Electrochemical devices and their preparation methods
By using a semi-dry fibrillation process of 1T′-MoS2xSe2(1-x) crystals and sulfur-carbon composite materials to form a three-dimensional network structure in lithium-sulfur batteries, the problems of lithium polysulfide migration and active material loss in lithium-sulfur batteries are solved, and high cycle stability and low charge transfer impedance of electrochemical devices under high sulfur loading are achieved.
Patent Information
- Application Number
- CN202611615482.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-17
AI Technical Summary
Soluble lithium polysulfides generated during the charging and discharging process of lithium-sulfur batteries are prone to migration, leading to irreversible loss of positive electrode active materials, affecting the capacity and rate performance of electrochemical devices and long-cycle stability. Existing improved materials have problems such as poor conductivity, insufficient chemical adsorption capacity, or low interfacial charge transport efficiency.
A three-dimensional network structure of inert polymer binder is formed by using 1T′-MoS2xSe2(1-x) crystal and sulfur-carbon composite material through a semi-dry fibrillation process. This network structure encapsulates the positive electrode composite film layer, providing a fast electron transport channel and efficient adsorption and conversion of lithium polysulfide products. Polytetrafluoroethylene (PTFE) is used as an inert polymer binder to ensure the connection stability of the crystal and that the active sites are not lost.
It significantly improves the 200-cycle retention rate of the electrochemical device under high sulfur loading, reduces the charge transfer impedance to 50Ω-90Ω, and improves the cycle stability to over 80%, thus solving the bottleneck of the traditional electrochemical device with a 200-cycle retention rate of only 60%.
Smart Images

Figure CN123120826A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrochemical device technology, and in particular to an electrochemical device and its preparation method. Background Technology
[0002] Lithium-sulfur batteries are considered a core development direction for next-generation high-energy-density electrochemical devices due to their extremely high theoretical energy density and abundant sulfur resources. However, lithium-sulfur batteries are mainly limited by the following bottlenecks: soluble lithium polysulfides generated during charging and discharging are prone to migration in the electrolyte, triggering a "shuttle effect" that leads to irreversible loss of the positive electrode active material, causing rapid capacity decay of the electrochemical device; simultaneously, the insulating properties of elemental sulfur and its discharge end product lithium sulfide in the positive electrode active material of lithium-sulfur batteries result in sluggish redox reaction kinetics at the positive electrode, affecting the rate performance and long-cycle stability of the battery device, especially in electrochemical devices with high sulfur loading, where these issues are more pronounced.
[0003] Existing technologies often use carbon materials or metal compounds to modify the separator and cathode of lithium-sulfur batteries; however, the following problems exist: simply adding carbon materials results in insufficient chemical adsorption capacity; simply adding metal compounds results in poor conductivity; or when carbon materials and metal compounds are added simultaneously, the physical interface between the carbon phase and the metal compound phase hinders the charge transport efficiency of the two phases, resulting in poor conductivity.
[0004] Molybdenum disulfide, molybdenum diselenide, and other transition metal chalcogenides possess conductivity, polar chemisorption capacity, and electrocatalytic activity, effectively addressing the problem of charge transport efficiency hindered by physical interfaces in traditional carbon-metal compound blends. Therefore, they exhibit high application potential in lithium-sulfur batteries, such as molybdenum trioxide and selenium dioxide in patent CN114267818 A, or molybdenum diselenide in patent CN 113839044 A. However, these transition metal chalcogenides, including molybdenum trioxide, selenium dioxide, and molybdenum diselenide, are all conventional stable 2H phases, exhibiting poor conductivity, insufficient chemisorption, and weak catalytic activity, significantly limiting their application in electrochemical devices.
[0005] To address the aforementioned technical issues, some researchers have attempted to utilize MoS2-transition metal single-atom-sulfur, as described in CN122370325A. This material modulates the electronic structure through dp hybridization between the MoS2 support and the transition metal single atom, thereby increasing the adsorption and conversion capabilities of polysulfides and promoting ion migration, thus giving it both ionic and electronic conductivity. However, due to the high interfacial contact resistance of the electrochemical device constructed from the transition metal single atom, MoS2, and sulfur, the electron transport and interfacial charge transfer capabilities of the MoS2-transition metal single-atom-sulfur material are poor, ultimately affecting the cycle stability of the battery device. In other words, traditional electrochemical devices typically only achieve a cycle retention rate of 60% after 200 cycles. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for adding 1T′-MoS 2x Se 2(1-x) The crystal possesses higher intrinsic electronic conductivity and a distorted lattice structure. Furthermore, the three-dimensional network structure of the inert polymer binder formed by the semi-dry fibrillation process enables the formation of 1T′-MoS₂. 2x Se 2(1-x) The encapsulation of crystals and sulfur-carbon composite materials effectively prevents 1T′-MoS 2x Se 2(1-x) An electrochemical device and its preparation method that effectively improves the cycle stability of an electrochemical device under high sulfur loading by removing crystals and sulfur-carbon composite materials.
[0007] The objective of this invention is achieved through the following technical solution: An electrochemical device includes a sulfur-based positive electrode, a negative electrode, an electrolyte, and a separator; the sulfur-based positive electrode is stacked with the negative electrode through the separator, and the electrolyte is respectively immersed between the sulfur-based positive electrode, the negative electrode, and the separator; the sulfur-based positive electrode includes a current collector and a positive electrode composite film layer disposed on the current collector, the positive electrode composite film layer comprising the following mass components: 30-70 parts of sulfur-carbon composite material; 1T′-MoS 2x Se 2(1-x) 5-15 parts of crystals; 15-25 parts of an inert polymer binder aqueous solution; Wherein, x satisfies 0 <x<1; The 1T′-MoS 2x Se 2(1-x) The crystals are mixed with the sulfur-carbon composite material and the inert polymer binder aqueous solution through a semi-dry fibrillation process, so that the inert polymer binder aqueous solution binds the sulfur-carbon composite material and the 1T′-MoS2x Se 2(1-x) The crystals are tightly interwoven and wrapped to form the positive electrode composite film; the 1T′-MoS 2x Se 2(1-x) The crystals provide a fast electron transport channel for the sulfur-carbon composite material and efficiently adsorb and convert the lithium polysulfide products generated by the sulfur-carbon composite material, enabling the electrochemical device to operate at 2.5 mg / cm³. 2 -6mg / cm 2 The retention rate after 200 cycles under high sulfur loading and current rate 2C-3C conditions is higher than 80%; the charge transfer impedance of the electrochemical device is 50Ω-90Ω; The inert polymer binder aqueous solution comprises an inert polymer binder and water, wherein the inert polymer binder is polytetrafluoroethylene (PTFE).
[0008] In one embodiment, the mass ratio of S to C in the sulfur-carbon composite material is (5-8):(1-3).
[0009] In one embodiment, the mass ratio of polymer binder to water in the inert polymer binder aqueous solution is 1:(2-5).
[0010] In one embodiment, the calendered thickness of the positive electrode composite film is 150μm-200μm.
[0011] In one embodiment, the diameter of the sulfur-based cathode is 8 mm-10 mm.
[0012] In one embodiment, the 1T′-MoS 2x Se 2(1-x) The method for preparing crystals includes the following steps: The molybdenum source, metal anion salt, sulfur source and selenium source were first ground and mixed in a mass ratio of (1-2):(3-6):y:(20-y) to obtain the reaction precursor; The reaction precursor was placed at 750℃-900℃ for 2-4 hours under a reducing atmosphere and an inert protective gas to obtain an alkali metal intercalation 1T′ precursor. The alkali metal intercalation 1T′ precursor was subjected to a water washing operation; The alkali metal intercalation 1T′ precursor, after being washed with water, is immersed in a reduction and displacement solution for reaction. The alkali-free metal intercalation 1T′ precursor was cleaned and dried to obtain the 1T′-MoS. 2x Se 2(1-x) Crystals; Wherein, y is an adjustable variable used to control the ratio of S / Se.
[0013] In one embodiment, the molybdenum source includes at least one of molybdenum oxide, molybdate, and molybdenum halide.
[0014] In one embodiment, the metal anion salt includes at least one selected from sodium carbonate, potassium carbonate, calcium carbonate, sodium sulfate, potassium sulfate, calcium sulfate, sodium oxalate, potassium oxalate, and calcium oxalate.
[0015] In one embodiment, the sulfur source includes at least one of sulfur powder, organic sulfides, and inorganic sulfides.
[0016] In one embodiment, the selenium source includes at least one of selenium powder, organic selenide, and inorganic selenide.
[0017] In one embodiment, the flow rate ratio of the reducing atmosphere to the inert protective gas is (20-40):(80-60).
[0018] In one embodiment, the reduction and displacement solution includes at least one of dilute sulfuric acid, iodine-acetonitrile solution, and acidic potassium dichromate solution.
[0019] In one embodiment, the alkali metal intercalation 1T′ precursor after soaking reaction is cleaned with water or acetonitrile solution and then vacuum dried at 15°C-30°C for 0.5-2 days.
[0020] In one embodiment, the grinding speed during the first grinding and mixing is 50 rpm / min-150 rpm / min, and the time is 5 min-10 min.
[0021] An electrochemical device preparation method is provided for preparing the electrochemical device described in any of the above embodiments, the electrochemical device preparation method comprising the following steps: sulfur-carbon composite material and 1T′-MoS 2x Se 2(1-x) The crystals are then subjected to a second grinding and mixing process to obtain a mixture. An inert polymer binder aqueous solution was added dropwise to the mixture to obtain a semi-dry mixture; The semi-dry mixture is subjected to multiple roll shearing processes to allow the inert polymer binder of the aqueous solution to bind the sulfur-carbon composite material and the 1T′-MoS2O3. 2x Se 2(1-x) The crystals are tightly interwoven and encapsulated, resulting in semi-dry inclusions; The semi-dry inclusions are calendered to obtain a self-supporting positive electrode composite film. The self-supporting positive electrode composite film is pressed onto the current collector to obtain the sulfur-based positive electrode sheet; Assembling the sulfur-based positive electrode sheet with the negative electrode sheet, electrolyte and separator to obtain the electrochemical device.
[0022] In one embodiment, the rotation speed of the second grinding and mixing is 50rpm / min-150rpm / min, and the duration is 5min-15min.
[0023] In one embodiment, the number of times of the multiple rolling shearing is 5 to 10, the rolling speed is 15mm / s-25mm / s, and the duration is 4min-8min.
[0024] Compared with the prior art, the present invention has at least the following advantages: 1) By setting x of 1T′-MoS 2x Se 2(1-x) crystal to satisfy 0<x<1, the stoichiometric ratio of Mo to anions S and anions Se in the layered molybdenum chalcogenide material can be reasonably controlled to be fixed at 1:2, so that S and Se are not simply physically mixed, but can be substituted at the lattice sites of the layered molybdenum chalcogenide material. In addition, since the atomic radius of Se is larger than that of S, the Se substituted by reasonable solid solution can introduce local tensile strain, bond length difference and charge redistribution in the lattice of the layered molybdenum chalcogenide material, which is beneficial to improve the asymmetry of the crystal structure, break the limitation of the stable and inert basal plane of the traditional conventional 2H phase, make the material change from "edge catalysis" as the main to "full-surface catalysis" as the main, and significantly increase the density of "lithiophilic-sulphiphilic" dual active sites. In this way, while reducing the structural symmetry, the heterogeneity of its surface electronic states is enhanced, which ensures that Se ions can be substituted by relatively uniform solid solution, and is conducive to promoting the formation of long-range ordered strip-shaped 1T′-MoS 2x Se 2(1-x) crystal, effectively reducing the structural defects of 1T′-MoS 2x Se 2(1-x) crystal, and is conducive to constructing high-density "lithiophilic-sulphiphilic" dual active sites on the surface of the 1T′-MoS 2x Se 2(1-x) crystal, so that S has lithiophilic sites, which helps to maintain a strong polar adsorption effect, Se has sulphiphilic sites, which helps to realize the anchoring of lithium polysulfide products, and also helps to improve the electron transfer ability and reaction kinetics of the 1T′-MoS 2x Se 2(1-x) crystal; it ensures that it has higher intrinsic electronic conductivity and a distorted lattice structure that is more conducive to surface charge transfer, which can provide a fast electron transmission channel for the conversion reaction of lithium polysulfide products, and further realize efficient adsorption and conversion of the lithium polysulfide products generated by the sulfur-carbon composite material, ensuring that 1T′-MoS 2x Se 2(1-x)The crystals can fully exert their catalytic activity to ensure that the charge transfer impedance of the final electrochemical device is 50Ω-90Ω, thereby ensuring that the electrochemical device operates at 2.5 mg / cm². 2 -6mg / cm 2 The retention rate of the device is higher than 80% after 200 cycles under high sulfur loading and current ratio 2C-3C conditions, which effectively breaks through the bottleneck that the retention rate of traditional electrochemical devices is only 60% after 200 cycles.
[0025] 2) Compared to traditional wet slurry coating processes, the prolonged NMP polar solvent wetting and subsequent high-temperature drying in wet slurry coating processes easily induce an irreversible phase transition from the 1T′ phase to the conventional 2H phase, and the 1T′-MoS phase... 2x Se 2(1-x) The lithium- and thiophilic dual active sites of the crystal are easily passivated and shielded by polar solvents, affecting the efficient adsorption and conversion performance of lithium polysulfide products; at the same time, 1T′-MoS 2x Se 2(1-x) The two-dimensional layered Mo-S / Se framework of the crystal is prone to agglomeration and stacking in a liquid environment, resulting in the loss of both lithophile-thiophile active sites; therefore, in this disclosure, the 1T′-MoS 2x Se 2(1-x) The crystals are mixed with the sulfur-carbon composite material and the inert polymer binder aqueous solution via a semi-dry fibrillation process. The inert polymer binder aqueous solution comprises an inert polymer binder and water, wherein the inert polymer binder is polytetrafluoroethylene (PTFE). This method introduces only a small amount of inert polymer binder aqueous solution, eliminating the need for prolonged liquid-phase immersion and high-temperature vacuum drying, thus maximizing the retention of 1T′-MoS. 2x Se 2(1-x) The 1T′ metastable phase and dual active sites of the crystal ensure 1T′-MoS 2x Se 2(1-x) The crystal possesses higher intrinsic electronic conductivity and a distorted lattice structure more conducive to surface charge transfer; simultaneously, through shear-induced inert polymer bonding aqueous solution, the inert polymer binder in the aqueous solution can interweave to form a three-dimensional network, and the formed three-dimensional network can bond the sulfur-carbon composite material and the 1T′-MoS 2x Se 2(1-x) The tightly interwoven crystals further stabilized 1T′-MoS. 2x Se 2(1-x) The bonding stability of Mo, S, and Se in the crystal is effectively improved, thus enhancing the stability of 1T′-MoS 2x Se 2(1-x) The problem of crystal transformation to the 2H phase and how to better avoid 1T′-MoS 2x Se 2(1-x)Crystalline or sulfur-carbon composite materials are prone to shedding during prolonged use, thus better ensuring the electrochemical device operates at 2.5 mg / cm³. 2 -6mg / cm 2 With high sulfur loading and current rate under 2C-3C conditions, the battery retains more than 80% of its capacity over 200 cycles, thus ensuring high cycle stability of the battery device.
[0026] 3) In addition, due to 1T′-MoS 2x Se 2(1-x) The crystals have a high density and are prone to sedimentation in wet slurries, leading to the formation of 1T′-MoS₂ crystals. 2x Se 2(1-x) The catalytic components of the crystal are unevenly distributed. However, the semi-dry fibrillation process used in this disclosure, through a second grinding and multiple rolling shearing processes, produces micron-sized 1T′-MoS₂ crystals. 2x Se 2(1-x) Crystals are uniformly distributed within the fibrillated three-dimensional network of the polymer adhesive, such as... Figure 3 As shown in Figure b, 1T′-MoS is guaranteed. 2x Se 2(1-x) The crystals can be evenly distributed across the positive electrode composite film layer, effectively avoiding the uneven sedimentation problem that exists in traditional wet methods. Attached Figure Description
[0027] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0028] Figure 1 In this paper, 'a' represents 1T′-MoS from Embodiment 1 of the present invention. 2x Se 2(1-x) Scanning electron microscope (SEM) images; Figure 1 In the middle b, 1T′-MoS is the 1T′-MoS in Embodiment 1 of the present invention. 2x Se 2(1-x) Energy dispersive X-ray spectroscopy (EDS) elemental distribution map of Mo in the corresponding region; Figure 1 c represents 1T′-MoS in Embodiment 1 of the present invention. 2x Se 2(1-x) Energy-dispersive X-ray spectroscopy (EDS) elemental distribution map of element S in the corresponding region; Figure 1 In this context, d represents 1T′-MoS from Embodiment 1 of the present invention. 2x Se2(1-x) Energy dispersive X-ray spectroscopy (EDS) elemental distribution map of Se element in the corresponding region; Figure 2 In Figure a, there is a comparison of the energy dispersive X-ray (EDS) spectra of Examples 1-4 and Comparative Examples 1-2 of the present invention; Figure 2 In Figure b, there is a comparison diagram of the X-ray diffraction (XRD) patterns of Examples 1-4 and Comparative Examples 1-2 of the present invention; Figure 2 In the middle c, there is a comparison diagram of the Raman spectra of Examples 1-4 and Comparative Examples 1-2 of the present invention; Figure 3 Image a is a scanning electron microscope (SEM) image of the sulfur-based cathode sheet of Comparative Example 1 of the present invention; Figure 3 Image b is a scanning electron microscope (SEM) image of the surface of the sulfur-based positive electrode sheet in Example 1 of the present invention; Figure 3 c is a scanning electron microscope (SEM) image of the sulfur-based cathode sheet of Comparative Example 2 of the present invention; Figure 4 In the figure, 'a' represents the lithium-sulfur battery of Example 1 and Comparative Examples 1-2 of this invention, with a scan rate of 0.1 mV / s. -1 CV curve comparison chart below; Figure 4 Figure b is a comparison diagram of the impedance spectra of lithium-sulfur batteries of Example 1 and Comparative Examples 1-2 of the present invention; Figure 5 Figure a is a comparison of the first-cycle constant current charge-discharge curves (GCD) of the lithium-sulfur batteries of Example 1 and Comparative Examples 1-2 at 0.1C. Figure 5 Figure b is a partial comparison of the first-cycle constant current discharge curves of the lithium-sulfur batteries of Example 1 and Comparative Examples 1-2 at 0.1C. Figure 5 In Figure c, the charging curves of the lithium-sulfur batteries of Example 1 and Comparative Examples 1-2 at 0.1C are compared. Figure 6 In Figure a, the lithium-sulfur batteries of Example 1 and Comparative Examples 1-2 are compared in terms of cycle stability performance at 2C. Figure 6 In Figure b, the lithium-sulfur battery of Comparative Example 1 of this invention operates at 2C and 2.9 mg / cm³. 2 The constant current charge-discharge curve under the given conditions; Figure 6 In the figure, c represents the lithium-sulfur battery of Example 1 of the present invention at 2C and 2.9 mg / cm³. 2 The constant current charge-discharge curve under the given conditions; Figure 6In the figure, d represents the lithium-sulfur batteries of Comparative Examples 1-2 of this invention at 2C and 2.9 mg / cm³. 2 The constant current charge-discharge curve under the given conditions; Figure 7 In Figure 'a', the lithium-sulfur battery of Example 1 of this invention operates at 3C and 5.5 mg / cm³. 2 The cyclic stability performance under the given conditions is shown in the figure. Figure 7 In Figure b, the lithium-sulfur battery of Example 1 of this invention operates at 3C and 5.5 mg / cm³. 2 The constant current charge-discharge curve under the given conditions. Detailed Implementation
[0029] The present application will be further described in detail below with reference to the embodiments and examples. It should be understood that these embodiments and examples are for illustrative purposes only and are not intended to limit the scope of the present application. The purpose of providing these embodiments and examples is to enable a more thorough and comprehensive understanding of the disclosure of the present application. It should also be understood that the present application can be implemented in many different forms and is not limited to the embodiments and examples described herein. Those skilled in the art can make various modifications or alterations without departing from the spirit of the present application, and the equivalent forms obtained also fall within the protection scope of the present application. Furthermore, numerous specific details are set forth in the following description to provide a fuller understanding of the present application. It should be understood that the present application can be implemented without one or more of these details.
[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0031] In this invention, the technical features described in an open-ended manner include both closed-ended technical solutions composed of the listed features and open-ended technical solutions that include the listed features.
[0032] In the present invention, where numerical intervals (i.e., numerical ranges) are involved, unless otherwise specified, optional numerical values are regarded as continuous within the above numerical interval, and include the two numerical endpoints (i.e., the minimum value and the maximum value) of the numerical range, as well as every numerical value between the two numerical endpoints. Unless otherwise specified, when a numerical interval refers only to integers within that numerical interval, it includes the two endpoint integers of the numerical range, as well as every integer between the two endpoints, which in this document is equivalent to explicitly enumerating every integer. For example, t being an integer selected from 1 to 10 means t is any integer selected from the integer group consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10. In addition, when multiple ranges are provided to describe a feature or characteristic, these ranges may be combined. In other words, unless otherwise indicated, the ranges disclosed in this document shall be construed to include any and all subranges subsumed therein.
[0033] The temperature parameters in the present invention, unless otherwise specifically limited, allow either constant temperature treatment or variation within a certain temperature interval. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument, and the fluctuation is allowed within a range of, for example, ±5°C, ±4°C, ±3°C, ±2°C, or ±1°C.
[0034] For a better understanding of the present application, the present application is further explained and described as follows: An electrochemical device according to one embodiment includes a sulfur-based positive electrode sheet, a negative electrode sheet, an electrolyte and a separator; the sulfur-based positive electrode sheet and the negative electrode sheet are arranged in a stacked manner with the separator interposed therebetween, and the electrolyte wets the sulfur-based positive electrode sheet, the negative electrode sheet and the separator respectively; the sulfur-based positive electrode sheet includes a current collector and a positive electrode composite film layer disposed on the current collector, and the positive electrode composite film layer includes the following components in parts by mass: 30 to 70 parts of a sulfur-carbon composite material; 1T′-MoS 2x Se 2(1-x) crystal: 5 to 15 parts; inert polymer binder aqueous solution: 15 to 25 parts, wherein x satisfies 0<x<1; the 1T′-MoS 2x Se 2(1-x) crystal is mixed with the sulfur-carbon composite material and the inert polymer binder aqueous solution through a semi-dry fibrillation process, so that the inert polymer binder in the inert polymer binder aqueous solution tightly interweaves and wraps the sulfur-carbon composite material and the 1T′-MoS 2x Se 2(1-x) crystal to form the positive electrode composite film layer; the 1T′-MoS 2x Se 2(1-x) crystal is configured to provide a fast electron transmission channel for the sulfur-carbon composite material and efficiently adsorb and convert lithium polysulfide products generated by the sulfur-carbon composite material, so that the electrochemical device achieves a performance at 2.5 mg / cm 2-6mg / cm 2 The 200-cycle retention rate under the conditions of high sulfur loading and a current rate of 2C-3C is higher than 80%; the charge transfer impedance of the electrochemical device is 50Ω-90Ω; the inert polymer binder aqueous solution includes an inert polymer binder and water, and the inert polymer binder is polytetrafluoroethylene (PTFE).
[0035] It should be noted that some scholars have attempted to introduce an alloying strategy, for example, introducing some transition metal anions such as Se to partially substitute S to form molybdenum sulfur selenide alloy crystals. Se atoms have low electronegativity and large atomic radius, which can theoretically adjust the energy band structure, generate lattice strain and introduce anion vacancies, thereby improving the electrical conductivity and ion diffusion kinetics of the material to a certain extent. However, when the ratio of the introduced anions S, anions Se and Mo is too high or too low, it is difficult to fully overcome the problems of basal plane inertness and limited electrical conductivity of the 2H phase, so that the finally prepared molybdenum sulfur selenide alloy crystal is a mixed phase with multiple domains coexisting, that is, there are problems of chemical disorder and numerous structural defects, and 1T' phase molybdenum sulfur selenide alloy crystals cannot be formed.
[0036] Therefore, in the present disclosure, by setting x of 1T'-MoS 2x Se 2(1-x) crystal to satisfy 0<x<1, the stoichiometric relationship between Mo and anions S, anions Se in the layered molybdenum chalcogenide material can be reasonably controlled to be fixed at 1:2, so that S and Se are not simply physically mixed, but can be substituted at the lattice sites of the layered molybdenum chalcogenide material. In addition, the atomic radius of Se is larger than that of S, so that Se substituted by reasonable solid solution can introduce local tensile strain, bond length difference and charge redistribution in the lattice of the layered molybdenum chalcogenide material, which is beneficial to improve the asymmetry of the crystal structure, break the limitation of stable and inert basal plane of the traditional conventional 2H phase, make the material change from "edge catalysis" as the main to "full-surface catalysis" as the main, and significantly increase the density of "lithiophilic-sulfiphilic" dual active sites. In this way, while reducing the structural symmetry, the heterogeneity of its surface electronic states is enhanced, ensuring that Se ions can be substituted by relatively uniform solid solution, which is beneficial to promoting the formation of long-range ordered strip-shaped 1T'-MoS 2x Se 2(1-x) crystal, effectively reducing the structural defects of 1T'-MoS 2x Se 2(1-x) crystal, and facilitating the construction of high-density "lithiophilic-sulfiphilic" dual active sites on the surface of 1T'-MoS 2x Se 2(1-x) crystal, so that S has lithiophilic sites, which helps to maintain a strong polar adsorption effect, Se has sulfiphilic sites, which helps to realize the anchoring of lithium polysulfide products, and also helps to improve 1T'-MoS 2x Se 2(1-x)The crystal's electron transfer capability and reaction kinetics are optimized; ensuring higher intrinsic electronic conductivity and a distorted lattice structure more favorable for surface charge transfer, it provides a rapid electron transport channel for the conversion reaction of lithium polysulfide products, thereby achieving efficient adsorption and conversion of lithium polysulfide products generated from the sulfur-carbon composite material, and ensuring the high efficiency of 1T′-MoS₂. 2x Se 2(1-x) The crystals can fully exert their catalytic activity to ensure that the charge transfer impedance of the final electrochemical device is 50Ω-90Ω, thereby ensuring that the electrochemical device operates at 2.5 mg / cm². 2 -6mg / cm 2 The retention rate of the device is higher than 80% after 200 cycles under high sulfur loading and current ratio 2C-3C conditions, which effectively breaks through the bottleneck that the retention rate of traditional electrochemical devices is only 60% after 200 cycles.
[0037] In other words, traditional 2H phase MoS2 or MoSe2 belongs to a highly symmetric semiconductor structure with relatively saturated basal plane atomic coordination, a relatively uniform surface electron distribution, and activity mainly concentrated at the edge sites, thus exhibiting strong basal plane chemical inertness. In contrast, the 1T′-MoS2 prepared by controlling the stoichiometric ratio of Mo to anions S and Se in this disclosure... 2x Se 2(1-x) The crystal exhibits higher electronic conductivity and lower structural symmetry, providing faster electron transport channels and more active surface electronic states, which is more conducive to the activation of basal plane sites. Specifically, the 1T′ phase primarily improves the poor conductivity and slow electron transfer of the 2H phase semiconductor, while Se further enhances the local strain and electronic polarization effects under the low-symmetry structure. The synergistic effect of these two phases can enhance the 1T′-MoS₂ 2x Se 2(1-x) The crystal structure shifts from "edge-dominated catalysis" to "basal-edge synergistic catalysis," thereby more effectively promoting the adsorption, activation, deposition, and decomposition of lithium polysulfides, and thus better utilizing 1T′-MoS 2x Se 2(1-x) The catalytic activity that crystals should possess.
[0038] It is also understandable that, compared to traditional wet slurry coating processes, the prolonged wetting with the polar NMP solvent and subsequent high-temperature drying in wet slurry coating processes easily induce an irreversible phase transition of the 1T′ phase to the conventional 2H phase, meaning that the 1T′ metastable phase cannot be well preserved; and 1T′-MoS 2x Se 2(1-x) The lithium- and thiophilic dual active sites of the crystal are easily passivated and shielded by polar solvents, affecting the efficient adsorption and conversion performance of lithium polysulfide products; at the same time, 1T′-MoS 2x Se 2(1-x)The two-dimensional layered Mo-S / Se framework of the crystal is prone to agglomeration and stacking in the liquid phase environment, which can lead to the loss of both lithophile-thiophile active sites.
[0039] Therefore, in this disclosure, the 1T′-MoS 2x Se 2(1-x) The crystals are mixed with the sulfur-carbon composite material and the inert polymer binder aqueous solution via a semi-dry fibrillation process. The inert polymer binder aqueous solution comprises an inert polymer binder and water, wherein the inert polymer binder is polytetrafluoroethylene (PTFE). This method introduces only a small amount of inert polymer binder aqueous solution, eliminating the need for prolonged liquid-phase immersion and high-temperature vacuum drying, thus maximizing the retention of 1T′-MoS. 2x Se 2(1-x) The 1T′ metastable phase and dual active sites of the crystal effectively suppress the structural degradation of the 1T′ metastable phase during the preparation process, thereby ensuring the stability of 1T′-MoS₂. 2x Se 2(1-x) The crystal possesses higher intrinsic electronic conductivity and a distorted lattice structure more conducive to surface charge transfer; simultaneously, through shear-induced inert polymer bonding aqueous solution, the inert polymer binder in the aqueous solution can interweave to form a three-dimensional network, and the formed three-dimensional network can bond the sulfur-carbon composite material and the 1T′-MoS 2x Se 2(1-x) The tightly interwoven crystals further stabilized 1T′-MoS. 2x Se 2(1-x) The bonding stability of Mo, S, and Se in the crystal is effectively improved, thus enhancing the stability of 1T′-MoS 2x Se 2(1-x) The problem of crystal transformation to the 2H phase and how to better avoid 1T′-MoS 2x Se 2(1-x) Crystalline or sulfur-carbon composite materials are prone to shedding during prolonged use, thus better ensuring the electrochemical device operates at 2.5 mg / cm³. 2 -6mg / cm 2 With high sulfur loading and current rate under 2C-3C conditions, the battery retains more than 80% of its capacity over 200 cycles, thus ensuring high cycle stability of the battery device.
[0040] Furthermore, due to 1T′-MoS 2x Se 2(1-x) The crystals have a high density and are prone to sedimentation in wet slurries, leading to the formation of 1T′-MoS₂ crystals. 2x Se 2(1-x) The catalytic components of the crystal are unevenly distributed. However, the semi-dry fibrillation process used in this disclosure, through a second grinding and multiple rolling shearing processes, produces micron-sized 1T′-MoS₂ crystals. 2x Se 2(1-x)The crystals are uniformly distributed in the fibrillated three-dimensional network of the polymer adhesive, as shown in Figure 3 in b, which ensures that the 1T′-MoS 2x Se 2(1-x) crystals can be relatively uniformly covered and distributed on the positive electrode composite film layer, effectively avoiding the problem of uneven sedimentation existing in the conventional wet process.
[0041] It should be noted that the three-dimensional network formed by mixing the inert polymer binder aqueous solution through the semi-dry fibrillation process can provide good structural support and protection for the 1T′-MoS 2x Se 2(1-x) crystals, ensuring that the finally prepared positive electrode composite film layer is a self-supporting positive electrode composite film layer. The three-dimensional network can buffer the volume expansion and contraction of the active material during charge and discharge, suppress the generation of penetrating microcracks inside the self-supporting positive electrode composite film layer, maintain the structural integrity of the high sulfur loading thick electrode film body, allow the volume stress generated by charge and discharge to be partially dissipated in advance by the three-dimensional network inside the self-supporting positive electrode composite film layer, reduce the stress borne by the interface between the self-supporting positive electrode composite film layer and the current collector, suppress delamination and powder falling failure during 200 weeks of long cycles, and improve the cycle capacity retention rate at 2C-3C rate under high sulfur loading conditions; it also reduces the interface contact impedance between the self-supporting positive electrode composite film layer and the current collector, makes the current distribution more uniform at the high 2C-3C rate, and further reduces the charge transfer impedance of the sulfur-based positive electrode sheet.
[0042] In one embodiment, x satisfies 0.15<x<0.4; y satisfies 4<y<12, such as x=0.15, 0.25, 0.3 and 0.4.
[0043] In one embodiment, the molecular weight of polytetrafluoroethylene (PTFE) is 50,000-60,000, which ensures that the molecular weight of polytetrafluoroethylene is relatively appropriate, and ensures that polytetrafluoroethylene can be stretched to form a continuous nanofibril network under the action of multiple rolling and shearing, so as to achieve good encapsulation of the sulfur-carbon composite material and the 1T′-MoS 2x Se 2(1-x) crystals, effectively avoiding insufficient molecular chain entanglement when the molecular weight of polytetrafluoroethylene is too low, which leads to easy chain breakage under shearing and failure to form a continuous fiber three-dimensional network; and effectively avoiding excessively strong molecular entanglement when the molecular weight of polytetrafluoroethylene is too high, which leads to difficulty in dispersion and short fibrils that are easy to break.
[0044] In one embodiment, the mass ratio of S to C in the sulfur-carbon composite material is (5-8):(1-3), so as to ensure that the content of the sulfur active material and the content of the conductive carbon material reach an appropriate balance, build a good conductive network while ensuring a high sulfur content, improve the utilization rate of the sulfur active material, and avoid the decrease of sulfur utilization rate or the reduction of the energy density of the electrode.
[0045] In one embodiment, the mass ratio of polymer binder to water in the inert polymer binder aqueous solution is 1:(2-5), ensuring that the added water content is appropriate. This guarantees that the added water can produce 30-70 parts of sulfur-carbon composite material and 5-15 parts of 1T′-MoS2. 2x Se 2(1-x) While thoroughly and uniformly mixing the crystals and 15-25 parts of an inert polymer binder aqueous solution, it is also ensured that the added water can be vacuum dried at room temperature within a short time, thereby maximizing the retention of 1T′-MoS 2x Se 2(1-x) The 1T′ metastable phase and dual active sites of the crystal.
[0046] Furthermore, the room temperature is 25℃-30℃, and the vacuum drying time is 10h-12h.
[0047] In one embodiment, the calendered thickness of the positive electrode composite film is 150μm-200μm to ensure that the positive electrode composite film has suitable mechanical strength and self-supporting properties, while taking into account electron transport, lithium ion diffusion and electrolyte wetting. This avoids the positive electrode composite film being too thick, which would lead to an excessively long ion transport path and increased polarization, or the positive electrode composite film being too thin, which would lead to insufficient electrode mechanical strength and reduced active material loading.
[0048] In one embodiment, the diameter of the sulfur-based positive electrode is 8mm-10mm, which facilitates the size matching and stable assembly of the sulfur-based positive electrode with the separator, negative electrode and battery casing, ensuring the consistency of the size of the sulfur-based positive electrode and the effective reaction area, avoiding assembly interference caused by the sulfur-based positive electrode being too large, or insufficient utilization of the active area caused by the sulfur-based positive electrode being too small.
[0049] It should be noted that most molybdenum sulfide selenide alloys are currently prepared using an oxygen-assisted system, such as the single-layer molybdenum sulfide selenide alloy composition disclosed in patent CN113278949A. This involves first cleaning high-purity molybdenum foil, then adding sodium bromide alkali metal halide, followed by introducing an oxygen-argon mixed gas and reacting in the central temperature zone of a high-temperature CVD tube furnace to obtain the single-layer molybdenum sulfide selenide alloy composition. However, because the molybdenum sulfide selenide alloy in this patent has a problem where introducing a trace amount of O2 during the reaction oxidizes the sodium bromide and releases Na+, this process can lead to the formation of a single-layer molybdenum sulfide selenide alloy. + ; make Na + Unable to be stably adsorbed at the growth interface, and unable to achieve effective electron doping, sodium bromide alkali metal halide only acts as a gas phase transport aid, improving the monolayer morphology, but loses the ability to induce phase transformation and cannot form 1T′ phase molybdenum sulfide selenide alloy.
[0050] Furthermore, although the transformation from the 2H phase to the 1T′ phase can be induced and promoted to some extent by reasonably setting the stoichiometric relationship between Mo and the anions S and Se, simple Se anion substitution can only produce local disorder distortion, resulting in the final preparation of 1T′-MoS. 2x Se 2(1-x) The crystal is a mixed product of 2H and 1T′ phases with a small amount of distorted domains, which has uncontrollable phase composition and poor reproducibility of preparation. That is, the ability of reasonably substituted Se to introduce local tensile strain, bond length difference and charge redistribution in the lattice of layered molybdenum chalcogenide materials is limited, and there is a lack of charge transfer driving force to drive molybdenum atoms to reconstruct from trigonal prism coordination to distorted octahedral coordination.
[0051] Therefore, in one embodiment, 1T′-MoS was prepared using a salt-assisted gas-solid phase synthesis method. 2x Se 2(1-x) The crystals, because the salt is a metal anion salt, cause the added metal anion salt to melt and decompose under high temperature conditions, continuously releasing alkali metal cations. The released alkali metal cations can reach 1T′-MoS 2x Se 2(1-x) Simultaneous crystal nucleation and growth enables intercalation of alkali metal cations, allowing these cations to inject charge into the molybdenum (Mo) atomic framework. This provides the charge transfer driving force for the reconfiguration of Mo from trigonal prism coordination to distorted octahedral coordination, thereby inducing the transformation from the conventional 2H phase to the 1T′ phase. In other words, the metal anion salt effectively performs electron doping. Simultaneously, the inserted alkali metal cations act as pinning agents, effectively suppressing the transformation of Mo to the 2H phase. This effectively preserves the metastable 1T′ phase and the dual active sites, facilitating the preparation of high-purity 1T′-MoS₂. 2x Se 2(1-x) The crystals are produced by soaking and washing with a reduction-displacement solution, resulting in a simple preparation process with high yield, good reproducibility, and ease of large-scale production. Furthermore, it induces the formation of high-purity 1T′-MoS₂. 2x Se 2(1-x) Crystals have higher intrinsic electronic conductivity and distorted lattice structures that are more conducive to surface charge transfer.
[0052] In one embodiment, 1T′-MoS 2x Se 2(1-x) High phase purity of crystals refers to a purity of 95%-100% for the 1T′ phase, with few impurities.
[0053] In this disclosure, the 1T′-MoS 2x Se 2(1-x)The crystal preparation method includes the following steps: First, a molybdenum source, a metal anion salt, a sulfur source, and a selenium source are ground and mixed in a mass ratio of (1-2):(3-6):y:(20-y), wherein y is an adjustable variable used to control the S / Se ratio; this ensures that the sulfur source and selenium source are uniformly distributed in the reaction precursor, thereby ensuring that Se ions can be uniformly dissolved and substituted, which is beneficial to promoting the formation of long-range ordered elongated morphology 1T′-MoS 2x Se 2(1-x) Crystals are formed; then, under a reducing atmosphere and an inert protective gas, the reaction precursor is kept at 750℃-900℃ for 2-4 hours to obtain an alkali metal intercalation 1T′ precursor; the molybdenum source is gradually converted into a low-valence molybdenum source under a high-temperature reducing atmosphere, and can further react with S and Se to form a layered Mo-S / Se framework; while the added metal anion salt can melt or decompose under a high-temperature reducing atmosphere to release low-valence alkali metal ions of monovalent or divalent alkali metal cations, and the generated low-valence alkali metal ions are formed in 1T′-MoS 2x Se 2(1-x) Simultaneously with crystal nucleation and growth, the material can be in-situ, uniformly, and slowly inserted into the interlayer of molybdenum sulfide selenide, causing charge transfer in the molybdenum atomic framework. The inserted low-valence alkali metal ions act as pinning agents, inhibiting the coordination rearrangement of molybdenum atoms towards the 2H phase. This effectively induces the transformation from the conventional 2H phase to the 1T′ phase without causing severe lattice distortion. Furthermore, under high-temperature reducing atmosphere conditions, the metal anions melt, forming a localized molten salt liquid phase environment that acts as a flux. This molten salt medium can enhance the solid-phase atomic diffusion rate of the molybdenum, sulfur, and selenium sources, regulate the molten salt viscosity and nucleation rate, achieve uniform mass transfer of materials, and avoid severe lattice distortion caused by intense local reactions. The process involves a transformation in which, under Se-rich, high-temperature, and reducing conditions, Se metal ions and low-valence alkali metal ions can intercalate into the layered Mo-S / Se framework. This achieves solid-solution substitution of S by Se and induces its transformation to the 1T′ phase, yielding a high-1T′ phase alkali metal intercalated 1T′ precursor. The alkali metal intercalated 1T′ precursor is then washed with water. Following this, the washed alkali metal intercalated 1T′ precursor is immersed in a reducing displacement solution. Finally, the alkali metal-free 1T′ precursor is washed and dried to effectively remove excess unreacted molybdenum source, metal anions, sulfur source, and selenium source, resulting in a high-phase-purity 1T′-MoS. 2x Se 2(1-x) Crystal.
[0054] The above-mentioned 1T′-MoS 2x Se 2(1-x) The crystal preparation method not only boasts advantages such as simple preparation process, high yield, good reproducibility, and ease of large-scale production, but also facilitates the induction of high-purity 1T′-MoS₂. 2xSe 2(1-x) crystal, thereby ensuring that the added 1T′-MoS 2x Se 2(1-x) crystal has higher intrinsic electronic conductivity and a distorted lattice structure that is more favorable for surface charge transfer.
[0055] A method for preparing 1T′-MoS according to an embodiment 2x Se 2(1-x) crystal comprises part or all of the following steps: S101. First, a molybdenum source, a metal acid radical salt, a sulfur source and a selenium source are subjected to first grinding and mixing at a mass ratio of (1-2):(3-6):y:(20-y) to obtain a reaction precursor, wherein y is an adjustable variable for controlling the S / Se ratio; it is ensured that the sulfur source and the selenium source can be uniformly distributed in the reaction precursor, so that Se ions can be uniformly dissolved and substituted, which is beneficial to promoting the formation of long-range ordered strip-shaped 1T′-MoS 2x Se 2(1-x) crystal. Further, y satisfies 0<y<20; it is ensured that x in the finally prepared long-range ordered strip-shaped 1T′-MoS 2x Se 2(1-x) crystal satisfies 0<x<1, which is beneficial to inducing the formation of a stable 1T′ metastable phase and dual active sites.
[0056] In a preferred embodiment, y satisfies 4<y<15, and x satisfies 0.15≤x≤0.4.
[0057] In one embodiment, the molybdenum source comprises at least one of molybdenum oxide, molybdate and molybdenum halide.
[0058] In one embodiment, the metal acid radical salt comprises at least one of sodium carbonate, potassium carbonate, calcium carbonate, sodium sulfate, potassium sulfate, calcium sulfate, sodium oxalate, potassium oxalate and calcium oxalate.
[0059] It can be understood that since sodium carbonate, potassium carbonate, calcium carbonate, sodium sulfate, potassium sulfate, calcium sulfate, sodium oxalate, potassium oxalate and calcium oxalate are all oxygen-containing acid radical metal salts, they can be melted or decomposed in a high-temperature reducing atmosphere to release low-valent alkali metal ions of monovalent alkali metal cations or divalent alkali metal cations, and the generated low-valent alkali metal ions act on 1T′-MoS 2x Se 2(1-x)During crystal nucleation and growth, the cations can be inserted in situ, uniformly, and slowly into the interlayer of molybdenum sulfoselenide (MoS2), causing charge transfer in the molybdenum atomic framework. Simultaneously, the inserted low-valence alkali metal ions act as pinning agents, effectively inducing the transformation from the conventional 2H phase to the 1T′ phase without causing severe lattice distortion. This effectively avoids the problem of high-valence metal cations having high charge density and strong Coulomb repulsion between ions, which prevents local embedding from driving the reconstruction of molybdenum atoms from trigonal prism coordination to distorted octahedral coordination. In other words, the in-situ inserted low-valence alkali metal cations can suppress the coordination rearrangement of molybdenum atoms to the 2H phase, ensuring that the generated 1T′ will not transform into the 2H phase even after holding at a high temperature of 750℃-900℃ for 2-4 hours, thus significantly improving the 1T′-MoS2 phase. 2x Se 2(1-x) The crystal preparation efficiency is improved; it also effectively avoids the problem of strong electrostatic bonding between high-valence metal cations and negatively charged molybdenum sulfide selenide layers, which easily leads to severe lattice distortion and a large number of crystal defects; and it facilitates the replacement of low-valence alkali metal ions during subsequent soaking reactions, which not only simplifies subsequent operations but also facilitates the preparation of long-range ordered 1T′-MoS with high phase purity, 1T′ metastable phase stability, high-density active sites across the entire surface, and excellent polysulfide conversion ability. 2x Se 2(1-x) Crystalline. Furthermore, under high-temperature reducing atmosphere conditions, the metal anion salt melts, forming a localized molten salt liquid phase environment, acting as a flux. This molten salt medium can enhance the solid-phase atomic diffusion rate of molybdenum, sulfur, and selenium sources, regulate the molten salt viscosity and nucleation rate, achieve uniform mass transfer of materials, and avoid severe lattice distortion caused by intense local reactions, thus realizing the salt-assisted reaction medium of the metal anion salt. Therefore, the added metal anion salt has a dual function: serving as both a salt-assisted reaction medium and an alkali metal intercalation doping source.
[0060] It is worth mentioning that the low charge density of the in-situ inserted low-valence alkali metal cations results in weak electrostatic bonding between them and the negatively charged two-dimensional layered Mo-S / Se framework. This allows for a mild topological ion exchange reaction during the subsequent reduction-displacement solution immersion reaction, ensuring that interlayer depletion and laminar collapse do not occur. This ensures the stability of the distorted octahedral framework of the two-dimensional layered Mo-S / Se framework throughout the exchange process, avoiding the problem of strong chemical potential-driven drastic perturbation of the crystal framework leading to a 2H phase transformation. Simultaneously, the low migration and diffusion barrier of low-valence alkali metals between the 1T′ phase layers ensures that interlayer ion exchange can be completed in a short immersion time, reducing the time the metastable framework is exposed to the perturbed environment. This further stabilizes and preserves the 1T′ phase crystal structure, which is beneficial for preparing 1T′-MoS with high phase purity, stable 1T′ metastable phase, high-density active sites across the entire surface, and excellent polysulfide conversion ability. 2x Se 2(1-x) Crystal.
[0061] In one embodiment, the sulfur source includes at least one of sulfur powder, organic sulfides, and inorganic sulfides.
[0062] In one embodiment, the selenium source includes at least one of selenium powder, organic selenide, and inorganic selenide.
[0063] In one embodiment, the grinding speed during the first grinding and mixing process is 50 rpm / min-150 rpm / min. Under these grinding and mixing conditions, the particle size of the molybdenum source, metal anion salt, sulfur source, and selenium source can be effectively reduced, thereby increasing the contact area of the molybdenum source, metal anion salt, sulfur source, and selenium source. This ensures that the molybdenum source, sulfur source, and selenium source are uniformly dispersed at the microscale, avoiding component segregation or the formation of MoS2 or MoSe2 impurity phases caused by local S / Se imbalances. This is beneficial for obtaining 1T′-MoS with uniform composition and high phase purity. 2x Se 2(1-x) Crystal, namely, high-phase-purity 1T′-MoS 2x Se 2(1-x) Crystal.
[0064] S102. Under a reducing atmosphere and an inert protective gas, the reaction precursor is kept at 750℃-900℃ for 2-4 hours to obtain an alkali metal intercalation 1T′ precursor. The molybdenum source is gradually converted into a low-valent molybdenum source under a high-temperature reducing atmosphere, and can further react with S and Se to form a layered Mo-S / Se framework. The added metal anion salt can melt or decompose under a high-temperature reducing atmosphere, releasing low-valent alkali metal ions, either monovalent or divalent alkali metal cations. The generated low-valent alkali metal ions are then used in the 1T′-MoS... 2x Se 2(1-x) During crystal nucleation and growth, molybdenum sulfide selenide can be inserted in situ uniformly and slowly into the interlayer of the molybdenum atoms, causing charge transfer in the molybdenum atomic framework. Simultaneously, the inserted low-valence alkali metal ions act as pinning agents, inhibiting the coordination rearrangement of molybdenum atoms to the 2H phase. This effectively induces the transformation of the conventional 2H phase to the 1T′ phase without causing severe lattice distortion. Furthermore, under high-temperature reducing atmosphere conditions, the metal anions melt, forming a local molten salt liquid phase environment, which acts as a flux. This molten salt medium can enhance the solid-phase atomic diffusion rate of the molybdenum, sulfur, and selenium sources, regulate the molten salt viscosity and nucleation rate, achieve uniform mass transfer of materials, and avoid severe lattice distortion caused by intense local reactions. Under Se-rich, high-temperature, and reducing environments, Se metal ions and low-valence alkali metal ions can intercalate into the layered Mo-S / Se framework, achieving solid solution substitution of S by Se and inducing its transformation to the 1T′ phase, thus obtaining a high-1T′ phase alkali metal intercalated 1T′ precursor.
[0065] It should be noted that although the formation of the 1T′ phase can be induced to some extent by reasonably controlling the S / Se ratio and introducing metal anions, the 1T′-MoS phase still has limitations. 2x Se 2(1-x) The 1T′ phase is a metastable metallic phase, and its thermodynamic stability is significantly lower than that of the corresponding 2H phase, leading to the final formation of 1T′-MoS. 2x Se 2(1-x) The problem of numerous heterogeneous phases still exists.
[0066] Therefore, in one embodiment, the flow rate ratio of the reducing atmosphere to the inert protective gas, expressed in sccm units, is (20-40):(80-60). This effectively regulates the redox potential of the reaction system of molybdenum, sulfur, and selenium sources, allowing the molybdenum source to be fully reduced in the reducing atmosphere and undergo a uniform gas-solid phase reaction with the sulfur and selenium sources. Simultaneously, under the synergistic effect of metal ions and the reducing atmosphere, it promotes the temporary insertion of metal ions into the interlayer of molybdenum sulfoselenide, inducing and stabilizing the unconventional 1T′ phase structure and inhibiting the transformation of the 1T′ phase to the thermodynamically stable 2H phase. Furthermore, it avoids excessively vigorous reactions and excessive volatilization of sulfur and selenium due to excessively high flow rates of the reducing gas, thereby facilitating the acquisition of 1T′-MoS with uniform composition, high phase purity, and good structural stability. 2x Se 2(1-x) Crystal.
[0067] In one embodiment, the reducing atmosphere comprises hydrogen.
[0068] In one embodiment, the inert protective gas includes at least one of argon and nitrogen.
[0069] In one embodiment, after the step of placing the reaction precursor at 750°C-900°C for 2-4 hours under a reducing atmosphere and an inert protective gas, and before the step of washing the alkali metal intercalation 1T′ precursor with water, a natural cooling operation is also included.
[0070] S103. Perform a water washing operation on the alkali metal intercalation 1T′ precursor to wash away unreacted molybdenum source, metal anion salt, sulfur source or selenium source.
[0071] S104. The alkali metal intercalated 1T′ precursor, after water washing, is immersed in a reduction-displacement solution to obtain an alkali metal-free 1T′ precursor. This allows the alkali metal intercalated 1T′ precursor to undergo a mild topological ion exchange reaction in the reduction-displacement solution, preventing interlayer depletion and lamination collapse. This ensures the stability of the distorted octahedral framework of the two-dimensional layered Mo-S / Se skeleton throughout the exchange process, avoiding the problem of strong chemical potential-driven drastic disturbance to the crystal skeleton and transformation to the 2H phase. Simultaneously, the low migration and diffusion barrier of low-valence alkali metals between 1T′ phase layers ensures that interlayer ion exchange can be completed with short immersion time, reducing the time the metastable framework is exposed to a disturbed environment. This further stabilizes and preserves the 1T′ phase crystal structure, which is beneficial for preparing 1T′-MoS with high phase purity, stable 1T′ metastable phase, high-density active sites across the entire surface, and excellent polysulfide conversion ability. 2x Se 2(1-x) Crystal.
[0072] In one embodiment, the soaking reaction conditions were 15°C-30°C; the time was 12h-24h.
[0073] In one embodiment, the reduction-displacement solution includes at least one of dilute sulfuric acid, iodine-acetonitrile solution, and acidic potassium dichromate solution to ensure that the alkali metal intercalation 1T′ precursor can undergo a relatively mild topological ion exchange reaction with the reduction-displacement solution.
[0074] In one embodiment, the concentration of dilute sulfuric acid is 0.01 mol / L to 0.03 mol / L, or the concentration of iodine-acetonitrile solution is 40 mg / mL to 60 mg / mL, thereby providing a milder topological ion exchange reaction environment for the alkali metal intercalation 1T′ precursor.
[0075] S105. The alkali-free metal intercalation 1T′ precursor is cleaned and dried to effectively remove excess unreacted molybdenum source, metal anions, sulfur source, and selenium source, thereby obtaining the 1T′-MoS with high phase purity. 2x Se 2(1-x) Crystal.
[0076] In one embodiment, the alkali metal intercalated 1T′ precursor after the soaking reaction is washed multiple times with water or acetonitrile solution, and then vacuum dried at 25°C-30°C for 0.5-2 days. This ensures that the washing and drying process does not affect the transformation of the 1T′ phase to the 2H phase, thereby facilitating the preparation of long-range ordered 1T′-MoS with high phase purity, stable 1T′ metastable phase, high-density active sites across the entire surface, and excellent polysulfide conversion ability. 2x Se 2(1-x) Crystals, to better fit 2.5 mg / cm 2-6mg / cm 2 Application of electrochemical devices with high sulfur loading and current ratios of 2C-3C.
[0077] In this disclosure, the water is deionized water.
[0078] In one embodiment, the cleaning is performed 3 to 8 times.
[0079] It should be noted that, compared to traditional wet slurry coating processes, the prolonged wetting with the polar NMP solvent and subsequent high-temperature drying in wet slurry coating processes easily induce an irreversible phase transition from the 1T′ phase to the conventional 2H phase, and the 1T′-MoS phase... 2x Se 2(1-x) The lithium- and thiophilic dual active sites of the crystal are easily passivated and shielded by polar solvents, affecting the efficient adsorption and conversion performance of lithium polysulfide products; at the same time, 1T′-MoS 2x Se 2(1-x) The two-dimensional layered Mo-S / Se framework of the crystal is prone to agglomeration and stacking in the liquid phase environment, which can lead to the loss of both lithophile-thiophile active sites.
[0080] Therefore, this disclosure adopts the method of using the 1T′-MoS 2x Se 2(1-x) The crystals are mixed with the sulfur-carbon composite material and the inert polymer binder aqueous solution through a semi-dry fibrillation process, introducing only a small amount of the inert polymer binder aqueous solution. This eliminates the need for prolonged liquid-phase immersion and high-temperature vacuum drying, thus maximizing the retention of 1T′-MoS. 2x Se 2(1-x) The 1T′ metastable phase and dual active sites of the crystal ensure 1T′-MoS 2x Se 2(1-x) The crystal possesses higher intrinsic electronic conductivity and a distorted lattice structure more conducive to surface charge transfer; simultaneously, through shear-induced inert polymer bonding aqueous solution, the inert polymer binder in the aqueous solution can interweave to form a three-dimensional network, and the formed three-dimensional network can bond the sulfur-carbon composite material and the 1T′-MoS 2x Se 2(1-x) The tightly interwoven crystals further stabilized 1T′-MoS. 2x Se 2(1-x) The bonding stability of Mo, S, and Se in the crystal is effectively improved, thus enhancing the stability of 1T′-MoS 2x Se 2(1-x) The problem of crystal transformation to the 2H phase and how to better avoid 1T′-MoS 2x Se 2(1-x) Crystalline or sulfur-carbon composite materials are prone to shedding during prolonged use, thus better ensuring the electrochemical device operates at 2.5 mg / cm³. 2-6mg / cm 2 With high sulfur loading and current rate under 2C-3C conditions, the battery retains more than 80% of its capacity over 200 cycles, thus ensuring high cycle stability of the battery device.
[0081] Furthermore, due to 1T′-MoS 2x Se 2(1-x) The crystals have a high density and are prone to sedimentation in wet slurries, leading to the formation of 1T′-MoS₂ crystals. 2x Se 2(1-x) The catalytic components of the crystal are unevenly distributed. However, the semi-dry fibrillation process used in this disclosure, through a second grinding and multiple rolling shearing processes, produces micron-sized 1T′-MoS₂ crystals. 2x Se 2(1-x) Crystals are uniformly distributed within the fibrillated three-dimensional network of the polymer adhesive, such as... Figure 3 As shown in Figure b, 1T′-MoS is guaranteed. 2x Se 2(1-x) The crystals can be evenly distributed across the positive electrode composite film layer, effectively avoiding the uneven sedimentation problem that exists in traditional wet methods.
[0082] Specifically, this disclosure also provides a method for preparing an electrochemical device, used to prepare the electrochemical device described in any of the above embodiments. The method for preparing the electrochemical device includes the following steps: First, a sulfur-carbon composite material and 1T′-MoS 2x Se 2(1-x) The crystals are subjected to a second grinding and mixing process to obtain a mixture; subsequently, an inert polymer binder aqueous solution is added dropwise to the mixture to obtain a semi-dry mixture; subsequently, the semi-dry mixture is subjected to multiple rolling and shearing processes to allow the inert polymer binder aqueous solution to bind the sulfur-carbon composite material and the 1T′-MoS 2x Se 2(1-x) The crystals are tightly interwoven and wrapped to obtain a semi-dry inclusion body; then, the semi-dry inclusion body is rolled to obtain a self-supporting positive electrode composite film layer; then, the self-supporting positive electrode composite film layer is pressed onto the current collector to obtain the sulfur-based positive electrode sheet; finally, the sulfur-based positive electrode sheet is assembled with the negative electrode sheet, electrolyte and separator to obtain the electrochemical device.
[0083] The above-described method for preparing the electrochemical device employs a semi-dry fibrillation process involving a second grinding and multiple rolling shearing steps. This effectively protects the metastable 1T′ phase while simultaneously allowing the micron-sized 1T′-MoS phase to be formed. 2x Se 2(1-x) Crystals are uniformly distributed within the fibrillated three-dimensional network of the polymer adhesive, such as... Figure 3 As shown in Figure b, 1T′-MoS is guaranteed. 2x Se 2(1-x)The crystals can be more uniformly distributed on the positive electrode composite film layer, effectively avoiding the problem of uneven sedimentation in traditional wet processes, which leads to poor polysulfide catalytic conversion kinetics and conductivity in electrochemical devices.
[0084] One embodiment of the method for preparing an electrochemical device includes some or all of the following steps: S201, sulfur-carbon composite material and 1T′-MoS 2x Se 2(1-x) The crystals undergo a second grinding and mixing process to obtain a mixture that combines sulfur-carbon composite material and 1T′-MoS. 2x Se 2(1-x) The crystals can be thoroughly mixed. Furthermore, the second grinding and mixing speed is 50 rpm / min-150 rpm / min, and the time is 5 min-15 min, thereby ensuring the 1T′-MoS 2x Se 2(1-x) Under these grinding and mixing conditions, the crystals do not undergo a 1T′ phase change, which helps ensure that the final sulfur-based cathode has excellent conductivity, abundant surface active sites, and excellent polysulfide conversion capability. This ensures that the final electrochemical device can provide a fast electron transport channel for the conversion reaction of lithium polysulfide products, thereby achieving efficient adsorption and conversion of lithium polysulfide products generated from the sulfur-carbon composite material, and guaranteeing the 1T′-MoS 2x Se 2(1-x) The crystals can fully exert their catalytic activity to ensure that the charge transfer impedance of the final electrochemical device is 50Ω-90Ω, thereby ensuring that the electrochemical device operates at 2.5 mg / cm². 2 -6mg / cm 2 The 200-cycle retention rate under high sulfur loading and current rate 2C-3C conditions is higher than 80%, which effectively breaks through the bottleneck of the traditional electrochemical device with a cycle retention rate of only 60% after 200 cycles. It has high reversible capacity and capacity retention rate, showing good prospects for practical application.
[0085] S202. Add an inert polymer binder aqueous solution dropwise to the mixture to obtain a semi-dry mixture; this ensures that the inert polymer binder aqueous solution is fully dispersed in the mixture, guaranteeing that the inert polymer binder can comprehensively encapsulate the sulfur-carbon composite material and 1T′-MoS during subsequent multiple rolling and shearing processes. 2x Se 2(1-x) Crystal.
[0086] S203. The semi-dry mixture is subjected to multiple roll pressing and shearing processes, allowing the inert polymer binder to undergo repeated pressing, folding, and stretching during these processes. This enables the inert polymer binder to exert a "fibrillation" effect, thereby promoting the bonding of the sulfur-carbon composite material and the 1T′-MoS in the inert polymer binder aqueous solution. 2x Se 2(1-x) The crystals are tightly interwoven and wrapped together, meaning that the inert polymer binder can interweave to form a three-dimensional network, and the formed three-dimensional network can bind the sulfur-carbon composite material and the 1T′-MoS 2x Se 2(1-x) The crystals are tightly interwoven and encapsulated within, resulting in a semi-dry inclusion state; this further stabilizes 1T′-MoS. 2x Se 2(1-x) The bonding stability of Mo, S, and Se in the crystal is effectively improved, thus enhancing the stability of 1T′-MoS 2x Se 2(1-x) The problem of crystal transformation to the 2H phase and how to better avoid 1T′-MoS 2x Se 2(1-x) Crystalline or sulfur-carbon composite materials are prone to shedding during prolonged use, thus better ensuring the electrochemical device operates at 2.5 mg / cm³. 2 -6mg / cm 2 With high sulfur loading and current rate under 2C-3C conditions, the battery retains more than 80% of its capacity over 200 cycles, thus ensuring high cycle stability of the battery device.
[0087] In one embodiment, the number of rolling shearing cycles is 5-10 times, the rolling speed is 15mm / s-25mm / s, and the time is 4min-8min; to ensure that the inert polymer binder can achieve the desired effect on 1T′-MoS 2x Se 2(1-x) While achieving comprehensive encapsulation of crystals and sulfur-carbon composite materials, it does not affect 1T′-MoS 2x Se 2(1-x) The stability of the 1T′ phase of a crystal.
[0088] S204. The semi-dry inclusion is subjected to a calendering operation to obtain a self-supporting positive electrode composite film layer. The calendering process is used to calender 1T′-MoS 2x Se 2(1-x)Crystalline and sulfur-carbon composite materials can become entangled with each other, which is beneficial for constructing a continuous three-dimensional conductive network. The sulfur-carbon composite material can be anchored inside the pores of the three-dimensional conductive network to obtain a self-supporting positive electrode composite film. This ensures the continuity of the electron transport path inside the positive electrode composite film. At the same time, the three-dimensional conductive network can buffer the volume expansion and contraction of the sulfur-carbon composite material during the charging and discharging process, suppress the problems of sulfur-carbon composite material pulverization and positive electrode composite film cracking, and also reduce the contact impedance at the interface between the self-supporting positive electrode composite film and the current collector.
[0089] S205. The self-supporting positive electrode composite film layer is pressed onto the current collector to obtain the sulfur-based positive electrode sheet. The current collector provides planar lateral conductivity, which effectively compensates for the deficiency of lateral conductivity in the self-supporting film. Pressing achieves tight anchoring contact between the self-supporting positive electrode composite film layer and the current collector, reducing the interfacial contact impedance between the self-supporting positive electrode composite film layer and the current collector, making the current distribution more uniform under high rate conditions. The volume stress generated by charging and discharging can be partially dissipated in advance by the three-dimensional network inside the self-supporting positive electrode composite film layer, reducing the stress borne by the interface between the self-supporting positive electrode composite film layer and the current collector, suppressing delamination and powder shedding failure during 200 cycles, and improving the cycle capacity retention rate at 2C-3C rate under high sulfur loading conditions. It also reduces the interfacial contact impedance between the self-supporting positive electrode composite film layer and the current collector, making the current distribution more uniform at 2C-3C high rate, and further reducing the charge transfer impedance of the sulfur-based positive electrode sheet.
[0090] In one embodiment, the current collector is a carbon-coated aluminum foil.
[0091] In one embodiment, the calendered thickness of the positive electrode composite film is 150μm-200μm.
[0092] In one embodiment, after pressing the self-supporting positive electrode composite film onto the current collector, the self-supporting positive electrode composite film pressed onto the current collector is vacuum dried at room temperature and then punched into a disc, which is a sulfur-based positive electrode sheet.
[0093] S206. Assemble the sulfur-based positive electrode, negative electrode, electrolyte, and separator to obtain the electrochemical device. Ensure that the prepared electrochemical device can suppress the loss of active materials and polysulfide shuttle under high sulfur loading and 2C-3C rate charge-discharge conditions, and improve the stability of the long cycle capacity retention rate of the electrochemical device.
[0094] The embodiments of this application will be described in detail below with reference to examples. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of this application. For experimental methods in the following embodiments where specific conditions are not specified, please refer to the guidelines given in this application, or follow experimental manuals or conventional conditions in the art, or follow the conditions recommended by the manufacturer, or refer to experimental methods known in the art.
[0095] In the specific embodiments described below, the measurement parameters involving raw material components may have slight deviations within the weighing accuracy range unless otherwise specified. Temperature and time parameters are subject to acceptable deviations due to instrument testing accuracy or operational precision.
[0096] It should be understood that in the various embodiments of this application, the order of the above-mentioned processes does not imply the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this application.
[0097] Example 1
[0098] S1. 2 mmol MoO3, 5 mmol K2CO3, 12 mmol S powder, and 8 mmol Se powder were mixed at a molar mass ratio of 2:5:12:8 at a grinding speed of 100 rpm / min for 10 min, with y = 12, to obtain the reaction precursor. Under a 30% hydrogen / 70% argon atmosphere at a flow rate of 100 sccm, the mixture was kept at 850℃ for 4 hours to obtain the alkali metal intercalation 1T′ precursor. After natural cooling, the alkali metal intercalation 1T′ precursor was washed 5 times with deionized water, then soaked in 0.02 mol / L dilute sulfuric acid at 25℃ for 12 h, washed 5 times with deionized water, and finally vacuum dried at 25℃ for 12 h to obtain 1T′-MoS. 0.5 Se 0.5 Crystal, where x is 0.25.
[0099] S2, 70 wt% sulfur / carbon complex (S to C mass ratio of 7:3, total mass 210 mg) and 10 wt% 1T′-MoS 0.5 Se 0.5The crystals (30 mg) were placed in an agate mortar and subjected to a second dry grinding (50 rpm - 150 rpm) for 10 min to ensure uniform mixing, resulting in a mixture. Subsequently, 20 wt% of a polytetrafluoroethylene (PTFE) binder aqueous solution (12 mg of PTFE binder (molecular weight 5 w) dispersed in 48 mg of deionized water to obtain 60 mg of PTFE binder aqueous solution) was gradually added dropwise to obtain a semi-dry mixture. The semi-dry mixture was then subjected to multiple rolling shearing processes in a roller press (rolling speed 15 mm / s, total 5 min, 6 rolling cycles) until the PTFE fully formed a three-dimensional network structure and the sulfur / carbon complex and 1T′-MoS 2x Se 2(1-x) The crystals are tightly interwoven and encapsulated to obtain a semi-dry inclusion. This semi-dry inclusion is then rolled to a thickness of 180 μm to obtain a self-supporting positive electrode composite film. Next, this self-supporting positive electrode composite film is pressed onto carbon-coated aluminum foil to form a sulfur-based positive electrode sheet. After drying the sulfur-based positive electrode at room temperature, it is punched into 8 mm discs to obtain the sulfur-based positive electrode sheet, which has a sulfur loading as high as 2.5 mg / cm³. 2 -6.0mg / cm 2 .
[0100] Example 2
[0101] The difference from Example 1 is that the amounts of S powder and Se powder in step S1 are changed to 10 mmol and 10 mmol respectively, and K2CO3 is replaced with potassium sulfate. That is, the first grinding and mixing of MoO3, potassium sulfate, S powder, and Se powder is carried out in a mass ratio of 2:5:10:10, with y = 10. Additionally, 0.02 mol / L dilute sulfuric acid is replaced with 50 mg / ml iodoacetonitrile solution, while the rest remains unchanged, to prepare 1T′-MoS 0.8 Se 1.2 Crystal, where x is 0.4.
[0102] Example 3
[0103] The difference from Example 1 is that the amounts of S powder and Se powder in step S1 are changed to 8 mmol and 12 mmol, respectively, and K2CO3 is replaced with sodium oxalate. Specifically, the first grinding and mixing of MoO3, sodium oxalate, S powder, and Se powder is carried out in a mass ratio of 2:5:8:12, with y = 8, and the rest remaining unchanged, to prepare 1T′-MoS 0.6 Se 1.4 Crystal, where x is 0.3.
[0104] Example 4
[0105] The difference from Example 1 is that the amounts of S powder and Se powder in step S1 are changed to 4 mmol and 16 mmol, respectively, and K2CO3 is replaced with potassium oxalate. Specifically, the first grinding and mixing of MoO3, potassium oxalate, S powder, and Se powder is carried out in a mass ratio of 2:5:4:16, with y = 4, and the rest remaining unchanged, to prepare 1T′-MoS 0.3 Se 1.7 Crystal, where x is 0.15.
[0106] Comparative Example 1 The difference from Example 1 is that the S1 raw material was replaced with 2 mmol MoO3, 5 mmol K2CO3, and 20 mmol S powder in a molar mass ratio of 2:5:20. The first grinding and mixing was carried out for 10 min at a grinding speed of 100 rpm / min to obtain the reaction precursor. Under a 30% hydrogen / 70% argon atmosphere and a flow rate of 100 sccm, the mixture was kept at 850°C for 4 hours to obtain the alkali metal intercalation 1T′ precursor. After natural cooling, the alkali metal intercalation 1T′ precursor was washed 5 times with deionized water, then soaked in 0.02 mol / L dilute sulfuric acid at 25°C for 12 h, washed 5 times with deionized water, and then vacuum dried at 25°C for 12 h to obtain 1T′-MoS2. The rest remained unchanged.
[0107] Comparative Example 2 The difference from Example 1 is that the S1 raw material was replaced with 2 mmol MoO3, 5 mmol K2CO3, and 20 mmol Se powder in a molar mass ratio of 2:5:20. The first grinding and mixing was carried out for 10 min at a grinding speed of 100 rpm / min to obtain the reaction precursor. Under a 30% hydrogen / 70% argon atmosphere and a flow rate of 100 sccm, the mixture was kept at 850°C for 4 hours to obtain the alkali metal intercalation 1T′ precursor. After natural cooling, the alkali metal intercalation 1T′ precursor was washed 5 times with deionized water, then soaked in 0.02 mol / L dilute sulfuric acid at 25°C for 12 h, washed 5 times with deionized water, and then vacuum dried at 25°C for 12 h to obtain 1T′-MoSe2. The rest remained unchanged.
[0108] Comparative Example 3 The difference from Example 1 is that step S1 is omitted, and the 1T′-MoS in step S2 is replaced with the step S2. 0.5 Se 0.5 The crystal was replaced with 2H-MoS 0.5 Se 0.5 The rest remain unchanged.
[0109] Comparative Example 4 The difference from Example 1 is that the 2 mmol MoO3, 5 mmol K2CO3, 10 mmol S powder and 10 mmol Se powder in step S1 are replaced with 2 mmol MoO3, 10 mmol K2CO3, 20 mmol S powder and 20 mmol Se powder, while the rest remain unchanged.
[0110] Comparative Example 5 The difference from Example 1 is that the 2 mmol MoO3, 5 mmol K2CO3, 10 mmol S powder and 10 mmol Se powder in step S1 are replaced with 2 mmol MoO3, 1 mmol K2CO3, 1 mmol S powder and 1 mmol Se powder, while the rest remain the same.
[0111] Comparative Example 6 The difference from Example 1 is that K2CO3 in step S1 is replaced with ferric nitrate, while the rest remains the same.
[0112] Comparative Example 7 The difference from Example 1 is that the 0.05 mol / L dilute sulfuric acid in step S1 is replaced with 1 mol / L dilute sulfuric acid, while the rest remains the same.
[0113] Comparative Example 8 The difference from Example 1 is that step S2 is replaced with a conventional wet process, i.e., by using the same proportion of 1T′-MoS 0.5 Se 0.5 The mixture is mechanically stirred with sulfur-carbon composite material and binder (PVDF) in dispersion solvent (NMP) to form a slurry. This slurry is then evenly coated onto carbon-coated aluminum foil and dried at 40-60°C under normal pressure. All other properties remain unchanged.
[0114] Comparative Example 9 The difference from Example 1 is that step S2, which involves multiple rolling and shearing operations (rolling speed of 15 mm / s, total time of 5 min, and 6 rolling operations), is replaced with (rolling speed of 50 mm / s, time of 1 min, and 2 rolling operations), while the rest remains unchanged.
[0115] The 1T′-MoS from Example 1 above 2x Se 2(1-x) Scanning electron microscope (SEM) images of the crystal were obtained. Figure 1 ;from Figure 1 As shown in Figure a, 1T′-MoS in Example 1 2x Se 2(1-x) The crystals exhibit a long-range ordered elongated morphology; from Figure 1 From middle b to Figure 1The energy-dispersive X-ray spectroscopy (EDS) elemental distribution map of region d in the middle shows that Mo, S, and Se exhibit a uniform spatial distribution throughout the crystal, indicating that the present invention has prepared a long-range ordered and uniformly distributed elongated morphology 1T′-MoS 2x Se 2(1-x) In the crystal, no significant phase separation occurred among the three elements Mo, S, and Se. Meanwhile, the 1T′-MoSc from Examples 2-4... 2x Se 2(1-x) The crystal also possesses the 1T′-MoS₂ of Example 1. 2x Se 2(1-x) The crystal structure morphology is similar to that of crystals, and the 1T′-MoS in Examples 1-4 2x Se 2(1-x) The purity of the 1T′ phase of the crystal is 95%-100%, with few impurities.
[0116] The 1T′-MoS2 of Examples 1-4 and Comparative Example 1 and 1T′-MoSe2 of Comparative Example 2 were subjected to corresponding energy-dispersive X-ray (EDS) energy spectrum comparison diagrams, X-ray diffraction (XRD) patterns, and Raman spectra measurements, respectively, to obtain... Figure 2 .
[0117] Among them, the 1T′-MoS prepared in Example 1 2x Se 2(1-x) denoted as 1T′-MoS 2x Se 2(1-x) -1, Example 2 prepared 1T′-MoS 2x Se 2(1-x) denoted as 1T′-MoS 2x Se 2(1-x) -2; The 1T′-MoS obtained in Example 3 2x Se 2(1-x) denoted as 1T′-MoS 2x Se 2(1-x) -3, the 1T′-MoS prepared in Example 4 2x Se 2(1-x) denoted as 1T′-MoS 2x Se 2(1-x) -4.
[0118] Figure 2 As shown in EDS spectra of Examples 1-4 and Comparative Examples 1-2 (a), the relative peak intensities of S and Se in the spectra show a regular change with the increase of Se content in the feed ratio, confirming the 1T′-MoS 2x Se 2(1-x) The alloy components can be synthesized in a controlled manner.
[0119] Figure 2Figure b shows the X-ray diffraction (XRD) patterns of Examples 1-4 and Comparative Examples 1-2. The results show that in Examples 1-4, with the gradual increase of Se content and the use of metal anions, the characteristic diffraction peak (200) gradually shifted from about 15.2° of the pure phase 1T′-MoS2 to about 13.9° of the pure phase 1T′-MoSe2. This continuous shift of the diffraction peak to a lower angle indicates that, due to the larger radius of Se atoms than S atoms, the substitution of Se atoms has increased the interlayer spacing of the material, further confirming the formation of the alloy solid solution.
[0120] Figure 2 Figure c shows the Raman spectra of Examples 1-4 and Comparative Examples 1-2. The results show that in Examples 1-4, with the increase of Se concentration and the use of metal anion salts, the characteristic vibrational peak of the 1T′ phase of the material underwent a continuous frequency shift from the pure phase 1T′-MoS2 to the pure phase 1T′-MoSe2. This is consistent with the XRD results, fully demonstrating that the present invention successfully achieves 1T′-MoS2 by controlling the ratio of reactants. 2x Se 2(1-x) The crystal can be continuously and controllably tuned, and the structural characteristics of the 1T′ phase can be induced and maintained.
[0121] Furthermore, because the mass ratio of molybdenum source, metal anion salt, sulfur powder, and selenium powder in Comparative Examples 4-5 was not within the range of 2:5:y:(20-y), because Comparative Example 6 used a metal anion salt as a trivalent metal cation, because the concentration of dilute sulfuric acid in Comparative Examples 7-8 was not within the range of 0.01mol / L-0.03mol / L, and because the rolling speed in Comparative Example 9 was not between 15mm / s and 25mm / s, the time was between 4min and 8min, and the number of rolling cycles was between 5 and 10, the 1T′-MoS prepared in Comparative Examples 4-9 was not... 2x Se 2(1-x) The high phase purity, 1T′ metastable phase stability, high density of active sites across the entire surface, and excellent polysulfide conversion ability of the crystals are all inferior to those of Examples 1-4.
[0122] Scanning electron microscope (SEM) images of the surface of the sulfur-based cathode sheets prepared in Example 1 and Comparative Examples 1-2 are shown below. Figure 3 From middle a to Figure 3 As shown by the yellow dashed circle in section c, the micron-sized bulk regions of Example 1 are uniformly distributed on the surface of the prepared sulfur-based cathode. These bulk regions correspond to the introduced 1T′-TMD crystal. For details, please refer to [link to documentation]. Figure 3 In addition, the semi-dry fibrillation process enables 1T′-MoS2 to be produced. 2x Se 2(1-x)The crystals are uniformly dispersed within the sulfur-based cathode, effectively increasing the catalytic conversion sites of polysulfides. This results in a significantly higher surface uniformity for the sulfur-based cathode in Example 1 compared to Comparative Examples 1-2. Furthermore, the three-dimensional network structure formed by the semi-dry fibrillation process enables the processing of sulfur-carbon composite materials and 1T′-MoS₂. 2x Se 2(1-x) Good crystal encapsulation is conducive to the formation of a self-supporting positive electrode composite film.
[0123] The lithium-sulfur batteries prepared in Example 1 and Comparative Examples 1-2 were subjected to CV and EIS tests to obtain... Figure 4 ,like Figure 4 As shown in the CV curve of a in Example 1, at 0.1 mV / s -1 At a scan rate based on 1T′-MoS 2x Se 2(1-x) The symmetric cell exhibits the largest current response, indicating that it has significantly accelerated interfacial redox kinetics; and so on. Figure 4 The EIS spectrum of 1T′-MoS₂ is shown in Figure b. 2x Se 2(1-x) Symmetric cells exhibit the lowest charge transfer impedance (Ri). ct The RΩ is only 88Ω, significantly lower than that of the comparative materials 1T′-MoS2 and 1T′-MoSe2. Therefore, the extremely low RΩ is significant. ct The value directly confirms 1T′-MoS 2x Se 2(1-x) The material possesses excellent electron transport capabilities and rapid interfacial charge transfer capabilities; the combination of the largest CV current response and the smallest impedance fully demonstrates that Example 1 has extremely strong catalytic conversion performance for lithium polysulfides, which is significantly better than that of Comparative Examples 1-2.
[0124] Similarly, the lithium-sulfur batteries of Examples 2-4 and Comparative Examples 3-9 were subjected to CV and EIS tests. The results showed that the experimental results of Examples 1-4 were significantly better than those of Comparative Examples 3-9, with Example 1 having the best overall performance.
[0125] The lithium-sulfur batteries prepared in Example 1 and Comparative Examples 1-2 were subjected to a temperature of 0.1C (100 mAg). -1 After 5 activation cycles at a high rate, constant current charge-discharge tests were performed at high rates of 2C or 3C to obtain... Figure 5 ,from Figure 5 The first-week charge-discharge curve of 1T′-MoS in Example 1 shows that... 2x Se 2(1-x) The lithium-sulfur battery exhibits a capacity of up to 1209.6 mAh g. -1 The discharge specific capacity of Example 1 is significantly better than that of Comparative Examples 1-2, and it has the smallest voltage difference (174mV), indicating that the 1T′-MoS₂ of Example 1 is superior.2x Se 2(1-x) It exhibits suppressed polarization. Furthermore, the 1T′-MoS₂ of Example 1... 2x Se 2(1-x) The lithium-sulfur battery exhibits minimum overpotentials of only 38.5 mV and 51 mV during Li2S (final product) nucleation (during discharge) and Li2S decomposition (during charging), respectively. For details, please refer to [link to relevant documentation]. Figure 5 b and Figure 5 c indicates that the 1T′ phase structure of molybdenum sulfide selenide material in Example 1, while maintaining its fast electron transport characteristics, further reduced the liquid-solid conversion energy barrier after S / Se composition regulation, thereby more effectively promoting the catalytic conversion of lithium polysulfides. This resulted in the first-cycle coulombic efficiency and stability of Example 1 being significantly higher than those of Comparative Examples 1-2.
[0126] Similarly, the lithium-sulfur batteries of Examples 2-4 and Comparative Examples 3-9 were subjected to 0.1C (100 mAg) testing. -1 After five activation cycles at a high rate, constant current charge-discharge tests were conducted at high rates of 2C or 3C. The results showed that the experimental results of Examples 1-4 were significantly better than those of Comparative Examples 3-9, with Example 1 having the best overall performance.
[0127] The lithium-sulfur batteries prepared in Examples 1 and 1-2 above achieved a high current density and a sulfur loading of 2.9 mg / cm² at 2C. 2 Long-cycle stability tests were conducted under the specified conditions, and the results were obtained. Figure 6 .from Figure 6 From middle a to Figure 6 As can be seen from d, the 1T′-MoS in Example 1 2x Se 2(1-x) The lithium-sulfur battery exhibits significant advantages, with a first-cycle discharge specific capacity as high as 775.1 mAh g. -1 After 200 cycles, the specific capacity remained at 646.6 mAh g. -1 The capacity retention rate was as high as approximately 83.4%. In contrast, the initial specific capacity of the lithium-sulfur batteries of Comparative Example 1 (pure-phase 1T′-MoS2) and Comparative Example 2 (1T′-MoSe2) was lower (approximately 510.5 mAh g⁻¹, respectively). -1 and 506.9mAhg -1 Furthermore, after 200 cycles, the capacity rapidly decreased to 400 mAh g. -1 Approximately 415.5 mAh g (each approximately 415.5 mAh g) -1 and 406.5mAhg -1 This indicates that the 1T′-MoS of Embodiment 1 of this disclosure... 2x Se 2(1-x)The material combines the advantages of rapid electron transport in the 1T′ phase with the advantages of high-density catalysis across the entire surface brought about by S / Se composition regulation. Therefore, it exhibits superior cycle durability at high rates, making the experimental results of Example 1 significantly better than those of Comparative Examples 1-2.
[0128] The lithium-sulfur batteries prepared in Example 1 and Comparative Examples 1-2 were tested at a high current density of 5.5 mg / cm³ at 3C. 2 Long-cycle stability tests were conducted under high surface sulfur loading to obtain... Figure 7 .from Figure 7 a and Figure 7 As can be seen from b, the 1T′-MoS in Example 1 2x Se 2(1-x) The lithium-sulfur battery achieved a first-cycle discharge specific capacity of 442.5 mAh g. -1 After initial electrochemical activation, its reversible specific capacity remained at 464.2 mAh g⁻¹ after 200 cycles. -1 This fully demonstrates 1T′-MoS 2x Se 2(1-x) The material still exhibits excellent adsorption and catalytic conversion capabilities for lithium polysulfides under high current and high loading conditions, and demonstrates excellent cycle stability, making the experimental results of Example 1 significantly better than those of Comparative Examples 1-2.
[0129] Similarly, the lithium-sulfur batteries of Examples 2-4 and Comparative Examples 3-9 were tested at a high current density of 2C and an areal sulfur loading of 2.9 mg / cm³. 2 Under these conditions, and with a high current density of 3C and 5.5 mg / cm³, 2 Long-cycle stability tests were conducted under high surface sulfur loading, and the results showed that: Comparative Example 3 directly uses 2H-MoS 0.5 Se 0.5 Typically exhibiting semiconductor properties, it lacks the metallic conductive network and metastable structure characteristic of the 1T′ phase. Its basal-plane electron transport capability is poor, and the number of active sites is limited, resulting in weak adsorption and catalytic conversion capabilities for lithium polysulfides. Therefore, Comparative Example 3 struggles to achieve rapid liquid-solid conversion of lithium polysulfides, exhibits significant polarization, and its battery performance is significantly lower than that of Examples 1-4.
[0130] In Comparative Example 4, the excessive amount of K₂CO₃ resulted in overly strong alkali metal intercalation and etching. Excessive S and Se sources led to supersaturation of the reaction system, causing uncontrolled nucleation and growth of the MoSSe alloy. This excess of alkali metals and sulfur-selenium sources easily disrupted the stability of the 1T′ metastable phase, promoting its transformation to the thermodynamically stable 2H phase and generating byproducts such as MoS₂, MoSe₂, polysulfides, polyselenides, or alkali metal sulfoselenides. Therefore, the 1T′ phase in Comparative Example 4 exhibited low purity, poor crystallinity, and insufficient active site density, resulting in decreased catalytic conversion ability for lithium polysulfides and performance lower than in Examples 1-4.
[0131] In Comparative Example 5, the amounts of K2CO3, S powder, and Se powder were too low, resulting in a lack of sufficient K. + Due to intercalation and stabilization effects, MoO3 is difficult to fully reduce and transform, and the 1T′ metastable phase cannot be effectively formed and maintained. Simultaneously, insufficient S and Se sources lead to incomplete sulfide-selenization reactions, easily leaving unreacted products such as MoO3 / MoO2, and generating sulfur- and selenium-deficient MoSSe alloys or MoS2 / MoSe2 impurity phases. Therefore, in Comparative Example 5, the proportion of the 1T′ phase is low, there are many byproducts, and the electron transport and catalytic conversion performance are poor, significantly lower than in Examples 1-4.
[0132] Fe in ferric nitrate of Comparative Example 6 3+ It is a trivalent metal cation, unlike K + The alkali metal ions can effectively intercalate and stabilize the metastable 1T′ phase, but they also introduce impurity phases such as FeS / FeSe, which leads to a decrease in the purity of the 1T′ phase and an increase in by-products. As a result, the electron transport and catalytic conversion performance of Comparative Example 6 is significantly lower than that of Examples 1-4.
[0133] The concentration of 1 mol / L dilute sulfuric acid in Comparative Example 7 was too high, resulting in excessive etching and deintercalation during the acid washing / soaking process. This damaged the 1T′ metastable structure, leading to an increase in defects, partial oxidation, or transformation to the 2H phase, which reduced catalytic activity. Consequently, the electron transport and catalytic conversion performance of Comparative Example 7 was significantly lower than that of Examples 1-4.
[0134] Comparative Example 8: The traditional wet PVDF / NMP slurry process makes it difficult to produce 1T′-MoS 2x Se 2(1-x) The sulfur / carbon complex forms a uniform three-dimensional network, and the NMP and drying processes destroy the metastable 1T′ phase, resulting in uneven distribution of active sites and high interfacial impedance. Consequently, the electron transport and catalytic conversion performance of Comparative Example 8 is significantly lower than that of Examples 1-4.
[0135] The excessively fast rolling speed, short rolling time, and insufficient number of rolling cycles in Comparative Example 9 prevented PTFE from being fully fibrillated to form a three-dimensional network. The sulfur / carbon composite was not in close contact with the 1T′ alloy, resulting in poor uniformity and self-support of the positive electrode composite film. This led to increased impedance and decreased cycle performance, causing the electron transport and catalytic conversion performance of Comparative Example 9 to be significantly lower than those of Examples 1-4.
[0136] In summary, the experimental results of Examples 1-4 are significantly better than those of Comparative Examples 3-9, with Example 1 showing the best overall performance.
[0137] The embodiments described above merely illustrate several implementation methods of this application to facilitate a detailed understanding of the technical solutions of this application, but should not be construed as limiting the scope of protection of the patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the scope of protection of this application. Furthermore, it should be understood that after reading the above teachings of this application, those skilled in the art can make various alterations or modifications to this application, and the equivalent forms obtained also fall within the scope of protection of this application. It should also be understood that technical solutions obtained by those skilled in the art based on the technical solutions provided in this application through logical analysis, reasoning, or limited experimentation are all within the scope of protection of the appended claims. Therefore, the scope of protection of this patent application should be determined by the content of the appended claims, and the specification and drawings can be used to interpret the content of the claims.
Claims
1. An electrochemical device comprising a sulfur-based positive electrode, a negative electrode, an electrolyte, and a separator; wherein the sulfur-based positive electrode is stacked with the negative electrode through the separator, and the electrolyte is respectively immersed between the sulfur-based positive electrode, the negative electrode, and the separator; the sulfur-based positive electrode comprises a current collector and a positive electrode composite film layer disposed on the current collector, characterized in that, The positive electrode composite film layer comprises the following components by mass: 30-70 parts of sulfur-carbon composite material; 1T′-MoS 2x Se 2(1-x) 5-15 parts of crystals; 15-25 parts of an inert polymer binder aqueous solution; Wherein, x satisfies 0 <x<1; The 1T′-MoS 2x Se 2(1-x) The crystals are mixed with the sulfur-carbon composite material and the inert polymer binder aqueous solution through a semi-dry fibrillation process, so that the inert polymer binder aqueous solution binds the sulfur-carbon composite material and the 1T′-MoS 2x Se 2(1-x) The crystals are tightly interwoven and wrapped to form the positive electrode composite film; the 1T′-MoS 2x Se 2(1-x) The crystals provide a fast electron transport channel for the sulfur-carbon composite material and efficiently adsorb and convert the lithium polysulfide products generated by the sulfur-carbon composite material, enabling the electrochemical device to operate at 2.5 mg / cm³. 2 -6mg / cm 2 The retention rate after 200 cycles under high sulfur loading and current rate 2C-3C conditions is higher than 80%; the charge transfer impedance of the electrochemical device is 50Ω-90Ω; The inert polymer binder aqueous solution comprises an inert polymer binder and water, wherein the inert polymer binder is polytetrafluoroethylene (PTFE).
2. The electrochemical device according to claim 1, characterized in that, The mass ratio of S to C in the sulfur-carbon composite material is (5-8):(1-3).
3. The electrochemical device according to claim 1, characterized in that, The mass ratio of polymer binder to water in the inert polymer binder aqueous solution is 1:(2-5).
4. The electrochemical device according to claim 1, characterized in that, The calendered thickness of the positive electrode composite film is 150μm-200μm; and / or, The diameter of the sulfur-based positive electrode is 8mm-10mm.
5. The electrochemical device according to claim 1, characterized in that, The 1T′-MoS 2x Se 2(1-x) The method for preparing crystals includes the following steps: The molybdenum source, metal anion salt, sulfur source and selenium source were first ground and mixed in a mass ratio of (1-2):(3-6):y:(20-y) to obtain the reaction precursor; The reaction precursor was placed at 750℃-900℃ for 2-4 hours under a reducing atmosphere and an inert protective gas to obtain an alkali metal intercalation 1T′ precursor. The alkali metal intercalation 1T′ precursor was subjected to a water washing operation; The alkali metal intercalation 1T′ precursor, after being washed with water, is immersed in a reduction and displacement solution for reaction. The alkali-free metal intercalation 1T′ precursor was cleaned and dried to obtain the 1T′-MoS. 2x Se 2(1-x) Crystals; Wherein, y is an adjustable variable used to control the ratio of S / Se.
6. The electrochemical device according to claim 5, characterized in that, The molybdenum source includes at least one of molybdenum oxide, molybdate, and molybdenum halide; and / or, The metal anion salt includes at least one selected from sodium carbonate, potassium carbonate, calcium carbonate, sodium sulfate, potassium sulfate, calcium sulfate, sodium oxalate, potassium oxalate, and calcium oxalate; and / or, The sulfur source includes at least one of sulfur powder, organic sulfides, and inorganic sulfides; and / or, The selenium source includes at least one of selenium powder, organic selenide, and inorganic selenide.
7. The electrochemical device according to claim 5, characterized in that, The flow rate ratio of the reducing atmosphere to the inert protective gas is (20-40):(80-60); and / or, The reduction and displacement solution includes at least one of dilute sulfuric acid, iodine-acetonitrile solution, and acidic potassium dichromate solution; and / or, The alkali metal intercalation 1T′ precursor, after soaking and reaction, is cleaned with water or acetonitrile solution, and then vacuum dried at 15℃-30℃ for 0.5-2 days; and / or, The grinding speed during the first grinding and mixing process is 50 rpm / min-150 rpm / min, and the time is 5 min-10 min.
8. A method for preparing an electrochemical device, characterized in that, The method for preparing the electrochemical device according to any one of claims 1-7 comprises the following steps: sulfur-carbon composite material and 1T′-MoS 2x Se 2(1-x) The crystals are then subjected to a second grinding and mixing process to obtain a mixture. An inert polymer binder aqueous solution was added dropwise to the mixture to obtain a semi-dry mixture; The semi-dry mixture is subjected to multiple roll shearing processes, causing the inert polymer binder of the inert polymer-bonded aqueous solution to bind the sulfur-carbon composite material and the 1T′-MoS2O3 composite material together. 2x Se 2(1-x) The crystals are tightly interwoven and encapsulated, resulting in semi-dry inclusions; The semi-dry inclusions are calendered to obtain a self-supporting positive electrode composite film. The self-supporting positive electrode composite film is pressed onto the current collector to obtain the sulfur-based positive electrode sheet; The sulfur-based positive electrode, negative electrode, electrolyte, and separator are assembled to obtain the electrochemical device.
9. The method for preparing the electrochemical device according to claim 8, characterized in that, The second grinding and mixing speed is 50 rpm / min-150 rpm / min, and the time is 5 min-15 min.
10. The method for preparing the electrochemical device according to claim 8, characterized in that, The number of times the roller shearing is 5-10, the roller speed is 15mm / s-25mm / s, and the time is 4min-8min.
Citation Information
Patent Citations
Lithium-sulfur battery positive electrode, preparation method thereof and lithium-sulfur battery
CN113839044A
MoS2-transition metal monatomic material-sulfur positive electrode and preparation method and application thereof
CN122370325A