A fluorinated crosslinked polyether gel electrolyte, its preparation and application

By employing a three-dimensional network structure of fluorinated cross-linked polyether gel electrolyte in potassium-ion batteries, the problems of low conductivity and interfacial compatibility of electrolytes in potassium-ion batteries are solved, achieving improved performance and safety. This method is suitable for high-voltage cathode materials and metallic potassium anodes.

CN123120861APending Publication Date: 2026-11-17QINGDAO INST OF BIOENERGY & BIOPROCESS TECH CHINESE ACADEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611438289.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polymer electrolytes for potassium-ion batteries suffer from low room-temperature ionic conductivity and poor compatibility with electrode interfaces in potassium-ion batteries, making it difficult to effectively suppress potassium dendrite growth. Furthermore, traditional gel electrolytes lack sufficient mechanical strength and safety.

Method used

Fluorinated crosslinked polyether gel electrolyte is used, which forms a three-dimensional network structure through in-situ copolymerization between the battery separator and/or electrodes. It is then copolymerized with PEGDE using a fluorinated hydrocarbon chain modifier to form a gel electrolyte with high mechanical strength and excellent interfacial compatibility.

Benefits of technology

It significantly improves room temperature ionic conductivity, broadens the electrochemical window, inhibits potassium dendrite growth, enhances the stability of the electrode interface, simplifies the production process, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120861A_ABST
    Figure CN123120861A_ABST
Patent Text Reader

Abstract

This invention relates to the field of potassium-ion battery technology, specifically to a fluorinated crosslinked polyether gel electrolyte, its preparation method, and its application in potassium-ion batteries. The electrolyte is a fluorinated crosslinked gel polymer electrolyte with a three-dimensional network structure, formed by in-situ copolymerization of a precursor solution system between the battery separator and / or electrodes. The precursor solution system contains poly(ethylene glycol) diglycidyl ether and a fluorinated hydrocarbon chain modifier; wherein the fluorinated hydrocarbon chain modifier is a fluorinated compound capable of ring-opening polymerization with poly(ethylene glycol) diglycidyl ether. This fluorinated crosslinked structure effectively inhibits polymer crystallization, improves ionic conductivity, and enhances the compatibility of the electrolyte with the positive and negative electrode interfaces. The preparation process of this invention is simple, the raw material cost is low, making it particularly suitable for industrial production, and the resulting electrolyte has good compatibility with the metal negative electrode, making it suitable for high-performance potassium-ion battery systems.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of potassium-ion battery technology, specifically to a fluorinated crosslinked polyether gel electrolyte, its preparation method, and its application in potassium-ion batteries. Background Technology

[0002] With growing global concerns about the scarcity and rising cost of lithium resources, potassium-ion batteries are considered a highly promising next-generation electrochemical energy storage system due to their abundant potassium resources, low cost, and standard electrode potential close to that of lithium. However, the commercialization of potassium-ion batteries still faces many challenges, with the electrolyte being one of the key bottlenecks. Traditional liquid organic electrolytes pose safety hazards such as easy leakage and flammability, and are prone to continuous side reactions with the highly active metallic potassium anode during cycling, leading to low coulombic efficiency and uncontrolled dendrite growth, seriously threatening the cycle life and safety of the battery. Using solid-state electrolytes is one of the fundamental ways to solve these problems. Among various solid-state electrolytes, polymer electrolytes, especially polyether-based electrolytes, have attracted widespread attention due to their good flexibility, ease of processing, and advantageous interfacial contact with the electrode. However, traditional polyether-based polymer solid electrolytes, represented by polyethylene oxide (PEO), have two main drawbacks: first, their high crystallinity leads to low room-temperature ionic conductivity, severely limiting the rate performance of batteries; second, they lack sufficient oxidative stability to high-voltage cathode materials and have poor interfacial compatibility with potassium metal anodes, making it difficult to effectively suppress potassium dendrite growth. In recent years, in-situ polymerization to prepare gel polymer electrolytes has become an effective strategy, maintaining the safety of solid electrolytes while improving ionic conductivity and interfacial compatibility. Currently, potassium-based gel polymer electrolytes mainly suffer from the following problems: ester-based systems (such as ethoxylated trimethylpropane triacrylate) have a rigid polymer backbone, requiring the addition of large amounts of plasticizers to achieve considerable ionic conductivity, but this weakens the mechanical strength and safety of the gel electrolyte; ether-based systems (such as 1,3-dioxolane) have poor controllability in ring-opening polymerization, resulting in a wide molecular weight distribution of products and difficulty in obtaining high molecular weight components. Simultaneously, the intrinsic oxidative stability of the polyether backbone is insufficient, leading to a narrow electrochemical window and difficulty in matching high-voltage cathodes. Therefore, developing a novel polymer electrolyte system that combines high ionic conductivity and excellent interfacial compatibility is crucial for promoting the development of high-performance and high-safety potassium-ion batteries. Summary of the Invention

[0003] This invention aims to overcome the technical shortcomings of existing polymer electrolytes for potassium-ion batteries, such as low room-temperature ionic conductivity and poor compatibility with electrode interfaces in potassium-ion batteries. To this end, this invention provides a fluorinated crosslinked polyether gel electrolyte, its preparation method, and its application in potassium-ion batteries.

[0004] To achieve the above objectives, the present invention adopts the following technical solution: A fluorinated crosslinked polyether gel electrolyte, wherein the electrolyte is formed by in-situ copolymerization of a precursor solution system between the separator and / or electrodes of a battery, and has a three-dimensional network structure; the precursor solution system contains poly(ethylene glycol) diglycidyl ether (PEGDE) and a fluorinated hydrocarbon chain modifier; wherein the fluorinated hydrocarbon chain modifier is a fluorinated compound capable of ring-opening polymerization with poly(ethylene glycol) diglycidyl ether (PEGDE).

[0005] The precursor solution system is composed of poly(ethylene glycol) diglycidyl ether (PEGDE), a fluorinated hydrocarbon chain modifier, a potassium salt, a plasticizer, and an initiator; the fluorinated hydrocarbon chain modifier is one or more of fluorinated alcohols, fluorinated amines, fluorinated carboxylic acids, and fluorinated epoxy monomers.

[0006] The fluorinated alcohols are one or more of perfluoropolyether alcohols, 1,1,1,3,3,3-hexafluoro-2-propanol, and 2,4-difluorophenol; the fluorinated amines are one or more of 4-trifluoromethylbenzylamine, 3,3,3-trifluoropropylamine, 4-fluoroaniline, and (2-aminoethyl)(3,3,3-trifluoropropyl)amine; the fluorinated carboxylic acids are one or more of trifluoroacetic acid, 2,2,2-trifluoro-1-phenyl-1-ethanolic acid, 2-(trifluoromethyl)acrylic acid, and hexafluoroglutaric anhydride; and the fluorinated epoxy monomers are one or more of glycidyltrifluoroethyl ether, glycidyl 2,2,3,3-tetrafluoropropyl ether, perfluorobutane diglycidyl ether, glycidyl ether hexafluorononyl ether, 1,1,5-trihydrooctafluoropentyl glycidyl ether, and 3,3,3-trifluoropropyl glycidyl ether.

[0007] Preferably, the fluorinated hydrocarbon chain modifier is one or more of perfluoropolyether alcohol, (2-aminoethyl)(3,3,3-trifluoropropyl)amine, hexafluoroglutaric anhydride, and trifluoropropyl glycidyl ether.

[0008] The added mass of the fluorinated hydrocarbon chain modifier is 1-15 wt% (preferably 2.5 wt%) of the mass of PEGDE; the volume ratio of the plasticizer to PEGDE is 1:100 to 10:100 (preferably 5:100); the final concentration of the potassium salt in the precursor solution system is 0.2-3 mol / L (preferably 1.5 mol / L); the final concentration of the initiator in the precursor solution system is 0.05-2 mol / L (preferably 0.5 mol / L).

[0009] The initiator is a Lewis acid initiator or a compound that can produce Lewis acids with trace amounts of water.

[0010] The initiator is at least one of boron trifluoride ether, aluminum trifluoromethanesulfonate, phosphorus pentafluoride, phosphorus trifluoride, aluminum fluoride, aluminum chloride, tin tetrachloride, titanium tetrachloride, antimony pentachloride, zinc chloride, bismuth chloride, lithium hexafluorophosphate, lithium difluorooxalate borate, lithium tetrafluoroborate, and lithium trifluoromethanesulfonate.

[0011] The potassium salt is selected from at least one of potassium hexafluorophosphate, potassium tetrafluoroborate, potassium bis(trifluoromethanesulfonyl)imide, potassium trifluoromethanesulfonate, potassium perfluoropinacolborate, and potassium perchlorate.

[0012] The plasticizer is one or more of the following: ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl carbonate, triethyl phosphate, trimethyl phosphate, ethylene glycol dimethyl ether, ethylene glycol dibutyl ether, and dipropylene glycol dimethyl ether.

[0013] The molecular weight of the PEGDE is 200-1000.

[0014] The copolymer structure of the fluorinated hydrocarbon chain modifier and PEGDE is as follows:

[0015] Where 1≤n≤20, A method for preparing the fluorinated crosslinked polyether gel electrolyte comprises mixing PEGDE, a fluorinated hydrocarbon chain modifier, a potassium salt, a plasticizer, and an initiator in the above proportions, stirring at 25-40 °C for 1-24 hours to obtain a homogeneous and clear precursor solution; then allowing it to stand at 25-55 °C for 6-48 hours to polymerize, allowing PEGDE and the fluorinated hydrocarbon chain modifier to undergo in-situ crosslinking copolymerization under initiation, forming a fluorinated crosslinked polyether gel electrolyte with a three-dimensional network structure.

[0016] The precursor solution is applied to the battery separator and / or electrodes, or injected into the battery, so that PEGDE and fluorinated hydrocarbon chain modifier undergo in-situ crosslinking copolymerization under initiation to form a fluorinated crosslinked gel polymer electrolyte with a three-dimensional network structure.

[0017] The battery separator is at least one of glass fiber membrane, cellulose membrane, polypropylene membrane, polyethylene membrane, polyester nonwoven fabric or polytetrafluoroethylene membrane.

[0018] An application of the fluorinated crosslinked polyether gel electrolyte, wherein the electrolyte is used in a potassium-ion battery.

[0019] The potassium salt in the precursor solution system can be replaced with sodium or lithium salt to prepare an electrolyte suitable for sodium-ion or lithium-ion batteries.

[0020] A potassium-ion battery includes a positive electrode, a negative electrode, a separator, and the fluorinated crosslinked gel polymer electrolyte; the electrolyte is formed in situ between the separator and / or the electrode of the battery by the method described above.

[0021] The positive electrode is one or more of layered oxides and Prussian blue; The negative electrode is one or more of the following: potassium metal, graphite, or hard carbon.

[0022] A method for preparing a solid-state battery. Step A: Assemble the positive electrode, negative electrode, and separator into a battery; Step B: Inject the precursor solution into the battery assembled in Step A, and let it stand for 1 to 10 hours to allow the solution to fully wet the electrodes and separator; Step C: Age the wetted battery at 25 to 55 °C for 6 to 48 hours to allow the mixed system to polymerize in situ inside the battery, forming a fluorinated crosslinked gel polymer electrolyte, thereby obtaining an integrated solid-state battery.

[0023] Beneficial effects: This invention's fluorinated crosslinked gel polymer electrolyte effectively disrupts the crystallinity of polyether segments by introducing fluorinated hydrocarbon chains, significantly improving room-temperature ionic conductivity. Simultaneously, the spontaneous formation of a stable SEI film at the electrode interface by fluorinated groups inhibits potassium dendrite growth and broadens the electrochemical window, making it compatible with high-voltage cathode materials. The in-situ polymerization process integrates electrolyte synthesis and battery assembly, greatly simplifying the production process and ensuring high performance while maintaining good industrial compatibility. Attached Figure Description

[0024] Figure 1 This is a scanning electron microscope image of the solid electrolyte of Example 1.

[0025] Figure 2 The images show the electrochemical impedance spectroscopy of the solid electrolyte in Example 1 at different temperatures.

[0026] Figure 3 This is an electrochemical window test diagram of the solid electrolyte in Example 1.

[0027] Figure 4 The stress-strain curve is shown for the solid electrolyte of Example 1.

[0028] Figure 5 This is a symmetric battery cycle diagram based on the solid electrolyte of Example 1.

[0029] Figure 6 This is the room temperature electrochemical impedance spectroscopy of the solid electrolyte based on Example 2.

[0030] Figure 7 This is a cycling diagram of a symmetrical battery assembled based on the solid electrolyte of Example 4.

[0031] Figure 8 The charge-discharge curves show the performance of K||Prussian blue assembled based on the solid electrolyte of Example 5.

[0032] Figure 9 The stress-strain diagram is for the solid electrolyte in Comparative Example 1.

[0033] Figure 10 The diagram shows the symmetric battery cycle diagram based on the solid electrolyte of Comparative Example 2. Detailed Implementation

[0034] The present invention will now be described in further detail with reference to the embodiments and accompanying drawings.

[0035] This invention introduces a fluorinated hydrocarbon chain modifier with functional groups capable of copolymerizing with glycidyl ether into an electrolyte. By controlling the ratio of the modifier to PEGDE, a unique three-dimensional cross-linked polyether network structure with fluorinated hydrocarbon chain modification is formed under the action of an initiator. Adjusting the ratio of the two modifiers can change the number of cross-linking sites, thereby optimizing the cross-linking density of the cross-linked polymer, which improves both the mechanical strength and ionic conductivity of the electrolyte. Simultaneously, this cross-linked polyether gel electrolyte reduces the content of terminal hydroxyl groups in the chain segments, thus broadening the electrochemical window. Furthermore, the network of the gel electrolyte contains potassium salts and plasticizers, which can inhibit polymer crystallization, enhance ion transport capacity, and strengthen interfacial stability with electrodes (especially potassium metal anodes), achieving multiple synergistic goals.

[0036] The preparation process of this invention is simple and the raw material cost is low, making it particularly suitable for industrial production. Furthermore, the resulting electrolyte has good compatibility with the metal anode and is suitable for high-performance potassium-ion battery systems.

[0037] Unless otherwise specified in the following examples, the conditions shall be performed in accordance with conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they shall be conventional products that can be purchased commercially.

[0038] Example 1 A method for preparing an in-situ fluorinated crosslinked polyether gel electrolyte includes the following steps: (1) Preparation of precursor solution:

[0039] The above substances were mixed evenly and stirred at 25°C for 2 hours to obtain a precursor solution.

[0040] (2) Preparation of polymer electrolyte membrane by precursor solution polymerization: The precursor solution is uniformly impregnated onto the membrane carrier (a polyethylene membrane is used in this embodiment), and then the battery is placed in a 50°C oven for 12 hours to complete the polymerization / crosslinking reaction, thereby obtaining a fluorinated crosslinked gel polymer electrolyte with a three-dimensional network structure (microscopic morphology as shown in the figure). Figure 1 ).

[0041] Depend on Figure 1 As shown, after in-situ polymerization, the precursor solution is uniformly filled into the three-dimensional porous network structure of the polyethylene membrane; the gel polymer electrolyte and the polyethylene membrane form a tight coating structure, and the coating structure has no phase separation interface.

[0042] The prepared fluorinated crosslinked gel polymer electrolyte was tested. The fluorinated crosslinked gel polymer electrolyte was assembled into a stainless steel symmetrical cell using stainless steel as the positive and negative electrodes. Its ionic conductivity at room temperature was measured to be 0.12 mS / cm. -1 It has an antioxidant window of over 4.3 V and excellent tensile properties (see [reference]). Figure 2-4 ).

[0043] The fluorinated crosslinked gel polymer electrolyte obtained above was used to assemble a symmetrical potassium battery with potassium metal as the positive and negative electrodes; the assembled battery was tested at 25 °C and 0.1 mA cm⁻¹. -2 The following test, such as Figure 5 As shown, the cycle life of the symmetric cell can reach 350 hours, and the deposition / stripping polarization voltage is only 0.11 V.

[0044] Example 2 (1) Preparation of precursor solution:

[0045] The above substances were mixed evenly and stirred at 25°C for 2 hours to obtain a precursor solution.

[0046] (2) Preparation of polymer electrolyte membrane by precursor solution polymerization: The precursor solution is uniformly impregnated into the glass fiber membrane carrier, and then the battery is placed in a 50°C oven for 12 hours to complete the polymerization / crosslinking reaction, thereby obtaining a fluorinated crosslinked gel polymer electrolyte with a three-dimensional network structure.

[0047] The fluorinated crosslinked gel polymer electrolyte obtained above was assembled into a stainless steel symmetrical cell using stainless steel as the positive and negative electrodes. Its ionic conductivity at room temperature was measured to be 0.10 mS / cm. -1 (See) Figure 6 ).

[0048] Example 3 A method for preparing an in-situ fluorinated crosslinked polyether gel electrolyte includes the following steps: (1) Preparation of precursor solution:

[0049] The above substances were mixed evenly and stirred at 25°C for 2 hours to obtain a precursor solution.

[0050] (2) Preparation of polymer electrolyte membrane by precursor solution polymerization: The precursor solution is uniformly impregnated into the glass fiber membrane carrier, and then the battery is placed in a 50°C oven for 12 hours to complete the polymerization / crosslinking reaction, thereby obtaining a fluorinated crosslinked gel polymer electrolyte with a three-dimensional network structure.

[0051] The fluorinated crosslinked gel polymer electrolyte obtained above was assembled into a stainless steel symmetrical cell using stainless steel as the positive and negative electrodes. Its ionic conductivity at room temperature was measured to be 0.20 mS / cm. -1 .

[0052] Example 4 A method for preparing an in-situ fluorinated crosslinked polyether gel electrolyte includes the following steps: (1) Preparation of precursor solution:

[0053] The above substances were mixed evenly and stirred at 25°C for 2 hours to obtain a precursor solution.

[0054] (2) Solid-state symmetric cell assembly: 50 μL of precursor solution was drop-coated onto one side of the glass fiber membrane (GA), and then placed on the potassium metal negative electrode. Another 50 μL of precursor solution was drop-coated onto the other side of the GA for encapsulation. The mixture was allowed to stand for 6 h to allow the precursor solution to fully wet the electrode and the membrane. (3) Precursor solution polymerization: The assembled battery was placed in an oven and kept at 50 °C for 12 h. Under the action of the initiator, perfluoropolyether alcohol and PEGDE monomer underwent in-situ polymerization to form a cross-linked solid electrolyte. A symmetrical battery was assembled using potassium metal as the electrode.

[0055] The assembled battery described above was subjected to conditions at 25 °C and 0.1 mA cm⁻¹. -2 The following test, such as Figure 7 As shown, the cycle life of a symmetrical battery can reach 400 hours.

[0056] Example 5 A method for preparing an in-situ fluorinated crosslinked polyether gel electrolyte includes the following steps: (1) Preparation of precursor solution:

[0057] The above substances were mixed evenly and stirred at 25°C for 2 hours to obtain a precursor solution.

[0058] (2) Solid-state battery assembly: 50 μL of precursor solution was dropped onto the positive electrode, followed by placing the glass fiber separator (GA) on the positive electrode. Another 50 μL of precursor solution was then dropped onto the GA, and finally the negative electrode was placed on top to encapsulate the battery. The battery was allowed to stand for 6 hours to allow the precursor solution to fully wet the electrodes and the separator. (3) Precursor solution polymerization: After the precursor solution wets the electrodes and separator, the battery is placed in an oven and kept at 50°C for 12 hours. Under the action of the initiator, trifluoropropyl glycidyl ether and PEGDE monomer undergo in-situ polymerization to form a cross-linked solid electrolyte. Using Prussian blue as the positive electrode and potassium metal as the negative electrode, a solid battery is prepared by combining the cross-linked solid electrolyte.

[0059] The assembled battery described above was subjected to conditions at 25 °C and 0.1 mA cm⁻¹. -2 The following test, such as Figure 8 As shown, the battery's first-cycle discharge specific capacity can reach 128 mAh g. -1 .

[0060] Comparative Example 1 The difference from Example 1 lies in the amount added during the preparation of the precursor solution. Specifically, the preparation of the precursor solution is as follows:

[0061] The above substances were mixed evenly and stirred at 25°C for 2 hours to obtain a precursor solution. Then, a stainless steel symmetrical battery was assembled according to the method described in Example 1.

[0062] The assembled batteries were subjected to mechanical tensile property tests at room temperature. For example... Figure 9 As shown, compared with Example 1, after reducing the content of fluorinated hydrocarbon chain modifier, the density of rigid physical crosslinking nodes in the system is reduced, the relative slippage between polyether chain segments is intensified, and stress cannot be efficiently transmitted in the three-dimensional network. At the same time, the weakening of chain entanglement leads to a decrease in cohesive energy, making the in-situ polyether electrolyte obtained in this example more prone to chain segment dissociation and macroscopic fracture when stretched, thus reducing its mechanical tensile properties compared with Example 1.

[0063] The difference between Comparative Example 2 and Example 1 lies in the amount of precursor solution added during preparation, specifically: Preparation of precursor solution:

[0064] The above substances were mixed evenly and stirred at 25°C for 2 hours to obtain a precursor solution. A symmetrical potassium battery was then assembled according to the method described in Example 1.

[0065] The assembled battery described above was subjected to conditions at 25 °C and 0.1 mA cm⁻¹. -2 The following test, such as Figure 10 As shown, based on Example 1, increasing the content of the fluorinated hydrocarbon chain modifier resulted in excessively high polymer network stiffness, hindering potassium ion migration, decreasing ionic conductivity, and increasing ohmic polarization. Simultaneously, the excessive fluorinated component was over-reduced on the electrode surface, forming an excessively thick and dense SEI layer, significantly increasing interfacial diffusion resistance. The combined effect of these factors resulted in a cycle life of only 200 h and a polarization voltage as high as 0.3 V. In contrast, existing literature records that a symmetric battery with a PEO-KFSI polymer electrolyte modified with polyvinylpyrrolidone iodine (PVP-I) has a polarization voltage of 0.26 V after 200 h of cycling at the same current density. This example exhibits a polarization voltage approximately 15% higher at the same cycle duration, indicating that the excessive fluorinated hydrocarbon chain modifier has a significant negative impact on interfacial stability.

Claims

1. A fluorinated crosslinked polyether gel electrolyte, characterized in that: The electrolyte is a fluorinated crosslinked gel polymer electrolyte with a three-dimensional network structure formed by in-situ copolymerization of a precursor solution system between the separator and / or electrodes of the battery; the precursor solution system contains poly(ethylene glycol) diglycidyl ether (PEGDE) and a fluorinated hydrocarbon chain modifier; wherein the fluorinated hydrocarbon chain modifier is a fluorinated compound that can undergo ring-opening polymerization with poly(ethylene glycol) diglycidyl ether (PEGDE).

2. The fluorinated crosslinked polyether gel electrolyte according to claim 1, characterized in that: The precursor solution system is composed of poly(ethylene glycol) diglycidyl ether (PEGDE), a fluorinated hydrocarbon chain modifier, a potassium salt, a plasticizer, and an initiator; the fluorinated hydrocarbon chain modifier is one or more of fluorinated alcohols, fluorinated amines, fluorinated carboxylic acids, and fluorinated epoxy monomers.

3. The fluorinated crosslinked polyether gel electrolyte according to claim 2, characterized in that: The fluorinated alcohols are one or more of perfluoropolyether alcohols, 1,1,1,3,3,3-hexafluoro-2-propanol, and 2,4-difluorophenol; the fluorinated amines are one or more of 4-trifluoromethylbenzylamine, 3,3,3-trifluoropropylamine, 4-fluoroaniline, and (2-aminoethyl)(3,3,3-trifluoropropyl)amine; the fluorinated carboxylic acids are one or more of trifluoroacetic acid, 2,2,2-trifluoro-1-phenyl-1-ethanolcarboxylic acid, 2-(trifluoromethyl)acrylic acid, and hexafluoroglutaric anhydride; and the fluorinated epoxy monomers are one or more of glycidyltrifluoroethyl ether, glycidyl 2,2,3,3-tetrafluoropropyl ether, perfluorobutane diglycidyl ether, glycidyl ether hexafluorononyl ether, 1,1,5-trihydrooctafluoropentyl glycidyl ether, and 3,3,3-trifluoropropyl glycidyl ether.

4. The fluorinated crosslinked polyether gel electrolyte according to claim 2, characterized in that: The added mass of the fluorinated hydrocarbon chain modifier is 0.1~15 wt% of the mass of PEGDE; the volume ratio of the plasticizer to PEGDE is 1:100~10:100; the final concentration of the potassium salt in the precursor solution system is 0.2~3 mol / L; and the final concentration of the initiator in the precursor solution system is 0.05~2 mol / L.

5. The fluorinated crosslinked polyether gel electrolyte according to claim 1, characterized in that: The initiator is a Lewis acid initiator or a compound that can produce Lewis acids with trace amounts of water.

6. A method for preparing the fluorinated crosslinked polyether gel electrolyte according to claim 1, characterized in that: PEGDE, fluorinated hydrocarbon chain modifier, potassium salt, plasticizer and initiator are mixed in the above proportions and stirred at 25~40 ℃ for 1~24 hours to obtain a homogeneous and clear precursor solution; then, the mixture is allowed to stand at 25~55 ℃ for 6~48 hours to polymerize, so that PEGDE and fluorinated hydrocarbon chain modifier undergo in-situ crosslinking copolymerization under initiation to form a fluorinated crosslinked polyether gel electrolyte with a three-dimensional network structure.

7. The preparation method according to claim 6, characterized in that: The precursor solution is applied to the surface of the battery separator and / or electrode, or injected into the battery. After initiation, PEGDE undergoes in-situ crosslinking copolymerization with a fluorinated hydrocarbon chain modifier to form a three-dimensional network structure of fluorinated crosslinked gel polymer electrolyte.

8. An application of the fluorinated crosslinked polyether gel electrolyte according to claim 1, characterized in that: The application of the electrolyte in potassium-ion batteries.

9. A potassium-ion battery, characterized in that: The battery comprises a positive electrode, a negative electrode, a separator, and a fluorinated crosslinked gel polymer electrolyte as described in claim 1; the electrolyte is in-situ polymerized between the separator and / or electrodes of the battery by the method described in claim 6.

10. A method for preparing a solid-state battery, characterized in that, Step A: Assemble the positive electrode, negative electrode, and separator into a battery; Step B: Inject the precursor solution described in claim 6 into the battery assembled in step A, and let it stand for 1 to 10 hours to allow the solution to fully wet the electrodes and separator; Step C: Age the wetted battery at 25 to 55 °C for 6 to 48 hours to allow the mixed system to polymerize in situ inside the battery to form a fluorinated crosslinked gel polymer electrolyte, thereby obtaining a solid-state battery in one piece.