A lithium-ion battery and power device
By optimizing the ratio of organic boron, inorganic boron, and fluorobenzene additives in the lithium-ion battery electrolyte, a composite film with synergistic effects at the positive and negative electrode interfaces is formed, solving the problems of insufficient thermal shock safety and high and low temperature cycle performance of high-nickel ternary lithium-ion batteries, and improving the thermal safety and cycle stability of the battery.
Patent Information
- Application Number
- CN202611318240.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-17
AI Technical Summary
Existing lithium-ion batteries using high-nickel ternary materials suffer from insufficient thermal shock safety and high- and low-temperature cycling performance. Furthermore, silicon-carbon anodes present challenges in terms of volume expansion and interface stability. Inappropriate formulation of traditional electrolyte additives leads to poor battery performance adaptability.
By employing a specific ratio of organic boron passivation aid, inorganic boron film-forming aid, and fluorobenzene low-resistance wetting aid, the electrolyte composition is optimized to form a composite film that works synergistically at the positive and negative electrode interfaces, thereby inhibiting transition metal dissolution, mitigating volume expansion, and enhancing interfacial wetting ability.
It achieves synergistic optimization of thermal shock safety and high and low temperature cycling performance of high-nickel ternary lithium-ion batteries, improving the battery's thermal safety and high and low temperature cycling stability while maintaining a high volumetric energy density.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, and in particular to a lithium-ion battery and an electrical device thereof. Background Technology
[0002] High-nickel ternary NCM cathode materials have become the core material for improving the energy density of current power batteries due to their high specific capacity advantage brought by high nickel content. However, this system has significant inherent technical shortcomings. During the deep delithiation process of the material, irreversible phase transition H2-H3 is prone to occur, which can cause problems such as lattice microcracks and large-scale dissolution of nickel ions. At the same time, the release of lattice oxygen will exacerbate the oxidative decomposition of the electrolyte, leading to the aggravation of side reactions at the battery high-temperature cycling interface and the high risk of thermal runaway under thermal shock conditions.
[0003] While existing manganese doping modification can stabilize high-nickel lattices and suppress material phase transitions to some extent, it cannot solve the critical problem of continuous SEI film damage and regeneration caused by nickel ions migrating to the anode after dissolution. Silicon-carbon composite anodes, relying on the ultra-high theoretical capacity of silicon, can effectively improve the volumetric energy density of power batteries. However, they have certain application drawbacks. Silicon undergoes volume expansion of up to 300% during lithium insertion / extraction cycles, causing repeated cracking and reconstruction of the anode SEI film, continuously consuming electrolyte and active lithium, resulting in rapid battery capacity decay. Simultaneously, at 0°C, the interface impedance of the silicon-carbon anode increases sharply, highlighting charge / discharge polarization problems and significantly reducing battery cycle life.
[0004] Currently, the industry mainly uses single boron-based additives to modify electrolytes to improve the degradation problem of the positive and negative electrode interface. Among them, organic boron esters can form a passivation CEI film on the surface of high nickel positive electrode and inhibit the dissolution of transition metals, but the film toughness is insufficient and cannot adapt to the volume expansion stress of silicon-carbon negative electrode. Inorganic boron lithium salts can form a high-toughness boron-oxygen cross-linked SEI film on the negative electrode and buffer the expansion deformation of silicon, but using them alone will significantly increase the overall impedance of the electrolyte and deteriorate the low-temperature dynamic performance of the battery.
[0005] Current technologies simply involve a physical mixing of organic and inorganic boron, which has several drawbacks. First, the boron additive ratio lacks constraints. Excessive boron content can lead to an overly thick interfacial film between the positive and negative electrodes, a surge in battery internal resistance, and deterioration in low-temperature cycle performance. Conversely, insufficient boron content results in inadequate interfacial protection, significantly reducing battery thermal stability and high / low temperature cycle life. Second, the amount of boron additive is not matched to the nickel-manganese ratio of the positive electrode, making it impossible to specifically address the lattice stability and interfacial protection requirements of positive electrodes with different nickel-manganese ratios, resulting in poor performance adaptability. Third, the boron-fluorine buffer system is not optimized in conjunction with the silicon content of the negative electrode, and a fixed additive ratio cannot meet the interfacial protection and impedance control requirements of negative electrodes with full silicon content. Furthermore, traditional electrolytes lack low-resistance fluorobenzene wetting components, resulting in insufficient wetting ability of electrode pores under wide temperature range conditions, which can easily cause blockage of ion transport channels. Simply adding organic boron, inorganic boron and fluorobenzene additives cannot achieve multiple synergistic effects such as electrode lattice stability, interface rigidity-flexibility balance and deformation stress buffering. It is also difficult to simultaneously improve battery thermal safety, low-temperature cycle performance, high-temperature service life and volumetric energy density. Summary of the Invention
[0006] To address the problem that existing high-nickel ternary batteries are difficult to optimize in a synergistic manner in terms of thermal shock safety and high and low temperature cycling performance, a lithium-ion battery and power device are provided.
[0007] The technical solution adopted by the present invention to solve the above-mentioned technical problems is as follows: On one hand, the present invention provides a lithium-ion battery, including a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode includes a positive electrode active material layer, the positive electrode active material layer includes a nickel-cobalt-manganese ternary positive electrode material, and the negative electrode includes a negative electrode active material layer, the negative electrode active material layer includes a silicon-carbon composite material. The electrolyte includes a solvent, a lithium salt, an organoboron passivation aid, an inorganic boron film-forming aid, and a fluorobenzene low-resistance wetting aid. The organoboron passivation aid is an organoborolate ester compound, the inorganic boron film-forming aid is a boron-based lithium salt, and the fluorobenzene low-resistance wetting aid is a fluorobenzene compound. The lithium-ion battery meets the following conditions: 1.33≤(B+L) / (B*L)≤23.33; 0.014≤(B*L)*100 / (D+0.4*E)≤11.278; 0.06≤(L+0.6*B+T) / F≤13.90; Wherein, B% is the mass percentage of the organoboron passivation aid in the electrolyte; L% represents the mass percentage of inorganic boron film-forming aid in the electrolyte; T% represents the mass percentage of fluorobenzene low-resistivity wetting aid in the electrolyte; D% represents the mass percentage of nickel in the positive electrode active material layer; E% represents the mass percentage of manganese in the positive electrode active material layer; F% represents the mass percentage of silicon in the negative electrode active material layer.
[0008] Optionally, the lithium-ion battery satisfies the following conditions: 1.67≤(B+L) / (B*L)≤21.00.
[0009] Optionally, the lithium-ion battery satisfies the following conditions: 0.022≤(B*L)*100 / (D+0.4*E)≤7.317.
[0010] Optionally, the lithium-ion battery satisfies the following conditions: 0.12≤(L+0.6*B+T) / F≤11.10.
[0011] Optionally, the lithium-ion battery satisfies at least one of the following conditions: (1) 0.1%≤B%≤4%; (2) 0.05% ≤ L% ≤ 1.5%; (3) 1%≤T%≤30%; (4) 20%≤D%≤60%; (5) 3%≤E%≤30%; (6) 1%≤F%≤40%.
[0012] Optionally, the lithium-ion battery satisfies at least one of the following conditions: (1) 0.5%≤B%≤2%; (2) 0.125%≤L%≤0.75%; (3) 2.5%≤T%≤15%; (4) 30%≤D%≤50%; (5) 5% ≤ E% ≤ 20%; (6) 6%≤F%≤24%.
[0013] Optionally, the organoboronate compound includes one or more of tris(trimethylsilyl)boronate, trimethylcycloboroxane, and triethylborate; and / or, The boron-based lithium salt includes one or more of lithium dioxaborate and lithium difluorooxaborate; and / or... The fluorobenzene compounds include one or more of fluorobenzene, 1,3-difluorobenzene, 1,3,5-trifluorobenzene, and hexafluorobenzene.
[0014] Optionally, the solvent includes one or more of ethylene carbonate, propylene carbonate, ethyl propionate, propyl propionate, dimethyl carbonate, methyl ethyl carbonate, and diethyl carbonate.
[0015] Optionally, the lithium salt includes one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethanesulfonyl)imide; The total molar concentration of the lithium salt in the electrolyte is 0.85 mol / L to 1.5 mol / L.
[0016] On the other hand, the present invention provides an electrical device including the aforementioned lithium-ion battery.
[0017] The beneficial effects of this application are as follows: In the lithium-ion battery provided in this application, organic boron ester-based organic boron passivation aids preferentially passivate and adsorb at the interface of high-nickel ternary cathodes, inhibiting the dissolution of transition metals in high-nickel materials and side reactions at the cathode interface. Boron-based lithium salt inorganic boron film-forming aids can construct a dense and flexible boron-containing inorganic-organic composite SEI film on the surface of silicon-carbon anodes, alleviating the film rupture problem caused by the volume expansion of silicon-carbon during charging and discharging. Fluorobenzene-based low-resistance wetting aids improve the wetting ability of the electrolyte on the positive and negative electrode sheets and reduce the interfacial contact resistance. On the other hand, they can participate in the construction of the interfacial film and enhance the ion conductivity of the interfacial film. The three types of aids work together, with organic boron focusing on cathode passivation, inorganic boron focusing on anode film formation, and fluorobenzene taking into account both wetting resistance reduction and interface auxiliary modification. This simultaneously inhibits side reactions and reduces interfacial resistance degradation at both the positive and negative electrode interfaces, laying a material foundation for thermal shock safety and high and low temperature cycling. Furthermore, through extensive prior verification, the inventors discovered that when the mass percentages of inorganic boron film-forming aid in the electrolyte are L%, fluorobenzene low-resistivity wetting aid in the electrolyte are T%, nickel in the positive electrode active material layer are D%, and manganese in the positive electrode active material layer are E%, the optimal concentration of inorganic boron film-forming aid in the electrolyte is 10%. When the mass percentage of silicon in the negative electrode active material layer, F%, satisfies 1.33≤(B+L) / (B*L)≤23.33, 0.014≤(B*L)*100 / (D+0.4*E)≤11.278, and 0.06≤(L+0.6*B+T) / F≤13.90, it can better avoid the increase in electrolyte viscosity and ionic impedance caused by excessive boron-based additives. At the same time, it can prevent the inability to form a complete and stable positive and negative electrode interface film due to insufficient additive content. It balances the risk of thermal decomposition of high-nickel positive electrode, the stability of silicon-carbon negative electrode interface, and electrolyte wetting and transport characteristics. It can reduce the exothermic side reaction at the interface under thermal shock conditions and improve the thermal shock safety performance of the battery. It can also maintain a low interface impedance at low temperature and inhibit the continuous degradation of the interface during high temperature cycling. Thus, it achieves synergistic optimization of thermal shock safety and high and low temperature cycling performance of high-nickel ternary-silicon-carbon lithium-ion battery. Detailed Implementation
[0018] To make the technical problems solved, the technical solutions, and the beneficial effects of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0019] The present invention provides a lithium-ion battery, comprising a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises a positive electrode active material layer, the positive electrode active material layer comprises a nickel-cobalt-manganese ternary positive electrode material, and the negative electrode comprises a negative electrode active material layer, the negative electrode active material layer comprises a silicon-carbon composite material. The electrolyte includes a solvent, a lithium salt, an organoboron passivation aid, an inorganic boron film-forming aid, and a fluorobenzene low-resistance wetting aid. The organoboron passivation aid is an organoborolate ester compound, the inorganic boron film-forming aid is a boron-based lithium salt, and the fluorobenzene low-resistance wetting aid is a fluorobenzene compound. The lithium-ion battery meets the following conditions: 1.33≤(B+L) / (B*L)≤23.33; 0.014≤(B*L)*100 / (D+0.4*E)≤11.278; 0.06≤(L+0.6*B+T) / F≤13.90; Wherein, B% is the mass percentage of the organoboron passivation aid in the electrolyte; L% represents the mass percentage of inorganic boron film-forming aid in the electrolyte; T% represents the mass percentage of fluorobenzene low-resistivity wetting aid in the electrolyte; D% represents the mass percentage of nickel in the positive electrode active material layer; E% represents the mass percentage of manganese in the positive electrode active material layer; F% represents the mass percentage of silicon in the negative electrode active material layer.
[0020] Specifically, in the lithium-ion battery provided in this application, organic boron ester-based organic boron passivation aids preferentially passivate and adsorb at the interface of the high-nickel ternary cathode, inhibiting the dissolution of transition metals in high-nickel materials and side reactions at the cathode interface. Boron-based lithium salt inorganic boron film-forming aids can construct a dense and flexible boron-containing inorganic-organic composite SEI film on the surface of the silicon-carbon anode, alleviating the problem of film rupture caused by the volume expansion of silicon-carbon during charging and discharging. Fluorobenzene-based low-resistance wetting aids improve the wetting ability of the electrolyte on the positive and negative electrode sheets and reduce the interfacial contact resistance. On the other hand, they can participate in the construction of the interfacial film and enhance the ion conduction capacity of the interfacial film. The three types of aids work together, with organic boron focusing on cathode passivation, inorganic boron focusing on anode film formation, and fluorobenzene taking into account both wetting resistance reduction and interface auxiliary modification. This simultaneously inhibits side reactions and reduces interfacial resistance degradation at both the positive and negative electrode interfaces, laying a material foundation for thermal shock safety and high and low temperature cycling. Furthermore, through extensive prior verification, the inventors discovered that when the mass percentages of inorganic boron film-forming aid in the electrolyte are L%, fluorobenzene low-resistivity wetting aid in the electrolyte are T%, nickel in the positive electrode active material layer are D%, and manganese in the positive electrode active material layer are E%, the optimal concentration of inorganic boron film-forming aid in the electrolyte is 10%. When the mass percentage of silicon in the negative electrode active material layer, F%, satisfies 1.33≤(B+L) / (B*L)≤23.33, 0.014≤(B*L)*100 / (D+0.4*E)≤11.278, and 0.06≤(L+0.6*B+T) / F≤13.90, it can better avoid the increase in electrolyte viscosity and ionic impedance caused by excessive boron-based additives. At the same time, it can prevent the inability to form a complete and stable positive and negative electrode interface film due to insufficient additive content. It balances the risk of thermal decomposition of high-nickel positive electrode, the stability of silicon-carbon negative electrode interface, and electrolyte wetting and transport characteristics. It can reduce the exothermic side reaction at the interface under thermal shock conditions and improve the thermal shock safety performance of the battery. It can also maintain a low interface impedance at low temperature and inhibit the continuous degradation of the interface during high temperature cycling. Thus, it achieves synergistic optimization of thermal shock safety and high and low temperature cycling performance of high-nickel ternary-silicon-carbon lithium-ion battery.
[0021] Furthermore, when 1.33≤(B+L) / (B*L)≤23.33, organic boron can construct a rigid CEI film to suppress the dissolution of the positive electrode transition metal, while inorganic boron can form a flexible SEI film to buffer the volume expansion of the silicon-carbon negative electrode. The two achieve a dynamic balance in film strength, without generating additional impedance loss or interface protection defects. If (B+L) / (B*L) > 23.33, the ratio of the two boron additives is unbalanced, and the system is dominated by a single component. If the system contains only organic boron, the anode cannot form a flexible SEI film, and the silicon-carbon anode will experience rapid degradation of cycle performance due to volume expansion. If the system contains only inorganic boron, the CEI passivation effect of the cathode is insufficient, and significant transition metal dissolution occurs in the high-nickel cathode, leading to thermal shock failure. When (B+L) / (B*L) < 1.33, the content of organic boron passivation additive B% and the addition amount of inorganic boron film-forming additive L% are both at high levels, resulting in excessive thickening of the positive and negative electrode interface film, a significant increase in lithium-ion transport impedance, intensified polarization during 0℃ low-temperature cycling, and rapid capacity degradation of the battery.
[0022] When 0.014≤(B*L)*100 / ( D+0.4*E)≤11.278, the material and additive dosage can be matched: the high nickel and low manganese cathode can be matched with a relatively higher total boron dosage of B*L, and the high manganese and low nickel cathode can be matched with a relatively lower boron dosage, achieving a precise match between lattice stability and interface protection effect. There is no ineffective redundancy of additive components, nor is there a problem of missing interface protection. When (B*L)*100 / (D+0.4*E) < 0.014, the overall film-forming activity of the double boron additive is far from sufficient to offset the risk of nickel dissolution in the cathode, the CEI passivation film coverage is insufficient, and side reactions continue to be induced at the microcrack sites of high-nickel particles, resulting in rapid degradation of the battery's high-temperature cycling performance and a low pass rate in the thermal shock test. When (B*L)*100 / (D+0.4*E) > 11.278, the amount of double boron additive added is too high, which will generate a large amount of redundant boron components for the high-manganese stable cathode system. The excess boron species continue to decompose and generate high-resistance byproducts, causing the internal resistance of the whole cell to rise continuously and the low-temperature performance to deteriorate.
[0023] When 0.06≤(L+0.6*B+T) / F≤13.90, the amount of additives can be adaptively matched according to the silicon content of the negative electrode: high silicon negative electrode is adapted to a relatively higher amount of L%, T%, thereby forming a highly elastic SEI film and a low-resistance ion transport channel; low silicon negative electrode will reduce the amount of additives accordingly to suppress side reactions and gas generation. When (L+0.6*B+T) / F < 0.06, the total addition of L%, B%, and T% is insufficient. When the silicon-carbon anode undergoes volume expansion, the SEI film lacks a sufficient boron-oxygen flexible framework to buffer stress, and the interface film continues to crack. At the same time, the system lacks sufficient fluorobenzene to reduce low-temperature impedance, resulting in a significant reduction in the battery's 0℃ cycle life. When (L+0.6*B+T) / F > 13.90, in the anode system with low silicon content, the buffer additive is added in excess. Inorganic boron and fluorobenzene undergo a large amount of decomposition and produce gas. Byproducts continuously accumulate at the electrode interface, which accelerates the degradation of high-temperature cycle performance and reduces the battery's volumetric energy density.
[0024] In some embodiments, the lithium-ion battery satisfies the following conditions: 1.67≤(B+L) / (B*L)≤21.00.
[0025] Specifically, when the lithium-ion battery further satisfies 1.67≤(B+L) / (B*L)≤21.00, the passivation effect of the organic boron positive electrode and the film-forming effect of the inorganic boron negative electrode can achieve an optimal synergistic state. This avoids the abnormal increase in electrolyte viscosity and the obstruction of low-temperature ion conduction caused by excessive total amount of dual-boron additives, ensuring the stability of interface impedance during low-temperature cycling. It also eliminates the defects of insufficient positive electrode passivation and insufficient SEI film integrity caused by imbalanced additive ratios and insufficient content. This limitation further enhances the balance of positive and negative electrode interface protection, significantly reduces the rate of continuous interface degradation under high-temperature cycling, and greatly improves the interface stability during battery thermal shock. It further optimizes the synergistic effect of high and low temperature cycle life and thermal safety performance, making the battery more adaptable to different operating conditions.
[0026] In some embodiments, the lithium-ion battery satisfies the following conditions: 0.022≤(B*L)*100 / (D+0.4*E)≤7.317.
[0027] Specifically, when the lithium-ion battery further satisfies 0.022≤(B*L)*100 / (D+0.4*E)≤7.317, it better achieves precise matching between the amount of boron-based composite additives and the nickel-manganese component content of the high-nickel cathode. Nickel, as the core active component of the high-nickel cathode, has a higher content resulting in higher cathode energy density, but also lower thermal stability and a greater risk of transition metal dissolution. Manganese can moderately stabilize the cathode structure, but abnormal content can affect interfacial activity. This preferred parameter range can precisely match the passivation protection capability of boron-based additives according to the nickel-manganese content of the cathode, effectively solving the problems of increased thermal decomposition side reactions caused by insufficient additives in the high-nickel cathode or increased electrolyte impedance caused by excessive additives in the low-nickel-manganese cathode under a wide parameter range. By precisely matching the cathode material characteristics, it maximizes the suppression of transition metal dissolution and thermally induced interfacial side reactions in the high-nickel cathode, significantly improving the battery's thermal shock safety performance. Simultaneously, it stabilizes the cathode interfacial structure, reducing cathode structural collapse and impedance degradation during high and low temperature cycling, further improving the battery's high and low temperature cycling stability.
[0028] In some embodiments, the lithium-ion battery satisfies the following conditions: 0.12≤(L+0.6*B+T) / F≤11.10.
[0029] Specifically, when the lithium-ion battery further satisfies 0.12≤(L+0.6*B+T) / F≤11.10, the matching optimization of the composite modification capability of the three types of functional additives in the electrolyte and the silicon content of the silicon-carbon anode is achieved. Silicon is the core component that provides high capacity for silicon-carbon anodes. The higher the silicon content, the more severe the volume expansion deformation of the anode during charging and discharging, and the higher the requirements for the flexibility and stability of the SEI film. This optimal range precisely controls the composite dosage of inorganic boron, organic boron, and fluorobenzene additives for anode systems with different silicon contents. This avoids the problems of cycle capacity decay and surge in interfacial impedance caused by insufficient modification capability of additives in high-silicon-content anodes, which leads to the SEI film being unable to adapt to volume expansion, frequent damage and regeneration. It also prevents the excessive accumulation of additives in low-silicon-content anodes, which causes problems such as increased electrolyte viscosity, hindered ion transport, and decreased low-temperature performance. This parameter optimization can stabilize the silicon-carbon anode interface structure, ensure the integrity of the anode interface and ion conduction efficiency under high and low temperature conditions, significantly improve the high and low temperature cycle performance of the battery, and at the same time reduce the side reactions of the overall battery system by stabilizing the anode interface, thus helping to improve the thermal shock safety of the battery.
[0030] In some embodiments, the lithium-ion battery satisfies at least one of the following conditions: (1) 0.1%≤B%≤4%; (2) 0.05% ≤ L% ≤ 1.5%; (3) 1%≤T%≤30%; (4) 20%≤D%≤60%; (5) 3%≤E%≤30%; (6) 1%≤F%≤40%.
[0031] Specifically, the content limit of the organic boron passivation aid (0.1% ≤ B% ≤ 4%) ensures that the positive electrode has basic passivation protection capabilities while avoiding the decrease in electrolyte system stability caused by excessive content; the content range of the inorganic boron film-forming aid (0.05% ≤ L% ≤ 1.5%) meets the basic requirements for the construction of the SEI film of the silicon-carbon anode, preventing film layer loss or aid aggregation; the content range of the fluorobenzene low-resistance wetting aid (1% ≤ T% ≤ 30%) effectively achieves electrolyte wetting modification and interface-assisted film formation, taking into account both wetting resistance reduction and ion conduction optimization; the content limits of nickel (20% ≤ D% ≤ 60%) and manganese (3% ≤ E% ≤ 30%) in the positive electrode are suitable for the composition system of high-nickel ternary positive electrodes, balancing the positive electrode energy density and structural stability; the content range of silicon (1% ≤ F% ≤ 40%) in the anode covers the ratio range of conventional silicon-carbon composite anodes, taking into account both battery capacity and anode structural stability. By limiting the parameters mentioned above, a material system basis is provided for dual-interface synergistic modification, thermal safety and high and low temperature cycling performance optimization, avoiding the impact on performance caused by abnormal content of a single component.
[0032] Furthermore, the mass percentage B% of the organoboron passivation aid in the electrolyte includes, but is not limited to, 0.1%, 0.15%, 0.2%, 0.3%, 0.5%, 1%, 1.5%, 2%, 3%, 3.5%, or 4%; The mass percentage (L%) of the inorganic boron film-forming aid in the electrolyte includes, but is not limited to, 0.05%, 0.06%, 0.08%, 0.1%, 0.125%, 0.25%, 0.3%, 0.5%, 0.8%, 1%, 1.2%, or 1.5%. The mass percentage (T%) of the fluorobenzene low-resistivity wetting aid in the electrolyte includes, but is not limited to, 1%, 1.5%, 2.5%, 3%, 4%, 5%, 10%, 15%, 18%, 20%, 25%, 28%, or 30%. The mass percentage D% of nickel in the positive electrode active material layer includes, but is not limited to, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, or 60%; The mass percentage E% of manganese in the positive electrode active material layer includes, but is not limited to, 3%, 4%, 5%, 10%, 15%, 18%, 20%, 25%, 28%, or 30%. The mass percentage F% of silicon in the negative electrode active material layer includes, but is not limited to, 1%, 1.5%, 2%, 2.5%, 3%, 5%, 6%, 10%, 12%, 15%, 18%, 20%, 24%, 30%, 35%, or 40%.
[0033] In some embodiments, the lithium-ion battery satisfies at least one of the following conditions: (1) 0.5%≤B%≤2%; (2) 0.125%≤L%≤0.75%; (3) 2.5%≤T%≤15%; (4) 30%≤D%≤50%; (5) 5% ≤ E% ≤ 20%; (6) 6%≤F%≤24%.
[0034] Specifically, when the lithium-ion battery further meets one of the above conditions, it is beneficial to improve the battery's thermal shock safety and the stability of its high and low temperature cycling performance.
[0035] Furthermore, the mass percentage B% of the organoboron passivation aid in the electrolyte includes, but is not limited to, 0.5%, 1%, 1.5%, or 2%; The mass percentage (L%) of the inorganic boron film-forming aid in the electrolyte includes, but is not limited to, 0.125%, 0.25%, 0.3%, 0.5%, or 0.75%. The mass percentage (T%) of the fluorobenzene low-resistivity wetting aid in the electrolyte includes, but is not limited to, 2.5%, 3%, 4%, 5%, 10%, or 15%. The mass percentage D% of nickel in the positive electrode active material layer includes, but is not limited to, 30%, 35%, 40%, 45%, or 50%. The mass percentage of manganese in the positive electrode active material layer, E %, includes, but is not limited to, 5%, 10%, 15%, 18%, or 20%. The mass percentage F% of silicon in the negative electrode active material layer includes, but is not limited to, 6%, 10%, 12%, 15%, 18%, 20%, or 24%.
[0036] In some embodiments, the organoboronate compounds include one or more of tris(trimethylsilyl)boronate TMSB, trimethylcycloboronic acid alkyl TMB, and triethylboronate; and / or, The boron-based lithium salt includes one or more of lithium bis(oxalato)borate (LiBOB) and lithium difluorooxalato)borate (LiDFOB); and / or... The fluorobenzene compounds include one or more of fluorobenzene FB, 1,3-difluorobenzene DFB, 1,3,5-trifluorobenzene TFB, and hexafluorobenzene HFB.
[0037] Specifically, the organoboroester compounds include one or more of tris(trimethylsilyl)boronic acid ester, trimethylcycloboroxane, and triethylborate. These compounds have excellent positive electrode interface adsorption characteristics, can uniformly coat the surface of high-nickel ternary positive electrode, block direct contact between the positive electrode and the electrolyte, effectively suppress the dissolution of transition metals and high-temperature thermal decomposition side reactions, and have excellent chemical stability without introducing additional interface impurities. The boron-based lithium salt is selected from one or more of lithium dioxaborate and lithium difluorooxaborate. This type of lithium salt can preferentially decompose on the surface of silicon-carbon anode to form an inorganic flexible SEI film rich in boron. The film has excellent density and flexibility, can adapt to the volume expansion of silicon-carbon anode for a long time, and also has good ion conduction performance. Fluorinated benzenes are selected from one or more of fluorobenzene, difluorobenzene, trifluorobenzene, and hexafluorobenzene. These compounds have strong polarity compatibility, which can quickly improve the wetting effect of the electrolyte on the dense positive and negative electrode sheets, effectively reduce the interfacial contact resistance, and participate in the construction of the interfacial film, optimize the pore structure of the interfacial film, and improve the ion migration efficiency at high and low temperatures.
[0038] In some embodiments, the solvent includes one or more of ethylene carbonate EC, propylene carbonate PC, ethyl propionate EP, propyl propionate PP, dimethyl carbonate DMC, ethyl methyl carbonate EMC, and diethyl carbonate DEC.
[0039] In some embodiments, the lithium salt includes one or more of lithium hexafluorophosphate, lithium bisfluorosulfonylimide, and lithium bistrifluoromethanesulfonylimide; The total molar concentration of the lithium salt in the electrolyte is 0.85 mol / L to 1.5 mol / L.
[0040] Specifically, the lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethanesulfonyl)imide selected above are all lithium salts with high stability and high ionic conductivity. If the above lithium salts are compounded, lithium hexafluorophosphate can ensure the basic ionic conductivity and interface stability of the electrolyte, while lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethanesulfonyl)imide can further improve the ion transport performance at high and low temperatures and suppress the side reactions of lithium salt decomposition at high temperatures.
[0041] Meanwhile, the optimal lithium salt molar concentration range is 0.85 mol / L to 1.5 mol / L. Too low a concentration leads to insufficient electrolyte ion loading, increased interfacial impedance, and deterioration of high and low temperature cycling performance; too high a concentration causes a surge in electrolyte viscosity, hinders ion migration, and easily induces lithium salt precipitation and exacerbates interfacial side reactions. This lithium salt system and concentration limit ensure stable ion conductivity of the electrolyte, adapts to the interfacial modification mechanisms of three types of functional additives, further optimizes the interfacial impedance characteristics of the positive and negative electrodes, avoids intensified electrochemical polarization under high and low temperature conditions, and synergistically improves battery thermal shock safety and high and low temperature cycling stability.
[0042] Another embodiment of the present invention provides an electrical device including the aforementioned lithium-ion battery.
[0043] Specifically, the electrical device includes the lithium-ion battery provided in this application. In the lithium-ion battery provided in this application, organic boron ester-type organic boron passivation aids preferentially passivate and adsorb at the interface of the high-nickel ternary cathode, inhibiting the dissolution of transition metals in high-nickel materials and side reactions at the cathode interface. Boron-based lithium salt inorganic boron film-forming aids can construct a dense and flexible boron-containing inorganic-organic composite SEI film on the surface of the silicon-carbon anode, alleviating the problem of film rupture caused by the volume expansion of silicon-carbon during charging and discharging. Fluorobenzene-type low-resistance wetting aids improve the wetting ability of the electrolyte on the positive and negative electrode sheets and reduce the interfacial contact resistance. On the other hand, they can participate in the construction of the interfacial film and enhance the ion conduction capacity of the interfacial film. The three types of aids work together. Organic boron focuses on cathode passivation, inorganic boron focuses on anode film formation, and fluorobenzene takes into account both wetting resistance reduction and interface auxiliary modification. From the dual interfaces of the positive and negative electrodes, side reactions are suppressed and interfacial resistance degradation is reduced, laying a material basis for thermal shock safety and high and low temperature cycling. Furthermore, through extensive prior verification, the inventors discovered that when the mass percentages of inorganic boron film-forming aid in the electrolyte are L%, fluorobenzene low-resistivity wetting aid in the electrolyte are T%, nickel in the positive electrode active material layer are D%, and manganese in the positive electrode active material layer are E%, the optimal concentration of inorganic boron film-forming aid in the electrolyte is 10%. When the mass percentage of silicon in the negative electrode active material layer, F%, satisfies 1.33≤(B+L) / (B*L)≤23.33, 0.014≤(B*L)*100 / (D+0.4*E)≤11.278, and 0.06≤(L+0.6*B+T) / F≤13.90, it can better avoid the increase in electrolyte viscosity and ionic impedance caused by excessive boron-based additives. At the same time, it can prevent the inability to form a complete and stable positive and negative electrode interface film due to insufficient additive content. It balances the risk of thermal decomposition of high-nickel positive electrode, the stability of silicon-carbon negative electrode interface, and electrolyte wetting and transport characteristics. It can reduce the exothermic side reaction at the interface under thermal shock conditions and improve the thermal shock safety performance of the battery. It can also maintain a low interface impedance at low temperature and inhibit the continuous degradation of the interface during high temperature cycling. Thus, it achieves synergistic optimization of thermal shock safety and high and low temperature cycling performance of high-nickel ternary-silicon-carbon lithium-ion battery.
[0044] The present invention will be further illustrated by the following examples.
[0045] Table 1 Continued from Table 1 Example 1 This embodiment illustrates the lithium-ion battery disclosed in this invention, and includes the following operational steps: Positive electrode preparation Nickel-manganese modified NCM ternary active material, conductive agent Super P, carbon nanotubes, and binder PVDF were mixed at a mass ratio of 95:2:1:2, and NMP solvent was added and stirred to prepare a uniform positive electrode slurry. This slurry was then coated onto a 12μm aluminum foil current collector, dried at 110℃, and rolled to a surface density of 180g / m². 2 The positive electrode is obtained by splitting. In the positive electrode active material layer, the mass percentage of nickel (D%) is 35% and the mass percentage of manganese (E%) is 15%.
[0046] Anode preparation Silicon-carbon composite active material (nano-silicon + graphite), conductive agent acetylene black, CMC thickener, and SBR binder are mixed in a ratio of 94:2:2:2 and stirred with deionized water to prepare a negative electrode slurry; the slurry is coated onto an 8μm copper foil, dried at 80℃, rolled, and slit to obtain the negative electrode; In the negative electrode active material layer, the silicon element mass percentage F% is 18%.
[0047] Electrolyte preparation Preparation in an argon glove box (water and oxygen content <1ppm): 1) Basic carbonate solvent mixture (EC:EMC:DEC = 3:4:3 mass ratio); 2) Add lithium salt LiPF6 and stir until completely dissolved, achieving a molar concentration of 1.0 mol / L; 3) Add the organic boron passivation aid TMSB, the inorganic boron film-forming aid LiDFOB, and the fluorobenzene low-resistance wetting aid FB in sequence, and stir continuously for 2 hours to mix completely to obtain the target electrolyte.
[0048] Lithium-ion battery assembly The positive electrode, PE ceramic separator, and negative electrode are wound in sequence and then aluminum / copper tabs are welded to obtain a bare battery cell. The mixture is encapsulated in an aluminum-plastic film, injected with the prepared electrolyte, and then vacuum-sealed. After standing at 40℃ for 24 hours, the cells were pre-charged at 0.02C for formation, capacity testing, and high-temperature shaping at 45℃ to obtain finished soft-pack batteries with a uniform capacity of 2Ah, which were then used for subsequent performance testing.
[0049] Examples 2-42 Examples 2-42 illustrate the lithium-ion battery disclosed in this invention, including most of the operations in Example 1, except that: In Examples 2-42, B%, organic boron passivation aid, L%, inorganic boron film-forming aid, T%, fluorobenzene low-resistance wetting aid T, D%, E%, F%, and (B+L) / (B*L), (B*L)*100 / (D+0.4*E), (L+0.6*B+T) / F are all based on Table 1.
[0050] Comparative Examples 1-27 Comparative Examples 1-27 are used to illustrate the lithium-ion battery disclosed in this invention, including most of the operations in Example 1, with the following differences: In Comparative Examples 1-27, B%, organic boron passivation aid, L%, inorganic boron film-forming aid, T%, fluorobenzene low-resistance wetting aid T, D%, E%, F%, and (B+L) / (B*L), (B*L)*100 / (D+0.4*E), (L+0.6*B+T) / F are all based on Table 1.
[0051] Performance testing The lithium-ion batteries prepared in Examples 1-42 and Comparative Examples 1-27 were subjected to the following performance tests: Thermal shock test: Fully charged batteries (charged to 4.3V at 1C constant current and constant voltage) are placed in an oven and heated to 130℃ at 5℃ / min and kept at that temperature for 1 hour. Twenty batteries are tested at a time, and the number of batteries that pass without catching fire or exploding is counted. The higher the number, the better the safety.
[0052] 0℃ low temperature cycling: In a constant temperature chamber at 0℃, with 0.5C charging / 1C discharging and a cutoff voltage of 2.75~4.3V, record the number of cycles corresponding to a capacity retention rate decay to 70%.
[0053] 45℃ high-temperature cycling: In a constant temperature chamber at 45℃, with 1C charge / 1C discharge, the number of cycles corresponding to the capacity retention rate decaying to 70% was recorded.
[0054] Volumetric energy density: Measure the cell volume and rated capacity, and calculate Wh / L.
[0055] The test results are entered into Table 2.
[0056] Table 2 Continued from Table 2 As can be seen from the test results in Table 2, among the overall test results of Examples 1-42 and Comparative Examples 1-27 of this application, the test results of Examples 1-42 are significantly better than those of Comparative Examples 1-27. Examples 1-42 all meet the limitations of component selection, parameter range and relationship formula of this application, and have superior comprehensive performance compared with the comparative examples.
[0057] Specifically, in Examples 1-5, the content of the organoboron passivation additive B% was increased from 0.1% to 4.0%. As B% increased from 0.1% to 1%, (B+L) / (B*L) decreased and (B*L)*100 / (D+0.4*E) increased, significantly enhancing the synergistic film-forming effect of the dual boron additives. This effectively optimized the passivation effect of the high-nickel positive electrode and the integrity of the SEI film of the silicon-carbon negative electrode. The number of cells that passed the thermal shock test increased from 11 to 16, and the high and low temperature cycle performance was improved simultaneously. When B% exceeded 2%, the excessive additive caused excessive deposition of the interfacial film and a thicker film layer, resulting in an increase in interfacial impedance and a slight decrease in cycle performance. Among them, Example 3, with B=1%, had the optimal additive ratio, achieving the best balance between positive electrode passivation, negative electrode film formation, and electrolyte ion transport, resulting in the best overall performance of battery thermal safety and high and low temperature cycle performance.
[0058] In Examples 6-10, the content of inorganic boron film-forming aid L% was increased from 0.05% to 1.5%. The experimental results showed that when L% was in the preferred range of 0.125% to 0.75% (Examples 7-9), the parameters (B+L) / (B*L) and (B*L)*100 / (D+0.4*E) fell into the optimal matching range, which could form a complete and flexible boron-containing composite SEI film on the silicon-carbon anode surface, effectively buffering the volume expansion of silicon-carbon. The number of qualified cells in the battery thermal shock could reach more than 15, and the number of high and low temperature cycles could be stably maintained at more than 530 cycles. However, when L% was too low (0.05%), the inorganic boron film-forming component was insufficient, the buffering and protection capacity of the anode interface was lacking, and the interface stability decreased. When L% was too high (1.5%), the excessive inorganic boron aid would increase the overall viscosity of the electrolyte, hinder low-temperature ion transport, and cause a significant decline in the low-temperature performance of the battery.
[0059] In Examples 11-15, the content (T%) of the fluorobenzene low-resistance wetting aid was increased from 1% to 30%. When T% was within the preferred range of 2.5% to 15% (Examples 12-14), the parameter (L+0.6*B+T) / F fell within the optimal matching range. The fluorobenzene aid could fully exert its effects of electrolyte wetting and resistance reduction and interface-assisted modification, significantly reducing the battery interface impedance and improving low-temperature cycling performance. When T% was below 1%, the amount of aid was insufficient, resulting in poor electrolyte wetting effect, high interface impedance, and limited low-temperature cycling performance. When T% was increased to a high content of 30%, excessive fluorobenzene was prone to side reactions and decomposition at the interface, damaging the stability of the interface film and accelerating the high-temperature cycling degradation rate of the battery.
[0060] In Examples 16-20, the nickel mass percentage D% was increased from 20% to 60%. As the nickel content increased, the risk of cathode lattice instability increased, and (B*L)*100 / (D+0.4*E) decreased simultaneously. When the nickel content was in the preferred range of 30%~50% (Examples 17-19), (B*L)*100 / (D+0.4*E) matched the film-forming modification ability of boron-based additives, and the battery could simultaneously achieve both energy density and cycle stability. When the nickel content was too low, the cathode activity was insufficient, resulting in a low battery capacity. When the nickel content was too high, it would exacerbate the destruction of the cathode lattice structure and deteriorate the overall electrochemical performance of the battery.
[0061] In Examples 21-25, the mass percentage of manganese in the positive electrode, E%, was adjusted. As the manganese content increased, the lattice structure of the positive electrode was strengthened, and (B*L)*100 / (D+0.4*E) increased accordingly. When the manganese content was in the preferred range of 5%~20% (Examples 22-24), the lattice stability of the positive electrode and the interface protection effect of the boron-based additives were well matched, and the battery thermal shock safety and cycle performance reached the optimal level. When the manganese content was too high, it would dilute the active components of the positive electrode, causing a decrease in the battery's positive electrode capacity.
[0062] In Examples 26-30, the mass percentage of silicon in the negative electrode, F%, was adjusted within the range of 1% to 40%. As the silicon content in the active material layer of the negative electrode increased, the expansion stress generated by the charging and discharging of the silicon-carbon negative electrode increased, and (L+0.6*B+T) / F decreased simultaneously. When the silicon content was in the preferred range of 6% to 24% (Examples 27-29), the boron-fluorine composite buffer system could adapt to the volume deformation of the negative electrode and achieve a balance between the volumetric energy density and cycle life of the battery. If the silicon content was too low, the energy density of the negative electrode would be insufficient. If the silicon content was too high, the volume expansion of the negative electrode would exceed the tolerance limit of the interface buffer system, resulting in the degradation of battery performance.
[0063] In Examples 31-36, the specific types of organic boron passivation aids, inorganic boron film-forming aids, and fluorobenzene low-resistivity wetting aids in the electrolyte were replaced. The organic boron passivation aids were trimethylcycloborane and triethyl borate, the inorganic boron film-forming aid was lithium bis(oxalato)borate, and the fluorobenzene low-resistivity wetting aids were 1,3-difluorobenzene, 1,3,5-trifluorobenzene, and hexafluorobenzene, respectively. The results showed that after changing the different aids, the number of cells that passed the thermal shock test could reach 16, and the number of cycles at 0°C and 45°C was maintained at around 560 cycles. This verifies that all the aids specified in this application can achieve the synergistic modification effect of the positive and negative electrode interfaces.
[0064] In Examples 37-42, the three sets of relational formulas were set as the upper and lower critical limit values of the range defined in this application, respectively. That is, (B+L) / (B*L) took values of 23.33 and 1.33, (B*L)*100 / (D+0.4*E) took values of 0.014 and 11.278, and (L+0.6*B+T) / F took values of 0.06 and 13.90. The test results showed that although the performance of the examples under the critical conditions was slightly lower than that of the examples within the preferred range, the overall performance was still significantly better than that of each comparative example. This verifies that the parameter range defined in this application has the effect of improving performance, and the preferred parameter range can better achieve the synergistic optimization of thermal shock safety and high and low temperature cycling.
[0065] Comparative Example 1 electrolyte did not contain three types of additives: organic boron passivation aid, inorganic boron film-forming aid, and fluorobenzene low-resistance wetting aid. It lacked boron-based interface protection and fluorinated drag-reducing components. Only 2 particles passed the thermal shock test, and the electrolyte cycled less than 310 times at 0℃ / 45℃, resulting in the worst overall performance.
[0066] Comparative Examples 2-4 lacked one type of additive, relying solely on a single component to function, failing to achieve a synergistic effect. Only 3 particles passed the thermal shock test, resulting in a severe decline in cycle performance.
[0067] Comparative Examples 5 to 7 all showed a deficiency of two functional additives in the electrolyte, which resulted in the failure of the dual boron synergy or boron-fluorine synergy.
[0068] In Comparative Examples 8-13, the amount of any single component of the organic boron passivation aid, inorganic boron film-forming aid, and fluorobenzene low-resistance wetting aid exceeds the limits specified in this application, for example, B%=5%, L%=0.025%, and T%=40%, which can easily lead to a surge in impedance or an aggravation of interfacial side reactions.
[0069] Comparative Examples 14-18 have issues with nickel, manganese, and silicon elements exceeding the specified limits in their negative electrode active material layers, making the negative electrode deformation buffering capacity unsuitable for the boron-fluorine system.
[0070] In Comparative Examples 19-21, the amount of one type of additive among the three additives in the electrolyte was set to 0. Similarly, the synergistic effect of boron and the drag-reducing effect of fluorobenzene could not be exerted.
[0071] Comparative Example 22's (B+L) / (B*L)=30.00 exceeded the upper limit of 23.33, indicating that the overall amount of boron additive was too low, the film protection at the positive and negative electrode interfaces was insufficient, only 8 particles passed the thermal shock test, and the cycle times at 0℃ and 45℃ were only 382 and 412, respectively.
[0072] In Comparative Example 23, the relationship (B+L) / (B*L) = 0.92, which is lower than the lower limit of (B+L) / (B*L) of 1.33, and (B*L)*100 / (D+0.4*E) = 14.634, which is higher than the upper limit of 11.278. The simultaneous excess of organic and inorganic boron additives caused the electrolyte viscosity to increase, the interfacial film to become too thick, the battery internal resistance to increase, the number of cells that passed the thermal shock was 11, and the high and low temperature cycles were only 380 and 410 cycles.
[0073] Comparative Example 24's (B*L)*100 / (D+0.4*E)=0.007, which is lower than the lower limit of 0.014. The boron additive is not matched with the nickel-manganese composition of the cathode, and the passivation effect of inhibiting transition metal dissolution in high-nickel cathode is insufficient. The number of particles that passed the thermal shock test was 7, and the cycles at 0℃ and 45℃ were 379 and 409, respectively.
[0074] The (B*L)*100 / (D+0.4*E) of Comparative Example 25 is 28.302, which is much higher than the upper limit of 11.278. The boron additive is in excess relative to the positive electrode component, and the excessive deposition of the interface film increases the battery impedance. The number of cells that pass the thermal shock is 8, and the high and low temperature cycling further decreases to 375 cycles and 405 cycles.
[0075] Comparative Example 26: (L+0.6*B+T) / F=0.03, which is lower than the lower limit of 0.06. The boron-fluorine composite modification capability is insufficient relative to the silicon content of the negative electrode, and it cannot effectively buffer the volume expansion of the silicon-carbon negative electrode. The SEI film is repeatedly damaged and regenerated. The number of thermal shock passes is 8, and the cycle time is 383 and 413 at 0℃ and 45℃, respectively.
[0076] The (L+0.6*B+T) / F=33.90 of Comparative Example 27 is much higher than the upper limit of 13.90. The total amount of additives is relatively low and the silicon anode is seriously over-supplied, which leads to an aggravation of electrolyte side reactions. The number of particles that pass the thermal shock is 7, and the cycle time at 0℃ and 45℃ is only 378 cycles and 408 cycles, respectively.
[0077] Comparing the test results of the above embodiments and comparative examples, it can be seen that in the lithium-ion battery provided by this application, the organic boron ester-type organic boron passivation aid preferentially undergoes passivation adsorption at the high-nickel ternary cathode interface, inhibiting the dissolution of transition metals in high-nickel materials and side reactions at the cathode interface. The boron-based lithium salt inorganic boron film-forming aid can construct a dense and flexible boron-containing inorganic-organic composite SEI film on the surface of silicon-carbon anode, alleviating the problem of film rupture caused by the volume expansion of silicon-carbon during charging and discharging. The fluorobenzene-type low-resistance wetting aid improves the wetting ability of the electrolyte on the positive and negative electrode sheets and reduces the interfacial contact resistance. On the other hand, it can participate in the construction of the interfacial film and enhance the ion conduction capacity of the interfacial film. The three types of aids work together, with organic boron focusing on cathode passivation, inorganic boron focusing on anode film formation, and fluorobenzene taking into account both wetting resistance reduction and interface auxiliary modification. From the dual interfaces of positive and negative electrodes, side reactions are suppressed and interfacial resistance degradation is reduced, laying a material basis for thermal shock safety and high and low temperature cycling. Furthermore, through extensive prior verification, the inventors discovered that when the mass percentages of inorganic boron film-forming aid in the electrolyte are L%, fluorobenzene low-resistivity wetting aid in the electrolyte are T%, nickel in the positive electrode active material layer are D%, and manganese in the positive electrode active material layer are E%, the optimal concentration of inorganic boron film-forming aid in the electrolyte is 10%. When the mass percentage of silicon in the negative electrode active material layer, F%, satisfies 1.33≤(B+L) / (B*L)≤23.33, 0.014≤(B*L)*100 / (D+0.4*E)≤11.278, and 0.06≤(L+0.6*B+T) / F≤13.90, it can better avoid the increase in electrolyte viscosity and ionic impedance caused by excessive boron-based additives. At the same time, it can prevent the inability to form a complete and stable positive and negative electrode interface film due to insufficient additive content. It balances the risk of thermal decomposition of high-nickel positive electrode, the stability of silicon-carbon negative electrode interface, and electrolyte wetting and transport characteristics. It can reduce the exothermic side reaction at the interface under thermal shock conditions and improve the thermal shock safety performance of the battery. It can also maintain a low interface impedance at low temperature and inhibit the continuous degradation of the interface during high temperature cycling. Thus, it achieves synergistic optimization of thermal shock safety and high and low temperature cycling performance of high-nickel ternary-silicon-carbon lithium-ion battery.
[0078] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A lithium-ion battery, characterized in that, It includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode includes a positive electrode active material layer, which includes a nickel-cobalt-manganese ternary positive electrode material. The negative electrode includes a negative electrode active material layer, which includes a silicon-carbon composite material. The electrolyte includes a solvent, a lithium salt, an organoboron passivation aid, an inorganic boron film-forming aid, and a fluorobenzene low-resistance wetting aid. The organoboron passivation aid is an organoborolate ester compound, the inorganic boron film-forming aid is a boron-based lithium salt, and the fluorobenzene low-resistance wetting aid is a fluorobenzene compound. The lithium-ion battery meets the following conditions: 1.33≤(B+L) / (B*L)≤23.33; 0.014≤(B*L)*100 / (D+0.4*E)≤11.278; 0.06≤(L+0.6*B+T) / F≤13.90; Wherein, B% is the mass percentage of the organoboron passivation aid in the electrolyte; L% represents the mass percentage of inorganic boron film-forming aid in the electrolyte; T% represents the mass percentage of fluorobenzene low-resistivity wetting aid in the electrolyte; D% represents the mass percentage of nickel in the positive electrode active material layer; E% represents the mass percentage of manganese in the positive electrode active material layer; F% represents the mass percentage of silicon in the negative electrode active material layer.
2. The lithium-ion battery according to claim 1, characterized in that, The lithium-ion battery meets the following conditions: 1.67≤(B+L) / (B*L)≤21.
00.
3. The lithium-ion battery according to claim 1, characterized in that, The lithium-ion battery meets the following conditions: 0.022≤(B*L)*100 / (D+0.4*E)≤7.
317.
4. The lithium-ion battery according to claim 1, characterized in that, The lithium-ion battery meets the following conditions: 0.12≤(L+0.6*B+T) / F≤11.
10.
5. The lithium-ion battery according to claim 1, characterized in that, The lithium-ion battery meets at least one of the following conditions: (1)0.1%≤B%≤4%; (2)0.05%≤L%≤1.5%; (3)1%≤T%≤30%; (4)20%≤D%≤60%; (5)3%≤E%≤30%; (6)1%≤F%≤40%。 6. The lithium-ion battery according to claim 1, characterized in that, The lithium-ion battery meets at least one of the following conditions: (1)0.5%≤B%≤2%; (2)0.125%≤L%≤0.75%; (3)2.5%≤T%≤15%; (4)30%≤D%≤50%; (5)5%≤E%≤20%; (6)6%≤F%≤24%。 7. The lithium-ion battery according to claim 1, characterized in that, The organoboronate compounds include one or more of tris(trimethylsilyl)boronate, trimethylcycloboroxane, and triethylborate; and / or, The boron-based lithium salt includes one or more of lithium dioxaborate and lithium difluorooxaborate; and / or... The fluorobenzene compounds include one or more of fluorobenzene, 1,3-difluorobenzene, 1,3,5-trifluorobenzene, and hexafluorobenzene.
8. The lithium-ion battery according to claim 1, characterized in that, The solvent includes one or more of ethylene carbonate, propylene carbonate, ethyl propionate, propyl propionate, dimethyl carbonate, methyl ethyl carbonate, and diethyl carbonate.
9. The lithium-ion battery according to claim 1, characterized in that, The lithium salt includes one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethanesulfonyl)imide; The total molar concentration of the lithium salt in the electrolyte is 0.85 mol / L to 1.5 mol / L.
10. An electrical device, characterized in that, The lithium-ion battery includes any one of claims 1 to 9.