A sulfide solid electrolyte and its preparation method

By controlling the composition of Li2S, P2S5, and LiI and performing a two-stage heat treatment process of first low temperature and then high temperature, a sulfide solid electrolyte with both high ion conductivity and air stability is formed, which solves the problem of performance in existing technologies and improves the adaptability of the material for engineering applications.

CN123120899APending Publication Date: 2026-11-17NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611374240.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing sulfide solid electrolytes, while maintaining good ion conductivity, have difficulty simultaneously improving air stability, resulting in strict environmental control requirements during preparation, storage, transportation, and battery assembly, which limits their engineering applications.

Method used

By using Li2S, P2S5 and LiI to regulate the composition, an amorphous precursor was formed by mechanical ball milling. Then, a two-stage heat treatment, first at low temperature and then at high temperature, was performed to form a thio-LISICON II related phase with high ion conductivity and a Li4PS4I related phase with good air stability.

Benefits of technology

This approach achieves improved air stability of the material while maintaining high ion conductivity, reduces performance degradation caused by environmental moisture, lowers environmental control requirements during preparation, storage, transportation, and assembly of all-solid-state lithium batteries, and improves adaptability for engineering applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of solid electrolyte technology, specifically to a sulfide solid electrolyte and its preparation method. The invention obtains a sulfide solid electrolyte by controlling the LiI content in the Li₂S-P₂S₅-LiI system and subjecting the mechanically ball-milled amorphous precursor to two-stage heat treatments at low and high temperatures. This preparation method is advantageous in balancing the material's ion conductivity and air stability, reducing H₂S release under humid air, and improving the retention of ion conductivity after exposure to humid air, making it suitable for all-solid-state lithium batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solid electrolyte technology, specifically relating to a sulfide solid electrolyte and its preparation method. Background Technology

[0002] All-solid-state lithium batteries possess high safety and energy density potential, making them a crucial development direction for next-generation energy storage technology. Solid electrolytes, as key materials in all-solid-state lithium batteries, must perform lithium-ion transport within the battery; their ion conductivity directly impacts the battery's rate performance and operating efficiency. Furthermore, solid electrolytes undergo processes such as preparation, storage, transportation, and battery assembly, thus their stability in the air directly affects processing conditions and practical application costs. Sulfide solid electrolytes exhibit high room-temperature ionic conductivity and good cold-pressing properties, showing significant application potential. However, they are sensitive to environmental moisture, easily hydrolyzing and releasing H2S in humid air, potentially accompanied by a decrease in ion conductivity, thus imposing high requirements on production and usage environments.

[0003] To address the air stability issue of sulfide solid electrolytes, existing technologies have proposed various solutions, such as surface coating and composite modification. For example, CN116072961B discloses a core-shell sulfide solid electrolyte, using a sulfide solid electrolyte as the core and forming a shell of lithium halide compounds on its surface to reduce the contact between the internal sulfide solid electrolyte and humid air. In a specific embodiment of this patent, a Li7P2S8I sulfide solid electrolyte is first prepared, and then a shell containing LiCl and LiI is formed on its surface through subsequent processing, thereby reducing the degree of hydrolysis of the material in humid air. In addition to the above methods, there are also technical routes in the art to improve the air stability of sulfide solid electrolytes through material composites, surface modification, and environmental isolation.

[0004] However, for practical applications of sulfide solid electrolytes, simply improving air stability is insufficient to meet usage requirements; the material also needs to maintain good lithium-ion conductivity. Existing sulfide solid electrolytes and their modification methods generally face the challenge of simultaneously achieving good ion conductivity and air stability: some materials exhibit good ion conductivity but are sensitive to humid air; some modification methods can improve the material's tolerance to environmental moisture, but the material's inherent ion transport performance still needs to be considered. This inherent performance conflict necessitates strict environmental control during the preparation, storage, transportation, and battery assembly of sulfide solid electrolytes, thus limiting their further engineering applications.

[0005] Therefore, improving the air stability of sulfide solid electrolytes while maintaining their good ion conductivity, and reducing hydrolysis, H2S release, and performance degradation caused by humid air, are urgent problems to be solved in the further application of sulfide solid electrolytes. Developing sulfide solid electrolytes and their preparation methods that can balance these two aspects is of great significance for reducing the environmental control requirements of materials and improving their practical application value. Summary of the Invention

[0006] To address the shortcomings of existing technologies, this invention proposes a sulfide solid electrolyte and its preparation method. Through compositional control and a two-stage heat treatment process, this invention provides an innovative solution that balances ion conductivity and air stability.

[0007] The first objective of this invention is achieved through the following technical solution:

[0008] A method for preparing a sulfide solid electrolyte includes the following steps:

[0009] (1) According to Li 6+x P2S8I x Li2S, P2S5 and LiI were weighed in stoichiometric ratios, where 1.2≤x≤1.8. Li2S, P2S5 and LiI were mechanically ball-milled to obtain an amorphous precursor.

[0010] (2) Place the amorphous precursor obtained in step (1) under an inert atmosphere or perform vacuum encapsulation;

[0011] (3) The amorphous precursor in step (2) is subjected to a first-stage heat treatment at a temperature of 175~185℃ and a holding time of 1.5~2.5 hours to obtain an intermediate product.

[0012] (4) The intermediate product obtained in step (3) is subjected to a second stage heat treatment. The temperature of the second stage heat treatment is 225~235℃ and the holding time is 0.5~1.5 hours to obtain sulfide solid electrolyte.

[0013] Preferably, in step (1), 1.35≤x≤1.50.

[0014] Preferably, in step (1), the purity of Li2S, P2S5 and LiI is not less than 99%.

[0015] Preferably, in step (1), the rotation speed of the mechanical ball mill is 200~600 rpm.

[0016] More preferably, the rotational speed of the mechanical ball mill is 400~600 rpm.

[0017] Preferably, in step (1), the mechanical ball milling time is 4 to 48 hours.

[0018] More preferably, the mechanical ball milling time is 10 to 20 hours.

[0019] Preferably, in step (1), the mass ratio of balls to material in the mechanical ball mill is (10~60):1.

[0020] More preferably, the ball-to-material mass ratio of the mechanical ball mill is (10~20):1.

[0021] Preferably, in step (1), ball milling and static cooling are alternated during the mechanical ball milling process.

[0022] More preferably, the single ball milling time is 5 to 30 minutes, and the static cooling time between two adjacent ball milling sessions is 5 to 30 minutes.

[0023] More preferably, the single ball milling time is 10-20 minutes, and the static cooling time between two adjacent ball milling sessions is 10-20 minutes.

[0024] Preferably, in step (1), the mechanical ball milling is performed using a planetary ball mill.

[0025] Preferably, in step (1), the mechanical ball mill uses zirconia balls or alumina balls as the milling medium.

[0026] Preferably, in step (1), the amorphous precursor is a completely amorphous precursor.

[0027] Preferably, in step (1), the weighing of Li2S, P2S5 and LiI and the mechanical ball milling are carried out in an inert atmosphere.

[0028] More preferably, the inert atmosphere is an argon atmosphere or a nitrogen atmosphere.

[0029] Preferably, in step (2), the sintering container is a crucible or a quartz tube.

[0030] Preferably, in step (2), when an inert atmosphere is used for protection, the inert atmosphere is argon or nitrogen.

[0031] Preferably, in step (2), when vacuum sealing is used, the vacuum level is not higher than 10 Pa.

[0032] More preferably, in step (2), when vacuum sealing is used, the vacuum degree is not higher than 10 Pa.

[0033] Preferably, in step (3), the temperature of the first stage heat treatment is 178~182℃ and the holding time is 1.8~2.2 hours.

[0034] Preferably, in step (3), the heating rate of the first stage heat treatment is 0.5~5℃ / min.

[0035] More preferably, the heating rate of the first stage heat treatment is 1~3℃ / min.

[0036] Preferably, step (4) is performed immediately after step (3). After the first stage of heat treatment is completed, the intermediate product is not cooled to room temperature, but the temperature is continued to rise and the second stage of heat treatment is performed.

[0037] Preferably, in step (4), the temperature of the second stage heat treatment is 228~232℃, and the holding time is 0.8~1.2 hours.

[0038] Preferably, in step (4), the heating rate of the second stage heat treatment is 0.5~5℃ / min.

[0039] More preferably, the heating rate of the second stage heat treatment is 1~3℃ / min.

[0040] Preferably, the heat treatment in steps (3) and (4) is carried out in a muffle furnace or a tube furnace.

[0041] Preferably, after the second stage of heat treatment in step (4) is completed, the obtained product is naturally cooled to room temperature.

[0042] Preferably, the product after natural cooling is ground, and the grinding is carried out under an inert atmosphere.

[0043] More preferably, the grinding method is mechanical grinding or manual grinding.

[0044] In a further preferred embodiment, when using manual grinding, grinding continues until the product forms a uniform powder, with a grinding time of 5 to 30 minutes.

[0045] This scheme employs a continuous preparation route involving compositional control of Li₂S, P₂S₅, and LiII, mechanical ball milling to form amorphous precursors, and a first-stage heat treatment followed by a second-stage heat treatment. Mechanical ball milling forms amorphous precursors from the raw materials, providing a material basis for phase evolution during subsequent heat treatment. Introducing LiI into the Li₂S-P₂S₅ system facilitates the formation of lithium-ion migration channels. The first-stage heat treatment promotes the formation and stabilization of the thio-LISICON II configuration-related phase with high ion conductivity. The second-stage heat treatment further promotes the formation of the Li₄PS₄I-related phase and the regulation of the microstructure of the two phases in the material. The low-temperature-then-high-temperature treatment sequence ensures that the highly conductive phase formed in the first stage retains its ion transport function while the phase continues to evolve in the second stage. Simultaneously, it allows the phase with good air stability to participate in material structure regulation, thus avoiding the problems of insufficient air stability when using only low-temperature heat treatment and reduced ion conductivity when using only high-temperature heat treatment. This results in a sulfide solid electrolyte that balances ion conductivity and air stability. The above mechanism is an explanation of the technical route of the present invention and does not require a specific spatial distribution of crystal phase as a necessary prerequisite for the implementation of this preparation method.

[0046] The second objective of this invention is achieved through the following technical solution:

[0047] A sulfide solid electrolyte is prepared by the above-described preparation method.

[0048] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0049] 1. This invention employs a two-stage heat treatment process, first at a low temperature and then at a high temperature, allowing the first and second stages of heat treatment to play different roles. This approach helps to improve the air stability of the material while maintaining high ion conductivity, thereby achieving a balance between the ion conductivity and air stability of the sulfide solid electrolyte.

[0050] 2. The first-stage heat treatment of the present invention is conducive to the formation and stabilization of the thio-LISICON II related phase with high ion conductivity. This structure is beneficial to broaden the three-dimensional migration channel of lithium ions and reduce the binding of lithium ion migration, thereby improving the room temperature ion conductivity of the sulfide solid electrolyte.

[0051] 3. The second-stage heat treatment of this invention facilitates the formation of a Li4PS4I related phase with good air stability. This related phase can form hydration products with barrier effects after contact with ambient moisture, which helps to increase the resistance to moisture migration into the material interior, reduce the hydrolysis of sulfide electrolytes and H2S release, and improve the retention rate of ionic conductivity after exposure to humid air.

[0052] 4. This invention involves subjecting the same amorphous precursor to two sequential heat treatment stages, which facilitates the synergistic effect of the related phase with higher ion conductivity and better air stability within the same material system, thereby further improving the overall performance of the sulfide solid electrolyte. This effect is significantly superior to materials obtained through simple mechanical mixing.

[0053] 5. The sulfide solid electrolyte obtained by this invention can reduce the performance degradation caused by environmental moisture while maintaining good lithium-ion conductivity. This is beneficial to reducing the requirements for environmental control conditions during the preparation, storage, transportation and assembly of all-solid-state lithium batteries, and improving the engineering application adaptability of the sulfide solid electrolyte. Detailed Implementation

[0054] The following will provide a clear and complete description of the concept, specific structure, and technical effects of the present invention in conjunction with embodiments, so as to fully understand the purpose, solution, and effects of the present invention. It should be noted that, unless otherwise specified, the embodiments and features described in the embodiments of the present invention can be combined with each other.

[0055] The materials used in the embodiments and comparative examples of this invention are described below:

[0056] Li2S: Purity ≥ 99%, Manufacturer: Alfa Aesar, Grade: 12136-58-2;

[0057] P2S5: Purity ≥ 99%, Manufacturer: Aladdin, Brand: 1314-80-3;

[0058] LiI: Purity above 99%, Manufacturer: Aladdin, Brand: 10377-51-2.

[0059] Example 1

[0060] Li in Example 1 7.4 P2S8I 1.4 The preparation method of sulfide solid electrolytes includes the following steps:

[0061] (1) Under an argon atmosphere, according to Li 7.4 P2S8I 1.4 Li₂S, P₂S₅, and LiI were weighed in stoichiometric proportions and loaded into a planetary ball mill jar with zirconia balls at a ball-to-material mass ratio of 10:1. The ball mill speed was set to 500 rpm, and the milling process was carried out for a total of 15 hours by alternating between 15 minutes of ball milling and 15 minutes of static cooling to obtain a completely amorphous precursor.

[0062] (2) The amorphous precursor obtained in step (1) is loaded into a quartz tube, and the quartz tube is evacuated to below 10 Pa before vacuum sealing.

[0063] (3) Place the quartz tube sealed in step (2) into a muffle furnace, heat it to 180°C at a heating rate of 2°C / min, perform the first stage of heat treatment and keep it at the temperature for 2 hours to obtain the intermediate product.

[0064] (4) After the first stage of heat treatment, the temperature was directly increased to 230°C at a heating rate of 2°C / min for the second stage of heat treatment and held at that temperature for 1 hour. After the second stage of heat treatment, the product was naturally cooled to room temperature, removed under an argon atmosphere, and ground under an argon atmosphere for 20 minutes to obtain the Li from Example 1. 7.4 P2S8I 1.4 Sulfide solid electrolyte.

[0065] Example 2

[0066] Li in Example 2 7.2 P2S8I 1.2 The preparation method of sulfide solid electrolytes includes the following steps:

[0067] (1) Under an argon atmosphere, according to Li 7.2 P2S8I 1.2 Li₂S, P₂S₅, and LiI were weighed in stoichiometric proportions and loaded into a planetary ball mill jar with zirconia balls at a ball-to-material mass ratio of 10:1. The ball mill speed was set to 500 rpm, and the milling process was carried out for a total of 15 hours by alternating between 15 minutes of ball milling and 15 minutes of static cooling to obtain a completely amorphous precursor.

[0068] (2)-(4) are performed according to steps (2)-(4) of Example 1 to obtain Li of Example 2. 7.2 P2S8I 1.2 Sulfide solid electrolyte.

[0069] Example 3

[0070] Li in Example 3 7.3 P2S8I 1.3 The preparation method of sulfide solid electrolytes includes the following steps:

[0071] (1) Under an argon atmosphere, according to Li 7.3 P2S8I 1.3 Li₂S, P₂S₅, and LiI were weighed in stoichiometric proportions and loaded into a planetary ball mill jar with zirconia balls at a ball-to-material mass ratio of 10:1. The ball mill speed was set to 500 rpm, and the milling process was carried out for a total of 15 hours by alternating between 15 minutes of ball milling and 15 minutes of static cooling to obtain a completely amorphous precursor.

[0072] (2)-(4) are carried out according to steps (2)-(4) of Example 1 to obtain Li of Example 3. 7.3 P2S8I 1.3 Sulfide solid electrolyte.

[0073] Example 4

[0074] Li in Example 4 7.35 P2S8I 1.35 The preparation method of sulfide solid electrolytes includes the following steps:

[0075] (1) Under an argon atmosphere, according to Li 7.35 P2S8I 1.35 Li₂S, P₂S₅, and LiI were weighed in stoichiometric proportions and loaded into a planetary ball mill jar with zirconia balls at a ball-to-material mass ratio of 10:1. The ball mill speed was set to 500 rpm, and the milling process was carried out for a total of 15 hours by alternating between 15 minutes of ball milling and 15 minutes of static cooling to obtain a completely amorphous precursor.

[0076] (2)-(4) are carried out according to steps (2)-(4) of Example 1 to obtain Li of Example 4. 7.35 P2S8I 1.35 Sulfide solid electrolyte.

[0077] Example 5

[0078] Example 5 L i7.5 P2S8I 1.5 The preparation method of sulfide solid electrolytes includes the following steps:

[0079] (1) Under an argon atmosphere, according to Li 7.5 P2S8I 1.5 Li₂S, P₂S₅, and LiI were weighed in stoichiometric proportions and loaded into a planetary ball mill jar with zirconia balls at a ball-to-material mass ratio of 10:1. The ball mill speed was set to 500 rpm, and the milling process was carried out for a total of 15 hours by alternating between 15 minutes of ball milling and 15 minutes of static cooling to obtain a completely amorphous precursor.

[0080] (2)-(4) are carried out according to steps (2)-(4) of Example 1 to obtain Li of Example 5. 7.5 P2S8I 1.5 Sulfide solid electrolyte.

[0081] Example 6

[0082] Example 6 L i7.5 7P2S8I 1.57 The preparation method of sulfide solid electrolytes includes the following steps:

[0083] (1) Under an argon atmosphere, according to L i7.5 7P2S8I 1.57 Li₂S, P₂S₅, and LiI were weighed in stoichiometric proportions and loaded into a planetary ball mill jar with zirconia balls at a ball-to-material mass ratio of 10:1. The ball mill speed was set to 500 rpm, and the milling process was carried out for a total of 15 hours by alternating between 15 minutes of ball milling and 15 minutes of static cooling to obtain a completely amorphous precursor.

[0084] (2)-(4) are carried out according to steps (2)-(4) of Example 1 to obtain L of Example 6. i7.5 7P2S8I 1.57 Sulfide solid electrolyte.

[0085] Example 7

[0086] Li in Example 7 7.6 P2S8I 1.6 The preparation method of sulfide solid electrolytes includes the following steps:

[0087] (1) Under an argon atmosphere, according to Li 7.6 P2S8I 1.6 Li₂S, P₂S₅, and LiI were weighed in stoichiometric proportions and loaded into a planetary ball mill jar with zirconia balls at a ball-to-material mass ratio of 10:1. The ball mill speed was set to 500 rpm, and the milling process was carried out for a total of 15 hours by alternating between 15 minutes of ball milling and 15 minutes of static cooling to obtain a completely amorphous precursor.

[0088] (2)-(4) are performed according to steps (2)-(4) of Example 1 to obtain Li of Example 7. 7.6 P2S8I 1.6 Sulfide solid electrolyte.

[0089] Example 8

[0090] Li in Example 8 7.64 P2S8I 1.64 The preparation method of sulfide solid electrolytes includes the following steps:

[0091] (1) Under an argon atmosphere, according to Li 7.64 P2S8I 1.64 Li₂S, P₂S₅, and LiI were weighed in stoichiometric proportions and loaded into a planetary ball mill jar with zirconia balls at a ball-to-material mass ratio of 10:1. The ball mill speed was set to 500 rpm, and the milling process was carried out for a total of 15 hours by alternating between 15 minutes of ball milling and 15 minutes of static cooling to obtain a completely amorphous precursor.

[0092] (2)-(4) were performed according to steps (2)-(4) of Example 1 to obtain Li of Example 8. 7.64 P2S8I 1.64 Sulfide solid electrolyte.

[0093] Example 9

[0094] Li in Example 9 7.7 P2S8I 1.7 The preparation method of sulfide solid electrolytes includes the following steps:

[0095] (1) Under an argon atmosphere, according to Li 7.7 P2S8I 1.7 Li₂S, P₂S₅, and LiI were weighed in stoichiometric proportions and loaded into a planetary ball mill jar with zirconia balls at a ball-to-material mass ratio of 10:1. The ball mill speed was set to 500 rpm, and the milling process was carried out for a total of 15 hours by alternating between 15 minutes of ball milling and 15 minutes of static cooling to obtain a completely amorphous precursor.

[0096] (2)-(4) were performed according to steps (2)-(4) of Example 1 to obtain Li of Example 9. 7.7 P2S8I 1.7 Sulfide solid electrolyte.

[0097] Example 10

[0098] Li in Example 10 7.8 P2S8I 1.8 The preparation method of sulfide solid electrolytes includes the following steps:

[0099] (1) Under an argon atmosphere, according to Li 7.8 P2S8I 1.8 Li₂S, P₂S₅, and LiI were weighed in stoichiometric proportions and loaded into a planetary ball mill jar with zirconia balls at a ball-to-material mass ratio of 10:1. The ball mill speed was set to 500 rpm, and the milling process was carried out for a total of 15 hours by alternating between 15 minutes of ball milling and 15 minutes of static cooling to obtain a completely amorphous precursor.

[0100] (2)-(4) are carried out according to steps (2)-(4) of Example 1 to obtain Li of Example 10. 7.8 P2S8I 1.8 Sulfide solid electrolyte.

[0101] Comparative Example 1

[0102] The preparation method of the Li7P2S8I sulfide solid electrolyte of Comparative Example 1 includes the following steps:

[0103] (1) Under an argon atmosphere, Li2S, P2S5, and LiI were weighed according to the stoichiometric ratio of Li7P2S8I. The raw materials and zirconia balls were loaded into a planetary ball mill jar with a ball-to-material mass ratio of 10:1. The ball mill speed was set to 500 rpm, and the ball milling was carried out for a total of 15 h by alternating between 15 min of ball milling and 15 min of static cooling to obtain a completely amorphous precursor.

[0104] (2)-(4) were carried out according to steps (2)-(4) of Example 1 to obtain the Li7P2S8I sulfide solid electrolyte of Comparative Example 1.

[0105] Comparative Example 2

[0106] The preparation method of the Li4PS4I sulfide solid electrolyte of Comparative Example 2 includes the following steps:

[0107] (1) Under an argon atmosphere, Li2S, P2S5, and LiI were weighed according to the stoichiometric ratio of Li4PS4I. The raw materials and zirconia balls were loaded into a planetary ball mill jar with a ball-to-material mass ratio of 10:1. The ball mill speed was set to 500 rpm, and the ball milling was carried out for a total of 15 h by alternating between ball milling for 15 min and static cooling for 15 min, to obtain a completely amorphous precursor.

[0108] (2)-(4) were carried out according to steps (2)-(4) of Example 1 to obtain the Li4PS4I sulfide solid electrolyte of Comparative Example 2. Comparative Example 1 and Comparative Example 2 correspond to the compositional comparisons on both sides of the existing compositional range, respectively.

[0109] Comparative Example 3

[0110] Comparative Example 3 Li 7.4 P2S8I 1.4 The preparation method of sulfide solid electrolytes includes the following steps:

[0111] (1)-(2) Follow the steps (1)-(2) of Example 1 to obtain a vacuum-encapsulated amorphous precursor.

[0112] (3) The quartz tube sealed in step (2) was placed in a muffle furnace and heated to 180°C at a heating rate of 2°C / min and held for 3 hours. After the heat treatment, it was naturally cooled to room temperature, and post-processed according to the product removal and grinding method in step (4) of Example 1 to obtain Li of Comparative Example 3. 7.4 P2S8I 1.4 Sulfide solid electrolyte.

[0113] Comparative Example 4

[0114] Comparative Example 4 Li 7.4 P2S8I 1.4The preparation method of sulfide solid electrolytes includes the following steps:

[0115] (1)-(2) Follow the steps (1)-(2) of Example 1 to obtain a vacuum-encapsulated amorphous precursor.

[0116] (3) The quartz tube sealed in step (2) was placed in a muffle furnace and heated directly to 230°C at a heating rate of 2°C / min and held at that temperature for 3 hours. After the heat treatment, it was naturally cooled to room temperature, and post-processed according to the product removal and grinding method in step (4) of Example 1 to obtain Li of Comparative Example 4. 7.4 P2S8I 1.4 Sulfide solid electrolyte.

[0117] Comparative Example 5

[0118] Comparative Example 5 Li 7.4 P2S8I 1.4 The preparation method of sulfide solid electrolytes includes the following steps:

[0119] (1)-(2) Follow the steps (1)-(2) of Example 1 to obtain a vacuum-encapsulated amorphous precursor.

[0120] (3) Place the quartz tube sealed in step (2) into a muffle furnace, heat it to 230°C at a heating rate of 2°C / min and hold it for 1 hour to obtain the intermediate product.

[0121] (4) The intermediate product obtained in step (3) was cooled to 180°C at a cooling rate of 2°C / min and held at that temperature for 2 hours. After the heat treatment, it was naturally cooled to room temperature, and post-processed according to the product extraction and grinding method in step (4) of Example 1 to obtain Li from Comparative Example 5. 7.4 P2S8I 1.4 Sulfide solid electrolyte.

[0122] Comparative Example 6

[0123] The preparation method of the sulfide solid electrolyte of Comparative Example 6 includes the following steps:

[0124] (1) Weigh out the Li prepared in Comparative Example 3 at a molar ratio of 60:40. 7.4 P2S8I 1.4 Sulfide solid electrolyte and Li prepared in Comparative Example 4 7.4 P2S8I 1.4 Sulfide solid electrolyte.

[0125] (2) The two sulfide solid electrolytes weighed in step (1) are mechanically mixed by manual grinding until they are evenly mixed to obtain the sulfide solid electrolyte of Comparative Example 6.

[0126] The performance of the sulfide solid electrolytes prepared in Examples 1-10 and Comparative Examples 1-6 was tested, and the results are shown in Table 1. The test methods are as follows:

[0127] Room temperature ionic conductivity testing method: 150 mg of sulfide solid electrolyte powder was weighed in a glove box and placed into a ceramic sleeve with an inner diameter of 10 mm. The sleeve was fixed using stainless steel molds at the top and bottom. A single-axis hydraulic press was used to press the electrolyte sheet into a 10 mm diameter sheet under a pressure of 20 MPa, and the actual thickness L of the electrolyte sheet was measured. Room temperature ionic conductivity was tested using an AC impedance meter at 25℃. The frequency range covering the impedance response of the electrolyte sheet was scanned, and the AC disturbance voltage was kept within the linear response range. The impedance R of the electrolyte sheet was determined based on the intercept of the high-frequency end of the impedance spectrum with the real axis. The room temperature ionic conductivity was calculated using σ = L / (R × S), where σ is the room temperature ionic conductivity, L is the thickness of the electrolyte sheet, R is the impedance of the electrolyte sheet, and S is the cross-sectional area of ​​the electrolyte sheet. The same testing equipment and parameters were used for all samples.

[0128] H2S release test method: Accurately weigh 150 mg of sulfide solid electrolyte and place it in a 2400 cm³ container. 3 In a sealed container, the temperature was controlled at 25°C and the relative humidity at 35%. A calibrated H2S gas detector with a range and accuracy meeting the requirements for the measured concentration was used to detect H2S in the sealed container; the same detector and settings were used for all samples. The sulfide solid electrolyte was exposed to the above environment for 60 minutes, and the volume concentrations C0 and C2 of H2S gas were recorded at the start of exposure and at 60 minutes. 60 (Unit: ppm), and according to V H2S =(C 60 -C0)×2400×10⁻ 6 The total volume of H2S released within 60 minutes, V, was calculated. H2S According to Q=V H2S The H2S release is calculated per m, where Q is the H2S release amount in cm³. 3 / g, V H2S The total volume of H2S released within 60 minutes, in cm³. 3 , where m is the mass of the sulfide solid electrolyte, in g.

[0129] Method for testing the retention rate of ionic conductivity after exposure to humid air: Accurately weigh 150 mg of sulfide solid electrolyte and expose it for 60 min in an environment with a temperature of 25℃ and a relative humidity of 35%, according to the H2S release test method described above. After exposure, recover the sulfide solid electrolyte powder and use it entirely for tableting. Following the room temperature ionic conductivity test method described above, re-press it into electrolyte tablets with a diameter of 10 mm under a pressure of 20 MPa. During testing, measure the actual thickness of the electrolyte tablets and use the same testing equipment and parameters as before exposure. Measure the room temperature ionic conductivity before humid air exposure as σ0, and the room temperature ionic conductivity after humid air exposure as σ1. Calculate the ionic conductivity retention rate using η = σ1 / σ0 × 100%.

[0130] Table 1. Performance test results of sulfide solid electrolytes prepared in Examples 1-10 and Comparative Examples 1-6

[0131] As shown in Table 1, the sulfide solid electrolyte prepared by this invention can balance ion conductivity and air stability. Examples 1-10 used the same ball milling and two-stage heat treatment conditions, only changing the Li... 6+x P2S8I x The x-values ​​obtained all indicate that the materials can achieve lithium-ion conduction. When the LiI content is within an appropriate range, a good balance can be achieved between room temperature ionic conductivity, H2S release, and ionic conductivity retention after exposure to humid air. Compared with the examples, Comparative Examples 1 and 2 used compositions outside the scope of this invention, and the overall performance of the obtained materials decreased, indicating that controlling the LiI content is beneficial for balancing the ionic conductivity and air stability of sulfide solid electrolytes.

[0132] Comparing Example 1 and Comparative Example 3, it can be seen that when only the first-stage low-temperature heat treatment is performed, the resulting material still exhibits good ion conductivity, but its air stability decreases. This indicates that the subsequent second-stage high-temperature heat treatment is beneficial for further improving the material's stability in humid air environments. Comparing Example 1 and Comparative Example 4, it can be seen that when only the second-stage high-temperature heat treatment is performed, although the resulting material exhibits a certain degree of air stability, its ion conductivity significantly decreases. This indicates that the first-stage low-temperature heat treatment is beneficial for maintaining good ion conductivity. Therefore, performing the first-stage low-temperature heat treatment and the second-stage high-temperature heat treatment sequentially can better balance the aforementioned two aspects of performance.

[0133] By comparing Example 1 and Comparative Example 5, it can be seen that when the material composition, the two heat treatment temperatures, the holding time of each stage and the total holding time are kept consistent, the ion conduction performance and air stability of the obtained material decrease when the heat treatment sequence is changed from low temperature first and then high temperature to high temperature first and then low temperature. This indicates that the two-stage heat treatment sequence of low temperature first and then high temperature is more conducive to obtaining better comprehensive performance.

[0134] By comparing Example 1 and Comparative Example 6, it can be seen that the ion conductivity and air stability of the sulfide solid electrolyte obtained by mechanically mixing the sulfide solid electrolytes obtained by low-temperature heat treatment and high-temperature heat treatment are lower than those of the material obtained by sequentially performing two-stage heat treatment on the same amorphous precursor. This indicates that using the same amorphous precursor and sequentially performing two-stage heat treatment, first at low temperature and then at high temperature, is more conducive to obtaining a sulfide solid electrolyte that has both ion conductivity and air stability.

[0135] In summary, this invention controls Li 6+x P2S8I x By controlling the LiI content in the precursor and subjecting the same amorphous precursor to two-stage heat treatment (low temperature and high temperature), a sulfide solid electrolyte with good ionic conductivity and air stability was obtained. Compared with materials outside the composition range, materials subjected to only single-stage heat treatment, materials obtained by reversing the two-stage heat treatment sequence, and materials obtained by mechanical mixing, this material exhibits better overall performance in terms of room temperature ionic conductivity, H2S release, and ionic conductivity retention after exposure to humid air. This indicates that the control of LiI content and the two-stage heat treatment (low temperature followed by high temperature) have a good synergistic effect, which is beneficial to improving the overall performance of the sulfide solid electrolyte.

[0136] The specific embodiments described herein are merely illustrative of the technical concept of the present invention. Those skilled in the art to which this invention pertains may make various modifications, additions, or similar substitutions to the described specific embodiments without departing from the spirit of the invention and the scope defined by the appended claims.

Claims

1. A method for preparing a sulfide solid electrolyte, characterized in that, Includes the following steps: (1) According to Li 6+x P2S8I x Li₂S, P₂S₅, and LiI were weighed in stoichiometric ratios, where 1.2 ≤ x ≤ 1.

8. The Li₂S, P₂S₅, and LiI were then mechanically ball-milled to obtain an amorphous precursor. (2) Place the amorphous precursor obtained in step (1) under an inert atmosphere or perform vacuum encapsulation; (3) The amorphous precursor in step (2) is subjected to a first-stage heat treatment at a temperature of 175~185℃ and a holding time of 1.5~2.5 hours to obtain an intermediate product. (4) The intermediate product obtained in step (3) is subjected to a second stage heat treatment. The temperature of the second stage heat treatment is 225~235℃ and the holding time is 0.5~1.5 hours to obtain sulfide solid electrolyte.

2. A method for preparing a sulfide solid electrolyte as described in claim 1, characterized in that, In step (1), the rotation speed of the mechanical ball mill is 200~600 rpm.

3. A method for preparing a sulfide solid electrolyte as described in claim 1, characterized in that, In step (1), the mechanical ball milling time is 4 to 48 hours.

4. A method for preparing a sulfide solid electrolyte as described in claim 1, characterized in that, In step (1), the mass ratio of balls to material in the mechanical ball mill is (10~60):

1.

5. A method for preparing a sulfide solid electrolyte as described in claim 1, characterized in that, In step (3), the heating rate of the first stage heat treatment is 0.5~5℃ / min; and / or, in step (4), the heating rate of the second stage heat treatment is 0.5~5℃ / min.

6. A method for preparing a sulfide solid electrolyte as described in claim 1, characterized in that, In step (2), when the inert atmosphere is used for protection, the gas in the inert atmosphere is any one or two of argon and nitrogen.

7. A method for preparing a sulfide solid electrolyte as described in claim 1, characterized in that, In step (2), when using the vacuum sealing method, the vacuum level is not higher than 10 Pa.

8. A method for preparing a sulfide solid electrolyte as described in claim 1, characterized in that, In step (1), during the mechanical ball milling process, ball milling and static cooling are performed alternately.

9. A method for preparing a sulfide solid electrolyte as described in claim 8, characterized in that, The single ball milling time is 5~30 minutes, and the static cooling time between two adjacent ball milling sessions is 5~30 minutes.

10. A sulfide solid electrolyte, characterized in that, It is prepared by the preparation method described in claim 1.