A lithium-sulfur battery and its preparation method

By employing a combination design of Co-modified sulfurized polyacrylonitrile cathode, sulfonyl-modified boron nitride nanomaterial modification layer, and gradient-distributed active lithium metal layer with silicon-carbon anode layer in lithium-sulfur batteries, the problems of insufficient conductivity, polysulfide shuttle, and lithium loss in lithium-sulfur batteries are solved, thereby improving the charge-discharge efficiency, cycle stability, and safety of the batteries.

CN123120831APending Publication Date: 2026-11-17CHINA ENERGY LITHIUM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611503240.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium-sulfur batteries suffer from problems such as insufficient electronic conductivity, polysulfide shuttle, and severe lithium loss in the positive electrode, separator, and negative electrode, resulting in low charge-discharge efficiency, poor cycle stability, and insufficient safety.

Method used

The design employs a combination of a Co-modified sulfurized polyacrylonitrile cathode layer, a sulfonyl-modified boron nitride nanomaterial modification layer, and a gradient-distributed active lithium metal layer with a silicon-carbon anode layer. This design utilizes the Co-N3S1 coordination structure to catalyze polysulfide reactions, the electrostatic repulsion of boron nitride nanomaterials and the Li-O coordination bonds to intercept polysulfides, and the gradient-distributed self-replenishing lithium structure to compensate for lithium loss.

Benefits of technology

It significantly improves the charge and discharge energy efficiency of lithium-sulfur batteries, reduces polysulfide shuttle, enhances cycle stability and safety performance, and achieves high initial coulombic efficiency and excellent battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120831A_ABST
    Figure CN123120831A_ABST
Patent Text Reader

Abstract

This invention discloses a lithium-sulfur battery and its preparation method, belonging to the field of lithium-sulfur battery technology. In the positive electrode of this lithium-sulfur battery, a Co-N3S1 coordination structure is formed by cobalt single atoms, pyridine nitrogen, and framework sulfur, which bidirectionally catalyzes the sulfur conversion reaction and anchors polysulfides. Carboxylated carbon nanotubes provide a three-dimensional conductive network, synergistically constructing a multi-level polysulfide trapping network with the cobalt single atoms. On the negative electrode, a sulfonyl-modified boron nitride modification layer intercepts polysulfides through a dual mechanism of electrostatic repulsion and chemical anchoring, and induces uniform lithium deposition. The active lithium metal layer and the garnet-structured silicon-carbon negative electrode form a gradient-distributed self-compensating lithium structure, which can precisely compensate for the loss of active lithium throughout the system. The synergistic effect of these three components gives the battery high initial coulombic efficiency, excellent cycle stability, and good safety performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-sulfur battery technology, specifically relating to a lithium-sulfur battery and its preparation method. Background Technology

[0002] Lithium-sulfur batteries are widely recognized as one of the most promising next-generation high-energy-density rechargeable battery systems due to their extremely high theoretical specific capacity (1675 mAh / g) and theoretical energy density (2600 Wh / kg). However, their practical application is still constrained by the combined limitations of the positive electrode, separator, and negative electrode, and existing technologies have not yet formed an effective systemic solution.

[0003] In the cathode, sulfurized polyacrylonitrile (SPAN) forms a conjugated conductive framework through thermally induced PAN cyclization, forming stable CS covalent bonds with sulfur. This transforms the charge-discharge path into a solid-solid reaction mechanism, effectively alleviating the dissolution and shuttle problems of polysulfides. However, SPAN cathodes still have the following shortcomings: First, the intrinsic electronic conductivity is insufficient, and the electron conduction inside the thick electrode is uneven, resulting in significant concentration polarization and voltage tailing during charge-discharge. Second, the solid-solid conversion reaction kinetic barrier is high, with large activation energies for Li2S nucleation and oxidation decomposition, leading to a significant difference in lithium insertion / extraction potential and a high polarization voltage in the full cell. Third, trace amounts of short-chain polysulfides are still released during charge-discharge, causing irreversible loss of active lithium under long cycles. To improve the reaction kinetics of SPAN cathodes, there are reports of introducing metal catalytic components in existing technologies. However, conventional metal doping is prone to migration and aggregation during high-temperature processing, making stable dispersion difficult. In addition, existing conductive additives for SPAN cathodes mostly only perform physical conductivity and lack the ability to chemically adsorb sulfur intermediates; the conductive network and sulfur fixation function have not yet been effectively coupled.

[0004] In terms of separator modification, boron nitride (BN) nanomaterials have been explored for use in lithium-sulfur battery separator modification due to their good chemical stability and certain adsorption capacity for polysulfides. However, BN has obvious limitations: First, its surface lacks active functional groups, resulting in poor dispersibility in slurry, weak bonding between the coating and the separator interface, and easy cracking and detachment during long cycles; Second, BN is a wide bandgap insulating material, and the modification layer will significantly increase the lithium-ion transmembrane transport impedance, which is detrimental to rate performance; Third, the blocking of polysulfides mainly relies on physical barrier effects, lacking a chemical capture mechanism, resulting in insufficient long-term effectiveness.

[0005] For the anode, replacing lithium metal anodes with silicon-carbon (Si / C) composites is an important direction for improving the safety of lithium-sulfur batteries. However, silicon-based materials have low initial coulombic efficiency, which needs to be compensated for through pre-lithiation. However, trace amounts of polysulfides generated during charging and discharging of the cathode can still pass through the separator to reach the anode, where they undergo irreversible side reactions with the pre-lithiated active lithium, causing additional lithium loss. Existing pre-lithiation processes typically only design the lithium source quantitatively for the initial SEI film lithium loss of silicon-carbon itself, without fully considering the lithium loss caused by the cycle side reactions caused by polysulfide shuttle, resulting in insufficient pre-lithiation to cover the total active lithium loss of the system. In addition, the release of lithium source in conventional pre-lithiated silicon-carbon lacks controllability and cannot match the actual lithium loss rate. Summary of the Invention

[0006] Therefore, the purpose of this invention is to provide a lithium-sulfur battery and a method for preparing the same.

[0007] In a first aspect, the present invention provides a lithium-sulfur battery, comprising: The positive electrode layer is a Co-modified vulcanized polyacrylonitrile positive electrode layer; A membrane layer is disposed on one side of the positive electrode layer; The boron nitride nanomaterial modification layer is a sulfonyl-modified boron nitride nanomaterial modification layer, which is disposed on the side of the separator layer away from the positive electrode layer; An active lithium metal layer is disposed on the side of the boron nitride nanomaterial modified layer away from the separator layer; A silicon-carbon anode layer is disposed on the side of the active lithium metal layer away from the boron nitride nanomaterial modification layer; An electrolyte is filled between the positive electrode layer, the separator layer, the boron nitride nanomaterial modification layer, the active lithium metal layer, and the silicon-carbon negative electrode layer.

[0008] Secondly, the present invention provides a method for preparing a lithium-sulfur battery, comprising the following steps: S1. Polyacrylonitrile, carbon nanotubes, and cobalt source are dispersed in a solvent to obtain an electrospinning solution; the electrospinning solution is loaded into an injection pump and electrospinning is performed. After spinning, a nanofiber membrane is obtained; the nanofiber membrane is pre-oxidized in an oxygen-containing atmosphere, and then sulfur vapor is introduced in an inert atmosphere to perform in-situ sulfurization treatment to obtain a sulfurized nanofiber membrane. S2. After the vulcanized nanofiber membrane is crushed, crushed material is obtained; the crushed material, conductive agent, and binder are mixed and a solvent is added to obtain a slurry; the slurry is coated on the positive electrode current collector and dried to obtain a positive electrode assembly composed of positive electrode layer and positive electrode current collector. S3. Mix silicon-carbon material, binder, and conductive agent, add solvent, and prepare slurry; coat the slurry onto the surface of the negative electrode current collector, and dry it to obtain silicon-carbon negative electrode layer-negative electrode current collector; load lithium source onto the surface of silicon-carbon negative electrode layer by any of the following methods: pressure bonding transfer, coating, or physical vapor deposition, to obtain a composite layer composed of active lithium metal layer-silicon-carbon negative electrode layer-negative electrode current collector layer. S4. After mixing the sulfonyl-modified boron nitride nanomaterials, lithium salt, binder and additives, add solvent to obtain a mixed slurry; coat the mixed slurry onto the active lithium metal layer of the composite layer, and after drying, obtain the negative electrode component; S5. Assemble the positive electrode assembly, separator, and negative electrode assembly into a battery cell, and inject electrolyte to obtain a lithium-sulfur battery.

[0009] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) The positive electrode layer of the lithium-sulfur battery of the present invention is pre-oxidized by a fiber membrane in an air atmosphere. During the pre-oxidation process, polyacrylonitrile undergoes cyclization, dehydrogenation and oxidative crosslinking. Cobalt ions and nitrogen-containing sites and oxygen-containing sites generated by cyclization are used to construct Co-N in situ. x O y Atomic coordination structure. During the pre-oxidation stage in an air atmosphere, the polymer backbone undergoes cyclization and pre-crosslinking and solidification, ensuring that cobalt is not easily reduced to metal particles by the carbon matrix during subsequent high-temperature sulfidation. In the subsequent high-temperature sulfidation stage in an inert atmosphere, oxygen-containing coordination is removed due to the thermal decomposition of oxygen-containing functional groups. Sulfur atoms in sulfur vapor form Co-S coordination bonds with cobalt, replacing the original Co-O coordination, while the thermally stable pyridine nitrogen Co-N coordination remains unchanged. Finally, the pyridine nitrogen formed by the cyclization of cobalt single atoms with polyacrylonitrile and the framework sulfur introduced by sulfidation constitute a stable Co-N3S1 four-coordinate structure. During charge and discharge, the Co-N3S1 sites form dynamically reversible Co-S coordination with polysulfide intermediates, bidirectionally catalyzing the sulfur conversion reaction, significantly reducing the energy barrier for Li2S nucleation and oxidative decomposition, effectively reducing lithium insertion / extraction polarization, and improving charge and discharge energy efficiency. At the same time, the cobalt single-atom sites have a strong polar anchoring effect on polysulfides, which can effectively suppress polysulfide shuttle from the positive electrode source. In addition, carboxylated carbon nanotubes provide a continuous three-dimensional conductive network, which can compensate for the insufficient intrinsic conductivity of sulfurized polyacrylonitrile, improve the uniformity of electron transport inside the thick electrode, and alleviate concentration polarization. The carboxyl polar sites on its surface can also assist in sulfur fixation and work with cobalt single-atom sites to construct a multi-level sulfur capture network, further enhancing the sulfur fixation capability of the cathode.

[0010] (2) In the boron nitride nanomaterial modification layer of the lithium-sulfur battery of the present invention, sulfonyl groups introduce high-density negatively charged sulfur-oxygen polar functional groups on the surface of boron nitride. On the one hand, they rely on the electrostatic repulsion of polysulfide anions by negative charges, and chemically anchor the trace sulfur intermediates that penetrate the separator through Li-O coordination bonds, thus constructing a second polysulfide interception barrier after the positive electrode polysulfide capture network, avoiding polysulfides from corroding the SEI film of the silicon-carbon negative electrode and reducing the additional loss of endogenous active lithium. On the other hand, sulfonyl groups can form abundant reversible coordination transport channels with lithium ions, balancing the lithium ion flux at the negative electrode interface and forming continuous Li + Clusters induce uniform lithium deposition and inhibit lithium dendrite growth; at the same time, the high mechanical modulus hard framework of boron nitride nanomaterials can physically block the continuous growth of lithium dendrites from piercing the separator, effectively improving battery safety and overcoming the problems of gas expansion and micro-short circuit failure in traditional silicon-sulfur systems; in addition, the dispersibility of modified boron nitride in slurry is significantly improved, the bonding force between the modified layer and the separator interface is enhanced, it is not easy to crack and fall off during long cycle, and maintains the stability of the negative electrode interface for a long time.

[0011] (3) The present invention prepares a self-compensating lithium structure silicon-carbon anode layer with a quantitative slow-release gradient distribution by setting an active lithium metal layer on the silicon-carbon anode layer; the active lithium metal layer will form an internal lithium source with a gradient distribution in the silicon-carbon anode layer. This lithium source has a slow-release characteristic, which can accurately compensate for the inherent active lithium loss caused by the formation of SEI film during the first charge and discharge, and continuously compensate for the lithium loss caused by polysulfide side reactions during the cycle, thus realizing the dual internal lithium self-compensation effect of the whole system. Combined with the dual-layer sulfur suppression design of positive electrode composite layer and modified boron nitride modification layer, the effective active lithium of the battery is retained to the greatest extent.

[0012] (4) In this invention, the above-mentioned single-atom modified polyacrylonitrile composite positive electrode, sulfonated boron nitride multifunctional modification layer and silicon-carbon negative electrode with quantitative slow-release gradient distribution self-replenishing lithium structure work together to effectively maintain the integrity of the negative electrode SEI film, reduce the damage of polysulfides to the negative electrode interface, and enable the battery to have high initial coulombic efficiency, excellent cycle stability and good safety performance. Attached Figure Description

[0013] Figure 1 SEM image of the garnet-structured silicon-carbon composite material prepared in Example 1.

[0014] Figure 2 This is a schematic diagram of the structure of a lithium-sulfur battery cell in an embodiment of the present invention. Detailed Implementation

[0015] To facilitate understanding of the present invention, the present invention will be described more fully and in detail below with reference to the accompanying drawings and preferred embodiments, but the scope of protection of the present invention is not limited to the following specific embodiments.

[0016] In a first aspect, the present invention provides a lithium-sulfur battery, comprising: The positive electrode layer is a Co-modified vulcanized polyacrylonitrile positive electrode layer; A membrane layer is disposed on one side of the positive electrode layer; The boron nitride nanomaterial modification layer is a sulfonyl-modified boron nitride nanomaterial modification layer, which is disposed on the side of the separator layer away from the positive electrode layer; An active lithium metal layer is disposed on the side of the boron nitride nanomaterial modified layer away from the separator layer; A silicon-carbon anode layer is disposed on the side of the active lithium metal layer away from the boron nitride nanomaterial modification layer; An electrolyte is filled between the positive electrode layer, the separator layer, the boron nitride nanomaterial modification layer, the active lithium metal layer, and the silicon-carbon negative electrode layer.

[0017] This invention improves the overall electrochemical performance of lithium-sulfur batteries through the synergistic design of the positive and negative electrodes. The positive electrode employs a composite system of cobalt-modified polyacrylonitrile (PPI) and carboxylated carbon nanotubes. The pyridine nitrogen formed by the cyclization of cobalt single atoms with PPI and the skeletal sulfur introduced by sulfidation form stable Co-N3S1 four-coordinate single-atom sites, which can bidirectionally catalyze the sulfur conversion reaction, significantly reducing the energy barrier for Li2S nucleation and decomposition, and helping to reduce lithium insertion / extraction polarization. The carboxylated carbon nanotubes provide a three-dimensional conductive network, helping to compensate for the insufficient intrinsic conductivity of PPI. Together, they construct a multi-level polysulfide trapping network, significantly reducing polysulfide shuttle at the positive electrode source. The negative electrode employs a sulfonyl-modified boron nitride nanomaterial modification layer. Through electrostatic repulsion and Li-O coordination bonds, it intercepts polysulfides penetrating the separator, constructing a second polysulfide barrier. Simultaneously, the sulfonyl coordination transport channels help balance the interfacial lithium-ion flux and induce uniform lithium deposition. Combined with the high mechanical modulus of the boron nitride framework, it helps suppress lithium dendrite growth and improve safety. An active lithium metal layer is placed between the silicon-carbon anode layer and the boron nitride modification layer, forming a gradient-distributed self-compensating lithium structure with the garnet-structured silicon-carbon anode. A slow-release internal lithium source is constructed within the silicon-carbon particles through a gradient-distribution pre-lithiation process. This lithium source helps compensate for the inherent active lithium loss during the initial film formation of the silicon-carbon anode and the lithium loss caused by polysulfide side reactions during cycling, based on the system's capacity ratio. The dual-barrier design of positive electrode sulfur suppression and negative electrode interception helps reduce polysulfide shuttle, thereby facilitating the effective retention of internally compensated lithium and reducing side reaction consumption. The synergistic effect of these components helps improve the battery's initial coulombic efficiency, cycle stability, and safety performance.

[0018] In some embodiments, the lithium-sulfur battery further includes: a positive electrode current collector layer disposed on the side of the positive electrode layer away from the separator layer; In some embodiments, the lithium-sulfur battery further includes a negative electrode current collector layer disposed on the side of the silicon-carbon negative electrode layer away from the active lithium metal layer.

[0019] In some embodiments, the thickness of the positive electrode layer is 80~500μm, including but not limited to: 80μm, 100μm, 200μm, 300μm, 400μm, 500μm, etc., preferably 100~300μm.

[0020] In some embodiments, the thickness of the boron nitride nanomaterial modification layer is 0.5~10μm, including but not limited to: 0.5μm, 1μm, 2μm, 5μm, 8μm, 10μm, etc.

[0021] In some embodiments, the thickness of the active lithium metal layer is 0.5~40μm, including but not limited to: 0.5μm, 1μm, 5μm, 10μm, 20μm, 30μm, 40μm, etc., preferably 1~20μm.

[0022] In some embodiments, the thickness of the silicon-carbon anode layer is 50~300μm, including but not limited to: 50μm, 80μm, 100μm, 200μm, 300μm, etc., preferably 80~200μm.

[0023] In some embodiments, the silicon-carbon material in the silicon-carbon anode layer is a garnet-structured silicon-carbon material.

[0024] In some embodiments, the boron nitride nanomaterial is one of boron nitride nanotubes, boron nitride nanosheets, and hexagonal boron nitride powder.

[0025] In some embodiments, the electrolyte is one of carbonate-based electrolyte, ether-based electrolyte, and gel polymer electrolyte.

[0026] Secondly, the present invention provides a method for preparing a lithium-sulfur battery, comprising the following steps: S1. Polyacrylonitrile, carbon nanotubes, and cobalt source are dispersed in a solvent to obtain an electrospinning solution; the electrospinning solution is loaded into an injection pump and electrospinning is performed. After spinning, a nanofiber membrane is obtained; the nanofiber membrane is pre-oxidized in an oxygen-containing atmosphere, and then sulfur vapor is introduced in an inert atmosphere to perform in-situ sulfurization treatment to obtain a sulfurized nanofiber membrane. S2. After the vulcanized nanofiber membrane is crushed, crushed material is obtained; the crushed material, conductive agent, and binder are mixed and a solvent is added to obtain a slurry; the slurry is coated on the positive electrode current collector and dried to obtain a positive electrode assembly composed of positive electrode layer and positive electrode current collector. S3. Mix silicon-carbon material, binder, and conductive agent, add solvent, and prepare slurry; coat the slurry onto the surface of the negative electrode current collector, and dry it to obtain silicon-carbon negative electrode layer-negative electrode current collector; load lithium source onto the surface of silicon-carbon negative electrode layer by any of the following methods: pressure bonding transfer, coating, or physical vapor deposition, to obtain a composite layer composed of active lithium metal layer-silicon-carbon negative electrode layer-negative electrode current collector layer. S4. After mixing the sulfonyl-modified boron nitride nanomaterials, lithium salt, binder and additives, add solvent to obtain a mixed slurry; coat the mixed slurry onto the active lithium metal layer of the composite layer, and after drying, obtain the negative electrode component; S5. Assemble the positive electrode assembly, separator, and negative electrode assembly into a battery cell, and inject electrolyte to obtain a lithium-sulfur battery.

[0027] In this invention, the positive electrode layer is prepared by electrospinning combined with in-situ vulcanization. By co-spinning polyacrylonitrile, carbon nanotubes and cobalt source, cobalt atoms are anchored to the pyridine nitrogen sites generated by PAN cyclization during the pre-oxidation stage, achieving atomic-level dispersion from the source and avoiding cobalt agglomeration. Subsequently, in-situ vulcanization with sulfur vapor allows sulfur atoms to be uniformly introduced into the fiber skeleton, forming a stable Co-N3S1 coordination structure in synergy with cobalt atoms. Carboxylated carbon nanotubes are uniformly coated in the fiber matrix during spinning. After crushing and pulping, they help to build a continuous three-dimensional conductive network inside the electrode. The process is simple and controllable, which helps to ensure the uniform distribution and structural stability of the positive electrode layer components.

[0028] This invention employs methods such as pressure bonding transfer, coating, or physical vapor deposition to load active lithium onto the surface of a silicon-carbon anode layer. During the loading process, active lithium can permeate and diffuse inward along the pores and interparticle gaps of the silicon-carbon anode layer, thereby forming a gradient distribution structure in the thickness direction of the silicon-carbon anode layer where the lithium concentration gradually decreases from the surface to the interior, and giving this structure quantitative sustained-release characteristics. The gradient distribution design with quantitative slow-release characteristics mentioned above has the following beneficial effects: (1) The surface lithium concentration is high, which can preferentially compensate for the active lithium consumed by the first lithium insertion of silicon-carbon anode to form SEI film; (2) The internal lithium concentration is low and uniformly distributed, which can continuously and slowly release active lithium during long cycle, compensate for lithium loss caused by polysulfide side reactions, and help maintain battery cycle stability; (3) The gradient distribution can avoid active lithium from being concentrated in a single area, which can cause local stress concentration and structural damage, and help alleviate the mechanical stress caused by volume expansion of silicon-carbon anode, and improve the structural integrity of anode; (4) The slow-release characteristics prevent the internal lithium source from being released in large quantities in a short period of time, which helps to avoid the aggravation of side reactions caused by over-lithiation, and achieve precise and on-demand compensation of lithium source.

[0029] In some embodiments, in step S1, the mass ratio of polyacrylonitrile, carbon nanotubes, and cobalt source is (70~90):(5~15):(0.5~15); including but not limited to: 70:15:15, 80:10:10, 90:9.5:0.5, 75:15:10, 85:10:5, 85:14:1, 83:12:5, etc.; the cobalt source is one or more of cobalt chloride, cobalt nitrate, and cobalt sulfate; and the carbon nanotubes are carboxylated carbon nanotubes.

[0030] In some embodiments, in step S1, the solvent is N,N-dimethylformamide (DMF), and the mass ratio of polyacrylonitrile to solvent is 1:(2~15), including but not limited to: 1:2, 1:5, 1:8, 1:10, 1:12, 1:15, etc., preferably 1:(5~10).

[0031] In some embodiments, in step S1, the solvent is a combination of DMF and TFA (trifluoroacetic acid) in a volume ratio of (90~95):(5~10), and the volume ratio includes, but is not limited to, 90:10, 91:9, 92:8, 93:7, 96:4, 95:5, etc.

[0032] In this invention, trifluoroacetic acid is used as an auxiliary solvent in combination with DMF, mainly for the following purposes: Trifluoroacetic acid is a strong organic acid that can ionize in solution to generate ions, which helps to improve the conductivity of the spinning solution and promotes the full stretching of the jet during spinning; its acidic environment can protonate the surface of carbon nanotubes, enhance the interfacial interaction between carbon nanotubes and the PAN matrix, reduce the tendency of carbon nanotubes to aggregate, and help them to be more uniformly dispersed in the spinning solution; at the same time, the addition of trifluoroacetic acid can promote the dissolution and dissociation of cobalt source through the acidic environment, which helps cobalt ions to be evenly distributed in the spinning solution, thereby facilitating the uniform anchoring of cobalt atoms in the fiber skeleton during subsequent pre-oxidation and vulcanization processes, and ensuring the uniform formation of Co-N3S1 coordination sites.

[0033] In some embodiments, in step S1, the electrospinning process parameters are as follows: the voltage is 10~20kV, including but not limited to: 10kV, 12kV, 15kV, 18kV, 20kV, etc.; the distance from the spinneret to the aluminum foil receiving plate is 12~18cm, including but not limited to: 12cm, 13cm, 14cm, 15cm, 16cm, 17cm, 18cm, etc.; the injection pump's feed rate is 0.1~1.5mL / h, including but not limited to: 0.1mL / h, 0.2mL / h, 0.5mL / h, 0.8mL / h, 1.0mL / h, 1.2mL / h, 1.5mL / h, etc., preferably 0.3~1.0mL / h.

[0034] In some embodiments, in step S1, the oxygen-containing atmosphere is an air atmosphere or an oxygen atmosphere; the temperature of the pre-oxidation treatment is 200~350℃, including but not limited to: 200℃, 250℃, 300℃, 350℃, etc.; the time of the pre-oxidation treatment is 2~6h, including but not limited to: 2h, 3h, 4h, 5h, 6h, etc.

[0035] In some embodiments, in step S1, the inert atmosphere is a nitrogen atmosphere or an argon atmosphere; the ratio of the total mass of sulfur vapor introduced to the mass of nanofibers is (2~5):1, including but not limited to: 2:1, 3:1, 4:1, 5:1, etc.; the in-situ vulcanization temperature is 350~600℃, including but not limited to: 350℃, 400℃, 450℃, 500℃, 550℃, 600℃, etc.; the in-situ vulcanization time is 2~6h, including but not limited to: 2h, 3h, 4h, 5h, 6h, etc.

[0036] In some embodiments, in step S2, the conductive agent is one or more of Super P, acetylene black, and Ketjen black; the binder is one or more of polyvinylidene fluoride (PVDF), acrylonitrile copolymer LA133, and acrylonitrile copolymer LA132; the solvent is N-methylpyrrolidone (NMP); and the positive electrode current collector is an aluminum foil current collector.

[0037] In some embodiments, in step S2, the mass ratio of the crushed material, the conductive agent, and the binder is (78~85):(5~10):(8~12), including but not limited to: 78:10:12, 80:9:11, 83:8:9, 84:5:11, 85:7:8, etc.; the solid content of the slurry is 15~60wt%, including but not limited to: 15wt%, 20wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, etc., preferably 20~50wt%.

[0038] In some embodiments, in step S3, the silicon-carbon material is a garnet-structured silicon-carbon material, which is prepared by: adding oligowalled carbon nanotubes to anhydrous ethanol, ultrasonically dispersing them to form a suspension; adding nano-silicon powder to the suspension, stirring and mixing it, then adding phenolic resin and polyvinylpyrrolidone (PVP), stirring evenly to obtain a spray slurry; spray drying the spray slurry, and then carbonizing it to obtain a garnet-structured silicon-carbon material.

[0039] This invention employs a garnet-structured silicon-carbon material as the negative electrode lithium storage substrate, which is more conducive to achieving a gradient concentration distribution of active lithium. In the garnet structure, silicon nanoparticles are coated with a carbon shell, and there are pores and gaps between the particles and between the silicon particles and the carbon shell. These pore structures provide channels for active lithium to permeate and diffuse inward along the thickness direction of the silicon-carbon layer during loading. Due to the influence of the pore structure and diffusion path on the permeation process, active lithium diffuses layer by layer from the surface of the silicon-carbon layer inward, with a natural decreasing concentration trend. This results in a gradient distribution structure in the thickness direction of the silicon-carbon negative electrode layer, with the lithium concentration gradually decreasing from the surface to the interior. This gradient distribution results in a higher lithium concentration at the surface, which can preferentially compensate for the active lithium consumed during the initial film formation, while the lower internal lithium concentration allows for slow release during cycling, continuously compensating for lithium loss caused by polysulfide side reactions, and realizing the slow-release self-replenishment function of the internal lithium source.

[0040] In some embodiments, the mass ratio of nano-silica powder, oligowalled carbon nanotubes, and phenolic resin is (55~75):(5~15):(10~35), including but not limited to: 55:15:30, 55:10:35, 60:10:30, 65:5:30, 70:5:25, 75:15:10, etc.; polyvinylpyrrolidone accounts for 1~5wt% of the total mass of the solid phase, including but not limited to: 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, etc.; the solid content of the spray granulation slurry is 10~30wt%, including but not limited to: 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, etc.

[0041] In some embodiments, the spray drying temperature is 130~200℃, including but not limited to: 130℃, 140℃, 150℃, 160℃, 170℃, 180℃, 190℃, 200℃, etc.; the carbonization temperature is 700~1000℃, including but not limited to: 700℃, 750℃, 800℃, 850℃, 900℃, 950℃, 1000℃, etc.; the carbonization time is 2~6h, including but not limited to: 2h, 3h, 4h, 5h, 6h, etc.

[0042] In some embodiments, in step S3, the adhesive is one or more of polyvinylidene fluoride (PVDF), sodium carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR); the solvent is one or more of N-methylpyrrolidone, tetrahydrofuran, dimethyl ethyl ether, dichloromethane, ethylene carbonate, dimethyl carbonate, diethyl carbonate, diethyl carbonate, methyl ethyl carbonate, ethylene glycol dimethyl ether, and water; and the conductive agent is one or more of Super P, acetylene black, and Ketjen black.

[0043] In some embodiments, in step S3, the mass ratio of silicon carbide material, conductive agent, and binder is (85~94):(3~10):(3~10), including but not limited to: 85:10:5, 85:5:10, 90:7:3, 92:4:4, 94:3:3, etc.; the solid content of the slurry is 30~60wt%, including but not limited to: 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, etc., preferably 40~50wt%.

[0044] In some embodiments, in step S3, the lithium source is either a lithium film or a lithium sheet.

[0045] In some embodiments, step S4, the method for preparing sulfonyl-modified boron nitride nanomaterials includes the following steps: (1) After mixing boron nitride nanomaterials with sodium hydroxide solution, a hydrothermal reaction was carried out. After the reaction was completed, centrifugation was performed, and the solid material was washed until neutral to obtain hydroxylated boron nitride nanomaterials. (2) After mixing silane coupling agent KH-550, ethanol and water, a pre-hydrolysis reaction was carried out to obtain a pre-hydrolysis solution. Then, hydroxylated boron nitride nanomaterials were added to the pre-hydrolysis solution for a grafting reaction. After the grafting reaction was completed, acetone was added to continue the reaction. After the reaction was completed, solid-liquid separation was carried out to obtain aminated boron nitride nanomaterials. (3) The aminated boron nitride nanomaterials were dispersed in dichloromethane to obtain a dispersion; the dispersion was placed in an ice bath and p-benzenesulfonyl chloride solution was added dropwise. After the addition was completed, triethylamine was added to obtain a pre-reaction solution; the pre-reaction solution was heated to room temperature under a nitrogen atmosphere to carry out the modification reaction. After the reaction was completed, centrifugation was performed to obtain sulfonyl-modified boron nitride powder.

[0046] In some embodiments, in step (1), the concentration of the sodium hydroxide solution is 3~10 mol / L, including but not limited to: 3 mol / L, 5 mol / L, 8 mol / L, 10 mol / L, etc.; the mass ratio of boron nitride nanomaterials to sodium hydroxide solution is 1:(25~100), including but not limited to: 1:25, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90, 1:100, etc.; the temperature of the hydrothermal reaction is 100~160℃, including but not limited to: 130℃, 140℃, 150℃, 160℃, etc.; the time of the hydrothermal reaction is 10~20h, including but not limited to: 10h, 12h, 15h, 18h, 20h, etc.

[0047] In some embodiments, in step (2), the volume ratio of ethanol to water is (7~10):1, including but not limited to: 7:1, 8:1, 9:1, 10:1, etc.; the total volume ratio of ethanol and water to the volume ratio of silane coupling agent KH-550 is (10~50):1, including but not limited to: 10:1, 20:1, 30:1, 40:1, 50:1, etc.; preferably (15~45):1; the temperature of the pre-hydrolysis reaction is 40~60℃, including but not limited to: 40℃, 45℃, 50℃, 55℃, 60℃, etc.; the time of the pre-hydrolysis reaction is 20~40min, including but not limited to: 20min, 25min, 30min, 35min, 40min, etc.

[0048] In some embodiments, in step (2), the mass of the silane coupling agent KH-550 is 1 to 20 wt% of the mass of the hydroxylated boron nitride nanomaterial, including but not limited to: 1 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, etc.; the grafting reaction temperature is 70 to 90°C, including but not limited to: 70°C, 75°C, 80°C, 85°C, 90°C, etc.; the grafting reaction time is 2 to 24 h, including but not limited to: 2 h, 5 h, 10 h, 15 h, 20 h, 24 h, etc.

[0049] In some embodiments, in step (2), after the grafting reaction is completed, after the system is cooled to 20~35°C, acetone is added according to the total volume ratio of ethanol and water to acetone of 1:(1.2~2.5), and the reaction continues for 15~40 min. After the solvent induces precipitation of powder, centrifugation, washing and drying are performed to obtain aminated boron nitride nanomaterials.

[0050] In some embodiments, in step (3), the mass ratio of the aminated boron nitride nanomaterial to dichloromethane is 1:(10~80), including but not limited to: 1:10, 1:20, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, etc., preferably 1:(20~60); the mass ratio of the aminated boron nitride nanomaterial to p-benzenesulfonyl chloride is 1:(0.1~0.6), including but not limited to: 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, etc., preferably 1:(0.2~0.5); p-benzenesulfonyl chloride The mass ratio of the benzenesulfonyl chloride to triethylamine is 1:(0.4~0.8), including but not limited to: 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, etc., preferably 1:(0.5~0.7); the solvent for the p-benzenesulfonyl chloride solution is DCM, with a concentration of 0.1~0.5mol / L, including but not limited to: 0.1mol / L, 0.2mol / L, 0.3mol / L, 0.4mol / L, 0.5mol / L, etc.; the modification reaction time is 10~15h, including but not limited to: 10h, 11h, 12h, 13h, 14h, 15h, etc.

[0051] In some embodiments, in step S4, the lithium salt is one or more of lithium fluoride, lithium nitride, lithium hexafluorophosphate, lithium trifluoromethanesulfonate, lithium perchlorate, lithium bisfluorosulfonylimide, lithium bistrifluoromethanesulfonylimide, lithium carbonate, lithium oxalate, lithium bicarbonate, lithium acetate, lithium halide, lithium sulfate, and lithium hydroxide. The adhesive is selected from one or more of the following: polyvinyl alcohol, polyethylene oxide, polybutene-styrene, polystyrene-butadiene copolymer, polyvinylidene fluoride, polystyrene, polycarboxymethyl cellulose, polyurethane, methacrylate, epoxy resin and its derivatives, styrene-butadiene rubber, and sodium carboxymethyl cellulose; The additive is selected from one or more of polyvinylpyrrolidone, sodium dodecylbenzenesulfonate, sodium dodecyl sulfate, and hexadecyltrimethylammonium bromide; The solvent is selected from one or more of N-methylpyrrolidone, tetrahydrofuran, dimethyl ethyl ether, dichloromethane, ethylene carbonate, dimethyl carbonate, diethyl carbonate, diethyl carbonate, methyl ethyl carbonate, and ethylene glycol dimethyl ether.

[0052] In some embodiments, in step S4, the mass ratio of sulfonyl-modified boron nitride powder to lithium salt is (1~20):(1~5), including but not limited to: 1:1, 1:3, 1:5, 10:1, 10:3, 10:5, 20:1, 20:3, 20:5, etc.; the mass ratio of sulfonyl-modified boron nitride powder to binder is (1~20):(1~5), including but not limited to: 1:1, 1:3, 1:5, 10:1, 10:3, 10:5, 20, etc. The mass ratio of sulfonyl-modified boron nitride powder to additives is (1~20):(0.5~2), including but not limited to: 1:0.5, 1:1, 1:2, 10:0.5, 10:1, 10:2, 20:0.5, 20:1, etc.; the solid content of the mixed slurry is 1~20wt%, including but not limited to: 1wt%, 5wt%, 10wt%, 15wt%, 20wt%, etc., preferably 2~15wt%.

[0053] Preparation Example 1 Oligowalled carbon nanotubes were added to anhydrous ethanol and sonicated to form a nanotube suspension. Then, silica powder was added to the suspension at a mass ratio of 65:10 (silica powder to oligowalled carbon nanotubes), and the mixture was stirred until homogeneous. Next, phenolic resin was added at a mass ratio of 10:25 (oligowalled carbon nanotubes to phenolic resin), along with 3 wt% PVP as a dispersant. The mixture was stirred until homogeneous, resulting in a uniform spray slurry with a solid content of 20 wt%. The spray slurry was then spray-dried at an inlet temperature of 160°C to obtain the precursor powder.

[0054] The precursor powder was placed in a tube furnace and carbonized at 850°C under a nitrogen protective atmosphere for 3 hours. After natural cooling to room temperature, the garnet-structured silicon-carbon composite material was obtained.

[0055] Figure 1 The image shows the microstructure of the pomegranate-structured silicon-carbon composite material obtained in this preparation example. It can be seen that the secondary particles are regularly spherical, composed of a large number of fine primary particles tightly packed together. Its morphology is highly similar to the packing of pomegranate seeds, hence it is named the pomegranate-structured silicon-carbon composite material.

[0056] Preparation Example 2 Oligowalled carbon nanotubes were added to anhydrous ethanol and sonicated to form a nanotube suspension. Then, silica powder was added to the suspension at a mass ratio of 55:15 (silica powder to oligowalled carbon nanotubes), and the mixture was stirred until homogeneous. Next, phenolic resin was added at a mass ratio of 15:30 (oligowalled carbon nanotubes to phenolic resin), and 1 wt% PVP was added as a dispersant. The mixture was stirred until homogeneous, resulting in a uniform spray slurry with a solid content of 10 wt%. The spray slurry was then spray-dried at an inlet temperature of 130°C to obtain the precursor powder.

[0057] The precursor powder was placed in a tube furnace and carbonized at 700°C under a nitrogen protective atmosphere for 6 hours. After natural cooling to room temperature, the garnet-structured silicon-carbon composite material was obtained.

[0058] Preparation Example 3 Oligowalled carbon nanotubes were added to anhydrous ethanol and sonicated to form a nanotube suspension. Then, nanosilica powder was added to the suspension at a mass ratio of 75:5 (nanosilica powder to oligowalled carbon nanotubes), and the mixture was stirred until homogeneous. Next, phenolic resin was added at a mass ratio of 5:10 (oligowalled carbon nanotubes to phenolic resin), along with 5 wt% PVP as a dispersant. The mixture was stirred until homogeneous, resulting in a uniform spray slurry with a solid content of 30 wt%. The spray slurry was then spray-dried at an inlet temperature of 200°C to obtain the precursor powder.

[0059] The precursor powder was placed in a tube furnace and carbonized at 1000°C under a nitrogen protective atmosphere for 2 hours. After natural cooling to room temperature, the garnet-structured silicon-carbon composite material was obtained.

[0060] Preparation Example 4 (1) After mixing boron nitride nanotubes with a NaOH solution of 6 mol / L at a mass-to-volume ratio of 1:50, the mixture was added to a hydrothermal reactor lined with polytetrafluoroethylene. The mixture was heated to 140°C and subjected to a hydrothermal reaction for 18 h. After the reaction was completed, the reactor was allowed to cool naturally to room temperature. The suspension was poured out and the solid precipitate was collected by centrifugation. The solid precipitate was acid-washed until the pH of the supernatant was 7. The mixture was then washed twice with water and dried under vacuum to obtain hydroxylated boron nitride nanotubes.

[0061] (2) Add silane coupling agent KH-550 to a mixed solvent of ethanol and water in a volume ratio of 9:1 and a volume ratio of silane coupling agent KH-550 to the mixed solvent of 1:30. Pre-hydrolyze at 50°C for 30 min to obtain a pre-hydrolyzed reaction solution. Add hydroxylated boron nitride nanomaterials to the pre-hydrolyzed reaction solution according to the mass of silane coupling agent KH-550 being 10 wt% of the mass of hydroxylated boron nitride nanomaterials. Perform a grafting reaction at 80°C for 12 h. After the grafting reaction is completed, after the system cools to room temperature, add acetone according to a volume ratio of mixed solvent to acetone of 1:1.8. Continue stirring for 25 min. After the solvent induces precipitation of powder, centrifuge, wash and dry in sequence to obtain aminated boron nitride nanomaterials.

[0062] (3) The aminated boron nitride nanomaterials and dichloromethane were added to anhydrous dichloromethane at a mass ratio of 1:40. After ultrasonic dispersion under nitrogen atmosphere for 40 min, a dispersion was obtained. The dispersion was placed in an ice bath, and a p-benzenesulfonyl chloride solution (the solvent of the p-benzenesulfonyl chloride solution was dichloromethane, and the concentration of p-benzenesulfonyl chloride was 0.3 mol / L) was added dropwise at a mass ratio of aminated boron nitride nanotubes to p-benzenesulfonyl chloride of 1:0.35. After the addition was completed, Triethylamine was added as an acid-binding agent to capture the HCl produced in the reaction, according to a mass ratio of p-benzenesulfonyl chloride to triethylamine of 1:0.6. Then, the ice bath was removed, and the mixture was naturally heated to room temperature. Under nitrogen protection, the mixture was stirred and modified for 12 hours. After the reaction was completed, the reaction solution was centrifuged and the solid material was washed three times with anhydrous DCM, twice with anhydrous ethanol, and then washed with deionized water until pH=7. Finally, it was vacuum dried at 60℃ for 12 hours to obtain sulfonyl-modified boron nitride nanotubes.

[0063] Preparation Example 5 The preparation method is basically the same as that in Example 4, except that in step (3), the mass ratio of aminated boron nitride nanotubes to p-benzenesulfonyl chloride is 1:0.1.

[0064] Preparation Example 6 The preparation method is basically the same as that in Example 4, except that in step (3), the mass ratio of amino boron nitride nanotubes to p-benzenesulfonyl chloride is 1:0.6.

[0065] Preparation Example 7 (1) After mixing boron nitride nanotubes with a 3 mol / L NaOH solution at a mass-to-volume ratio of 1:25, the mixture was added to a polytetrafluoroethylene-lined hydrothermal reactor and heated to 100°C for 10 h of hydrothermal reaction. After the reaction was completed, the reactor was allowed to cool naturally to room temperature. The suspension was poured out and the solid precipitate was collected by centrifugation. The solid precipitate was acid-washed until the pH of the supernatant was 7, then washed twice with water and dried under vacuum to obtain hydroxylated boron nitride nanotubes.

[0066] (2) Add silane coupling agent KH-550 to a mixed solvent of ethanol and water in a volume ratio of 7:1 and a volume ratio of silane coupling agent KH-550 to the mixed solvent of 1:10. Pre-hydrolyze at 40°C for 20 min to obtain a pre-hydrolyzed reaction solution. Add hydroxylated boron nitride nanomaterials to the pre-hydrolyzed reaction solution according to the mass of silane coupling agent KH-550 being 1 wt% of the mass of hydroxylated boron nitride nanomaterials. Perform a grafting reaction at 70°C for 24 h. After the grafting reaction is completed, after the system cools to room temperature, add acetone according to a volume ratio of mixed solvent to acetone of 1:1.2. Continue stirring for 15 min. After the solvent induces precipitation of powder, centrifuge, wash and dry in sequence to obtain aminated boron nitride nanomaterials.

[0067] (3) The aminated boron nitride nanomaterials and dichloromethane were added to anhydrous dichloromethane at a mass ratio of 1:10. After ultrasonic dispersion under a nitrogen atmosphere for 40 min, a dispersion was obtained. The dispersion was placed in an ice bath, and a p-benzenesulfonyl chloride solution (the solvent of the p-benzenesulfonyl chloride solution was dichloromethane, and the concentration of p-benzenesulfonyl chloride was 0.1 mol / L) was added dropwise at a mass ratio of aminated boron nitride nanotubes to p-benzenesulfonyl chloride of 1:0.4. After the addition was completed, Triethylamine was added as an acid-binding agent to capture the HCl produced in the reaction at a mass ratio of 1:0.4 to p-benzenesulfonyl chloride and triethylamine. Then, the ice bath was removed, and the mixture was naturally heated to room temperature. Under nitrogen protection, the mixture was stirred and modified for 10 hours. After the reaction was completed, the reaction solution was centrifuged, and the solid material was washed three times with anhydrous DCM, twice with anhydrous ethanol, and then washed with deionized water until pH=7. Finally, it was vacuum dried at 60℃ for 12 hours to obtain sulfonyl-modified boron nitride nanotubes.

[0068] Preparation Example 8 (1) After mixing boron nitride nanotubes with a 10 mol / L NaOH solution at a mass-to-volume ratio of 1:100, the mixture was added to a polytetrafluoroethylene-lined hydrothermal reactor and heated to 160°C for 20 h of hydrothermal reaction. After the reaction was completed, the reactor was allowed to cool naturally to room temperature. The suspension was poured out and the solid precipitate was collected by centrifugation. The solid precipitate was acid-washed until the pH of the supernatant was 7, then washed twice with water and dried under vacuum to obtain hydroxylated boron nitride nanotubes.

[0069] (2) Add silane coupling agent KH-550 to a mixed solvent of ethanol and water in a volume ratio of 10:1 and a volume ratio of silane coupling agent KH-550 to the mixed solvent of 1:50. Pre-hydrolyze at 60°C for 40 min to obtain a pre-hydrolyzed reaction solution. Add hydroxylated boron nitride nanomaterials to the pre-hydrolyzed reaction solution according to the mass of silane coupling agent KH-550 being 20 wt% of the mass of hydroxylated boron nitride nanomaterials. Perform a grafting reaction at 90°C for 6 h. After the grafting reaction is completed, after the system cools to room temperature, add acetone according to a volume ratio of mixed solvent to acetone of 1:2.5. Continue stirring for 40 min. After the solvent induces precipitation of powder, centrifuge, wash and dry in sequence to obtain aminated boron nitride nanomaterials.

[0070] (3) The aminated boron nitride nanomaterials and dichloromethane were added to anhydrous dichloromethane at a mass ratio of 1:80. After ultrasonic dispersion under nitrogen atmosphere for 40 min, a dispersion was obtained. The dispersion was placed in an ice bath, and a p-benzenesulfonyl chloride solution (the solvent of the p-benzenesulfonyl chloride solution was dichloromethane, and the concentration of p-benzenesulfonyl chloride was 0.5 mol / L) was added dropwise at a mass ratio of aminated boron nitride nanotubes to p-benzenesulfonyl chloride of 1:0.3. After the addition was completed, Triethylamine was added as an acid-binding agent to capture the HCl produced in the reaction at a mass ratio of 1:0.8 to p-benzenesulfonyl chloride and triethylamine. The mixture was then removed from the ice bath and allowed to naturally warm to room temperature. Under nitrogen protection, the mixture was stirred and modified for 15 hours. After the reaction was completed, the reaction solution was centrifuged and the solid material was washed three times with anhydrous DCM, twice with anhydrous ethanol, and then washed with deionized water until pH=7. Finally, the solid material was vacuum dried at 60℃ for 12 hours to obtain sulfonyl-modified boron nitride nanotubes.

[0071] Example 1 The schematic diagram of the battery structure in this embodiment is shown below. Figure 2 As shown, the electrode includes an aluminum foil positive current collector; a Co-modified sulfurized polyacrylonitrile positive electrode layer disposed on one side surface of the positive current collector; a separator layer disposed on the side surface of the positive electrode layer away from the positive current collector; a sulfonyl-modified boron nitride nanotube modification layer disposed on the side surface of the separator layer away from the positive electrode layer; an active lithium metal layer disposed on the side surface of the boron nitride nanotube modification layer away from the separator layer; a silicon-carbon negative electrode layer disposed on the side surface of the active lithium metal layer away from the boron nitride nanotube modification layer; a copper foil negative current collector disposed on the side surface of the silicon-carbon negative electrode layer away from the active lithium metal layer; and an electrolyte filling the space between the positive electrode layer, the separator layer, the boron nitride nanotube modification layer, the active lithium metal layer, and the silicon-carbon negative electrode layer.

[0072] The electrolyte consists of a PE membrane, a 1M LiPF6 solution, and a mixed solvent composed of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 3:5:2. The additives are FEC (fluoroethylene carbonate) and vitamin C (VC), with contents of 8wt% and 1wt% of the total weight of the electrolyte, respectively.

[0073] The specific preparation method is as follows: S1. Polyacrylonitrile, carboxylated carbon nanotubes, and cobalt nitrate were dispersed in DMF at a mass ratio of 82:10:8 to obtain an electrospinning solution with a polyacrylonitrile concentration of 12wt%. The electrospinning solution was loaded into an injection pump, and the injection pump rate was adjusted to 0.72 mL / h, the voltage to 15 kV, and the distance between the spinneret and the aluminum foil receiving plate to 15 cm for electrospinning. After spinning, a nanofiber membrane was obtained. The nanofiber membrane was heated to 280℃ in air for pre-oxidation treatment for 3 h, and then the atmosphere was changed to nitrogen atmosphere. After heating to 420℃, sulfur vapor with a mass three times that of the nanofiber membrane was introduced for in-situ sulfurization treatment for 3 h to obtain the sulfurized nanofiber membrane.

[0074] S2. After the vulcanized nanofiber membrane is crushed, crushed material is obtained. The crushed material, Super P and PVDF are mixed in a mass ratio of 82:8:10, and NMP is added until the solid content of the slurry is 40wt%, and the slurry is obtained. The slurry is coated on an aluminum foil current collector and dried. The thickness of the positive electrode layer is about 200μm, and a positive electrode module composed of positive electrode layer and positive electrode current collector is obtained.

[0075] S3. The garnet-structured silicon-carbon material, PVDF, and Super P prepared in Example 1 were mixed at a mass ratio of 90:5:5. NMP was added until the solid content of the slurry was 48 wt%, and the slurry was prepared. The slurry was coated onto the surface of the copper foil negative electrode current collector. After drying, the thickness of the silicon-carbon negative electrode layer was about 100 μm, and a silicon-carbon negative electrode layer-negative electrode current collector was obtained. A 15 μm thick lithium film was coated and transferred onto the surface of the silicon-carbon negative electrode layer by a roll forming process, and a composite layer composed of an active lithium metal layer, a silicon-carbon negative electrode layer, and a negative electrode current collector layer was obtained.

[0076] S4. The sulfonyl-modified boron nitride nanotubes, lithium difluorosulfonylimide, PVDF and polyvinylpyrrolidone prepared in Preparation Example 4 were mixed in a mass ratio of 10:3:3:1. NMP was added until the solid content of the slurry was 10wt% to obtain a mixed slurry. The mixed slurry was coated onto the active lithium metal layer of the composite layer. After drying, the thickness of the modified layer was 5μm to obtain the negative electrode component.

[0077] S5. Assemble the positive electrode assembly, separator, and negative electrode assembly into a battery cell, and inject electrolyte to obtain a lithium-sulfur battery.

[0078] Comparative Example 1 The structure is basically the same as in Example 1, except that the lithium-sulfur battery does not have a sulfonyl-modified boron nitride nanomaterial modification layer, i.e., an active lithium metal layer disposed on the side of the separator layer away from the positive electrode layer.

[0079] Step S4 is omitted in the corresponding preparation method; that is, the composite layer consisting of an active lithium metal layer, a silicon-carbon anode layer, and an anode current collector layer is used as the anode component.

[0080] Comparative Example 2 The results are basically the same as in Example 1, except that the positive electrode layer is a sulfurized polyacrylonitrile positive electrode layer and the modification layer is a boron nitride nanomaterial modification layer.

[0081] The corresponding step S1 is: S1. Polyacrylonitrile and carboxylated carbon nanotubes were dispersed in DMF at a mass ratio of 82:10 to obtain an electrospinning solution with a polyacrylonitrile concentration of 12wt%. The electrospinning solution was loaded into an injection pump, and the injection pump rate was adjusted to 0.72 mL / h, the voltage to 15 kV, and the distance between the spinneret and the aluminum foil receiving plate to 15 cm for electrospinning. After spinning, a nanofiber membrane was obtained. The nanofiber membrane was heated to 280℃ in air for pre-oxidation treatment for 3 h, and then the atmosphere was changed to nitrogen atmosphere. After heating to 420℃, sulfur vapor with a mass three times that of the nanofiber membrane was introduced for in-situ sulfurization treatment for 3 h to obtain the sulfurized nanofiber membrane.

[0082] The corresponding step S4 is: S4. After mixing boron nitride nanotubes, lithium bis(fluorosulfonyl)imide, PEO and sodium dodecylbenzenesulfonate in a mass ratio of 10:3:3:1, NMP is added until the solid content of the slurry is 10wt% to obtain a mixed slurry. The mixed slurry is coated onto the active lithium metal layer of the composite layer. After drying, the thickness of the modified layer is 5μm to obtain the negative electrode component.

[0083] Comparative Example 3 The example is basically the same as in Example 1, except that the sulfonyl-modified boron nitride nanotube modification layer is a boron nitride nanotube modification layer. The corresponding step S4 is: S4. After mixing boron nitride nanomaterials, lithium bis(fluorosulfonyl)imide, PEO and sodium dodecylbenzenesulfonate in a mass ratio of 10:3:3:1, NMP is added until the solid content of the slurry is 10wt% to obtain a mixed slurry. The mixed slurry is coated onto the active lithium metal layer of the composite layer. After drying, the thickness of the modified layer is 5μm to obtain the negative electrode component.

[0084] Comparative Example 4 It is basically the same as Example 1, except that the positive electrode layer is a vulcanized polyacrylonitrile positive electrode layer.

[0085] The corresponding step S1 is: S1. Polyacrylonitrile and carboxylated carbon nanotubes were dispersed in DMF at a mass ratio of 82:10 to obtain an electrospinning solution with a polyacrylonitrile concentration of 12wt%. The electrospinning solution was loaded into an injection pump, and the injection pump rate was adjusted to 0.72 mL / h, the voltage to 15 kV, and the distance between the spinneret and the aluminum foil receiving plate to 15 cm for electrospinning. After spinning, a nanofiber membrane was obtained. The nanofiber membrane was heated to 280℃ in air for pre-oxidation treatment for 3 h, and then the atmosphere was changed to nitrogen atmosphere. After heating to 420℃, sulfur vapor with a mass three times that of the nanofiber membrane was introduced for in-situ sulfurization treatment for 3 h to obtain the sulfurized nanofiber membrane.

[0086] Comparative Example 5 It is basically the same as Example 1, except that there is no active lithium metal layer.

[0087] The corresponding step S3 is: S3. The garnet-structured silicon-carbon material, PVDF and Super P prepared in Example 1 were mixed in a mass ratio of 90:5:5. NMP was added until the solid content of the slurry was 48wt% to prepare a slurry. The slurry was coated onto the surface of the copper foil negative electrode current collector. After drying, the thickness of the silicon-carbon negative electrode layer was about 100μm, and a composite layer consisting of silicon-carbon negative electrode layer and negative electrode current collector was obtained.

[0088] Example 2 It is basically the same as Example 1, except that TFA is added to the electrospinning solution in step S1.

[0089] The corresponding step S1 is as follows: S1. Polyacrylonitrile, carboxylated carbon nanotubes, and cobalt nitrate were dispersed in a mixed solvent of DMF and TFA in a mass ratio of 82:10:8 to obtain an electrospinning solution with a polyacrylonitrile concentration of 12wt%. The electrospinning solution was loaded into an injection pump, and the injection pump rate was adjusted to 0.72 mL / h, the voltage to 15 kV, and the distance between the spinneret and the aluminum foil receiving plate to 15 cm for electrospinning. After spinning, a nanofiber membrane was obtained. The nanofiber membrane was heated to 280℃ in an air atmosphere for pre-oxidation treatment for 3 h. Then, the atmosphere was changed to nitrogen atmosphere, and the temperature was raised to 420℃. Sulfur vapor with a mass three times that of the nanofiber membrane was introduced for in-situ sulfurization treatment for 3 h to obtain the sulfurized nanofiber membrane.

[0090] Example 3 It is basically the same as Example 1, except that the thickness of the active lithium metal layer is 5 μm.

[0091] Example 4 It is basically the same as Example 1, except that the thickness of the active lithium metal layer is 30 μm.

[0092] Example 5 The process is basically the same as in Example 1, except that in step S4, the sulfonyl-modified boron nitride nanotubes prepared in Example 5 are used.

[0093] Example 6 The process is basically the same as in Example 1, except that in step S4, the sulfonyl-modified boron nitride nanotubes prepared in Example 6 are used.

[0094] Example 7 The schematic diagram of the battery structure in this embodiment is shown below. Figure 2 As shown, the electrode includes an aluminum foil positive current collector; a Co-modified sulfurized polyacrylonitrile positive electrode layer disposed on one side surface of the positive current collector; a separator layer disposed on the side surface of the positive electrode layer away from the positive current collector; a sulfonyl-modified boron nitride nanosheet modification layer disposed on the side surface of the separator layer away from the positive electrode layer; an active lithium metal layer disposed on the side surface of the boron nitride nanosheet modification layer away from the separator layer; a silicon-carbon negative electrode layer disposed on the side surface of the active lithium metal layer away from the boron nitride nanosheet modification layer; a copper foil negative current collector disposed on the side surface of the silicon-carbon negative electrode layer away from the active lithium metal layer; and an electrolyte filling the space between the positive electrode layer, the separator layer, the boron nitride nanosheet modification layer, the active lithium metal layer, and the silicon-carbon negative electrode layer.

[0095] The electrolyte consists of 1M LiPF6, a mixed solvent of EC and DMC in a 1:1 volume ratio, and 5wt% FEC as an additive.

[0096] The specific preparation method is as follows: S1. Polyacrylonitrile, carboxylated carbon nanotubes, and cobalt chloride were dispersed in a mixed solvent of DMF and TFA at a mass ratio of 70:5:0.5 (the volume ratio of DMF to TFA was 90:10) to obtain an electrospinning solution with a polyacrylonitrile concentration of 10 wt%. The electrospinning solution was loaded into an injection pump, and the injection pump rate was adjusted to 0.3 mL / h, the voltage to 10 kV, and the distance between the spinneret and the aluminum foil receiving plate to 12 cm for electrospinning. After spinning, a nanofiber membrane was obtained. The nanofiber membrane was heated to 200 °C in an air atmosphere for pre-oxidation treatment for 6 h. Then, the atmosphere was changed to nitrogen atmosphere, and the temperature was raised to 350 °C. Sulfur vapor with a total mass twice that of the nanofiber membrane was introduced for in-situ sulfurization treatment for 6 h to obtain the sulfurized nanofiber membrane.

[0097] S2. After the vulcanized nanofiber membrane is crushed, crushed material is obtained. The crushed material, acetylene black and LA133 are mixed in a mass ratio of 78:10:12, and NMP is added until the solid content of the slurry is 20wt% to obtain a slurry. The slurry is coated on an aluminum foil current collector and dried. The thickness of the positive electrode layer is about 80μm, and a positive electrode module composed of positive electrode layer and positive electrode current collector is obtained.

[0098] S3. The garnet-structured silicon-carbon material, PVDF, and Ketjen black prepared in Example 2 were mixed at a mass ratio of 85:10:5. Deionized water was added until the solid content of the slurry was 30 wt%, and the slurry was prepared. The slurry was coated onto the surface of the copper foil negative electrode current collector. After drying, the thickness of the silicon-carbon negative electrode layer was about 50 μm, and a silicon-carbon negative electrode layer-negative electrode current collector was obtained. A lithium film with a thickness of 1 μm was loaded onto the surface of the silicon-carbon negative electrode layer by physical vapor deposition to obtain a composite layer composed of an active lithium metal layer, a silicon-carbon negative electrode layer, and a negative electrode current collector layer.

[0099] S4. The sulfonyl-modified boron nitride nanosheets prepared in Preparation Example 7, lithium hexafluorophosphate, polyethylene oxide and sodium dodecylbenzenesulfonate were mixed in a mass ratio of 1:1:1:0.5, and NMP was added until the solid content of the slurry was 2wt% to obtain a mixed slurry. The mixed slurry was coated onto the active lithium metal layer of the composite layer, and after drying, the thickness of the modified layer was 0.5μm to obtain the negative electrode component.

[0100] S5. Assemble the positive electrode assembly, separator, and negative electrode assembly into a battery cell, and inject electrolyte to obtain a lithium-sulfur battery.

[0101] Example 8 The schematic diagram of the battery structure in this embodiment is shown below. Figure 2 As shown, the electrode includes an aluminum foil positive current collector; a Co-modified sulfurized polyacrylonitrile positive electrode layer disposed on one side surface of the positive current collector; a separator layer disposed on the side surface of the positive electrode layer away from the positive current collector; a sulfonyl-modified boron nitride nanotube modification layer disposed on the side surface of the separator layer away from the positive electrode layer; an active lithium metal layer disposed on the side surface of the boron nitride nanotube modification layer away from the separator layer; a silicon-carbon negative electrode layer disposed on the side surface of the active lithium metal layer away from the boron nitride nanotube modification layer; a copper foil negative current collector disposed on the side surface of the silicon-carbon negative electrode layer away from the active lithium metal layer; and an electrolyte filling the space between the positive electrode layer, the separator layer, the boron nitride nanotube modification layer, the active lithium metal layer, and the silicon-carbon negative electrode layer.

[0102] Wherein: the diaphragm is a PE diaphragm; the electrolyte consists of 1M LiTFSI and 0.1M LiNO3, and the solvent is a mixed solvent composed of DOL (1,3-dioxolane) and DME (1,2-dimethoxyethane) in a volume ratio of 1:1.

[0103] The specific preparation method is as follows: S1. Polyacrylonitrile, carboxylated carbon nanotubes, and cobalt sulfate were dispersed in a mixed solvent of DMF and TFA at a mass ratio of 90:15:15 (the volume ratio of DMF to TFA was 95:5) to obtain an electrospinning solution with a polyacrylonitrile concentration of 18wt%. The electrospinning solution was loaded into an injection pump, and the injection pump rate was adjusted to 1.0 mL / h, the voltage to 20 kV, and the distance between the spinneret and the aluminum foil receiving plate to 18 cm for electrospinning. After spinning, a nanofiber membrane was obtained. The nanofiber membrane was heated to 350℃ in an oxygen atmosphere for 2 h for pre-oxidation treatment. Then, the atmosphere was changed to argon atmosphere, and the temperature was raised to 600℃. Sulfur vapor with a mass of 5 times that of the nanofiber membrane was introduced for in-situ sulfurization treatment for 2 h to obtain a sulfurized nanofiber membrane.

[0104] S2. After the vulcanized nanofiber membrane is crushed, crushed material is obtained. The crushed material, Ketjen black and PVDF are mixed in a mass ratio of 85:5:10, and NMP is added until the solid content of the slurry is 58wt%, and the slurry is obtained. The slurry is coated on the aluminum foil current collector and dried. The thickness of the positive electrode layer is about 300μm, and the positive electrode module composed of positive electrode layer and positive electrode current collector is obtained.

[0105] S3. The garnet-structured silicon-carbon material prepared in Example 3 (with a mass ratio of nano-silicon powder, oligo-walled carbon nanotubes, and phenolic resin of 75:15:10, PVP accounting for 5 wt% of the total solid phase mass, a spray granulation slurry solid content of 30 wt%, a spray drying temperature of 200℃, a carbonization temperature of 1000℃, and a carbonization time of 2 h), PVDF, and Super P were mixed in a mass ratio of 94:3:3. NMP was then added until the solid content of the slurry reached 60 wt%, and a slurry was prepared. The slurry was coated onto the surface of a copper foil negative electrode current collector. After drying, the thickness of the silicon-carbon negative electrode layer was approximately 200 μm, resulting in a silicon-carbon negative electrode layer-negative electrode current collector. A 20 μm thick lithium sheet was pressure-coated onto the surface of the silicon-carbon negative electrode layer to obtain a composite layer consisting of an active lithium metal layer, a silicon-carbon negative electrode layer, and a negative electrode current collector layer.

[0106] S4. The sulfonyl-modified boron nitride nanotubes prepared in Preparation Example 8, lithium bis(trifluoromethanesulfonylimide), polyvinylidene fluoride, and hexadecyltrimethylammonium bromide were mixed in a mass ratio of 20:5:5:2. NMP was added until the solid content of the slurry was 15wt% to obtain a mixed slurry. The mixed slurry was coated onto the active lithium metal layer of the composite layer. After drying, the thickness of the modified layer was 10μm to obtain the negative electrode component.

[0107] S5. Assemble the positive electrode assembly, separator, and negative electrode assembly into a battery cell, and inject electrolyte to obtain a lithium-sulfur battery.

[0108] The lithium-sulfur batteries from Examples 1-8 and Comparative Examples 1-5 were left to stand for 12 hours before performance testing. Specific test conditions were as follows: constant current charging and discharging at 25°C, with a charging / discharging voltage range of 1.7-2.6V and a charge / discharge rate of 0.2C. The initial capacity of the battery was denoted as C0. One full charge-discharge cycle was recorded. The charging and discharging process was repeated as described above, and the battery capacity was tested after each cycle until the battery capacity reached 80% of C0 or a short circuit occurred. The number of cycles at this point was recorded, and the first-efficiency period was calculated. The test results are shown in Table 1.

[0109] Table 1 As can be seen from the data in Table 1, the lithium-sulfur battery in Example 1 exhibits good cycle performance and high initial efficiency. Compared with Example 1, the lithium-sulfur battery in Example 2 shows further improvements in both cycle performance and initial efficiency. This may be because, during the preparation of the nanofiber membrane, trifluoroacetic acid can further improve the dispersion of cobalt in the fiber skeleton, which helps to uniformly form Co-N3S1 coordination sites, thereby enhancing the catalytic activity and sulfur fixation efficiency of the cathode. Compared with Example 1, the lithium-sulfur batteries prepared in Examples 3 and 4 show a certain degree of decrease in both cycle performance and initial efficiency. This may be because when the lithium membrane is thin, the gradient distribution depth of active lithium within the silicon-carbon layer is insufficient, resulting in a low total amount of endogenous lithium source, making it difficult to continuously compensate for lithium loss during cycling. Conversely, when the lithium membrane is thick, it is not conducive to the pore permeation effect of the garnet-structured silicon-carbon material, and excessive active lithium concentrated on the surface may trigger excessive lithiation side reactions. Compared with Example 1, the lithium-sulfur batteries prepared in Examples 5 and 6 showed a certain degree of reduction in cycle performance and initial efficiency. This may be because when there are too few sulfonyl groups in the modified layer, the ability to chemically intercept polysulfides is insufficient, making it difficult to effectively protect the SEI film of the negative electrode; while when there are too many sulfonyl groups, too many lithium clusters are formed, hindering the normal transport of lithium ions and being detrimental to uniform lithium deposition. In Examples 7 and 8, the material selection and preparation process parameters were adjusted, and the performance of the corresponding batteries fluctuated to some extent, but the overall performance was better, indicating that the technical solution of the present invention has a wide process applicability window.

[0110] In Comparative Example 1, the lithium-sulfur battery lacked a modification layer, resulting in a significant decrease in cycle performance and initial efficiency compared to Example 1. This is likely due to the absence of a second polysulfide barrier, allowing polysulfides to penetrate the separator and directly corrode the SEI film of the silicon-carbon anode, causing substantial irreversible loss of active lithium and leading to a significant performance degradation. In Comparative Example 2, the lithium-sulfur battery also showed a significant decrease in both cycle performance and initial efficiency compared to Example 1. This is likely because Co was not introduced into the cathode layer, preventing the formation of Co-N3S1 coordination sites and thus losing its bidirectional catalytic function for sulfur conversion and its polar anchoring effect on polysulfides. Furthermore, the modification layer was not sulfonated, lacking both electrostatic repulsion and chemical anchoring mechanisms, limiting its effectiveness in blocking polysulfides and inducing uniform lithium deposition. In Comparative Example 3, the lithium-sulfur battery showed some improvement in cycle performance and initial efficiency compared to Comparative Example 2, but significantly lower than Example 1. This is likely because the boron nitride in the modification layer only relies on physical barriers to block polysulfides, lacking the chemical capture mechanism introduced by sulfonyl groups, resulting in limited ability to block polysulfides and induce lithium deposition. The lithium-sulfur battery in Comparative Example 4 showed some improvement in cycle performance and initial efficiency compared to Comparative Example 2, but was significantly inferior to Example 1. This may be because the cathode layer lacks Co, preventing the formation of Co-N3S1 coordination sites and resulting in insufficient catalytic activity and sulfur fixation capacity at the cathode source. Comparative Example 5, lacking a lithium metal layer, exhibited a significant decrease in cycle performance and initial efficiency compared to Example 1. This may be because without a lithium metal layer, the active lithium consumed during the initial film formation of the silicon-carbon anode and the lithium loss caused by polysulfide side reactions during cycling cannot be compensated, leading to continuous depletion of active lithium and a significant performance decline.

[0111] The above are merely preferred embodiments of the present invention and are not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of the present invention.

Claims

1. A lithium-sulfur battery, characterized in that, include: The positive electrode layer is a Co-modified vulcanized polyacrylonitrile positive electrode layer; A membrane layer is disposed on one side of the positive electrode layer; The boron nitride nanomaterial modification layer is a sulfonyl-modified boron nitride nanomaterial modification layer, which is disposed on the side of the separator layer away from the positive electrode layer; An active lithium metal layer is disposed on the side of the boron nitride nanomaterial modified layer away from the separator layer; A silicon-carbon anode layer is disposed on the side of the active lithium metal layer away from the boron nitride nanomaterial modification layer; An electrolyte is filled between the positive electrode layer, the separator layer, the boron nitride nanomaterial modification layer, the active lithium metal layer, and the silicon-carbon negative electrode layer.

2. The lithium-sulfur battery according to claim 1, characterized in that, The lithium-sulfur battery further includes: a positive electrode current collector layer, disposed on the side of the positive electrode layer away from the separator layer; The lithium-sulfur battery further includes a negative electrode current collector layer disposed on the side of the silicon-carbon negative electrode layer away from the active lithium metal layer.

3. The lithium-sulfur battery according to claim 1 or 2, characterized in that, The thickness of the positive electrode layer is 80~500μm; And / or, the thickness of the boron nitride nanomaterial modification layer is 0.5~10 μm; And / or, the thickness of the active lithium metal layer is 0.5~40μm; And / or, the thickness of the silicon-carbon anode layer is 50~300μm; And / or, the silicon-carbon material in the silicon-carbon anode layer is a garnet-structured silicon-carbon material; And / or, the boron nitride nanomaterial is one of boron nitride nanotubes, boron nitride nanosheets, and hexagonal boron nitride powder; And / or, the electrolyte is one of carbonate-based electrolyte, ether-based electrolyte, and gel polymer electrolyte.

4. A method for preparing a lithium-sulfur battery, characterized in that, Includes the following steps: S1. Polyacrylonitrile, carbon nanotubes, and cobalt source are dispersed in a solvent to obtain an electrospinning solution; the electrospinning solution is loaded into an injection pump and electrospinning is performed. After spinning, a nanofiber membrane is obtained; the nanofiber membrane is pre-oxidized in an oxygen-containing atmosphere, and then sulfur vapor is introduced in an inert atmosphere to perform in-situ sulfurization treatment to obtain a sulfurized nanofiber membrane. S2. After the vulcanized nanofiber membrane is crushed, crushed material is obtained; the crushed material, conductive agent, and binder are mixed and a solvent is added to obtain a slurry; the slurry is coated on the positive electrode current collector and dried to obtain a positive electrode assembly composed of positive electrode layer and positive electrode current collector. S3. Mix silicon-carbon material, binder, and conductive agent, add solvent, and prepare slurry; coat the slurry onto the surface of the negative electrode current collector, and dry it to obtain silicon-carbon negative electrode layer-negative electrode current collector; load lithium source onto the surface of silicon-carbon negative electrode layer by any of the following methods: pressure bonding transfer, coating, or physical vapor deposition, to obtain a composite layer composed of active lithium metal layer-silicon-carbon negative electrode layer-negative electrode current collector layer. S4. After mixing the sulfonyl-modified boron nitride nanomaterials, lithium salt, binder and additives, add solvent to obtain a mixed slurry; coat the mixed slurry onto the active lithium metal layer of the composite layer, and after drying, obtain the negative electrode component; S5. Assemble the positive electrode assembly, separator, and negative electrode assembly into a battery cell, and inject electrolyte to obtain a lithium-sulfur battery.

5. The method for preparing a lithium-sulfur battery according to claim 4, characterized in that, In step S1, the mass ratio of polyacrylonitrile, carbon nanotubes, and cobalt source is (70~90):(5~15):(0.5~15); the cobalt source is one or more of cobalt chloride, cobalt nitrate, and cobalt sulfate; the carbon nanotubes are carboxylated carbon nanotubes. And / or, in step S1, the solvent is DMF, and the mass ratio of polyacrylonitrile to solvent is 1:2 to 1:15; And / or, in step S1, the process parameters for electrospinning are: voltage of 10~20kV, distance from the spinneret to the aluminum foil receiving plate of 12~18cm, and injection pump speed of 0.1~1.5mL / h. And / or, in step S1, the oxygen-containing atmosphere is an air atmosphere or an oxygen atmosphere; the temperature of the pre-oxidation treatment is 200~350℃, and the time of the pre-oxidation treatment is 2~6h; And / or, in step S1, the inert atmosphere is a nitrogen atmosphere or an argon atmosphere; the ratio of the total mass of sulfur vapor introduced to the mass of nanofibers is (2~5):1; the in-situ sulfurization temperature is 350~600℃; and the in-situ sulfurization time is 2~6h.

6. The method for preparing a lithium-sulfur battery according to claim 4, characterized in that, In step S1, the solvent is a combination of DMF and TFA in a volume ratio of (90~95):(5~10); And / or, in step S2, the conductive agent is one or more of Super P, acetylene black, and Ketjen black; the binder is one or more of polyvinylidene fluoride, acrylonitrile copolymer LA133, and acrylonitrile copolymer LA132; the solvent is N-methylpyrrolidone; and the positive electrode current collector is an aluminum foil current collector. And / or, in step S2, the mass ratio of crushed material, conductive agent, and binder is (78~85):(5~10):(8~12); the solid content of the slurry is 15~60 wt%. And / or, in step S3, the silicon-carbon material is a garnet-structured silicon-carbon material, which is prepared by: adding oligowalled carbon nanotubes to anhydrous ethanol, ultrasonically dispersing them to form a suspension; adding nano-silicon powder to the suspension, stirring and mixing it, then adding phenolic resin and polyvinylpyrrolidone, stirring evenly to obtain a spray slurry; spray drying the spray slurry, and then carbonizing it to obtain a garnet-structured silicon-carbon material; And / or, in step S3, the adhesive is one or more of polyvinylidene fluoride, sodium carboxymethyl cellulose, and styrene-butadiene rubber; the solvent is one or more of N-methylpyrrolidone, tetrahydrofuran, dimethyl ethyl ether, dichloromethane, ethylene carbonate, dimethyl carbonate, diethyl carbonate, diethyl carbonate, methyl ethyl carbonate, ethylene glycol dimethyl ether, and water; and the conductive agent is one or more of Super P, acetylene black, and Ketjen black. And / or, in step S3, the mass ratio of silicon carbide material, conductive agent, and binder is (85~94):(3~10):(3~10); the solid content of the slurry is 30~60 wt%. And / or, in step S3, the lithium source is either a lithium film or a lithium sheet.

7. The method for preparing a lithium-sulfur battery according to claim 6, characterized in that, The mass ratio of the nano-silicon powder, oligowalled carbon nanotubes, and phenolic resin is (55~75):(5~15):(10~35), PVP accounts for 1~5wt% of the total solid phase mass, and the solid content of the spray-granulated slurry is 10~30wt%. And / or, the spray drying temperature is 130~200℃; the carbonization temperature is 700~1000℃; and the carbonization time is 2~6h.

8. The method for preparing a lithium-sulfur battery according to claim 4, characterized in that, In step S4, the preparation method of sulfonyl-modified boron nitride nanomaterials includes the following steps: (1) After mixing boron nitride nanomaterials with sodium hydroxide solution, a hydrothermal reaction was carried out. After the reaction was completed, centrifugation was performed, and the solid material was washed until neutral to obtain hydroxylated boron nitride nanomaterials. (2) After mixing silane coupling agent KH-550, ethanol and water, a pre-hydrolysis reaction was carried out to obtain a pre-hydrolysis solution. Then, hydroxylated boron nitride nanomaterials were added to the pre-hydrolysis solution for a grafting reaction. After the grafting reaction was completed, acetone was added to continue the reaction. After the reaction was completed, solid-liquid separation was carried out to obtain aminated boron nitride nanomaterials. (3) The aminated boron nitride nanomaterials were dispersed in dichloromethane to obtain a dispersion; the dispersion was placed in an ice bath and p-benzenesulfonyl chloride solution was added dropwise. After the addition was completed, triethylamine was added to obtain a pre-reaction solution; the pre-reaction solution was heated to room temperature under a nitrogen atmosphere to carry out the modification reaction. After the reaction was completed, centrifugation was performed to obtain sulfonyl-modified boron nitride powder.

9. The method for preparing a lithium-sulfur battery according to claim 8, characterized in that, In step (1), the concentration of sodium hydroxide solution is 3~10 mol / L; the mass ratio of boron nitride nanomaterial to sodium hydroxide solution is 1:(25~100); the temperature of hydrothermal reaction is 100~160℃, and the time of hydrothermal reaction is 10~20h; And / or, in step (2), the volume ratio of ethanol to water is (7~10):1; the total volume of ethanol and water to the volume ratio of silane coupling agent KH-550 is (10~50):1, preferably (15~45):1; the temperature of the pre-hydrolysis reaction is 40~60℃, and the time of the pre-hydrolysis reaction is 20~40min; And / or, in step (2), the mass of the silane coupling agent KH-550 is 1~20wt% of the mass of the hydroxylated boron nitride nanomaterial; the grafting reaction temperature is 70~90℃, and the grafting reaction time is 2~24h; And / or, in step (2), after the grafting reaction is completed, after the system is cooled to 20~35℃, acetone is added according to the total volume ratio of ethanol and water to acetone of 1:(1.2~2.5), and the reaction is continued for 15~40min. After the solvent induces the precipitation of powder, centrifugation, washing and drying are performed to obtain aminated boron nitride nanomaterials. And / or, in step (3), the mass ratio of aminated boron nitride nanomaterial to dichloromethane is 1:(10~80), preferably 1:(20~60); the mass ratio of aminated boron nitride nanomaterial to p-benzenesulfonyl chloride is 1:(0.1~0.6), preferably 1:(0.2~0.5); the mass ratio of p-benzenesulfonyl chloride to triethylamine is 1:(0.4~0.8), preferably 1:(0.5~0.7); the solvent of the p-benzenesulfonyl chloride solution is DCM with a concentration of 0.1~0.5mol / L; and the modification reaction time is 10~15h.

10. The method for preparing a lithium-sulfur battery according to claim 4, characterized in that, In step S4, the lithium salt is one or more of the following: lithium fluoride, lithium nitride, lithium hexafluorophosphate, lithium trifluoromethanesulfonate, lithium perchlorate, lithium bisfluorosulfonylimide, lithium bistrifluoromethanesulfonylimide, lithium carbonate, lithium oxalate, lithium bicarbonate, lithium acetate, lithium halide, lithium sulfate, and lithium hydroxide. The adhesive is selected from one or more of the following: polyvinyl alcohol, polyethylene oxide, polybutene-styrene, polystyrene-butadiene copolymer, polyvinylidene fluoride, polystyrene, polycarboxymethyl cellulose, polyurethane, methacrylate, epoxy resin and its derivatives, styrene-butadiene rubber, and sodium carboxymethyl cellulose; The additive is selected from one or more of polyvinylpyrrolidone, sodium dodecylbenzenesulfonate, sodium dodecyl sulfate, and hexadecyltrimethylammonium bromide; The solvent is selected from one or more of N-methylpyrrolidone, tetrahydrofuran, dimethyl ethyl ether, dichloromethane, ethylene carbonate, dimethyl carbonate, diethyl carbonate, diethyl carbonate, methyl ethyl carbonate, and ethylene glycol dimethyl ether; And / or, in step S4, the mass ratio of sulfonyl-modified boron nitride powder to lithium salt is (1~20):(1~5); the mass ratio of sulfonyl-modified boron nitride powder to binder is (1~20):(1~5); the mass ratio of sulfonyl-modified boron nitride powder to additive is (1~20):(0.5~2); and the solid content of the mixed slurry is 1~20wt%, preferably 2~15wt%.