application, the molar content of O is only a theoretical value. Oxygen release from the crystal lattice will cause changes in the molar content of oxygen, and the actual molar content of O will fluctuate.

[0133] In some embodiments of this application, the positive electrode active material layer may optionally include a binder. As an example, the binder may include at least one selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.

[0134] In some embodiments of this application, the positive electrode active material layer may optionally include a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0135] In some embodiments of this application, the positive electrode sheet can be prepared by dispersing the above-mentioned components for preparing the positive electrode sheet, such as positive active material, conductive agent, binder and any other components, in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry; coating the positive electrode slurry onto the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0136] In some embodiments of this application, the positive electrode sheet can be prepared by dispersing the positive electrode active material, conductive agent, binder and any other components in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry; coating the positive electrode slurry onto the positive electrode current collector, and after drying, cold pressing and other processes, forming a positive electrode active material layer; and then using spraying, secondary coating or other methods to composite the first lithium salt with the positive electrode active material layer on the surface of the positive electrode active material layer.

[0137] [Electrolytes]

[0138] The electrolyte acts as a conductor of ions between the positive and negative electrodes. This application does not impose specific restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel, or entirely solid.

[0139] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.

[0140] In some embodiments of this application, the solvent may be selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.

[0141] In some embodiments of this application, the electrolyte salt includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate.

[0142] In some embodiments of this application, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.

[0143] [Negative electrode plate]

[0144] In some embodiments, referring to the figures, the negative electrode sheet includes a negative current collector and a negative active material layer disposed on at least one side surface of the negative current collector, the negative active material layer including a negative active material.

[0145] As an example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode active material layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0146] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0147] In some embodiments, the negative electrode active material may be a negative electrode active material known in the art for use in batteries. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, etc. Silicon-based materials include at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Tin-based materials include at least one of elemental tin, tin oxide compounds, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0148] In some embodiments, the negative electrode active material layer may optionally include a binder.

[0149] As an example, the binder in the negative electrode active material layer may include at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0150] In some embodiments, the negative electrode active material layer may optionally include a conductive agent.

[0151] As an example, conductive agents include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0152] In some embodiments, the negative electrode active material layer may also optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).

[0153] In some embodiments, the negative electrode sheet can be prepared by dispersing the above-mentioned components for preparing the negative electrode sheet, such as negative electrode active material, conductive agent, binder and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto the negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing and other processes.

[0154] In some embodiments of this application, the positive electrode, the negative electrode, and the separator can be fabricated into an electrode assembly by a winding process or a stacking process.

[0155] In some embodiments of this application, the secondary battery may include an outer packaging. This outer packaging may be used to encapsulate the aforementioned electrode assembly and electrolyte.

[0156] In some embodiments of this application, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the secondary battery can also be a soft pack, such as a pouch. The material of the soft pack can be plastic; examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0157] This application does not impose any particular limitation on the shape of the secondary battery; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 1 This is an example of a square-structured secondary battery 5.

[0158] In some embodiments of this application, reference is made to Figure 2 The outer packaging may include a housing 51 and a top cover assembly 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the top cover assembly 53 can cover the opening to close the receiving cavity. A positive electrode, a negative electrode, and a separator can be formed into an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. ​​The secondary battery 5 may contain one or more electrode assemblies 52, which can be selected by those skilled in the art according to specific practical needs.

[0159] In some embodiments of this application, the secondary batteries can be assembled into a battery module, and the number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0160] Figure 3 This is battery module 4, used as an example. (See reference...) Figure 3 In battery module 4, multiple secondary batteries 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple secondary batteries 5 can be fixed in place using fasteners.

[0161] Optionally, the battery module 4 may also include a housing with a receiving space in which a plurality of secondary batteries 5 are received.

[0162] In some embodiments of this application, the battery modules described above can also be assembled into a battery pack. The number of battery modules contained in the battery pack can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery pack.

[0163] Figure 4 and Figure 5 This is battery pack 1 as an example. (See reference...) Figure 4 and Figure 5 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0164] In addition, this application also provides an electrical device, which includes the secondary battery described in the first aspect of this application, or the secondary battery prepared by the method described in the second aspect. The electrical device includes at least one of the secondary battery, battery module, or battery pack provided in this application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0165] As for the aforementioned electrical equipment, a secondary battery, battery module, or battery pack can be selected according to its usage requirements.

[0166] Figure 6 This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery for this device, a battery pack or battery module can be used.

[0167] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a rechargeable battery as their power source.

[0168] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0169] Example 1

[0170] (1) Preparation of the separating membrane:

[0171] Synthetic polymer emulsion: 1000g of each of the following monomers were weighed out according to a mass ratio of 100:35:10: ethyl acrylate (first monomer), acrylonitrile (second monomer), and acrylamide (third monomer). The monomers were mixed thoroughly. In a 5L four-necked flask equipped with a mechanical stirrer, thermometer, and condenser, 1000g of the mixed monomers, 20g of sodium dodecylbenzenesulfonate (emulsifier), 5g of potassium persulfate (initiator), and 1200g of deionized water were added. The mixture was stirred at high speed for 30 minutes to emulsify. Under nitrogen protection, the mixture was heated to 80℃ and reacted for 4 hours. The temperature was then lowered to below 40℃, the pH was adjusted to neutral, and the mixture was filtered to obtain the polymer emulsion.

[0172] Halloysite nanotubes were added to the polymer emulsion at a mass ratio of 90:10 and stirred until homogeneous to obtain a spray slurry. The halloysite nanotubes had a porosity of 35% and a specific surface area of ​​75 m². 2 / g, with a Dv50 particle size of 1.8μm, the aforementioned spray slurry was spray-dried to obtain an adhesive for the release membrane. The spray-drying conditions were: inlet air temperature 110℃, outlet air temperature 50℃, and air pressure 0.5kPa. The resulting adhesive had a Dv50 particle size of 6.8μm.

[0173] A commercially available PE microporous film with a thickness of 7 μm and an average pore size of 80 nm (from Zhuogao Electronics Technology Co., Ltd.) was used as the base film. The adhesive prepared above was stirred and mixed evenly in deionized water to obtain an adhesive slurry (solid content 20%). The adhesive slurry was sprayed onto both surfaces of the base film, dried to remove the solvent, and the polymer coating density on the base film was 1.5 g / m². 2 An isolation membrane is obtained.

[0174] (2) Preparation of positive electrode sheet

[0175] A positive electrode slurry was prepared by thoroughly mixing polyvinylidene fluoride (PVDF), lithium iron phosphate (LFP), conductive agent carbon black, and N-methylpyrrolidone (NMP) at a mass ratio of 1.2:60.38:0.42:38. The positive electrode slurry was then subjected to a process at 197 g / m³. 2The loading is uniformly coated on the positive current collector aluminum foil, and then dried, cold-pressed and cut to obtain the positive electrode sheet.

[0176] (3) Preparation of negative electrode sheet

[0177] Natural graphite, conductive agent acetylene black, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) were added to deionized water at a mass ratio of 95.5:1.2:1.6:1.7. The mixture was thoroughly stirred and mixed to prepare a negative electrode slurry (solid content 64%). This negative electrode slurry was then subjected to a concentration of 102 g / m³. 2 The loading amount is coated on the negative electrode current collector copper foil, and then dried, cold pressed and slit to obtain the negative electrode sheet.

[0178] (4) Preparation of electrolyte

[0179] At 25°C, ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain a mixed solvent. LiPF6 is then dissolved in the above mixed solvent to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.

[0180] (5) Battery manufacturing

[0181] The positive electrode, separator, and negative electrode are stacked, wound, and hot-pressed in sequence to obtain a battery cell. The battery cell is placed in an outer packaging, and the electrolyte prepared above is added. After processes such as encapsulation, standing, formation, and aging, a secondary battery is obtained.

[0182] The differences between the remaining embodiments and comparative examples and Example 1 are shown in Table 1. In Example 13, the mass ratio of polymer to porous material is 50:50; in Example 14, the mass ratio of polymer to porous material is 99:1; in Comparative Example 1, no porous material is added, and polymer emulsion is used directly as the spray-dried slurry. The parameters of the secondary battery are shown in Table 1.

[0183] Method for testing the areal density of the adhesive layer on the base film: Cut three 100mm × 100mm samples from the left, middle, and right sides, perpendicular to the coating direction of the release liner. Weigh each sample on an analytical balance with an accuracy of 0.0001 (m1). Then scrape off the adhesive layer and weigh it again (m2). Calculate the average areal density of the three samples, which is recorded as the areal density of the adhesive layer, in g / m³. 2 The formula is as follows: Surface density (g / m³) 2 = (m1-m2) / 0.01m1. The test results are shown in Table 1.

[0184] Table 1

[0185]

[0186] Scanning electron microscopy (SEM) images of the adhesives prepared in Example 4 and Comparative Example 1 were obtained respectively. Figure 7 , Figure 8 and Figure 9 ,from Figure 7 and Figure 8 It can be seen that, Figure 7 and Figure 8 In this process, acrylate copolymers and porous materials (haloysite nanotubes) together form secondary particles. The porous materials are located inside and on the surface of the secondary particles. The linear particles are the porous material, haloysite nanotubes, while the others are the main polymer. The binder prepared in Example 4 has significantly more pores on both the surface and inside due to the presence of porous materials. Figure 9 It can be seen that Comparative Example 1, without the addition of porous materials, forms a relatively dense secondary sphere with virtually no pores on its surface.

[0187] The secondary batteries of Examples 1-14 and Comparative Example 1 were tested as follows:

[0188] The aforementioned separator membrane was subjected to the following tests:

[0189] ① Adhesion between separator and electrode: The negative electrode and separator are overlapped and placed on a hot press. The hot press parameters are set as follows: temperature 25℃, pressure 7t, time 15s. A bonded separator / negative electrode sample is obtained by applying pressure. The separator / electrode sample is cut into rectangular strips of 150×20mm. The electrode side of the rectangular strip is attached to a steel plate with double-sided adhesive. At one end of the rectangular strip, the separator and electrode are separated by 2cm along the length direction to obtain the test sample.

[0190] Keep the steel plate horizontal and fix it with the lower clamp of the universal testing machine (Xieqiang Instrument Manufacturing (Shanghai) Co., Ltd., model CTM2100). Fix the peeled end of the separator as described above with the upper clamp of the universal testing machine and connect it to a tensile testing machine. Set the test conditions to a tensile rate of 20 mm / min and a horizontal pull of 10 cm. After the tensile force stabilizes, record the tensile force value. The adhesion force between the separator and the electrode is obtained by the ratio of the tensile force value to the sample width.

[0191] ② Ionic conductivity test of the separator: Preparation of a 2025 button cell for testing: In a vacuum glove box, a lithium sheet was placed in the negative electrode shell of the battery, and 150 μL of the electrolyte mentioned above was added. Then, the separator prepared above (with an area of ​​3.14 cm²) was placed in the box. 2 A 12μm thick coin cell was tightly attached to the lithium sheet, and then 25μL of the electrolyte was added. Finally, the positive electrode was placed on top and the cell was sealed. The assembled coin cell was removed from the vacuum glove box and left to stand for 24 hours for further testing. The tests specifically included: at an electrochemical workstation, at 10...-1 -10 6 The isolation film resistance Rb was obtained by testing within a frequency range of Hz, and the ionic conductivity σ (unit: S / cm) was calculated using the following formula:

[0192]

[0193] Where Rb is the bulk resistance of the isolation membrane, and L and S are the thickness and area of ​​the isolation membrane under test, respectively.

[0194] The battery cells in the aforementioned embodiments and comparative examples were tested as follows, and the test results are shown in Table 2.

[0195] Rate performance at room temperature and high temperature:

[0196] The CT-2001ALAND battery testing system from Wuhan Jinno Electronics was used. The testing environment was ambient temperature (25℃) and high temperature (60℃), with a voltage range of 2.8V-4.3V. The test cells assembled from the prepared electrode materials were subjected to five constant-current charge-discharge cycles at each rate: 0.2C, 0.5C, 1C, 2C, 5C, and 0.2C (1C = 200mAh). The battery discharge capacity corresponding to the fifth constant-current charge-discharge cycle at the first 0.2C rate was recorded as C1, and the battery discharge capacity corresponding to the fifth constant-current charge-discharge cycle at the second 0.2C rate was recorded as C2. The 0.2C rate performance P = (C2 / C1) × 100%. The test results are shown in Table 2.

[0197] Table 2

[0198]

[0199]

[0200] As can be seen from Table 2, in Examples 1-14 of this application, the addition of porous materials to the binder resulted in better adhesive strength and the secondary battery containing it exhibited excellent rate performance. In Comparative Example 1, no porous materials were added to the binder, and although the binder had good adhesive performance, the rate performance of the secondary battery was poor.

[0201] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," "some implementations," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0202] Although embodiments of this application have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this application. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this application.

Claims

1. A secondary battery, characterized in that, The secondary battery includes a positive electrode, an electrolyte, a separator, and a negative electrode. The separator includes a base membrane and an adhesive layer disposed on at least one side of the base membrane. The adhesive layer includes an adhesive, which includes a polymer and a porous material. The polymer includes an acrylate copolymer. The acrylate copolymer and the porous material together form secondary particles, and the porous material is located inside and / or on the surface of the secondary particles.

2. The secondary battery according to claim 1, characterized in that, The mass ratio of the polymer to the porous material is (60:40)-(95:5); and / or, The areal density of the adhesive layer on the base film is 1 g / m³. 2 -1.8g / m 2 .

3. The secondary battery according to claim 1 or 2, characterized in that, The mass ratio of the polymer to the porous material is (80:20)-(95:5).

4. The secondary battery according to any one of claims 1-3, characterized in that, The Dv50 particle size of the adhesive is 1μm-20μm.

5. The secondary battery according to any one of claims 1-4, characterized in that, The secondary battery satisfies one or more of the following conditions: At least some of the channels in the porous material penetrate the porous material; The porous material includes one or more of the following: molecular sieve, zeolite, mesoporous silica, halloysite nanotubes, diatomaceous earth, porous titanium dioxide, porous boron nitride, porous graphene, carbon nanotubes, hydrated aluminum silicate, and activated carbon.

6. The secondary battery according to any one of claims 1-5, characterized in that, The acrylate copolymer is formed by polymerization of monomers, wherein the monomers include one or more of a first monomer, a second monomer, and a third monomer, and the structure of the first monomer is shown in Formula 1: Wherein, R1 includes a hydrogen atom or a C1-C6 alkyl group, and R2 includes a substituted or unsubstituted C1-C6 alkyl group. 15 Alkyl, substituted or unsubstituted C3-C6 isobornyl, wherein the C1-C 15 The alkyl substituents include hydroxyl groups or C1-C6 alkyl groups; The structure of the second monomer is shown in Equation 2, and / or Equation 3: R3 includes hydrogen atoms or C1-C atoms. 18 The alkyl group, where R4 includes a hydrogen atom or a C1-C6 alkyl group; The structure of the third monomer is shown in Equation 4: R5 includes a hydrogen atom, a hydroxyl-substituted C1-C6 alkyl group or a C1-C6 alkoxy group, and R6 includes a hydrogen atom or a C1-C6 alkyl group.

7. The secondary battery according to claim 6, characterized in that, The secondary battery satisfies one or more of the following conditions: The first monomer includes at least one of the following: ethyl acrylate, n-butyl acrylate, n-propyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, cyclohexyl acrylate, isooctyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, vinyl acetate, trimethylolpropane triacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate. The second monomer includes at least one of acrylonitrile, methacrylonitrile, ethyl acrylonitrile, acrylic acid, methacrylic acid, butenoic acid, and heptenoic acid; The third monomer includes at least one of acrylamide, N-hydroxymethylacrylamide, and N-butoxymethylacrylamide.

8. The secondary battery according to claim 6 or 7, characterized in that, The polymer comprises a first monomer, a second monomer, and a third monomer, wherein the mass ratio of the first monomer, the second monomer, and the third monomer is 100:(1-70):(5-20).

9. A method for preparing a secondary battery, comprising a method for preparing a separator, characterized in that, The method for preparing the isolation membrane includes: The emulsifier, initiator, and polymer monomers are blended and stirred, and then heated to react to obtain a polymer emulsion. An emulsion of porous material and polymer is mixed and stirred, and then spray-dried to obtain an adhesive, wherein the polymer includes acrylate copolymers; The adhesive is disposed on at least one side of the base film to obtain a release film; The isolation membrane includes a base membrane and an adhesive layer disposed on at least one side of the base membrane. The adhesive layer includes an adhesive, which includes a polymer and a porous material. The polymer includes an acrylate copolymer. The acrylate copolymer and the porous material together form secondary particles, and the porous material is located inside and / or on the surface of the secondary particles.

10. The method according to claim 9, characterized in that, The adhesive is dispersed in a solvent and sprayed onto at least one side of the base film to obtain a release film.

11. The method according to claim 9 or 10, characterized in that, The porosity of the porous material is 5%-85%; and / or, The specific surface area of ​​the porous material is 10m². 2 / g-2000m 2 / g; and / or, The Dv50 particle size of the porous material is less than or equal to 3 μm.