A gel polymer electrolyte additive and a lithium metal battery, and their preparation method and application
By constructing a stable CEI interface layer through synergistic modification of gel polymer electrolytes with borate and fluorinated carbonate, the problems of low lithium-ion transference number and slow transport kinetics of existing gel polymer electrolytes are solved, and high cycle stability and safety of lithium metal batteries are achieved in a wide temperature range.
Patent Information
- Application Number
- CN202611581415.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing gel polymer electrolytes suffer from low lithium-ion transference number and slow ion transport kinetics. After long-term cycling, the battery becomes severely polarized and its capacity decays rapidly, making it difficult to meet the requirements of high cycle stability and high safety performance.
A gel polymer electrolyte modified with borates and fluorinated carbonates was used to reconstruct the electric double layer structure through the electric dipole effect of the polymer. The strong electron-withdrawing inductive effect of trifluoromethyl groups was used to form a hydrogen bond cross-linking network, constructing a stable CEI interface layer rich in LiF and BO/BF, which inhibits lithium dendrite growth and interfacial side reactions.
It significantly improves the cycle life and safety performance of lithium metal batteries, enables stable long-term cycling of batteries in a wide temperature range, enhances the stability of the electrode/electrolyte interface, and suppresses changes in interface impedance at high and low temperatures.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium metal battery technology, and more specifically to a gel polymer electrolyte additive and a lithium metal battery, as well as their preparation methods and applications. Background Technology
[0002] With the rapid development of new energy storage, intelligent electric vehicles, and portable electronic devices, the market is placing increasingly stringent demands on battery energy density, cycle life, and safety performance. Gel polymer electrolytes (GPEs) are battery materials that fall between liquid and solid states, combining the advantages of both liquid electrolytes and solid polymer electrolytes. They possess excellent ionic conductivity, good interfacial compatibility, and leak-proof characteristics, effectively improving the safety defects of liquid electrolytes. However, existing conventional gel polymer electrolytes still have significant technical shortcomings, generally exhibiting low lithium-ion transference numbers and slow ion transport kinetics. After long-term cycling, these electrolytes suffer from severe battery polarization and rapid capacity decay, making it difficult to simultaneously meet the requirements for high cycle stability and high safety performance.
[0003] To optimize the interfacial properties and electrochemical performance of gel polymer electrolytes, existing studies mostly employ single fluorination modification or inorganic salt modification to optimize the electrolyte system. Fluorinated carbonate modification can improve interfacial oxidation resistance and structural stability by inducing the formation of a highly stable CEI component containing LiF. However, single fluorination modification suffers from limited modification effects and limited improvement in ion conduction, and high-fluorine content systems are characterized by high cost and insufficient compatibility. Borate modification possesses excellent film-forming properties and can optimize lithium-ion transport kinetics, but its individual modification is insufficient to form a complete CEI film with high mechanical strength and high stability, resulting in limited interfacial modulation effects.
[0004] Therefore, how to develop a high-performance gel polymer electrolyte is a problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0005] In view of this, the purpose of the present invention is to provide a gel polymer electrolyte additive and a lithium metal battery, as well as the preparation method and application thereof, to solve the problems of severe side reactions at the positive electrode interface and poor high and low temperature cycling performance of traditional gel polymer electrolytes under high pressure.
[0006] To achieve the above objectives, the present invention adopts the following technical solution: A gel polymer electrolyte additive includes 0.1-1 parts of borate additive and 0.1-1 parts of fluorinated carbonate additive, preferably 1 part of borate additive and 1 part of fluorinated carbonate additive.
[0007] Furthermore, the aforementioned borate additive is an inorganic or organic compound containing at least one borate ion; the borate ion is tetrafluoroborate (BF4). - ), metaborate (BO2) - ) and bis(oxalate)borate (BOB) - At least one of the following.
[0008] Furthermore, the aforementioned borate additive is at least one of tetrabutylammonium tetrafluoroborate, lithium tetrafluoroborate, 2-(diphenylphosphino)ethylamine tetrafluoroborate, lithium metaborate, and lithium dioxalate borate.
[0009] Furthermore, the aforementioned fluorinated carbonate additive is an organic compound containing at least one fluoroalkyl group; the fluoroalkyl group is trifluoroethyl.
[0010] Furthermore, the aforementioned fluorinated carbonate additive is at least one of (2,2,2-trifluoroethyl) ethyl carbonate, trifluoroethyl methyl carbonate, and bis(trifluoroethyl) carbonate.
[0011] A gel polymer electrolyte includes an electrolyte salt, an organic solvent, a polymer monomer and a thermal initiator, as well as the above-mentioned gel polymer electrolyte additives; The concentration of the electrolyte salt in the gel polymer electrolyte is 0.5-2 mol / L, preferably 1 mol / L; The molar ratio of organic solvent to electrolyte salt is (10-12):1, preferably 11.5:1; The amount of polymer monomer added is 0.1wt%-5wt% of the gel polymer electrolyte, preferably 0.1wt%-3wt%, and more preferably 1.5wt%. The amount of thermal initiator added is 0.1wt%-1wt% of the gel polymer electrolyte, preferably 0.5wt%; The amount of gel polymer electrolyte additive added is 0.1wt%-5wt% of the gel polymer electrolyte, preferably 0.1wt%-3wt%, and more preferably 2wt%.
[0012] Furthermore, the polymer monomers mentioned above are at least one of N,N'-methylenebismethylacrylamide, polyethylene glycol diacrylate, ethoxylated trimethylolpropane triacrylate, and pentaerythritol triacrylate.
[0013] Furthermore, the aforementioned thermal initiator is azobisisobutyronitrile (AIBN).
[0014] Furthermore, the aforementioned organic solvent is at least one of ethylene carbonate (EC), diethyl carbonate (DEC), and dimethyl carbonate (DMC).
[0015] Furthermore, the electrolyte salt mentioned above is lithium hexafluorophosphate (LiPF6).
[0016] A method for preparing a gel polymer electrolyte specifically includes the following steps: (1) Weigh each raw material according to the amount of the gel polymer electrolyte mentioned above; (2) Add the electrolyte salt to the organic solvent and stir until homogeneous to obtain the electrolyte solution; (3) Add the polymer monomer, thermal initiator, borate additive and fluorinated carbonate additive to the electrolyte and stir evenly to obtain gel polymer electrolyte.
[0017] The present invention also claims protection for the use of the above-described gel polymer electrolyte in the preparation of lithium metal batteries.
[0018] A lithium metal battery includes a positive electrode material, a negative electrode material, a separator, and the aforementioned gel polymer electrolyte.
[0019] Furthermore, the aforementioned cathode material is at least one of nickel-cobalt-manganese ternary cathode, lithium cobalt oxide, and lithium iron phosphate, preferably NCM811, a ternary cathode material containing nickel-cobalt-manganese oxide.
[0020] Furthermore, the aforementioned negative electrode material is lithium metal.
[0021] Furthermore, the aforementioned diaphragm is a polypropylene diaphragm.
[0022] As can be seen from the above technical solution, compared with the prior art, the beneficial effects of the present invention are as follows: 1. This invention provides a borate-fluorinated carbonate synergistic modified gel polymer electrolyte and a lithium metal battery containing the same. By utilizing the synergistic effect of the two modified components, ions can be induced to accumulate in an orderly manner and decompose into a film in the Helmholtz layer region within the electrode. This not only effectively suppresses lithium dendrite growth and continuous interfacial side reactions, but also constructs a dense and stable CEI interface layer rich in LiF, significantly improving the cycle life and safety performance of the lithium metal battery. It solves the problems of interface impedance surge caused by low temperature and accelerated interfacial film damage and continuous side reactions caused by high temperature.
[0023] 2. This invention, from the perspective of intermolecular interactions, employs a synergistic modification of the electrolyte system using borate and fluorinated carbonate. It reconstructs the electric double layer (EDL) structure through the polymer's electric dipole effect, and leverages the strong electron-withdrawing inductive effect of trifluoromethyl groups to increase the dipole moment of the fluorinated carbonate molecules, thereby driving the BF4... -Functional additives preferentially occupy the inner Helmholtz layer plane on the electrode surface, replacing carbonate solvent molecules and forming a hydrogen bond cross-linking network through in-situ thermal polymerization. This binds the free solvent, reducing solvent side reactions at the source at high temperatures, forming a stable CEI on the positive electrode side, and inhibiting the dissolution of high-nickel NCM811 transition metals. At low temperatures, they reduce the large-scale reduction of solvents to form a high-resistivity organic interface. They also synergistically construct an inorganic dominant interface layer rich in LiF and BO / BF, improving the stability of the electrode / electrolyte interface and enabling the battery to achieve stable long-term cycling in a wide temperature range of -40 to 60°C. Attached Figure Description
[0024] Figure 1 The images show SEM images of NCM811, a ternary cathode material containing nickel-cobalt-manganese oxide, in lithium metal batteries of Example 1 and Comparative Example 1 after 100 cycles. Figure 2 The XRD characterization results of NCM811, a ternary cathode material containing nickel cobalt manganese oxide, in lithium metal batteries of Example 1 and Comparative Example 1 after 100 cycles are shown in the figure. Figure 3 The F-spectrum of NCM811, a ternary cathode material containing nickel cobalt manganese oxide, in lithium metal batteries of Example 1 and Comparative Example 1, is obtained in XPS etching after 100 cycles.
[0025] Figure 4 The room temperature cycling performance of lithium metal batteries in Example 1 and Comparative Examples 1-3; Figure 5 The high-temperature cycling performance of lithium metal batteries in Example 1 and Comparative Example 1; Figure 6 The low-temperature cycling performance of lithium metal batteries in Example 1 and Comparative Example 1 is shown. Detailed Implementation
[0026] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Example
[0027] The gel polymer electrolyte additives include lithium tetrafluoroborate and ethyl (2,2,2-trifluoroethyl) carbonate in a mass ratio of 1:1.
[0028] Gel polymer electrolytes include lithium hexafluorophosphate (LiPF6), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), N,N'-methylenebismethylacrylamide (MBA) and azobisisobutyronitrile (AIBN), as well as the above gel polymer electrolyte additives. The concentration of lithium hexafluorophosphate (LiPF6) in the gel polymer electrolyte is 1 mol / L. The molar ratio of ethylene carbonate (EC), diethyl carbonate (DEC), and dimethyl carbonate (DMC) is 1:1:1; the molar ratio of the sum of the three to lithium hexafluorophosphate (LiPF6) is 11.5:1. The amount of N,N'-methylenebismethylacrylamide (MBA) added was 1.5 wt% of the gel polymer electrolyte; The amount of azobisisobutyronitrile (AIBN) added is 0.5 wt% of the gel polymer electrolyte; The amount of lithium tetrafluoroborate added is 1 wt% of the gel polymer electrolyte; The amount of (2,2,2-trifluoroethyl) ethyl carbonate added is 1 wt% of the gel polymer electrolyte; The preparation method of the above-mentioned gel polymer electrolyte specifically includes the following steps: (1) Weigh each raw material according to the amount of the gel polymer electrolyte mentioned above; (2) Lithium hexafluorophosphate (LiPF6) is added to a mixed solvent of ethylene carbonate (EC), diethyl carbonate (DEC) and dimethyl carbonate (DMC), and stirred until homogeneous to obtain an electrolyte. (3) Add N,N'-methylenebismethylacrylamide (MBA), azobisisobutyronitrile (AIBN), lithium tetrafluoroborate and (2,2,2-trifluoroethyl) ethyl carbonate to the electrolyte and stir thoroughly for 2 hours to obtain the gel polymer electrolyte.
[0029] A lithium metal battery, comprising a ternary cathode material NCM811 containing lithium nickel cobalt manganese oxide, lithium metal and a polypropylene separator, and the aforementioned gel polymer electrolyte; The above-mentioned method for preparing lithium metal batteries specifically includes the following steps: (1) A battery was made using NCM811, a ternary cathode material containing nickel cobalt manganese oxide, as the working electrode, lithium metal as the counter electrode, and a polypropylene separator. (2) 80 μL of the above-mentioned gel polymer electrolyte is assembled into the battery and thermally polymerized at a high temperature of 70°C for 5 h to obtain a lithium metal battery.
[0030] The only difference from Example 1 is that the gel polymer electrolyte and lithium metal battery do not contain gel polymer electrolyte additives.
[0031] The only difference from Example 1 is that the gel polymer electrolyte and lithium metal battery contain only (2,2,2-trifluoroethyl) ethyl carbonate and no lithium tetrafluoroborate.
[0032] The only difference from Example 1 is that the gel polymer electrolyte and lithium metal battery contain only lithium tetrafluoroborate and not (2,2,2-trifluoroethyl) ethyl carbonate.
[0033] The lithium metal batteries prepared in Example 1 and Comparative Examples 1-3 were subjected to room temperature, high temperature and low temperature tests, respectively.
[0034] Among them, the room temperature test: at a constant temperature of 30℃, the voltage range is 3V to 4.6V, and the constant current is charged and discharged 3 times at 0.1C (1C=210mAh / g). The subsequent long cycle is charged and discharged at 1C constant current and constant voltage. High temperature test: In a 60℃ constant temperature chamber, the voltage range is 3V to 4.6V, and the constant current is charged and discharged 3 times at 0.1C (1C=210mAh / g). The subsequent long cycle is charged and discharged at 1C constant current and constant voltage. Low temperature test: In a low temperature -40℃ constant temperature chamber, the voltage range is 3V to 4.6V, and the constant current is charged and discharged 3 times at 0.1C (1C=210mAh / g). The subsequent long cycle is charged and discharged at 0.3C constant current and constant voltage.
[0035] Calculate the capacity retention rate of the lithium metal battery after cycling, where the capacity retention rate (%) of the battery after the Nth cycle = discharge capacity of the (N+3)th cycle / discharge capacity of the 3rd cycle × 100%.
[0036] The results are as follows Figure 1-6 As shown.
[0037] Depend on Figure 1 As can be seen from the SEM images of the NCM811 ternary cathode material containing nickel-cobalt-manganese oxide in the lithium metal battery of Example 1 and Comparative Example 1 after 100 cycles, the images show that the NCM811 particles on the surface of the cathode material in Comparative Example 1 have severe cracks and a very rough surface. In contrast, the NCM811 particles on the surface of Example 1 remain relatively smooth and flat. This indicates that the electrolyte-derived CEI layer of Example 1, with its excellent flexibility and stability, effectively buffers the lattice strain during the lithium delithiation / lithiation process of the cathode material during cycling. It also mitigates the side reactions that occur when the electrolyte and cathode come into contact, thus reducing the continuous consumption of electrolyte and irreversible damage to the cathode material, thereby better protecting the relative integrity of the cathode material structure.
[0038] Depend on Figure 2 It can be seen that, by comparing the XRD characterization results of the ternary cathode material NCM811 containing nickel cobalt manganese oxide in the lithium metal battery of Example 1 and Comparative Example 1 after 100 cycles, the ratio I of the two diffraction peaks indicating the degree of disorder of transition metal ions can be calculated. (003) / I (104)To evaluate the reconstruction of the NCM crystal structure. According to the data plots, Comparative Example 1, 1100 cycles of I... (003) / (104) The value is 3.16, compared to 4.43 in Example 1. The Ielectrolyte value of Comparative Example 1 is... (003) / (104) The relatively small value indicates that the degree of cation disorder in the cathode crystal structure is greater after cycling, which shows that the electrolyte system of Example 1 effectively reduces the disorder of the cathode crystal structure during cycling.
[0039] Depend on Figure 3 It can be seen that by comparing the F-s spectra of the lithium metal battery containing nickel cobalt manganese oxide ternary cathode material NCM811 in Example 1 and Comparative Example 1 in XPS etching after 100 cycles, in the F 1s spectrum of Comparative Example 1, the LiF component mainly originated from the decomposition of LiPF6. From the etching time 0s to 180s, the LiF component only increased slightly. However, by observing the F 1s spectrum of Example 1, the LiF component mainly originated from the decomposition of LiBF4 and ETFEC. From the etching time 0s to 180s, the LiF content also increased layer by layer and was more than that of Comparative Example 1, indicating that a LiF-rich CEI interface layer was formed.
[0040] Depend on Figure 4 As can be seen from the comparison of the room temperature cycling performance of lithium metal batteries in Example 1 and Comparative Examples 1-3, long-term cycling tests were conducted under the conditions of 30℃, 1C, and 4.6V high voltage. The figure shows that after 300 cycles, the Li ||NCM811 battery with the electrolyte system in Comparative Example 1 retained only 3.91% of its initial specific capacity (172.8 mAh g⁻¹), indicating severe capacity decay. In contrast, the electrolyte system in Comparative Example 2 improved the battery's cycle stability, retaining 32.91% of its initial specific capacity (170.5 mAh g⁻¹) after 300 cycles. The electrolyte system in Comparative Example 3 also improved the battery's cycle stability, retaining 53.9% of its initial specific capacity (177.4 mAh g⁻¹) after 300 cycles. This starkly contrasts with the electrolyte system in Example 1, which significantly improved the battery's cycle stability. Its electrolyte system has an initial specific capacity of up to 185.46 mAh g⁻¹, and after 300 cycles, the capacity can still be maintained at 149.1 mAh g⁻¹, with a capacity retention rate of up to 80.42%.
[0041] Depend on Figure 5As can be seen from the comparison of the high-temperature cycling performance of the lithium metal batteries in Example 1 and Comparative Example 1, long-term cycling tests were conducted under conditions of 60℃, 1C, and 4.6V high voltage. The figure shows that after 450 cycles, the Li ||NCM811 battery with the electrolyte system of Comparative Example 1 retained only 43.5% of its initial specific capacity (204.67 mAh g⁻¹), indicating severe capacity decay. In stark contrast, the electrolyte system of Example 1 significantly improved the battery's cycle stability. Its electrolyte system battery had an initial specific capacity as high as 209.08 mAh g⁻¹, and after 450 cycles, the capacity still remained at 165.37 mAh g⁻¹, with a capacity retention rate as high as 79.1%.
[0042] Depend on Figure 6 As can be seen from the comparison of the low-temperature cycling performance of the lithium metal batteries in Example 1 and Comparative Example 1, long-term cycling tests were conducted under conditions of -40℃, 0.3C, and 4.6V high voltage. The figure shows that after 400 cycles, the Li||NCM811 battery with the electrolyte system of Comparative Example 1 retained only 27.2% of its initial specific capacity (71.61 mAh g⁻¹), indicating severe capacity decay. In stark contrast, the electrolyte system of Example 1 significantly improved the battery's cycle stability. Its electrolyte system battery had an initial specific capacity of 70.08 mAh g⁻¹, and after 650 cycles, the capacity still remained at 68.14 mAh g⁻¹, achieving a capacity retention rate as high as 97.3%.
[0043] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A gel polymer electrolyte additive, characterized in that, It includes 0.1-1 parts of borate additive and 0.1-1 parts of fluorinated carbonate additive.
2. The gel polymer electrolyte additive according to claim 1, characterized in that, The borate additive is an inorganic or organic compound containing at least one borate ion; the borate ion is at least one of tetrafluoroborate, metaborate, and dioxaborate.
3. The gel polymer electrolyte additive according to claim 2, characterized in that, The borate additive is at least one of tetrabutylammonium tetrafluoroborate, lithium tetrafluoroborate, 2-(diphenylphosphino)ethylamine tetrafluoroborate, lithium metaborate, and lithium dioxalate borate.
4. The gel polymer electrolyte additive according to claim 1, characterized in that, The fluorinated carbonate additive is an organic compound containing at least one fluoroalkyl group; the fluoroalkyl group is trifluoroethyl.
5. The gel polymer electrolyte additive according to claim 4, characterized in that, The fluorinated carbonate additive is at least one of (2,2,2-trifluoroethyl) ethyl carbonate, trifluoroethyl methyl carbonate, and bis(trifluoroethyl) carbonate.
6. A gel polymer electrolyte, characterized in that, It includes electrolyte salts, organic solvents, polymer monomers and thermal initiators, as well as gel polymer electrolyte additives as described in any one of claims 1-5; The concentration of the electrolyte salt in the gel polymer electrolyte is 0.5-2 mol / L; The molar ratio of the organic solvent to the electrolyte salt is (10-12):1; The amount of the polymer monomer added is 0.1wt%-5wt% of the gel polymer electrolyte; The amount of the thermal initiator added is 0.1wt%-1wt% of the gel polymer electrolyte; The amount of the gel polymer electrolyte additive added is 0.1wt%-5wt% of the gel polymer electrolyte.
7. The gel polymer electrolyte according to claim 6, characterized in that, The polymer monomer is at least one of N,N'-methylenebismethylacrylamide, polyethylene glycol diacrylate, ethoxylated trimethylolpropane triacrylate, and pentaerythritol triacrylate. The thermal initiator is azobisisobutyronitrile; The organic solvent is at least one of ethylene carbonate, diethyl carbonate, and dimethyl carbonate; The electrolyte salt is lithium hexafluorophosphate.
8. A method for preparing a gel polymer electrolyte, characterized in that, Specifically, the following steps are included: (1) Weigh each raw material according to the amount of the gel polymer electrolyte as described in claim 6 or 7; (2) Add the electrolyte salt to the organic solvent and stir until homogeneous to obtain the electrolyte solution; (3) Add the polymer monomer, thermal initiator, borate additive and fluorinated carbonate additive to the electrolyte and stir evenly to obtain the gel polymer electrolyte.
9. The use of a gel polymer electrolyte as described in claim 6 or 7 in the preparation of lithium metal batteries.
10. A lithium metal battery, characterized in that, It includes a positive electrode material, a negative electrode material, and a separator, as well as a gel polymer electrolyte as described in claim 6 or 7.