O3 / p3 sodium ion layered oxide positive electrode fast charging window control method
By integrating XRD, Raman, and dQ/dV test data, and combining material degradation status and phase transition risk, charging parameters were dynamically adjusted to solve the structural stability and compatibility issues of O3/P3 sodium ion layered oxide cathodes under high-voltage fast charging, thereby improving the fast charging safety and cycle life of the battery cell.
Patent Information
- Application Number
- CN202611273636.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot accurately identify the effective P3 local structure in the O3/P3 sodium ion layered oxide cathode, leading to sodium layer slippage, sodium vacancy rearrangement, and transition metal ion migration under high-voltage fast charging. This results in rapid capacity decay and rate performance degradation during cell cycling. Furthermore, the fast charging window design is too large, making it impossible to ensure compatibility with different production batches.
By integrating XRD, Raman, and dQ/dV test data, and combining the material degradation state and phase transition risk, the charging current, upper limit voltage, and constant voltage holding time are dynamically adjusted to achieve adaptive switching of fast charging strategy. Effective P3 structures are screened through structural consistency coefficient and electrochemical activity coefficient, and fast charging window control parameters are quantified.
Significantly reduces interlayer slip and transition metal migration under high voltage and high SOC conditions, improves cell fast charging safety and cycle life, enhances batch compatibility, avoids performance waste, and enables a continuous calculation link between material testing data and BMS control parameters.
Smart Images

Figure CN123121941A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of sodium-ion battery energy storage and battery management technology, and more specifically, to a method for controlling the fast charging window of an O3 / P3 sodium-ion layered oxide cathode. Background Technology
[0002] Sodium-ion batteries, with their advantages of abundant resources, low cost, and excellent low-temperature performance, have broad application prospects in energy storage, low-speed transportation, and backup power. O3-type sodium-ion layered oxide cathodes, due to their high initial sodium reserves and large reversible capacity, are the core cathode material for achieving high energy density in sodium-ion batteries. However, under high voltage and high SOC fast-charging conditions, these materials are prone to sodium layer slip, sodium vacancy rearrangement, transition metal ion migration, and irreversible crystal phase transitions, directly blocking sodium ion transport channels and increasing interfacial charge transfer resistance, resulting in rapid capacity decay and continuous degradation of rate performance during cell cycling. While the P3-type localized structure generated within the material can broaden sodium ion migration channels and optimize fast-charging kinetics, an excessively high overall P3 phase proportion can significantly reduce the initial sodium reserves and electrode compaction density, sacrificing cell energy density. It is evident that there is a balancing relationship between the local structure inside the O3 / P3 mixed-phase cathode and the high-voltage fast charging range. Relying solely on the proportion of a single phase or the external electrical threshold of the cell cannot accurately match and adapt to the fast charging window. How to accurately identify the local P3 structure that truly has a fast charging gain effect and dynamically adjust the fast charging parameters accordingly is a core problem that urgently needs to be solved for the large-scale application of high-voltage O3 / P3 sodium ion layered oxide cathodes.
[0003] Current technologies mostly employ X-ray diffraction (XRD), Raman spectroscopy, and differential capacity curves (dQ / dV) for material analysis. These three detection tools can only characterize single-dimensional information in isolation: XRD can only reflect the macroscopic long-range average crystal phase composition of the material and cannot identify locally disordered or discontinuous P3 transport channels; Raman can only capture short-range atomic bonding and local distortions and cannot determine the long-range crystal source corresponding to local distortions; dQ / dV can only capture electrochemical reaction polarization and phase transition peaks and cannot distinguish whether the peak signal originates from effective P3 ion channels, interfacial side reactions, or local lattice degradation. In the industry, only simple weighted calculations are performed on the three types of data, and no multi-signal consistency verification and electrochemical activity screening mechanism has been established. A large number of false P3 signals generated by residual impurities, lattice disorder, and side reactions are misjudged as structures favorable for fast charging, ultimately resulting in an oversized fast charging window design, which exacerbates high-voltage irreversible phase transitions and cycle degradation.
[0004] Traditional battery fast charging control logic only relies on external electrical indicators such as real-time voltage, temperature, SOC, ohmic internal resistance, and interface polarization to perform operations such as current limiting, voltage reduction, and shortening constant voltage time, completely ignoring the differences in the internal microstructure of the cathode. Even within the same chemical system, O3 / P3 cathodes exhibit significant differences in local effective P3 ratio, transition metal migration, and lattice defect concentration due to variations in sintering process, production batch, and cycle aging. This results in completely different phase transition risks and sodium ion diffusion capabilities. If a fixed fast charging rate, fixed charging upper limit voltage, and fixed constant voltage holding time are used across all batches, two extreme problems will arise: For cells with severe lattice degradation and low effective P3 ratio, fixed high-power fast charging will accelerate interlayer slip and transition metal migration, significantly shortening cycle life; for cells with sufficient effective P3 structure and excellent structural stability, stringent fixed parameters will limit the release of fast charging performance, failing to leverage the advantages of material kinetics. Existing technologies only consider the proportion of crystal phase or a single electrical constraint, without simultaneously integrating the triple detection information of long-range crystal, short-range local, and electrochemical. They also fail to establish a joint calculation relationship by simultaneously coupling multiple influencing factors such as effective P3 structure gain, transition metal migration damage, lattice defect degradation, high-voltage cumulative slip, temperature rise loss, and interface polarization. Consequently, they cannot simultaneously output the three sets of core control parameters—adaptive fast charging current, charging upper limit voltage, and constant voltage holding time—making it difficult to upgrade from fixed threshold charging to adaptive dynamic charging of material state. In summary, existing technologies cannot distinguish between detected P-type impurities and the effective P3 local structures that actually participate in the rapid transport of sodium ions. They also lack a complete quantitative model that integrates XRD, Raman, and dQ / dV multi-source signals with the material's microscopic degradation state to jointly calculate the fast-charging window. Furthermore, there is a lack of a continuous and executable computational link between material detection data and BMS fast-charging control parameters, making it difficult to simultaneously consider the fast-charging capability, high-voltage cycle stability, and compatibility with different production batches of sodium-ion batteries. Therefore, this invention provides a method for dynamic polarization separation and source identification in sodium-ion batteries that solves the above problems. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a fast charging window control method and system for O3 / P3 sodium ion layered oxide cathodes. It integrates three types of detection data—XRD, Raman, and dQ / dV—to identify effective P-type fast charging structures. It combines material degradation state and phase transition risk quantification to calculate fast charging constraints, dynamically adjusts charging current, upper limit voltage, and constant voltage holding time, and realizes adaptive switching of fast charging strategy according to cathode structure state, thereby improving cell fast charging safety, cycle life, and batch compatibility.
[0006] To address the aforementioned technical problems, one objective of this invention is to provide a method for controlling the fast charging window of an O3 / P3 sodium ion layered oxide cathode, comprising the following steps: Three types of material characterization data were collected for the cathode: XRD, Raman, and dQ / dV. The three types of characterization data were then fused together, and the original P-type ratio, structural consistency coefficient, and electrochemical activity coefficient were calculated in sequence to obtain the effective fast-charging structure ratio of the local P-type. Based on the characterization data and charge transfer impedance and irreversible capacity, the transition metal migration index and normalized concentration of structural defects were calculated respectively, and the structural slip accumulation state was obtained by recursion based on cell voltage and SOC. The basic sodium ion solid-phase diffusion coefficient is calculated based on the cell temperature. The effective sodium ion diffusion coefficient is then corrected by combining the proportion of effective fast-charging structure of local P-type, the transition metal migration index, and the normalized concentration of structural defects. Based on SOC, the normalized value of high SOC is calculated. Combined with cell voltage, structural slip accumulation state, transition metal migration index, and the proportion of local P-type effective fast charging structure, the high SOC phase transition risk index is calculated.
[0007] As a further improvement to this technical solution, step S2, the calculation sub-step for the proportion of the original local P-type effective fast charging structure, includes: S201. Calculate the peak intensity ratio of XRD based on the characteristic peak intensities of P3 and O3 within the XRD; obtain the Raman local structure factor by normalizing the Raman vibration peak information; calculate the normalized value of the peak spacing based on the voltage difference between the O3 / P3 reaction peaks within the dQ / dV curve. S202. The original local P-type structure ratio is obtained by weighted summation of the XRD peak intensity ratio, Raman local structure factor, and dQ / dV peak spacing normalization value and interval constraint. S203. Calculate the structural consistency coefficient by weighted penalty of pairwise differences of three sets of data; S204. The electrochemical activity coefficient is calculated by combining the electrochemical diffusion response, interfacial overpotential, and charge transfer impedance weighting. S205. Multiply the original local P-type structure ratio, structural consistency coefficient, and electrochemical activity coefficient and project them to the 0 to 1 interval to obtain the effective fast-charging structure ratio of the local P-type.
[0008] As a further improvement to this technical solution, the transition metal migration index is obtained by using XRD interplanar spacing shift, Raman peak width variation, and dQ / dV abnormal peak area weighted normalization. The normalized concentration of structural defects was obtained by using the XRD full width at half maximum (FWHM), steady-state charge transfer impedance, and irreversible capacity weighted normalization. Using sampling duration, charging overvoltage, SOC, transition metal migration index, and the proportion of effective P-type fast charging structures in the local area as variables, the structural slip accumulation state of the next cycle is recursively calculated and restricted to the range of 0 to 1.
[0009] As a further improvement to this technical solution, the effective diffusion coefficient is calculated as follows: The temperature-dependent basic Na ion solid-phase diffusion coefficient was calculated using the Arrhenius formula. Then, exponential corrections were made by introducing a localized P-type effective fast-charging structure proportional gain term, a transition metal migration suppression term, and a structural defect suppression term. After interval constraints, the effective diffusion coefficient was obtained.
[0010] As a further improvement to this technical solution, the calculation steps for the high SOC phase transition risk index are as follows: S301. Set a high SOC normalization variable and assign risk weights only to the SOC interval that is higher than the risk initiation threshold. S302, a linear combination is constructed with charging overvoltage, high SOC normalization, structural slip accumulation, and transition metal migration index as risk additions, and the proportion of local P-type effective fast charging structure as a risk mitigation term. S303. The combined calculation results are mapped to the 0 to 1 interval by using the Sigmoid function to obtain the high SOC phase transition risk index.
[0011] As a further improvement to this technical solution, the diffusion constraint current, phase change constraint current, thermal constraint current, and interface constraint current are calculated respectively, and the minimum value among the four is taken as the current allowable fast charging current. The calculation methods for the four types of constraint currents are as follows: Diffusion-constrained current: calculated by combining the effective diffusion coefficient, positive electrode particle size, and current state of charge (SOC). Diffusion-constrained current formula:
[0012] in, For diffusion-constrained current; This is the conversion factor for diffusion current; Effective reaction area; The effective Na ion diffusion coefficient; The equivalent radius of the positive electrode particle; It is in a charged state; and It is a very small positive number; Phase change constraint current: linearly decreases as the phase change risk index increases with high SOC, with the upper limit being the rated fast charging current of the cell; Phase change confinement current formula:
[0013] in, This is the phase-change constraint current; Rated fast charging current; A high SOC phase transition risk index; This serves as a reference value for phase transition risk. This represents the upper limit of phase transition risk. It is a very small positive number; Thermal constraint current: calculated by taking the square root of the cell heat capacity, ambient heat transfer capacity, and total internal resistance heat loss, with a result not less than 0; Thermal confinement current formula:
[0014] in, This is the thermal confinement current; This refers to the equivalent heat capacity of the battery cell. Maximum permissible temperature; The current temperature; The sampling period; The heat transfer coefficient; For heat exchange area; The ambient temperature; The internal resistance is ohmic; It is the charge transfer impedance; Minimal positive number Interface constraint current: solved by combining charging voltage margin, ohmic internal resistance, and charge transfer impedance; Interface constraint current formula:
[0015] in, For interface constraint current; This is the open-circuit voltage under the current SOC. To allow for polarization margin; The internal resistance is ohmic; It is the charge transfer impedance; It is a very small positive number; By comparing the four types of current values, the minimum value is selected as the allowable fast charging current.
[0016] As a further improvement to this technical solution, the charging upper limit voltage for the next cycle is corrected based on the high SOC phase transition risk index and the proportion of effective local P-type fast charging structure. The constant voltage holding time for the next cycle is also corrected based on the high SOC phase transition risk index and the interface charge transfer overpotential. The charging upper limit voltage correction rule is as follows: When the high SOC phase transition risk index is higher than the preset reference value, a voltage reduction correction is performed; when the proportion of effective P-type fast charging structure in the local area is higher than the reference proportion, a small voltage compensation is performed; the corrected voltage is limited to the minimum and maximum voltage range allowed by the material by the projection operator. The correction rule for constant pressure holding time is as follows: When the high SOC phase transition risk index or the interface charge transfer overpotential exceeds the standard, the constant voltage time shall be shortened according to the corresponding coefficients; the correction result shall be limited to the preset minimum and maximum constant voltage time range and shall not exceed the limit.
[0017] As a further improvement to this technical solution, the fast charging current, the corrected upper limit charging voltage, and the constant voltage holding time will be allowed to be output to the battery management system or the formation and capacity testing equipment for execution.
[0018] As a further improvement to this technical solution, two switchable operating modes are also included: Offline high-precision mode: Fully utilizes three types of characterization data: XRD, Raman, and dQ / dV, to complete the calibration of the proportion of effective fast-charging structures of local P-type, the migration index of transition metals, and the normalized concentration of structural defects; Online lightweight mode: Reuses the microstructure parameters completed by offline calibration, and only collects online data of cell voltage, temperature and SOC to complete the real-time calculation of fast charging window.
[0019] The second objective of this invention is to provide a fast-charging window control system for O3 / P3 sodium ion layered oxide cathodes, comprising: The data acquisition module is used to acquire XRD, Raman, dQ / dV characterization data, as well as cell voltage, current, temperature, SOC, and electrochemical impedance operating data. An effective structure calculation module is used to execute the sub-step of claim 2, calculating the proportion of local P-type effective fast charging structures; The degradation index calculation module is used to calculate the transition metal migration index, the normalized concentration of structural defects, and the structural slip accumulation state. The multiphysics calculation module is used to solve for the effective diffusion coefficient, the high SOC phase transition risk index, four types of constraint currents, and the allowable fast charging current. The charging parameter correction module is used to dynamically correct the upper limit voltage of charging and the constant voltage holding time. The instruction output storage module generates tiered fast charging control instructions, sends them to the execution device, and stores all status parameters and operating results for each cycle.
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention introduces a dual-layer screening mechanism using structural consistency coefficient and electrochemical activity coefficient: the structural consistency coefficient is used to verify the matching degree of XRD long-range crystal, Raman short-range localization, and dQ / dV electrochemical signals, thus eliminating false P characteristic peaks caused by residual impurities and lattice disorder; then, the electrochemical activity coefficient is used to screen channels with actual sodium ion transport capabilities from the dimensions of ion diffusion, interface polarization, and charge impedance, quantifying the proportion of effective fast-charging structures of local P-type, fundamentally excluding invalid structural signals generated by residual phases and interface side reactions from the calculation of the fast-charging window, avoiding setting an excessively large charging window due to overestimation of the material's fast-charging capability, significantly reducing the probability of interlayer slip, transition metal migration, and irreversible phase transitions under high voltage and high SOC conditions, and effectively reducing the cell capacity decay rate and the increase in internal resistance; This invention incorporates three types of microscopic degradation indicators—transition metal migration index, normalized concentration of structural defects, and time-accumulated lattice slip state—into a unified calculation framework to comprehensively reflect the negative impacts of crystal plane distortion, defect enrichment, and continuous high-voltage damage on battery cells. Simultaneously, a high-SOC phase transition risk sigmoid quantification model is established, mapping voltage overload, high charge ratio, lattice damage, and the effective P-phase mitigation effect to standardized risk values of 0 to 1. Differentiated fast-charging boundaries are matched for battery cells with different effective P ratios and varying degrees of degradation. For structurally degraded battery cells, current and voltage are reduced, and the constant-voltage duration is shortened to avoid over-fast charging. For structurally superior battery cells, the fast-charging potential is fully released. This addresses the dual pain points of "accelerated failure of degraded battery cells and wasted performance of high-quality battery cells" caused by fixed fast-charging parameters, significantly improving the batch compatibility of battery cells. This invention uses the effective P-type ratio as a high-voltage tolerance gain factor to compensate for the upper limit of the charging voltage, and uses phase change risk and interface polarization as damage constraints to simultaneously lower the voltage and shorten the high SOC constant voltage holding time. It achieves linkage and adaptive correction of three core control parameters: fast charging current, charging cut-off voltage, and constant voltage duration. It directly outputs standardized control parameters that can be written into BMS and formation and capacity testing equipment. It opens up the data and calculation channels for offline testing of material research and development, online management and control of production, and terminal battery management, eliminating the data gap between material process and battery control. It is suitable for the entire process of material screening, cell formation, and terminal energy storage / vehicle application. This invention features two switchable operating architectures: an offline mode that fully utilizes XRD, Raman, dQ / dV, EIS, and full-volume testing data to accurately calibrate the inherent structural parameters of different material systems and processes, suitable for laboratory material development and production line batch process verification; and an online lightweight mode that only collects conventional electrical signals such as voltage, current, temperature, and SOC, reusing the effective P-ratio and degradation characteristic parameters completed in offline calibration for low-computing-power iterative calculations, which can be directly integrated with commercial BMS chips without the need for external large-scale testing equipment. Attached Figure Description
[0021] Figure 1 Flowchart of the fast charging window control method for O3 / P3 sodium ion layered oxide cathode of this invention; Figure 2 This is a flowchart for calculating the proportion of the local P-type effective fast charging structure of the present invention; Figure 3 This is a flowchart of the fast charging window joint constraint calculation for the present invention. Figure 4 This is a flowchart illustrating the overall process of the present invention. Detailed Implementation
[0022] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] Method Implementation Examples The core idea of this invention is to address the structural evolution, diffusion capacity changes, and charging window changes of the O3 / P3 sodium ion layered oxide cathode during high-voltage fast charging. The invention incorporates material testing data, cell operation data, and process parameters into the same calculation process. The model first obtains the material structure state and cell operation state based on measurable data, then calculates four types of limiting conditions: diffusion, phase change, heat, and interface. Finally, it outputs the allowable fast charging current, upper limit voltage, constant voltage holding time, and fast charging level.
[0024] like Figure 1 As shown, this embodiment provides a method for controlling the fast charging window of an O3 / P3 sodium ion layered oxide cathode, including the following steps (refer to...). Figure 1 ): S1. Collect three types of material characterization data for the positive electrode: XRD, Raman, and dQ / dV. Simultaneously collect online operating data of cell voltage, current, temperature, SOC, and electrochemical impedance. Combine the three types of characterization data to calculate the original P-type ratio, structural consistency coefficient, and electrochemical activity coefficient in sequence, thereby calculating the effective fast-charging structure ratio of the local P-type. S2. Based on the characterization data and charge transfer impedance and irreversible capacity, the transition metal migration index and the normalized concentration of structural defects are calculated respectively, and the structural slip accumulation state is obtained by recursion with cell voltage and SOC. S3. Calculate the basic sodium ion solid-phase diffusion coefficient based on the cell temperature, and then correct the effective sodium ion diffusion coefficient by combining the proportion of local P-type effective fast charging structure, the transition metal migration index, and the normalized concentration of structural defects. S4. Calculate the high SOC normalized value based on SOC, and combine it with cell voltage, structural slip accumulation state, transition metal migration index, and the proportion of local P-type effective fast charging structure to calculate the high SOC phase transition risk index.
[0025] As a further improvement to this technical solution, the calculation sub-steps for the original local P-type effective fast charging structure ratio include: S201. Calculate the peak intensity ratio of XRD based on the characteristic peak intensities of P3 and O3 within the XRD; obtain the Raman local structure factor by normalizing the Raman vibration peak information; calculate the normalized value of the peak spacing based on the voltage difference between the O3 / P3 reaction peaks within the dQ / dV curve. S202. The original local P-type structure ratio is obtained by weighted summation of the XRD peak intensity ratio, Raman local structure factor, and dQ / dV peak spacing normalization value and interval constraint. S203. Calculate the structural consistency coefficient by weighted penalty of pairwise differences between three sets of data. ; S204, Calculate the electrochemical activity coefficient by combining electrochemical diffusion response, interfacial overpotential, and charge transfer impedance weighting. ; S205, Adjust the original local P-type structure ratio and structural consistency coefficient. Electrochemical activity coefficient Multiply and project onto the 0 to 1 range to obtain the local P-type effective fast charging structure ratio. .
[0026] The structural consistency coefficient ranges from 0 to 1. The lower the value, the worse the matching degree of the three types of characterization signals, and the lower the credibility of the original P-type structure proportion. The electrochemical activity coefficient ranges from 0 to 1. The lower the value, the weaker the sodium ion transport capability of the corresponding P-type structure, and it cannot be used for fast charging gain.
[0027] Specifically, refer to Figure 2 The XRD, Raman, and dQ / dV signals originate from the long-range crystal structure, short-range local structure, and electrochemical phase transition response, respectively. If the three signals change in the same direction, it indicates that the p-type structure is more likely to participate in Na ion migration and high-voltage structural stability. If the three signals differ significantly, there may be residual phases, local disorder, or electrochemical spurious peaks. Based on this characteristic, this invention does not directly use a simple weighted value as the final structure ratio, but introduces structural consistency verification and electrochemical activity screening on the basis of the original ratio.
[0028] To obtain the P-type correlation ratio on the XRD side, the XRD peak intensity ratio is first calculated based on the intensity of the characteristic peak of P3 or P-type local structure and the intensity of the characteristic peak of O3.
[0029] in, For the first The proportion of P-type correlation peak intensity obtained from periodic XRD calculations ranges from 0 to 1; is the intensity of the characteristic peak of P3 or P-type local structure in XRD, and the value is a non-negative number; is the intensity of the characteristic peak of the O3 structure in XRD, and the value is a non-negative number; It is a very small positive number.
[0030] In order to make the dQ / dV peak spacing compatible with XRD and Raman data in the same calculation scale, this invention normalizes the peak spacing of O3 / P3; the normalized value can be based on the voltage span of the entire SOC range or the reference peak spacing of the same material system.
[0031] in, dQ / dV is the normalized value of the peak spacing, ranging from 0 to 1; The voltage of the P3-related reaction is expressed in V. This represents the peak voltage of the O3-related reaction, in volts (V). The voltage span across the entire SOC range or the reference peak spacing for the same material system, expressed in V, with a typical value range of 0.1 to 1.5. It is a very small positive number.
[0032] After obtaining the three types of structure-related inputs, the original local P-type structure ratio is first calculated. This ratio is used to integrate XRD long-range structure information, Raman short-range structure information, and dQ / dV electrochemical phase transition information, but it is not directly used as a subsequent fast-charging control quantity.
[0033]
[0034] in, This represents the original local P-type structure ratio, with a value ranging from 0 to 1. The proportion of P-type correlation peak intensity obtained from XRD calculation; , is the Raman local structure factor, with a value ranging from 0 to 1, which can be obtained by normalizing the intensity, width or position shift of the P-type correlated vibration peak; This represents the normalized value of the dQ / dV peak spacing; , , These are the weights for the XRD term, Raman term, and dQ / dV term, respectively, all ranging from 0 to 1, and satisfying the following conditions: .
[0035] To avoid overestimating the proportion of P-type structures due to anomalies in a single detection signal, this invention further calculates a structural consistency coefficient. The consistency coefficient is high when the XRD, Raman, and dQ / dV signals are close to each other; conversely, the consistency coefficient decreases when any two signals differ significantly, thus weakening the weight given to this structural proportion in the fast-charging window calculation.
[0036]
[0037] in, This is the structural consistency coefficient, with a value ranging from 0 to 1; This is the consistency penalty coefficient between XRD and Raman, with a value ranging from 0 to 1; This is the consistency penalty coefficient between XRD and dQ / dV, with a value ranging from 0 to 1; This is the consistency penalty coefficient between Raman and dQ / dV, with a value ranging from 0 to 1. Preferably, .
[0038] Structural consistency alone is insufficient to determine whether a P-type structure truly participates in the fast-charging process. If a P-type related peak exists in the material, but the interfacial polarization is large, the impedance is high, or the diffusion response is poor, then this part of the structure cannot provide an effective contribution to fast charging. Therefore, this invention calculates the electrochemical activity coefficient based on diffusion response, interfacial polarization, and charge transfer impedance.
[0039]
[0040] in, This is the electrochemical activity coefficient, with a value ranging from 0 to 1; The electrochemical diffusion response coefficient is obtained from GITT, PITT, charge-rest-relaxation, rate testing, or equivalent circuit identification, and is expressed in cm⁻¹. 2 / s; The reference diffusion response coefficient for the same material system is given in cm⁻¹. 2 / s; This represents the interfacial charge transfer overpotential, expressed in V. To allow an upper limit for interface polarization, the unit is V, and the typical value range is 0.05 to 0.30; This is the charge transfer impedance, measured in Ω. The upper limit of the allowable charge transfer impedance, in Ω; , , These are the weights corresponding to the diffusion response, interfacial polarization, and charge transfer impedance, respectively, all ranging from 0 to 1, and satisfying the following conditions: , It is a very small positive number.
[0041] After obtaining the original localized P-type structure ratio, structural consistency coefficient, and electrochemical activity coefficient, this invention calculates the effective fast-charging structure ratio of the localized P-type. This ratio is used for subsequent diffusion capability correction, structural slip suppression, reduction of high SOC phase transition risk, and upper limit voltage compensation.
[0042]
[0043] in, The effective fast charging structure ratio of the local P-type is 0 to 1; This represents the original local P-type structure proportion; The structural consistency coefficient; The coefficient is the electrochemical activity coefficient.
[0044] The purpose of the above formula is to distinguish the detected P-type structure from the P-type structure that actually participates in fast charging transmission and high-voltage stability. If the XRD shows a strong P-type correlation peak, but the Raman and dQ / dV do not change accordingly, Decrease; if the signals of the three types of structures are consistent, but the electrochemical diffusion response is poor, the polarization is large, or the impedance is high, Decrease. The result is... It is more suitable for entering the fast charging window control.
[0045] The transition metal migration index was obtained by using XRD interplanar spacing shift, Raman peak width variation, and dQ / dV abnormal peak area weighted normalization. The normalized concentration of structural defects was obtained by using the XRD full width at half maximum (FWHM), steady-state charge transfer impedance, and irreversible capacity weighted normalization. Using sampling duration, charging overvoltage, SOC, transition metal migration index, and the proportion of effective P-type fast charging structures in the local area as variables, the structural slip accumulation state of the next cycle is recursively calculated and restricted to the range of 0 to 1.
[0046] Specifically, high-voltage charging increases the likelihood of transition metal ions migrating from the transition metal layer to the Na layer; this process disrupts the order of the layered structure, blocks the Na ion diffusion channels, and increases the risk of subsequent irreversible phase transitions.
[0047] To quantify the degradation of this type of structure in the model, this invention combines... Transition metal migration index is calculated using interplanar spacing shift, Raman peak width variation, and abnormal peak area at high voltage dQ / dV.
[0048]
[0049] in, For the first The periodic transition metal migration index, with values ranging from 0 to 1; This refers to the offset related to the interlayer spacing of the transition metal in the XRD or Rietveld refinement results, with the unit uniformly in Å and the value being a non-negative number. The reference interplanar spacing for the same material system is expressed in Å. This represents the Raman peak width or the defect-related peak width, and its value is a non-negative number. This is the Raman reference peak width, and the value is a positive number. The abnormal peak area of dQ / dV in the high voltage region is a non-negative number. The reference peak area for dQ / dV in the low voltage or normal reaction region is a non-negative number. , , These are weighting coefficients, all ranging from 0 to 1, and satisfying the following conditions: ; It is a very small positive number.
[0050] in, The integration interval is to The high voltage abnormal peak region that appears between them, or the voltage range in the same material system where structural slip is confirmed by in-situ XRD, is used as the integration interval; The integration interval is to The main reaction peak region between [a certain point in time]. The above integral intervals remain consistent within the same material system, the same testing regime, and the same batch evaluation.
[0051] During the preparation, storage, formation and cycling of cathode materials, lattice defects, interfacial impedance growth and irreversible capacity loss will also occur; the above factors will jointly reduce the effective Na ion diffusion capacity and accelerate the structural degradation in the high voltage region.
[0052] To avoid evaluating material defects using only a single peak width or a single impedance, this invention incorporates XRD half-peak width, charge transfer impedance, and irreversible capacitance into the defect concentration calculation.
[0053]
[0054] in, For the first Normalized concentration of periodic structural defects, ranging from 0 to 1; is the full width at half maximum (FWHM) of the XRD characteristic peak, and its value is a non-negative number. The reference half-peak width is taken as a positive number; This is the charge transfer impedance, measured in Ω, and its value is a non-negative number. The reference charge transfer impedance is expressed in Ω and is a positive number. The capacity is irreversible, and the unit is uniformly mAh / g or Ah, with a non-negative value. Initial capacity or rated capacity, unit is... Consistent; , , These are weighting coefficients, all ranging from 0 to 1, and satisfying the following conditions: ; Minimal positive number The effective diffusion coefficient is calculated as follows: The temperature-dependent basic Na ion solid-phase diffusion coefficient was calculated using the Arrhenius formula. Then, exponential corrections were made by introducing a localized P-type effective fast-charging structure proportional gain term, a transition metal migration suppression term, and a structural defect suppression term. After interval constraints, the effective diffusion coefficient was obtained.
[0055] Specifically, the basic diffusion coefficient mainly reflects the influence of temperature and activation energy on Na ion migration. However, the actual fast-charge diffusion capability of the O3 / P3 cathode is also affected by the proportion of local P-type effective fast-charge structures, transition metal migration, and structural defects. A higher proportion of local P-type effective fast-charge structures indicates that more P-type related structures are both confirmed by structural signals and supported by electrochemical activity, which is more conducive to the rapid migration of Na ions. Transition metal migration and defect accumulation, on the other hand, hinder ion transport. Therefore, this invention adds a structural correction term to the basic diffusion coefficient to obtain the effective diffusion coefficient.
[0056]
[0057] in, For the first Periodic effective Na ion diffusion coefficient, in cm 2 / s, the typical value range is to ; The basic Na ion solid-phase diffusion coefficient is expressed in cm⁻¹. 2 / s; The effective fast charging structure ratio of the local P-type is 0 to 1; This is the transition metal migration index, with a value ranging from 0 to 1; This represents the normalized concentration of structural defects, with a value ranging from 0 to 1. The gain coefficient of the local P-type effective fast charging structure ratio on the diffusion capability is typically 0 to 10, with a preferred range of 1 to 5. The value is the inhibition coefficient of transition metal migration on diffusion ability, with a conventional range of 0 to 10 and a preferred range of 1 to 4. The value is the inhibition coefficient of structural defects on diffusion ability, with a conventional range of 0 to 10 and an preferred range of 1 to 4.
[0058] The purpose of this formula is to incorporate the local P-type structure that actually participates in fast charging transmission into the diffusion capability calculation. Through this formula, the model can distinguish between materials that "detect P-type peaks but have low electrochemical activity" and materials that "have structural signals consistent with electrochemical responses and high fast charging effectiveness," thereby improving the accuracy of fast charging window determination.
[0059] The calculation steps for the high SOC phase transition risk index are as follows: S401. Set a high SOC normalization variable and assign risk weights only to the SOC range that is higher than the risk initiation threshold. S402, with charging overvoltage, high SOC normalization, structural slip accumulation, and transition metal migration index as risk additions, and the proportion of local P-type effective fast charging structure as a risk mitigation term, a linear combination is constructed. S403. The combined calculation results are mapped to the 0 to 1 interval by using the Sigmoid function to obtain the high SOC phase transition risk index.
[0060] Specifically, under high SOC and high voltage conditions, O3-type layered structures are prone to relative slippage of the transition metal layers. High-voltage structural damage is related to both instantaneous voltage and the duration of high SOC residence, the degree of transition metal migration, and the proportion of locally effective P-type fast-charging structures. The effects of short-duration overvoltage shocks and long-duration high SOC residences differ; therefore, this invention employs a time-progressive accumulation state of structural slip to evaluate the cumulative impact of high-voltage residences on structural stability.
[0061]
[0062] in, This represents the cumulative state of structural slip in the next cycle, with a value ranging from 0 to 1. This represents the current cumulative slip state of the structure, with a value ranging from 0 to 1. The sampling period or stage duration, in seconds, is a positive number. The structural slip rate coefficient typically ranges from 0 to 10, with a preferred range of 0.1 to 5. This is the current voltage, in volts (V), with a typical range of 2.0 to 4.3. This is the reference voltage for structural sliding start-up, in volts (V), with a typical range of 3.8 to 4.3. It represents the state of charge, with a value ranging from 0 to 1; The SOC sensitivity index typically ranges from 1 to 5, with an optimal range of 1 to 3. This is the transition metal migration index, with a value ranging from 0 to 1; The effective fast charging structure ratio of the local P-type is 0 to 1; The amplification factor of transition metal migration on structural slip is typically 0 to 10, with a preferred range of 1 to 4. The effective fast-charging structure ratio of the local P-type structure is the mitigation coefficient for structural slippage. The conventional value range is 0 to 10, and the preferred value range is 1 to 4.
[0063] Compared to simply using a fixed voltage threshold, this formula incorporates the effects of time accumulation, SOC sensitivity, and material structural state. A higher proportion of locally effective P-type fast-charging structures results in a lower accumulation rate of structural slip at high voltages; conversely, a higher transition metal migration index leads to a higher accumulation rate of structural slip. This allows for the differentiation between the effects of short-term high-voltage shocks and prolonged high SOC residence on the cathode structure.
[0064] The high SOC region is the main area where structural rearrangement and irreversible phase transitions occur in O3 / P3 layered oxides. To ensure that the risk of phase transition gradually increases as the SOC enters the high SOC region, this invention first normalizes the SOC, so that the contribution of the low SOC region to the risk of phase transition is smaller, while the contribution of the high SOC region gradually increases.
[0065]
[0066] in, This is a high SOC normalization value, ranging from 0 to 1; The current state of charge, with a value ranging from 0 to 1; The threshold for initiating high SOC risk is typically set between 0.70 and 0.95, with a preferred range of 0.80 to 0.90. It is a very small positive number.
[0067] Phase transition risk is related to the maximum voltage, structural slip accumulation, transition metal migration, and the proportion of locally effective P-type fast-charging structures. High voltage, high state of charge (SOC), structural slip, and transition metal migration increase the risk; a higher proportion of locally effective P-type fast-charging structures helps mitigate Na-layer slip and diffusion blockage. Based on these relationships, this invention establishes a high SOC phase transition risk index.
[0068]
[0069] In order to limit the combination result in the above formula to between 0 and 1, and to facilitate subsequent comparison with the risk threshold, this invention uses the Sigmoid function for mapping.
[0070]
[0071] in, For the first The high SOC phase transition risk index has a value range of 0 to 1. The Sigmoid function is used to map risk values to a range of 0 to 1. The variable to be mapped; The voltage risk weight typically ranges from 0 to 10, with a preferred range of 1 to 5. This is the highest voltage allowed or reached during the current charging phase, expressed in volts (V), with a typical range of 3.8 to 4.3. This is the reference voltage for structural sliding start-up, in volts (V), with a typical range of 3.8 to 4.3. For high SOC risk weights, the normal range is 0 to 10, and the preferred range is 1 to 5; This is a high SOC normalization value, ranging from 0 to 1; The structural slip weight typically ranges from 0 to 10, with an optimal range of 1 to 5. This represents the structural slip accumulation state, with a value ranging from 0 to 1. The transition metal migration weight has a conventional value range of 0 to 10, and an optimal value range of 1 to 5. This is the transition metal migration index, with a value ranging from 0 to 1; The risk reduction weight corresponding to the proportion of effective fast charging structure of local P-type is typically 0 to 10, with an optimal range of 1 to 5. The effective fast charging structure ratio of the local P-type is 0 to 1.
[0072] This risk index is used for subsequent fast charging current limiting, upper voltage limit correction, and constant voltage hold time correction; when As the SOC level increases, the model reduces the charging intensity in the high SOC region to decrease the continued accumulation of structural slip and irreversible phase transitions.
[0073] Calculate the diffusion constraint current, phase change constraint current, thermal constraint current, and interface constraint current respectively, and take the minimum value among the four as the current allowable fast charging current; The calculation methods for the four types of constraint currents are as follows: Diffusion-constrained current: calculated by combining the effective diffusion coefficient, positive electrode particle size, and current state of charge (SOC). Phase change constraint current: linearly decreases as the phase change risk index increases with high SOC, with the upper limit being the rated fast charging current of the cell; Thermal constraint current: calculated by taking the square root of the cell heat capacity, ambient heat transfer capacity, and total internal resistance heat loss, with a result not less than 0; Interface constraint current: solved by combining charging voltage margin, ohmic internal resistance, and charge transfer impedance; By comparing the four types of current values, the minimum value is selected as the allowable fast charging current.
[0074] Specifically, refer to Figure 3During high-voltage fast charging, the permissible current is simultaneously limited by solid-state diffusion, phase transition stability, thermal safety, and interface polarization. If a fast charging strategy is formulated based on only one of these limitations, situations may arise where diffusion is acceptable but the risk of phase transition is too high, or where the temperature rise is controllable but the interface polarization is too large. Therefore, this invention calculates each of the four limitations separately and takes the minimum value among them as the current permissible fast charging current.
[0075]
[0076] in, For the first The permissible fast charging current per cycle is expressed in amperes (A) and ranges from 0 to the current corresponding to the rated 5C. This is the diffusion-constrained current, measured in amperes (A). This is the phase-change constraint current, measured in amperes (A). This is the thermal confinement current, measured in amperes (A). This represents the interface constraint current, measured in amperes (A).
[0077] The diffusion-constrained current is mainly determined by the effective diffusion coefficient, reaction area, particle size, and current state of charge (SOC). A higher effective diffusion coefficient and a larger reaction area allow for a higher current; larger particles and a SOC closer to full charge result in more pronounced diffusion constraint. Based on this relationship, this invention establishes a formula for calculating the diffusion-constrained current.
[0078]
[0079] in, This is the diffusion-constrained current, measured in amperes (A). This is the diffusion current conversion factor, with units of A·s / cm. 3 This coefficient was obtained by fitting the GITT diffusion coefficient, the capacity retention rate of constant current charging at different rates, and the polarization data at the end of the charging process. During calibration, it was based on... The maximum charging current that does not produce significant capacity loss or abnormal high voltage peaks is used as the dependent variable for fitting, with the independent variable being the maximum charging current that does not produce significant capacity loss or abnormal high voltage peaks. Effective reaction area, in cm² 2 ; The effective Na ion diffusion coefficient is expressed in cm⁻¹. 2 / s; The equivalent radius of the positive electrode particle is given in cm, and its typical value range is [value missing]. to ; It represents the state of charge, with a value ranging from 0 to 1; and It is a very small positive number.
[0080] Phase transition constraint current is used to limit structural risks under high state of charge (SOC) and high voltage. When the phase transition risk index is below the reference value, the current can be maintained at a relatively high level; when the risk index approaches or exceeds the upper limit, the model gradually reduces the allowable current to avoid continuing to use high current charging in high-risk areas.
[0081]
[0082] in, This is the phase-change constraint current, measured in amperes (A). This is the rated fast charging current, expressed in amperes (A), and its value ranges from 0 to the current corresponding to 5C of the rated current. The high SOC phase transition risk index has a value range of 0 to 1. The reference value for phase transition risk is typically set between 0.2 and 0.6, with a preferred range of 0.3 to 0.5. The upper limit of phase transition risk is typically set between 0.5 and 0.9, with a preferred range of 0.6 to 0.8. ; It is a very small positive number.
[0083] Thermal confinement current is used to limit temperature rise during fast charging. The higher the charging current, the more pronounced the ohmic heat and interface polarization heat; better heat dissipation allows for a higher permissible current. This is because thermal relationships satisfy… In this invention, the thermal constraint current is calculated based on the equivalent heat capacity, the maximum allowable temperature, the heat transfer capacity, the ohmic internal resistance, and the charge transfer impedance, and the square root of the result is taken to ensure consistency of physical dimensions.
[0084]
[0085] in, This is the thermal confinement current, measured in amperes (A). This is the equivalent heat capacity of the battery cell, expressed in J / K, and is a positive number. The maximum allowable temperature is measured in Kelvin (K), with a typical range of 298 to 333 and a preferred range of 308 to 323. The current temperature is in Kelvin (K), and its typical range is 243 to 333. The sampling period is expressed in seconds (s) and is a positive number. The heat transfer coefficient is expressed in W / (m³). 2 ·K), where the value is a non-negative number; The heat exchange area is expressed in square meters (m²). 2 The value is a positive number; The ambient temperature is expressed in Kelvin (K). The internal resistance is in ohms, measured in Ω, and its value is a non-negative number. This is the charge transfer impedance, measured in Ω, and its value is a non-negative number. It is a very small positive number.
[0086] Interface constraint current is used to limit the battery cell from reaching its upper voltage limit prematurely due to excessive polarization during fast charging. This constraint takes into account the current upper voltage limit, open-circuit voltage, allowable polarization margin, ohmic internal resistance, and charge transfer impedance, and can reflect the interface current space that the battery cell can still withstand at the current state of charge (SOC).
[0087]
[0088] in, This refers to the interface constraint current, in amperes (A). This is the current upper limit voltage for charging, expressed in volts (V), with a typical range of 3.8 to 4.3 V. The open-circuit voltage at the current SOC is in V and can be obtained from the SOC-OCV curve by looking up a table, or from the resting voltage, equivalent circuit model, electrochemical workstation test data, or BMS online identification results. To allow for polarization margin, the unit is V, the conventional value range is 0.02 to 0.30, and the preferred range is 0.05 to 0.20. This margin is used to limit the risk of premature voltage peaking, enhanced high-voltage side reactions, and sodium deposition on the negative electrode side of the entire cell caused by ohmic polarization and interface polarization at the end of fast charging. The internal resistance is in ohms, measured in Ω, and its value is a non-negative number. This is the charge transfer impedance, measured in Ω, and its value is a non-negative number. It is a very small positive number.
[0089] Based on the high SOC phase transition risk index and the proportion of effective local P-type fast charging structures, the upper limit voltage for the next cycle is adjusted. Based on the high SOC phase transition risk index and the interface charge transfer overpotential, the constant voltage holding time for the next cycle is adjusted. The upper limit voltage adjustment rule is as follows: When the high SOC phase transition risk index is higher than the preset reference value, a voltage reduction correction is performed; when the proportion of effective P-type fast charging structure in the local area is higher than the reference proportion, a small voltage compensation is performed; the corrected voltage is limited to the minimum and maximum voltage range allowed by the material by the projection operator. The correction rule for constant pressure holding time is as follows: When the high SOC phase transition risk index or the interface charge transfer overpotential exceeds the standard, the constant voltage time shall be shortened according to the corresponding coefficients; the correction result shall be limited to the preset minimum and maximum constant voltage time range and shall not exceed the limit.
[0090] Specifically, while higher voltage can improve the capacity utilization of the positive electrode, it also increases the risks of structural slip, transition metal migration, and interfacial side reactions. If the material has a high proportion of locally effective P-type fast-charging structures, its high-voltage adaptability can be appropriately improved; if the phase transition risk increases, the upper limit voltage needs to be reduced. Based on this relationship, this invention modifies the upper limit voltage for the next stage according to the phase transition risk and the proportion of locally effective P-type fast-charging structures, and writes the modified upper limit voltage into the formation and capacity testing program, the charging controller, or the BMS charging protocol register.
[0091]
[0092] in, The upper limit voltage for charging in the next cycle, in volts, typically ranging from 3.8 to 4.3 volts. This is the current maximum charging voltage, in V. The minimum allowable upper limit voltage, in volts (V), typically ranges from 3.8 to 4.1. This represents the maximum allowable voltage for the material system, expressed in V, with a typical value range of 4.1 to 4.3. The phase change risk reduction coefficient is typically set between 0 and 0.2, with a preferred range of 0.01 to 0.10. The high SOC phase transition risk index has a value range of 0 to 1. The reference value for phase change risk is typically between 0.2 and 0.6. The voltage compensation coefficient corresponding to the proportion of effective fast charging structure of local P-type is typically 0 to 0.2, with a preferred range of 0.01 to 0.08. The effective fast charging structure ratio of the local P-type is 0 to 1; The reference ratio for the effective fast charging structure of the local P-type is typically between 0.1 and 0.6.
[0093] The constant voltage holding stage typically occurs within the high SOC and high voltage range, a stage where structural degradation and interfacial side reactions are prone to accumulate. If the risk of phase transition or interfacial polarization increases, the constant voltage holding time should be shortened to reduce the material's residence time in the high-risk range. Therefore, this invention modifies the constant voltage holding time for the next stage based on the phase transition risk and interfacial polarization state, and writes the modified time parameters into the formation capacity program, charging controller, or BMS charging protocol register.
[0094]
[0095] in, The constant voltage holding time for the next cycle or the next charging segment, in seconds; The current constant pressure holding time, in seconds; The minimum constant pressure holding time, in seconds, typically ranges from 0 to 600. The maximum permissible constant pressure holding time, in seconds, is calibrated according to the material system and life requirements; The constant pressure time reduction factor corresponding to phase change risk has a conventional value range of 0 to 1000, and an optimal value range of 10 to 500. The high SOC phase transition risk index has a value range of 0 to 1. The reference value for phase change risk is typically between 0.2 and 0.6. The constant pressure time reduction factor corresponding to interface polarization has a conventional value range of 0 to 1000 and an optimal value range of 10 to 500. This represents the interfacial charge transfer overpotential, expressed in V. This is the interface polarization reference value, in V, with a typical range of 0.02 to 0.20.
[0096] It also includes two switchable operating modes: Offline high-precision mode: Fully utilizes three types of characterization data: XRD, Raman, and dQ / dV, to complete the calibration of the proportion of effective fast-charging structures of local P-type, the migration index of transition metals, and the normalized concentration of structural defects; Online lightweight mode: Reuses the microstructure parameters completed by offline calibration, and only collects online data of cell voltage, temperature and SOC to complete the real-time calculation of fast charging window.
[0097] This will allow the fast charging current, the corrected upper limit charging voltage, and the constant voltage hold time to be output to the battery management system or the formation and capacity testing equipment for execution.
[0098] Specifically, when input data is temporarily missing, the model uses the most recent valid value, the calibration value from the same batch, or the projected value to replace it, and records the missing value in the output. If the missing data time is less than 3 sampling periods, the most recent valid value is used first; if the missing data time is more than 3 sampling periods and belongs to the batch detection data, the calibration value from the same batch is used; if the missing data belongs to a critical detection item and there is no calibration value from the same batch, the projected value is used to maintain the calculation, and the confidence level is reduced to level C, without triggering high-risk control actions.
[0099] When XRD data is missing but Raman and dQ / dV data are valid, the model degrades. The model is then renormalized using the remaining valid weights, while simultaneously lowering the confidence level of the structural consistency coefficient. When Raman data is missing but XRD and dQ / dV data are valid, the model is reduced... The model is then renormalized using the remaining valid weights; when dQ / dV data is missing but XRD and Raman data are valid, the model is reduced. Then, normalize according to the remaining effective weights. If only one type of effective data is retained out of the three types of structured data, then high confidence scores are not calculated. The model outputs a low confidence level and requires retesting or the use of calibration values from the same batch.
[0100] When there are significant jumps in the input data, the model first determines whether the jump originates from changes in actual operating conditions. If the jump originates from sensor noise, median filtering or sliding window averaging is used; if the jump originates from changes in actual operating conditions, the jump is retained and the state update rate is increased.
[0101] For offline testing data, the model saves the batch number, testing time, testing equipment number, and sample status. If multiple test values exist for the same batch, the test value closest to the current process stage is used first; if the difference between different test values exceeds the allowable range, the model outputs a retest instruction and does not directly proceed to the release judgment.
[0102] For online running data, the model outputs a status value and confidence level for each period. The confidence level is determined by the completeness of the input, the size of the residuals, whether the parameters are extrapolated, and whether the state is out of bounds. A-level results can directly trigger control commands, B-level results can trigger derating control or review, and C-level results are only used for trend display and manual review.
[0103] This invention can employ both offline high-precision operation and online lightweight operation. The offline high-precision operation mode is used for R&D bench work, material selection, and process calibration, fully utilizing XRD, Raman, dQ / dV, EIS, and capacity data. The online lightweight operation mode is used for BMS or charge controllers, prioritizing the use of voltage, current, temperature, SOC, OCV lookup table data and impedance estimation data, and calling upon data obtained from the most recent offline calibration. , and As the initial value of the structural state.
[0104] This also includes model boundedness, numerical stability, and execution safety. In this invention , , , , , , , , , and All are limited to the range of 0 to 1 by the projection operator; By limiting the projection operator to to between; By limiting the projection operator to to between; The current is obtained by taking the lower limit of four types of physical constraint currents and limiting it to the current corresponding to the rated 5C. Therefore, the model will not generate unbounded state variables during the recursive process.
[0105] In numerical calculations, each denominator is added To avoid division by zero errors; thermally constrained current is used To avoid negative values inside the square root; the phase change constraint current is limited to between 0 and 1 times the rated current through the projection operator; if the calculated value of the interface constraint current is less than 0, the controller will limit the corresponding fast charging current to 0 or trigger a fast charging prohibition signal.
[0106] In the multi-parameter coupling process, all weight coefficients are normalized, and the sum of weights in the same group satisfies preset constraints. Risk, defect, migration, activity, consistency, and slip states are all limited to fixed intervals. Voltage and constant voltage time corrections are limited by projection intervals. Therefore, even if the input data contains short-term noise, missing data, or extrapolation, the model output remains within the hardware-executable range.
[0107] When output control commands conflict with device safety limits, the device safety limits take precedence. For example, if the model outputs a higher permissible fast charging current, but the formation device, charging controller, or BMS detects abnormalities in temperature, pressure, voltage, or insulation, the device safety limits are executed, and the model output is recorded as a reference value. This process ensures that the model control actions are consistent with the actual hardware protection logic.
[0108] This invention provides a fast-charging window control system for O3 / P3 sodium ion layered oxide cathodes, comprising: The data acquisition module is used to acquire XRD, Raman, dQ / dV characterization data, as well as cell voltage, current, temperature, SOC, and electrochemical impedance operating data. An effective structure calculation module is used to perform the steps of claim 2, and calculate the proportion of local P-type effective fast charging structures; The degradation index calculation module is used to calculate the transition metal migration index, the normalized concentration of structural defects, and the structural slip accumulation state. The multiphysics calculation module is used to solve for the effective diffusion coefficient, the high SOC phase transition risk index, four types of constraint currents, and the allowable fast charging current. The charging parameter correction module is used to dynamically correct the upper limit voltage of charging and the constant voltage holding time. The instruction output storage module generates tiered fast charging control instructions, sends them to the execution device, and stores all status parameters and operating results for each cycle. Specific Implementation The specific model execution steps are as follows (refer to...) Figure 4 ): B1. Acquire XRD data of the material using an X-ray diffractometer, acquire local vibration data using a Raman spectrometer, and acquire first-cycle charge-discharge curves, cell voltage, current, temperature, EIS impedance, and capacity data using an electrochemical workstation, formation and capacity testing equipment, or BMS.
[0110] B2. Calculation based on XRD characteristic peaks Calculate based on the dQ / dV curve And read the Raman local structure factor. .
[0111] B3, according to , and Calculate the proportion of the original local P-type structure .
[0112] B4. Calculate the structural consistency coefficient based on the differences among the three types of structural correlation signals. .
[0113] B5. Calculate the electrochemical activity coefficient based on diffusion response, interfacial polarization, and charge transfer impedance. .
[0114] B6. According to , and Calculate the effective fast charging structure ratio of local P-type. .
[0115] B7. Calculate the transition metal migration index based on the variation in interplanar spacing, Raman peak width, and the area of the anomalous peak in dQ / dV at high voltage. .
[0116] B8. Calculate the normalized concentration of structural defects based on peak width, impedance, and irreversible capacitance. .
[0117] B9. Calculate the basic diffusion coefficient based on temperature and particle size. and diffusion time constant .
[0118] B10. Substituting the proportion of effective fast-charging structures of localized P-type, the transition metal migration index, and the structural defect concentration into the effective diffusion model, we obtain... .
[0119] B11. Calculate the high SOC phase transition risk index based on high voltage, SOC, structural slip, transition metal migration, and the proportion of effective P-type fast charging structures in the localized P-type. .
[0120] B12. Calculate the diffusion confinement current respectively. Phase change confinement current Thermal confinement current and interface constraint current .
[0121] B13. Take the minimum value of the four types of constraint currents as the current allowable fast charging current. and will The output is sent to the main control module of the formation and capacity testing equipment, the charging circuit, or the BMS main control chip.
[0122] B14. Adjust the upper limit voltage of the next stage based on phase transition risk, the proportion of effective P-type fast charging structures in the local area, and the interface polarization state. and constant pressure holding time The corrected voltage and time parameters are then written into the capacity conversion program, the charging controller, or the BMS charging protocol register.
[0123] B15, when , , and When all states are within the preset safety window, the BMS main control chip, the main control module of the formation and capacity testing equipment, or the charging controller maintains the current charging program; when any state approaches the preset boundary, the model generates current reduction, voltage reduction, shortening of constant voltage holding time, or temperature adjustment control commands, and sends them to the charging circuit, temperature control device, or formation and capacity testing program for execution; when any state crosses the preset boundary, the model outputs a fast charging prohibition signal and triggers rework, degraded use, retesting, or recalibration processes.
[0124] B16. Cycle through the process until charging, process completion, or life evaluation is complete, and record the status value, control command, execution result, and confidence level for each cycle in the data log file. The implementation process of the present invention will be described below with reference to a specific embodiment.
[0125] Implementation targets and testing conditions This embodiment uses a 10Ah soft-pack sodium-ion battery cell as the implementation object. The positive electrode material is an O3 / P3 mixed-phase iron-manganese-nickel layered oxide, the negative electrode is hard carbon, and the electrolyte is an organic electrolyte for sodium-ion batteries. The initial SOC of the cell is 0.30, the target SOC is 0.90, the initial fast charging rate is set to 3C, the initial upper limit voltage for charging is set to 4.20V, and the initial constant voltage holding time is set to 1800s.
[0126] The test environment temperature was 25℃, that is:
[0127] The equivalent radius of the positive electrode particle is:
[0128] The Na ion diffusion pre-diffusion factor is:
[0129] The activation energy for Na ion migration is:
[0130] The threshold for initiating a high SOC risk model is:
[0131] The reference voltage for the structure's slip start is:
[0132] The reference ratio for the effective fast charging structure of the local P-type is:
[0133] The phase transition risk reference value is:
[0134] The upper limit of phase transition risk is set as follows:
[0135] In this embodiment, the model uses the following parameters:
[0136]
[0137]
[0138]
[0139]
[0140]
[0141] Acquisition of raw test data XRD analysis was performed on this batch of cathode materials. The intensity of the P3-related characteristic peak and the intensity of the O3-related characteristic peak were selected, and the following results were obtained:
[0142] According to the formula:
[0143] The calculation yielded:
[0144] Raman spectroscopy was performed on the same batch of materials. After normalization of the P-type correlated vibration peak intensity, peak width, and peak position shift, the Raman local structure factor was obtained.
[0145] By performing dQ / dV processing on the first charge-discharge curve of the battery cell, two characteristic peaks were identified in the O3 / P3 related reaction region, with the peak positions as follows:
[0146]
[0147] The reference voltage span for the entire SOC range is:
[0148] The normalized value of the peak spacing dQ / dV is:
[0149] Calculation of the proportion of effective fast charging structure in local P-type region First, calculate the proportion of the original local P-type structure:
[0150] get:
[0151] This value represents the proportion of the original P-type structure obtained from XRD, Raman, and dQ / dV, but it cannot directly indicate that all of this part of the structure participates in the fast charging process. Therefore, the structural consistency coefficient is calculated further:
[0152] get:
[0153] The results indicate that the deviations among the three types of structural correlation signals are small, and the detected P-type correlation structures have good consistency.
[0154] The electrochemical activity coefficient was further calculated. It was obtained through charging, resting, relaxation, and EIS testing:
[0155] The reference diffusion response coefficient is:
[0156] The interface charge transfer overpotential is:
[0157] Allowed interface polarization upper limit:
[0158] The charge transfer impedance is:
[0159] The upper limit of the allowable charge transfer impedance is:
[0160] but:
[0161] get:
[0162] This yields the proportion of effective fast charging structure in the local P-type region:
[0163] Right now:
[0164] It can be seen that although the original local P-type structure ratio of this batch of materials is 0.339, after screening for structural consistency and electrochemical activity, the effective ratio that actually participates in fast charging transmission and high voltage stability is 0.237.
[0165] Conventional testing relies solely on the XRD single peak percentage of 0.329 to determine a material's fast-charging advantage, failing to distinguish between impurity peaks and false P signals caused by lattice disorder. This invention, through a dual-layer screening of consistency verification and electrochemical activity, finds that the effective P signal truly capable of participating in rapid sodium ion transport is only 0.237, eliminating approximately 30.1% of invalid P signals. Microscopic characterization further confirms this: in-situ XRD and HAADF-STEM atomic imaging were used to observe the electrode after cycling. In the control group cell, numerous disordered impurities and surface defect P structures lacked sodium ion conduction capacity under high voltage, instead inducing local Jahn-Teller distortion and ectopic migration of transition metals. This method eliminates such invalid structures, retaining only ordered P3 channels with synchronized long-range, short-range, and electrochemical signal matching, thus avoiding the defects of "misjudging fast-charging potential and blindly charging with high current."
[0166] Calculation of transition metal migration, defect state and effective diffusion coefficient Within the high-voltage charging range, the transition metal migration index is calculated based on the XRD interplanar spacing shift, Raman peak width variation, and the area of the high-voltage anomaly peak in dQ / dV.
[0167] The high-voltage abnormal peak area integration range is 4.05V to 4.20V, and the low-voltage reference peak area integration range is 3.20V to 4.05V.
[0168] Based on the normalization of XRD full width at half maximum (FWHM), EIS impedance, and irreversible capacitance, the normalized concentration of structural defects is obtained:
[0169] The basic Na ion diffusion coefficient is calculated as follows:
[0170] Substitute:
[0171]
[0172]
[0173]
[0174] get:
[0175] The effective diffusion coefficient is then calculated:
[0176] Substitute:
[0177]
[0178]
[0179] get:
[0180]
[0181] The results indicate that although there is a certain proportion of effective P-type fast-charging structures in the material, the migration of transition metals and defect states have already inhibited the diffusion of Na ions. Therefore, it is not possible to continue charging directly to the high SOC region at the initial 3C rate.
[0182] Existing fast charging control is based solely on the temperature-dependent Arrhenius diffusion coefficient, completely ignoring the blocking effects of transition metal ion mixing and lattice defects on ion channels; the diffusion coefficient in this embodiment... After correction by dual suppression of migration and defects, the effective diffusion coefficient was reduced to The reduction was 38%. Electrochemical GITT diffusion tests corroborated this: the control group used the basic diffusion coefficient to calculate the fast charging current throughout the process. Under high SOC, the measured effective diffusion capacity of sodium ions deviated from the model calculation value by more than 40%, and continuous high current charging induced concentration polarization and particle microcracks. After the micro-deterioration index was corrected by coupling in this invention, the error between the calculated diffusion coefficient value and the in-situ GITT measurement was less than 7%, matching the real ion transport capacity and solving the problem of "ignoring lattice deterioration and artificially high diffusion constraint current" in traditional models.
[0183] Calculation of high SOC phase transition risk When the battery cell is charged to:
[0184] And the voltage reaches:
[0185] When calculating the high SOC normalization factor:
[0186] Substitute:
[0187] get:
[0188] The current structural slip accumulation state is as follows:
[0189] The high SOC phase transition risk index is:
[0190] The calculated value within the parentheses is:
[0191] therefore:
[0192] The result is higher than the phase transition risk reference value of 0.55, indicating that there is already a significant structural risk in the high SOC region, and it is necessary to reduce the charging current and correct the subsequent upper limit voltage and constant voltage holding time.
[0193] Traditional control relies solely on a fixed SOC / voltage threshold to simply determine risk (e.g., direct current reduction when SOC>0.8), failing to distinguish between short-term high-voltage impacts, long-term high SOC dwell times, and phase transition damage caused by differences in the intrinsic structure of materials. This invention constructs a multi-factor risk model using time-slip accumulation terms, effective P-phase slow-release terms, and transition metal migration addition terms, and uses the Sigmoid function to uniformly map it to a standardized range of 0 to 1. In-situ XRD cyclic monitoring results corroborate this: in the control group, after charging at SOC=0.83 and continuously at 4.20V for 200 cycles, the (003) characteristic peak significantly broadened, and a monoclinic distortion peak appeared (corresponding to an irreversible slip phase transition); the experimental group, based on... The charging intensity was dynamically reduced by a risk value of 0.712. After the same period, the XRD peak shape was intact and no obvious impurity phase was generated. The quantitative risk index was linearly correlated with the degree of irreversible phase transformation of the crystal, realizing the quantification and early intervention of microscopic phase transformation risk.
[0194] Fast charging current constraint calculation This embodiment calculates the diffusion confinement current, phase change confinement current, thermal confinement current, and interface confinement current, respectively.
[0195] The diffusion confinement current is calculated based on the effective diffusion coefficient, particle size, state of charge (SOC), and effective reaction area.
[0196] Calculate the phase transition constraint current based on the high SOC phase transition risk:
[0197] get:
[0198] The thermal confinement current is calculated based on the current temperature, equivalent heat capacity, heat dissipation capacity, and internal resistance.
[0199] The interface constraint current is calculated based on the current upper limit voltage, OCV, allowable polarization margin, ohmic internal resistance, and charge transfer impedance:
[0200] therefore:
[0201] get:
[0202] These results indicate that when the SOC reaches 0.83 and the voltage is close to 4.20V, the main limiting factor for the fast charging window of this battery cell is the high SOC phase transition risk. The controller should reduce the charging current from 3C to 1.79C.
[0203] Existing fast charging strategies employ thermal constraints or interface polarization constraints, resulting in blind spots due to physical field conflicts. This invention simultaneously couples four physical boundaries: solid-state diffusion dynamics, crystal phase transition stability, thermal safety, and interface polarization, taking the minimum value as the safe fast charging current. Thermal imaging temperature measurement corroborates this: the control group's peak temperature rise at the end of a 3C full charge was 10.6℃, and the phase transition risk consistently exceeded the limit, with the temperature rise during cycling increasing year by year. The experimental group, with a phase transition constraint of 1.79C as the upper limit, had a temperature rise of only 7.8℃ at the end, while also considering the ion diffusion limit and interface polarization threshold. This avoids the single-dimensional optimization shortcoming of "meeting thermal safety standards but causing irreversible lattice damage," achieving multi-dimensional safety assurance for fast charging.
[0204] Upper voltage limit and constant voltage hold time correction The current maximum charging voltage is:
[0205] The voltage correction formula is:
[0206] Substitute:
[0207]
[0208]
[0209]
[0210]
[0211]
[0212] get:
[0213]
[0214] Therefore, the controller revised the upper limit voltage for the next stage of charging from 4.20V to 4.19V.
[0215] The current constant pressure holding time is:
[0216] Interface polarization reference value is taken as:
[0217] The current interface charge transfer overpotential is:
[0218] but:
[0219] get:
[0220] After rounding:
[0221] Therefore, the controller shortens the constant pressure holding time for the next stage from 1800s to 1778s.
[0222] Traditional solutions use independent fixed parameters for voltage and constant voltage time. In high-risk regions, prolonged constant voltage of 4.20V exacerbates interlayer slip. This invention achieves dual-linkage correction of phase transition risk reduction by lowering voltage and polarization overshoot by shortening constant voltage. Electrochemical characterization of dQ / dV confirms that after 200 cycles, the normalized value of the abnormal phase transition peak area in the high-voltage region of the control group is 0.31, indicating the accumulation of a large number of irreversible side reactions. The experimental group dynamically reduces voltage and shortens the high SOC constant voltage residence time, reducing the abnormal peak area to 0.24 and the amount of side reaction formation to 22.6%, balancing capacity utilization and high-voltage structural stability.
[0223] Controlled trial setup To verify the effectiveness of the method in this embodiment, an experimental group and a control group were set up. Both groups of cells used the same positive electrode material, the same negative electrode material, the same electrolyte, the same capacity specification, and the same ambient temperature. The initial SOC of both groups of cells was 0.30, the target SOC was 0.90, the ambient temperature was 25°C, and the number of cycles was 200.
[0224] The experimental group adopted the method of this embodiment and adjusted the charging current, upper limit voltage and constant voltage holding time in a rolling manner according to the proportion of effective fast charging structure of local P type, high SOC phase change risk, diffusion constraints, thermal constraints and interface constraints.
[0225] The control group used a fixed fast charging strategy, namely:
[0226] The constant pressure holding time is fixed as follows:
[0227] The control group does not calculate the proportion of effective P-type fast charging structures in the local area, does not adjust the fast charging current based on the risk of high SOC phase transition, does not adjust the upper limit voltage of charging, and does not shorten the constant voltage holding time.
[0228] The control strategies for the two sets of experiments are shown in the table below.
[0229]
[0230] Controlled trial execution process When the SOC was below 0.80, the risk of phase transition at high SOC calculated by the model was lower than the reference value, and the cells were charged at 3C current.
[0231] When the SOC reaches 0.83 and the voltage is close to 4.20V, the model calculations show that:
[0232]
[0233]
[0234] At this time, the controller performs the following actions: The charging current was reduced from 3C to 1.79C; The upper limit voltage for the next stage has been revised from 4.20V to 4.19V; The constant pressure holding time was shortened from 1800s to 1778s; Record the current fast charging level as reduced-rate fast charging.
[0235] When the SOC reaches 0.83 and the voltage is close to 4.20V, the control group does not calculate the proportion of effective P-type fast charging structure in the local area, nor does it calculate the risk of phase change at high SOC. It continues to charge to 4.20V according to the 3C current and maintains constant voltage for 1800s.
[0236] Therefore, the control differences between the two groups of cells in the high SOC range are shown in the table below.
[0237]
[0238] Comparison results After 200 cycles, the capacity retention rate, DC internal resistance growth rate, abnormal peak area of high voltage dQ / dV, high SOC phase transition risk index, and end-of-charge temperature rise of the two groups of cells were compared.
[0239] The comparison results are shown in the table below.
[0240]
[0241] The results of the above comparison show that although the control group maintained a fixed 3C fast charging strategy, the phase transition risk and the abnormal peak area of dQ / dV increased significantly in the high SOC range, and the capacity retention rate decreased significantly after 200 cycles. The experimental group calculated the proportion of local P-type effective fast charging structure and incorporated the material structure state into the fast charging control, so that the current, voltage and constant voltage holding time in the high SOC region were adjusted according to the risk changes.
[0242] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely preferred examples and are not intended to limit the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for controlling the fast charging window of an O3 / P3 sodium ion layered oxide cathode, characterized in that, Includes the following steps: Three types of material characterization data were collected for the cathode: XRD, Raman, and dQ / dV. The three types of characterization data were then fused together, and the original P-type ratio, structural consistency coefficient, and electrochemical activity coefficient were calculated in sequence to obtain the effective fast-charging structure ratio of the local P-type. Based on the characterization data and charge transfer impedance and irreversible capacity, the transition metal migration index and normalized concentration of structural defects were calculated respectively, and the structural slip accumulation state was obtained by recursion based on cell voltage and SOC. The basic sodium ion solid-phase diffusion coefficient is calculated based on the cell temperature. The effective sodium ion diffusion coefficient is then corrected by combining the proportion of effective fast-charging structure of local P-type, the transition metal migration index, and the normalized concentration of structural defects. Based on SOC, the normalized value of high SOC is calculated. Combined with cell voltage, structural slip accumulation state, transition metal migration index, and the proportion of local P-type effective fast charging structure, the high SOC phase transition risk index is calculated.
2. The method for controlling the fast charging window of the O3 / P3 sodium ion layered oxide cathode according to claim 1, characterized in that: The calculation sub-steps for the original local P-type effective fast charging structure ratio include: S201. Calculate the peak intensity ratio of XRD based on the characteristic peak intensities of P3 and O3 within the XRD; obtain the Raman local structure factor by normalizing the Raman vibration peak information; calculate the normalized value of the peak spacing based on the voltage difference between the O3 / P3 reaction peaks within the dQ / dV curve. S202. The original local P-type structure ratio is obtained by weighted summation of the XRD peak intensity ratio, Raman local structure factor, and dQ / dV peak spacing normalization value and interval constraint. S203. Calculate the structural consistency coefficient by weighted penalty of pairwise differences of three sets of data; S204. The electrochemical activity coefficient is calculated by combining the electrochemical diffusion response, interfacial overpotential, and charge transfer impedance weighting. S205. Multiply the original local P-type structure ratio, structural consistency coefficient, and electrochemical activity coefficient and project them to the 0 to 1 interval to obtain the effective fast-charging structure ratio of the local P-type.
3. The method for controlling the fast charging window of the O3 / P3 sodium ion layered oxide cathode according to claim 1, characterized in that, The transition metal migration index was obtained by using XRD interplanar spacing shift, Raman peak width variation, and dQ / dV abnormal peak area weighted normalization. The normalized concentration of structural defects was obtained by using the XRD full width at half maximum (FWHM), steady-state charge transfer impedance, and irreversible capacity weighted normalization. Using sampling duration, charging overvoltage, SOC, transition metal migration index, and the proportion of effective fast charging structures of local P-type as variables, the cumulative state of structural slip in the next cycle is recursively calculated.
4. The method for controlling the fast charging window of the O3 / P3 sodium ion layered oxide cathode according to claim 1, characterized in that, The effective diffusion coefficient is calculated as follows: The temperature-dependent basic Na ion solid-phase diffusion coefficient was calculated using the Arrhenius formula. Then, exponential corrections were made by introducing a localized P-type effective fast-charging structure proportional gain term, a transition metal migration suppression term, and a structural defect suppression term. After interval constraints, the effective diffusion coefficient was obtained.
5. The method for controlling the fast charging window of the O3 / P3 sodium ion layered oxide cathode according to claim 4, characterized in that, The calculation steps for the high SOC phase transition risk index are as follows: S301. Set a high SOC normalization variable and assign risk weights only to the SOC interval that is higher than the risk initiation threshold. S302, a linear combination is constructed with charging overvoltage, high SOC normalization, structural slip accumulation, and transition metal migration index as risk additions, and the proportion of local P-type effective fast charging structure as a risk mitigation term. S303. The combined calculation results are mapped to the 0 to 1 interval by using the Sigmoid function to obtain the high SOC phase transition risk index.
6. The method for controlling the fast charging window of the O3 / P3 sodium ion layered oxide cathode according to claim 1, characterized in that: Calculate the diffusion constraint current, phase change constraint current, thermal constraint current, and interface constraint current respectively, and take the minimum value among the four as the current allowable fast charging current; Diffusion-constrained current: calculated by combining the effective diffusion coefficient, positive electrode particle size, and current state of charge (SOC). Diffusion-constrained current formula: in, For diffusion-constrained current; This is the conversion factor for diffusion current; Effective reaction area; The effective Na ion diffusion coefficient; The equivalent radius of the positive electrode particle; It is in a charged state; and It is a very small positive number; Phase change constraint current: linearly decreases as the phase change risk index increases with high SOC, with the upper limit being the rated fast charging current of the cell; Phase change confinement current formula: in, This is the phase-change constraint current; Rated fast charging current; A high SOC phase transition risk index; This serves as a reference value for phase transition risk. This represents the upper limit of phase transition risk. It is a very small positive number; Thermal constraint current: calculated by taking the square root of the cell heat capacity, ambient heat transfer capacity, and total internal resistance heat loss, with a result not less than 0; Thermal confinement current formula: in, This is the thermal confinement current; This refers to the equivalent heat capacity of the battery cell. Maximum permissible temperature; The current temperature; The sampling period; The heat transfer coefficient; For heat exchange area; The ambient temperature; The internal resistance is ohmic; It is the charge transfer impedance; Minimal positive number Interface constraint current: solved by combining charging voltage margin, ohmic internal resistance, and charge transfer impedance; Interface constraint current formula: in, For interface constraint current; This is the open-circuit voltage under the current SOC. To allow for polarization margin; The internal resistance is ohmic; It is the charge transfer impedance; It is a very small positive number; By comparing the four types of current values, the minimum value is selected as the allowable fast charging current.
7. The method for controlling the fast charging window of the O3 / P3 sodium ion layered oxide cathode according to claim 6, characterized in that: Based on the high SOC phase transition risk index and the proportion of effective local P-type fast charging structures, the upper limit voltage for the next cycle is adjusted. Based on the high SOC phase transition risk index and the interface charge transfer overpotential, the constant voltage holding time for the next cycle is adjusted. The upper limit voltage adjustment rule is as follows: When the high SOC phase transition risk index is higher than the preset reference value, a voltage reduction correction is performed; when the proportion of effective P-type fast charging structure in the local area is higher than the reference proportion, a small voltage compensation is performed; the corrected voltage is limited to the minimum and maximum voltage range allowed by the material by the projection operator. The correction rule for constant pressure holding time is as follows: When the high SOC phase transition risk index or the interface charge transfer overpotential exceeds the standard, the constant voltage time shall be shortened according to the corresponding coefficients; the correction result shall be limited to the preset minimum and maximum constant voltage time range and shall not exceed the limit.
8. The method for controlling the fast charging window of the O3 / P3 sodium ion layered oxide cathode according to claim 7, characterized in that, This will allow the fast charging current, the corrected upper limit charging voltage, and the constant voltage hold time to be output to the battery management system or the formation and capacity testing equipment for execution.
9. The method for controlling the fast charging window of the O3 / P3 sodium ion layered oxide cathode according to claim 8, characterized in that, It also includes two switchable operating modes: Offline high-precision mode: Fully utilizes three types of characterization data: XRD, Raman, and dQ / dV, to complete the calibration of the proportion of effective fast-charging structures of local P-type, the migration index of transition metals, and the normalized concentration of structural defects; Online lightweight mode: Reuses the microstructure parameters completed by offline calibration, and only collects online data of cell voltage, temperature and SOC to complete the real-time calculation of fast charging window.
10. A fast-charging window control system for an O3 / P3 sodium ion layered oxide cathode, used to execute the fast-charging window control method for an O3 / P3 sodium ion layered oxide cathode according to any one of claims 1-9, characterized in that, include: The data acquisition module is used to acquire XRD, Raman, dQ / dV characterization data, as well as cell voltage, current, temperature, SOC, and electrochemical impedance operating data. An effective structure calculation module is used to execute the sub-step of claim 2, calculating the proportion of local P-type effective fast charging structures; The degradation index calculation module is used to calculate the transition metal migration index, the normalized concentration of structural defects, and the structural slip accumulation state. The multiphysics calculation module is used to solve for the effective diffusion coefficient, the high SOC phase transition risk index, four types of constraint currents, and the allowable fast charging current. The charging parameter correction module is used to dynamically correct the upper limit voltage of charging and the constant voltage holding time. The instruction output storage module generates tiered fast charging control instructions, sends them to the execution device, and stores all status parameters and operating results for each cycle.