Solid-state battery cells, battery devices, electrical devices, modified sulfide electrolytes and their preparation methods
By forming a Si-OS covalently linked silane and fluorosilane coating layer on the surface of the sulfide electrolyte matrix, the sensitivity of the sulfide electrolyte to water and oxygen was solved, improving the cycle performance and stability of solid-state battery cells and reducing the manufacturing cost.
Patent Information
- Application Number
- CN202510628926.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-15
- Publication Date
- 2026-11-17
AI Technical Summary
Sulfide solid electrolytes are sensitive to water and oxygen, which leads to increased side reactions, affects cycling performance and stability, and limits their large-scale application.
A modified sulfide electrolyte is used, and the sulfide electrolyte matrix and the coating layer are connected by Si-OS covalent bonds. The coating layer is composed of silane and/or fluorosilane, which reduces contact with air, especially water vapor, and forms stable Si-OS covalent bonds, thereby improving hydrophobicity and ion transport performance.
It effectively improves the stability and ion transport performance of sulfide electrolytes, reduces the impedance of solid-state battery cells, enhances cycle performance and production efficiency, and reduces manufacturing costs.
Smart Images

Figure CN123120836A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to a solid-state battery cell, a battery device, an electrical device, a modified sulfide electrolyte, and a method for preparing the same. Background Technology
[0002] Compared to battery cells using liquid electrolytes, solid-state battery cells use solid electrolyte materials, making them less prone to combustion and explosion, and offering high reliability and high energy density. Sulfide solid electrolytes possess ionic conductivity comparable to liquid electrolyte solutions; however, they are particularly sensitive to water and oxygen, requiring extremely stringent environmental conditions during preparation and use, severely limiting their large-scale application. Furthermore, side reactions between sulfide solid electrolytes and water or oxygen in the air can degrade the cycle performance of solid-state battery cells. Summary of the Invention
[0003] This disclosure provides a solid-state battery cell, a battery device, an electrical device, a modified sulfide electrolyte, and a method for preparing the same. The solid-state battery cell has good cycle performance.
[0004] In a first aspect, this disclosure provides a solid-state battery cell, including a positive electrode, an electrolyte layer, and a negative electrode, wherein the electrolyte layer is located between the positive electrode and the negative electrode, and at least one of the positive electrode, the electrolyte layer, and the negative electrode includes a modified sulfide electrolyte; the modified sulfide electrolyte includes a sulfide electrolyte matrix and a coating layer covering at least a portion of the surface of the sulfide electrolyte matrix; the sulfide electrolyte matrix and the coating layer are connected by Si-OS covalent bonds; the coating layer includes silane and / or fluorosilane.
[0005] The modified sulfide electrolyte in a solid-state battery cell includes a sulfide electrolyte matrix and a coating layer covering the sulfide electrolyte matrix. The sulfide electrolyte matrix and the coating layer are connected by Si-OS covalent bonds, thereby allowing the S-coating on the surface of the sulfide electrolyte to be bonded. 2-The S atoms are converted into stable S atoms in the Si-OS covalent bond. This allows them to occupy active sites on the surface of the sulfide electrolyte matrix, reducing side reactions between the sulfide electrolyte matrix and air. The coating layer of the modified sulfide electrolyte includes silanes and / or fluorosilanes, thus providing good hydrophobic effects. By coating at least a portion of the surface of the sulfide electrolyte matrix, the coating layer reduces the contact between the sulfide electrolyte matrix and air, particularly reducing the contact between the sulfide electrolyte matrix and water vapor in the air, thereby further reducing side reactions between the sulfide electrolyte matrix and air. This effectively improves the stability of the sulfide electrolyte matrix in air, allowing it to maintain good ion transport performance. Furthermore, it effectively improves the interfacial properties between the electrolyte and the positive / negative electrode active materials, reduces the impedance of the solid-state battery cell, and improves the cycle performance of the solid-state battery cell.
[0006] In some embodiments, the covering layer includes one or more of the structures shown in Formula 1.
[0007] R n SiY 4-n Formula 1
[0008] In Formula 1, n is 1, 2, or 3; R independently represents C1-C10 alkyl groups or C1-C10 alkyl groups substituted with F atoms. Optionally, at least one R represents a C1-C10 alkyl group substituted with F atoms. Y represents -OS-#, and the O atom in Y is connected to the Si atom in Formula 1, and # represents the connection position between the structure shown in Formula 1 and the sulfide electrolyte matrix.
[0009] In the structure shown in Formula 1, Y is formed by Si-OH reacting with S on the surface of the sulfide electrolyte matrix. 2- The reaction occurs, thereby consuming the side reaction active sites on the surface of the sulfide electrolyte matrix. This helps reduce side reactions between the sulfide electrolyte matrix and air. Furthermore, the structure shown in Formula 1 has high hydrophobicity, which helps reduce the contact between the sulfide electrolyte matrix and water vapor in the air, further reducing side reactions between the sulfide electrolyte matrix and air. Thus, the sulfide electrolyte matrix can maintain good ion transport performance, thereby improving the cycle performance of solid-state battery cells.
[0010] In some embodiments, R independently represents CF3(CF2)7CH2CH2-, CF3(CF2)5CH2CH2-, or CF3CH2CH2-.
[0011] In some embodiments, the coating layer further includes LiF.
[0012] The F atoms in R can react with lithium-containing impurities (e.g., lithium metal, or other lithium-containing materials) on the surface of the sulfide electrolyte matrix to generate LiF. LiF has extremely low solubility in water and exhibits excellent hydrophobic properties. Including LiF in the coating layer further enhances its hydrophobicity, reducing contact between the sulfide electrolyte matrix and water vapor in the air, thereby further reducing side reactions between the sulfide electrolyte matrix and air. Furthermore, LiF can improve the ion transport performance of the coating layer, thereby increasing the ionic conductivity of the modified sulfide electrolyte. This, in turn, is beneficial for improving the cycle performance of solid-state battery cells.
[0013] In some embodiments, the F element content in the coating layer is 0.3% to 1% based on the total mass of the modified sulfide electrolyte (100%). An appropriate amount of F element can better improve the hydrophobicity of the coating layer, thereby reducing side reactions between the sulfide electrolyte matrix and air. This can improve the interfacial properties between the modified sulfide electrolyte and the positive and / or negative electrode active materials, thereby improving the cycle performance of the solid-state battery cell.
[0014] In some embodiments, the coating layer further includes carbon (C), with the C content in the coating layer being 0.3% to 1% based on 100% of the total mass of the modified sulfide electrolyte. This allows the coating layer to have lower polarity, thereby enhancing its hydrophobicity. This, in turn, helps reduce the contact between the sulfide electrolyte matrix and water vapor in the air, further reducing side reactions between the sulfide electrolyte matrix and air.
[0015] In some embodiments, the coating layer includes carbon (C) and sulfur (F) elements, with the mass ratio of C to F elements in the coating layer being (0.3:1) to (0.7:1). This allows the coating layer to possess both good hydrophobicity and good flexibility.
[0016] In some embodiments, the thickness of the coating layer is 2 nm to 10 nm. This allows the modified sulfide electrolyte to have lower impedance while effectively isolating the sulfide electrolyte matrix from air, thereby improving the kinetic performance of the solid-state battery cell.
[0017] In some embodiments, the coating area ratio of the modified sulfide electrolyte is 90% or more, where the coating area ratio represents the ratio of the surface area of the coating layer to the surface area of the modified sulfide electrolyte.
[0018] In some embodiments, the coating area ratio of the modified sulfide electrolyte is 100%.
[0019] This effectively isolates the sulfide electrolyte matrix from air, thereby reducing side reactions between the sulfide electrolyte matrix and air, allowing the sulfide electrolyte matrix to maintain high ionic conductivity, and thus improving the cycle performance of solid-state battery cells.
[0020] In some embodiments, the volumetric particle size distribution (Dv50) of the modified sulfide electrolyte is 1 μm to 10 μm. This can improve the ion transport performance of the positive and / or negative electrodes, thereby enhancing the cycle performance of the solid-state battery cell.
[0021] In some embodiments, the ionic conductivity of the modified sulfide electrolyte is 1 × 10⁻⁶. -3 S / cm~8×10 -3 S / cm. This can effectively improve the interfacial performance between the electrolyte and the positive / negative electrode active materials, reduce the impedance of solid-state battery cells, and improve the cycle performance of solid-state battery cells.
[0022] In some embodiments, the positive electrode includes a positive electrode film layer, the positive electrode film layer includes a positive electrode active material and a modified sulfide electrolyte, and the positive electrode active material includes one or more of lithium transition metal oxides and their modified materials, lithium phosphates and their modified materials, lithium titanate, lithium niobate, sulfur, selenium, and tellurium.
[0023] In some embodiments, the electrolyte layer comprises a modified sulfide electrolyte.
[0024] In some embodiments, the negative electrode comprises lithium or a lithium alloy, or the negative electrode comprises a negative electrode active material and a modified sulfide electrolyte, wherein the negative electrode active material comprises one or more of natural graphite, artificial graphite, mesophase micro carbon spheres, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, and metal oxides.
[0025] In a second aspect, this disclosure provides a battery device comprising a plurality of solid-state battery cells as described in the first aspect.
[0026] Thirdly, this disclosure provides an electrical device that includes a solid-state battery cell (as described in the first aspect) or a battery device (as described in the second aspect).
[0027] Fourthly, this disclosure provides a modified sulfide electrolyte, comprising a sulfide electrolyte matrix and a coating layer covering at least a portion of the surface of the sulfide electrolyte matrix; the sulfide electrolyte matrix and the coating layer are connected by Si-OS covalent bonds; the coating layer comprises silane and / or fluorosilane.
[0028] The modified sulfide electrolyte provided in this embodiment includes a sulfide electrolyte matrix and a coating layer covering the sulfide electrolyte matrix. The sulfide electrolyte matrix and the coating layer are connected by Si-OS covalent bonds, thereby allowing the SiO2 on the surface of the sulfide electrolyte to be coated.2- The S atoms are converted into stable S atoms in the Si-OS covalent bond. This allows them to occupy active sites on the surface of the sulfide electrolyte matrix, reducing side reactions between the sulfide electrolyte matrix and air. The coating layer of the modified sulfide electrolyte provided in this disclosure includes silane and / or fluorosilane, thus exhibiting good hydrophobicity. By coating at least a portion of the surface of the sulfide electrolyte matrix, the coating layer reduces the contact between the sulfide electrolyte matrix and air, particularly reducing the contact between the sulfide electrolyte matrix and water vapor in the air, thereby further reducing side reactions between the sulfide electrolyte matrix and air. This effectively improves the stability of the sulfide electrolyte matrix in air, allowing it to maintain good ion transport performance. Furthermore, when the modified sulfide electrolyte of this disclosure is applied to a solid-state battery cell, it can effectively improve the interfacial performance between the electrolyte and the positive / negative electrode active materials, reduce the impedance of the solid-state battery cell, and improve the cycle performance of the solid-state battery cell.
[0029] Furthermore, the modified sulfide electrolyte of this disclosure has high stability in air and is not prone to side reactions with air. It can also reduce the environmental requirements during the preparation of solid-state battery cells, improve the production efficiency of solid-state battery cells, and reduce the preparation cost of solid-state battery cells.
[0030] In some embodiments, the covering layer includes one or more of the structures shown in Formula 1.
[0031] R n SiY 4-n Formula 1
[0032] In Formula 1, n is 1, 2, or 3; R independently represents C1-C10 alkyl groups or C1-C10 alkyl groups substituted with F atoms. Optionally, at least one R represents a C1-C10 alkyl group substituted with F atoms. Y represents -OS-#, and the O atom in Y is connected to the Si atom in Formula 1, and # represents the connection position between the structure shown in Formula 1 and the sulfide electrolyte matrix.
[0033] The structure shown in Formula 1 consists of Si-OH and S on the surface of the sulfide electrolyte matrix. 2- The reaction occurs, thereby consuming the side reaction active sites on the surface of the sulfide electrolyte matrix. This helps reduce side reactions between the sulfide electrolyte matrix and air. Furthermore, the structure shown in Formula 1 has high hydrophobicity, which helps reduce the contact between the sulfide electrolyte matrix and water vapor in the air, further reducing side reactions between the sulfide electrolyte matrix and air. Thus, the sulfide electrolyte matrix can maintain good ion transport performance, thereby improving the cycle performance of solid-state battery cells.
[0034] In some embodiments, R independently represents CF3(CF2)7CH2CH2-, CF3(CF2)5CH2CH2-, or CF3CH2CH2-.
[0035] In some embodiments, the coating layer further includes LiF.
[0036] The F atoms in R can react with lithium-containing impurities (e.g., lithium metal, or other lithium-containing materials) on the surface of the sulfide electrolyte matrix to generate LiF. LiF has extremely low solubility in water and exhibits excellent hydrophobic properties. Including LiF in the coating layer further enhances its hydrophobicity, reducing contact between the sulfide electrolyte matrix and water vapor in the air, thereby further reducing side reactions between the sulfide electrolyte matrix and air. Furthermore, LiF can improve the ion transport performance of the coating layer, thereby increasing the ionic conductivity of the modified sulfide electrolyte. This, in turn, is beneficial for improving the cycle performance of solid-state battery cells.
[0037] In some embodiments, the carbon (C) content in the coating layer is 0.3% to 1% based on the total mass of the modified sulfide electrolyte (100%). An appropriate amount of phosphorus (F) can better enhance the hydrophobicity of the coating layer, thereby reducing side reactions between the sulfide electrolyte matrix and air. This improves the interfacial properties between the modified sulfide electrolyte and the positive and / or negative electrode active materials, thus improving the cycle performance of the solid-state battery cell.
[0038] In some embodiments, the F element content in the coating layer is 0.3% to 1% based on the total mass of the modified sulfide electrolyte (100%). This allows the coating layer to have lower polarity, thereby enhancing its hydrophobicity. This, in turn, helps reduce the contact between the sulfide electrolyte matrix and water vapor in the air, further reducing side reactions between the sulfide electrolyte matrix and air.
[0039] In some embodiments, the coating layer includes carbon (C) and sulfur (F) elements, with the mass ratio of C to F elements in the coating layer being (0.3:1) to (0.7:1). This allows the coating layer to possess both good hydrophobicity and good flexibility.
[0040] Fifthly, this disclosure provides a method for modifying a sulfide electrolyte, comprising the following steps: providing a sulfide electrolyte matrix and a coating layer precursor gas; contacting the coating layer precursor gas with the sulfide electrolyte matrix to form a coating layer on at least a portion of the surface of the sulfide electrolyte matrix, thereby obtaining a modified sulfide electrolyte, wherein the coating layer precursor includes a silane containing Si-OH and / or a fluorosilane containing Si-OH, the modified sulfide electrolyte includes a sulfide electrolyte matrix and a coating layer covering at least a portion of the surface of the sulfide electrolyte matrix; the sulfide electrolyte and the coating layer are connected by Si-OS covalent bonds, and the coating layer includes a silane and / or a fluorosilane.
[0041] The preparation method provided in this disclosure involves contacting a coating layer precursor gas with a sulfide electrolyte matrix. Through the reaction between the coating layer precursor and the sulfide electrolyte matrix, a coating layer is formed on the surface of the sulfide electrolyte matrix. This allows for a relatively thin coating layer on the surface of the sulfide electrolyte matrix, resulting in modified sulfide electrolytes exhibiting good ion transport properties.
[0042] The modified sulfide electrolyte prepared according to the embodiments of this disclosure includes a sulfide electrolyte matrix and a coating layer covering the sulfide electrolyte matrix. The sulfide electrolyte matrix and the coating layer are connected by Si-OS covalent bonds. When applied to solid-state battery cells, it can effectively improve the interfacial performance between the electrolyte and the positive / negative electrode active materials, reduce the impedance of the solid-state battery cells, and improve the cycle performance of the solid-state battery cells.
[0043] In some embodiments, the step of providing the coating layer precursor gas includes the following steps:
[0044] Provide the compound shown in Formula 2, and hydrolyze the compound shown in Formula 2 to release Si-OH to obtain the coating layer precursor, wherein the coating layer precursor includes a silane containing Si-OH and / or a fluorosilane containing Si-OH.
[0045] R n SiX 4-n Formula 2
[0046] Where n is 1, 2 or 3;
[0047] R independently represents a C1-C10 alkyl group or a C1-C10 alkyl group substituted with an F atom. Optionally, at least one R represents a C1-C10 alkyl group substituted with an F atom; X independently represents an alkoxy group, an F-substituted alkoxy group, an aryloxy group, an acyloxy group, or a chloro group.
[0048] The coating precursor is heated to obtain the coating precursor gas.
[0049] By heating the coating precursor, a coating precursor gas is obtained. This gas is then brought into contact with the sulfide electrolyte matrix, thereby forming a coating layer on at least a portion of the surface of the sulfide electrolyte matrix, resulting in a modified sulfide electrolyte. This allows for flexible adjustment of the coating layer thickness by controlling the reaction time, ensuring a uniform and dense coating layer. Consequently, it effectively isolates the sulfide electrolyte matrix from air, reducing side reactions between the sulfide electrolyte matrix and air.
[0050] In some embodiments, the compound shown in Formula 2 includes one or more of tridecafluorooctyltriethoxysilane, tridecafluorooctyltrimethoxysilane, heptadecafluorodecyltrimethoxysilane, heptadecafluorodecyltriethoxysilane, trifluoropropyltrimethoxysilane, and trifluoropropyltriethoxysilane. The above substances have suitable C and F element contents, which can adjust the mass content of C and F elements in the coating layer, making the coating layer possess both good hydrophobicity and good flexibility.
[0051] In some embodiments, the heating temperature is 80°C to 140°C. This can improve the safety of the preparation process and also allow the sulfide electrolyte matrix to maintain good ionic conductivity. Attached Figure Description
[0052] To more clearly illustrate the technical solutions of the embodiments of this disclosure, the accompanying drawings used in the embodiments of this disclosure will be briefly described below. Obviously, the drawings described below are merely some embodiments of this disclosure. For those skilled in the art, other drawings can be obtained based on the drawings without any creative effort.
[0053] Figure 1 A schematic diagram of a solid-state battery cell provided in some embodiments of this disclosure is shown.
[0054] Figure 2 A schematic diagram of an electrical device provided in some embodiments of this disclosure is shown.
[0055] Figure 3 A schematic diagram is shown illustrating the reaction of the compound of Formula 2 provided in some embodiments of this disclosure with a sulfide electrolyte matrix.
[0056] The accompanying drawings are not necessarily drawn to scale. Detailed Implementation
[0057] The following detailed description, with appropriate reference to the accompanying drawings, provides specific embodiments of the solid-state battery cell, battery device, power-consuming device, modified sulfide electrolyte, and methods for preparing the present disclosure. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand the present disclosure and are not intended to limit the subject matter of the claims.
[0058] The "range" disclosed in this disclosure is defined by a lower limit and an upper limit, whereby a given range is defined by selecting a lower limit and an upper limit, which define the boundaries of the particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also expected. Furthermore, if minimum range values 1 and 2 are listed, and if maximum range values 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this disclosure, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0059] Unless otherwise specified, all embodiments and optional embodiments of this disclosure may be combined with each other to form new technical solutions, and such technical solutions should be considered as included in the disclosure of this disclosure.
[0060] Unless otherwise specified, all technical features and optional technical features of this disclosure can be combined to form new technical solutions, and such technical solutions should be considered as included in the disclosure of this disclosure.
[0061] Unless otherwise specified, all steps in this disclosure may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order; for example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0062] Unless otherwise specified, in this disclosure, the terms "first," "second," etc., are used to distinguish different objects, rather than to describe a specific order or primary / secondary relationship.
[0063] In this disclosure, substituents of compounds are disclosed by groups or ranges. It is expressly intended that such a description include each individual sub-combination of members of these ranges. For example, it is expressly intended that the term "C1-C10 alkyl" individually discloses C1, C2, C3, C4, C5, C6, C7, C9, C10, C1-C2, C1-C3, C1-C4, C1-C5, C1-C6, C1-C7, C1-C8, C1-C9, C1-C10, C2-C3, C2-C4, C2-C5, C2-C6, C2-C7, C2-C8, C2-C9, C2-C10, C3-C4, C3-C 5. C3–C6, C3–C7, C3–C8, C3–C9, C3–C10, C4–C5, C4–C6, C4–C7, C4–C8, C4–C9, C4–C10, C5–C6, C5–C7, C5–C8, C5–C9, C5–C10, C6–C7, C6–C8, C6–C9, C6–C10, C7–C8, C7–C9, C7–C10, C8–C9, C8–C10, and C9–C10 alkyl groups. Unless otherwise stated, the term "alkyl" encompasses both straight-chain alkyl and branched-chain alkyl groups.
[0064] In this disclosure, "F-atom substitution" can mean that the H atom on the substituent is partially or completely replaced by an F atom. For example, the term "F-atom-substituted C1-C10 alkyl" is explicitly intended to separately disclose the group obtained by partially or completely replacing the H atom in the aforementioned "C1-C10 alkyl" with an F atom. As an example, "F-atom-substituted methyl" can include -CH2F, -CHF2, and -CF3.
[0065] In this disclosure, the terms "multiple" or "a variety" refer to two or more kinds.
[0066] In the description of the embodiments of this disclosure, unless otherwise specified, "above" or "below" the second feature can mean that the first feature is in direct contact with the second feature, or that the first feature is in indirect contact with the second feature through an intermediate medium. Furthermore, "above," "over," and "on top" of the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.
[0067] Unless otherwise stated, the test temperature for all parameters mentioned in this disclosure is 25°C.
[0068] The solid-state battery cells mentioned in the embodiments of this disclosure can independently perform charging and discharging functions. Solid-state battery cells can be cylindrical, cuboid, or other shapes, etc., and the embodiments of this disclosure are not limited in this respect. Figure 1 This is an example of a rectangular solid-state battery cell 5.
[0069] The battery apparatus mentioned in the embodiments of this disclosure may include one or more battery cell assemblies for providing voltage and capacity. The battery cell assembly may include multiple solid-state battery cells, which are connected in series, parallel, or mixed connections via busbars.
[0070] In some embodiments, a battery cell assembly is typically formed by arranging multiple solid-state battery cells.
[0071] As an example, a battery cell assembly can be a battery module, which is formed by arranging and fixing multiple solid-state battery cells together to form an independent module. As another example, a battery module can be formed by bundling multiple solid-state battery cells together with cable ties.
[0072] In some embodiments, the battery device may be a battery pack, which includes a housing and one or more individual battery cells housed within the housing.
[0073] As an example, the battery cell assembly can be a battery module, which can be housed in a housing by fixing the battery module in the housing.
[0074] As an example, battery cell assemblies can also be housed in a housing by directly fixing multiple solid-state battery cells to the housing.
[0075] As an example, the enclosure may include a first enclosure and a second enclosure. The first enclosure and the second enclosure are fastened together to form a closed space inside the enclosure to house the individual battery cells. Here, "closed" refers to covering or closing, and can be either sealed or unsealed. The first enclosure may be a top cover or a bottom plate.
[0076] As an example, the enclosure may include a top cover, a frame, and a bottom plate. The top cover and bottom plate are connected to the frame, creating an enclosed space inside the enclosure to house the individual battery cells.
[0077] In some embodiments, the housing may be part of the vehicle's chassis structure. For example, a portion of the housing may be at least a part of the vehicle's floor, or a portion of the housing may be at least a part of the vehicle's crossbeams and longitudinal beams.
[0078] The technical solutions described in this disclosure are applicable to various electrical devices that use solid-state battery cells or battery devices, such as, but not limited to, mobile devices (e.g., mobile phones, tablets, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc. Solid-state battery cells and battery devices are used to store or provide electrical energy.
[0079] Figure 2 This is a schematic diagram of an example electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc.
[0080] The solid-state battery cells disclosed herein may include coin cells, molded cells, hard-case cells, pouch cells, etc.
[0081] In view of the problems mentioned in the background art, the present disclosure provides a modified sulfide electrolyte and a method for preparing the same, as well as a solid-state battery cell, a battery device and an electrical device containing the same, wherein the solid-state battery cell using the modified sulfide electrolyte has good cycle performance.
[0082] The modified sulfide electrolyte provided in this disclosure includes a sulfide electrolyte matrix and a coating layer covering at least a portion of the surface of the sulfide electrolyte matrix. The sulfide electrolyte matrix and the coating layer are connected by Si-OS covalent bonds. The coating layer includes silanes and / or fluorosilanes.
[0083] The modified sulfide electrolyte provided in this embodiment includes a sulfide electrolyte matrix and a coating layer covering the sulfide electrolyte matrix. The sulfide electrolyte matrix and the coating layer are connected by Si-OS covalent bonds, thereby allowing the SiO2 on the surface of the sulfide electrolyte to be coated. 2-The S atoms are converted into stable S atoms in the Si-OS covalent bond. This allows them to occupy active sites on the surface of the sulfide electrolyte matrix, reducing side reactions between the sulfide electrolyte matrix and air. The coating layer of the modified sulfide electrolyte provided in this disclosure includes silane and / or fluorosilane, thus exhibiting good hydrophobicity. By coating at least a portion of the surface of the sulfide electrolyte matrix, the coating layer reduces the contact between the sulfide electrolyte matrix and air, particularly reducing the contact between the sulfide electrolyte matrix and water vapor in the air, thereby further reducing side reactions between the sulfide electrolyte matrix and air. This effectively improves the stability of the sulfide electrolyte matrix in air, allowing it to maintain good ion transport performance. Furthermore, when the modified sulfide electrolyte of this disclosure is applied to a solid-state battery cell, it can effectively improve the interfacial performance between the electrolyte and the positive / negative electrode active materials, reduce the impedance of the solid-state battery cell, and improve the cycle performance of the solid-state battery cell.
[0084] Furthermore, the modified sulfide electrolyte of this disclosure has high stability in air and is not prone to side reactions with air. It can also reduce the environmental requirements during the preparation of solid-state battery cells, improve the production efficiency of solid-state battery cells, and reduce the preparation cost of solid-state battery cells.
[0085] Si-OS covalent bonds can be determined using X-ray photoelectron spectroscopy (XPS).
[0086] This disclosure does not limit the type of sulfide electrolyte matrix. In some embodiments, the sulfide electrolyte matrix may include sulfide electrolytes commonly used in the art.
[0087] Optionally, the sulfide electrolyte may include Li 6+m+l P 1-m M m S 5-n+l N n Y 1-l The material, with the molecular formula Li 10±δ Ge 1-g G g P 2-q Q q S 12-w W w Materials, Li 4-v Ge 1-v P vS4, one or more of Li2S-P2S5-based materials, Li2S-SiS2-based materials, Li2S-MeS-P2S5-based materials, and LiGeGaS-based materials, 0≤m<1, 0≤n<1, -1<l<1, M includes one or more elements selected from Ge, Si, Sn, Al, Zr and Sb, N includes one or more elements selected from O, Se and Te, Y includes one or more elements selected from Cl, Br and I, 0≤δ<1, 0≤g≤1, 0≤q≤2, 0≤w<1, G includes one or two elements selected from Si and Sn, Q includes Sb, W includes one or more elements selected from O, Se, Te, Cl, Br and I, 0<v<1, Me includes one or more elements selected from Si, Ge, Sn and Al. By way of example, the sulfide electrolyte may include Li6PS5Cl, Li6PS5Br, Li6PS5I, Li6PS5Cl 0.5 Br 0.5 , Li 5.5 PS 4.5 Cl 1.5 , Li 5.5 PS 4.5 Br 1.5 , Li 10 GeP2S 12 , Li3PS4, Li7P3S 11 , Li 3.25 Ge 0.25 P 0.75 S4, one or more of Li6GaGe2S 10 .
[0088] In some embodiments, the coating layer may include one or more of the structures represented by Formula 1.
[0089] R n SiY 4-n Formula 1
[0090] In Formula 1, n is 1, 2 or 3.
[0091] Each R independently represents a C1-C10 alkyl group, or a C1-C10 alkyl group substituted by a fluorine atom. Optionally, at least one R represents a C1-C10 alkyl group substituted by a fluorine atom.
[0092] Optionally, in some embodiments, n is 1 or 2, and at least one R represents a C1-C10 alkyl group substituted by a fluorine atom.
[0093] Optionally, in some embodiments, n is 1 or 2, and at least one R represents a C3-C10 alkyl group substituted by a fluorine atom. This can enable the coating layer to have both good hydrophobicity and good flexibility.
[0094] Y represents -OS-#, and the O atom in Y is connected to the Si atom in Formula 1. # represents the connection position between the structure shown in Formula 1 and the sulfide electrolyte matrix.
[0095] It is understandable that the structure shown in Equation 1 can be formed by Si-OH reacting with S on the surface of the sulfide electrolyte matrix. 2- The reaction yields a structure that can consume side-reactive sites on the surface of the sulfide electrolyte matrix. This helps reduce side reactions between the sulfide electrolyte matrix and air. Furthermore, the structure shown in Formula 1 exhibits high hydrophobicity, which helps reduce contact between the sulfide electrolyte matrix and water vapor in the air, thereby further reducing side reactions between the sulfide electrolyte matrix and air. Thus, the sulfide electrolyte matrix can maintain good ion transport performance, which is beneficial for improving the cycle performance of solid-state battery cells.
[0096] Optionally, in Formula 1, n is 1, and R represents a C1 to C10 alkyl group substituted with an F atom.
[0097] Optionally, n is 1, and R represents a C3 to C10 alkyl group substituted with an F atom.
[0098] In some embodiments, in Equation 1, R can independently represent CF3(CF2)7CH2CH2-, CF3(CF2)5CH2CH2-, or CF3CH2CH2-.
[0099] In some embodiments, the coating layer may further include LiF.
[0100] Due to limitations in the manufacturing process, lithium-containing impurities (e.g., lithium metal, or other lithium-containing raw materials) inevitably remain in the sulfide electrolyte matrix. In the coating layer of the modified sulfide electrolyte of this disclosure embodiment, the F atoms in the aforementioned R group can react with the lithium-containing impurities on the surface of the sulfide electrolyte matrix to generate LiF. LiF has extremely low solubility in water and exhibits excellent hydrophobic properties. The inclusion of LiF in the coating layer further enhances its hydrophobicity, which helps reduce the contact between the sulfide electrolyte matrix and water vapor in the air, thereby further reducing side reactions between the sulfide electrolyte matrix and air. In addition, LiF can also improve the ion transport performance of the coating layer, thereby increasing the ionic conductivity of the modified sulfide electrolyte. This is beneficial for improving the cycle performance of solid-state battery cells.
[0101] LiF in the coating layer can be determined by XPS.
[0102] In some embodiments, based on the total mass of the modified sulfide electrolyte, the mass content of F element in the coating layer can be 0.3% to 1%, for example, it can be 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, or any range of the above values.
[0103] An appropriate amount of sulfur (F) can better enhance the hydrophobicity of the coating layer, thereby reducing the contact between the sulfide electrolyte matrix and water vapor in the air, and reducing side reactions between the sulfide electrolyte matrix and air. This can improve the interfacial properties between the modified sulfide electrolyte and the positive and / or negative electrode active materials, thus improving the cycle performance of the solid-state battery cell.
[0104] In some embodiments, the coating layer includes element C. The mass content of element C in the coating layer can be 0.3% to 1% based on the total mass of the modified sulfide electrolyte of 100%, for example, it can be 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, or any range of the above values.
[0105] When the carbon content in the coating layer is within the aforementioned suitable range, the coating layer exhibits lower polarity, thereby enhancing its hydrophobicity. This helps reduce the contact between the sulfide electrolyte matrix and water vapor in the air, further reducing side reactions between the sulfide electrolyte matrix and air.
[0106] The mass content of F and C elements in the coating layer can be obtained by elemental analysis.
[0107] In some embodiments, the mass ratio of C element to F element in the coating layer can be (0.3:1) to (0.7:1), for example, it can be 0.3:1, 0.32:1, 0.35:1, 0.37:1, 0.4:1, 0.45:1, 0.5:1, 0.55:1, 0.6:1, 0.65:1, 0.7:1, or any range of the above ratios.
[0108] When the mass ratio of carbon (C) to phosphorus (F) is within the aforementioned suitable range, the coating layer exhibits both good hydrophobicity and flexibility. This benefits the coating layer by reducing contact between the sulfide electrolyte matrix and water vapor in the air, thereby further minimizing side reactions between the sulfide electrolyte matrix and air. Furthermore, it allows for closer contact between the modified sulfide electrolyte and the positive and / or negative electrode active material particles, forming a larger effective contact area. This helps reduce interfacial impedance and improve lithium-ion transport efficiency. Consequently, the cycle performance of solid-state battery cells can be further enhanced.
[0109] In some embodiments, the thickness of the coating layer can be 2nm to 10nm, for example, it can be 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, or any range of the above values.
[0110] An appropriate coating thickness can effectively isolate the sulfide electrolyte matrix from air, thereby enabling the modified sulfide electrolyte to have lower impedance and thus improving the kinetic performance of solid-state battery cells.
[0111] The thickness of the coating layer can be measured using methods and equipment known in the art. For example, it can be measured using transmission electron microscopy (TEM). As an example, the thickness of the coating layer can be measured by the following steps: first, turning on the transmission electron microscope, measuring the thickness of the sample coating layer, testing the thickness at five points, and taking the average value as the thickness of the coating layer.
[0112] In some embodiments, the coating area ratio of the modified sulfide electrolyte can be 90% or more, for example, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%, or any range of the above values. When the coating area ratio of the modified sulfide electrolyte is within the above-mentioned suitable range, it can effectively isolate the sulfide electrolyte matrix from air, thereby reducing side reactions between the sulfide electrolyte matrix and air, allowing the sulfide electrolyte matrix to maintain a high ionic conductivity, and thus improving the cycle performance of the solid-state battery cell.
[0113] In some embodiments, the coating area ratio of the modified sulfide electrolyte can be 100%.
[0114] In some embodiments, the volume distribution particle size Dv50 of the modified sulfide electrolyte can be 1 μm to 10 μm, for example, it can be 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, or any range of the above values.
[0115] Appropriate particle size can improve the ion transport performance of the positive and / or negative electrodes, thereby improving the cycle performance of solid-state battery cells.
[0116] Dv50 represents the particle size corresponding to a cumulative volumetric distribution percentage of 50% for the material. It can be measured using a laser particle size analyzer, referring to GB / T19077-2016. During testing, add 1g of the sample to a clean small beaker and 20ml of deionized water. Sonicate at 53kHz / 120W for 5 minutes to ensure complete dispersion. Turn on the laser particle size analyzer, clean the optical path system, and automatically test the background. Stir the sonicated solution to ensure uniform dispersion, place it in the sample cell as required, and begin measuring the particle size. A MasterSizer 3000 laser particle size analyzer can be used as the testing instrument.
[0117] In some embodiments, the ionic conductivity of the modified sulfide electrolyte can be 1 × 10⁻⁶. -3 S / cm~8×10 - 3 S / cm, for example, can be 1×10 -3 S / cm, 2×10 -3 S / cm, 3×10 -3 S / cm, 4×10 -3 S / cm, 5×10 -3 S / cm, 6×10 -3 S / cm, 7×10 -3 S / cm, 8×10 -3 S / cm, or any range of the above values.
[0118] In modified sulfide electrolytes, the coating layer can occupy the active sites on the surface of the sulfide electrolyte matrix and effectively reduce the contact between the sulfide electrolyte matrix and air, thereby reducing the risk of side reactions between the sulfide electrolyte matrix and air, and thus allowing the sulfide electrolyte matrix to maintain good ion transport performance. Therefore, modified sulfide electrolytes can possess the aforementioned ionic conductivity. When applied to solid-state battery cells, they can effectively improve the interfacial performance between the electrolyte and the positive / negative electrode active materials, reduce the impedance of solid-state battery cells, and improve the cycle performance of solid-state battery cells.
[0119] Ionic conductivity can be measured using an impedance analyzer. The test temperature is 25℃.
[0120] This disclosure also provides a method for preparing a modified sulfide electrolyte.
[0121] The preparation method of modified sulfide electrolyte includes the following steps:
[0122] A sulfide electrolyte matrix and a coating layer precursor gas are provided; the coating layer precursor gas is contacted with the sulfide electrolyte matrix to form a coating layer on at least a portion of the surface of the sulfide electrolyte matrix, thereby obtaining a modified sulfide electrolyte. The coating layer precursor includes a silane containing Si-OH and / or a fluorosilane containing Si-OH. The modified sulfide electrolyte includes the sulfide electrolyte matrix and a coating layer covering at least a portion of the surface of the sulfide electrolyte matrix. The sulfide electrolyte and the coating layer are connected by Si-OS covalent bonds, and the coating layer includes a silane and / or a fluorosilane.
[0123] In the method disclosed herein, the coating step can be implemented in various ways. For example, the coating precursor and the sulfide electrolyte are placed in the same chamber, and the coating precursor is heated to vaporize and obtain a coating precursor gas. After the coating precursor gas comes into contact with the sulfide electrolyte matrix, it can react with Si-OH groups on the surface of the sulfide electrolyte matrix. 2- A reaction occurs, forming Si-OS covalent bonds, which then connect with the sulfide electrolyte matrix and deposit on the surface of the sulfide electrolyte matrix to form the aforementioned coating layer. Alternatively, atomic layer deposition (ALD) technology can be used, placing the sulfide electrolyte in a reaction chamber and introducing a coating layer precursor gas to deposit the coating layer precursor layer by layer on the surface of the sulfide electrolyte matrix. After the coating layer precursor comes into contact with the sulfide electrolyte matrix, Si-OH bonds can react with the S bonds on the surface of the sulfide electrolyte matrix. 2- A reaction occurs, thereby connecting the coating layer to the sulfide electrolyte matrix through Si-OS covalent bonds.
[0124] The preparation method provided in this disclosure involves contacting a coating layer precursor gas with a sulfide electrolyte matrix. Through the reaction between the coating layer precursor and the sulfide electrolyte matrix, a coating layer is formed on the surface of the sulfide electrolyte matrix. This allows for a relatively thin coating layer on the surface of the sulfide electrolyte matrix, resulting in modified sulfide electrolytes exhibiting good ion transport properties.
[0125] The modified sulfide electrolyte prepared in this embodiment includes a sulfide electrolyte matrix and a coating layer covering the sulfide electrolyte matrix. The sulfide electrolyte matrix and the coating layer are connected by Si-OS covalent bonds, thereby allowing the S on the surface of the sulfide electrolyte to be coated. 2-The S atoms are converted into stable S atoms in the Si-OS covalent bond. This allows them to occupy active sites on the surface of the sulfide electrolyte matrix, reducing side reactions between the sulfide electrolyte matrix and air. The method provided in this disclosure prepares a modified sulfide electrolyte with a coating layer comprising silane and / or fluorosilane, thereby exhibiting good hydrophobicity. By coating at least a portion of the surface of the sulfide electrolyte matrix, the coating layer reduces the contact between the sulfide electrolyte matrix and air, particularly reducing the contact between the sulfide electrolyte matrix and water vapor in the air, thereby further reducing side reactions between the sulfide electrolyte matrix and air. This effectively improves the stability of the sulfide electrolyte matrix in air, allowing it to maintain good ion transport performance. Furthermore, the modified sulfide electrolyte prepared in this disclosure, when applied to a solid-state battery cell, can effectively improve the interfacial performance between the electrolyte and the positive / negative electrode active materials, reduce the impedance of the solid-state battery cell, and improve the cycle performance of the solid-state battery cell.
[0126] Furthermore, the modified sulfide electrolyte prepared in this embodiment has high stability in air and is not prone to side reactions with air. It can also reduce the environmental requirements during the preparation of solid-state battery cells, improve the production efficiency of solid-state battery cells, and reduce the preparation cost of solid-state battery cells.
[0127] In some embodiments, the step of providing the coating layer precursor gas may include the following steps:
[0128] Provide the compound shown in Formula 2, and hydrolyze the compound shown in Formula 2 to release Si-OH to obtain a coating layer precursor, the coating layer precursor including a silane containing Si-OH and / or a fluorosilane containing Si-OH.
[0129] R n SiX 4-n Formula 2
[0130] Where n is 1, 2 or 3.
[0131] R independently represents C1-C10 alkyl groups or C1-C10 alkyl groups substituted with an F atom. Optionally, at least one R represents a C1-C10 alkyl group substituted with an F atom. Optionally, in some embodiments, n is 1 or 2, and at least one R represents a C1-C10 alkyl group substituted with an F atom. Optionally, in some embodiments, n is 1 or 2, and at least one R represents a C3-C10 alkyl group substituted with an F atom.
[0132] X independently represents an alkoxy group, an alkoxy group substituted with an F atom, an aryloxy group, an acyloxy group, or a chlorine group.
[0133] The coating precursor is heated to obtain the coating precursor gas.
[0134] Optionally, in Formula 2, n is 1, R represents a C1 to C10 alkyl group substituted with an F atom, and X independently represents an alkoxy group.
[0135] Optionally, in Formula 2, n is 1, R represents a C3 to C10 alkyl group substituted with an F atom, and X independently represents an alkoxy group.
[0136] It is understandable that after the compound shown in Formula 2 is prepared, it will inevitably come into contact with water vapor in the air and hydrolyze to release Si-OH during storage, thus obtaining the above-mentioned coating layer precursor. In some embodiments, the compound shown in Formula 2 can also be contacted with an appropriate amount of water or water vapor to hydrolyze to release Si-OH, and then the water in the hydrolysis product can be further removed to obtain the above-mentioned coating layer precursor.
[0137] In the compound shown in Formula 2, X is an alkoxy group, an alkoxy group substituted with an F atom, an aryloxy group, an acyloxy group, or a chlorine group, which can be hydrolyzed to produce Si-OH.
[0138] The coating precursor contains Si-OH, which can react with S on the surface of the sulfide electrolyte matrix. 2- A reaction occurs, forming Si-OS covalent bonds, which consumes the side reactive sites on the surface of the sulfide electrolyte matrix. As an example, in Equation 2, n can be 3. Figure 3 As shown, the compound R3SiX represented by Formula 2 can react with the sulfide electrolyte matrix 10, thereby attaching to the surface of the sulfide electrolyte matrix 10 via Si-OS covalent bonds. This helps to reduce side reactions between the sulfide electrolyte matrix and air.
[0139] Furthermore, the compound shown in Formula 2 exhibits high hydrophobicity, which helps reduce the contact between the sulfide electrolyte matrix and water vapor in the air, thereby further reducing side reactions between the sulfide electrolyte matrix and the air. This allows the sulfide electrolyte matrix to maintain good ion transport performance, thus improving the cycle performance of solid-state battery cells.
[0140] In the above embodiments, the heating temperature can be adjusted according to the pressure of the reaction environment and the properties of the coating layer precursor, as long as the coating layer precursor can be vaporized, and is not limited here. The reaction time between the coating layer precursor and the sulfide electrolyte matrix can be adjusted according to factors such as the properties of the coating layer precursor, the type of sulfide electrolyte matrix, and the target thickness of the coating layer, and is not limited here.
[0141] This disclosure does not limit the reaction apparatus for the reaction of the coating precursor with the sulfide electrolyte matrix. As an example, the sulfide electrolyte matrix can be placed on a perforated partition on the upper layer of a vacuum heating device, and the coating precursor can be placed on the bottom layer of the vacuum heating device. The heating temperature of the apparatus is set according to the temperature required for the vaporization of the coating precursor, and the modified sulfide electrolyte is obtained by adjusting the vaporization time.
[0142] The method described in the above embodiment is simple to operate. A coating precursor gas is obtained by heating the coating precursor; this gas is then brought into contact with the sulfide electrolyte matrix, thereby forming a coating layer on at least a portion of the surface of the sulfide electrolyte matrix, resulting in a modified sulfide electrolyte. This allows for flexible adjustment of the coating layer thickness by controlling the reaction time, ensuring a uniform and dense coating layer. Consequently, it effectively isolates the sulfide electrolyte matrix from air, reducing side reactions between the sulfide electrolyte matrix and air.
[0143] In some embodiments, the heating temperature can be 80°C to 140°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 130°C, 140°C, or any range of the above values.
[0144] The heating temperature mentioned above can be a temperature that matches the Si-OH-containing fluorosilane or Si-OH-containing silane and the pressure of the reaction system.
[0145] Heating within the aforementioned suitable range can improve the safety of the preparation process and also allow the sulfide electrolyte matrix to maintain good ionic conductivity.
[0146] In some embodiments, the compound shown in Formula 2 may include one or more of trimethylmethoxysilane, triethylmethoxysilane, and trimethylethoxysilane.
[0147] In some embodiments, the compound shown in Formula 2 may include one or more of the following: tridecylfluorooctyltriethoxysilane CF3(CF2)5(CH2)2Si(OC2H5)3, tridecylfluorooctyltrimethoxysilane CF3(CF2)5(CH2)2Si(OCH3)3, heptadecafluorodecyltrimethoxysilane CF3(CF2)7CH2CH2Si(OCH3)3, heptadecafluorodecyltriethoxysilane CF3(CF2)7CH2CH2Si(OC2H5)3, trifluoropropyltrimethoxysilane CF3CH2CH2Si(OCH3)3, and trifluoropropyltriethoxysilane CF3CH2CH2Si(OC2H5)3.
[0148] The aforementioned substances possess suitable vaporization temperatures, which enhances the safety of the preparation process and facilitates the large-scale preparation and production of modified sulfide electrolytes. Furthermore, these substances have appropriate C and F content, allowing for adjustment of the C and F mass content in the coating layer, resulting in a coating layer with both good hydrophobicity and flexibility. This, on the one hand, helps reduce the contact between the sulfide electrolyte matrix and water vapor in the air, thereby further reducing side reactions between the sulfide electrolyte matrix and air; on the other hand, it allows for closer contact between the modified sulfide electrolyte and the positive and / or negative electrode active material particles, forming a larger effective contact area, thus helping to reduce interfacial impedance and improve lithium-ion transport efficiency. This further improves the cycle performance of solid-state battery cells. Additionally, the LiF generated by the reaction of an appropriate amount of F with lithium-containing impurities (e.g., lithium metal, or other lithium-containing raw materials) can better enhance the hydrophobicity of the coating layer, thereby further reducing the contact between the sulfide electrolyte matrix and water vapor in the air and minimizing side reactions between the sulfide electrolyte matrix and air.
[0149] The solid-state battery cell provided in this disclosure includes a positive electrode, an electrolyte layer, and a negative electrode, with the electrolyte layer located between the positive and negative electrodes. At least one of the positive electrode, electrolyte layer, and negative electrode includes the modified sulfide electrolyte provided in this disclosure or a modified sulfide electrolyte prepared by the preparation method of this disclosure.
[0150] [positive electrode]
[0151] The positive electrode includes a positive electrode film, which in turn includes the positive electrode active material and a solid electrolyte.
[0152] In some embodiments, the positive electrode further includes a positive current collector, and the positive electrode film layer is located on at least one surface of the positive current collector. The positive current collector has two surfaces opposite each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive current collector.
[0153] In some embodiments, the positive current collector may be a metal foil or a composite current collector. The metal foil may be a pure metal, an alloy, or a surface-treated metal, such as, but not limited to, stainless steel foil, carbon-coated aluminum foil, or aluminum foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. As an example, the metal layer may include, but is not limited to, one or more of aluminum, aluminum alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. As an example, the polymer substrate may include, but is not limited to, one or more of polypropylene, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene.
[0154] In some embodiments, the positive electrode active material may include one or more of lithium transition metal oxides and modified materials thereof, lithium-containing phosphates and modified materials thereof, lithium titanate, lithium niobate, sulfur, selenium, and tellurium.
[0155] Optionally, examples of the lithium transition metal oxide may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and lithium-rich manganese-based materials.
[0156] Optionally, examples of the lithium-containing phosphate may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, and a composite material of lithium manganese iron phosphate and carbon.
[0157] In some embodiments, to further improve the energy density of the solid-state battery cell, the positive electrode active material may include a lithium transition metal oxide of the general formula Li a Ni b Co c M d O e A f and one or more of modified materials thereof, where 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M may include one or more of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and A may include one or more of N, F, S and Cl. Optionally, 0.6≤b<1, 0.8≤b<1.
[0158] As an example, the positive electrode active material may include, but is not limited to, LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (abbreviated as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (abbreviated as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (abbreviated as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (abbreviated as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (abbreviated as NCM811), LiNi 0.96 Co 0.02Mn 0.02 O2 (abbreviated as Ni96), LiNi 0.80 Co 0.15 Al 0.05 One or more of O2, LiFePO4, LiMnPO4 and their respective modified materials.
[0159] The modified materials for the above-mentioned positive electrode active materials can be doped and / or surface coated.
[0160] During the charging and discharging process, solid-state battery cells undergo Li insertion / extraction and consumption, resulting in varying Li molar content at different discharge states. In this disclosure, the Li molar content listed for positive electrode active materials represents the initial state of the material, i.e., the state before material addition. As the positive electrode active material is applied to a solid-state battery cell, the Li molar content changes after charge-discharge cycles. Similarly, the O molar content listed for positive electrode active materials in this disclosure is only a theoretical value; lattice oxygen release causes changes in the O molar content, leading to fluctuations in the actual O molar content.
[0161] In some embodiments, the positive electrode film layer may further include a positive electrode conductive agent.
[0162] Optionally, the positive electrode conductive agent may be one or more of the following, including but not limited to superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes (CNTs), graphene, carbon nanofibers, and vapor-grown carbon fibers (VGCF).
[0163] In some embodiments, the positive electrode film layer may further include a positive electrode binder.
[0164] Optionally, the positive electrode binder may include, but is not limited to, one or more of the following: polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene-propylene terpolymer, ethylene-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, methyl vinyl silicone rubber, nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), thermoplastic styrene-butadiene rubber (SBS), isoprene rubber, cis-butadiene rubber (BR), ethyl cellulose, fluororubber, and acrylate rubber.
[0165] In some embodiments, the mass percentage of the solid electrolyte in the positive electrode film layer can be 5%-30%, for example, it can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, or any range of the above values.
[0166] In some embodiments, the solid electrolyte in the positive electrode film layer may include one or more of sulfide electrolytes, halide electrolytes, and oxide electrolytes commonly used in the art.
[0167] Optionally, the sulfide electrolyte may include a material with the molecular formula Li 6+m+l P 1-m M m S 5-n+l N n Y 1-l , a material with the molecular formula Li 10±δ Ge 1-g G g P 2-q Q q S 12-w W w , one or more of Li 4-v Ge 1-v P v S4, Li2S-P2S5-based materials, Li2S-SiS2-based materials, Li2S-MeS-P2S5-based materials, and LiGeGaS-based materials, where 0≤m<1, 0≤n<1, -1<l<1, M includes one or more elements selected from Ge, Si, Sn, Al, Zr and Sb, N includes one or more elements selected from O, Se and Te, Y includes one or more elements selected from Cl, Br and I, 0≤δ<1, 0≤g≤1, 0≤q≤2, 0≤w<1, G includes one or two elements selected from Si and Sn, Q includes Sb, W includes one or more elements selected from O, Se, Te, Cl, Br and I, 0<v<1, and Me includes one or more selected from Si, Ge, Sn and Al. As examples, the sulfide electrolyte may include one or more of Li6PS5Cl, Li6PS5Br, Li6PS5I, Li6PS5Cl 0.5 Br 0.5 , Li 5.5 PS 4.5 Cl 1.5 , Li 5.5 PS 4.5 Br 1.5 , Li 10 GeP2S 12 , Li3PS4, Li7P3S 11 , Li 3.25 Ge 0.25 P 0.75 S4, Li6GaGe2S 10 .
[0168] Optionally, the halide electrolyte may be one or more of Li3YCl6, Li3YBr6, Li3ErCl6, Li3InCl6, and Li3InBr6, including but not limited to.
[0169] Optionally, the oxide electrolyte may include one or more of the following: NASICON-type solid-state electrolyte, LISICON-type solid-state electrolyte, perovskite-type solid-state electrolyte, and garnet-type solid-state electrolyte. As an example, the oxide electrolyte may include, but is not limited to, Li5La3Ti2O 12 Li7La3Zr2O 12 Li4Ti5O 12 Li 14 Zn(GeO4)4, LiTi2(PO4)3, Li 1+x Al x Ti 2-x (PO4)3, Li 1+y Al y Ge 2-y One or more of (PO4)3, 0 <x<2,0<y<2。
[0170] In other embodiments, the solid electrolyte in the positive electrode film may include the modified sulfide electrolyte provided in the embodiments of this disclosure.
[0171] The modified sulfide electrolyte provided in this disclosure includes a sulfide electrolyte matrix and a coating layer covering the sulfide electrolyte matrix. The sulfide electrolyte matrix and the coating layer are connected by Si-OS covalent bonds. This reduces the contact between the sulfide electrolyte matrix and air, particularly reducing the contact between the sulfide electrolyte matrix and water vapor in the air, thereby further reducing side reactions between the sulfide electrolyte matrix and air. Thus, the modified sulfide electrolyte of this disclosure exhibits good interfacial properties with the positive electrode active material, which can reduce the impedance of the solid-state battery cell and improve the cycle performance of the solid-state battery cell.
[0172] Furthermore, the modified sulfide electrolyte provided in this disclosure exhibits high stability in air. Therefore, the preparation of the aforementioned positive electrode does not require a specific dry room, significantly improving production efficiency and reducing production costs.
[0173] In some other embodiments, the solid electrolyte in the positive electrode film may include the modified sulfide electrolyte provided in the embodiments of this disclosure and other solid electrolytes, which may include one or more of the sulfide electrolytes, halide electrolytes and oxide electrolytes commonly used in the art.
[0174] [Electrolyte layer]
[0175] The electrolyte layer includes a solid electrolyte.
[0176] In some embodiments, the solid electrolyte in the electrolyte layer may include one or more of a sulfide electrolyte, a halide electrolyte, and an oxide electrolyte commonly used in the art.
[0177] Alternatively, the sulfide electrolyte may include a material with the molecular formula Li 6+m+l P 1-m M m S 5-n+l N n Y 1-l , a material with the molecular formula Li 10±δ Ge 1-g G g P 2-q Q q S 12-w W w , one or more of Li 4-v Ge 1-v P v S4, Li2S-P2S5-based materials, Li2S-SiS2-based materials, Li2S-MeS-P2S5-based materials, and LiGeGaS-based materials, where 0≤m<1, 0≤n<1, -1<l<1, M includes one or more elements selected from Ge, Si, Sn, Al, Zr and Sb, N includes one or more elements selected from O, Se and Te, Y includes one or more elements selected from Cl, Br and I, 0≤δ<1, 0≤g≤1, 0≤q≤2, 0≤w<1, G includes one or two elements selected from Si and Sn, Q includes Sb, W includes one or more elements selected from O, Se, Te, Cl, Br and I, 0<v<1, and Me includes one or more elements selected from Si, Ge, Sn and Al. By way of example, the sulfide electrolyte may include Li6PS5Cl, Li6PS5Br, Li6PS5I, Li6PS5Cl 0.5 Br 0.5 , Li 5.5 PS 4.5 Cl 1.5 , Li 5.5 PS 4.5 Br 1.5 , Li 10 GeP2S 12 , one or more of Li3PS4, Li7P3S 11 , Li 3.25 Ge 0.25 P 0.75 S4, and Li6GaGe2S 10 .
[0178] Optionally, the halide electrolyte may be one or more of Li3YCl6, Li3YBr6, Li3ErCl6, Li3InCl6, and Li3InBr6, including but not limited to.
[0179] Optionally, the oxide electrolyte may include one or more of the following: NASICON-type solid-state electrolyte, LISICON-type solid-state electrolyte, perovskite-type solid-state electrolyte, and garnet-type solid-state electrolyte. As an example, the oxide electrolyte may include, but is not limited to, Li5La3Ti2O 12 Li7La3Zr2O 12 Li4Ti5O 12 Li 14 Zn(GeO4)4, LiTi2(PO4)3, Li 1+x Al x Ti 2-x (PO4)3, Li 1+y Al y Ge 2-y One or more of (PO4)3, 0 <x<2,0<y<2。
[0180] In other embodiments, the solid electrolyte in the electrolyte layer may include the modified sulfide electrolyte provided in the embodiments of this disclosure.
[0181] In some other embodiments, the solid electrolyte in the electrolyte layer may include the modified sulfide electrolyte provided in the embodiments of this disclosure and other solid electrolytes, which may include one or more of the sulfide electrolytes, halide electrolytes and oxide electrolytes commonly used in the art.
[0182] In some embodiments, the electrolyte layer may further include an adhesive. Optionally, the adhesive may include, but is not limited to, one or more of the following: polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, methyl vinyl silicone rubber, nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), thermoplastic styrene-butadiene rubber (SBS), isoprene rubber, cis-butadiene rubber (BR), ethyl cellulose, fluororubber, and acrylate rubber.
[0183] [negative electrode]
[0184] In some embodiments, the negative electrode may include lithium or a lithium alloy.
[0185] For example, the negative electrode can be a metal sheet, such as a lithium sheet or a lithium alloy sheet. Alternatively, the negative electrode can include a negative electrode current collector and a lithium-based metal layer located on at least one surface of the negative electrode current collector. The lithium-based metal layer can be metallic lithium or a lithium alloy. The negative electrode current collector has two surfaces opposite each other in its thickness direction, and the lithium-based metal layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0186] Optionally, other elements in the lithium alloy may include, but are not limited to, one or more of In, Mg, Al, Zn, Sn, Ag, Au, Ga, Pt, and Fe.
[0187] Alternatively, the lithium alloy may include, but is not limited to, InLi alloy, Li-Mg alloy, Li-Al alloy, Li-Zn alloy, Li-Fe alloy, etc.
[0188] In other embodiments, the negative electrode may include a negative electrode current collector and a negative electrode film layer located on at least one surface of the negative electrode current collector, the negative electrode film layer comprising a negative electrode active material. The negative electrode current collector has two surfaces opposite each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0189] Optionally, the negative electrode active material may include one or more of the following: natural graphite, artificial graphite, mesophase micro carbon spheres, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, and metal oxides.
[0190] Optionally, the silicon-based material may include, but is not limited to, one or more of elemental silicon, silicon oxide, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Optionally, the tin-based material may include, but is not limited to, one or more of elemental tin, tin oxide, and tin alloys. Optionally, the metal oxide may include, but is not limited to, one or more of TiO2, MoO2, In2O3, Al2O3, Cu2O, VO2, Ga2O3, Sb2O5, and Bi2O5.
[0191] In some embodiments, the negative electrode film layer may further include a negative electrode binder.
[0192] Optionally, the negative electrode binder may include, but is not limited to, one or more of the following: polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene-propylene terpolymer, ethylene-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, polyacrylic acid, polymethacrylic acid, sodium polyacrylate, polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), carboxymethyl chitosan (CMCS), methyl vinyl silicone rubber, nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), thermoplastic styrene-butadiene rubber (SBS), isoprene rubber, butadiene rubber (BR), ethyl cellulose, fluororubber, and acrylate rubber.
[0193] In some embodiments, the negative electrode film layer may or may not include a negative electrode conductive agent.
[0194] Optionally, the negative electrode conductive agent may be one or more of the following, including but not limited to superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes (CNTs), graphene, carbon nanofibers, and vapor-grown carbon fibers (VGCF).
[0195] In some embodiments, the negative electrode film layer may or may not include a solid electrolyte.
[0196] Optionally, the mass percentage of the solid electrolyte in the negative electrode film can be less than 30%.
[0197] In some embodiments, the negative electrode film layer includes a solid electrolyte, which may include one or more of the commonly used sulfide electrolytes, halide electrolytes, and oxide electrolytes in the art.
[0198] Optionally, the sulfide electrolyte may include Li 6+m+l P 1-m M m S 5-n+l N n Y 1-l The material, with the molecular formula Li 10±δ Ge 1-g G g P 2-q Q q S 12-w W w Materials, Li 4-v Ge 1-v P vS4, one or more of Li2S-P2S5-based materials, Li2S-SiS2-based materials, Li2S-MeS-P2S5-based materials, and LiGeGaS-based materials, 0≤m<1, 0≤n<1, -1<l<1, M includes one or more elements of Ge, Si, Sn, Al, Zr and Sb, N includes one or more elements of O, Se and Te, Y includes one or more elements of Cl, Br and I, 0≤δ<1, 0≤g≤1, 0≤q≤2, 0≤w<1, G includes one or two elements of Si and Sn, Q includes Sb, W includes one or more elements of O, Se, Te, Cl, Br and I, 0<v<1, Me includes one or more of Si, Ge, Sn and Al. By way of example, the sulfide electrolyte may include Li6PS5Cl, Li6PS5Br, Li6PS5I, Li6PS5Cl 0.5 Br 0.5 , Li 5.5 PS 4.5 Cl 1.5 , Li 5.5 PS 4.5 Br 1.5 , Li 10 GeP2S 12 , Li3PS4, Li7P3S 11 , Li 3.25 Ge 0.25 P 0.75 S4, Li6GaGe2S 10 one or more of the above.
[0199] Optionally, the halide electrolyte may include, but is not limited to, one or more of Li3YCl6, Li3YBr6, Li3ErCl6, Li3InCl6, and Li3InBr6.
[0200] Optionally, the oxide electrolyte may include one or more of a NASICON-type solid electrolyte, a LISICON-type solid electrolyte, a perovskite-type solid electrolyte, and a garnet-type solid electrolyte. By way of example, the oxide electrolyte may include, but is not limited to, Li5La3Ti2O 12 , Li7La3Zr2O 12 , Li4Ti5O 12 , Li 14 Zn(GeO4)4, LiTi2(PO4)3, Li 1+x Al x Ti 2-x (PO4)3, Li 1+y Al y Ge 2-yOne or more of (PO4)3, 0 <x<2,0<y<2。
[0201] In other embodiments, the negative electrode film layer includes a solid electrolyte, which may include the modified sulfide electrolyte provided in the embodiments of this disclosure.
[0202] The modified sulfide electrolyte provided in this disclosure includes a sulfide electrolyte matrix and a coating layer covering the sulfide electrolyte matrix. The sulfide electrolyte matrix and the coating layer are connected by Si-OS covalent bonds. This reduces the contact between the sulfide electrolyte matrix and air, particularly reducing the contact between the sulfide electrolyte matrix and water vapor in the air, thereby further reducing side reactions between the sulfide electrolyte matrix and air. Thus, the modified sulfide electrolyte of this disclosure exhibits good interfacial properties with the negative electrode active material, which can reduce the impedance of the solid-state battery cell and improve the cycle performance of the solid-state battery cell.
[0203] Furthermore, the modified sulfide electrolyte provided in this embodiment exhibits high stability in air. Therefore, the preparation of the aforementioned negative electrode does not require a specific dry room, greatly improving production efficiency and reducing production costs.
[0204] In some other embodiments, the negative electrode film layer includes a solid electrolyte, which may include the modified sulfide electrolyte provided in the embodiments of this disclosure and other solid electrolytes. Other solid electrolytes may include one or more of the commonly used sulfide electrolytes, halide electrolytes, and oxide electrolytes in the art.
[0205] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. The metal foil may be a pure metal, an alloy, or a surface-treated metal, such as, but not limited to, stainless steel foil, copper foil, and nickel foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. As an example, the metal layer may include, but is not limited to, one or more of copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. As an example, the polymer substrate may include, but is not limited to, one or more of polypropylene, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene, and polyethylene.
[0206] In some embodiments, the solid-state battery cell may further include an outer packaging for accommodating the electrode assembly formed by assembling the negative electrode, electrolyte layer, and positive electrode. The outer packaging may be a rigid shell, such as a hard plastic shell, aluminum shell, or steel shell. The outer packaging may also be a flexible package, such as a pouch. The material of the flexible package may be plastic, such as one or more of aluminum-plastic film, polypropylene, polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0207] [Preparation Method]
[0208] The methods for preparing solid-state battery cells are well known. For example, the assembly methods of solid-state battery cells include, but are not limited to, coin cells, hard-case cells, and pouch cells.
[0209] Example
[0210] The following embodiments describe the disclosure of this disclosure in more detail. These embodiments are merely illustrative, as various modifications and variations will be apparent to those skilled in the art within the scope of this disclosure. Unless otherwise stated, all parts, percentages, and ratios reported in the following embodiments are based on mass, and all reagents used in the embodiments are commercially available or synthesized by conventional methods and can be used directly without further processing, and the instruments used in the embodiments are commercially available.
[0211] Example 1
[0212] Preparation of modified sulfide electrolytes
[0213] 10g of sulfide electrolyte matrix Li6PS5Cl was placed on a perforated partition plate on the upper layer of a vacuum heating device. 0.5g of fluorosilane CF3(CF2)7CH2CH2Si(OCH3)3 was exposed to air, resulting in Si-OH hydrolysis and the formation of a coating layer precursor, which was a Si-OH-containing fluorosilane. The coating layer precursor was placed at the bottom of the vacuum heating device, which was set to 120°C. Heating produced a coating layer precursor gas, allowing it to contact the sulfide electrolyte matrix and form a coating layer on at least a portion of the matrix surface, thus obtaining a modified sulfide electrolyte.
[0214] Preparation of solid-state battery cells
[0215] LiNi, the positive electrode active material 0.8 Co 0.1 Mn 0.1 O2 (NCM811) was mixed with the modified sulfide electrolyte and positive electrode conductive agent vapor-grown carbon fiber (VGCF) prepared above at a mass ratio of 85:13:2 and then rolled to form the positive electrode active material layer.
[0216] Solid-state battery cells are assembled using a 10mm diameter solid-state battery cell mold: 100mg of the modified sulfide electrolyte prepared above is added to the solid-state battery cell mold and flattened to form an electrolyte layer; then 100mg of a mixture of Li6PS5Cl and indium powder in a mass ratio of 70:30 is added to one side of the electrolyte layer, flattened, and then a layer of lithium foil is applied and pressed together; then the prepared positive electrode active material layer is installed on the other side of the electrolyte layer, and finally the solid-state battery cell mold is pressurized to obtain the solid-state battery cell.
[0217] Example 2
[0218] Except for adjusting the composition and amount of fluorosilane, the preparation of the solid-state battery cell is the same as in Example 1, except that the modified sulfide electrolyte is prepared by following the steps below.
[0219] Preparation of modified sulfide electrolytes
[0220] 10g of sulfide electrolyte matrix Li6PS5Cl was placed on a perforated partition plate on the upper layer of a vacuum heating device. Fluorosilane CF3(CF2)5(CH2)2Si(OC2H5)3 was exposed to air, resulting in hydrolysis to release Si-OH, yielding a coating precursor, which was a Si-OH-containing fluorosilane. The coating precursor was placed at the bottom of the vacuum heating device, which was set to 140°C. Heating produced a coating precursor gas, allowing it to contact the sulfide electrolyte matrix and form a coating layer on at least a portion of the matrix's surface, thus obtaining a modified sulfide electrolyte.
[0221] Example 3
[0222] Except for adjusting the composition and amount of fluorosilane, the preparation of the solid-state battery cell is the same as in Example 1, except that the modified sulfide electrolyte is prepared by following the steps below.
[0223] Preparation of modified sulfide electrolytes
[0224] 10g of sulfide electrolyte matrix Li6PS5Cl was placed on a perforated partition plate on the upper layer of a vacuum heating device. Fluorosilane CF3CH2CH2Si(OCH3)3 was exposed to air, hydrolyzing to release Si-OH, yielding a coating layer precursor, which was a Si-OH-containing fluorosilane. The coating layer precursor was placed at the bottom of the vacuum heating device, which was set to 100℃, and heated to produce a coating layer precursor gas. This gas was then brought into contact with the sulfide electrolyte matrix, forming a coating layer on at least a portion of the matrix's surface, thus obtaining a modified sulfide electrolyte.
[0225] Example 4
[0226] Except for adjusting the composition and amount of fluorosilane and the composition of the sulfide electrolyte matrix, the preparation of the solid-state battery cell is the same as in Example 1.
[0227] Preparation of modified sulfide electrolytes
[0228] 10g of sulfide electrolyte matrix Li 10 GeP2S 12 The fluorosilane CF3(CF2)7CH2CH2Si(OCH3)3 is placed on a perforated partition in the upper layer of a vacuum heating device. The fluorosilane CF3(CF2)7CH2CH2Si(OCH3)3 is exposed to air, causing hydrolysis to release Si-OH, yielding a coating precursor. This coating precursor is a fluorosilane containing Si-OH. The coating precursor is placed in the bottom layer of the vacuum heating device, which is set to 120°C. Heating produces a coating precursor gas, which then contacts the sulfide electrolyte matrix, forming a coating layer on at least a portion of the sulfide electrolyte matrix, thus obtaining a modified sulfide electrolyte.
[0229] Example 5
[0230] Except for adjusting the amount of fluorosilane, the preparation of the solid-state battery cell is the same as in Example 1.
[0231] Example 6
[0232] Except for adjusting the amount of fluorosilane, the preparation of the solid-state battery cell is the same as in Example 1.
[0233] Example 7
[0234] Except for replacing fluorosilane with silane and adjusting the amount of silane, the preparation of the modified sulfide electrolyte is the same as in Example 1, except that the solid-state battery cell is prepared by following the steps below.
[0235] Preparation of modified sulfide electrolytes
[0236] 10g of sulfide electrolyte matrix Li6PS5Cl was placed on a perforated partition plate on the upper layer of a vacuum heating device. Silane CH3O-Si(CH3)3 was exposed to air, hydrolyzing to release Si-OH, yielding a coating layer precursor, which was a silane containing Si-OH. The coating layer precursor was placed at the bottom of the vacuum heating device, which was set to 90°C, and heated to produce a coating layer precursor gas. This gas was then brought into contact with the sulfide electrolyte matrix, forming a coating layer on at least a portion of the matrix's surface, thus obtaining a modified sulfide electrolyte.
[0237] Example 8
[0238] Except for adjusting the composition and amount of fluorosilane, the preparation of the solid-state battery cell is the same as in Example 1, except that the modified sulfide electrolyte is prepared through the following steps.
[0239] Preparation of modified sulfide electrolytes
[0240] 10g of sulfide electrolyte matrix Li6PS5Cl was placed on a perforated partition plate on the upper layer of a vacuum heating device. Fluorosilane CF3O-Si(CH3)3 was exposed to air, hydrolyzing to release Si-OH, yielding a coating layer precursor, which was a silane containing Si-OH. The coating layer precursor was placed at the bottom of the vacuum heating device, which was set to 80°C. Heating produced a coating layer precursor gas, allowing it to contact the sulfide electrolyte matrix and form a coating layer on at least a portion of the matrix surface, thus obtaining a modified sulfide electrolyte.
[0241] Comparative Example 1
[0242] Except for replacing the modified sulfide electrolyte in the positive electrode and electrolyte layer with the sulfide electrolyte Li6PS5Cl, the preparation of the solid-state battery cell is the same as in Example 1.
[0243] Performance testing
[0244] (1) Ionic conductivity test
[0245] The ionic conductivity was tested using the modified sulfide electrolytes of each embodiment and the sulfide electrolyte of Comparative Example 1 as samples.
[0246] 150 mg of sample powder was pressed into a 10 mm diameter mold under a pressure of 4 tons to prepare an electrolyte disc with a diameter of 10 mm. A conductive agent, VGCF, was spread on both sides of the electrolyte disc as a blocking electrode, and then molded under a pressure of 1 ton. The blocking electrode was connected to an electrochemical impedance spectroscopy workstation for testing. The testing temperature was 25℃, the pressure was 150 MPa, the test bias voltage was 10 mV, and the frequency range was 1 MHz-10 Hz. The resistance value R was obtained by reading the intersection of the impedance spectrum curve with the horizontal axis. The ionic conductivity σ of the sample was calculated using the formula σ = D / (R × S), where σ is the ionic conductivity, D is the thickness of the electrolyte disc, and S is the contact area between the blocking electrode and the electrolyte disc.
[0247] 150 mg of sample powder was placed in a dry room at 25 °C and dew point -40 °C for 4 hours, and then the ionic conductivity σ' of the sample was determined by the above steps.
[0248] Calculate (σ-σ') / σ×100% to obtain the rate of change (%) of the ionic conductivity of the sample.
[0249] (2) Cyclic performance test
[0250] At 25°C, solid-state battery cells were charged to 4.3V (vs. Li) at a current density of 0.1C. + / Li), let stand for 10 minutes, then discharge at a current density of 0.1C to 2.6V (vs. Li). + / Li); then the solid-state battery cells are charged to 4.3V (vs. Li) at a current density of 0.33C. + / Li), let stand for 10 minutes, then discharge at a current density of 0.33C to 2.6V (vs. Li). + / Li), the discharge capacity at this time is recorded as C1; the solid-state battery cell is cycled at a current density of 0.33C according to the above charge and discharge process. The capacity retention rate of the solid-state battery cell after 100 cycles at 0.33C is measured.
[0251] Please refer to Tables 1 and 2 for the preparation and testing parameters of each embodiment and comparative example.
[0252] Table 1
[0253]
[0254] Table 2
[0255] Serial Number σ(mS / cm) σ'(mS / cm) Change rate of ionic conductivity / % 100-cycle capacity retention rate / % Example 1 9.70 9.60 1.03 96.0 Example 2 9.56 9.07 5.13 94.3 Example 3 9.61 9.22 4.06 94.8 Example 4 8.70 8.50 2.30 95.7 Example 5 9.80 8.90 9.18 91.5 Example 6 9.27 9.27 0 96.2 Example 7 8.78 7.52 14.35 91.3 Example 8 9.67 8.09 16.34 90.5 Comparative Example 1 10.00 7.14 28.60 70.0
[0256] As can be seen from the test results in Tables 1 and 2, the modified sulfide electrolyte of this disclosure has a hydrophobic coating layer on its surface that is connected to the sulfide electrolyte groups through Si-OS covalent bonds. This can reduce the side reactions between the sulfide electrolyte matrix and the air, so that the modified sulfide electrolyte can maintain a high ionic conductivity after being exposed to the air, thereby improving the cycle performance of the solid-state battery cell.
[0257] It should be noted that this disclosure is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this disclosure are included within the technical scope of this disclosure. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, are also included within the scope of this disclosure without departing from the spirit of this disclosure.
Claims
1. A solid-state battery cell, comprising a positive electrode, an electrolyte layer, and a negative electrode, wherein the electrolyte layer is located between the positive electrode and the negative electrode, characterized in that, At least one of the positive electrode, the electrolyte layer, and the negative electrode comprises a modified sulfide electrolyte; The modified sulfide electrolyte includes a sulfide electrolyte matrix and a coating layer covering at least a portion of the surface of the sulfide electrolyte matrix; The sulfide electrolyte matrix and the coating layer are connected by Si-OS covalent bonds; The coating layer includes silane and / or fluorosilane.
2. The solid-state battery cell according to claim 1, characterized in that, The covering layer includes one or more of the structures shown in Formula 1; R n SiY 4-n Formula 1 Where n is 1, 2 or 3; R independently represents C1 to C10 alkyl groups, or C1 to C10 alkyl groups substituted with F atoms; Y represents -OS-#, and the O atom in Y is connected to the Si atom in Formula 1.
3. The solid-state battery cell according to claim 2, characterized in that, The R represents CF3(CF2)7CH2CH2-, CF3(CF2)5CH2CH2-, or CF3CH2CH2-, respectively.
4. The solid-state battery cell according to any one of claims 1-3, characterized in that, The coating layer also includes LiF.
5. The solid-state battery cell according to any one of claims 1-4, characterized in that, The coating layer includes element F, and based on the total mass of the modified sulfide electrolyte (100%), the mass content of element F in the coating layer is 0.3% to 1%.
6. The solid-state battery cell according to any one of claims 1-5, characterized in that, The coating layer includes carbon (C) element, and based on the total mass of the modified sulfide electrolyte (100%), the mass content of C element in the coating layer is 0.3% to 1%; and / or The coating layer includes C and F elements, and the mass ratio of C to F elements in the coating layer is (0.3:1) to (0.7:1).
7. The solid-state battery cell according to any one of claims 1-6, characterized in that, The thickness of the coating layer is 2nm to 10nm.
8. The solid-state battery cell according to any one of claims 1-7, characterized in that, The coating area ratio of the modified sulfide electrolyte is 90% or more, where the coating area ratio represents the ratio of the surface area of the coating layer to the surface area of the modified sulfide electrolyte.
9. The solid-state battery cell according to any one of claims 1-8, characterized in that, The volume distribution particle size Dv50 of the modified sulfide electrolyte is 1 μm to 10 μm.
10. The solid-state battery cell according to any one of claims 1-9, characterized in that, The modified sulfide electrolyte has an ionic conductivity of 1×10⁻⁶. -3 S / cm~8×10 -3 S / cm.
11. The solid-state battery cell according to any one of claims 1-10, characterized in that, The positive electrode includes a positive electrode film layer, the positive electrode film layer includes a positive electrode active material and a modified sulfide electrolyte according to any one of claims 1-10, wherein the positive electrode active material includes one or more of lithium transition metal oxides and their modified materials, lithium phosphates and their modified materials, lithium titanate, lithium niobate, sulfur, selenium, and tellurium; and / or, The electrolyte layer comprises the modified sulfide electrolyte according to any one of claims 1-10; and / or, The negative electrode comprises lithium or a lithium alloy, or the negative electrode comprises a negative electrode active material and the modified sulfide electrolyte according to any one of claims 1-10, wherein the negative electrode active material comprises one or more of natural graphite, artificial graphite, mesophase micro carbon spheres, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, and metal oxides.
12. A battery device, characterized in that, It includes any one of the solid-state battery cells according to claims 1-11.
13. An electrical appliance, characterized in that, Includes the solid-state battery cell according to any one of claims 1-11 or the battery device according to claim 12.
14. A modified sulfide electrolyte, characterized in that, It includes a sulfide electrolyte matrix and a coating layer covering at least a portion of the surface of the sulfide electrolyte matrix; The sulfide electrolyte matrix and the coating layer are connected by Si-OS covalent bonds; The coating layer includes silane and / or fluorosilane.
15. The modified sulfide electrolyte according to claim 14, characterized in that, The covering layer includes one or more of the structures shown in Formula 1; R n SiY 4-n Formula 1 Where n is 1, 2 or 3; R independently represents C1 to C10 alkyl groups, or C1 to C10 alkyl groups substituted with F atoms; Y represents -OS-#, and the O atom in Y is connected to the Si atom in Formula 1.
16. The modified sulfide electrolyte according to claim 15, characterized in that, The R represents CF3(CF2)7CH2CH2-, CF3(CF2)5CH2CH2-, or CF3CH2CH2-, respectively.
17. The modified sulfide electrolyte according to any one of claims 14-16, characterized in that, The coating layer also includes LiF.
18. The modified sulfide electrolyte according to any one of claims 14-17, characterized in that, The coating layer includes element C, and based on the total mass of the modified sulfide electrolyte (100%), the mass content of element C in the coating layer is 0.3% to 1%; and / or, The coating layer includes element F, and based on the total mass of the modified sulfide electrolyte (100%), the mass content of element F in the coating layer is 0.3% to 1%; and / or, The coating layer includes C and F elements, and the mass ratio of C to F elements in the coating layer is (0.3:1) to (0.7:1).
19. A method for preparing a modified sulfide electrolyte, characterized in that, The method includes the following steps: providing a sulfide electrolyte matrix and a coating layer precursor gas; contacting the coating layer precursor gas with the sulfide electrolyte matrix to form a coating layer on at least a portion of the surface of the sulfide electrolyte matrix, thereby obtaining a modified sulfide electrolyte, wherein the coating layer precursor includes a silane containing Si-OH and / or a fluorosilane containing Si-OH, the modified sulfide electrolyte includes a sulfide electrolyte matrix and a coating layer covering at least a portion of the surface of the sulfide electrolyte matrix; the sulfide electrolyte and the coating layer are connected by Si-OS covalent bonds, and the coating layer includes a silane and / or a fluorosilane.
20. The preparation method according to claim 19, characterized in that, The steps of providing the coating precursor gas include the following steps: Provide the compound shown in Formula 2, and hydrolyze the compound shown in Formula 2 to release Si-OH to obtain the coating layer precursor, wherein the coating layer precursor includes a silane containing Si-OH and / or a fluorosilane containing Si-OH. R n SiX 4-n Formula 2 Where n is 1, 2 or 3; R independently represents C1 to C10 alkyl groups, or C1 to C10 alkyl groups substituted with F atoms; X independently represents an alkoxy group, an alkoxy group substituted with an F atom, an aryloxy group, an acyloxy group, or a chlorine group; The coating precursor is heated to obtain a coating precursor gas.
21. The preparation method according to claim 20, characterized in that, The compound shown in Formula 2 includes one or more of the following: tridecylfluorooctyltriethoxysilane, tridecylfluorooctyltrimethoxysilane, heptadecafluorodecyltrimethoxysilane, heptadecafluorodecyltriethoxysilane, trifluoropropyltrimethoxysilane, and trifluoropropyltriethoxysilane.
22. The preparation method according to claim 20 or 21, characterized in that, The heating temperature is 80℃~140℃.