A solar cell and its preparation method

By incorporating a light-absorbing layer and a light conversion and carrier transport structure into crystalline silicon solar cells, the problem of insufficient utilization of short-wavelength light is solved, photoelectric conversion efficiency and lifespan are improved, and resistance is reduced.

CN123124450APending Publication Date: 2026-11-17BAOTOU JA SOLAR TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611363944.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Crystalline silicon solar cells do not make sufficient use of short-wavelength light, resulting in low photoelectric conversion efficiency and easy overheating, which affects their service life.

Method used

A light absorption layer and a light conversion and carrier transport structure are set on a crystalline silicon substrate. The conductivity type of the light conversion and carrier transport structure is opposite to that of the crystalline silicon substrate. By absorbing short-wavelength photons and releasing long-wavelength photons, the light absorption layer absorbs long-wavelength photons to generate electron-hole pairs, thereby separating and collecting carriers.

Benefits of technology

It improves light utilization and photoelectric conversion efficiency, reduces the temperature rise of solar cells, extends their service life, and reduces series resistance and contact resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124450A_ABST
    Figure CN123124450A_ABST
Patent Text Reader

Abstract

This invention discloses a solar cell and its fabrication method. The solar cell may include: a crystalline silicon substrate; a light-absorbing layer disposed on a first main surface of the crystalline silicon substrate; a light conversion and carrier transport structure disposed on the side of the light-absorbing layer away from the crystalline silicon substrate, the conductivity type of the light conversion and carrier transport structure being opposite to that of the crystalline silicon substrate; and a first electrode disposed on the side of the light conversion and carrier transport structure away from the crystalline silicon substrate, the first electrode being electrically connected to the light conversion and carrier transport structure. This solar cell can effectively improve light utilization and photoelectric conversion efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a solar cell and a method for its fabrication. Background Technology

[0002] Crystalline silicon solar cells generally rely on a crystalline silicon substrate (n-type or p-type) to absorb solar photons. The photon energy generates electron-hole pairs, producing the photovoltaic effect. This is further enhanced by a carrier collection layer and electrodes to separate, collect, and transport carriers. Research has found that short-wavelength light (below 450 nm) has limited penetration into crystalline silicon substrates. Crystalline silicon solar cells struggle to absorb and utilize large amounts of this short-wavelength light, resulting in insufficient utilization of short-wavelength light and consequently, low photoelectric conversion efficiency. Summary of the Invention

[0003] In view of this, the present invention provides a solar cell and a method for fabricating the same. The solar cell combines a light-absorbing layer with a light conversion and carrier transport structure. The light conversion and carrier transport structure can absorb short-wavelength photons and release or emit long-wavelength photons based on the energy of the absorbed short-wavelength photons. The light-absorbing layer absorbs long-wavelength photons and excites the crystalline silicon substrate to generate electron-hole pairs. Therefore, the solar cell provided by the present invention can utilize short-wavelength light, improve light utilization, and thus improve the photoelectric conversion efficiency of the solar cell.

[0004] To solve the above-mentioned technical problems, the present invention provides the following technical solution: In a first aspect, the present invention provides a solar cell, comprising: Crystalline silicon substrate; A light-absorbing layer is disposed on the first main surface of the crystalline silicon substrate; A light conversion and carrier transport structure is disposed on the side of the light absorption layer away from the crystalline silicon substrate, and the conductivity type of the light conversion and carrier transport structure is opposite to that of the crystalline silicon substrate; A first electrode is disposed on the side of the light conversion and carrier transport structure away from the crystalline silicon substrate, and the first electrode is electrically connected to the light conversion and carrier transport structure.

[0005] Secondly, embodiments of the present invention provide a method for preparing a solar cell, comprising: Step S1: Provide an initial crystalline silicon substrate; Step S2: A light absorption layer and a light conversion and carrier transport structure are sequentially stacked on the first main surface of the initial crystalline silicon substrate. The portion of the initial crystalline silicon substrate (10') excluding the light absorption layer (20) and the light conversion and carrier transport structure (30) forms a crystalline silicon substrate. The conductivity type of the light conversion and carrier transport structure is opposite to that of the crystalline silicon substrate. Step S3: Form a first electrode on the optical conversion and carrier transport structure that is electrically connected to the optical conversion and carrier transport structure.

[0006] The technical solution of the first aspect of the above invention has the following advantages or beneficial effects: the light conversion and carrier transport structure of the solar cell can absorb short-wavelength photons in sunlight and release or emit long-wavelength photons based on the energy of the absorbed short-wavelength photons. The light absorption layer absorbs the long-wavelength photons released or emitted by the light conversion and carrier transport structure, thereby generating electron-hole pairs. The light conversion and carrier transport structure further separates and collects hole carriers or electron carriers. The first electrode transports the carriers collected by the light conversion and carrier transport structure. Therefore, the solar cell provided by the embodiments of the present invention can utilize short-wavelength sunlight, improve light utilization, and thus improve photoelectric conversion efficiency. Attached Figure Description

[0007] Figure 1 This is a partial cross-sectional structural diagram of a solar cell with the first structure provided in the embodiments of the present invention; Figure 2 This is a partial cross-sectional structural diagram of a solar cell with a second structure provided according to an embodiment of the present invention; Figure 3 This is a schematic diagram of the main process of a solar cell fabrication method according to an embodiment of the present invention; Figure 4 This is a schematic cross-sectional view of the structural changes corresponding to each step in the preparation method according to an embodiment of the present invention; Figure 5 This is a schematic cross-sectional view of the structural changes corresponding to each step in the fabrication of a solar cell of the first structure according to the fabrication method of the present invention. Figure 6 This is a schematic cross-sectional view of the structural changes at each step in the fabrication process of a solar cell with a second structure according to an embodiment of the present invention.

[0008] The attached figures are labeled as follows: 10 - Crystalline silicon substrate; 10' - Initial crystalline silicon substrate; 20 - Light absorption layer; 30 - Light conversion and carrier transport structure; 31 - Light conversion layer; 32 - First intrinsic amorphous silicon layer; 33 - First doped amorphous silicon layer; 40 - First electrode; 41 - Transparent conductive film layer; 42 - Metal electrode; 50 - Carrier collection layer; 51 - First passivation layer; 52 - Doped polycrystalline silicon layer; 60 - Second electrode; 70 - Passivation antireflection layer; 80 - Second passivation layer; H1 - First depth; H2 - Second depth; H3 - Third depth. Detailed Implementation

[0009] Existing solar cells based on crystalline silicon substrate 10 (hereinafter referred to as existing solar cells) mainly utilize light in the wavelength range of 450nm~780nm to generate photogenerated carriers. However, photons with shorter wavelengths in sunlight (generally less than 450nm, and particularly less than 400nm) have very weak penetration ability in the crystalline silicon substrate 10, resulting in most of the short-wavelength light not being fully utilized by existing solar cells. Furthermore, short-wavelength photons have relatively high energy and are converted into heat in the solar cell, causing it to heat up. Therefore, the light utilization rate and photoelectric conversion efficiency of existing solar cells are both low. Moreover, the heating effect of short-wavelength light on existing solar cells also affects their photoelectric conversion efficiency and lifespan.

[0010] To address the aforementioned problems of existing solar cells, embodiments of the present invention provide a novel solar cell structure and a new method for fabricating the novel solar cell structure.

[0011] It should be noted that the terms "first," "second," "third," "fourth," and "fifth," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined as "first," "second," "third," "fourth," and "fifth" may explicitly or implicitly include one or more of that feature. In the description of this invention, "a plurality of" means two or more, unless otherwise explicitly specified.

[0012] The first main surface of the crystalline silicon substrate 10 involved in the embodiments of the present invention generally refers to the main surface of the crystalline silicon substrate 10 facing sunlight during the operation of the solar cell. The second main surface of the crystalline silicon substrate 10 generally refers to the main surface of the crystalline silicon substrate 10 facing away from sunlight during the operation of the solar cell.

[0013] The doped particles involved in the embodiments of the present invention can be doped atoms, doped ions, or a mixture of doped atoms and doped ions.

[0014] Unless otherwise contradictory, the doping concentration and content of doped particles in the embodiments of this invention are generally calculated as the amount of activated doped particles. Specifically, the doping concentration in the embodiments of this invention generally refers to the number of doped atoms and / or doped ions contained in a unit volume or unit area of ​​any cross-section of a certain film layer or structure (such as a light absorption layer or a light conversion and carrier transport structure). The content of doped particles in the embodiments of this invention generally refers to the number of parts of doped particles per million parts of silicon (the silicon unit of measurement is generally a number or a mass) in a certain film layer or structure (such as a light absorption layer or a light conversion and carrier transport structure). For example, a doped particle content of X ppm in a certain film layer or structure means that X or X moles of doped particles are doped per million silicon atoms or 1 million moles of silicon. In the film layer provided in the embodiments of the present invention, the unit indicating the content of each doped particle or silicon is ppm, and the unit indicating the doping concentration of each doped particle or silicon is atoms / cm. 3 The conversion relationship is: 1 ppm = 5 × 10 16 atoms / cm 3 .

[0015] In this embodiment of the invention, a "doped non-polycrystalline silicon layer" refers to a non-polycrystalline silicon layer containing p-type or n-type doped atoms. An "intrinsic non-polycrystalline silicon layer" refers to a non-polycrystalline silicon layer that does not contain p-type or n-type doped atoms.

[0016] A "non-polycrystalline silicon layer" refers to a film layer in which the silicon is not in a polycrystalline state. The non-polycrystalline silicon layer can include a single amorphous silicon layer or a microcrystalline silicon layer, or a stacked structure of amorphous silicon layers and microcrystalline silicon layers. The microcrystalline silicon layer has a mixed-phase structure, comprising at least amorphous silicon and silicon grains, and may contain silicon grains with a particle size no greater than 100 nanometers, preferably silicon grains with a particle size no greater than 10 nanometers. The non-polycrystalline silicon layer may also include at least one of silicon oxide or silicon carbide layers. Silicon carbide can have a crystalline structure, an amorphous structure, or a mixture of crystalline and amorphous silicon structures.

[0017] In the embodiments of this invention, "from the inside out" generally refers to the crystalline silicon substrate 10 as a reference, and the direction from the position closest to the crystalline silicon substrate 10 to the position furthest away from the crystalline silicon substrate 10 is "from the inside out". Correspondingly, the inner and outer sides of a film layer are also based on the crystalline silicon substrate 10. The side of the film layer closest to the crystalline silicon substrate 10 is the inner side of the film layer, and the side of the film layer furthest from the crystalline silicon substrate 10 is the outer side of the film layer.

[0018] In the embodiments of the present invention, one film layer is located on another film layer. This film layer may be located on the side of the other film layer away from the crystalline silicon substrate 10. In the absence of other conflicting descriptions, the one film layer and the other film layer may be in direct contact, and other film layers may also be included between the one film layer and the other film layer.

[0019] In the embodiments of this invention, an n-type doped or n-type conductive film generally means that the film is doped with n-type doped atoms such as phosphorus atoms, antimony atoms, or arsenic atoms. A p-type doped or p-type conductive film generally means that the film is doped with p-type doped atoms such as boron atoms or gallium atoms.

[0020] Specifically, embodiments of the present invention provide a solar cell with a novel structure. More specifically, as... Figure 1 and Figure 2 As shown, the solar cell may include: a crystalline silicon substrate 10, a light-absorbing layer 20, a light conversion and carrier transport structure 30, and a first electrode 40, wherein, The light-absorbing layer 20 is disposed on the first main surface of the crystalline silicon substrate 10; The light conversion and carrier transport structure 30 is disposed on the side of the light absorption layer 20 away from the crystalline silicon substrate 10, and the conductivity type of the light conversion and carrier transport structure 30 is opposite to that of the crystalline silicon substrate 10. The first electrode 40 is disposed on the side of the light conversion and carrier transport structure 30 away from the crystalline silicon substrate 10, and the first electrode 40 is electrically connected to the light conversion and carrier transport structure 30.

[0021] More specifically, the optical conversion and carrier transport structure 30 can be used to absorb short-wavelength photons and emit or release long-wavelength photons. It is worth noting that the optical conversion and carrier transport structure 30 can also utilize some of the long-wavelength photons it emits or releases, as well as some long-wavelength photons originating from sunlight. Furthermore, the optical conversion and carrier transport structure 30 can allow long-wavelength photons that are not currently being utilized to pass through.

[0022] The light absorption layer 20 can be used to absorb some of the long-wavelength photons emitted or released by the light conversion and carrier transport structure 30, as well as some of the long-wavelength photons from sunlight, to excite the light absorption layer 20 and the crystalline silicon substrate 10 to generate electron-hole pairs. The light conversion and carrier transport structure 30 can further separate, collect, and transport carriers of the same conductivity type according to its conductivity type. For example, if the conductivity type of the light conversion and carrier transport structure 30 is n-type, it separates, collects, and transports electron carriers from electron-hole pairs; if the conductivity type of the light conversion and carrier transport structure 30 is p-type, it separates, collects, and transports hole carriers from electron-hole pairs. By positioning the light conversion and carrier transport structure 30 on the side of the light absorption layer 20 away from the crystalline silicon substrate 10, a greater number of short-wavelength photons (wavelength less than or equal to 450 nm) with shorter propagation distances can reach the light conversion and carrier transport structure 30. Most of these short-wavelength photons can be absorbed by the light conversion and carrier transport structure 30. After absorbing the energy of higher-energy short-wavelength photons (wavelength less than or equal to 450 nm), the light conversion and carrier transport structure 30 emits or releases lower-energy long-wavelength photons. Generally, absorbing the energy of one short-wavelength photon (wavelength less than or equal to 450 nm) can emit or release two long-wavelength photons. These long-wavelength photons are absorbed and utilized by the light absorption layer 20 to generate electron-hole pairs.

[0023] As described above, the light conversion and carrier transport structure 30 can also absorb some long-wavelength photons to generate electron-hole pairs, and it can separate electrons and holes. Among the long-wavelength photons absorbed by the light conversion and carrier transport structure 30, one part is from the long-wavelength photons generated by the structure 30 being absorbed again, and the other part originates from a small number of long-wavelength photons in sunlight. Compared to the crystalline silicon substrate 10, the sensitizer ions and activator ions in the light conversion and carrier transport structure 30 work together to utilize more solar energy, improve electron-hole pair separation efficiency and the light utilization rate of the solar cell. Simultaneously, the sensitizer ions and activator ions have higher conductivity than crystalline silicon, resulting in a lower potential barrier between the light conversion and carrier transport structure 30 and the electrode, forming a good ohmic contact between them. This reduces the series resistance of the solar cell and improves its fill factor.

[0024] It is worth noting that, in addition to the photoconversion and carrier transport structure 30 and the photoabsorption layer 20 being able to utilize long-wavelength photons, long-wavelength photons generated by the photoconversion and carrier transport structure 30 that are not utilized by itself and the photoabsorption layer 20, as well as long-wavelength photons from sunlight that are not utilized by the photoconversion and carrier transport structure 30 and the photoabsorption layer 20, can be absorbed by the crystalline silicon substrate 10, generating electron-hole pairs in the crystalline silicon substrate 10. These electron-hole pairs generated by the crystalline silicon substrate 10 can also be separated and collected by the photoconversion and carrier transport structure 30. In other words, the light absorption layer 20 and the light conversion and carrier transport structure 30 provided in this embodiment of the invention can absorb some long-wavelength (generally wavelength greater than 450nm) photons, while also ensuring that unabsorbed long-wavelength (generally wavelength greater than 450nm) photons pass through, allowing the unabsorbed long-wavelength photons to reach the crystalline silicon substrate 10. The crystalline silicon substrate 10 absorbs the long-wavelength photons and generates electron-hole pairs. Electron carriers or hole carriers can tunnel through the light absorption layer 20, thereby enabling the light conversion and carrier transport structure 30 to separate, collect, and transport carriers of the same conductivity type. Understandably, the light absorption layer 20 can also utilize some long-wavelength photons in sunlight to generate electron-hole pairs, and the long-wavelength photons generated by the light conversion and carrier transport structure 30 can also partially reach the crystalline silicon substrate 10 and be utilized by the crystalline silicon substrate 10 to generate electron-hole pairs. Therefore, the solar cell provided in this embodiment of the invention, through the cooperation of the light absorption layer 20 and the light conversion and carrier transport structure 30, can make greater use of short-wavelength light, enhance the response to the ultraviolet spectrum, and improve the light utilization rate of the solar cell.

[0025] Furthermore, the light conversion and carrier transport structure 30 converts short-wavelength photons into more long-wavelength photons, so that the light absorption layer 20 and the crystalline silicon substrate 10 work together to generate more electron-hole pairs, thereby improving the photoelectric conversion efficiency of the solar cell.

[0026] As can be seen from the above, the light conversion and carrier transport structure 30 of the solar cell provided in this embodiment of the invention can absorb short-wavelength photons in sunlight and release or emit long-wavelength photons based on the energy of the absorbed short-wavelength photons. The light absorption layer 20 absorbs the long-wavelength photons released or emitted by the light conversion and carrier transport structure 30, thereby generating electron-hole pairs. The light conversion and carrier transport structure 30 further separates and collects hole carriers or electron carriers. The first electrode 40 transmits the carriers collected by the light conversion and carrier transport structure 30. Therefore, the solar cell provided in this embodiment of the invention can utilize short-wavelength sunlight, improve light utilization, and thus improve photoelectric conversion efficiency.

[0027] In addition, since the light absorption layer 20 and the light conversion and carrier transport structure 30 work together, short-wavelength photons can be utilized to reduce or even avoid the generation of heat in the solar cell by short-wavelength photons, thereby reducing the temperature rise of the solar cell and improving the efficiency and lifespan of the solar cell.

[0028] Furthermore, the light conversion and carrier transport structure 30, in conjunction with the light absorption layer 20, can effectively improve the conductivity of the solar cell, thereby reducing both the contact resistance and series resistance of the solar cell. The fill factor of the solar cell is related to the series resistance; as the series resistance decreases, the fill factor increases. Therefore, the fill factor of the solar cell provided in this embodiment of the invention is significantly increased, thereby improving the photoelectric conversion efficiency of the solar cell.

[0029] In the solar cell provided in this embodiment of the invention, the crystalline silicon substrate 10 can be an n-type crystalline silicon substrate or a p-type crystalline silicon substrate. The n-type crystalline silicon substrate is generally doped with n-type dopant atoms such as phosphorus, antimony, or arsenic, while the p-type crystalline silicon substrate is generally doped with p-type dopant atoms such as boron or gallium. Understandably, the conductivity type of the n-type crystalline silicon substrate is n-type, and the conductivity type of the p-type crystalline silicon substrate is p-type. Correspondingly, the opposite of the conductivity type of the light conversion and carrier transport structure 30 to the conductivity type of the crystalline silicon substrate 10 means that when the conductivity type of the crystalline silicon substrate 10 is n-type, the conductivity type of the light conversion and carrier transport structure 30 is p-type, and the light conversion and carrier transport structure 30 is doped with p-type doped atoms (such as boron or gallium); when the conductivity type of the crystalline silicon substrate 10 is p-type, the conductivity type of the light conversion and carrier transport structure 30 is n-type, and the light conversion and carrier transport structure 30 is doped with n-type doped atoms (such as phosphorus, arsenic or antimony).

[0030] In a preferred embodiment, the silicon substrate 10 is an n-type silicon substrate, meaning that the silicon substrate 10 is doped with n-type dopant atoms. More preferably, the silicon substrate 10 is further doped with a second dopant particle (described below) on the basis of the n-type silicon substrate. The second dopant particle can be germanium and / or tin. Taking germanium as an example, the content of germanium in the silicon substrate 10 can be 0.01ppm to 10ppm. For example, the content of germanium in the silicon substrate 10 can be 0.01ppm, 0.05ppm, 0.1ppm, 0.5ppm, 1ppm, 5ppm, 6ppm, 8ppm, or 10ppm, etc. By doping the silicon substrate 10 with the second dopant particle, the conductivity of the silicon substrate 10 can be improved, thereby improving the carrier mobility. In addition, by combining the content of the second doped particles in the crystalline silicon substrate 10 with that of the light absorption layer 20, more electron-hole pairs can be generated in or near the light absorption layer 20, reducing the diffusion length of charge carriers to the light conversion and charge carrier transport structure 30, thereby reducing the diffusion loss of charge carriers. This allows the light conversion and charge carrier transport structure 30 to collect more charge carriers, improving the open-circuit voltage while reducing the requirements for minority carrier lifetime and thickness of the crystalline silicon substrate 10.

[0031] Furthermore, compared to existing silicon wafers doped with second doped particles, the crystalline silicon substrate 10 selected in this embodiment of the invention has a lower content of second doped particles, which can effectively reduce the bulk defects of the crystalline silicon substrate 10, thereby improving the yield of solar cells and reducing the concentric circle problem of solar cells.

[0032] In one embodiment of the present invention, the light-absorbing layer 20 generally includes monocrystalline silicon and a first doped particle and a second doped particle doped in the monocrystalline silicon. The first doped particle is the same as the doped particles included in the crystalline silicon substrate 10, and the second doped particle is germanium and / or tin. It should be noted that "the first doped particle is the same as the doped particles included in the crystalline silicon substrate 10" generally means that the first doped particle is the same as the doped particle in the crystalline silicon substrate 10 used to define the conductivity type (e.g., n-type or p-type) of the crystalline silicon substrate 10. For example, if the crystalline silicon substrate 10 contains phosphorus, then the light-absorbing layer 20 also contains phosphorus; if the crystalline silicon substrate 10 contains arsenic, then the light-absorbing layer 20 also contains arsenic; if the crystalline silicon substrate 10 contains boron, then the light-absorbing layer 20 also contains boron, etc. Through the combination of monocrystalline silicon and the first doped particle, the light-absorbing layer 20 can form a relatively good combination with the crystalline silicon substrate 10. The light absorption layer 20 can quickly absorb long-wavelength photons generated by the light conversion and carrier transport structure 30, so as to generate electron-hole pairs faster and more.

[0033] In one embodiment, the light-absorbing layer 20 contains a first doped particle with a doping concentration consistent with that of the doped particles in the crystalline silicon substrate 10, enabling the light-absorbing layer 20 to be formed on the crystalline silicon substrate 10. Specifically, germanium and / or tin are implanted onto the first main surface of the initial crystalline silicon substrate via ion implantation. A portion of the germanium and / or tin implanted serves as the light-absorbing layer 20, while the portion without germanium and / or tin implantation constitutes the aforementioned crystalline silicon substrate 10. Therefore, in the solar cell provided by this embodiment, the light-absorbing layer 20 and the crystalline silicon substrate 10 are generally an integral structure, formed on the same initial crystalline silicon substrate. It can be understood that the crystalline silicon substrate 10 is a part of the initial crystalline silicon substrate. By forming the light-absorbing layer 20 and the crystalline silicon substrate 10 on the same initial crystalline silicon substrate, a significant interface between the light-absorbing layer 20 and the crystalline silicon substrate 10 can be avoided, ensuring light transmission and carrier transport, and reducing interfacial recombination of carriers.

[0034] The content of the second doped particles in the light-absorbing layer 20 is 0.05 ppm to 10 ppm. 4 For example, the content of the second doped particles in the light-absorbing layer 20 can be 0.05ppm, 1ppm, 5ppm, 10ppm, 50ppm, 100ppm, 500ppm, 1000ppm, 5000ppm, or 10 ppm. 4 By controlling the content of the second doped particles in the light absorption layer 20, such as ppm, a stable and reliable asymmetric environment can be ensured for the light conversion and carrier transport structure 30, and the absorption and utilization efficiency of long-wavelength photons emitted or released by the light absorption layer 20 can be guaranteed. Furthermore, the light absorption layer 20 can be made to have strong conductivity, ensuring carrier transport. It is worth noting that, for cases where germanium is doped in the crystalline silicon substrate 10, the content of the second doped particles in the light absorption layer 20 is generally greater than the content of germanium in the crystalline silicon substrate 10.

[0035] In one embodiment of the present invention, in the thickness direction, the content of the second doped particles in the light absorption layer 20 increases from the side away from the light conversion and carrier transport structure 30 to the side closer to the light conversion and carrier transport structure 30. This ensures that the light absorption layer 20 can not only match the crystalline silicon substrate 10 but also match the light conversion and carrier transport structure 30. This guarantees that the region of the light absorption layer 20 close to the light conversion and carrier transport structure 30 can also absorb a large amount of infrared light to generate a large number of electron-hole pairs, enabling the light conversion and carrier transport structure 30 to rapidly separate electrons and holes. Compared to uniform doping of the second doped particles, the regulation of the content of the second doped particles in the light absorption layer 20 provided in this embodiment of the invention can effectively reduce the diffusion length of charge carriers, thereby reducing the loss during the carrier diffusion process, improving the open-circuit voltage of the solar cell, and further reducing the requirements for the minority carrier lifetime and thickness of the crystalline silicon substrate 10. That is, the solar cell provided in this embodiment of the invention can select a thinner crystalline silicon substrate 10 with a poorer minority carrier lifetime to reduce the requirements for the crystalline silicon substrate 10, thereby reducing the cost of the solar cell and reducing the thickness of the solar cell.

[0036] In a preferred embodiment, the doping concentration of the second doped particles in the portion of the light-absorbing layer 20 furthest from the light conversion and carrier transport structure 30 is typically 5 × 10⁻⁶. 15 atoms / cm 3 ~5×10 17 atoms / cm 3 The doping concentration of the portion near the optical conversion and carrier transport structure 30 is typically 1 × 10⁻⁶. 18 atoms cm 3 ~1×10 19 atoms / cm 3 For example, the doping concentration of the second doped particle in the portion farthest from the light conversion and carrier transport structure 30 can be 5 × 10⁻⁶. 15 atoms / cm 3 6×10 15 atoms / cm 3 7×10 15 atoms / cm 3 9×10 15 atoms / cm 3 1×10 16 atoms / cm 3 5×10 16 atoms / cm 3 Or 1×10 17 atoms / cm 3 The doping concentration near the portion of the optical conversion and carrier transport structure 30 can be 1 × 10⁻⁶.18 atoms / cm 3 3×10 18 atoms / cm 3 5×10 18 atoms / cm 3 8×10 18 atoms / cm 3 Or 1×10 19 atoms / cm 3 These measures further reduce the diffusion length of charge carriers, thereby reducing losses during the carrier diffusion process and increasing the open-circuit voltage of the solar cell.

[0037] In this embodiment of the invention, the thickness of the light-absorbing layer 20 is generally 0.2 μm to 0.7 μm. The thickness of the light-absorbing layer 20 generally refers to the distance between the interface of the light-absorbing layer 20 in contact with the light conversion and carrier transport structure 30 and the interface of the light-absorbing layer 20 in contact with the crystalline silicon substrate 10. By controlling the thickness of the light-absorbing layer 20, a stable and reliable asymmetric coordination environment can be ensured for the light-absorbing layer 20 to provide the light conversion and carrier transport structure 30, and the absorption rate of the light-absorbing layer 20 for long-wavelength photons emitted or released by the light conversion and carrier transport structure 30 can be guaranteed. For example, the thickness of the light-absorbing layer 20 can be 0.2 μm, 0.4 μm, 0.5 μm, or 0.7 μm, etc.

[0038] Based on the structure of the light absorption layer 20 provided in any of the above embodiments, the structure of the light conversion and carrier transport structure 30 can be of two types.

[0039] Specifically, the first structure of the light conversion and carrier transport structure 30 includes: single-crystal silicon, a first doped particle doped in the single-crystal silicon, a second doped particle, sensitizer ions of a rare-earth system, activator ions of a rare-earth system, and a fourth doped particle with a conductivity type opposite to that of the crystalline silicon substrate 10. The first doped particle is the same as the doped particle included in the crystalline silicon substrate 10. The doping concentration of the first doped particle in the light conversion and carrier transport structure 30 is the same as the doping concentration of the doped particle included in the crystalline silicon substrate 10. More specifically, the second doped particle in the first structure of the light conversion and carrier transport structure 30 is the same as the second doped particle in the light absorption layer 20, i.e., germanium and / or tin are implanted from the first main surface of the original crystalline silicon substrate to a certain depth in a one-step ion implantation method. Both the light conversion and carrier transport structure 30 and the light absorption layer 20 are formed based on the portion of the original crystalline silicon substrate implanted with germanium and / or tin. The first structural essence of the light conversion and carrier transport structure 30 is that, in the doped diffusion layer formed by doping diffusion, a fourth doped particle with a conductivity type opposite to that of the crystalline silicon substrate 10 is present, along with germanium and / or tin, as well as sensitizer ions and activator ions of the rare earth system. On the one hand, the germanium and / or tin in the doped diffusion layer, along with the sensitizer ions and activator ions of the rare earth system, work together to further ensure that the light conversion and carrier transport structure 30 is in a stable and reliable asymmetric coordination environment, thereby making the light conversion and carrier transport structure 30 a stable and reliable light-emitting center. Furthermore, the sensitizer ions and activator ions in the rare earth system can work together to produce a quantum trimming effect. That is, compared to the activator ions, the sensitizer ions can absorb the energy of short-wavelength photons with a wider wavelength range, thus absorbing more energy from short-wavelength photons. The sensitizer ions transfer the absorbed energy to the activator ions, which then release or emit weaker long-wavelength photons. Since the energy of short-wavelength photons is relatively high and the energy of long-wavelength photons is relatively weak, and since the energy of the short-wavelength photons absorbed by the light conversion and carrier transport structure 30 is basically consistent with the energy of the long-wavelength photons released or emitted, the light conversion and carrier transport structure 30 can release or emit a greater number of long-wavelength photons than the number of short-wavelength photons absorbed by the sensitizer ions. This achieves the conversion of higher-energy short-wavelength photons into more lower-energy long-wavelength photons, allowing these more long-wavelength photons to be utilized by the light absorption layer 20, thereby improving the light utilization rate and photoelectric conversion efficiency of the solar cell.

[0040] The first structure of the optical conversion and carrier transport structure 30 has the functions of optical conversion (converting short-wavelength photons into long-wavelength photons) as well as carrier separation, collection and transport.

[0041] In addition, the first structure of the optical conversion and carrier transport structure 30 can also absorb some long-wavelength photons to generate electron-hole pairs, and the first structure of the optical conversion and carrier transport structure 30 can separate electrons and holes.

[0042] For the first structure of the light conversion and carrier transport structure 30, its thickness is 0.3 μm to 0.5 μm. Since the penetration depth of short-wavelength light (light with a wavelength less than 450 nm) is limited, by controlling the thickness of the first structure of the light conversion and carrier transport structure 30 to be no less than 0.3 μm, as much short-wavelength light as possible can reach the light conversion and carrier transport structure 30. This also allows the light conversion and carrier transport structure 30 to carry sufficient sensitizer ions and activator ions, ensuring the sensitizer ions capture short-wavelength photons and guaranteeing the efficiency of emitting or releasing long-wavelength photons, thereby improving the light utilization rate of the solar cell. Furthermore, by controlling the thickness of the first structure of the light conversion and carrier transport structure 30 to be no greater than 0.5 μm, impurity defects caused by the introduction of sensitizer ions and activator ions can be reduced, thereby reducing carrier recombination in the solar cell. For example, the thickness of the first structure of the light conversion and carrier transport structure 30 can be 0.3 μm, 0.4 μm, or 0.5 μm, etc.

[0043] In this embodiment of the invention, for the first structure of the light conversion and carrier transport structure 30, the content of both the rare-earth system sensitizer ions and the rare-earth system activator ions is 0.05 ppm to 10 ppm. 4 ppm. By controlling the content of sensitizer ions and activator ions, the efficiency of the light conversion and carrier transport structure 30 in absorbing and utilizing short-wavelength photons and emitting or releasing long-wavelength photons can be ensured. For example, the content of sensitizer ions and activator ions can both be 0.05ppm, 1ppm, 5ppm, 10ppm, 50ppm, 100ppm, 1000ppm, or 10 4 ppm, etc.

[0044] Furthermore, for the first structure of the light conversion and carrier transport structure 30, the content of the second doped particles included in the light conversion and carrier transport structure 30 is 20 ppm to 5 × 10⁻⁶. 5 For example, the content of the second doped particles included in the light conversion and carrier transport structure 30 can be 20 ppm, 50 ppm, 100 ppm, 500 ppm, or 10 ppm. 3 ppm, 1×10 4 ppm, 5×10 4 ppm, 1×10 5 ppm or 5×10 5ppm, etc. It is worth noting that the content of the second doped particles in the light conversion and carrier transport structure 30 is greater than that in the light absorption layer 20, so as to ensure that the light conversion and carrier transport structure 30 has a stable and reliable asymmetric environment, which makes it easier for the rare earth ion pairs (sensitizer ions and activator ions) in the light conversion and carrier transport structure 30 to generate energy level splitting, thereby generating luminescent centers and quantum trimming effects, which can enhance the ability of the light conversion and carrier transport structure 30 to absorb short-wavelength photons and generate long-wavelength photons.

[0045] Furthermore, from the side closer to the light absorption layer 20 to the side farther away from the light absorption layer 20, the content of the second doped particles in the light conversion and carrier transport structure 30 increases, so as to provide a more stable and reliable asymmetric environment for the rare earth ion pairs (sensitizer ions and activator ions) in the light conversion and carrier transport structure 30, which is more conducive to the generation of light-emitting centers and quantum clipping effect in the light conversion and carrier transport structure 30, thereby further enhancing the ability of the light conversion and carrier transport structure 30 to absorb short-wavelength photons and generate long-wavelength photons.

[0046] As can be seen from the above, the relationship between the first structure of the light conversion and carrier transport structure 30 provided in the embodiments of the present invention and the crystalline silicon substrate 10 and the light absorption layer 20 is as follows: germanium and / or tin are implanted into a part of the initial crystalline silicon substrate by ion implantation, and the part of the initial crystalline silicon substrate in which germanium and / or tin are not ion implanted serves as the crystalline silicon substrate 10. Further, a part of the part of the initial crystalline silicon substrate in which germanium and / or tin are ion implanted is further ion implanted with sensitizer ions of the rare earth system and activator ions of the rare earth system. Then, the part of the initial crystalline silicon substrate in which germanium and / or tin are ion implanted is partially doped with fourth doped particles. In this structure, the portion of the initial crystalline silicon substrate implanted with germanium and / or tin, without implanted rare earth system sensitizer ions and rare earth system activator ions and without fourth doped particles, serves as the light absorption layer 20. The portion implanted with germanium and / or tin and with implanted rare earth system sensitizer ions and rare earth system activator ions constitutes the first structure of the light conversion and carrier transport structure 30. Furthermore, the light conversion and carrier transport structure 30 is further doped with fourth doped particles.

[0047] In this embodiment of the invention, the second structure of the light conversion and carrier transport structure 30 may include: a light conversion layer 31, a first intrinsic amorphous silicon layer 32, and a first doped non-polycrystalline silicon layer 33. The light conversion layer 31 is disposed on the side of the light absorption layer 20 away from the crystalline silicon substrate 10, and includes monocrystalline silicon, first doped particles, second doped particles, rare-earth system sensitizer ions, and rare-earth system activator ions. The first doped particles are the same as those included in the crystalline silicon substrate 10. The first intrinsic amorphous silicon layer 32 is disposed on the side of the light conversion layer 31 away from the crystalline silicon substrate 10 and is used to passivate the surface of the light conversion layer 31. The first doped non-polycrystalline silicon layer 33 is disposed on the side of the first intrinsic amorphous silicon layer 32 away from the crystalline silicon substrate 10, and includes fourth doped particles with a conductivity type opposite to that of the crystalline silicon substrate 10. The first electrode 40 is electrically connected to the first doped non-polycrystalline silicon layer 33. The light conversion layer 31 is used to convert short-wavelength light into long-wavelength light.

[0048] The doping concentration of the first doped particles in the light conversion layer 31 is consistent with the doping concentration of the doped particles in the crystalline silicon substrate 10. The doping concentration of the second doped particles in the light conversion layer 31 is 20 ppm to 5 × 10⁻⁶. 5 ppm. The doping concentration of the second doped particles in the light conversion layer 31 increases from the side closest to the light absorption layer 20 towards the side furthest from the light absorption layer 20. For example, the doping concentration of the second doped particles in the light conversion layer 31 can be 20 ppm, 50 ppm, 100 ppm, 500 ppm, 10 ppm, or even 10 ppm. 3 ppm, 1×10 4 ppm, 5×10 4 ppm, 1×10 5 ppm or 5×10 5 ppm, etc. It is worth noting that the content of the second doped particles in the light conversion and carrier transport structure 30 is greater than the content of the second doped particles in the light absorption layer 20. The first doped particles, second doped particles, and sensitizer ions and activator ions of the rare earth system in the light conversion layer 31 of this second structure have essentially the same effects as the first doped particles, second doped particles, and sensitizer ions and activator ions of the rare earth system in the light conversion and carrier transport structure 30 of the first structure, and will not be described again here.

[0049] In one optional embodiment, the thickness of the light conversion layer 31 is 0.3 μm to 0.5 μm. This allows as much short-wavelength light as possible to reach the light conversion layer 31, and enables the light conversion layer 31 to carry sufficient sensitizer ions and activator ions. This ensures that the sensitizer ions capture short-wavelength photons and maintain the efficiency of emitting or releasing long-wavelength photons, thereby improving the light utilization rate of the solar cell. Furthermore, by controlling the thickness of the light conversion layer 31 to be no greater than 0.5 μm, impurity defects caused by the introduction of sensitizer ions and activator ions can be reduced, thereby reducing carrier recombination in the solar cell. For example, the thickness of the light conversion layer 31 can be 0.3 μm, 0.4 μm, or 0.5 μm, etc.

[0050] In this embodiment of the invention, the content of both the sensitizer ions and the activator ions in the light conversion layer 31 is 0.05 ppm to 10 ppm. 4 ppm. By controlling the content of sensitizer ions and activator ions, the efficiency of the light conversion layer 31 in absorbing and utilizing short-wavelength photons and emitting or releasing long-wavelength photons can be ensured. For example, the content of sensitizer ions and activator ions in the light conversion layer 31 can both be 0.05ppm, 1ppm, 5ppm, 10ppm, 50ppm, 100ppm, 1000ppm, or 10 4 ppm, etc.

[0051] It is worth noting that, for the second structure of the light conversion and carrier transport structure 30, the first intrinsic amorphous silicon layer 32 and the first doped non-polycrystalline silicon layer 33 generally do not affect the arrival of short-wavelength photons at the light conversion layer 31. In a preferred embodiment, the thickness of the first intrinsic amorphous silicon layer 32 can be 4nm to 6nm. The thickness of the first doped non-polycrystalline silicon layer 33 can be 6nm to 8nm. By coordinating the thicknesses of the first intrinsic amorphous silicon layer 32 and the first doped non-polycrystalline silicon layer 33 with the light absorption layer 20, the amount of short-wavelength photons reaching the light absorption layer 20 can be guaranteed, and the solar cell can be guaranteed to have a high light utilization rate. For example, the thickness of the first intrinsic amorphous silicon layer 32 can be 4nm, 4.5nm, 5nm, 5.5nm, or 6nm. The thickness of the first doped non-polycrystalline silicon layer 33 can be 6nm, 6.5nm, 6.8nm, 7nm, 7.5nm, or 8nm, etc.

[0052] In addition, for the second structure of the light conversion and carrier transport structure 30, the light conversion layer 31 can also absorb some long-wavelength photons to generate electron-hole pairs, and separate electrons and holes through the first doped non-polycrystalline silicon layer 33. Compared with the crystalline silicon substrate 10, the sensitizer ions and activator ions in the light conversion layer 31 can utilize more solar light, thereby improving the light utilization rate of the solar cell. At the same time, the sensitizer ions and activator ions are conductive, which can improve the conductivity of the solar cell.

[0053] Regardless of the first structure of the aforementioned light conversion and carrier transport structure 30, or the light conversion layer 31, the doping amount of sensitizer ions and activator ions can be controlled relatively precisely by injecting sensitizer ions and activator ions through ion implantation.

[0054] It is worth noting that germanium and / or tin, as well as sensitizer ions and activator ions, can be implanted into the textured initial silicon substrate after texturing the surface of the initial silicon substrate by ion implantation, thus avoiding the influence of sensitizer ions and activator ions on the texturing process.

[0055] Furthermore, in this embodiment of the invention, the molar ratio of sensitizer ions to activator ions in the light conversion and carrier transport structure 30 is 0.1:1 to 3:1. By controlling the molar ratio of sensitizer ions to activator ions, the absorption of short-wavelength photons and the emission or release of long-wavelength photons by the light conversion and carrier transport structure 30 can be effectively balanced, thereby effectively improving the light utilization rate and photoelectric conversion efficiency of the solar cell. For example, the molar ratio of sensitizer ions to activator ions in the light conversion and carrier transport structure 30 can be 0.1:1, 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1, or 3:1, etc.

[0056] In this embodiment of the invention, the sensitizer ions include at least one of terbium ions, cerium ions, gadolinium ions, and praseodymium ions; the activator ions include europium ions and / or ytterbium ions. By selecting these ions, the performance of the light conversion and carrier transport structure 30 can be effectively guaranteed, the asymmetric coordination environment of the light conversion and carrier transport structure 30 can be improved, and the light conversion capability of the light conversion and carrier transport structure 30 can be enhanced.

[0057] In a preferred embodiment, at least one of terbium ions, cerium ions, and gadolinium ions is combined with europium ions, and / or praseodymium ions are combined with ytterbium ions to further enhance the optical conversion capability of the optical conversion and carrier transport structure 30.

[0058] Furthermore, regardless of whether it is the first or second structure of the light conversion and carrier transport structure 30 described above, the combination of germanium and / or tin with sensitizer ions and activator ions makes it easier for the light conversion and carrier transport structure 30 to generate light-emitting centers, converting short-wavelength photons into long-wavelength photons. Additionally, since germanium and / or tin have high conductivity, they can also improve carrier mobility, which is beneficial for carrier transport and reduces the series resistance of the solar cell. Compared to existing solar cells based on silicon wafers doped only with germanium and phosphorus or boron, where the high-temperature source absorption process makes germanium prone to surface segregation and increased series resistance, the solar cell provided in this embodiment of the invention combines germanium and / or tin with sensitizer ions and activator ions. These sensitizer ions and activator ions have relatively large ionic radii, which can prevent germanium and tin from segregating to the surface, thereby ensuring the stability of the doped particles while reducing the series resistance of the solar cell.

[0059] Furthermore, regardless of whether it is a solar cell with the first structure of the light conversion and carrier transport structure 30 or a solar cell with the second structure of the light conversion and carrier transport structure 30, the combination of the light absorption layer 20 and the light conversion and carrier transport structure 30 allows for the utilization of most of the energy within a relatively small area. Compared to the germanium-doped silicon wafers used in the prior art, the embodiments of the present invention can use a crystalline silicon substrate 10 with lower germanium and / or tin doping, thereby reducing the bulk defects of the crystalline silicon substrate 10, which is beneficial to improving the yield of solar cells based on the crystalline silicon substrate 10 and reducing the concentric circle problem in solar cells. The concentric circle problem in solar cells is generally due to the high-temperature processing in the cell fabrication process, where oxygen in the crystalline silicon substrate 10 accumulates at defect locations in the crystalline silicon substrate 10, easily resulting in concentric circles on the cell.

[0060] Furthermore, in this embodiment of the invention, the optical conversion and carrier transport structure 30 includes a single-crystal silicon structure (i.e., the first structure of the optical conversion and carrier transport structure 30 described above), such as... Figure 1 As shown, the solar cell also includes a passivation antireflection layer 70 disposed on the side of the light conversion and carrier transport structure 30 away from the light absorption layer 20. By providing the passivation antireflection layer 70, the light conversion and carrier transport structure 30 can be passivated, further reducing defects and carrier recombination. In addition, providing the passivation antireflection layer 70 can also reduce light reflection and increase the amount of light reaching the light conversion and carrier transport structure 30, thereby further improving light utilization efficiency.

[0061] In this embodiment of the invention, the optical conversion and carrier transport structure 30 is a second structure, such as... Figure 2As shown, the first electrode 40 may include: a transparent conductive film layer 41 disposed on the first doped non-polycrystalline silicon layer 33 and a metal electrode 42 disposed on the transparent conductive film layer 41.

[0062] Furthermore, the aforementioned solar cell may further include: a carrier collection layer 50 disposed on the second main surface of the crystalline silicon substrate 10, the conductivity type of the carrier collection layer 50 being the same as that of the crystalline silicon substrate 10; and a second electrode 60 disposed on the side of the carrier collection layer 50 away from the crystalline silicon substrate 10, the second electrode 60 being electrically connected to the carrier collection layer 50. That is, if the conductivity type of the crystalline silicon substrate 10 is n-type, then the conductivity type of the carrier collection layer 50 is n-type; if the conductivity type of the crystalline silicon substrate 10 is p-type, then the conductivity type of the carrier collection layer 50 is p-type.

[0063] Among them, the carrier collection layer 50 has various structures.

[0064] The first structure of the carrier collection layer 50: The carrier collection layer 50 is a doped diffusion layer containing a fifth doped particle, the conductivity type of which is the same as that of the crystalline silicon substrate 10.

[0065] The second structure of the carrier collection layer 50: The carrier collection layer 50 includes a first passivation layer 51 stacked from the inside to the outside and a doped polysilicon layer 52 containing a fifth doped particle, the conductivity type of the fifth doped particle being the same as that of the crystalline silicon substrate 10.

[0066] The third structure of the carrier collection layer 50: The carrier collection layer 50 includes a second intrinsic amorphous silicon layer stacked from the inside to the outside and a second doped non-polycrystalline silicon layer containing a fifth doped particle, wherein the conductivity type of the fifth doped particle is the same as that of the crystalline silicon substrate 10.

[0067] For example, if the conductivity type of the crystalline silicon substrate 10 is n-type, then the fifth doped particle is phosphorus, arsenic or antimony, etc.; if the conductivity type of the crystalline silicon substrate 10 is p-type, then the fifth doped particle is boron or gallium, etc.

[0068] The three structures of the carrier collection layer 50 described above can be arbitrarily combined with the two structures of the optical conversion and carrier transmission structure 30 to better meet the needs of users or the market.

[0069] In a preferred embodiment, the crystalline silicon substrate 10 has an n-type conductivity, the light conversion and carrier transport structure 30 has a p-type conductivity, and the carrier collection layer 50 has an n-type conductivity. Compared with the p-type crystalline silicon substrate 10, the n-type crystalline silicon substrate 10 has fewer defects and can effectively improve the photoelectric conversion efficiency of the solar cell.

[0070] It is worth noting that the light absorption layer 20 and the light conversion and carrier transport structure 30 are located on the light-receiving surface of the solar cell to ensure the conversion of short-wavelength light and further improve light utilization and photoelectric conversion efficiency.

[0071] It is worth noting that the light-receiving surface of the solar cell provided in any of the above embodiments can be... Figure 1 The velvet structure shown can also be Figure 2 The structure of the polished surface is shown.

[0072] Furthermore, embodiments of the present invention provide a method for fabricating a solar cell. Specifically, as shown in the figure... Figure 3 As shown, the preparation method may include: Step S1: Provide an initial crystalline silicon substrate 10'.

[0073] The initial crystalline silicon substrate 10' can be an n-type crystalline silicon substrate or a p-type crystalline silicon substrate.

[0074] Step S2: A light absorption layer 20 and a light conversion and carrier transport structure 30 are sequentially stacked on the first main surface of the initial crystalline silicon substrate 10'. The portion of the initial crystalline silicon substrate 10' other than the light absorption layer 20 and the light conversion and carrier transport structure 30 forms the crystalline silicon substrate 10. The conductivity type of the light conversion and carrier transport structure 30 is opposite to that of the crystalline silicon substrate 10.

[0075] Step S3: Form a first electrode 40 electrically connected to the light conversion and carrier transport structure 30 on the light conversion and carrier transport structure 30.

[0076] Among them, the structural changes corresponding to steps S1 to S3 are as follows: Figure 4 As shown.

[0077] The above preparation method is used to prepare the solar cell provided in any of the above embodiments.

[0078] The solar cell prepared by the method provided in this embodiment of the invention utilizes a light absorption layer 20 and a light conversion and carrier transport structure 30. The light conversion and carrier transport structure 30 can absorb short-wavelength photons in sunlight and release or emit long-wavelength photons based on the energy of the absorbed short-wavelength photons. The light absorption layer 20 absorbs the long-wavelength photons released or emitted by the light conversion and carrier transport structure 30, thereby generating electron-hole pairs. The light conversion and carrier transport structure 30 further separates and collects hole carriers or electron carriers. The first electrode 40 transmits the carriers collected by the light conversion and carrier transport structure 30. Therefore, the solar cell prepared by the method provided in this embodiment of the invention can utilize short-wavelength sunlight, improve light utilization, and thus improve photoelectric conversion efficiency.

[0079] In one embodiment, the initial crystalline silicon substrate 10' provided in step S1 is generally obtained by cutting a single-crystal silicon rod doped with n-type dopant atoms (such as phosphorus) and germanium. Specifically, high-purity polycrystalline silicon is selected as the substrate material, with a purity of not less than 99.9999999% (9N grade), and surface oxide layers, dust, and metallic impurities are removed to avoid substrate impurities interfering with the doping effect; high-purity germanium particles are selected as the dopant, with a purity of not less than 99.999% (5N grade), and the germanium particle size is controlled between 1 mm and 5 mm to ensure rapid melting and uniform diffusion during doping, without the introduction of additional impurities. Polycrystalline silicon material is immersed in a mixed solution of hydrofluoric acid and nitric acid (volume ratio 1:3) for 30-40 minutes to remove the natural oxide layer and metallic contaminants on the surface. It is then repeatedly rinsed with ultrapure water until the pH is neutral (6.8-7.2), and placed in a clean drying oven at 120-150℃ for 2-3 hours to completely remove moisture. High-purity germanium granules are ultrasonically cleaned with anhydrous ethanol for 15-20 minutes to remove surface oil, and then dried at 100-120℃ for 1 hour. After cooling to room temperature, they are sealed for later use. Based on the formula for segregation and concentration, the corresponding mass of germanium granules (approximately 100-200g per rod) is weighed. During the melting process, before the last batch is finished, the germanium granules are added to the crucible melt using a silicon box to ensure the germanium doping concentration in the silicon wafer. The crystal pulling, necking, shoulder formation, equal diameter setting, and tailing processes are performed using conventional methods. The total cooling time for the crystal rod is 24-36 hours. Slow cooling eliminates internal stress in the crystal rod, preventing defects such as cracks and dislocations. After cooling, the argon gas supply is shut off, the furnace door is opened, and the germanium- and n-type doped single-crystal silicon rods are removed. The single-crystal silicon rods are then truncated using diamond wire, with the truncated length controlled between 750mm and 850mm to achieve optimal slicing results. During truncating, the cutting speed is controlled between 0.5mm / s and 1mm / s, and the cooling water flow rate is 10L / min to 15L / min. The dimensional accuracy of the squared ingot is controlled within ±0.1 mm, and the flatness is ≤0.05 mm / m. Strict control of cutting precision is necessary during the squaring process to avoid problems such as ingot skewing and edge chipping. A multi-wire slicing machine was used to slice the crystalline silicon substrate. The silicon wafer thickness was set to 110μm~180μm, and the slicing speed was 0.1mm / s~0.3mm / s to ensure that the sliced ​​surface was flat, free of scratches, and met other silicon wafer quality requirements. After slicing, the wafers were sequentially subjected to alkaline washing, acid washing, ultrapure water rinsing, slow lifting, and drying to obtain an n-type crystalline silicon substrate with low germanium content.

[0080] For step S2 above, one specific implementation may include steps S21 to S23: Step S21: Ion implant second doped particles into the initial silicon substrate 10' from the first main surface of the initial silicon substrate 10' at a first depth H1. The portion of the initial silicon substrate 10' without implantation of the second doped particles is the silicon substrate 10.

[0081] The second doped particle is germanium and / or tin. Step S22: Ion implant sensitizer ions and activator ions of the rare earth system into the initial crystalline silicon substrate 10' at a second depth H2 from the first main surface of the initial crystalline silicon substrate 10', and anneal it, wherein the second depth H2 is less than the first depth H1, and the portion of the initial crystalline silicon substrate 10' located between the first depth H1 and the second depth H2 forms a light absorption layer 20.

[0082] The structural changes corresponding to steps S21 and S22 above, as well as the first depth H1 and the second depth H2, are as follows: Figure 5 and Figure 6 As shown.

[0083] It is worth noting that, Figures 4 to 6 Taking the first main surface of the initial crystalline silicon substrate 10' as a textured structure as an example, the formation process of each film layer is explained. It can be understood that the first main surface of the initial crystalline silicon substrate 10' can also be a polished surface. The film layers formed on the polished surface are basically the same as the film layers formed on the textured surface. Therefore, the process of forming each film layer on the polished surface will not be described again.

[0084] The above steps S21 and S22, by implanting the second doped particles, sensitizer ions and activator ions through ion implantation, can more accurately control the doping amount and doping range of the second doped particles, sensitizer ions and activator ions. Furthermore, the doping can be carried out after the first main surface of the initial crystalline silicon substrate 10' has been textured, which can avoid the second doped particles, sensitizer ions and activator ions affecting the texturing process.

[0085] Step S23: Based on the intermediate product obtained in step S22, prepare the optical conversion and carrier transport structure 30.

[0086] More specifically, for the first structure of the aforementioned light conversion and carrier transport structure 30, step S23 includes: diffusing fourth doped particles of the opposite conductivity type to the initial silicon substrate 10' from the first main surface of the initial silicon substrate 10', wherein the third depth H3 of the fourth doped particles is less than the second depth H2, and the portion of the initial silicon substrate 10' from the first main surface to the second depth forms the light conversion and carrier transport structure 30. Specifically, for the first structure of the light conversion and carrier transport structure 30, the structural change and third depth H3 corresponding to step S23 are as follows: Figure 5As shown. For n-type silicon substrates, the fourth doped particle is boron or gallium, etc.; for p-type silicon substrates, the fourth doped particle is phosphorus, arsenic, or antimony, etc.

[0087] Furthermore, based on the fabrication of the first structure of the light conversion and carrier transport structure 30, after step S2, the method may further include: step S2': depositing a passivation antireflection layer 70 on the light conversion and carrier transport structure 30; after step S2', the method may further include: step S2'': fabricating a carrier collection layer 50 on the second main surface of the crystalline silicon substrate 10, for example, as shown in... Figure 5 The diagram illustrates the cross-sectional structural changes of the carrier collection layer 50 prepared in steps S2' and S2'', which includes a first passivation layer 51 and a doped polysilicon layer 52, with a second passivation layer 80 fabricated on the doped polysilicon layer 52. The passivation antireflection layer 70 and the carrier collection layer 50, including the first passivation layer 51, the doped polysilicon layer 52, and the second passivation layer 80 located on the carrier collection layer 50, can be implemented using existing technologies and will not be elaborated upon here.

[0088] Furthermore, in addition to fabricating the first electrode 40 electrically connected to the light conversion and carrier transport structure 30, step S3 can also fabricate a second electrode 60 electrically connected to the carrier collection layer 50. The cross-sectional structure change corresponding to step S3 is as follows: Figure 5 As shown.

[0089] Regarding the second structure of the aforementioned light conversion and carrier transport structure 30, in the intermediate product obtained in step S22, the implantation range of sensitizer ions and activator ions (i.e., the portion of the initial crystalline silicon substrate 10' from the first main surface to the second depth) constitutes the light conversion layer 31; step S23 includes: sequentially stacking a first intrinsic amorphous silicon layer 32 and a first doped non-polycrystalline silicon layer 33 on the light conversion layer 31, wherein the first doped non-polycrystalline silicon layer 33 contains fourth doped particles with a conductivity type opposite to that of the crystalline silicon substrate 10. The corresponding cross-sectional structure changes are as follows: Figure 6 As shown.

[0090] Furthermore, for the fabrication of a solar cell with a second structure having a light conversion and carrier transport structure 30, step S1' may be included after step S1: fabricating a carrier collection layer 50 on the second main surface of the crystalline silicon substrate 10. Specifically, for cases where the carrier collection layer 50 is a doped diffusion layer or includes a stacked first passivation layer 51 and a doped polycrystalline silicon layer 52, step S1' further includes: fabricating a second passivation layer 80 on the carrier collection layer 50, and fabricating a second electrode 60 electrically connected to the carrier collection layer 50. For example, Figure 6The prepared carrier collection layer 50 is shown to include a stacked first passivation layer 51 and a doped polysilicon layer 52. Based on this, step S2 is performed on the first main surface of the initial crystalline silicon substrate 10' in the intermediate product prepared in step S1'.

[0091] Furthermore, for the fabrication of a solar cell with a second structure having a light conversion and carrier transport structure 30, a specific implementation of step S3 may include: forming a transparent conductive film layer 41 on the first doped non-polycrystalline silicon layer 33, and forming a metal electrode 42 on the transparent conductive film layer 41. The structural change corresponding to step S3 is as follows: Figure 6 As shown.

[0092] It is worth noting that, Figure 5 and Figure 6 This is merely an illustrative example of a structure where the first main surface of the crystalline silicon substrate 10 is polished. Based on the above description, those skilled in the art will understand that the first main surface of the crystalline silicon substrate 10 can also be textured. For example, the initial crystalline silicon substrate 10' can be treated using an alkaline texturing method. <001> (Crystal orientation) Sodium hydroxide was selected as the main etchant, and a sodium hydroxide aqueous solution with a mass fraction of 1%~2% was prepared. Isopropanol with a volume fraction of 0.5%~1% was added as a corrosion inhibitor. The initial crystalline silicon substrate 10' was inserted into a basket and slowly placed into the constant temperature texturing solution to ensure that the initial crystalline silicon substrate 10' was completely immersed. The reaction time was controlled at 15min~25min. During the reaction, the basket was gently shaken once every 5min to promote reaction uniformity. After immersion, acid washing, ultrapure water washing, slow lifting, and drying were performed to obtain the texturized initial crystalline silicon substrate 10'.

[0093] The technical solutions provided by the embodiments of the present invention will be described in detail below with reference to several examples and comparative examples.

[0094] Example 1

[0095] Step A: Provide an initial n-type crystalline silicon substrate doped with 8 ppm germanium.

[0096] Step B: Select an aqueous solution containing 1.5% sodium hydroxide by mass. Add a certain amount of isopropanol (20% by mass) to the sodium hydroxide solution as a texturing solution. Insert the germanium-doped n-type silicon substrate provided in Step A into a basket and slowly immerse it in the constant-temperature texturing solution, ensuring that the germanium-doped n-type silicon substrate is completely submerged. Control the reaction time to 20 minutes. During the reaction, gently shake the basket once every 5 minutes to promote reaction uniformity. After immersion, perform acid washing, ultrapure water washing, slow lifting, and drying to obtain the initial germanium-doped n-type silicon substrate after texturing (hereinafter referred to as the textured germanium-doped silicon substrate).

[0097] Step C: Adsorb the textured germanium-doped silicon substrate onto the worktable, with the front side facing the ion beam direction and the back side completely covered by a high-purity quartz shield to prevent back-side mis-implantation. Maintain a 4mm spacing between adjacent textured germanium-doped silicon substrates to ensure uniform ion beam coverage. Place the worktable into the vacuum chamber and start evacuating to a vacuum level of 5×10⁻⁶. -5 The concentration was maintained below a certain level for 30 minutes. High-purity germanium (purity greater than 99.999%) was used as the ion source to generate Ge through ionization. + Germanium was implanted into a textured germanium-doped silicon substrate within a depth range of 0 μm to 0.5 μm (depth refers to the distance from any implanted germanium location to the surface of the textured germanium-doped silicon substrate; the depth corresponding to the surface of the textured germanium-doped silicon substrate is 0 μm, meaning that the implantation depth range refers to the area within 0.5 μm inward from the surface of the textured germanium-doped silicon substrate being doped with germanium). The implantation concentration was controlled by ion beam dosing, maintaining a surface implantation concentration of 1 ppm and an attenuation rate of 50% / μm within the implantation depth range of 0 μm to 0.3 μm. This was to enhance red light absorption while providing an asymmetric crystal field environment for rare earth ions. At a depth of 0.3 μm, the implantation concentration was maintained at 0.5 ppm, with an attenuation rate of 10% / μm within the depth range of 0.3 μm to 0.5 μm, achieving the preset implantation concentration.

[0098] Step D: Using high-purity oxides Tb₂O₃ and Eu₂O₃ as ion source raw materials, pure Tb is obtained through ion source ionization and screening by a mass analyzer. 3+ and Eu 3+ The ion beam was used to implant the substrate at a depth range of 0 μm to 3 μm (meaning that the substrate was doped with Tb within a 3 μm radius from the surface of the textured germanium-doped silicon substrate). 3+ and Eu 3+ ), corresponding to an accelerating voltage of 75keV; Tb 3+ The injection concentration was 0.5 ppm, Eu 3+ The implantation concentration was 1 ppm. After reaching the preset implantation dose, the ion beam system was shut off, and the vacuum chamber was maintained in a vacuum state for 25 minutes to allow the textured germanium-doped silicon substrate with germanium and rare earth ions implanted in some areas to cool naturally to below 80°C, releasing the thermal stress accumulated during the implantation process. Then, high-purity argon gas was slowly introduced to gradually restore the chamber pressure to atmospheric pressure, avoiding impurity adsorption caused by sudden pressure changes. After ion implantation, the textured germanium-doped silicon substrate with germanium and rare earth ions implanted in some areas needed to be rapidly annealed: the temperature was raised to 750°C at a rate of 40°C / s in an annealing furnace and annealed for 90 seconds, followed by rapid cooling at a rate of 80°C / min to repair lattice defects caused by ion implantation.

[0099] Step E: Immerse the product obtained in step D in a 5% dilute HF solution for 120 seconds to remove the natural oxide layer on the surface; rinse with ultrapure water for 5 minutes, and dry in a 130℃ oven for 12 minutes.

[0100] In steps F and E, the surface of the product after cleaning, in which germanium and rare earth ions were implanted, underwent boron diffusion. The diffusion source for boron diffusion was liquid trimethylboron (TMB), and the carrier gas was high-purity N2 (99.9999%). During the boron diffusion process, the temperature was increased from room temperature to 880°C at a heating rate of 8°C / min. At 880°C and an O2 flow rate of 300 sccm, the surface of the product in which germanium and rare earth ions were implanted was pre-oxidized: held for 10 min to grow a thin oxide buffer layer of 1.2 nm. Then, at the same temperature of 880°C, a TMB bubbling flow rate of 15 sccm, and an N2 flow rate of 1200 sccm, a boron source layer was deposited for 25 min. After that, the temperature was increased to 920°C and held in a pure N2 atmosphere for 40 min to advance boron atoms to a depth of 0.5 μm. Then, the temperature is reduced to 600°C at a cooling rate of 5°C / min, and then removed from the furnace and cooled to room temperature. The part implanted with germanium but not implanted with rare earth ions and diffused with boron atoms is the light absorption layer 20, and the part implanted with germanium and rare earth ions and partially diffused with boron atoms is the light conversion and carrier transport structure 30. In addition, this step also forms a borosilicate glass layer (BSG) on the surface of the light conversion and carrier transport structure 30.

[0101] Step G: Remove BSG by washing with HF solution.

[0102] Step H: By atomic layer deposition, an aluminum oxide passivation layer with a thickness of 10 nm is prepared on the light conversion and carrier transport structure 30 with trimethylaluminum as a precursor and H2O as an oxidant at a process temperature of 200 °C. Annealing is then carried out at a temperature of 400 °C in a nitrogen atmosphere for 15 min to activate the hydrogen passivation centers of the aluminum oxide passivation layer and reduce the surface recombination rate.

[0103] The second main surface of the product obtained in steps I and H is subjected to low-pressure plasma chemical vapor deposition at a vacuum degree ≤8×10⁻⁶. -4 Oxidation was carried out at a temperature of 600℃ and an N2O flow rate of 400 sccm for 18 min to obtain a tunneling oxide layer with a thickness of 1.3 nm (i.e., the first passivation layer 51 mentioned above).

[0104] Step J: Plasma-enhanced chemical vapor deposition (PECVD) is used to deposit a 200 nm thick phosphorus doping concentration of 1 × 10² on the tunneling oxide layer at a temperature of 200 °C, a SiH₄ flow rate of 120 sccm, a PH₃ doping source flow rate of 8 sccm, and an H₂ flow rate of 500 sccm. 0 A phosphorus-doped polycrystalline silicon layer with atoms / cm³ was deposited in 32 minutes.

[0105] Step K: Under a nitrogen atmosphere, the phosphorus-doped polycrystalline silicon layer is annealed and activated. During the annealing process, a pure N2 protective atmosphere with a flow rate of 2000 sccm is used, the heating rate is 10℃ / min, the peak temperature is 900℃, the isothermal annealing time is 50min, the cooling rate is 6℃ / min, and the temperature is reduced to 300℃.

[0106] Step L: Deposit silicon nitride anti-reflection passivation films on the alumina passivation layer and the phosphorus-doped polycrystalline silicon layer respectively by plasma-enhanced chemical vapor deposition.

[0107] Step M, front-side double-layer SiN x Antireflective coating preparation was carried out under constant temperature of 220℃ and chamber pressure of 0.9 Torr, with continuous layer-by-layer deposition to meet the full-spectrum antireflection requirements. Specifically, the bottom high-refractive-index layer, close to the silicon nitride antireflective passivation film, had a gas ratio of SiH4:NH3 = 1:8, RF power of 750W, and was deposited for 4 min; the resulting refractive index was 2.15 and the thickness was 8 nm, used to match the silicon nitride antireflective passivation film and optimize interface optical matching. The top low-refractive-index layer maintained a constant gas ratio, with the RF power finely adjusted to 680W, and was deposited for 24 min; the resulting refractive index was 2.05 and the thickness was 75 nm, achieving an average reflectivity of <2.0% in the 300~1100nm wavelength range. After deposition, the chamber was purged with high-flow-rate nitrogen for 3 min to remove residual process gases.

[0108] Step N: Fabrication of a monolayer SiN on the back side x Protective film, continuously deposited for 20 min at a constant temperature of 200℃, a cavity pressure of 0.9 Torr, a gas ratio of SiH4:NH3 = 1:10, and a radio frequency power of 580W; monolayer SiN x The protective film has a refractive index of 1.90 and a thickness of 80 nm.

[0109] Step O: Using a 1064nm wavelength laser, at a power of 13W, a reverse bias of -1000V, and a scanning speed of 4000mm / s, the laser locally etches the passivation antireflection layer, creating grooves to expose the phosphorus-doped polycrystalline silicon layer and the light conversion and carrier transport structure 30, reserving a channel for subsequent screen printing and sintering to form ohmic contacts.

[0110] Step P: Screen printing metallization, using 30 silver paste for the light conversion and carrier transport structure. The screen specifications are: line width opening 18μm, grid line height ≥12μm, aspect ratio ≥0.65. The printing parameters are: squeegee speed 220mm / s, squeegee pressure 0.35MPa, printing gap 2.0mm, and ink return speed 300mm / s.

[0111] Step Q: Print silver-aluminum paste onto the phosphorus-doped polycrystalline silicon layer with a width of 1.2 mm, a printing thickness of 15 μm, a printing gap of 2.0 mm, a squeegee hardness of 75°, an ink return speed of 300 mm / s, an ink return pressure of 0.25 MPa, a printing speed of 220 mm / s, and a printing pressure of 0.35 MPa.

[0112] Step R: After printing, the product is dried in a chain oven at 180°C in stages for a total time of 120 seconds to remove organic solvents from the paste. Then, a chain-type high-temperature co-sintering process is performed. Specifically, this involves a four-zone sintering furnace with a belt speed of 1800 mm / min. The low-temperature debinding zone is at 400°C to remove the organic carrier. The medium-temperature glass melting zone is at 600°C, where silver paste and glass powder soften and etch silicon nitride. The peak sintering zone temperature is 700°C, held for 12 seconds, and silver and silicon form a dense ohmic contact with a sintering penetration depth ≤0.1 μm. The rapid cooling zone uses forced air cooling at a cooling rate of 80°C / min, resulting in a furnace exit temperature <120°C.

[0113] Example 2

[0114] The difference from Example 1 is that Ge is injected in step C. + The surface injection concentration was 2 ppm, and the injection concentration at a depth of 0.25 μm was maintained at 1 ppm.

[0115] Comparative Example 1

[0116] The difference from Example 1 is that the n-type crystalline silicon substrate provided in step A is undoped with germanium, and steps C and D are omitted.

[0117] Comparative Example 2

[0118] The difference from Example 1 is that steps C and D are omitted.

[0119] Comparative Example 3

[0120] The difference from Example 1 is that step D is omitted.

[0121] Comparative Example 4

[0122] The difference from Example 1 is that step C is omitted, and only Eu is injected in step D. 3+ Eu 3+ The injection concentration was 0.2 ppm, without the sensitizer Tb. 3+ injection.

[0123] Comparative Example 5

[0124] The difference from Example 1 is that step C is omitted, and Tb is added in step D. 3+ The injection concentration was 0.1 ppm, Eu 3+ The injection concentration was 0.2 ppm.

[0125] Comparative Example 6

[0126] The difference from Example 1 is that step C is omitted.

[0127] Comparative Example 7

[0128] The difference from Example 1 is that Ge is injected in step C. + The surface implantation concentration was 20,000 ppm, and the implantation concentration at a depth of 0.2 μm was maintained at 10,000 ppm; in step D, Tb 3+ The injection concentration was 20,000 ppm, Eu 3+ The injection concentration was 20,000 ppm.

[0129] The solar cells prepared in the above embodiments and comparative examples were subjected to IV photoelectric performance testing at an AM1.5 standard light intensity of 1000 W / m². 2 The tests were conducted at a constant temperature of 25℃, and the results were statistically analyzed and calculated to obtain the photoelectric conversion efficiency (Eta), open-circuit voltage (Voc), short-circuit current (Jsc), fill factor (FF), and series resistance of the solar cell. The test results are shown in Table 1 below.

[0130] Table 1

[0131] As can be seen from Table 1 above, compared with Comparative Example 1 (conventional solar cell), Comparative Example 2 (solar cell based on a low-doped germanium crystalline silicon substrate, without secondary germanium implantation, and without implantation of rare-earth system sensitizer ions and rare-earth system activator ions), Comparative Example 3 (solar cell without implantation of rare-earth system sensitizer ions and rare-earth system activator ions), Comparative Example 4 (solar cell without implantation of high surface concentration germanium and rare-earth system sensitizer ions, only implantation of rare-earth system activator ions), and Comparative Examples 5 and 6 (solar cell without germanium implantation, only implantation of rare-earth system sensitizer ions and rare-earth system activator ions), the solar cells prepared in Examples 1 and 2 show improved cell efficiency, short-circuit current, series resistance, and fill factor. It is evident that the performance of solar cells can be effectively improved by combining the light absorption layer 20 and the light conversion and carrier transport structure 30 in the technical solution provided by the embodiments of the present invention.

[0132] Comparing Comparative Example 1 and Comparative Example 2, it can be seen that doping the crystalline silicon substrate 10 with germanium optimizes the ohmic contact of the solar cell and improves the carrier collection capability of the solar cell's electrodes, thus reducing the series resistance of the solar cell (i.e., the series resistance of the solar cell in Comparative Example 2 is lower than that in Comparative Example 1). Furthermore, doping the crystalline silicon substrate 10 with germanium also helps to improve the fill factor of the solar cell. Additionally, germanium doping can increase the light absorption of the crystalline silicon substrate, thereby increasing the short-circuit current of the solar cell. Although the cell efficiency, open-circuit voltage, short-circuit current, series resistance, and fill factor of Comparative Example 2 are all changed compared to Comparative Example 1 by using low-doped germanium, the changes are still not significant.

[0133] Compared to Comparative Example 2, Comparative Example 3 introduced a light-absorbing layer 20 on a low-doped germanium n-type crystalline silicon substrate. Compared to Comparative Example 2, the open-circuit voltage of Comparative Example 3 showed a slight decrease. This is because the introduction of the light-absorbing layer 20 increases the germanium doping concentration, which generates more defects, resulting in a slight decrease in open-circuit voltage. The introduction of the light-absorbing layer 20 can increase light absorption, thereby increasing the short-circuit current of Comparative Example 3. Compared to Comparative Example 2, the cell efficiency of the solar cell in Comparative Example 3 is not significantly improved, indicating that the light-absorbing layer 20 alone does not significantly improve the performance of the solar cell.

[0134] Compared to Comparative Example 2, Comparative Example 4 only injected one type of activator ion, Eu. 3+ Without the injection of sensitizer ions, the short-circuit current increased and the open-circuit voltage decreased slightly, indicating that the single activator ion produced defects, leading to a decrease in open-circuit voltage and making the change in the efficiency of the photo-absorbing cell insignificant.

[0135] Compared to Comparative Example 1, Comparative Examples 5 and 6 only introduced the light conversion and carrier transport structure 30, resulting in a slight decrease in their open-circuit voltage. This indicates that the introduction of activator and sensitizer ions also introduces certain defects. However, compared to Comparative Examples 1, 2, and 4, Comparative Examples 5 and 6 showed a significant increase in short-circuit current. This suggests that simultaneously introducing activator and sensitizer ions into the light conversion and carrier transport structure 30 can improve light utilization and conductivity, thereby increasing the short-circuit current and fill factor of the solar cell and reducing the series resistance. However, the improvement in the photoelectric conversion efficiency of the solar cell is still not significant.

[0136] Compared with Comparative Examples 1 to 6, Examples 1 and 2 show significant improvements in short-circuit current and fill factor, and significant reductions in series resistance, indicating that the combination of the light absorption layer 20 and the light conversion and carrier transport structure 30 can effectively improve light utilization and conductivity. Although germanium in the light absorption layer 20 and rare earth ions in the light conversion and carrier transport structure 30 introduce certain defects, resulting in a slight decrease in open-circuit voltage, the overall efficiency of the solar cell is significantly improved. That is, the overall benefit from the combination of the light absorption layer 20 and the light conversion and carrier transport structure 30 far outweighs the adverse effects of the reduced open-circuit voltage caused by the defects in the light absorption layer 20 and the light conversion and carrier transport structure 30. Therefore, the solar cell provided in this embodiment of the invention, through the combination of the light absorption layer 20 and the light conversion and carrier transport structure 30, can effectively improve the performance of the solar cell.

[0137] Comparing Comparative Example 7 with Examples 1 and 2, it can be seen that the photoelectric conversion efficiency, open-circuit voltage, short-circuit current, fill factor, and series resistance of Comparative Example 7 are all significantly reduced. This indicates that when the content of various dopants exceeds the range provided by the embodiments of the present invention, the photoelectric conversion efficiency, open-circuit voltage, short-circuit current, and fill factor of the solar cell all decrease significantly. The decrease in series resistance of Comparative Example 7 is mainly due to the increased content of various dopants, which enhances conductivity. However, the decrease in series resistance of Comparative Example 7 cannot offset the negative impact of the reduced photoelectric conversion efficiency, open-circuit voltage, short-circuit current, and fill factor of the solar cell caused by the content of various dopants exceeding the range provided by the embodiments of the present invention.

[0138] The above steps are provided only to help understand the method, structure, and core ideas of this invention. Those skilled in the art can make various improvements and modifications to this invention without departing from its principles, and these improvements and modifications also fall within the scope of protection of the claims.

Claims

1. A solar cell, characterized in that, include: Crystalline silicon substrate (10); A light-absorbing layer (20) is disposed on the first main surface of the crystalline silicon substrate (10); A light conversion and carrier transport structure (30) is disposed on the side of the light absorption layer (20) away from the crystalline silicon substrate (10), and the conductivity type of the light conversion and carrier transport structure (30) is opposite to that of the crystalline silicon substrate (10). The first electrode (40) is disposed on the side of the light conversion and carrier transport structure (30) away from the crystalline silicon substrate (10), and the first electrode (40) is electrically connected to the light conversion and carrier transport structure (30).

2. The solar cell according to claim 1, characterized in that, The light absorption layer (20) includes monocrystalline silicon and a first doped particle and a second doped particle doped in the monocrystalline silicon, wherein the first doped particle is the same as the doped particles included in the crystalline silicon substrate (10), and the second doped particle is germanium and / or tin. Optionally, the light-absorbing layer (20) contains the same doping concentration of the first doped particles as the doping concentration of the doped particles contained in the crystalline silicon substrate (10); Optionally, the content of the second doped particles in the light-absorbing layer (20) is 0.05 ppm to 10 ppm. 4 ppm; Optionally, the content of the second doped particles in the light absorption layer (20) increases from the side away from the light conversion and carrier transport structure (30) to the side closer to the light conversion and carrier transport structure (30); Optionally, for the light absorption layer (20), the doping concentration of the second doped microparticles away from the interface of the light conversion and carrier transport structure (30) is 5 × 10⁻⁶. 15 atoms / cm 3 ~5×10 17 atoms / cm 3 The doping concentration near the interface of the optical conversion and carrier transport structure (30) is 1×10⁻⁶. 18 atoms / cm 3 ~1×10 19 atoms / cm 3 ; And / or, The thickness of the light absorption layer (20) is 0.2μm~0.7μm.

3. The solar cell according to claim 1 or 2, characterized in that, The optical conversion and carrier transport structure (30) includes: single crystal silicon, a first doped particle, a second doped particle, a rare earth system sensitizer ion, a rare earth system activator ion, and a fourth doped particle with a conductivity type opposite to that of the crystalline silicon substrate (10), wherein the first doped particle is the same as the doped particle included in the crystalline silicon substrate (10). Optionally, the optical conversion and carrier transport structure (30) includes a doping concentration of the first doped particles that is consistent with the doping concentration of the doped particles included in the crystalline silicon substrate (10); Optionally, the doping concentration of the second doped particles included in the optical conversion and carrier transport structure (30) is 20 ppm to 5 × 10⁻⁶. 5 ppm; Optionally, the doping concentration of the second doped particles in the light conversion and carrier transport structure (30) increases from the side closer to the light absorption layer (20) to the side farther away from the light absorption layer (20). Optionally, the thickness of the optical conversion and carrier transport structure (30) is 0.3 μm to 0.5 μm; Optionally, in the light conversion and carrier transport structure (30), the content of both the sensitizer ions and the activator ions of the rare earth system is 0.05 ppm to 10 ppm. 4 ppm; or, The optical conversion and carrier transport structure (30) includes: an optical conversion layer (31), a first intrinsic amorphous silicon layer (32), and a first doped non-polycrystalline silicon layer (33). The light conversion layer (31) is disposed on the side of the light absorption layer (20) away from the crystalline silicon substrate (10), and includes monocrystalline silicon, a first doped particle, a second doped particle, a rare earth system sensitizer ion and a rare earth system activator ion, wherein the first doped particle is the same as the doped particle included in the crystalline silicon substrate (10). The first intrinsic amorphous silicon layer (32) is disposed on the side of the light conversion layer (31) away from the crystalline silicon substrate (10) and is used to passivate the surface of the light conversion layer (31); The first doped amorphous silicon layer (33) is disposed on the side of the first intrinsic amorphous silicon layer (32) away from the crystalline silicon substrate (10), and contains a fourth doped particle with a conductivity type opposite to that of the crystalline silicon substrate (10). The first electrode (40) is electrically connected to the first doped non-polycrystalline silicon layer (33); Optionally, the doping concentration of the first doped particles included in the light conversion layer (31) is consistent with the doping concentration of the doped particles included in the crystalline silicon substrate (10); Optionally, the doping concentration of the second doped particles included in the light conversion layer (31) is 20 ppm to 5 × 10⁻⁶. 5 ppm; Optionally, the doping concentration of the second doped particles in the light conversion layer (31) increases from the side closer to the light absorption layer (20) to the side farther away from the light absorption layer (20). Optionally, the thickness of the light conversion layer (31) is 0.3 μm to 0.5 μm; Optionally, in the light conversion layer (31), the content of the sensitizer ions and the activator ions is both 0.05 ppm to 10 ppm. 4 ppm; Optionally, the thickness of the first intrinsic amorphous silicon layer (32) is 4 nm to 6 nm; Optionally, the thickness of the first doped non-polycrystalline silicon layer (33) is 6 nm to 8 nm.

4. The solar cell according to claim 3, characterized in that, The molar ratio between the sensitizer ions and the activator ions in the optical conversion and carrier transport structure (30) is 0.1:1 to 3:1; And / or, The sensitizer ions include at least one of terbium ions, cerium ions, gadolinium ions, and praseodymium ions; The activator ions include europium ions and / or ytterbium ions; Optionally, at least one of the terbium ion, cerium ion and gadolinium ion may coordinate with the europium ion, and / or the praseodymium ion may coordinate with the ytterbium ion.

5. The solar cell according to any one of claims 1, 2, and 4, characterized in that, Also includes: A carrier collection layer (50) is disposed on the second main surface of the crystalline silicon substrate (10), and the conductivity type of the carrier collection layer (50) is the same as that of the crystalline silicon substrate (10). and a second electrode (60) disposed on the side of the carrier collection layer (50) away from the crystalline silicon substrate (10), the second electrode (60) being electrically connected to the carrier collection layer (50); Optionally, the carrier collection layer (50) is a doped diffusion layer containing a fifth doped particle, the conductivity type of which is the same as that of the crystalline silicon substrate (10); or, the carrier collection layer (50) includes a first passivation layer (51) stacked from the inside to the outside and a doped polycrystalline silicon layer (52) containing a fifth doped particle, the conductivity type of which is the same as that of the crystalline silicon substrate (10); or, the carrier collection layer (50) includes a second intrinsic amorphous silicon layer stacked from the inside to the outside and a second doped non-polycrystalline silicon layer containing a fifth doped particle, the conductivity type of which is the same as that of the crystalline silicon substrate (10).

6. The solar cell according to claim 5, characterized in that, The conductivity type of the crystalline silicon substrate (10) is n-type, the conductivity type of the light conversion and carrier transport structure (30) is p-type, and the conductivity type of the carrier collection layer (50) is n-type. Optionally, the crystalline silicon substrate (10) is further doped with a second doped particle, the second doped particle being germanium and / or tin, wherein the content of the second doped particle in the crystalline silicon substrate (10) is 0.01ppm to 10ppm.

7. The solar cell according to claim 3, characterized in that, The optical conversion and carrier transport structure (30) includes a structure in which the fourth doped particle is doped in single-crystal silicon. The solar cell further includes a passivation antireflection layer (70) disposed on the side of the light conversion and carrier transport structure (30) away from the light absorption layer (20).

8. A method for preparing a solar cell, characterized in that, include: Step S1: Provide an initial crystalline silicon substrate (10'); Step S2: A light absorption layer (20) and a light conversion and carrier transport structure (30) are sequentially stacked on the first main surface of the initial crystalline silicon substrate (10'). The portion of the initial crystalline silicon substrate (10') excluding the light absorption layer (20) and the light conversion and carrier transport structure (30) forms the crystalline silicon substrate (10). The conductivity type of the light conversion and carrier transport structure (30) is opposite to that of the crystalline silicon substrate (10). Step S3: Form a first electrode (40) on the optical conversion and carrier transport structure (30) and electrically connect it to the optical conversion and carrier transport structure (30).

9. The preparation method according to claim 8, characterized in that, Step S2 includes: Step S21: Ion implant second doped particles into the initial silicon substrate (10') to a first depth from the first main surface of the initial silicon substrate (10'), wherein the portion of the initial silicon substrate (10') not implanted with the second doped particles is the silicon substrate (10). Step S22: Ion implant sensitizer ions and activator ions of the rare earth system into the initial silicon substrate (10') at a second depth from the first main surface of the initial silicon substrate (10'), and anneal the substrate, wherein the second depth is less than the first depth, and the portion of the initial silicon substrate (10') located between the first depth and the second depth is formed as the light absorption layer (20). Step S23: Based on the intermediate product obtained in step S22, prepare the optical conversion and carrier transport structure (30).

10. The preparation method according to claim 9, characterized in that, Step S23 includes: diffusing a fourth doped particle with a conductivity type opposite to that of the initial silicon substrate (10') from the first main surface of the initial silicon substrate (10'), wherein the third depth of the diffusion of the fourth doped particle is less than the second depth, and the portion of the initial silicon substrate (10') between the first main surface and the second depth forms the light conversion and carrier transport structure (30). or, In the intermediate product obtained in step S22, the implantation range of the sensitizer ions and the activator ions constitutes the light conversion layer (31); step S23 includes: on the light conversion layer (31), a first intrinsic amorphous silicon layer (32) and a first doped non-polycrystalline silicon layer (33) are sequentially stacked, wherein the first doped non-polycrystalline silicon layer (33) contains a fourth doped microparticle with a conductivity type opposite to that of the crystalline silicon substrate (10).