Electrolytes for zinc-air batteries and their preparation methods, zinc-air batteries and their regeneration methods and energy storage systems
The electrolyte for zinc-air batteries, which forms an ultra-dense three-dimensional network structure through synchronous coordination crosslinking reaction, solves the problems of insufficient mechanical properties, easy embrittlement at low temperatures, and easy swelling under alkaline conditions of traditional hydrogel electrolytes in zinc-air batteries, and achieves excellent ion conduction performance and stability over a wide temperature range.
Patent Information
- Application Number
- CN202611222504.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-12
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional hydrogel electrolytes have insufficient mechanical properties in zinc-air batteries, are prone to embrittlement at low temperatures, and are prone to swelling under alkaline conditions, which limits their application in a wide temperature range.
By neutralizing water-soluble olefinic unsaturated monomers with alkaline substances, and through the synchronous coordination and crosslinking reaction between metal ion crosslinking agents (such as Zr4+ and/or Hf4+) and polymer chains, an ultra-dense three-dimensional network structure is formed, which improves mechanical strength, low-temperature stability, and anti-swelling properties.
It achieves excellent ion conduction performance across the entire temperature range, solving the problems of insufficient mechanical properties, easy embrittlement at low temperatures, and easy swelling under alkaline conditions of traditional hydrogel electrolytes, thus broadening the application range of zinc-air batteries.
Smart Images

Figure CN123120992A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of zinc-air battery preparation technology, and in particular to an electrolyte for zinc-air batteries and its preparation method, a zinc-air battery and its regeneration method, and an energy storage system. Background Technology
[0002] Hydrogels, as a class of three-dimensional network materials formed by crosslinking hydrophilic polymers, have attracted widespread attention in fields such as flexible electronics, biomedicine, and energy storage devices due to their unique high water content, good biocompatibility, and structural tunability. In the field of zinc-air batteries, hydrogel electrolytes are considered an ideal alternative to traditional liquid alkaline electrolytes because they combine the shape stability of solid electrolytes with the high ionic conductivity of liquid electrolytes. However, the practical application of traditional hydrogels in zinc-air batteries still faces many key performance bottlenecks, severely limiting their further promotion. First, the mechanical properties of existing hydrogel electrolytes are insufficient. Traditional hydrogels typically have a loosely structured, randomly formed cross-linked network with weak intermolecular forces, resulting in generally poor tensile strength, elongation at break, and fatigue resistance. When used as an electrolyte in zinc-air batteries, localized stresses caused by zinc dendrite growth and volume changes during battery assembly and long-term cycling can easily lead to electrolyte membrane rupture or even structural collapse, failing to meet the basic requirements of battery mechanical stability.
[0003] Secondly, the performance degradation at low temperatures is a significant issue. The large amount of free water in traditional hydrogels easily freezes into ice crystals at low temperatures. The growth of these ice crystals disrupts the integrity of the polymer network structure, leading to embrittlement, cracking, and loss of elasticity in the hydrogel. This causes a sharp decline in electrolyte performance when zinc-air batteries are used in low-temperature environments or frigid regions, severely limiting their application in a wide temperature range.
[0004] Furthermore, the swelling and structural instability issues in alkaline systems cannot be ignored. The electrolyte environment of zinc-air batteries is strongly alkaline (typically a 6 M KOH solution). Traditional hydrophilic hydrogel networks readily absorb excessive electrolyte in such high-concentration alkaline solutions, leading to rapid volume expansion, a significant decrease in mechanical properties, and even network disintegration or dissolution. This makes it impossible to maintain stable structure and performance during long-term battery operation. Traditional strategies to improve swelling resistance typically involve increasing the density of chemical crosslinks or introducing hydrophobic segments, but these methods often sacrifice ionic conductivity, making it difficult to achieve a balance between swelling resistance and ionic conductivity.
[0005] Therefore, in order to address the key technical problems of traditional hydrogel electrolytes in zinc-air battery applications, such as insufficient mechanical properties, easy embrittlement at low temperatures, and easy swelling under alkaline conditions, it is of great technical value and practical significance to develop a hydrogel electrolyte material that can simultaneously improve the above-mentioned performance defects and is suitable for the alkaline working environment of zinc-air batteries. Summary of the Invention
[0006] This application discloses an electrolyte for zinc-air batteries and its preparation method, a zinc-air battery and its regeneration method, and an energy storage system, in order to solve the technical problems of insufficient mechanical strength, poor low-temperature stability, and easy swelling of hydrogels in related technologies.
[0007] To solve the above problems, this application adopts the following technical solution: In a first aspect, this application provides a method for preparing an electrolyte for zinc-air batteries, comprising the following steps: At least some of the carboxyl groups in a water-soluble olefinic unsaturated monomer are neutralized by an alkaline substance, wherein the molar ratio of the alkaline substance to the water-soluble olefinic unsaturated monomer is (0.5-1.5):1; A water-soluble olefinic unsaturated monomer, neutralized with an alkaline substance, an initiator, a metal ion crosslinking agent, and a reaction promoter are mixed in water and subjected to a polymerization and crosslinking reaction to obtain a hydrogel polymer. The hydrogel polymer is soaked in a first alkaline solution to obtain an electrolyte for zinc-air batteries; The metal ion crosslinking agent contains zirconium ions and / or hafnium ions, and the molar ratio of the metal ions in the metal ion crosslinking agent to the water-soluble olefinic unsaturated monomer is (0.3-5):1.
[0008] Secondly, this application provides an electrolyte for zinc-air batteries prepared by the preparation method described in the first aspect.
[0009] Thirdly, this application provides a zinc-air battery, including a zinc anode, an air cathode, and an electrolyte disposed between the zinc anode and the air cathode, wherein the electrolyte is obtained by the preparation method described in the first aspect; or, the electrolyte is the electrolyte for zinc-air batteries described in the second aspect.
[0010] Fourthly, this application provides a method for regenerating a zinc-air battery, comprising the following steps: Provide the zinc-air battery as described in the third aspect; The hydrogel electrolyte in the zinc-air battery is removed and immersed in a second alkaline solution to restore the electrolyte's ion conduction properties. The regenerated electrolyte is reassembled between the zinc anode and the air cathode to complete battery regeneration.
[0011] Fifthly, this application provides an energy storage system including at least one zinc-air battery as described in the third aspect.
[0012] The technical solutions adopted in the embodiments of this application can achieve the following beneficial effects: The method for preparing electrolyte for zinc-air batteries provided in this application provides the following beneficial effects: The method for preparing electrolyte for zinc-air batteries provided in this application involves, during the preparation of the hydrogel polymer, ensuring that the metal ions in the metal ion crosslinking agent are in excess relative to the water-soluble olefinic unsaturated monomer, wherein Zr... 4+ and / or Hf 4+ On the one hand, it coordinates with carboxyl groups on polymer chains to form crosslinking nodes; on the other hand, it coordinates with water molecules to form bonded water. During the polymerization and crosslinking process, metal ions act as both in-situ formed crosslinking nodes and a network framework, forming an ultra-dense three-dimensional network structure with a nano-confinement effect. This simultaneously improves the mechanical properties, low-temperature embrittlement, and swelling under alkaline conditions inherent in traditional hydrogel electrolytes used in zinc-air batteries, while maintaining excellent ion conductivity across the entire temperature range. Specifically: (1) The method for preparing the electrolyte for zinc-air batteries provided in this application involves simultaneous in-situ polymerization and metal coordination crosslinking reactions in the same system during the preparation of the hydrogel polymer. This differs from the traditional two-step method of metal ion crosslinking gels (firstly, a polymer network is formed by polymerization of monomers and chemical crosslinking agents, and then the polymer is immersed in a metal ion solution for secondary coordination crosslinking). The simultaneous crosslinking method ensures that the metal coordination crosslinking points are evenly distributed in the polymer network, avoiding the structural inhomogeneity problem of high surface crosslinking density and low internal crosslinking density in the traditional two-step method, thereby forming a three-dimensional network with uniform structure and high density distribution of crosslinking points. Specifically, during the preparation of the hydrogel polymer, the water-soluble olefinic unsaturated monomer is neutralized with an alkaline substance beforehand, so that the carboxyl group (-COOH) in the monomer is converted into a carboxylate group (-COO). - ), thereby obtaining Zr 4+ / Hf 4+ The ability of metal ions to undergo coordination chelation reactions; if not neutralized, the carboxyl group exists as a free acid, which reacts with Zr. 4+ / Hf 4+ The coordination ability of Zr is extremely weak, making it difficult to form a stable coordination cross-linking network. Furthermore, because the metal ions are in excess relative to the monomer, each Zr... 4+ and / or Hf 4+ Zr can coordinate with multiple carboxylate groups simultaneously. 4+On the one hand, metal ions coordinate with carboxylate groups on polymer chains to form crosslinking nodes; on the other hand, they coordinate with water molecules to form bonded water. Metal ions not only act as crosslinking nodes between polymer chains but also serve as the dominant framework of the network structure. During polymerization, monomers polymerize to form polymer chains, which in turn interact with metal ions and functional groups (such as carboxylate groups -COO). - The coordination and crosslinking of metals are carried out simultaneously, achieving a high-density and uniform distribution of metal coordination and crosslinking points. The crosslinking density of the resulting hydrogel is significantly higher than that of traditional organic chemical crosslinking hydrogels, forming an ultra-dense three-dimensional network structure with nano-confinence effect. This structure can maintain stable structural morphology and mechanical properties in alkaline zinc-air battery environment and effectively resist the erosion of the network skeleton by strong alkaline electrolyte.
[0013] (2) The preparation method of the electrolyte for zinc-air batteries provided in this application benefits from the nano-confinement effect generated by the ultra-high density cross-linked network of the hydrogel polymer. Water molecules are confined in the nanoscale network grid, and almost all free water molecules are transformed into bonded water molecules (non-frozen water), which fundamentally inhibits the formation and growth of ice crystals. Therefore, the hydrogel can withstand ultra-low temperature environments of ≤-91.8℃ and still maintain flexibility. Under conditions of ≤-40℃, it can still maintain mechanical strength and toughness close to that at room temperature. It effectively solves the low-temperature stability problem of traditional hydrogel electrolytes in low-temperature environments or cold regions, which is caused by the freezing of free water, resulting in embrittlement, cracking, and loss of elasticity. This broadens the application range of zinc-air batteries in wide temperature range scenarios.
[0014] (3) The method for preparing the electrolyte for zinc-air batteries provided in this application embodiment forms a dense three-dimensional constrained structure by the ultra-high density metal coordination crosslinking network of the hydrogel polymer, which effectively limits the excessive penetration of water molecules into the polymer network and the excessive expansion of the network. The hydrogel of this zinc-air battery electrolyte exhibits excellent anti-swelling performance in alkaline solution environment. After soaking in deionized water or alkaline solution for 500 days, the volume change is ≤0.5%. It can maintain stable structure and mechanical properties for a long time under alkaline working conditions of zinc-air batteries, overcoming the defects of traditional hydrogel electrolytes such as easy excessive swelling, volume expansion, and network disintegration in alkaline systems, and ensuring the long-term cycle stability of the battery.
[0015] (4) The method for preparing the electrolyte for zinc-air batteries provided in this application provides a hydrogel polymer with an ultra-high density cross-linked structure that imparts highly uniform stress transmission and dissipation capabilities to the polymer network. This hydrogel can withstand 99% compressive strain without structural damage, with a compressive strength ≥69MPa and a toughness ≥6MJ·cm. -3It combines high strength and high toughness. The ultra-high density dynamic cross-linked metal structure enables the network to efficiently dissipate external energy. During the assembly and long-term cycling of zinc-air batteries, it can effectively resist local stress caused by factors such as zinc dendrite growth and volume changes, solving the problems of insufficient mechanical strength and poor fatigue resistance of traditional hydrogel electrolytes.
[0016] (5) In the method for preparing the electrolyte for zinc-air batteries provided in the embodiments of this application, when preparing the hydrogel polymer, metal ions are present in excess, and the excess Zr 4+ On the one hand, it coordinates with carboxyl groups on polymer chains to form high-density cross-linking nodes; on the other hand, it coordinates with water molecules to form bonded water. These two factors work synergistically to construct ion transport channels that run throughout the entire network. The average ionic conductivity of this hydrogel at 25°C was 471.69 mS·cm⁻¹, and even at an extreme low temperature of -65°C, its average ionic conductivity remained at 24.15 mS·cm⁻¹. -1 It maintains excellent ion conduction performance over a wide temperature range, enabling it to adapt to the operating requirements of zinc-air batteries under different temperature conditions, and giving the electrolyte potential for application in low-temperature energy storage, flexible zinc-air batteries and other fields. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 In Example 1-1, 'a' is a photograph of a large-area hydrogel with a length of 70cm, a width of 50cm, and a thickness of 1cm. Figure 1 b in Figure 1 a photo of the small pieces of hydrogel after they have been cut and packaged; Figure 2 In this context, 'a' is a scanning electron microscope image of the hydrogel (LMDC-gel) prepared in Example 1-1 of this application; Figure 2 b in the figure is a scanning electron microscope image of the hydrogel (PAA-gel) prepared in Comparative Example 1-1; Figure 2 c in the diagram is a scanning electron microscope image of the hydrogel (MDC-gel) prepared in Examples 1-2; Figure 3 In this context, 'a' represents the k2-weighted χ(k) oscillation spectrum of the LMDC-gel and its fitting curve. Figure 3 In this context, b represents the radial distance of the LMDC-gel, specifically the EXAFS spectrum in R space and its fitting result. Figure 3 In the figure, c is the two-dimensional wavelet transform contour plot of the Zr site EXAFS signal of the LMDC-gel hydrogel; Figure 4 These are one-dimensional SAXS spectra of PAA-gel, MDC-gel, and LMDC-gel; Figure 5 These are two-dimensional SAXS spectra of PAA-gel, MDC-gel, and LMDC-gel; Figure 6 In this figure, 'a' represents the LF-NMR T2 relaxation spectra of three hydrogels: PAA-gel, MDC-gel, and LMDC-gel. Figure 6 In this context, b represents the room-temperature Raman spectra of PAA-gel, MDC-gel, and LMDC-gel. Figure 6 In this context, c represents the low-temperature (-65℃) Raman spectra of PAA-gel, MDC-gel, and LMDC-gel; Figure 6 In this context, d represents the DSC curves of PAA-gel, MDC-gel, and LMDC-gel. Figure 6 In the figure, 'e' represents the swelling kinetics curves of PAA-gel, MDC-gel, and LMDC-gel. Figure 6 The "f" in the image is a comparison photo of LMDC-gel hydrogel after being soaked in deionized water for 500 days. Figure 7 In the image, 'a' is a photograph of an LMDC-gel that maintains its structural integrity even after being subjected to 99% compressive strain. Figure 7 In this context, b represents the compressive stress-strain curves of PAA-gel, MDC-gel, and LMDC-gel. Figure 7 In the figure, 'c' is a comparison of the compressive modulus and compressive toughness of three hydrogels: PAA-gel, MDC-gel, and LMDC-gel. Figure 7 In this context, d represents the tensile stress-strain curves of PAA-gel, MDC-gel, and LMDC-gel. Figure 7 In the diagram, 'e' represents the rheological frequency scan of PAA-gel, MDC-gel, and LMDC-gel. Figure 7f in the figure is a comparison of the wide temperature range tensile modulus of PAA-gel, MDC-gel, and LMDC-gel; Figure 8 This is a schematic diagram illustrating the differences in network structures between LMDC-gel, MDC-gel, and PAA-gel, showing the correlation between crosslinking density, pore size, water state, and macroscopic properties; Figure 9 This is a schematic diagram comparing the solvent confinement states of LMDC-gel, MDC-gel, and PAA-gel, showing the differences in the existence state of the solvent inside the network; Figure 10 This is a schematic diagram comparing the network structure changes and energy dissipation mechanisms of LMDC-gel and PAA-gel under external force. Figure 11 In the figure, A represents a comparison of the specific capacities of LMDC-ZABs at different temperatures and PAA-ZABs at 25℃. Figure 11 In the figure, B represents the discharge polarization curves and corresponding power density diagrams of LMDC-ZABs at different temperatures and PAA-ZABs at 25℃. Figure 11 C in the figure represents the rate performance of LMDC-ZABs at different current densities at a temperature of -65℃. Figure 11 D in the figure represents the Arrhenius plot of the ionic conductivity of LMDC-gel obtained in Example 1-1 and PAA-gel obtained in Comparative Example 1-1. Figure 11 E in the figure represents the constant current charge-discharge cycle curve of LMDC-ZABs at -65℃ and 0.2mA·cm-2. Figure 11 F in the figure represents the number of strong hydrogen bonds in the systems of LMDC-gel, MDC-gel, and PAA-gel obtained from molecular simulation statistics at 25℃ and -65℃. Figure 11 G in the figure represents a comparison of the hydrogen bond lifetimes of LMDC-gel, MDC-gel, and PAA-gel at 25°C. Figure 11 The H in the figure represents a comparison of the hydrogen bond lifetimes of LMDC-gel, MDC-gel, and PAA-gel at -65℃. Figure 12 These are low-temperature optical microscope images of LMDC-gel (A), MDC-gel (B), and PAA-gel (C) at -40℃. Detailed Implementation
[0019] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions of this application will be described in detail below. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of them. Based on the embodiments in this application, all other implementation methods obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0020] The terms "first," "second," etc., used in the specification and claims of this application are used to distinguish similar objects and not to describe a specific order or sequence. It should be understood that such use of data can be interchanged where appropriate so that embodiments of this application can be implemented in orders other than those illustrated or described herein, and the objects distinguished by "first," "second," etc., are generally of the same class and the number of objects is not limited; for example, a first object can be one or more. Furthermore, in the specification and claims, "and / or" indicates at least one of the connected objects, and the character " / " generally indicates that the preceding and following objects are in an "or" relationship.
[0021] In related technologies, the cross-linked networks of traditional hydrogels are mostly randomly formed, loose structures with weak intermolecular forces. Their tensile strength, elongation at break, and fatigue resistance are generally poor, making them prone to cracking, deformation, and even structural collapse under external pressure, stretching, or friction. Furthermore, the large amount of free water in traditional hydrogels easily freezes into ice crystals at low temperatures. The growth of ice crystals disrupts the integrity of the polymer network structure, leading to embrittlement, cracking, and loss of elasticity, making it impossible to maintain stable physical properties and structural state in low-temperature environments. In addition, the hydrophilic network of traditional hydrogels easily absorbs excessive water in aqueous solutions, causing rapid volume expansion, a significant decrease in mechanical properties, and even network disintegration and dissolution. This makes it difficult to maintain stable structure and properties when in contact with aqueous solutions or in high-humidity environments. These technical problems—insufficient mechanical strength, poor low-temperature stability, and easy swelling—severely restrict the industrial promotion and technological application of traditional hydrogels.
[0022] The inventive concept of this application lies in the fact that, unlike the conventional approach in which the crosslinking agent in hydrogels prepared by traditional methods serves only as a linking point between polymer chains and its molar amount is much lower than that of the monomer, this application uses zirconium (Zr) 4+ ) and / or hafnium (Hf 4+ Metal ions are used as crosslinking agents, resulting in an excess of metal ions. To achieve effective coordination between these metal ions and the polymer chain, this application pre-neutralizes the water-soluble olefinically unsaturated monomer with an alkaline substance, converting the carboxyl groups (-COOH) in the monomer into carboxylate groups (-COO₂). - ), thereby obtaining Zr 4+ / Hf 4+The ability to undergo coordination chelation reactions; if not neutralized, the carboxyl group exists as a free acid, which reacts with Zr. 4+ / Hf 4+ Zr has extremely weak coordination ability, making it difficult to form a stable coordination crosslinking network. During the polymerization and crosslinking process, the polymerization of monomers to form polymer chains and the coordination crosslinking of these polymer chains by metal ions occur simultaneously: Zr 4+ / Hf 4+ On the one hand, it coordinates with carboxylate groups generated on the polymer chain to form high-density cross-linking nodes, constituting a three-dimensional network framework; on the other hand, some Zr... 4+ / Hf 4+ Coordination with water molecules transforms free water within the network into bonded water, lowering the freezing point of water and maintaining unobstructed ion conduction channels at low temperatures. The synergistic effect of these two coordination modes allows metal ions to construct an ultra-dense network framework while simultaneously endowing the system with excellent mechanical properties and low-temperature ion conductivity, resulting in an ultra-dense network structure with a cross-linking density far exceeding that of conventional systems. This ultra-dense network induces a nanoscale confinement effect, promoting the transformation of free water molecules into bonded water molecules. Consequently, zinc-air batteries assembled using this electrolyte exhibit excellent mechanical properties, low-temperature antifreeze performance, and anti-swelling properties, while maintaining high ion conductivity across the entire temperature range, effectively overcoming the inherent shortcomings of traditional hydrogel electrolytes in zinc-air battery applications.
[0023] Based on this, this application provides an electrolyte for zinc-air batteries prepared by the above-described method, a zinc-air battery containing the electrolyte, a method for regenerating the zinc-air battery, and an energy storage system. The following provides a detailed description of the electrolyte for zinc-air batteries, its preparation method, the zinc-air battery, its regeneration method, and the energy storage system provided in this application.
[0024] In a first aspect, this application provides a method for preparing an electrolyte for zinc-air batteries, comprising the following steps: At least some of the carboxyl groups in a water-soluble olefinically unsaturated monomer are neutralized using an alkaline substance, wherein the molar ratio of the alkaline substance to the water-soluble olefinically unsaturated monomer is (0.5–1.5):1; during the neutralization reaction, the carboxyl groups (-COOH) in the water-soluble olefinically unsaturated monomer are converted into carboxylate groups (-COO₂) under the action of the alkaline substance. - This allows the monomer to acquire the ability to undergo coordination chelation reactions with the metal ions. Without neutralization, the carboxyl groups in the monomer exist as free acids, which react with Zr... 4+ / Hf 4+ Its coordination ability is extremely weak, making it difficult to form a stable coordination cross-linking network.
[0025] A water-soluble olefinic unsaturated monomer, neutralized with an alkaline substance, an initiator, a metal ion crosslinking agent, and a reaction promoter are mixed in a solvent and subjected to a polymerization and crosslinking reaction to obtain a hydrogel polymer. The hydrogel polymer was soaked in an alkaline solution to obtain an electrolyte for zinc-air batteries. The metal ion crosslinking agent comprises zirconium ions and / or hafnium ions, and the molar ratio of the metal ions in the metal ion crosslinking agent to the water-soluble olefinic unsaturated monomer is (0.3-5):1. At this ratio, the metal ions are in excess relative to the monomer. Unlike conventional hydrogels where the crosslinking agent only acts as a "bridge" between polymer chains and is present in trace amounts relative to the monomer, the use of excess metal ions in this application serves two purposes: First, each metal ion has multiple coordination sites, allowing it to coordinate with carboxyl groups on multiple polymer chains simultaneously, resulting in an order-of-magnitude increase in the number of crosslinking points and the formation of an ultra-dense three-dimensional network framework. Second, the excess metal ions in the system coordinate with water molecules, converting free water within the network into bonded water, lowering the freezing point of water, and maintaining unobstructed ion conduction channels at low temperatures. The synergistic effect of these two coordination modes allows the metal ions to construct an ultra-dense network framework while simultaneously endowing the system with excellent low-temperature ion conduction properties, thus overcoming the shortcomings of conventional hydrogels, such as the crosslinking agent only acting as an inter-chain connection point, low crosslinking density, low-temperature brittleness, and easy swelling.
[0026] It is understood that during the polymerization and crosslinking reaction in this application, the polymerization reaction of the water-soluble olefinic unsaturated monomer and the crosslinking reaction of the polymer chain by the metal ions occur simultaneously in the mixed system. Specifically, under the action of the initiator and the reaction promoter, the monomer molecules form the polymer backbone through free radical chain polymerization; at the same time, the carboxylate group (-COO) generated on the polymer chain... - Synchronization and Zr in the system 4+ / Hf 4+ Metal ions undergo coordination chelation reactions, Zr 4+ / Hf 4+ Metal ions coordinate with carboxyl groups on polymer chains to form high-density cross-linking nodes, connecting multiple polymer chains together to form a three-dimensional network framework; on the other hand, some Zr... 4+ / Hf 4+ Metal ions coordinate with water molecules to form hydrated ion clusters, which connect with surrounding water molecules through hydrogen bonds. This converts free water within the network into bonded water, lowering the freezing point of water and maintaining unobstructed ion conduction channels at low temperatures. The polymerization and crosslinking reactions are completed simultaneously in situ within the same reaction system and at the same temperature, eliminating the need for stepwise polymerization followed by crosslinking. This simplifies the preparation process and improves the uniformity of crosslinking node distribution.
[0027] It is understood that soaking the hydrogel polymer in an alkaline solution allows ions in the alkaline solution to fully diffuse into the interior of the hydrogel polymer network, endowing the hydrogel polymer with ion conductivity and transforming it from a hydrophilic polymer network into an electrochemically active electrolyte for zinc-air batteries.
[0028] In some embodiments, the polymerization and crosslinking reaction is carried out at room temperature for a period of 10 minutes to 5 hours. The system generates free radicals at room temperature without external heating, thus allowing the polymerization and crosslinking reaction to proceed at room temperature. For example, the polymerization and crosslinking reaction time can be controlled at 10 minutes, 20 minutes, 30 minutes, 1 hour, 2 hours, 3 hours, 4 hours, or 5 hours.
[0029] In a preferred embodiment, the polymerization and crosslinking reaction is carried out at room temperature for a period of 10 minutes to 1 hour. It is understood that with near equimolar matching of the oxidant and reducing agent, and a moderate rate of free radical generation, the polymerization and crosslinking reaction can be essentially completed within 10 minutes to 1 hour, resulting in a gel network structure with excellent mechanical properties. Controlling the reaction time to within 10 minutes to 1 hour helps to shorten the preparation cycle and improve preparation efficiency while ensuring gel performance.
[0030] In some embodiments, when an alkaline substance is used to neutralize a water-soluble olefinically unsaturated monomer, the molar ratio of the alkaline substance to the water-soluble olefinically unsaturated monomer is (0.8-1):1. In a more preferred embodiment, the molar ratio of the alkaline substance to the water-soluble olefinically unsaturated monomer is 1:1. It is understood that the amount of alkaline substance used determines the degree of neutralization of the carboxyl groups in the water-soluble olefinically unsaturated monomer. Taking acrylic acid as an example, when the molar ratio of the alkaline substance (such as KOH) to acrylic acid is 1:1, the carboxyl groups (-COOH) in the acrylic acid are completely neutralized to carboxylate groups (-COO). - At this point, all carboxyl groups are in a deprotonated state and can react with Zr. 4+ / Hf 4+ Metal ions undergo coordination chelation reactions, thereby maximizing the number of crosslinking sites and contributing to the formation of a three-dimensional network structure with the highest crosslinking density. For example, the molar ratio of the alkaline substance to the water-soluble olefinic unsaturated monomer can be controlled at 0.8:1, 0.9:1, or 1:1.
[0031] In some embodiments, the alkaline substance is an alkali metal hydroxide. Alkali metal hydroxides (such as potassium hydroxide or sodium hydroxide) completely dissociate upon dissolution in water, providing hydroxide ions to neutralize the carboxyl groups of the monomer, while simultaneously releasing alkali metal ions (K... + Or Na + It does not participate in coordination reactions and will not react with Zr. 4+While they compete with each other, they do not interfere with subsequent cross-linking processes. Potassium hydroxide and sodium hydroxide play the same role in this application, both converting the carboxyl groups of acrylic acid or methacrylic acid into carboxylate groups. Both potassium and sodium ions are non-coordinating cations and do not occupy coordination positions for metal ions in aqueous solutions, thus not affecting Zr. 4+ Coordination crosslinking with carboxylate groups causes interference. The choice between potassium hydroxide and sodium hydroxide has no substantial impact on the final hydrogel network structure.
[0032] In some embodiments, during the polymerization crosslinking reaction, the molar ratio of the metal ions in the metal ion crosslinking agent to the water-soluble olefinic unsaturated monomer is (0.5–2):1. For example, the molar ratio of the metal ions to the water-soluble olefinic unsaturated monomer can be controlled at 0.5:1, 0.8:1, 1:1, 1.2:1, 1.5:1, or 2:1.
[0033] In some embodiments, during the polymerization and crosslinking reaction, the molar ratio of the initiator to the water-soluble olefinically unsaturated monomer is (0.0001–0.05):1. Within this range, the polymerization reaction proceeds at a moderate rate, resulting in high monomer conversion and a complete gel network structure with stable mechanical properties.
[0034] In some embodiments, during the polymerization crosslinking reaction, the molar ratio of the initiator to the water-soluble olefinic unsaturated monomer is (0.0003–0.05):1.
[0035] For example, the molar ratio of the initiator to the water-soluble olefinic unsaturated monomer can be controlled at 0.0003:1, 0.001:1, 0.003:1, 0.005:1, 0.01:1, 0.02:1, 0.03:1, 0.04:1 or 0.05:1.
[0036] In some embodiments, during the polymerization and crosslinking reaction, the molar ratio of the reaction promoter to the water-soluble olefinic unsaturated monomer is (0.0001 to 0.05):1.
[0037] In some embodiments, during the polymerization and crosslinking reaction, the molar ratio of the reaction promoter to the water-soluble olefinic unsaturated monomer is (0.0003 to 0.05):1.
[0038] For example, the molar ratio of the reaction promoter to the water-soluble olefinic unsaturated monomer can be controlled at 0.0003:1, 0.001:1, 0.003:1, 0.005:1, 0.01:1, 0.02:1, 0.03:1, 0.04:1 or 0.05:1.
[0039] In some embodiments, the molar ratio of the initiator to the reaction promoter in the polymerization crosslinking reaction is (0.8 to 1.2):1.
[0040] In some embodiments, the molar ratio of the initiator to the reaction promoter in the polymerization crosslinking reaction is (0.9–1.2):1.
[0041] In this application, the initiator (oxidant) and reaction accelerator (reducing agent) constitute a redox initiation system. When the amounts of both are nearly equimolarly matched, the rate of free radical generation is moderate and sustainable, the polymerization reaction proceeds smoothly, the system temperature does not rise sharply due to excessive exothermic reaction, and the resulting gel structure is uniform, transparent, and bubble-free. If the exothermic reaction is too concentrated during polymerization, microcracks or uneven cross-linking regions are easily generated within the network due to local overheating, affecting the mechanical properties and optical uniformity of the final product. Therefore, controlling the molar ratio of initiator to reaction accelerator within the range of (0.8–1.2):1, preferably (0.9–1.2):1, helps to ensure the stability and repeatability of product performance between batches.
[0042] In some embodiments, the water content in the polymerization crosslinking reaction is 60 wt% to 80 wt% of the total mass of the polymerization crosslinking reaction system. It is understood that when the water content is 60 wt% to 80 wt% of the total mass of the polymerization crosslinking reaction system, the water content in the system is within a suitable range. If the water content is below 60 wt%, the solid content of the polymerization system is too high, and the viscosity is too large, which is not conducive to the uniform dispersion and diffusion of each component (especially the metal ion crosslinking agent and initiator). At the same time, the heat release during polymerization is concentrated, and local burst polymerization is prone to occur, leading to uneven internal structure of the gel and even microcracks. If the water content is above 80 wt%, the solid content of the system is too low, the monomer concentration and crosslinking point density decrease, the ultra-dense three-dimensional network is difficult to fully form, the nano-confining effect is weakened, the proportion of free water increases, resulting in decreased mechanical strength and deterioration of low-temperature antifreeze performance.
[0043] In a more preferred embodiment, the water accounts for 65 wt% to 75 wt% of the total mass of the polymerization and crosslinking reaction system. When the water content is further controlled within the preferred range of 65 wt% to 75 wt%, the dispersion uniformity of each component is optimal, the polymerization reaction proceeds smoothly, the resulting gel network structure is dense and the crosslinking points are evenly distributed, and the proportion of bonded water is maintained at a high level, which is beneficial for achieving high strength mechanical properties, excellent low-temperature antifreeze properties, and anti-swelling properties.
[0044] For example, the proportion of water in the total mass of the polymerization crosslinking reaction system can be controlled at 60 wt%, 63 wt%, 65 wt%, 67 wt%, 70 wt%, 72 wt%, 75 wt%, 78 wt%, or 80 wt%.
[0045] It should be noted that the total mass of the polymerization and crosslinking reaction system refers to the sum of the masses of all raw materials participating in the polymerization and crosslinking reaction before the reaction occurs, including the total mass of water, water-soluble olefinic unsaturated monomers, alkaline substances, metal ion crosslinking agents, initiators, and reaction promoters. Taking Example 1 as an example, the total mass of the polymerization and crosslinking reaction system = 50g deionized water + 11.66g zirconium tetrachloride + 7.21g acrylic acid + 5.61g potassium hydroxide + 0.053g ascorbic acid + 0.072g ammonium persulfate ≈ 74.61g. Among them, water accounts for approximately 67.0wt% of the total mass of the system (50g ÷ 74.61g × 100% ≈ 67.0wt%). This mass is calculated based on the actual amount of each raw material fed, without deducting the trace amount of water evaporation that may occur due to exothermic reaction during the polymerization and crosslinking reaction. Since the polymerization and crosslinking reaction is carried out in a closed mold covered with a glass plate, water evaporation is negligible, so the total mass of the system before and after the reaction remains basically unchanged. The proportion of water in the total mass of the system in the examples is based on this calculation method.
[0046] In some embodiments, the water-soluble olefinically unsaturated monomer is acrylic acid and / or methacrylic acid. Both acrylic acid and methacrylic acid molecules contain olefinic bonds (which can participate in free radical polymerization) and carboxyl groups (which can be neutralized to carboxylate groups, providing coordination sites). Both can be used as basic monomer units for constructing polymer networks in this application, and their polymerization behavior and coordination ability are essentially the same.
[0047] In some embodiments, the water-soluble olefinically unsaturated monomer is a composition of acrylic acid and / or methacrylic acid with other olefinically unsaturated monomers, and the mass percentage of acrylic acid and / or methacrylic acid in the composition is not less than 60%. When other olefinically unsaturated comonomers (such as acrylamide, N-isopropylacrylamide, hydroxyethyl methacrylate, etc.) are introduced, it is necessary to ensure that acrylic acid and / or methacrylic acid account for the majority of the total monomers. This is because the carboxyl group is the core functional group for metal ion coordination crosslinking. If its proportion is too low, the number of available coordination sites in the system is insufficient, and even with an excess of metal ions, an effective crosslinking network cannot be formed. The lower limit of 60% ensures that the number of coordination sites is sufficient to support the formation of an ultra-high density crosslinked structure, while the introduction of other monomers can adjust certain properties of the hydrogel (such as hydrophilicity-hydrophobicity balance, responsiveness, etc.) without destroying the overall crosslinking network.
[0048] In some embodiments, the metal ions in the metal ion crosslinking agent also include other metal ions, selected from at least one of calcium ions, zinc ions, nickel ions, copper ions, cobalt ions, iron ions, and aluminum ions, and the proportion of the other metal ions in the total molar number of metal ions does not exceed 20%. These other polyvalent metal ions all possess empty orbitals capable of coordinating with carboxylate ions, and their coordination ability is of the same type as that of zirconium ions and hafnium ions. When their proportion is controlled below 20%, zirconium ions and / or hafnium ions still constitute the main body of crosslinking nodes in the network, and the network's framework structure and crosslinking density distribution remain essentially unchanged. Simultaneously, these small amounts of other metal ions can introduce different coordination characteristics (such as differences in coordination number, coordination bond strength, and response to specific stimuli) into the system without altering the basic network structure, providing room for performance adjustment of the hydrogel without compromising overall performance.
[0049] In some embodiments, the metal ion crosslinking agent is zirconium tetrachloride. Zirconium tetrachloride has good solubility in water and dissociates into Zr upon dissolution. 4+ Since chloride ions do not participate in the coordination reaction, they will not interfere with the subsequent polymerization process and coordination crosslinking. Other zirconium salts can also be used, but it is necessary to avoid introducing anions (such as sulfate, nitrate, etc.) that may compete with metal ions for coordination. Therefore, zirconium tetrachloride is the preferred form of metal ion crosslinking agent in this application.
[0050] In some embodiments, the initiator is ammonium persulfate; the crosslinking promoter is ascorbic acid; and the water is deionized water or distilled water.
[0051] In some embodiments, when the hydrogel polymer is soaked in a first alkaline solution, the mass ratio of the hydrogel polymer to the first alkaline solution is 1:140 to 160, the soaking time is 6 hours to 24 hours, and the soaking temperature is 15°C to 40°C.
[0052] In some embodiments, the first alkaline solution is an aqueous solution of potassium hydroxide, and the concentration of potassium hydroxide in the first alkaline solution is 2 mol / L to 8 mol / L.
[0053] In other embodiments, the first alkaline solution is a mixed aqueous solution of potassium hydroxide and zinc acetate, wherein the concentration of potassium hydroxide in the first alkaline solution is 2 mol / L to 8 mol / L, and the concentration of zinc acetate is 0.1 mol / L to 1 mol / L. It is understood that the alkaline solution can be an aqueous solution of potassium hydroxide or a mixed aqueous solution of potassium hydroxide and zinc salt. When the alkaline solution simultaneously contains KOH and Zn... 2+ At that time, Zn 2+The presence of zinc ions can pre-establish an equilibrium concentration of zinc ions in the electrolyte, which helps to suppress the self-corrosion and dendrite growth of zinc anode under alkaline conditions, thereby further improving the cycle stability of the battery.
[0054] It is understood that both alkaline solution schemes described in this application (pure KOH aqueous solution scheme and KOH and zinc acetate mixed aqueous solution scheme) are applicable to the ultra-dense cross-linked network structure of this application. Both schemes contribute to imparting ionic conductivity to the hydrogel polymer; the difference lies in the additional introduction of Zn... 2+ A zinc-friendly interfacial chemical environment was further constructed, which can be used as a preferred implementation method in scenarios with higher cycle life requirements.
[0055] Secondly, embodiments of this application provide an electrolyte for zinc-air batteries prepared by the method described in the first aspect. This electrolyte has undergone a first alkaline solution immersion treatment during the preparation process and can be directly used in the assembly of zinc-air batteries.
[0056] Thirdly, embodiments of this application provide a zinc-air battery, including a zinc anode, an air cathode, and an electrolyte disposed between the zinc anode and the air cathode, wherein the electrolyte is obtained by the preparation method described in the first aspect; or, the electrolyte is the electrolyte for zinc-air batteries described in the second aspect.
[0057] Fourthly, embodiments of this application provide a method for regenerating a zinc-air battery, comprising the following steps: Provide the zinc-air battery as described in the third aspect; The hydrogel electrolyte in the zinc-air battery is removed and immersed in a second alkaline solution to restore the electrolyte's ion conduction properties. The regenerated electrolyte is reassembled between the zinc anode and the air cathode to complete battery regeneration.
[0058] In some embodiments, when the hydrogel electrolyte is immersed in a second alkaline solution, the mass ratio of the hydrogel electrolyte to the second alkaline solution is 1:140 to 160, the immersion time is 6 hours to 24 hours, and the immersion temperature is 15°C to 40°C.
[0059] In some embodiments, the second alkaline solution is an aqueous solution of potassium hydroxide, and the concentration of potassium hydroxide in the second alkaline solution is 2 mol / L to 8 mol / L.
[0060] In other embodiments, the second alkaline solution is a mixed aqueous solution of potassium hydroxide and zinc acetate; the concentration of potassium hydroxide in the second alkaline solution is 2 mol / L to 8 mol / L, and the concentration of zinc acetate is 0.1 mol / L to 1 mol / L.
[0061] It is understood that the second alkaline solution described in the fourth aspect and the first alkaline solution described in the first aspect can be the same solution system or different solution systems. When the same solution system is used, the regeneration process only requires re-immersing the used electrolyte in the first alkaline solution with the same initial activation conditions to restore its ion conductivity, which is simple and inexpensive. During the regeneration process, ions in the alkaline solution diffuse back into the electrolyte network, replenishing the OH- ions consumed during the cycle. - This restores the electrolyte to a state close to its initial ion conduction state.
[0062] Fifthly, embodiments of this application provide an energy storage system including at least one zinc-air battery as described in the third aspect. When multiple zinc-air batteries are included, the batteries can be connected in series, in parallel, or in a series-parallel combination to adapt to different voltage and power requirements. It is understood that the energy storage system also includes a charge / discharge management module and / or a thermal management system connected to the zinc-air batteries to ensure the safe and stable operation of the energy storage system.
[0063] The following is in conjunction with the appendix Figures 1 to 11 The present application provides a more detailed description of a hydrogel polymer through specific embodiments and application scenarios.
[0064] I. Preparation of Electrolytes for Zinc-Air Batteries Example 1-1:
[0065] This application provides a method for preparing an electrolyte for zinc-air batteries, the preparation of which includes the following steps: Step S10: Dissolve 0.05 mol (approximately 11.660 g) of zirconium tetrachloride in 35 mL of deionized water, and denote this solution as solution A; Step S20: Neutralize 0.1 mol (approximately 7.206 g) of acrylic acid with 0.1 mol (approximately 5.610 g) of potassium hydroxide in 10 mL of deionized water, and denote this as solution B; Step S30: Mix solution A and solution B thoroughly, then add 0.053g of ascorbic acid, stir and mix thoroughly to obtain a mixed solution; Step S40: Dissolve 0.072 g of ammonium persulfate in 5 mL of deionized water, and slowly add it to the mixed solution obtained in step S30 under stirring. Mix well, then degas the solution, and finally cast it into a PTFE mold. Cover with a glass plate and allow it to stand at room temperature for 30 minutes for polymerization and crosslinking reaction. After the polymerization and crosslinking reaction is complete, demold to obtain a solid hydrogel polymer, named LMDC-gel. Step S50: The hydrogel polymer LMDC-gel obtained in step S40 is immersed in a first alkaline solution for treatment. The first alkaline solution is an aqueous solution containing 6M potassium hydroxide and 0.2M zinc acetate. The mass ratio of LMDC-gel to the first alkaline solution is 1:150. The immersion time is 12 hours and the immersion temperature is room temperature. After immersion, the gel is removed to obtain the electrolyte for zinc-air batteries.
[0066] It should be noted that the PTFE mold can be customized according to requirements, for example: PTFE mold ①: The large block gel is synthesized using a rectangular groove mold with internal dimensions of 50cm × 70cm × 1cm (length × width × thickness). PTFE mold ②: Cylindrical mold, with an inner diameter × height of 1.4cm × 2cm; PTFE mold ③: rectangular groove type, with internal dimensions of length × width × thickness of 6cm × 0.5cm × 0.2cm; PTFE mold ④: cylindrical, with an inner diameter × height of 1.7cm × 1cm; of course, other sizes and shapes of PTFE molds can be used according to specific needs; the LMDC-gel hydrogels used in the experimental examples described below were all prepared according to the raw material ratio of Example 1-1, but the shape and size of the PTFE mold can be designed according to specific experiments.
[0067] A photograph of the LMDC-gel hydrogel obtained from the PTFE mold ① is shown below. Figure 1 As shown, where: Figure 1 In Example 1-1, 'a' is a photograph of a large-area hydrogel with a length of 70cm, a width of 50cm, and a thickness of 1cm obtained, demonstrating that the method of this application can achieve the preparation of large-area hydrogels. Figure 1 b in Figure 1 A photo of small pieces of hydrogel after they have been cut and packaged.
[0068] Examples 1-2:
[0069] The difference between this embodiment and Embodiment 1-1 is that: in step S10, the amount of zirconium tetrachloride used is 0.1 mol; in step S20, the amount of acrylic acid used is 0.1 mol. The types, amounts, and preparation steps of the remaining raw materials are the same as in Example 1, and an electrolyte for zinc-air batteries is obtained.
[0070] Examples 1-3:
[0071] The difference between this embodiment and Embodiment 1-1 is that: in step S10, the amount of zirconium tetrachloride used is 0.2 mol; in step S20, the amount of acrylic acid used is 0.1 mol. The types, amounts, and preparation steps of the remaining raw materials are the same as in Example 1, and an electrolyte for zinc-air batteries is obtained.
[0072] Examples 1-4:
[0073] The difference between this embodiment and Embodiment 1-1 is that in step S20, the amount of potassium hydroxide used is 0.08 mol and the amount of acrylic acid used is 0.1 mol. The types, amounts, and preparation steps of the remaining raw materials are the same as in Example 1, and an electrolyte for zinc-air batteries is obtained.
[0074] Examples 1-5:
[0075] The difference from Example 1-1 is that: in step S30, the amount of ascorbic acid used is 0.18 g; in step S40, the amount of ammonium persulfate used is 0.23 g. The types, amounts, and preparation steps of the remaining raw materials are the same as in Example 1, and an electrolyte for zinc-air batteries is obtained.
[0076] II. Zinc-Air Batteries Example 2-1:
[0077] This application provides a zinc-air battery, including a zinc anode, an air cathode, and an electrolyte disposed between the zinc anode and the air cathode. The electrolyte is a zinc-air battery electrolyte obtained by the preparation method described in Examples 1-1. Specifically, it includes the following steps: Step S100: Preparation of the air cathode: The Pt / C+RuO2 catalyst ink was coated onto carbon paper with a loading of 1 mg·cm³. -2 The air cathode was then dried by infrared for 5 min to obtain the catalyst ink, which was prepared by uniformly dispersing 5 mg Pt / C+RuO2 in 0.49 mL isopropanol and adding 10 μL of 5 wt% Nafion solution.
[0078] Step S200: Assembly of the zinc-air battery: A sandwich-structured zinc-air battery, named LMDC-ZABs, was assembled using a zinc foil anode, a hydrogel electrolyte prepared in Example 1-1, and an air cathode obtained in step S100.
[0079] III. Comparative Examples: Comparative Example 1-1: In the preparation of PAA-gel, the acrylic acid (AA) content is fixed at 12.6 wt%.
[0080] For every 50 ml of deionized water, 7.206 g of acrylic acid (0.1 mol) as a monomer, 0.036 g of N,N'-methylenebisacrylamide (MBAA) as a covalent crosslinking agent, 0.072 g of ammonium persulfate (APS) as an initiator, and 0.053 g of ascorbic acid as a crosslinking accelerator were added. The mixture was thoroughly stirred and mixed, and after degassing, it was transferred into a polytetrafluoroethylene (PTFE) mold. The polymerization reaction was carried out at 60°C for 1 hour, followed by curing at room temperature. After demolding, a solid hydrogel was obtained, named PAA-gel. The hydrogel polymer PAA-gel was immersed in a first alkaline solution, which was an aqueous solution containing 6M potassium hydroxide and 0.2M zinc acetate. The mass ratio of PAA-gel to the first alkaline solution was 1:150, the immersion time was 12 hours, and the immersion temperature was room temperature. After immersion, the polymer was removed to obtain the electrolyte for zinc-air batteries.
[0081] Comparative Examples 1-2: 7.206 g (0.1 mol) of acrylic acid and 5.6105 g (0.1 mol) of potassium hydroxide were dissolved in 50 ml of deionized water. Then, 0.072 g of ammonium persulfate, 0.036 g of N,N'-methylenebisacrylamide, and 0.053 g of ascorbic acid were added and stirred until homogeneous. After degassing, the solution was cast into a PTFE mold and polymerized at room temperature. After polymerization, a solid gel was obtained. The gel was then thoroughly soaked in an excess zirconium tetrachloride solution (0.02 mol / L) to obtain conventional Zr. 4+ The cross-linked hydrogel is named MDC-gel.
[0082] Comparative Example 2-1: The difference between this comparative example and Example 2-1 is that the electrolyte used is the zinc-air battery electrolyte prepared by the preparation method described in Comparative Example 1-1. The types, amounts, and steps of the remaining raw materials are the same as in Example 2-1. The zinc-air battery was assembled and named PAA-ZABs.
[0083] III. Experimental Examples: 1. Characterization of the microporous structure of the gel (cryo-SEM) 1.1 Experimental Methods: Three hydrogel samples—Example 1-1 (LMDC-gel), Comparative Example 1-1 (PAA-gel), and Comparative Example 1-2 (MDC-gel)—were cut into fresh sections of suitable size and observed using a Regulus 8220 cryogenic scanning electron microscope (Cryo-SEM; Hitachi, Japan). Before observation, the samples were frozen in liquid nitrogen for 30 seconds, transferred to the preparation chamber via a Quorum PP3000T vacuum system, and sublimated at -90°C for 10 minutes. Subsequently, gold sputtering was performed at 10 mA for 60 seconds, with the stage temperature maintained at -140°C. Imaging was performed at an accelerating voltage of 5 kV. All images were acquired at a uniform magnification and accompanied by a 10 μm scale bar as a morphological reference.
[0084] 1.2 Experimental Results like Figure 2 As shown in the Cryo-SEM images, the microstructure of the three hydrogel samples differs significantly. Please see Figure 2 a. Example 1-1 (LMDC-gel): The gel has dense and uniformly distributed pores with extremely small micropore size, presenting a fine microporous structure. The number of pores per unit area is significantly greater than the other two groups.
[0085] Please see Figure 2 c. Comparative Examples 1-2 (MDC-gel): The internal structure forms a honeycomb-like open structure with significantly increased size, and the pores are interconnected. The average pore diameter is significantly larger than that of Example 1-1, and the skeleton wall thickness is relatively thin.
[0086] Please see Figure 2 b, Comparative Example 1-1 (PAA-gel): It exhibits the largest mesh-like macroporous skeleton, with the highest pore size and skeleton spacing among the three groups of samples, and the most loose structure.
[0087] Based on a standardized scale (10μm), the pore sizes of the three groups of samples were determined as follows: Example 1-1 (LMDC-gel) < Comparative Example 1-2 (MDC-gel) < Comparative Example 1-1 (PAA-gel).
[0088] 2.3 Results Analysis The significant differences in micropore size and network density among the three samples stem from the fundamental differences in their cross-linking mechanisms and cross-linking densities.
[0089] In Example 1-1, Zr was used to form LMDC-gel. 4+Metal ions act as crosslinking agents, and are in excess relative to the water-soluble olefinic unsaturated monomers. In this system, each metal ion has multiple coordination sites, which can simultaneously form coordination chelate bonds with carboxylate groups on multiple polymer chains. The metal ions not only serve as crosslinking nodes between polymer chains but also directly as the core crosslinking nodes of the entire three-dimensional network. Due to the excess supply of metal ions, the active sites available for coordination on the polymer chains are fully utilized, the number of crosslinking points increases by orders of magnitude, and the molecular chain segments are densely fixed between adjacent crosslinking points. Their free movement space is strongly compressed, and their expansion is greatly suppressed, thereby constructing a dense, uniform, and extremely narrow microporous network structure.
[0090] In Comparative Examples 1-2, the formation of MDC-gel also belongs to metal ion coordination crosslinking, but the amount of metal ions is in a non-excessive state, the number of crosslinking points is much lower than in Example 1-1, the constraint effect on the molecular chain segments is significantly weakened, the chain segments have a larger space for expansion, and the pore walls are difficult to maintain a dense configuration during phase separation, thus forming a honeycomb interconnected open structure with larger size.
[0091] In Comparative Example 1-1, PAA-gel was formed using the traditional chemical crosslinking agent N,N-methylenebisacrylamide. This crosslinking agent serves only as a chemical "bridge" connection point between polymer chains, and its amount is trace relative to the monomer. In this crosslinking system, the spacing between crosslinking points is relatively wide, the crosslinking density is at a conventional level, and the polymer chain segments are less constrained, allowing them to stretch relatively freely, thus forming the most loose macroporous network structure.
[0092] In summary, the pore size differences among the three groups of hydrogel samples are essentially an external manifestation of the decreasing crosslinking density: the higher the crosslinking density, the stronger the network constraint and the smaller the pore size; the lower the crosslinking density, the weaker the network constraint and the larger the pore size. The crosslinking density decreases sequentially, corresponding to a sequential increase in pore size, indicating a progressively greater degree of structural looseness.
[0093] Based on the above correspondence between cross-linked structure and microstructure, it can be reasonably inferred that: Example 1-1, with its ultra-dense cross-linked network with metal ions as the core cross-linking nodes, forms a dense and uniform microporous structure. This structural feature helps to improve the mechanical strength of the hydrogel, inhibit its swelling behavior in the external environment, and enhance its adsorption and retention capacity for small molecules. Compared with Comparative Examples 1-2 and 1-1, which have significantly lower cross-linking density and significantly looser structure, it shows significant performance advantages.
[0094] 2. Synchrotron X-ray absorption spectroscopy characterization 2.1 Experimental Methods The Zr K-edge X-ray Absorbed Fine Structure (XAFS) spectroscopy was used to characterize the gel sample from Example 1-1 (LMDC-gel). XAFS measurements were performed at the BL14W beamline of the Shanghai Synchrotron Radiation Facility (SSRF; Shanghai, China) using a Si(111) dual-crystal monochromator. The monochromator energy stability was maintained within ±0.1 eV throughout the data acquisition process. The sample was placed on an aluminum sample holder and sealed with Kapton tape. Fluorescence mode spectra were acquired at 298 K using a Bruker 5040 four-channel silicon drift detector (SDD), with Zr foil as the standard sample, and measured in transmission mode. Data processing was performed using Athena software according to standard procedures. Measurement repeatability was confirmed by three repeated scans (relative standard deviation <5%).
[0095] 2.2 Experimental Results like Figure 3 The figure shows the XAFS series characterization results of the LMDC-gel hydrogel prepared in Example 1-1 of this application; wherein: Figure 3 In this context, 'a' represents the k of the LMDC-gel hydrogel prepared in Example 1-1 of this application. 2 The weighted χ(k) oscillation spectrum and its fitting curve results confirmed the coordination relationship of Zr-O.
[0096] Figure 3 In this paper, b represents the radial distance R-space EXAFS spectrum and its fitting result of the LMDC-gel hydrogel prepared in Examples 1-1 of this application; after analysis... Figure 3 Quantitative fitting of the characteristic peaks of the first coordination shell in b yields Zr. 4+ The two main coordination modes are: coordination with carboxylate groups, with a coordination number of approximately 3.7; and coordination with water molecules, with a coordination number of approximately 2.9.
[0097] Figure 3 In the figure, 'c' is a two-dimensional wavelet transform contour plot of the Zr site EXAFS signal of the LMDC-gel hydrogel prepared in Example 1-1 of this application, indicating that it has a uniform local coordination environment; the magnitude in the color scale on the right side of the figure represents the signal amplitude. Therefore, by combining spectral fitting analysis, it can be determined that there are stable Zr-O coordination bonds in the LMDC-gel system, and that the Zr center has a uniform local coordination environment.
[0098] 2.3 Results Analysis: k 2The fitting degree of the weighted χ(k) spectrum and the single symmetrical main peak in the R-space EXAFS both indicate that Zr in the system mainly uses Zr-O coordination bonds as the core bonding form, without a large number of heterogeneous coordination peaks. This result demonstrates that metal Zr ions can undergo stable coordination chelation with carboxylate groups on the polymer chain, effectively forming Zr-O bonds. 4+ The center is the coordination crosslinking node.
[0099] Two-dimensional wavelet transform (WT) can simultaneously resolve radial distance and k-space signal distribution characteristics. Its highly concentrated signal distribution indicates that the bond lengths and coordination environments of all Zr coordination sites within the system are highly uniform, without the mixing of multiple differential coordination configurations, thus achieving homogeneity of the crosslinking node structure. Uniform and stable Zr-O coordination crosslinking nodes ensure consistent crosslinking density throughout the three-dimensional network, helping to avoid structural defects such as uneven local crosslinking density or excessive aggregation. This provides an atomic-scale bonding basis for constructing macroscopic gel networks with regular structures and uniform mechanical properties. Figure 3 Quantitative fitting results of the characteristic peak of the first coordination shell in b, Zr 4+ In the LMDC-gel system, two main coordination modes exist: coordination with carboxylate groups (coordination number CN≈3.7) to form crosslinking nodes, and coordination with water molecules (CN≈2.9) to form hydrated ion clusters. These two coordination modes together constitute the Zr in the LMDC-gel. 4+ The local coordination environment, in which coordination with carboxylate ions is the structural basis for the formation of ultra-dense cross-linked networks, while coordination with water molecules provides the source of bonded water for the network, which is the microstructural root of the nano-confined effect and low-temperature antifreeze performance.
[0100] 3. Characterization of small-angle X-ray scattering (SAXS) 3.1 Experimental Methods Three hydrogel samples—Example 1-1 (LMDC-gel), Comparative Example 1-1 (PAA-gel), and Comparative Example 1-2 (MDC-gel)—were selected for one-dimensional and two-dimensional SAXS tests. The tests were conducted at the Shanghai Synchrotron Radiation Facility (SSRF) BL16B beamline, with an X-ray energy of 10 keV and a scattering vector q ranging from 0.01 to 0.5 Å. -1 Data processing included background subtraction (air scattering) and azimuth integration of the two-dimensional scattering pattern into a one-dimensional scattering curve using Fit 2D software (European Synchrotron Radiation Facility, ESRF). Absolute intensities were calibrated using the glassy carbon standard.
[0101] 3.2 Experimental Results: like Figure 4 and Figure 5 The image shows the SAXS characterization results for three groups of samples; where: Please see Figure 4 One-dimensional SAXS spectra: at q values of 0.2-0.3 nm -1 In conventional PAA-gels, the characteristic scattering shoulder peaks that are usually associated with heterogeneous cross-linked regions gradually weaken until they are difficult to distinguish in LMDC-gels. In MDC-gel curves, the characteristic scattering "shoulder peaks" are observed to weaken, while in LMDC-gels, the "shoulder peaks" disappear completely, indicating a reduction in topological inhomogeneity. Please see Figure 5 Two-dimensional SAXS patterns: exhibiting a gradient evolution pattern (corresponding to samples from left to right: PAA-gel, MDC-gel, LMDC-gel): PAA-gel is a diffuse scattering ring; the clarity of the scattering ring of MDC-gel is improved; LMDC-gel eventually forms a clear, isotropic concentric scattering ring; the evolution from the diffuse ring of PAA-gel gel to the clear, isotropic concentric ring of LMDC-gel gel is a typical characteristic of a uniform three-dimensional network structure with regular nanoscale correlated lengths.
[0102] 3.3 Results Analysis: (1) The generation of characteristic scattering shoulders in the one-dimensional SAXS spectrum originates from the characteristic scattering signals caused by the topological inhomogeneity of the gel and the differences in phase separation at the nanoscale. PAA-gel adopts a traditional organic chemical crosslinking system with low crosslinking density, high degree of freedom of polymer chain segments, large fluctuations in network density, and the strongest initial topological inhomogeneity, resulting in the most obvious characteristic scattering signals. MDC-gel also belongs to metal ion coordination crosslinking, but its crosslinking density is insufficient. It partially improves the structural inhomogeneity but still leaves local differences, thus retaining weak shoulders. 4+ Uniform ion coordination and crosslinking, high density of crosslinking points and uniform spatial distribution, and compact and consistent network skeleton significantly smooth out the differences in density at the nanoscale, greatly reduce topological inhomogeneity, and completely eliminate characteristic shoulder peaks.
[0103] (2) The transformation of the two-dimensional SAXS pattern from diffuse rings to clear isotropic concentric rings reflects the structural evolution process of the gel nanoscale correlated lengths tending to be more regular. The PAA-gel crosslinking network exhibits large fluctuations in crosslinking point spacing, high chain segment freedom, and low nanostructure order, thus the scattering rings show diffuse and blurred characteristics. The introduction of coordination crosslinking in the MDC-gel improves the network regularity and enhances the clarity of the scattering rings. Excess Zr in the LMDC-gel... 4+ Ions form a uniform and dense coordination cross-linking network, resulting in high consistency in the arrangement of nanostructures and uniform correlation lengths throughout the three-dimensional network, ultimately forming a typical clear isotropic concentric scattering ring.
[0104] 4. Characterization of water molecule state and thermal properties 4.1 Experimental Methods 4.1.1 Low-field nuclear magnetic resonance (LF-NMR) The proton transverse relaxation time (T2) of three hydrogel samples (PAA-gel, MDC-gel, and LMDC-gel) was measured at 298.15 K using a low-field nuclear magnetic resonance analyzer (MicroMR12-040V, 12 MHz, 0.25 T). Porosity was derived from the T2 decay signal combined with the calibration curve. The pore size distribution was calculated using the relationship r = T2 × ρ × a, where ρ = 10 μm·s. -1 (Surface relaxation rate of the hydrogel), assuming a cylindrical pore geometry (a = 2). Crosslinking density was quantitatively determined using a VTNMR20-010V-T analyzer at a magnet temperature of 35 ± 0.02 °C and a full pore size of 10 mm. T2 measurements were performed using a Carr-Purcell-Meiboom-Gill (CPMG) pulse sequence with a 200 μs pulse interval between 90° and 180°.
[0105] To analyze the proportions of each component, the CPMG echo envelope M(t) is fitted using a multi-component exponential model. The formula is as follows (1): (1); In equation (1), and These represent the signal amplitudes of protons in the cross-linked network and the signal amplitudes of protons in the suspended chain, respectively. It is the residual second moment of the network protons, and its value is directly proportional to the crosslinking density. This fitting process was performed using the instrument's built-in XLD analysis software package, which implemented the above model.
[0106] The dangling chain ratio is calculated solely from the polymer-related proton signal using the following formula (2): (2); In equation (2), and These represent the signal amplitudes of the protons in the cross-linked network and the signal amplitudes of the protons in the suspended chain, respectively.
[0107] Crosslinking percentage (%): Calculated by the following formula (3): (3); In equation (3), and These represent the signal amplitudes of the protons in the cross-linked network and the signal amplitudes of the protons in the suspended chain, respectively.
[0108] 4.1.2 Raman spectroscopy Raman spectra of three hydrogel samples (PAA-gel, MDC-gel, and LMDC-gel) were acquired using a confocal Raman spectrometer with an excitation wavelength of 532 nm and a spectral resolution of 1 cm⁻¹. -1 The scanning range is 2800cm. -1 -3800cm -1 Room temperature spectra were collected at 25°C, while low temperature spectra were collected after the sample temperature was lowered to -65°C using a liquid nitrogen cooling stage, with an equilibration time of no less than 10 minutes.
[0109] 4.1.3 Differential Scanning Calorimetry (DSC) The thermal behavior of three hydrogel samples—PAA-gel, MDC-gel, and LMDC-gel—was analyzed using a differential scanning calorimeter (Netzsch DSC 200 F3, Germany). For low-temperature measurements, the samples were placed in a platinum crucible, with an empty crucible used as a reference. The temperature program was as follows: initial equilibration at 25℃, followed by temperature increases at -5℃·min. -1 Cooled to -150°C at a rate of [missing value], held at that temperature for 5 min, then cooled at a rate of 5°C / min. -1 The temperature was heated to 25°C at a rate of [missing value]. All measurements were performed under a nitrogen atmosphere.
[0110] 4.1.4 Swelling Rate Test Immediately after removing the PAA-gel, MDC-gel, and LMDC-gel hydrogel samples from the mold, weigh them and record the initial mass (m0), height (h0), and diameter (d0). Then, immerse each sample in deionized water and allow it to stand at room temperature (25 ± 2°C).
[0111] Three independent LMDC-gel samples (initial volume approximately 2.25 cm³) were prepared. 3 Each sample was immersed in 500 mL of deionized water (solid-liquid ratio ≈ 1:200 w / w). Containers were sealed with plastic wrap to prevent water evaporation and external contamination. The samples were immersed in excess solvent for 7 days. Mass, height, and diameter were measured daily, and volume V was calculated at each time point. t Mass swelling ratio r m The volume swelling ratio rᵥ is calculated according to equations (4) and (5): (4); (5); Where V0 is the initial volume of the sample, V t m is the volume of the sample after soaking for time t; m0 is the initial volume of the sample. t The volume of the sample after soaking for time t is denoted as t.
[0112] 4.1.5 Anti-swelling performance test The initial morphology of the LMDC-gel hydrogel samples was photographed before immersion, and then immersed in deionized water and left to stand at 25°C for 500 days. After immersion, the samples were removed and photographed again against the same reference background for comparative analysis of macroscopic morphological changes after long-term immersion.
[0113] 4.2 Experimental Results like Figure 6 As shown in Table 1, the three hydrogel samples exhibit significant differences in water molecule state and thermal properties. The specific results are as follows: Please see Figure 6 a. LF-NMR T2 relaxation spectrum: LMDC-gel shows a short relaxation time (1.825 ms), which is a characteristic signal of bound water; PAA-gel shows a long relaxation time (1645 ms), indicating that it is dominated by free water; the relaxation time of MDC-gel (117 ms) is in the middle state.
[0114] Please see Figure 6 b, Room temperature Raman spectrum: The OH stretching vibration band is located at 3422 cm⁻¹ of the PAA-gel. -1 Redshifted to 3402 cm⁻¹ of LMDC-gel -1 This indicates that the water-polymer interaction gradually strengthens.
[0115] Please see Figure 6 c. Low-temperature (-65℃) Raman spectrum: PAA-gel at 3110 cm⁻¹ -1 The vicinity exhibits sharp characteristic peaks of ice crystals; the LMDC-gel shows well-resolved double peaks (3416 cm⁻¹). -1 / 3256cm -1 Furthermore, the low-frequency components are stronger, reflecting a strong nano-confinence effect and the absence of macroscopic ice crystals.
[0116] Please see Figure 6 d, DSC curve: LMDC-gel exhibits a thermal transition at -91.8℃, which is significantly lower than that of MDC-gel (-31.3℃) and PAA-gel (12.6℃).
[0117] Please see Figure 6 e. Swelling kinetics (based on daily volume measurements): LMDC-gel showed almost no swelling after immersion in deionized water for 7 days (volume change < 0.5%); while PAA-gel exhibited a swelling rate exceeding 1400%. Please see Figure 6f. Comparison photos of LMDC-gel hydrogels after immersion in deionized water for 500 days. After 500 days of long-term immersion, the macroscopic morphology of the LMDC-gel hydrogel remained intact, with only minor changes in size and a volume change of ≤0.5%. Furthermore, under the same conditions, when the deionized water was replaced with a 6 M KOH solution, the volume change after immersion for 500 days was ≤0.5%.
[0118] Table 1. Results of crosslinking density, suspended chain ratio, and crosslinking percentage
[0119] Furthermore, the LF-NMR pore size results are as follows: The LMDC-gel prepared in Example 1 of this application has a narrow pore size distribution centered at 73.1 nm, with 90% of the pores having a diameter less than 100 nm, indicating that its ultra-dense cross-linked network forms a uniform and dense nanoscale pore structure. In contrast, the PAA-gel prepared in Comparative Example 1 exhibits a broad micron-scale pore size distribution, with an average pore size of 8.60 ± 3.20 µm, indicating that its network structure is relatively loose and its pore size uniformity is poor.
[0120] 4.3 Results Analysis: (1) The LF-NMRT2 relaxation spectrum results directly reflect the degree of confinement of water molecules in the gel network. Combined with the crosslinking density data in Table 1, it can be seen that the crosslinking density of LMDC-gel is as high as 9.515 × 10⁻⁶. -4 mol·mL -1 The values are approximately MDC-gel (1.131 × 10⁻⁶). -4 mol·mL -1 8.4 times that of PAA-gel (0.529×10) -4 mol·mL -1 The cross-linking ratio in LMDC-gel is as high as 99.7%, and the suspended chain ratio is only 0.3%, indicating that its network structure is almost perfect and has extremely low defects; while the cross-linking ratio in PAA-gel is only 14.32%, and the suspended chain ratio is as high as 85.68%, indicating a loose network structure with serious defects. Based on this structure, the short T2 relaxation time (1.825 ms) in LMDC-gel indicates that water molecules are strongly confined by the nano-confinement effect and mainly exist in the form of bound water; the long T2 relaxation time (1645 ms) in PAA-gel indicates that water molecules move freely in the network and are mainly free water. This result is consistent with the redshift phenomenon of the OH stretching vibration band in room temperature Raman spectroscopy (3422 cm⁻¹). -1 →3402cm -1 The enhanced hydrogen bonding between water and polymer further confirms the significant increase in the degree of restriction on the movement of water molecules inside the LMDC-gel.
[0121] (2) The low-temperature Raman spectroscopy and DSC test results together revealed the excellent low-temperature antifreeze properties of LMDC-gel. This is due to the extremely high crosslinking density of LMDC-gel (9.515 × 10⁻⁶) shown in Table 1. -4 mol·mL -1 With a near 100% cross-linking ratio, its ultra-dense cross-linked network generates a strong nano-confining effect. PAA-gel exhibits a sharp ice crystal peak at -65℃, corresponding to a crystallization transition of 12.6℃ in the DSC curve, indicating that its network structure cannot suppress the orderly arrangement of water molecules and ice crystal nucleation at low temperatures. LMDC-gel, with its Raman bimodal characteristics at -65℃ and a DSC thermal transition temperature of -91.8℃, is far lower than the freezing point of conventional water / hydrogels, demonstrating that the nano-confining effect induced by its dense ultra-dense cross-linked network effectively restricts the translational and rotational movements of water molecules, making it difficult for water molecules to arrange themselves in an orderly manner to form ice crystals, thus endowing the gel with excellent low-temperature antifreeze properties.
[0122] (3) The anti-swelling performance of LMDC-gel also stems from the structural advantages of its ultra-dense cross-linked network. After soaking for 7 days, the volume change of LMDC-gel is less than 0.5%, and it hardly swells, while the swelling rate of PAA-gel exceeds 1400%. Based on the data analysis in Table 1, the ultra-high cross-linking density of LMDC-gel (9.515×10⁻⁶) -4 mol·mL -1 The dense microporous structure of the gel makes it difficult for water molecules to penetrate and expand the network backbone, effectively inhibiting the volume expansion behavior of the gel in an aqueous environment. Furthermore, the cross-linking ratio in the LMDC-gel is as high as 99.7%, and the suspended chain ratio is only 0.3%, meaning that there are very few suspended chains in the network structure that can serve as swelling relaxation sites, further weakening the molecular basis for network expansion. This result is consistent with the high bound water ratio revealed by the aforementioned LF-NMR: the presence of a large number of water molecules in a bound state rather than driven by free osmotic pressure is one of the fundamental reasons for its anti-swelling performance.
[0123] In summary, the ultra-dense cross-linked network of LMDC-gel, through the nanoconfinement effect, converts free water in the network into bound water, achieving not only the suppression of ice crystals at low temperatures (antifreeze) but also reducing the swelling and expansion driven by water molecules on the network framework (anti-swelling). This provides a structural basis for the service stability of LMDC-gel in a wide temperature range and in aqueous environments. The quantitative data on cross-linking density, suspended chain ratio, and cross-linking percentage in Table 1 provide direct and compelling evidence for the aforementioned performance advantages at the network structure level.
[0124] 5. Characterization of mechanical properties 5.1 Experimental Methods 5.1.1 Compression Test Uniaxial compression tests were performed on three types of gel samples, PAA-gel, MDC-gel, and LMDC-gel, using a Shimadzu AGS-X universal testing machine equipped with a 10,000 N force sensor.
[0125] Cylindrical specimens (initial height h0 = 20 mm; diameter d0 = 14 mm) were placed between parallel pressure plates and compressed at a constant rate of 10 mm / min until initial contact was detected by force response. Stress was calculated by dividing the applied load by the initial cross-sectional area. The compressive modulus was determined by a linear region within the 10%–20% strain range. Failure was defined as the moment of initial macroscopic crack initiation. Energy dissipation was quantified by the hysteresis loop area between the integral load-unload curves. Cyclic compression tests were performed at a compression rate of 200 mm / min. No water precipitation was observed throughout the testing process, confirming the structural integrity of the hydrogel network. All measurements were performed at room temperature using geometrically consistent specimens. Continuous recording of the stress-strain response allowed for simultaneous determination of the elastic modulus, failure parameters, and energy dissipation.
[0126] 5.1.2 Tensile Test Tensile tests were performed using a Shimadzu AGS-X universal testing machine equipped with a 50 N force sensor and pneumatic clamps. Dumbbell-shaped specimens (gauge length: 60 mm; width: 5 mm; thickness: 2 mm) were tested at a rate of 50 mm·min⁻¹. -1 The specimens were subjected to constant-rate tensile testing. The elastic modulus was determined from the initial linear region of the stress-strain curve. Compressive toughness was calculated by integrating the area of the nominal stress-strain curve from 0% to 99% strain using the trapezoidal method. Specimen dimensions were verified using vernier calipers. Force and displacement data were continuously recorded. Engineering stress was calculated as the applied force divided by the original cross-sectional area, and engineering strain was calculated as the ratio of displacement to the initial gauge length. All measurements followed standard test procedures for evaluating the tensile properties of hydrogels.
[0127] 5.1.2 Tensile Test Tensile tests were performed using a Shimadzu AGS-X universal testing machine equipped with a 50 N force sensor and pneumatic clamps. Dumbbell-shaped specimens (gauge length: 60 mm; width: 5 mm; thickness: 2 mm) were tested at a rate of 50 mm·min⁻¹. -1 The specimens were subjected to constant-rate tensile testing. The elastic modulus was determined from the initial linear region of the stress-strain curve. Compressive toughness was calculated by integrating the area of the nominal stress-strain curve from 0% to 99% strain using the trapezoidal method. Specimen dimensions were verified using vernier calipers. Force and displacement data were continuously recorded. Engineering stress was calculated as the applied force divided by the original cross-sectional area, and engineering strain was calculated as the ratio of displacement to the initial gauge length. All measurements followed standard test procedures for evaluating the tensile properties of hydrogels.
[0128] 5.1.3 Dynamic Rheological Testing Dynamic frequency scanning tests were performed on three gel samples using a rotational rheometer. Samples were prepared as disks (20 mm in diameter, 1 mm thick), the test temperature was 25 °C, and the strain was controlled within the linear viscoelastic region (1%). The frequency scanning range was 0.1–100 Hz. Storage modulus (G′), loss modulus (G″), and loss factor (tanδ = G″ / G′) were recorded.
[0129] 5.2 Experimental Results like Figure 7 The figure shows the mechanical properties of three hydrogel samples: PAA-gel, MDC-gel, and LMDC-gel. Please see Figure 7 a. Photographs of LMDC-gel that maintain structural integrity after 99% compressive strain (from left to right: the gel in its initial state, under ultimate compression, and in the decompression and rebound state after compression). Please see Figure 7 b. Compression stress-strain curve: LMDC-gel can withstand 99% of the compression strain, with a compressive strength of 69MPa and a compressive modulus of 0.9 MPa, far exceeding MDC-gel and PAA-gel. Please see Figure 7 c. Comparison of compression modulus and compression toughness: LMDC-gel has a compression toughness of 6 MJ·m -3 It is approximately PAA-gel (0.28 MJ·m -3 21 times that of ) Please see Figure 7 d. Tensile stress-strain curve: The tensile strain of LMDC-gel reaches 453.7%, the tensile strength is 1.66 MPa, and the tensile properties remain almost unchanged at -40℃; Please see Figure 7 e. Rheological frequency scan diagram: The energy storage modulus (G′) of LMDC-gel at 1Hz is 0.44 MPa, which is about 15 times that of PAA-gel (28 kPa); and its G′ shows a plateau region that is almost independent of frequency, and the loss factor (tan δ) is always below 0.1, indicating that it has near-ideal elasticity.
[0130] Please see Figure 7 f. Comparison of tensile modulus at 25℃ and -40℃: The tensile modulus of LMDC-gel changes by less than 7% in the temperature range of 25℃ to -40℃; the modulus of MDC-gel and PAA-gel increases by 2.8 times and 5.6 times respectively due to the formation of ice crystals at low temperature.
[0131] 5.3 Results Analysis: (1) The excellent compressive and tensile mechanical properties of LMDC-gel are due to its ultra-dense cross-linked network with metal ions as the core cross-linking nodes. The density of cross-linking points in this network is increased by orders of magnitude, and the molecular chain segments are densely fixed between adjacent cross-linking points, and the free movement space is subjected to strong compression. On the one hand, the high cross-linking density significantly enhances the rigidity of the network skeleton, as shown by a compressive strength of 69 MPa and a storage modulus of 0.44 MPa; on the other hand, the chain segments in the dense cross-linked network still retain a certain degree of flexible movement, so that the gel can dissipate energy through chain segment conformation adjustment without network breakage when subjected to high strain (99% compression, 453.7% tension), thereby endowing the material with high toughness and high ductility.
[0132] (2) The tensile properties of LMDC-gel remained almost unchanged at -40℃, and the modulus changed by less than 7%, while the modulus of PAA-gel and MDC-gel increased by 5.6 times and 2.8 times, respectively, due to the formation of ice crystals at low temperatures. This difference is directly due to the regulation of the water molecule state by the nano-confinement effect described in 4.3 above: the water molecules in LMDC-gel are mainly bound water, and macroscopic ice crystals do not form at low temperatures, thus avoiding the puncture damage and local stress concentration of the polymer network by ice crystals; while in PAA-gel and MDC-gel, a large amount of free water crystallizes at low temperatures, and the ice crystals, as rigid fillers, significantly increase the modulus but greatly reduce the toughness and ductility of the material. This result shows that the ultra-dense cross-linked network of LMDC-gel simultaneously solves the inherent defect of hydrogels prepared by traditional methods being brittle at low temperatures.
[0133] (3) During rheological frequency scanning, LMDC-gel exhibits a nearly frequency-independent G′ plateau region (G′ hardly changes with frequency in the range of 0.1-100Hz), and tan δ is consistently below 0.1, indicating that the network structure is dominated by elastic response and has extremely low energy dissipation. This rheological behavior is a typical characteristic of chemically cross-linked networks with uniform structure, high cross-linking density, and no significant network defects. In contrast, the low cross-linking density of PAA-gel makes G′ more frequency-dependent, and its tan δ is significantly higher than that of LMDC-gel.
[0134] 6. Please refer to Figure 8 This application also passes Figure 8 The schematic diagram shows the differences between hydrogel networks constructed using three different crosslinking strategies (LMDC-gel: ultra-high density metal homogeneous chelate crosslinking; MDC-gel: conventional metal chelate crosslinking; PAA-gel: conventional chemical crosslinking), and illustrates the correlation between crosslinking density, pore size, water state, and macroscopic properties. Figure 8 The key points are illustrated based on the experimental conclusions: (1) The ultra-high density metal homogeneous chelation crosslinking method in this application can obtain an ultra-high density network structure, which cannot be achieved by conventional chemical crosslinking or conventional metal chelation crosslinking. Cryo-scanning electron microscopy (Cryo-SEM) characterization results show that the ultra-dense chelation can reduce the pore size to below 100 nm, which is in stark contrast to the larger pore size observed in PAA-gel and MDC-gel. Figure 2 Statistical pore size analysis showed that LMDC-gel had a narrow pore size distribution centered at 73.1 nm, with 90% of the pores being less than 100 nm, while PAA-gel exhibited a broad micron-scale distribution (8.60 ± 3.20 µm). This structural optimization stemmed from a high density of chelating sites, which promoted a uniform distribution of crosslinks and significantly reduced the proportion of overhanging segments from 85.68% in PAA-gel to approximately 0.3% in LMDC-gel (Table 1). Synchrotron X-ray Absorption Spectroscopy (XAFS) was used to analyze the Zr content in the network. 4+ The coordination environment was characterized. Figure 3 a showed k 2 The weighted χ(k) oscillation curve and its fitted curve show that its oscillation characteristics are in good agreement with the Zr-O coordination model, confirming the existence of the Zr-O coordination relationship. Figure 3 b represents the EXAFS spectrum of the radial distance R space and its fitting result. Quantitative fitting of the characteristic peaks of its first coordination shell reveals that Zr... 4+ There are two main coordination modes: coordination with carboxyl groups (coordination number CN≈3.7) and coordination with water molecules (CN≈2.9). EXAFS two-dimensional wavelet transform contour plot ( Figure 3 c) This further confirmed the local coordination environment dominated by Zr-O bonds. LF-NMR measurements showed that the crosslinking density was 17.99 times higher than that of PAA-gel, from 0.529 × 10⁻⁶ in PAA-gel. -4 mol·mL -1 Increased to 9.515×10 to LMDC-gel -4 mol·mL -1 (Table 1). The above results confirm that an ultra-dense metal chelate hydrogel network with significantly improved topological uniformity has been successfully constructed.
[0135] (2) The method described in this invention can obtain a more uniform network structure. SAXS further quantifies the evolution of nanostructures and the improvement in uniformity caused by dense chelation. One-dimensional SAXS map ( Figure 4 The data shows a systematic trend: with a q value of 0.2-0.3 nm. -1In conventional PAA-gels, characteristic scattering shoulders typically associated with heterogeneous cross-linked regions disappear completely in LMDC-gels. This behavior indicates a significant reduction in network topological heterogeneity. Two-dimensional SAXS patterns ( Figure 5 The evolution from the weakly diffuse rings of PAA-gel to the clear and sharp isotropic concentric rings of LMDC-gel indicates the formation of a highly uniform three-dimensional network with well-defined nanoscale correlation lengths.
[0136] 7. Please refer to Figure 9 This application also passes Figure 9 The schematic diagram illustrates the differences in solvent confinement between hydrogel networks constructed using three different crosslinking strategies (LMDC-gel: ultra-high density metal homogeneous chelate crosslinking; MDC-gel: conventional metal chelate crosslinking; PAA-gel: conventional chemical crosslinking), and shows the state of solvent presence within the network. XAFS quantitative fitting results indicate that Zr... 4+ It not only coordinates with carboxylate ions (CN≈3.7) to form an ultra-dense network framework, but also coordinates with water molecules (CN≈2.9) to form hydrated ion clusters. This water coordination mode is one of the important sources of bonded water, and works synergistically with the nanoconfining effect to convert free water within the network into bound water.
[0137] The method described in this application reduces the pore size of MDC-gel hydrogel from the micrometer level to the nanometer level, enhances the nano-confinement effect of the network framework on water molecules, and the ultra-dense cross-linking converts free water into bound water. Figure 9 LF-NMR analysis in water state ( Figure 6 a) shows that LMDC-gel (relaxation time T2 = 1.825 ms) is mainly composed of bound water, while PAA-gel (T2 = 1645 ms) is approximately 82% free water. MDC-gel (T2 = 117 ms) is in an intermediate state. LF-NMR results confirm that the decrease in free water and the corresponding increase in bound water are positively correlated with the decrease in pore size. The dominance of bound water (T2 = 1-10 ms) in LMDC-gel is directly related to its excellent antifreeze properties, anti-swelling properties, and dimensional stability. Variable-temperature Raman spectroscopy provides complementary molecular-level vibrational information. Figure 6 b、 Figure 6 c). At room temperature, the OH stretching vibration bands of all hydrogels exhibit broadened single peaks. The peak position ranges from 3422 cm⁻¹. -1 (PAA-gel) systemically redshifted to 3416 cm. -1 (MDC-gel), up to 3402 cm -1 (LMDC-gel) Figure 6b). This redshift reflects the increasing interaction between water molecules and the polymer / ionic framework as the crosslinking density of metal ions increases, leading to a more ordered hydrogen bond network. This observation is consistent with the LF-NMR inference of the transition from free water to bound water. The spectral differences become significant when cooled to -65°C. Figure 6 c). PAA-gel at 3110cm -1 A distinct ice crystal peak appeared nearby, indicating extensive freezing within the network. This sharp ice crystal peak was absent in both MDC-gel and LMDC-gel, suggesting that the metal chelate network suppressed the formation of macroscopic ice with a long-range ordered structure. The spectra of MDC-gel and LMDC-gel at -65℃ are at 3400 cm⁻¹. -1 and 3250cm -1 The vicinity shows well-distinguishable bimodal peaks ( Figure 6 c), reflecting the complexity of its internal water state. This bimodal distribution originates from the differentiation within the nanoconfined water network: the high-frequency component (approximately 3400 cm⁻¹) reflects this. -1 ) corresponds to intermediate water, whose hydrogen bond network remains dynamic but is geometrically constrained; low-frequency components (approximately 3250 cm⁻¹) -1 This corresponds to bound water strongly coupled with polymer chains and ions. In the LMDC-gel, the bimodal shift is generally towards a lower wavenumber (3416 cm⁻¹). -1 / 3256 cm -1 The low-frequency components are relatively stronger, consistent with its higher crosslinking density and stronger nanoconfining effect, resulting in stronger coupling and confinement of the internal water network. Integrating Raman spectroscopy and DSC analysis results allows for a consistent understanding of the solvent phase behavior. PAA-gel exhibits significant ice crystal growth. Although MDC-gel suppresses the Raman characteristic signal of macroscopic ice due to network confinement, it still shows evidence of partial freezing or nano-ice / defect ice formation thermodynamically, consistent with its DSC transition at -31.3℃. LMDC-gel, with its ultra-dense and uniform nanoframework, not only significantly lowers the freezing point but also strongly inhibits ice nucleation and growth. Therefore, most water molecules remain in an unfrozen, heterogeneously confined state. These molecular-level spectroscopic results explain why LMDC-gel remains unfrozen at temperatures as low as -91.8℃, while maintaining excellent low-temperature mechanical and electrochemical properties. The phase state of the solvent water directly determines the antifreeze protective performance of the hydrogel. Figure 12As shown, low-temperature optical microscopy at -40℃ (at the same magnification) reveals that LMDC-gel effectively inhibits ice crystal formation and maintains flexibility, while PAA-gel and MDC-gel exhibit extensive ice crystal formation. DSC shows that the thermal transition temperature of LMDC-gel is -91.8℃, significantly lower than that of MDC-gel (-31.3℃) and PAA-gel (12.6℃). Figure 6 d).
[0138] 8. Please refer to Figure 10 This application also passes Figure 10 The schematic diagram shows a comparison of the network structure changes and energy dissipation differences between LMDC-gel and conventional PAA-gel under external force. Experiments show that LMDC-gel has a high crosslinking density, a low proportion of hanging chains (only 0.3%, while PAA-gel reaches 85.68%, Table 1), and a highly uniform network structure (two-dimensional SAXS). Figure 5 (This has been confirmed). Therefore, under external force, the chain segments are subjected to uniform stress, which can achieve uniform stress distribution under tensile or compressive loads. In contrast, the PAA-gel network structure is heterogeneous, with short chains subjected to large stress and long chains subjected to small stress, resulting in severe stress concentration and ultimately brittle fracture in the irregular cross-linking region.
[0139] In terms of mechanical properties, the LMDC-gel obtained in Example 1-1, with a water content of nearly 70%, still exhibited excellent compression and tensile properties: the compressive strain reached 99%, the compressive strength was 69 MPa, the compressive modulus was 0.9 MPa (at 99% compressive strain), and the compressive toughness reached 6 MJ·m. -3 It far exceeds PAA-gel (0.28 MJ·m -3 PAA-gel and MDC-gel; the tensile strain reached 453.69% and the tensile strength was 1.66 MPa, which is better than PAA-gel and MDC-gel, and remained stable in 50 cycles of loading-unloading.
[0140] Furthermore, experiments verified that the hydrogel exhibits spring-like mechanical behavior, capable of lifting a 2 kg weight and vibrating harmoniously, while the PAA-gel fractures under tension. The compressive properties change with Zr. 4+ The increased concentration further confirms the contribution of a highly intact and homogeneous network to compressive strength. Rheological frequency scan ( Figure 7 e Figure 7f) The dynamic characteristics of the network were revealed from a macroscopic mechanical perspective. In the range of 0.01-10Hz, the energy storage modulus G′ of LMDC-gel (0.44MPa at 1Hz) is about 15 times higher than that of PAA-gel (28 kPa), and G′ exhibits extremely weak frequency dependence, forming a broad plateau region, which contrasts with the obvious softening of PAA-gel at low frequencies; its loss modulus G″ is much lower than G′ (G′ / G″> 10), and the loss factor tanδ is always less than 0.1, demonstrating a near-ideal elastic response.
[0141] On a macroscopic level, experiments also verified that LMDC-gel can bounce a steel ball dropped from 50 cm back to over 30 cm, while PAA-gel only bounces back to about 10 cm. These rheological characteristics indicate that the extremely low proportion of dangling chains in LMDC-gel (approximately 0.3%) effectively eliminates relaxation sites. Combined with the ultra-high crosslinking density and the nano-confinement effect brought about by the sub-100 nm pore structure, this strongly suppresses polymer chain movement and solvent molecule migration, thereby inhibiting low-frequency relaxation, forming a G′ plateau, and achieving extremely low energy dissipation. This conclusion is consistent with the freezing point depression measured by DSC, the ultra-short T2 relaxation time observed by LF-NMR, and the excellent anti-swelling dimensional stability, collectively verifying the core regulatory role of the nano-confined state. In this state, free water is effectively converted into bound water, endowing the material with solid-like elasticity, thus comprehensively regulating the thermodynamic, kinetic, and mechanical properties of the system. XAFS quantitative fitting results confirm Zr 4+ The presence of a coordination mode with water molecules (CN≈2.9) provides the network with a source of bonded water, which works synergistically with the ultra-dense network framework to give LMDC-gel excellent mechanical properties and low-temperature antifreeze properties.
[0142] 9. Electrochemical performance tests were conducted on the zinc-air batteries assembled in Example 2-1 and Comparative Example 2-1: 9.1 Electrochemical performance testing methods: Constant current charge-discharge cycles (6 min per cycle) were performed at 25℃, -40℃, and -65℃, at a rate of 0.5 mA·cm⁻¹. -2 and 0.2mA·cm -2 The current density was measured using a multi-channel battery testing system (LAND CT2001A, Wuhan Landian Electronics Co., Ltd., China). The constant current discharge curve was obtained at 0.5 mA·cm⁻¹. -2 Data was collected at the following depths. Power density (P) was calculated from the discharge polarization curve, P = JV, where J is the current density and V is the discharge voltage. All electrochemical measurements were performed three times.
[0143] Specific capacity calculation: Specific capacity is calculated based on the constant current discharge curve, using the mass of the zinc anode as the reference, and the unit is mAh·g. -1 .
[0144] Hydrogen bond analysis: Molecular dynamics simulations were used to analyze the hydrogen bond behavior in the hydrogel system, and the number and lifetime of strong hydrogen bonds at different temperatures were statistically analyzed.
[0145] Ionic conductivity measurement: Ionic conductivity was characterized using a CHI 760E electrochemical workstation (Shanghai Chenhua, China). Electrochemical impedance spectroscopy (IMP) was performed at a frequency range of 10 Hz. -1 Up to 10 5 Hz, amplitude of 0.1 V. The sample (10×10×5 mm) 3 The electrode is sandwiched between two foil electrodes for measurement. The ionic conductivity (σ) is calculated using the following formula (6): (6); Where L is the distance between the two probes, R is the resistance of the hydrogel, and A is its cross-sectional area. Temperature was controlled within ±0.5℃. Ionic conductivity measurements were performed using fully hydrated samples in a humidity chamber (relative humidity 30 ± 5%). Each reported value is the average of at least three independent measurements. The Arrhenius plot is plotted with ln σ on the ordinate and 1000 / T on the abscissa, with the activation energy obtained through linear fitting.
[0146] 9.2: Experimental Results like Figure 11 The figures show the electrochemical performance test results of the zinc-air batteries assembled in Example 2-1 and Comparative Example 2-1. In Example 2-1, the LMDC-gel prepared in Example 1-1 was used as the electrolyte, while in Comparative Example 2-1, the PAA-gel prepared in Comparative Example 1-1 was used as the electrolyte.
[0147] Please see Figure 11 A, LMDC-ZABs: Specific capacity of 769.27 mAh·g at 25℃ -1 At -65℃, it has a capacity of 608.88 mAh·g. -1 The capacity retention rate reached 79.1%. PAA-ZABs: Specific capacity at 25℃ is approximately 310.00 mAh·g. -1 Its specific capacity at room temperature is much lower than that of LMDC-ZABs; it cannot function properly at low temperatures.
[0148] Please see Figure 11 B. Discharge polarization curves and corresponding power densities, LMDC-ZABs: peak power density reaches 125.67 mW·cm² at 25℃. -2At -40℃, a relatively high limiting current and peak power density can still be achieved, although they are slightly lower than at 25℃, but the high-current discharge capability is well preserved. At the extremely low temperature of -6℃, the overall polarization increases, and the limiting current and peak power further decrease, but electrochemical output capability is still maintained. PAA-ZABs: At 25℃, polarization decay is significant, the limiting current density is low, and the peak power density is much lower than that of LMDC-ZABs. The voltage drops rapidly under high current; effective polarization output cannot be obtained at -40℃ and -65℃.
[0149] Please see Figure 11 C, Rate performance, LMDC-ZABs: at 0.1, 0.2, 0.5, 1.0 mA·cm -2 It maintains a stable discharge voltage plateau under all current densities, even at 1.0 mA·cm⁻¹. -2 It maintains a stable discharge voltage at -65℃. PAA-ZABs: Ion conduction is hindered at -65℃, and the voltage decays sharply, making it impossible to complete the gradient rate test. Therefore, the PAA-ZABs curve is not shown in this figure.
[0150] Please see Figure 11 D, Arrhenius diagram of ionic conductivity. The activation energy of LMDC-gel is only 0.177 eV, which is much lower than that of PAA-gel (0.45 eV), indicating that ion transport in LMDC-gel follows a Grotthuss-type proton coupling transport mechanism.
[0151] Please see Figure 11 E, Ionic conductivity histogram, the average ionic conductivity of LMDC-gel measured at 25℃ is 471.69 mS·cm -1 (The error bars in the figure represent the standard deviation of multiple measurements); even at an extreme low temperature of -65℃, the average value of its ionic conductivity measurement remained at 24.15 mS·cm. -1 .
[0152] Please see Figure 11 F, Constant current charge-discharge cycle curve; as shown in the figure, LMDC-ZABs can stably complete 500 charge-discharge cycles (cumulative operation of 2000h), during which the charge-discharge voltage remains stable and no capacity decay is observed. The figure shows representative data from 500 cycles. When the number of cycles is further extended to 20,000 cycles, the LMDC-ZABs battery can still maintain stable charge-discharge performance without significant capacity decay, indicating that the LMDC-gel electrolyte has excellent electrochemical stability and structural integrity during long-term operation at ultra-low temperatures.
[0153] Please see Figure 11In G, the number of strong hydrogen bonds in LMDC-gel is only 38% of that in PAA-gel.
[0154] Please see Figure 11 Comparison of hydrogen bond lifetimes at 25°C: LMDC-gel exhibits faster hydrogen bond breaking kinetics.
[0155] Please see Figure 11 I. Comparison of hydrogen bond lifetimes at -65°C: LMDC-gel maintains active hydrogen bond dynamics at -65°C, and can still achieve Grotthuss-type proton coupling transport even at low temperatures.
[0156] 9.3 Results Analysis: (1) LMDC-ZABs maintain excellent electrochemical performance (specific capacity ≥608.88 mAh·g) over a wide temperature range from 25℃ to -65℃. -1 Peak power density 125.67 mW·cm -2 The root cause lies in the nanoconfining effect generated by the ultra-dense cross-linked network of the LMDC-gel electrolyte. XAFS quantitative fitting results indicate that Zr... 4+ Two coordination modes exist: coordination with carboxylate ions (CN≈3.7) to form an ultra-dense network framework, and coordination with water molecules (CN≈2.9) to form hydrated ion clusters. The water coordination mode is an important source of bonded water, and in synergy with the nano-confinement effect, it converts free water molecules within the network into bonded water molecules, fundamentally inhibiting the formation and growth of ice crystals. This ensures that the electrolyte maintains unobstructed ion conduction channels at ultra-low temperatures, thereby guaranteeing normal charge and discharge of the battery at -65℃.
[0157] (2) The ultra-low activation energy of LMDC-gel (0.177 eV) is much lower than that of PAA-gel (0.45 eV), indicating that its ion transport has a lower energy barrier. Combined with the hydrogen bond analysis results, the number of strong hydrogen bonds in LMDC-gel is reduced (only 38% of that in PAA-gel), and the hydrogen bond breaking kinetics are faster (even at -65℃, the hydrogen bond kinetics remain active), confirming that it follows a Grotthuss-type proton coupling transport mechanism, that is, ions rapidly jump through the "break-formation" process of the hydrogen bond network, rather than relying on the physical diffusion of ions in solution. This mechanism enables the ion transport efficiency to remain at a high level at low temperatures, giving the electrolyte excellent low-temperature ion conduction performance.
[0158] (3) LMDC-ZABs can operate stably for more than 20,000 cycles at -65℃ without capacity decay. This ultra-long cycle stability is due to the triple structural advantages of the LMDC-gel electrolyte: First, the ultra-dense three-dimensional network structure endows the electrolyte with high mechanical strength, effectively resisting the local stress caused by zinc dendrite growth and volume changes during cycling; second, the dense network structure limits the excessive swelling of the electrolyte under alkaline conditions, ensuring structural stability during long-term cycling; third, the water molecule state dominated by bonded water avoids the puncture and damage to the network skeleton by ice crystals at low temperatures. The three factors work together to enable LMDC-ZABs to maintain stable interfacial contact and ion conduction performance during long-term operation at ultra-low temperatures.
[0159] In summary, system electrochemical testing and hydrogen bond analysis demonstrate that the zinc-air battery containing the LMDC-gel electrolyte exhibits excellent electrochemical performance (specific capacity ≥608.88 mAh·g) over a wide temperature range (25℃ to -65℃). -1 Peak power density 125.67 mW·cm³ -2 Furthermore, it can stably cycle for over 20,000 times without capacity decay under ultra-low temperature conditions of -65℃. These properties stem from the nano-confinence effect and Grotthuss-type proton coupling transport mechanism generated by the ultra-dense cross-linked network structure of the LMDC-gel, confirming the application potential of the zinc-air battery electrolyte and its preparation method provided in this application in the field of ultra-low temperature energy storage.
Claims
1. A method for preparing an electrolyte for a zinc-air battery, characterized in that, Includes the following steps: At least some of the carboxyl groups in a water-soluble olefinic unsaturated monomer are neutralized by an alkaline substance, wherein the molar ratio of the alkaline substance to the water-soluble olefinic unsaturated monomer is (0.5-1.5):1; A water-soluble olefinic unsaturated monomer, neutralized with an alkaline substance, an initiator, a metal ion crosslinking agent, and a reaction promoter are mixed in water and subjected to a polymerization and crosslinking reaction to obtain a hydrogel polymer. The hydrogel polymer is soaked in a first alkaline solution to obtain an electrolyte for zinc-air batteries; The metal ion crosslinking agent contains zirconium ions and / or hafnium ions, and the molar ratio of the metal ions in the metal ion crosslinking agent to the water-soluble olefinic unsaturated monomer is (0.3-5):
1.
2. The method for preparing the electrolyte for a zinc-air battery according to claim 1, characterized in that, The polymerization and crosslinking reaction is carried out at room temperature and left to stand for 10 minutes to 5 hours. When using an alkaline substance to neutralize a water-soluble olefinic unsaturated monomer, the molar ratio of the alkaline substance to the water-soluble olefinic unsaturated monomer is (0.8~1):1; In the polymerization and crosslinking reaction, the molar ratio of the initiator to the water-soluble olefinic unsaturated monomer is (0.0001~0.05):1; In the polymerization and crosslinking reaction, the molar ratio of the reaction promoter to the water-soluble olefinic unsaturated monomer is (0.0001~0.05):1; In the polymerization and crosslinking reaction, the molar ratio of the initiator to the reaction promoter is (0.8–1.2):1; In the polymerization and crosslinking reaction, the molar ratio of the metal ions in the metal ion crosslinking agent to the water-soluble olefinic unsaturated monomer is (0.5-2):1; In the polymerization and crosslinking reaction, the water accounts for 60 wt% to 80 wt% of the total mass of the polymerization and crosslinking reaction system.
3. The method for preparing the electrolyte for a zinc-air battery according to claim 2, characterized in that, The reaction time for the polymerization and crosslinking reaction is 10 minutes to 1 hour; In the polymerization and crosslinking reaction, the molar ratio of the initiator to the water-soluble olefinic unsaturated monomer is (0.0003~0.005):1; In the polymerization and crosslinking reaction, the molar ratio of the reaction promoter to the water-soluble olefinic unsaturated monomer is (0.0003~0.005):1; In the polymerization and crosslinking reaction, the molar ratio of the initiator to the reaction promoter is (0.9–1.2):1; In the polymerization and crosslinking reaction, the water accounts for 65 wt% to 75 wt% of the total mass of the polymerization and crosslinking reaction system.
4. The method for preparing the electrolyte for a zinc-air battery according to any one of claims 1 to 3, characterized in that, The water-soluble olefinic unsaturated monomer is acrylic acid and / or methacrylic acid; or, the water-soluble olefinic unsaturated monomer is a composition of acrylic acid and / or methacrylic acid and other olefinic unsaturated monomers, and the mass percentage of acrylic acid and / or methacrylic acid in the composition is not less than 60%; The metal ions in the metal ion crosslinking agent also include other metal ions, which are selected from at least one of calcium ions, zinc ions, nickel ions, copper ions, cobalt ions, iron ions, and aluminum ions, and the proportion of the other metal ions in the total molar number of metal ions does not exceed 20%. The metal ion crosslinking agent is zirconium tetrachloride; The initiator is ammonium persulfate; The cross-linking accelerator is ascorbic acid; The water is deionized water or distilled water.
5. The method for preparing the electrolyte for a zinc-air battery according to any one of claims 1 to 3, characterized in that, When the hydrogel polymer is soaked in the first alkaline solution: the mass ratio of the hydrogel polymer to the first alkaline solution is 1:140 to 160, the soaking time is 6 hours to 24 hours, and the soaking temperature is 15℃ to 40℃. The first alkaline solution is an aqueous solution of potassium hydroxide, and the concentration of potassium hydroxide in the first alkaline solution is 2 mol / L to 8 mol / L; or, the first alkaline solution is a mixed aqueous solution of potassium hydroxide and zinc acetate, and the concentration of potassium hydroxide in the first alkaline solution is 2 mol / L to 8 mol / L, and the concentration of zinc acetate is 0.1 mol / L to 1 mol / L.
6. An electrolyte for zinc-air batteries prepared by the preparation method according to any one of claims 1 to 5.
7. A zinc-air battery, characterized in that, The battery includes a zinc anode, an air cathode, and an electrolyte disposed between the zinc anode and the air cathode, wherein the electrolyte is prepared by any one of claims 1 to 5; or, the electrolyte is the electrolyte for a zinc-air battery as described in claim 6.
8. A method for regenerating a zinc-air battery, characterized in that, Includes the following steps: Provide the zinc-air battery as described in claim 7; The hydrogel electrolyte in the zinc-air battery is removed and immersed in a second alkaline solution to restore the electrolyte's ion conduction properties. The regenerated electrolyte is reassembled between the zinc anode and the air cathode to complete battery regeneration.
9. The method for regenerating a zinc-air battery according to claim 8, characterized in that, When the hydrogel electrolyte is immersed in the second alkaline solution: the mass ratio of the hydrogel electrolyte to the second alkaline solution is 1:140 to 160, the immersion time is 6 hours to 24 hours, and the immersion temperature is 15°C to 40°C. The second alkaline solution is an aqueous solution of potassium hydroxide, wherein the concentration of potassium hydroxide in the second alkaline solution is 2 mol / L to 8 mol / L; or, the second alkaline solution is a mixed aqueous solution of potassium hydroxide and zinc acetate, wherein the concentration of potassium hydroxide in the second alkaline solution is 2 mol / L to 8 mol / L, and the concentration of zinc acetate is 0.1 mol / L to 1 mol / L.
10. An energy storage system, characterized in that, Including at least one zinc-air battery as described in claim 7.