Solar cells, multi-junction solar cells, solar cell modules and solar power systems
By repairing Cu defects on the surface of the cuprous oxide light-absorbing layer and adjusting the carrier concentration using specific elements, the efficiency problem caused by Cu defects was solved, and the photoelectric conversion performance of the solar cell was improved.
Patent Information
- Application Number
- CN202610670948.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2026-04-27
- Filing Date
- 2026-05-15
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, Cu defects in the light-absorbing layer of cuprous oxide-based solar cells lead to uneven carrier concentration, affecting cell efficiency and conversion efficiency.
By repairing Cu defects on the surface of the cuprous oxide light-absorbing layer, elements such as Zn, Mg, Li, Na, K, Rb, Cs, Be, Ca, Sr and Ba are used to repair Cu defects and adjust the carrier concentration to ensure the light transmittance of the light-absorbing layer and the continuity of the conduction band.
This improved the fill factor (FF) and conversion efficiency of the solar cell, reduced the surface resistance, and enhanced the photoelectric conversion performance of the light absorption layer.
Smart Images

Figure CN123124453A_ABST
Abstract
Description
Citation of relevant applications
[0001] This application is based on Japanese Patent Application 2025-0821851 (filed on May 15, 2025) and Japanese Patent Application 2026-073593 (filed on April 27, 2026), and enjoys priority from those applications. This application incorporates the entire contents of those applications by reference. Technical Field
[0002] This invention relates to solar cells, multijunction solar cells, solar cell modules, and solar power generation systems. Background Technology
[0003] As one type of new solar cell, there is a solar cell that uses cuprous oxide (Cu2O) as the light-absorbing layer. Cu2O is a wide-bandgap semiconductor. Because Cu2O is a safe and inexpensive material composed of copper and oxygen, which are abundant on Earth, it is expected to enable high-efficiency and low-cost solar cells. Summary of the Invention
[0004] The implementation provides high-performance solar cells, multi-junction solar cells, solar cell modules, and solar power generation systems.
[0005] The solar cell of the embodiment includes: a first electrode, a p-type light-absorbing layer on the first electrode, an n-type layer on the p-type light-absorbing layer, and a second electrode on the n-type layer. When measuring the photoluminescence spectrum of the p-type light-absorbing layer at a temperature below 100K, a first region is defined as the area extending from the surface of the p-type light-absorbing layer on the n-type layer side toward the first electrode side to a depth of 100nm, and a second region is defined as the area extending from the center of the p-type light-absorbing layer in the thickness direction toward the first electrode side to a depth of 100nm. The highest value of the luminescence intensity in the wavelength region of the first region ranging from 900nm to 950nm is 0 to 2 times the highest value of the luminescence intensity in the wavelength region of the second region ranging from 900nm to 950nm.
[0006] Based on the above configuration, an excellent solar cell can be provided. Attached Figure Description
[0007] Figure 1 This is a schematic cross-sectional view of the solar cell according to the embodiment.
[0008] Figure 2 This is a diagram illustrating the analysis points of a solar cell in an embodiment.
[0009] Figure 3 This is a schematic cross-sectional view of the solar cell according to the embodiment.
[0010] Figure 4 This is a flowchart of a method for manufacturing a solar cell according to an embodiment.
[0011] Figure 5 This is a schematic cross-sectional view of the solar cell according to the embodiment.
[0012] Figure 6 This is a schematic cross-sectional view of a multi-junction solar cell according to an embodiment.
[0013] Figure 7 This is a three-dimensional schematic diagram of the solar cell module according to the implementation method.
[0014] Figure 8 This is a three-dimensional schematic diagram of the solar cell module according to the implementation method.
[0015] Figure 9 This is a structural diagram of a solar power generation system according to an implementation method.
[0016] Figure 10 This is a schematic diagram of the vehicle used in the implementation method.
[0017] Figure 11 This is a schematic diagram of the drone used in the implementation method.
[0018] Figure 12 This is a schematic diagram of the electrolysis apparatus according to the embodiment.
[0019] Figure 13 This is a table relating to the embodiments.
[0020] Figure 14 This is the photoluminescence spectrum of the embodiment.
[0021] Figure 15 This is the photoluminescence spectrum of the embodiment.
[0022] Figure 16 This is a table relating to the embodiments.
[0023] Figure 17 This is a table relating to the embodiments.
[0024] Figure 18 This is a cross-sectional SEM image of the p-type light-absorbing layer.
[0025] Figure 19 This is a table relating to the embodiments.
[0026] Figure 20 This is a table relating to the embodiments.
[0027] Figure 21 This is a table relating to the embodiments.
[0028] Figure 22 This is a table relating to the embodiments.
[0029] Figure 23 This is a table relating to the embodiments.
[0030] Figure 24 This is a table relating to the embodiments.
[0031] Figure 25 This is a table relating to the embodiments.
[0032] Explanation of reference numerals in the attached figures 1: Substrate 2: First electrode 3: p-type light absorption layer 3a: First area 3b: Second Area 3c: Third Region 3D: Fourth Region 3e: Fifth District 3f: Area Six 3G: Region Seven 3h: Area 8 3i: Depression 4: n-type layer 4A: First n-type layer 4B: Second n-type layer 5: Second electrode 100: Solar cells 110: Solar cells 120: Solar cell 200: Multijunction Solar Cell 201: Second solar cell 300: Solar cell module 301: First solar cell module 302: Second solar cell module 310: Solar cell module 400: Solar power generation system 401: Solar cell module 402: Converter 403: Storage battery 404: Overload 500: Vehicles 501: Vehicle body 502: Solar cell module 503: Power conversion device 504: Storage battery 505: Motor 506: Wheels 600: Drone 601: Solar cell module 602: Machine frame 603: Motor 604: Rotating blade 605: Control Unit 700: Electrolysis apparatus 701: Anode 702: Cathode 703: Diaphragm 704: Anode Rectifier Plate 705: Cathode rectifier plate 706: Power conversion device 707: Solar cell module. Detailed Implementation
[0033] Hereinafter, a preferred embodiment of the present invention will be described in detail with reference to the accompanying drawings. It should be noted that, unless otherwise specified, the values refer to physical property values at 25°C and 1 atmosphere (atmosphere). Furthermore, "average" refers to the arithmetic mean. "Each concentration" refers to the average concentration of the target region or layer. In each layer, "containing a specific element" means, for example, an element confirmed to be present by SIMS (Secondary Ion Mass Spectrometry), while "not containing a specific element" means, for example, an element that cannot be confirmed to be present by secondary ion mass spectrometry (SIMS).
[0034] In the instruction manual, " / " represents the division symbol. However, the " / " in "and / or" refers to "or". The instruction manual also uses "•" and "...". The dot "" indicates the multiplication symbol. In the instruction manual, the period "." represents the decimal point.
[0035] The thickness and structure of the components described in the specification can be obtained, for example, from images of the cross-section obtained using scanning electron microscopy (SEM), transmission electron microscopy (TEM), high-angle Annular DarkField Scanning Transmission Electron Microscopy (HAADF-STEM). Furthermore, the boundaries of the components described in the specification can be determined from images obtained by scanning electron microscopy or transmission electron microscopy, measurements taken by scanning electron microscopy with energy dispersive X-ray spectroscopy (SEM-EDS) or transmission electron microscopy with energy dispersive X-ray spectroscopy (TEM-EDX), or secondary ion mass spectrometry analysis. Furthermore, the composition of the components described in the specification can be determined using secondary ion mass spectrometry, inductively coupled plasma mass spectrometry (ICP-MS), scanning electron microscopy with energy-dispersive X-ray spectrometry (EDX-S), or transmission electron microscopy with EDH-S. Additionally, the crystallinity of the components described in the specification can be evaluated using images obtained through X-ray diffraction (XRD), electron backscatter diffraction (EBSD), or high-angle annular dark-field scanning transmission electron microscopy, scanning electron microscopy, or transmission electron microscopy. The materials contained in the components described in the specification (crystal defects, bonding states, etc.) can be evaluated using high-angle annular dark-field scanning transmission electron microscopy, photoluminescence (PL), or X-ray photoelectron spectrophotometry (XPS). These analytical methods are examples and do not negate the specific analytical methods described in the specification.
[0036] (First Implementation) The first embodiment relates to a solar cell. Figure 1 A schematic cross-sectional view of the solar cell 100 according to the first embodiment is shown in the figure. Figure 1The solar cell 100 shown has a substrate 1, a first electrode 2, a p-type light-absorbing layer 3, an n-type layer 4, and a second electrode 5. Preferably, an anti-reflection layer is provided on the light-incident side of the solar cell 100, for example, on the second electrode 5.
[0037] When the first electrode 2 and the second electrode 5 are transmissive electrodes, the solar cell 100 of the embodiment is a transmissive solar cell with high transmittance of light in the wavelength band of 700 nm or higher and 1200 nm or lower.
[0038] In the case of a transmission-type solar cell in which the first electrode 2 and the second electrode 5 are transmission-type electrodes, the solar cell 100 of the embodiment is preferably used on the top cell side (light incident side).
[0039] Substrate 1 is a transparent substrate. Substrate 1 can be made of light-transmitting acrylic resin, polyimide, polycarbonate, polyethylene terephthalate (PET), polypropylene (PP), fluorine-based resins (polytetrafluoroethylene (PTFE), perfluoroethylene propylene copolymer (FEP), ethylene tetrafluoroethylene copolymer (ETFE), polychlorotrifluoroethylene (PCTFE), perfluoroalkoxyalkane (PFA), etc.), polyarylate, polysulfone, polyethersulfone, or polyetherimide, or inorganic substrates such as soda-lime glass, white glass, chemically strengthened glass, or quartz. Substrate 1 can also be made by laminating the substrates listed above.
[0040] Substrate 1 is preferably made of soda-lime glass, white glass, chemically strengthened glass, or quartz, and more preferably of soda-lime glass, white glass, or quartz. Substrate 1 can be omitted.
[0041] The first electrode 2 is disposed on the substrate 1 and is a planar conductive film. The first electrode 2 is a metal layer, an oxide conductive layer, or a transparent conductive layer. Preferably, the first electrode 2 comprises one or more layers of oxide transparent conductive films. As an oxide transparent conductive film, semiconductor conductive films such as indium tin oxide (ITO), aluminum-doped zinc oxide (AZO), boron-doped zinc oxide (BZO), gallium-doped zinc oxide (GZO), doped tin oxide, titanium-doped indium oxide (ITiO), indium zinc oxide (IZO), indium gallium zinc oxide (IGZO), and hydrogen-doped indium oxide (IOH) can be used, without particular limitation. The oxide transparent conductive film can also be a stacked film having multiple films. As a dopant in films such as tin oxide, there is no particular limitation as long as it is selected from one or more elements chosen from the group consisting of In, Si, Ge, Ti, Cu, Sb, Nb, Ta, W, Mo, F, and Cl. The first electrode 2 preferably comprises a tin oxide film doped with one or more elements selected from the group consisting of In, Si, Ge, Ti, Cu, Sb, Nb, Ta, W, Mo, F, and Cl. In the doped tin oxide film, the element selected from the group consisting of In, Si, Ge, Ti, Cu, Sb, Nb, Ta, W, Mo, F, and Cl preferably comprises 10 atomic% or less relative to the tin contained in the tin oxide film. The first electrode 2 can be a laminated film formed by stacking an oxide transparent conductive film and a metal film. The metal (including alloys) contained in the metal film is not particularly limited to Mo, Au, Cu, Ag, Al, Ta, W, etc. Furthermore, the first electrode 2 preferably includes a dot-shaped, line-shaped, or mesh-shaped electrode (selected from one or more of metals, alloys, graphene, conductive nitrides, and conductive oxides) between the oxide transparent conductive film and the substrate 1. The dot-shaped, line-shaped, or mesh-shaped metal preferably has an aperture ratio of 50% or more relative to the oxide transparent conductive film. The dot-shaped, line-shaped, or mesh-shaped metal is Mo, Au, Cu, Ag, Al, Ta, or W, etc., and is not particularly limited. When a metal film is used in the first electrode 2, from the viewpoint of transmissivity, a film thickness of about 5 nm or less is preferably set. When a line-shaped or mesh-shaped metal film is used, since transmissivity is ensured by the openings, the film thickness of the metal film is not limited thereto.
[0042] Specific examples of the first electrode 2 include a transparent electrode made of an ITO film, and a transparent electrode with a tin oxide film formed by a laminate of an ITO film and a doped tin oxide film located on the side of the p-type light absorption layer 3.
[0043] The thickness of the first electrode 2 is preferably 50 nm or more and 500 nm or less, more preferably 50 nm or more and 300 nm or less, and even more preferably 75 nm or more and 200 nm or less.
[0044] The solar cell 100 may also include an intermediate layer between the substrate 1 and the first electrode 2, which includes an insulating layer with a low refractive index such as SiO2 or MgF2.
[0045] The solar cell 100 may include an intermediate layer between the p-type light-absorbing layer 3 and the n-type layer 4.
[0046] The p-type light-absorbing layer 3 is generally a p-type semiconductor layer. The p-type light-absorbing layer 3 is disposed on the first electrode 2. Preferably, the p-type light-absorbing layer 3 is in direct contact with the first electrode 2. The p-type light-absorbing layer 3 is disposed between the first electrode 2 and the n-type layer 4. Preferably, the p-type light-absorbing layer 3 is in direct contact with the n-type layer 4. The p-type light-absorbing layer 3 in direct contact with the n-type layer 4 is preferably pn-bonded with the n-type layer 4. The p-type light-absorbing layer 3 is preferably a compound semiconductor layer. Preferably, the p-type light-absorbing layer 3 is a semiconductor layer containing a compound with a cuprous oxide structure, such as cuprous oxide. The p-type light-absorbing layer 3 is preferably mainly composed of a cuprous oxide compound. The cuprous oxide compound preferably has a cuprous oxide structure. Hereinafter, an example will be described using a solar cell containing a cuprous oxide compound in the p-type light-absorbing layer 3. When using other compounds in a solar cell with a p-type light-absorbing layer 3, it is preferable to adopt a configuration suitable for the solar cell 100 of the first embodiment and the respective compounds.
[0047] The p-type light-absorbing layer 3 is preferably a semiconductor layer containing a cuprous oxide compound. The p-type light-absorbing layer 3 is preferably a grain boundary of the cuprous oxide compound. In the p-type light-absorbing layer 3, as part of the impurities, one or more cuprous oxide impurities selected from the group consisting of copper (Cu), copper oxide (CuO) and copper hydroxide (Cu(OH)2) may also be included in trace amounts.
[0048] When all elements except oxygen contained in the p-type light absorption layer 3 are set to 100%, the copper content in the p-type light absorption layer 3 is preferably 90% or more and 100% or less, preferably 95% or more and 100% or less, more preferably 98% or more and 100% or less, and even more preferably 99% or more and 100% or less.
[0049] When all elements except oxygen in the p-type light absorption layer 3 are set to 100%, the copper content in the p-type light absorption layer 3 is preferably 90% or more and 99.9% or less, preferably 95.0% or more and 99.9% or less, more preferably 98% or more and 99.9% or less, and even more preferably 99.0% or more and 99.9% or less.
[0050] The cuprous oxide compound contains copper and oxygen, and optionally contains an element represented by M1. The element represented by M1 is preferably one or more elements selected from the group consisting of Cl, F, Br, I, Sn, Sb, Ag, Li, Na, K, Cs, Rb, Al, In, Zn, Mg, Ga, Si, Ge, N, P, B, Ti, Hf, Zr, Be, Ca, Sr, and Ba.
[0051] If the number of copper atoms is set to 1, the number of oxygen atoms in the cuprous oxide compound is preferably 0.48 or more and 0.56 or less. If there is more oxygen relative to copper, the proportion of copper oxide in the cuprous oxide compound becomes higher, resulting in a narrower band gap and reduced light transmittance of the p-type light absorption layer 3, which is not preferred. If there is less oxygen relative to copper, the proportion of copper in the cuprous oxide compound becomes higher, resulting in reduced light transmittance, which is also not preferred. Furthermore, when the oxygen-to-copper ratio does not meet the above range, the cuprous oxide compound becomes less likely to have a cuprite-type structure.
[0052] Preferably, 95% to 100% of the p-type light-absorbing layer 3 is a cuprous oxide compound, more preferably 98% to 100% of the p-type light-absorbing layer 3 is a cuprous oxide compound, and even more preferably 99% to 100% of the p-type light-absorbing layer 3 is a cuprous oxide compound. 100% of the p-type light-absorbing layer 3 may be composed of a cuprous oxide compound.
[0053] When the p-type light-absorbing layer 3 contains few heterogeneous phases and has good crystallinity, the light transmittance of the p-type light-absorbing layer 3 becomes higher, which is therefore preferred. The band gap of the p-type light-absorbing layer 3 can be adjusted by including elements other than Cu and O in the p-type light-absorbing layer 3. The band gap of the p-type light-absorbing layer 3 is preferably 2.0 eV or higher and 2.2 eV or lower. If the band gap is within this range, in a multi-junction solar cell where Si is used in the light-absorbing layer for the bottom unit and the solar cell of the embodiment is used in the top unit, sunlight can be efficiently utilized in both the top and bottom units. The p-type light-absorbing layer 3 preferably contains Sn and / or Sb. The Sn or Sb in the p-type light-absorbing layer 3 can be Sn or Sb added to the p-type light-absorbing layer 3, or Sn or Sb derived from the first electrode 2. The Ga contained in the p-type light-absorbing layer 3 is not included in the raw material for forming the p-type light-absorbing layer 3, but rather is Ga diffused from the n-type layer 4 into the p-type light-absorbing layer 3. When other elements are used during the formation of the n-type layer 4, these elements sometimes diffuse into the p-type light-absorbing layer 3. Additionally, there are cases where elements diffuse from the intermediate layer (not shown) into the p-type light-absorbing layer 3.
[0054] The composition ratio of the p-type light-absorbing layer 3 described above is the overall composition ratio of the p-type light-absorbing layer 3. Furthermore, the compound composition ratio of the p-type light-absorbing layer 3 described above is preferably satisfied overall within the p-type light-absorbing layer 3.
[0055] The p-type light-absorbing layer 3 preferably has a p-type light-absorbing layer on the side of the first electrode 2. + Type of area.
[0056] The p-type light-absorbing layer 3 is preferably located on the side of the n-type layer 4. - Type of area.
[0057] The p-type light-absorbing layer 3 is preferably located on the side of the n-type layer 4. - Type region, having p on the first electrode 2 side + Type of area.
[0058] The thickness of the p-type light-absorbing layer 3 is preferably 2 μm or more and 10 μm or less, more preferably 2.5 μm or more and 7.0 μm or less. The p-type light-absorbing layer 3 is preferably the thickest layer among the layers included between the first electrode 2 and the second electrode 5. The p-type light-absorbing layer 3 is preferably the thickest among the semiconductor layers included in the solar cell 100.
[0059] The thickness of the p-type light-absorbing layer 3 is not limited to the above-mentioned thickness when Cu2O is epitaxially grown or when the copper plate is oxidized. When Cu2O is epitaxially grown, the thickness of the p-type light-absorbing layer 3 is preferably 0.2 μm or more and 3 μm or less. When the copper plate is oxidized, the thickness of the p-type light-absorbing layer 3 is preferably 100 μm or more and 1 mm or less.
[0060] Preferably, the surface of the p-type light-absorbing layer 3 on the n-type layer 4 side has fine irregularities. The average deviation of the surface roughness on the n-type layer 4 side of the p-type light-absorbing layer 3 is preferably 50 nm or more, more preferably 50 nm or more and 500 nm or less, and even more preferably 55 nm or more and 300 nm or less.
[0061] The p-type light-absorbing layer 3 is preferably formed by, for example, sputtering. Specifically, it is preferable to heat the component on which the first electrode 2 is formed on the substrate 1 to 300°C or higher and 1000°C or lower, and to perform the deposition within a range of 0.02 μm / min or higher and 20 μm / min or lower, where the oxygen partial pressure is 0.01 Pa or higher and 4.8 Pa or lower. From the viewpoint of forming a polycrystalline film with high transmittance and large particle size, when the deposition rate is set to d μm / min (wherein, the unit of deposition rate is ignored in the calculation of oxygen partial pressure), the oxygen partial pressure is more preferably satisfied to be 0.20 × d Pa or higher and 1.00 × d Pa or lower (for example, in the case of high-temperature sputtering, it is preferably 0.20 × d Pa or higher and 0.50 × d Pa or lower, and in the case of low-temperature sputtering, it is preferably 0.55 × d Pa or higher and 1.00 × d Pa or lower). Furthermore, the heating temperature is more preferably higher than 550°C and lower than 850°C. Element M1 can be added to the film.
[0062] By forming the p-type light-absorbing layer 3 using the above method, a large-particle-size cuprous oxide compound is formed. The p-type light-absorbing layer 3 is preferably a polycrystalline form containing cuprous oxide compound crystals with a particle size that is at least 5 times the thickness of the p-type light-absorbing layer 3.
[0063] The p-type light-absorbing layer 3 can be a Cu2O layer formed by epitaxial growth. When the p-type light-absorbing layer 3 is epitaxially grown, Cu2O can be grown using the first electrode 2 or an intermediate layer disposed on the first electrode 2 as a substrate.
[0064] The p-type light-absorbing layer 3 can also be a Cu2O layer obtained by oxidizing a Cu plate.
[0065] If Cu defects exist in the p-type light-absorbing layer 3, the carrier concentration will increase. However, at the pn interface, the increased carrier concentration leads to a decrease in the p-type light-absorbing layer 3 on the n-type layer 4 side. +The p-type light-absorbing layer 3 is locally high on the n-type layer 4 side, leading to increased conduction band discontinuity. This n-type layer 4 side becomes a barrier to carrier movement, resulting in increased recombination. Therefore, the locally high carrier concentration on the n-type layer 4 side of the p-type light-absorbing layer 3 contributes to reduced flyback factor (FF) and conversion efficiency. The characteristics of the solar cell 100 can be improved by repairing Cu defects.
[0066] In the case of cuprous oxide compounds, if Cu defects are located on the crystal surface and the p-type light-absorbing layer 3 is polycrystalline, Cu defects may sometimes be relatively abundant on the crystal surface and at grain boundaries. For example, in the case of cuprous oxide compounds formed by Cu oxidation, Cu defects are not limited to the center of the crystal; Cu defects tend to move towards the crystal surface.
[0067] In this invention, Cu defects on the surface of the p-type light-absorbing layer 3 are evaluated by photoluminescence analysis, thereby enabling the acquisition of a laminate (a laminate of substrate 1, first electrode 2 and p-type light-absorbing layer 3) or solar cell 100 having a p-type light-absorbing layer 3 with effectively reduced Cu defects on the n-type layer 4 side.
[0068] When the photoluminescence spectrum of the p-type light-absorbing layer 3 is measured at a temperature below 100 K (hereinafter, all luminescence intensities are luminescence intensities measured by photoluminescence at a temperature below 100 K), without a reduction in Cu defects, when measuring the surface of the p-type light-absorbing layer 3 on the side opposite to the first electrode 2 side (n-type layer 4 side), the luminescence intensity in the wavelength region (first wavelength region) ranging from 900 nm to 950 nm becomes higher. Since the luminescence intensity of the first wavelength region on the first electrode 2 side or the main body of the p-type light-absorbing layer 3 is low, the luminescence intensity of the first wavelength region is relatively higher on the side of the p-type light-absorbing layer 3 opposite to the first electrode 2 side.
[0069] If the luminescence intensity in the first wavelength region is low in the range from the surface of the p-type light-absorbing layer 3 on the n-type layer 4 side towards the first electrode 2 to a depth of 100 [nm], i.e., in the first region 3a, then the FF (FF=(Vmpp) of the solar cell 100) is low. Jmpp) / (Voc Improving Jsc)) helps to improve conversion efficiency.
[0070] The luminescence in the first wavelength region is considered to originate from Cu defects, while the luminescence intensity in the wavelength region above 600 nm and below 650 nm (the second wavelength region) is attributed to undefected Cu₂O. The band gap energy corresponding to the second wavelength region is approximately 2.0 eV, and the band gap energy corresponding to the first wavelength region is approximately 1.3 eV.
[0071] As with the p-type light-absorbing layer 3 of the solar cell in this embodiment, if all Cu defects are not repaired, no emission in the first wavelength region is observed inside the p-type light-absorbing layer 3 during photoluminescence analysis. Even when emission is substantially only observed in the second wavelength region, emission in the first wavelength region is still detected on the surface of the p-type light-absorbing layer 3. Whether it is a poor-quality Cu₂O p-type light-absorbing layer 3 with a large CuO phase or a p-type light-absorbing layer 3 that is considered to be a single Cu₂O phase, Cu defects exist on the surface of the p-type light-absorbing layer 3 (the surface opposite to the first electrode 2 side). When repairing the Cu defects in the poor-quality Cu₂O p-type light-absorbing layer 3 with a large CuO phase, Cu defect repair can be performed on the entire p-type light-absorbing layer 3. However, when repairing the Cu defects in the p-type light-absorbing layer 3 not only on the film surface but also on the entire layer, the overall carrier concentration of the p-type light-absorbing layer 3 decreases, which is not preferable. From this perspective, it is preferable to perform the process on a component in which a p-type light absorption layer 3 is formed and the Cu defect is locally present on the surface of the p-type light absorption layer 3 before the Cu defect is repaired.
[0072] By repairing the Cu defects on the surface of the p-type light-absorbing layer 3, the luminescence in the first wavelength region of the surface of the p-type light-absorbing layer 3 is reduced, thus achieving the same level of luminescence as the first wavelength region of the main body p-type light-absorbing layer 3. The second region 3b is defined as the area extending from the center of the p-type light-absorbing layer 3 in the thickness direction (the direction from the surface on the first electrode 2 side towards the surface on the opposite side is the thickness direction of the p-type light-absorbing layer 3) towards the first electrode 2 side to a depth of 100 [nm]. Taking the second region 3b as the main body, the highest value of the luminescence intensity in the first wavelength region of the first region 3a is preferably 0 times (or greater than 0 times) and less than 2 times the highest value of the luminescence intensity in the first wavelength region of the second region 3b, more preferably 0 times (or greater than 0 times) and less than 1 times, and even more preferably 0 times (or greater than 0 times) and less than 0.5 times.
[0073] From the viewpoint of improving FF, ([the highest value of luminous intensity in the first wavelength region of the first region 3a] × [the highest value of luminous intensity in the second wavelength region of the second region]) / ([the highest value of luminous intensity in the second wavelength region of the first region 3a] × [the highest value of luminous intensity in the first wavelength region of the second region 3b]) is preferably 0 or more (or greater than 0) and 20 or less, more preferably 0 or more (or greater than 0) and 3.3 or less, and even more preferably 0 or more (or greater than 0) and 0.5 or less. If the Cu defect is not repaired, then ([the highest value of luminous intensity in the first wavelength region of the first region 3a] × [the highest value of luminous intensity in the second wavelength region of the second region 3b]) / ([the highest value of luminous intensity in the second wavelength region of the first region 3a] × [the highest value of luminous intensity in the first wavelength region of the second region 3b]) becomes a value larger than the above range.
[0074] The element used to repair Cu defects is preferably one or more of the first element selected from Zn, Mg, Li, Na, K, Rb, Cs, Be, Ca, Sr, and Ba, or / and Cu. The element for repairing Cu defects is preferably locally present on the surface of the p-type light-absorbing layer 3 opposite to the first electrode 2. The region containing the element for repairing Cu defects tends to have a lower carrier concentration. It is preferable that the carrier concentration is lower on the side of the p-type light-absorbing layer 3 opposite to the first electrode 2, but it is not preferable that the overall carrier concentration of the p-type light-absorbing layer 3 is lower. It is considered that even if the p-type light-absorbing layer 3 contains the element for repairing Cu defects, the carrier concentration will still be lower even if the Cu defects can be repaired.
[0075] When the p-type light-absorbing layer 3 is a polycrystalline form of cuprous oxide compound, it is preferable that the grain boundaries in the first region 3a contain an element for repairing Cu defects. When the p-type light-absorbing layer 3 is a polycrystalline form of cuprous oxide compound, it is preferable that the grain boundaries in the first region 3a contain a first element.
[0076] Cu is the preferred element for repairing Cu defects. When using Cu as the element for repairing Cu defects, the number of oxygen atoms contained in the cuprous oxide compound in the entire p-type light-absorbing layer 3 and the first region 3a is preferably 0.48 or more and 0.56 or less when the number of copper atoms is set to 1.
[0077] The preferred element for repairing Cu defects is Zn, and more preferably a combination of Zn and Cu.
[0078] The preferred element for repairing Cu defects is Mg, preferably Mg and Cu, and preferably Zn, Mg and Cu.
[0079] The preferred element for repairing Cu defects is Ca, preferably Ca and Cu, and preferably Zn, Ca and Cu.
[0080] The first element for repairing Cu defects is preferably one or more selected from Zn, Mg, Li, Na and Ca, and more preferably Zn, Mg and Ca.
[0081] If the continuity of the conduction band is taken into consideration, when the third region 3c is defined as the range from the surface of the p-type light absorption layer 3 opposite to the side of the first electrode 2 toward the side of the first electrode 2 to a depth of 1 [μm], the concentration of the first element contained in the third region 3c is preferably 90 [atomic%] or more and 100 [atomic%] or less of the first element contained in the p-type light absorption layer 3.
[0082] Considering factors such as the continuity of the conduction band, when the fourth region 3d is defined as a depth of 50 nm from the surface of the p-type light-absorbing layer 3 opposite to the side of the first electrode 2 towards the side of the first electrode 2, the concentration of the first element contained in the fourth region 3d is preferably 30 atomic percent or more and 80 atomic percent or less of the first element contained in the p-type light-absorbing layer 3. Rather than containing approximately all of the first element in the fourth region 3d, the first element is contained in a region closer to the side of the first electrode 2 than in the fourth region 3d. To reliably repair Cu defects on the surface, it is preferable that the first element is present in a region wider than the fourth region 3d.
[0083] If the continuity of the conduction band is taken into consideration, when the fifth region 3e is defined as the range from the surface of the p-type light absorption layer 3 opposite to the side of the first electrode 2 toward the side of the first electrode 2 to a depth of 0.7 [μm], the concentration of the first element contained in the fifth region 3e is preferably 90 [atomic%] or more and 100 [atomic%] or less of the first element contained in the p-type light absorption layer 3.
[0084] If the continuity of the conduction band is taken into consideration, when the range from the surface of the p-type light absorption layer 3 opposite to the side of the first electrode 2 toward the side of the first electrode 2 to a depth of 0.6 [μm] is defined as the sixth region 3f, the concentration of the first element contained in the sixth region 3f is preferably 90 [atomic%] or more and 100 [atomic%] or less of the first element contained in the p-type light absorption layer 3.
[0085] If the continuity of the conduction band is taken into consideration, when the range from the surface of the p-type light absorption layer 3 opposite to the side of the first electrode 2 toward the side of the first electrode 2 up to 30% of the thickness H of the p-type light absorption layer 3 is defined as the seventh region 3g, the concentration of the first element contained in the seventh region 3g is preferably 90% or more and 100% or less of the first element contained in the p-type light absorption layer 3.
[0086] If the continuity of the conduction band is taken into consideration, when the depth range from the surface of the p-type light absorption layer 3 opposite to the side of the first electrode 2 toward the side of the first electrode 2 up to 20% of the thickness H of the p-type light absorption layer 3 is defined as the eighth region 3h, the concentration of the first element contained in the eighth region 3h is preferably 90% or more and 100% or less of the first element contained in the p-type light absorption layer 3.
[0087] In the thickness direction of the p-type light-absorbing layer 3, the surface resistivity of the first region 3a of the cross-section of the solar cell 100 is [Ω / cm]. 2 The surface resistivity of the second region 3b of the preferred cross-section is [Ω / cm]. 2 The resistivity is more than 0.3 times and less than 10,000 times, more preferably more than 1 times and less than 10,000 times, and even more preferably more than 10 times and less than 10,000 times. Regions with Cu defects tend to have low resistance. If regions with Cu defects exist, carrier recombination may occur, leading to a decrease in current density. In this embodiment, the solar cell 100 has high overall resistance because the Cu defects on the side of the p-type light-absorbing layer 3 opposite to the first electrode 2 are reduced. The surface resistivity is determined by scanning extended resistance microscopy (SSRM).
[0088] The preferred carrier concentration in the first region 3a is 1×10⁻⁶. 11 [cm -3 Above and 1×10 15 [cm -3 Below, 1×10 is more preferred. 11 [cm -3 ] and above and 3×10 14 [cm -3 The following is further preferred: 1×10 11 [cm -3 Above and 1×10 14 [cm -3 [The following is an example.] If the Cu defect is not repaired, the carrier concentration in the first region 3a can easily become, for example, 3 × 10⁻⁶. 15 [cm -3 The carrier concentration is determined by using device simulation (e.g., e-ARC method) to determine the current-voltage characteristics of the solar cell.
[0089] The preferred carrier concentration in the second region 3b is 1×10⁻⁶. 12 [cm -3 Above and 1×10 15 [cm -3 Below, 1×10 is more preferred. 13 [cm -3 ] and above 7.5×10 14[cm -3 The following is further preferred: 1×10 14 [cm -3 ] and above and 5×10 14 [cm -3 [The following is a continuation of the previous statement.] Even when the Cu defects are not repaired, the carrier concentration in the second region 3b tends to satisfy the aforementioned range. If a large amount of elements for repairing Cu defects are present up to the second region 3b, the overall carrier concentration of the p-type light-absorbing layer 3 decreases. Therefore, the carrier concentration of the main body (second region 3b) preferably satisfies the aforementioned range.
[0090] The carrier concentration in the first region 3a is preferably 0.0001 times or more and 3 times or less than the carrier concentration in the second region 3b, more preferably 0.0001 times or more and 1 time or less, and even more preferably 0.0001 times or more and 0.3 times or less. If the Cu defect is not repaired, the carrier concentration in the first region 3a is likely to be 3 times or more than the carrier concentration in the second region 3b.
[0091] Regarding the element for repairing Cu defects, it is sufficient to deposit the element for repairing Cu defects on the surface of the p-type light-absorbing layer 3 after the p-type light-absorbing layer 3 is formed. If the first element is added during the formation of the p-type light-absorbing layer 3, the first element diffuses throughout the p-type light-absorbing layer 3, resulting in Cu defects as described above. Therefore, if the first element and / or the element represented by M1 are added during the formation of the p-type light-absorbing layer 3, it is also possible to deposit the element for repairing Cu defects on the surface of the p-type light-absorbing layer 3 after the formation of the p-type light-absorbing layer 3 to obtain the solar cell 100.
[0092] Regarding the repair of Cu defects described above, a more specific example is shown below. After forming a layer mainly composed of cuprous oxide compound (50 wt% or more, preferably 90 wt% or more, more preferably 95 wt% or more, and even more preferably 98 wt% or more of cuprous oxide compound) by sputtering or the like, the element for repairing Cu defects is deposited on the surface of the cuprous oxide compound-based layer and diffuses. Deposition is preferably performed directly on the surface of the cuprous oxide compound-based layer. The element for repairing Cu defects diffuses into the cuprous oxide compound-based layer by deposition of the cuprous oxide compound containing Cu defects and heating above room temperature (25 °C) and below the sputtering temperature mentioned under sputtering conditions. The preferred temperature for the diffusion of the element for repairing Cu defects is the temperature at which a small excess of the element for repairing Cu defects is deposited, the temperature at which the PL emission in the first wavelength region of the first region 3a identified on the surface of the cuprous oxide compound-based layer before Cu defect repair is reduced, or the temperature at which the carrier concentration of the main component changes before and after Cu defect repair. The preferred processing temperature range can be determined by this phenomenon. An appropriate temperature range is determined through multiple experiments. Regarding the deposition amount of Cu defect repair elements when repairing Cu defects at this temperature (temperature range), multiple experiments are conducted to gradually reduce the deposition amount, and the carrier concentration on the host side is evaluated. Preferably, the conditions under which Cu defect repair elements are not over-deposited are investigated according to the type of Cu defect repair element, thereby achieving a balance between repairing the target Cu defect and suppressing the decrease in carrier concentration on the host side. The preferred processing time is also determined similarly. Alternatively, after Cu defect repair, an oxidation process can be performed on an extremely thin region (e.g., a region narrower than the first region 3a) of the surface of the p-type light-absorbing layer 3.
[0093] The n-type layer 4 is an n-type semiconductor layer that transmits visible light. The n-type layer 4 is disposed between the p-type light-absorbing layer 3 and the second electrode 5. The n-type layer 4 is preferably disposed on the p-type light-absorbing layer 3. The n-type layer 4 is formed, for example, by the ALD method. The n-type layer 4 is primarily amorphous, but may also contain a portion of crystalline material.
[0094] The n-type layer 4 preferably comprises a compound (oxide) mainly composed of Ga and a compound (oxide) mainly composed of Zn. In the case that the n-type layer 4 is a multilayer n-type layer, the semiconductor layer comprising a compound (oxide) mainly composed of Ga or a compound (oxide) mainly composed of Zn is preferably in direct contact with the p-type light-absorbing layer 3.
[0095] The thickness of the n-type layer 4 is typically 3 nm or more and 100 nm or less. If the thickness of the n-type layer 4 is less than 3 nm, leakage current will occur due to poor coverage of the n-type layer 4, which may sometimes degrade the characteristics. The film thickness is not limited to the above when the coverage is good. If the thickness of the n-type layer 4 exceeds 50 nm, the characteristics may be degraded due to excessive high resistivity of the n-type layer 4, or the short-circuit current may be reduced due to reduced transmittance. Therefore, the thickness of the n-type layer 4 is more preferably 3 nm or more and 20 nm or less, and even more preferably 5 nm or more and 20 nm or less.
[0096] Compounds with Ga as the main component preferably contain Ga₂O₃ or are oxides containing the element represented by M₂ and Ga. Oxides with Ga as the main component are preferably, for example, those with an average composition of Ga. h1 M2 i1 O j1 The oxide represented by M2. h1, i1, and j2 preferably satisfy 1.8 ≤ h1 ≤ 2.1, 0.0 ≤ i1 ≤ 0.2, and 2.9 ≤ j1 ≤ 3.1. It is an oxide containing the element represented by M2 and Ga. M2 is preferably selected from one or more elements chosen from the group consisting of H, Sn, Sb, Cu, Ag, Li, Na, K, Cs, Rb, Al, In, Zn, Mg, Si, Ge, N, B, Ti, Hf, Zr, Ca, Ce, La, Pr, and Nd. The first layer preferably contains an average composition of 90% to 100% or less Ga. h1 M2 i1 O j1 The oxide is represented.
[0097] The second electrode 5 is disposed on the n-type layer 4. When the second electrode 5 side is the light incident side, the second electrode 5 is an electrode that is transparent to visible light. For the second electrode 5, an oxide transparent conductive film is preferably used. The oxide transparent conductive film used in the second electrode 5 is preferably one or more semiconductor conductive films selected from the group consisting of indium tin oxide, doped tin oxide, aluminum-doped zinc oxide, boron-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, titanium-doped indium oxide, indium gallium zinc oxide, and hydrogen-doped indium oxide. As for the dopant in the tin oxide film, it is not particularly limited as long as it is one or more selected from the group consisting of In, Si, Ge, Ti, Cu, Sb, Nb, Ta, W, Mo, F, and Cl. To reduce the resistance of the oxide transparent conductive film, the second electrode 5 may include a mesh or wire-shaped electrode. For the mesh or wire-shaped electrode, it is not particularly limited to Mo, Au, Cu, Ag, Al, Ta, or W. Graphene may also be used for the second electrode 5. Graphene is preferably stacked with silver nanowires.
[0098] The thickness of the second electrode 5 was determined by cross-sectional observation using an electron microscope and by using a height difference meter.
[0099] The thickness of the second electrode 5 is 30 nm or more and 2 μm or less, more preferably 30 nm or more and 100 nm or less, and even more preferably 30 nm or more and 70 nm or less.
[0100] The second electrode 5 is preferably formed by, for example, ALD, sputtering, etc.
[0101] The compositional analysis of the p-type light-absorbing layer 3, for example, was performed using methods such as SEM-EDX (Scanning Electron Microscopy-Energy Dispersive X-ray Spectroscopy) and TEM-EDX (Transmission Electron Microscopy-Energy Dispersive X-ray Spectroscopy). Figure 2 The analysis points are obtained by analyzing points (A1~A9) that are distributed at equal intervals and as close to no gaps as possible, as shown in the diagram. Figure 2 This is a schematic diagram of the solar cell 100 as observed from the second electrode 5 side. In analyzing the composition of the solar cell 100, D1 is the length of the solar cell 100 in the width direction (long side direction), and D2 is the length of the solar cell 100 in the depth direction (short side direction). By magnifying the image at 2 million times using TEM, the composition can be determined by analyzing a 100 nm × 100 nm region encompassing the center of each analytical point. Furthermore, by analyzing the center of each analytical point in the thickness direction of the solar cell 100 using XPS, the chemical bonding state can be evaluated, and the compounds of elements contained in each layer can be determined. Additionally, by observing the solar cell 100 from the second electrode 5 side using a scanning electron microscope or similar instrument, the surface irregularities and the particle size of each layer can be analyzed.
[0102] (Second Implementation) The second embodiment relates to a solar cell and a method for manufacturing a solar cell. The solar cell of the second embodiment is an example of a solar cell having the p-type light-absorbing layer 3 of the first embodiment with the Cu defect repaired.
[0103] Figure 3This is a schematic cross-sectional view showing the solar cell 110 according to the second embodiment. The solar cell 110 of the second embodiment has a substrate 1, a first electrode 2, a p-type light-absorbing layer 3, an n-type layer 4, and a second electrode 5. Preferably, an anti-reflection layer is provided on the light-incident side of the solar cell 100, for example, on the second electrode 5. A recess 3i is present on the surface of the p-type light-absorbing layer 3 on the n-type layer 4 side.
[0104] In the second embodiment, the substrate 1, the first electrode 2, the n-type layer 4, and the second electrode 5 are common to those in the first embodiment. In the second embodiment, the description of the substrate 1, the first electrode 2, the n-type layer 4, and the second electrode 5 is omitted.
[0105] The p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 is an overall p-type semiconductor layer. The p-type light-absorbing layer 3 is disposed on the first electrode 2. A thin layer of Cu is deposited on the cuprous oxide compound-based layer, allowing Cu to diffuse into the cuprous oxide compound-based layer, thereby obtaining the p-type light-absorbing layer 3. The p-type light-absorbing layer 3 is preferably in direct contact with the first electrode 2. The p-type light-absorbing layer 3 is disposed between the first electrode 2 and the n-type layer 4. The p-type light-absorbing layer 3 is preferably in direct contact with the n-type layer 4. The p-type light-absorbing layer 3 in direct contact with the n-type layer 4 is preferably pn-bonded with the n-type layer 4. The p-type light-absorbing layer 3 is preferably a compound semiconductor layer. The p-type light-absorbing layer 3 is preferably a semiconductor layer containing a compound with a cuprous oxide-type structure, such as cuprous oxide. The p-type light-absorbing layer 3 is preferably mainly composed of a cuprous oxide compound. The cuprous oxide compound preferably has a cuprous oxide-type structure. Hereinafter, an example of a solar cell using a compound containing a cuprous oxide compound in the p-type light-absorbing layer 3 will be described. In the case of using other compounds in the solar cell of the p-type light-absorbing layer 3, it is preferable to adopt the configuration of the solar cell 110 and the respective compounds that are suitable for the second embodiment.
[0106] The p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 is preferably a semiconductor layer containing cuprous oxide compound. The p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 is preferably a polycrystalline cuprous oxide compound. In the p-type light-absorbing layer 3, as part of the impurities, it may also contain trace amounts of one or more cuprous oxide impurities selected from the group consisting of copper (Cu), copper oxide (CuO), and copper hydroxide (Cu(OH)2).
[0107] When all elements except oxygen in the p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 are set to 100%, the copper content in the p-type light-absorbing layer 3 is preferably 90% or more and 100% or less, preferably 95% or more and 100% or less, more preferably 98% or more and 100% or less, and even more preferably 99% or more and 100% or less.
[0108] When all elements except oxygen in the p-type light-absorbing layer (layer mainly composed of cuprous oxide compound) 3 are set to 100%, the copper content in the p-type light-absorbing layer (layer mainly composed of cuprous oxide compound) 3 is preferably 90% or more and 99.9% or less, preferably 95.0% or more and 99.9% or less, more preferably 98% or more and 99.9% or less, and even more preferably 99.0% or more and 99.9% or less.
[0109] The cuprous oxide compound contains copper and oxygen, and optionally contains an element represented by M1. The element represented by M1 is preferably one or more elements selected from the group consisting of Cl, F, Br, I, Sn, Sb, Ag, Li, Na, K, Cs, Rb, Al, In, Zn, Mg, Ga, Si, Ge, N, P, B, Ti, Hf, Zr, Be, Ca, Sr, and Ba.
[0110] If the number of copper atoms is set to 1, the number of oxygen atoms in the cuprous oxide compound is preferably 0.48 or more and 0.56 or less. If there is more oxygen relative to copper, the proportion of copper oxide in the cuprous oxide compound becomes higher, resulting in a narrower band gap and reduced light transmittance of the p-type light absorption layer 3, which is therefore undesirable. If there is less oxygen relative to copper, the proportion of copper in the cuprous oxide compound becomes higher, resulting in reduced light transmittance, which is also undesirable. Furthermore, when the oxygen-to-copper ratio does not meet the above range, the cuprous oxide compound becomes less likely to have a cuprite-type structure.
[0111] Preferably, 95% to 100% of the p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 is cuprous oxide compound; more preferably, 98% to 100% of the p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 is cuprous oxide compound; and even more preferably, 99% to 100% of the p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 is cuprous oxide compound. 100% of the p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 may be composed of cuprous oxide compound.
[0112] When the p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 contains few heterogeneous phases and has good crystallinity, the light transmittance of the p-type light-absorbing layer 3 becomes higher, which is therefore preferable. The band gap of the p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 can be adjusted by including elements other than Cu and O in the p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound). The band gap of the p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 is preferably 2.0 eV or higher and 2.2 eV or lower. If the band gap is within this range, in a multi-junction solar cell where Si is used in the light-absorbing layer for the bottom unit and the solar cell of the embodiment is used in the top unit, sunlight can be efficiently utilized in both the top and bottom units. The p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 preferably contains Sn and / or Sb. Sn and Sb in the p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 can be added to the p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3, or they can originate from the first electrode 2. The Ga contained in the p-type light-absorbing layer 3 is not included in the raw materials used to form the p-type light-absorbing layer 3, but rather diffuses from the Ga contained in the n-type layer 4 into the p-type light-absorbing layer 3. When other elements are used during the formation of the n-type layer 4, these elements sometimes also diffuse into the p-type light-absorbing layer 3. Additionally, there are cases where elements diffuse from the intermediate layer (not shown) into the p-type light-absorbing layer 3.
[0113] The composition ratio of the aforementioned p-type light-absorbing layer (the layer mainly composed of cuprous oxide compound) 3 is the overall composition ratio of the p-type light-absorbing layer (the layer mainly composed of cuprous oxide compound) 3. Furthermore, the compound composition ratio of the aforementioned p-type light-absorbing layer (the layer mainly composed of cuprous oxide compound) 3 is preferably satisfied in all of the p-type light-absorbing layer (the layer mainly composed of cuprous oxide compound) 3.
[0114] The p-type light-absorbing layer (a layer mainly composed of cuprous oxide compounds) 3 preferably has p-type light-absorbing layers on the side of the first electrode 2. + Type of area.
[0115] The p-type light-absorbing layer (a layer mainly composed of cuprous oxide compounds) 3 preferably has p-type light-absorbing layers on the n-type layer 4 side. - Type region, having p on the first electrode 2 side + Type of area.
[0116] The thickness of the p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 is preferably 2 μm or more and 10 μm or less, more preferably 2.5 μm or more and 7.0 μm or less. The p-type light-absorbing layer 3 is preferably the thickest layer among the layers included between the first electrode 2 and the second electrode 5. The p-type light-absorbing layer 3 is preferably the thickest among the semiconductor layers included in the solar cell 100.
[0117] Preferably, the surface of the p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 on the n-type layer 4 side has fine irregularities. The average deviation of the surface roughness on the n-type layer 4 side of the p-type light-absorbing layer (a layer mainly composed of cuprous oxide compound) 3 is preferably 50 nm or more, more preferably 50 nm or more and 500 nm or less, and even more preferably 55 nm or more and 300 nm or less. The fine irregularities are generated during the crystal growth of the cuprous oxide compound, and therefore already exist before Cu is deposited on the layer mainly composed of cuprous oxide compound.
[0118] The layer primarily composed of cuprous oxide compounds is preferably formed by methods such as sputtering. Specifically, it is preferable to heat the component on which the first electrode 2 is formed on the substrate 1 to 300°C or higher and 1000°C or lower, and to perform the deposition within a range of 0.02 μm / min or higher and 20 μm / min or lower, where the oxygen partial pressure is 0.01 Pa or higher and 4.8 Pa or lower. From the viewpoint of forming a polycrystalline film with high permeability and large particle size, when the deposition rate is set as d (wherein the unit of deposition rate is ignored in the calculation of oxygen partial pressure), the oxygen partial pressure is more preferably satisfied to be 0.20 × d Pa or higher and 1.00 × d Pa or lower (for example, in the case of high-temperature sputtering, it is preferably 0.20 × d Pa or higher and 0.50 × d Pa or lower, and in the case of low-temperature sputtering, it is preferably 0.55 × d Pa or higher and 1.00 × d Pa or lower). Furthermore, the heating temperature is more preferably higher than 550°C and lower than 850°C. Element M1 can be added to the film.
[0119] By forming a film of cuprous oxide compound using the above method, a layer is formed mainly composed of large-particle-size cuprous oxide compound. The p-type light-absorbing layer (the layer mainly composed of cuprous oxide compound) 3 is preferably a polycrystalline material containing cuprous oxide compound crystals with a particle size at least 5 times the thickness of the p-type light-absorbing layer (the layer mainly composed of cuprous oxide compound) 3.
[0120] If Cu defects exist in the p-type light-absorbing layer 3, the carrier concentration will increase. However, at the pn interface, the increased carrier concentration leads to a decrease in the p-type light-absorbing layer 3's p-type layer 4 side. + The p-type light-absorbing layer 3 is locally high on the n-type layer 4 side, leading to increased conduction band discontinuity. This n-type layer 4 side becomes a barrier to carrier movement, resulting in increased recombination. Therefore, the locally high carrier concentration on the n-type layer 4 side of the p-type light-absorbing layer 3 is a cause of reduced flyback factor (FF) and conversion efficiency. The characteristics of the solar cell 110 can be improved by repairing Cu defects.
[0121] When the p-type light-absorbing layer 3 is a polycrystalline form of cuprous oxide compound, it is preferable that the grain boundaries contained in the first region 3a (a range extending from the surface of the p-type light-absorbing layer 3 on the n-type layer 4 side towards the first electrode 2 to a depth of 100 [nm]) contain an element for repairing Cu defects. When the p-type light-absorbing layer 3 is a polycrystalline form of cuprous oxide compound, it is preferable that the grain boundaries contained in the first region 3a contain a first element.
[0122] Cu is the preferred element for repairing Cu defects. When using Cu as the element for repairing Cu defects, the number of oxygen atoms contained in the cuprous oxide compound in the entire p-type light-absorbing layer 3 and the first region 3a is preferably 0.48 or more and 0.56 or less when the number of copper atoms is set to 1.
[0123] The preferred carrier concentration in the first region 3a is 1×10⁻⁶. 11 [cm -3 Above and 1×10 15 [cm -3 Below, 1×10 is more preferred. 11 [cm -3 ] and above and 3×10 14 [cm -3 The following is further preferred: 1×10 11 [cm -3 Above and 1×10 14 [cm -3 [The following is an example.] If the Cu defect is not repaired, the carrier concentration in the first region 3a can easily become, for example, 3 × 10⁻⁶. 15 [cm -3 The carrier concentration is determined by using device simulation (e.g., e-ARC method) to determine the current-voltage characteristics of the solar cell.
[0124] The preferred carrier concentration in the second region 3b is 1×10⁻⁶. 12 [cm -3 Above and 1×10 15 [cm -3 Below, 1×10 is more preferred. 13 [cm -3 ] and above 7.5×10 14 [cm -3 The following is further preferred: 1×10 14 [cm -3 ] and above and 5×10 14 [cm -3[The following is a continuation of the previous statement.] Even when the Cu defects are not repaired, the carrier concentration in the second region 3b tends to satisfy the aforementioned range. If a large amount of elements for repairing Cu defects are present up to the second region 3b, the overall carrier concentration of the p-type light-absorbing layer 3 decreases. Therefore, the carrier concentration of the main body (second region 3b) preferably satisfies the aforementioned range.
[0125] The carrier concentration in the first region 3a is preferably 0.0001 times or more and 3 times or less than the carrier concentration in the second region 3b, more preferably 0.0001 times or more and 1 time or less, and even more preferably 0.0001 times or more and 0.3 times or less. If the Cu defect is not repaired, the carrier concentration in the first region 3a is likely to be 3 times or more than the carrier concentration in the second region 3b.
[0126] In the second embodiment, Cu defects in the cuprous oxide compound are repaired using Cu. The layer formed by sputtering, primarily composed of polycrystalline cuprous oxide compound, has high crystal quality; therefore, even before Cu defect repair, the number of Cu defect sites is small, making it difficult to evaluate Cu defect repair based on the Cu-to-oxygen ratio. Regarding Cu defects on the surface of the p-type light-absorbing layer 3, it is preferable to evaluate them using PL intensity, as in the first embodiment. The p-type light-absorbing layer 3 of the second embodiment also preferably satisfies the photoluminescence spectrum characteristics of the first embodiment.
[0127] Thinly deposited Cu adheres to the surface of the cuprous oxide-dominated layer and diffuses into its interior. This layer, where the thinly deposited Cu diffuses into the cuprous oxide-dominated layer, is the p-type light-absorbing layer 3. In other words, the cuprous oxide-dominated layer is the precursor to the p-type light-absorbing layer 3. If the thinly deposited Cu remains in its Cu state, it becomes a Cu-precipitated state. If the precipitated Cu exists between the p-type light-absorbing layer 3 and the n-type layer 4, the FF (field-effect) of the solar cell 110 decreases compared to a solar cell without compensated Cu defects, resulting in a lower conversion efficiency.
[0128] If a thin Cu film is deposited on a layer mainly composed of polycrystalline cuprous oxide compound by sputtering to the extent that Cu does not precipitate, small depressions 3i are generated on the surface of the p-type light-absorbing layer 3. The depressions 3i are different from grooves extending in the surface direction such as grain boundaries on the surface of the p-type light-absorbing layer 3 that exist before the deposition of the thin Cu, and shapes that bulge from the grain boundaries on the crystalline surface towards the center of the crystal (the surface roughness of the first embodiment), and are dot-like depressions.
[0129] The average depth of the recess 3i (the length of the first electrode 2 and the p-type light absorption layer 3 in the stacking direction) is 10 nm or more and 80 nm or less, 20 nm or more and 70 nm or less, or 30 nm or more and 60 nm or less.
[0130] The maximum diameter of the 3i depression is 15nm or more and 80nm or less, 20nm or more and 70nm or less, or 30nm or more and 60nm or less.
[0131] The minimum diameter of the depression 3i is 10 nm or more. The maximum diameter of the depression 3i is 1 to 5 times, 1 to 3 times, or 1.1 times to 3 times the minimum diameter of the depression 3i. In addition, the depth of the depression 3i is 1 to 3 times, or 1.1 times to 3 times the minimum diameter of the depression 3i.
[0132] Furthermore, the diameter of the recess 3i is the length of the opening surface (inner side of the edge of the recess 3i) of the recess 3i on the surface side of the p-type light absorption layer 3.
[0133] The density of the 3i depressions is 1 or more and less than 250, 10 or more and less than 200, or 15 or more and less than 100 within a 500nm×500nm square area.
[0134] The depression 3i is not present in the layer mainly composed of cuprous oxide compounds, but in the p-type light-absorbing layer 3.
[0135] like Figure 4 As shown in the flowchart, the manufacturing method of the solar cell 110 according to the embodiment includes the following steps: The process of forming a layer mainly composed of cuprous oxide compound on the first electrode 2 by sputtering; After the formation of a cuprous oxide-based layer, Cu is deposited on the surface of the cuprous oxide-based layer opposite to the first electrode 2 (the surface forming the n-type layer 4) to obtain the p-type light-absorbing layer 3. The process of forming an n-type layer 4 on the surface of a p-type light-absorbing layer 3 deposited with Cu; and The process of forming the second electrode 5 on the n-type layer 4.
[0136] A layer primarily composed of cuprous oxide compound is formed on the first electrode 2 using the sputtering method described in the first embodiment. The first electrode 2 is disposed on the substrate 1. The p-type light-absorbing layer (a layer primarily composed of cuprous oxide compound) 3 formed by sputtering is polycrystalline.
[0137] Cu is formed on the surface opposite to the first electrode 2 of a layer mainly composed of cuprous oxide compound. The preferred method for depositing Cu is sputtering or CVD, with sputtering being more preferred.
[0138] The amount of Cu deposited on the copper oxide-based layer is preferably very small. The average thickness of Cu deposited on the cuprous oxide-based layer is preferably 0.02 nm or more and 0.08 nm or less, more preferably 0.02 nm or more and 0.07 nm or less.
[0139] Since the amount of Cu deposited is minute, it is possible to calculate, for example, the conditions for depositing Cu of a specific measurable thickness on a glass plate, and to deposit Cu with an average thickness of 0.02 nm or more and 0.07 nm or less based on the calculated conditions.
[0140] If a large amount of Cu is deposited (the average thickness of Cu is high), depression 3i will not form, and Cu will easily precipitate. Therefore, it is preferable to satisfy the above-mentioned average Cu thickness. If Cu precipitates, the FF of the solar cell 110 will be lower than when Cu is not deposited, and the conversion efficiency will decrease.
[0141] Even if the amount of deposited Cu is very small (the average thickness of Cu is thinner than the range described above), Cu diffuses into the cuprous oxide-dominated layer, but the FF is the same as when no Cu is deposited. Therefore, it is preferable to satisfy the average thickness condition described above.
[0142] The Cu deposited on the cuprous oxide-based layer is preferably formed on the surface of the heated cuprous oxide-based layer. The surface temperature (or stage temperature) of the cuprous oxide-based layer during Cu deposition is preferably 100°C or higher and 350°C or lower, more preferably 150°C or higher and 300°C or lower, and even more preferably 180°C or higher and 270°C or lower.
[0143] When the temperature for Cu deposition is too high, Cu tends to agglomerate during deposition, making it difficult for it to diffuse into the interior of the cuprous oxide-dominated layer. If it is difficult to diffuse into the interior of the cuprous oxide-dominated layer, Cu tends to precipitate. Therefore, it is preferable to satisfy the above-mentioned temperature range.
[0144] If the Cu deposition temperature is too low, Cu will not diffuse into the interior of the cuprous oxide-dominated layer, but will remain precipitated on the surface. In this case, the Cu defects in the first region 3a of the cuprous oxide-dominated layer are difficult to repair, and Cu, as a heterogeneous phase of the cuprous oxide compound, remains on the surface of the cuprous oxide-dominated layer. Therefore, the conversion efficiency decreases as the flow rate (FF) decreases. Therefore, except for the case where post-heating of the cuprous oxide-dominated layer is performed within the above-mentioned temperature range after Cu deposition, it is preferable to satisfy the above-mentioned conditions related to the surface temperature of the cuprous oxide-dominated layer during Cu deposition.
[0145] It is believed that the depression 3i is formed during the process of Cu adhering to the surface of the cuprous oxide compound-dominated layer and diffusing into the interior of the cuprous oxide compound-dominated layer.
[0146] Cu deposition is preferably carried out in a non-oxidizing atmosphere. Such a non-oxidizing atmosphere may include, for example, nitrogen or argon.
[0147] The oxidation process can also be performed after sputtering of the cuprous oxide compound and before Cu deposition. The oxidation process oxidizes a very thin region of the surface of the film formed by sputtering. The oxidation conditions for the oxidation process are preferably any of the first to fourth conditions described below.
[0148] (first condition) In the oxidation process, the oxygen partial pressure is above 5000 Pa and below 200000 Pa, and the water vapor concentration is 9.4 × 10⁻⁶. -1 [g / m 3 ] and above 2.5×10 3 [g / m 3 The processing temperature is 40°C or higher and 150°C or lower, and the processing time is 5 seconds or higher and 150 minutes or lower. The atmosphere (gas) for oxidation treatment contains oxygen. The atmosphere for oxidation treatment under the first, second, and fourth conditions may contain ozone with an oxygen partial pressure (or oxygen concentration) of 0.0% or higher and 0.1% or lower (maximum 1 Pa or lower). In addition to oxygen, the atmosphere for oxidation treatment may also contain substances that are unavoidably mixed in with the atmosphere, such as carbon monoxide, carbon dioxide, hydrocarbons, and hydrogen. For example, the presence of substances such as carbon monoxide, carbon dioxide, hydrocarbons, and hydrogen that are unavoidably mixed in with the atmosphere in the atmosphere is 5000 ppm or lower. The atmosphere for oxidation treatment may further contain inactive gases such as nitrogen and argon, and hydrogen. The atmosphere for oxidation treatment does not substantially contain oxidizing reactive gases other than oxygen and ozone; therefore, reactive gases other than oxygen and ozone are not introduced into the oxidation treatment chamber. Therefore, it is preferable to introduce only oxygen and any ozone and / or inactive gases into chamber 21. The sum of the partial pressure of oxygen and the partial pressure of inactive gases in the total pressure of the gas after removing water vapor from the oxidizing atmosphere (=([partial pressure of oxygen] + [partial pressure of inactive gases]) / (total pressure of the gas after removing water vapor from the oxidizing atmosphere)) is preferably 99.0% or more and 100% or less, more preferably 99.3% or more and 100% or less (or 99.3% or more and 99.9% or less). Several preferred first conditions are described below.
[0149] In the oxidation process, the water vapor concentration was 9.4 × 10⁻⁶. -1 [g / m 3 ] and above 2.5×103 [g / m 3 The following describes the conditions for oxidation treatment: treatment time ≥ 10 seconds and < 5 minutes, treatment temperature ≥ 40°C and < 110°C, and oxygen partial pressure ≥ 50000 Pa and < 100000 Pa; treatment time ≥ 10 seconds and < 5 minutes, treatment temperature ≥ 110°C and < 150°C, and oxygen partial pressure ≥ 15000 Pa and < 50000 Pa; treatment time ≥ 5 minutes and < 10 minutes, treatment temperature ≥ 40°C and < 80°C, and oxygen partial pressure ≥ 15000 Pa and < 10000 Pa. The following conditions are also applicable: 1. Treatment time of 10 minutes or more but less than 60 minutes, treatment temperature of 40°C or more but less than 80°C, and oxygen partial pressure of 15000 Pa or more but less than 40000 Pa; 2. Treatment time of 60 minutes or more but less than 90 minutes, treatment temperature of 40°C or more but less than 120°C, and oxygen partial pressure of 15000 Pa or more but less than 35000 Pa; 3. Treatment time of 90 minutes or more but less than 150 minutes, treatment temperature of 40°C or more but less than 60°C, and oxygen partial pressure of 5000 Pa or more but less than 21000 Pa.
[0150] In the oxidation treatment, the oxygen partial pressure is above 5000 Pa and below 50000 Pa, the treatment temperature is above 50 °C and below 150 °C, the treatment time is above 5 minutes and below 60 minutes, and the water vapor concentration is 9.4 × 10⁻⁶. -1 [g / m 3 ] and above 2.5×10 1 [g / m 3 ]the following.
[0151] In the oxidation treatment, the treatment temperature is above 75°C and below 125°C, the oxygen partial pressure is above 5000 Pa and below 100000 Pa, the treatment time is above 5 minutes and below 45 minutes, and the water vapor concentration is 9.4 × 10⁻⁶. -1 [g / m 3 ] and above 2.5×10 1 [g / m 3 ]the following.
[0152] The treatment temperature is above 80°C and below 120°C, the oxygen partial pressure is above 5000 Pa and below 100000 Pa, the treatment time is above 10 minutes and below 45 minutes, and the water vapor concentration is 9.4 × 10⁻⁶. -1 [g / m 3] and above 2.5×10 1 [g / m 3 ]the following.
[0153] The following conditions apply: processing time of 10 seconds or more but less than 5 minutes, processing temperature of 110°C or more but less than 150°C, and oxygen partial pressure of 15,000 Pa or more but less than 50,000 Pa; processing time of 5 minutes or more but less than 10 minutes, processing temperature of 40°C or more but less than 80°C, and oxygen partial pressure of 15,000 Pa or more but less than 100,000 Pa; processing time of 10 minutes or more but less than 60 minutes, processing temperature of 40°C or more but less than 80°C, and oxygen partial pressure of 15,000 Pa or more but less than 40,000 Pa; and processing time of 90 minutes or more but less than 150 minutes, processing temperature of 40°C or more but less than 60°C, and oxygen partial pressure of 5,000 Pa or more but less than 21,000 Pa.
[0154] (Second condition) In the oxidation treatment, the oxygen partial pressure is 100 Pa or higher and less than 5000 Pa; the treatment temperature is 100°C or higher and less than 300°C; and the treatment time is 1 second or higher and less than 90 minutes. Several preferred second conditions are described below.
[0155] In the oxidation process, the oxygen partial pressure is above 100 Pa and below 5000 Pa, the processing temperature is above 125 °C and below 250 °C, and the processing time is above 1 second and below 90 minutes.
[0156] In the oxidation process, the oxygen partial pressure is above 300 Pa and below 2000 Pa, the processing temperature is above 180 °C and below 250 °C, and the processing time is above 5 seconds and below 45 minutes.
[0157] In the oxidation process, the oxygen partial pressure is above 500 Pa and below 2000 Pa, the processing temperature is above 180 °C and below 250 °C, and the processing time is above 1 minute and below 30 minutes.
[0158] In the oxidation process, the oxygen partial pressure is above 100 Pa and below 2000 Pa, the processing temperature is above 250 °C and below 300 °C, and the processing time is above 1 minute and below 10 minutes.
[0159] In the oxidation process, the oxygen partial pressure is above 1000 Pa and below 5000 Pa, the treatment temperature is above 200 °C and below 250 °C, and the treatment time is above 1 minute and below 10 minutes.
[0160] In the oxidation process, the oxygen partial pressure is above 1000 Pa and below 5000 Pa, the treatment temperature is above 100 °C and below 250 °C, and the treatment time is above 10 minutes and below 60 minutes.
[0161] In the oxidation process, the oxygen partial pressure is above 500 Pa and below 5000 Pa, the treatment temperature is above 100 °C and below 175 °C, and the treatment time is above 10 minutes and below 30 minutes.
[0162] In the oxidation process, the oxygen partial pressure is above 300 Pa and below 1500 Pa, the treatment temperature is above 150 °C and below 200 °C, and the treatment time is above 10 minutes and below 30 minutes.
[0163] In the oxidation process, the oxygen partial pressure is above 1000 Pa and below 5000 Pa, the treatment temperature is above 100 °C and below 150 °C, and the treatment time is longer than 60 minutes and less than 90 minutes.
[0164] (Third condition) In the oxidation process, the ozone partial pressure is 5 Pa or higher and 200 Pa or lower; the oxidation temperature is 273 K or higher and 323 K or lower; and the oxidation time is 1 second or higher and 60 minutes or lower. Several preferred third conditions are described below.
[0165] In the oxidation process, the ozone partial pressure is above 7 Pa and below 100 Pa, the treatment temperature is above 283 K and below 308 K, and the treatment time is above 1 minute and below 30 minutes.
[0166] In the oxidation process, the ozone partial pressure is above 10 Pa and below 50 Pa, the treatment temperature is above 283 K and below 308 K, and the treatment time is above 1 minute and below 10 minutes.
[0167] (Fourth condition) In the oxidation treatment, the treatment time is more than 1 hour and less than 1600 hours, and the oxygen concentration is 5.0 × 10⁻⁶. -8 [g / L] or higher and 5.0×10 -5 [g / L] or less. The following describes the preferred fourth condition.
[0168] In the oxidation treatment, the treatment time is more than 1 hour and less than 1600 hours, and the oxygen concentration is 5.0 × 10⁻⁶. -8 [g / L] or higher and 5.0×10 -5Below [g / L], the water vapor concentration is 5.0 × 10⁻⁶. -8 [g / L] or higher and 5.0×10 -5 [g / L] or less, and the temperature is above 0℃ and below 100℃.
[0169] Before and after oxidation treatment, to prevent undesirable oxidation reactions, it is preferable to store the component with the sputtered p-type light-absorbing layer 3. After oxidation treatment, it is preferable to store the oxidized component in an atmosphere with an oxygen partial pressure of 50 Pa or less and 80 °C or less, more preferably 50 °C or less, or to continue the deposition of the n-type layer 4 for solar cell applications. Before the deposition of the n-type layer 4, for example, the component that has undergone oxidation treatment can be stored in an atmospheric atmosphere (the component temperature is the same, and so on) at 30 °C or less for 1 hour or less, preferably 30 minutes or less. Before oxidation treatment, it can be stored in an atmosphere with an oxygen partial pressure of 50 Pa or less and 80 °C or less, more preferably 50 °C or less, or in an atmospheric atmosphere at 30 °C or less for 1 hour or less, preferably 30 minutes or less. In these storage atmospheres, ozone with a partial pressure of 0.1% or less relative to the oxygen partial pressure may be present.
[0170] In these storage atmospheres, the water vapor concentration (mass / volume) is preferably 5.0 × 10⁻⁶. -8 [g / L] or higher and 5.0×10 -5 [g / L] or less, more preferably 5.0 × 10 -8 [g / L] or higher and 4.0×10 -5 Below [g / L].
[0171] In these storage atmospheres, a gas that does not contain plasma is preferred.
[0172] Before Cu deposition or after Cu deposition and diffusion, when cooling is performed on a component with a sputtered p-type light-absorbing layer 3 after sputtering or oxidation treatment, for example, preferably at an oxygen partial pressure of 10. -6 [Pa] and above and 10 4 In atmospheres below [Pa], with -10 3 Cooling is performed at a cooling rate of [K / min] or higher and -0.1 [K / min] or lower. The temperature of the component formed by sputtering a layer mainly composed of cuprous oxide compound onto the cooled substrate (or the temperature of the cooled component) is preferably, for example, -80 [°C] or higher and 250 [°C] or lower.
[0173] Then, an n-type layer 4 is formed on the p-type light-absorbing layer 3, and a second electrode 5 is formed on the n-type layer 4 to obtain a solar cell 110.
[0174] (Third implementation method) The third embodiment relates to a solar cell. Figure 5 A schematic cross-sectional view showing the solar cell 120 of the third embodiment. Figure 5 The solar cell 120 shown has a substrate 1, a first electrode 2, a p-type light-absorbing layer 3, an n-type layer 4 (a first n-type layer 4A and a second n-type layer 4B), and a second electrode 5. Preferably, light is incident from the side of the second electrode 5 in the solar cell 120.
[0175] When the first electrode 2 and the second electrode 5 are transmission-type electrodes, the solar cell 120 of the embodiment is a transmission-type solar cell with high transmittance of light in the wavelength band of 700 [nm] and above and 1200 [nm] and below.
[0176] In the case of a transmission-type solar cell in which the first electrode 2 and the second electrode 5 are transmission-type electrodes, the solar cell 120 of the embodiment is preferably used on the top cell side (light incident side).
[0177] The substrate 1, first electrode 2, and second electrode 5 in the third embodiment are common to those in the first and second embodiments. In the first to third embodiments, common descriptions related to the substrate 1, first electrode 2, and second electrode 5 will be omitted below.
[0178] The solar cell 120 (solar cell 100, solar cell 110) may include an intermediate layer between the substrate 1 and the first electrode 2, the intermediate layer including a low refractive index insulating layer such as SiO2, MgF2, etc.
[0179] The solar cell 120 (solar cell 100, solar cell 110) may include an intermediate layer with a thickness of more than 0.1 nm and less than 50 nm between the first electrode 2 and the p-type light-absorbing layer 3. The intermediate layer contains one or more of SiO2, Na2O, CaO, B2O3, Al2O3, SiN, SiON and MgO and has a non-uniform thickness.
[0180] When the solar cell 120 (solar cell 100, solar cell 110) is a non-transmittent type, the first electrode 2 can also be a metal electrode such as Mo. In the case of a metal electrode, the thickness of the first electrode 2 is not limited to the thickness described above.
[0181] The p-type light-absorbing layer 3 is generally a p-type semiconductor layer. The p-type light-absorbing layer 3 is disposed on the first electrode 2. Preferably, the p-type light-absorbing layer 3 is in direct contact with the first electrode 2. The p-type light-absorbing layer 3 is disposed between the first electrode 2 and the first n-type layer 4A. Preferably, the p-type light-absorbing layer 3 in direct contact with the first n-type layer 4A forms a pn junction with the first n-type layer 4A. The p-type light-absorbing layer 3 is preferably a compound semiconductor layer. Preferably, the p-type light-absorbing layer 3 is a semiconductor layer containing a cuprous oxide compound or a compound having a chalcopyrite-type structure.
[0182] The p-type light-absorbing layer 3 is preferably composed of a cuprous oxide compound. The cuprous oxide compound preferably has a cuprite-type structure such as cuprous oxide (Cu₂O). The p-type light-absorbing layer 3 can be a layer in which a very thin layer of Cu is deposited on a layer composed of a cuprous oxide compound, and Cu diffuses into the interior of the cuprous oxide-based layer.
[0183] The p-type light-absorbing layer 3 is preferably composed mainly of compounds with a chalcopyrite-type structure. Among the compounds with a chalcopyrite-type structure, compounds of the I-III-VI2 series or the I-II-IV-VI4 series are preferred.
[0184] The thickness of the p-type light-absorbing layer 3 is preferably 500 nm or more and 10 μm or less, more preferably 750 nm or more and 7.0 μm or less. The p-type light-absorbing layer 3 is preferably the thickest layer among the layers included between the first electrode 2 and the second electrode 5. The p-type light-absorbing layer 3 is preferably the thickest among the semiconductor layers included in the solar cell 120.
[0185] Preferably, the surface of the p-type light-absorbing layer 3 on the side of the first n-type layer 4A has fine irregularities. The average deviation of the surface roughness on the side of the first n-type layer 4A of the p-type light-absorbing layer 3 is preferably 50 nm or more, more preferably 50 nm or more and 500 nm or less, and even more preferably 55 nm or more and 300 nm or less.
[0186] The band gap of the p-type light-absorbing layer 3 is preferably above 1.5 eV and below 2.3 eV.
[0187] The preferred carrier concentration (hole concentration) of the p-type light-absorbing layer 3 is 1.0 × 10⁻⁶. 13 cm -3 Above and 1.0×10 18 cm -3 Hereinafter, 1.0 × 10 is more preferred. 14 cm -3 Above and 1.0×10 17 cm -3 The following is a further preferred value: 2.0 × 10 14 cm -3 Above and 5.0×1016 cm -3 In cases where the carrier concentration of the p-type light-absorbing layer 3 is relatively low as described above (or, where it is difficult to increase the carrier concentration due to the wide bandgap of the p-type light-absorbing layer 3), increasing any one or more of the open-circuit voltage (Voc), short-circuit current density (Jsc), and fill factor (FF) by setting the first n-type layer 4A helps to improve the conversion efficiency (Eff).
[0188] Preferably, 95% to 100% of the p-type light-absorbing layer 3, which contains a cuprous oxide compound, is a cuprous oxide compound; more preferably, 98% to 100% of the p-type light-absorbing layer 3 is a cuprous oxide compound; and even more preferably, 99% to 100% of the p-type light-absorbing layer 3 is a cuprous oxide compound. 100% of the p-type light-absorbing layer 3 may be composed of a cuprous oxide compound.
[0189] When the p-type light-absorbing layer 3 contains a cuprous oxide compound, the cuprous oxide compound may contain 10% or less, preferably 5% or less, or 1% or less of an additive element. The additive element of the cuprous oxide compound is preferably selected from one or more of Cl, F, Br, I, Sn, Sb, Ag, Li, Na, K, Cs, Rb, Al, In, Zn, Mg, Ga, Si, Ge, N, P, B, Ti, Hf, Zr, and Ca.
[0190] The p-type light-absorbing layer 3 is preferably a semiconductor layer containing a cuprous oxide compound. The p-type light-absorbing layer 3 is preferably a polycrystalline cuprous oxide compound. In the p-type light-absorbing layer 3, as part of the impurities, one or more cuprous oxide impurities selected from the group consisting of copper (Cu), copper oxide (CuO) and copper hydroxide (Cu(OH)2) may also be included in trace amounts.
[0191] If the number of copper atoms is set to 1, the number of oxygen atoms in the cuprous oxide compound is preferably 0.48 or more and 0.56 or less. If there is more oxygen relative to copper, the proportion of copper oxide in the cuprous oxide compound becomes higher, resulting in a narrower band gap and reduced light transmittance of the p-type light absorption layer 3, which is not preferred. If there is less oxygen relative to copper, the proportion of copper in the cuprous oxide compound becomes higher, resulting in reduced light transmittance, which is also not preferred. Furthermore, when the oxygen-to-copper ratio does not meet the above range, the cuprous oxide compound becomes less likely to have a cuprite-type structure.
[0192] When the p-type light-absorbing layer 3 contains a cuprous oxide compound, the p-type light-absorbing layer 3 contains fewer heterogeneous phases and has good crystallinity, resulting in higher light transmittance, which is therefore preferable. By including elements other than Cu and O in the p-type light-absorbing layer 3, the band gap of the p-type light-absorbing layer 3 can be adjusted. The band gap of the p-type light-absorbing layer 3 containing a cuprous oxide compound is preferably 2.0 eV or higher and 2.2 eV or lower. If the band gap is within this range, in a multi-junction solar cell where a Si-based light-absorbing layer is used in the bottom unit and the solar cell of the embodiment is used in the top unit, sunlight can be efficiently utilized in both the top and bottom units.
[0193] The p-type light-absorbing layer 3 preferably contains Sn and / or Sb. Sn and Sb in the p-type light-absorbing layer 3 containing cuprous oxide compounds can be added to the p-type light-absorbing layer 3 or can be derived from the first electrode 2. Elements such as Ga contained in the first n-type layer 4A and the second n-type layer 4B of the p-type light-absorbing layer 3 are not included in the raw materials for forming the p-type light-absorbing layer 3, and these elements diffuse into the p-type light-absorbing layer 3. When other elements are also used in forming the first n-type layer 4A and the second n-type layer 4B, these elements may also diffuse into the p-type light-absorbing layer 3. The carrier concentration in the p-type light-absorbing layer 3 with a large band gap tends to be low, making the first n-type layer 4A in this embodiment more efficient.
[0194] The p-type light-absorbing layer 3 containing cuprous oxide compound is preferably formed by, for example, sputtering. Specifically, it is preferable to heat the component on which the first electrode 2 is formed on the substrate 1 to 300°C or higher and 1000°C or lower, and to perform the deposition at a rate of 0.02 μm / min or higher and 20 μm / min or lower, within a range where the oxygen partial pressure is 0.01 Pa or higher and 4.8 Pa or lower. From the viewpoint of forming a polycrystalline film with high transmittance and large particle size, when the deposition rate is set to d, the oxygen partial pressure is more preferably 0.20 × d Pa or higher and 1.00 × d Pa or lower (for example, in the case of high-temperature sputtering, it is preferably 0.20 × d Pa or higher and 0.50 × d Pa or lower, and in the case of low-temperature sputtering, it is preferably 0.55 × d Pa or higher and 1.00 × d Pa or lower). In addition, the heating temperature is more preferably higher than 550°C and lower than 850°C. M1 can be added to the film.
[0195] By forming the p-type light-absorbing layer 3 using the above method, a large-particle cuprous oxide compound is formed. Preferably, the p-type light-absorbing layer 3 comprises cuprous oxide crystals with a particle size that is more than 5 times the thickness of the p-type light-absorbing layer 3.
[0196] The p-type light-absorbing layer 3 containing a cuprous oxide compound, as a third embodiment, can be either the p-type light-absorbing layer 3 of the first embodiment or the p-type light-absorbing layer 3 of the second embodiment.
[0197] As a compound of the I-III-VI2 system, it is preferably selected from one or more of CuGaSe2, CuGaS2, CuGaTe2, CuInSe2, CuInS2, and CuInTe2. In the case of compounds containing multiple I-III-VI2 systems, it may be represented, for example, as a compound such as Cu(Ga,In)Se2.
[0198] As compounds in the I-II-IV-VI4 system, Cu2ZnSnS4, Cu2ZnSnSe4, or Cu2ZnSn(S,Se)4 are preferred.
[0199] When the p-type light-absorbing layer 3 contains a compound with a chalcopyrite-like structure, it is preferable that 95 wt% to 100 wt% of the p-type light-absorbing layer 3 is a compound with a chalcopyrite-like structure; more preferably, 98 wt% to 100 wt% of the p-type light-absorbing layer 3 is a compound with a chalcopyrite-like structure; and even more preferably, 99 wt% to 100 wt% of the p-type light-absorbing layer 3 is a compound with a chalcopyrite-like structure. The 100 wt% of the p-type light-absorbing layer 3 may be composed of a cuprous oxide compound.
[0200] When the p-type light-absorbing layer 3 contains a compound with a chalcopyrite-like structure, the p-type light-absorbing layer 3 has fewer heterogeneous phases and better crystallinity, resulting in higher light transmittance, which is therefore preferable. By increasing the proportion of Ga and / or increasing the proportion of S in the p-type light-absorbing layer 3, the band gap (BG3) of the p-type light-absorbing layer 3 can be adjusted to be higher. The band gap of the p-type light-absorbing layer 3 containing a compound with a chalcopyrite-like structure is preferably 1.1 eV or more and 2.4 eV or less, more preferably 1.5 eV or more and 2.2 eV or less. If the band gap is within the range described above, in a multi-junction solar cell where the solar cell using Si in the light-absorbing layer is used in the bottom unit and the solar cell of the embodiment is used in the top unit, sunlight can be efficiently utilized in both the top and bottom units.
[0201] Furthermore, when the p-type light-absorbing layer 3 contains compounds with a chalcopyrite-type structure (Ga and S are abundant to very abundant, In and Se are scarce to very scarce), and the p-type light-absorbing layer 3 has a band gap of 1.6 eV or more and 2.4 eV or less, by using the solar cell 120 of the embodiment as the top cell and using the Si solar cell as the top cell, it is possible to efficiently utilize sunlight in both the top and bottom cells. The conventional second n-type layer, which is well-compatible with the p-type light-absorbing layer 3 with its large band gap, is a material with low carrier concentration; therefore, providing the first n-type layer 4A of the embodiment is more effective.
[0202] Compounds with chalcopyrite-type structures are formed on the first electrode 2 by methods such as evaporation, sputtering, nanoparticle printing, and electrodeposition.
[0203] The first n-type layer 4A is an n-type semiconductor layer that transmits visible light. The first n-type layer 4A is disposed between the p-type light-absorbing layer 3 and the second n-type layer 4B. Preferably, the first n-type layer 4A is disposed on the p-type light-absorbing layer 3. Preferably, the first n-type layer 4A is in direct contact with the p-type light-absorbing layer 3. Preferably, the surface of the first n-type layer 4A facing the p-type light-absorbing layer 3 is in direct contact with the p-type light-absorbing layer 3. The first n-type layer 4A and the p-type light-absorbing layer 3 form a pn junction.
[0204] The second n-type layer 4B is an n-type semiconductor layer that transmits visible light. The second n-type layer 4B is disposed between the second n-type layer 4B and the second electrode 5. The second n-type layer 4B is preferably disposed on the first n-type layer 4A. The second n-type layer 4B is preferably in direct contact with the first n-type layer 4A. The surface of the second n-type layer 4B facing the first n-type layer 4A is preferably in direct contact with the first n-type layer 4A. The second n-type layer 4B can be a single layer or a stack of multiple layers with different compositions.
[0205] The band gap BG4 of the first n-type layer 4A is preferably smaller than the band gap BG3 of the p-type light-absorbing layer 3. Considering band alignment, the band gap of the n-type layer including the first n-type layer 4A is preferably larger than the band gap of the p-type light-absorbing layer 3. Through device simulation, it can be seen that using the n-type layer with a larger band gap as the second n-type layer 4B and the n-type layer with a band gap BG4 smaller than that of the p-type light-absorbing layer 3 as the first n-type layer 4A improves the conversion efficiency of the solar cell 120.
[0206] Preferably, the band gap BG4 of the first n-type layer 4A is smaller than the band gap BG3 of the p-type light-absorbing layer 3, and the band gap BG5 of the second n-type layer 4B is larger than the band gap BG4 of the first n-type layer 4A, and the band gap BG5 of the second n-type layer 4B is larger than the band gap BG3 of the p-type light-absorbing layer 3. From the p-type light-absorbing layer 3 to the second n-type layer 4B, the band gap preferably satisfies a relationship of medium, small, and large.
[0207] The first n-type layer 4A, which forms a pn junction with the p-type light absorption layer 3, satisfies the above-mentioned band gap, thus generating a band mismatch. Moreover, according to the band gap relationship, it is expected that surface recombination will increase, but it is known that in device simulation, Jsc actually increases, which helps to improve the conversion efficiency.
[0208] The difference (BG3-BG4) between the band gap BG4 of the first n-type layer 4A and the band gap BG3 of the p-type light-absorbing layer 3 is preferably 0.05 eV or more and 0.60 eV or less, more preferably 0.10 eV or more and 0.55 eV or less, and even more preferably 0.15 eV or more and 0.50 eV or less. If the band gap difference is small, the carrier concentration of the first n-type layer decreases, and the effect of the first n-type layer weakens. If the band gap difference is large, the conduction band shift between the p-type light-absorbing layer 3 and the first n-type layer 4A becomes larger, making it difficult for electrons to flow. If electrons cannot flow, the current of the solar cell decreases.
[0209] The difference between the band gap BG4 of the first n-type layer 4A and the band gap BG5 of the second n-type layer 4B (BG5-BG4) is preferably 3.0 eV or more and 4.8 eV or less, more preferably 3.1 eV or more and 3.9 eV or less, and even more preferably 3.2 eV or more and 4.0 eV or less. If the band gap difference is small, the carrier concentration of the first n-type layer decreases, and the effect of the first n-type layer weakens. If the band gap difference is large, the conduction band shift between the first n-type layer 4A and the second n-type layer 4B becomes larger, making it difficult for electrons to flow. If electrons cannot flow, the current of the solar cell decreases.
[0210] The difference between the band gap BG4 of the first n-type layer 4A and the band gap BG5 of the second n-type layer 4B (BG5-BG4) is preferably greater than the difference between the band gap BG4 of the first n-type layer 4A and the band gap BG3 of the p-type light-absorbing layer 3 (BG3-BG4). The difference between the band gap BG4 of the first n-type layer 4A and the band gap BG5 of the second n-type layer 4B (BG5-BG4) is preferably more than 1.5 times and less than 30 times, more preferably more than 2.0 times and less than 20 times, and even more preferably more than 2.5 times and less than 15 times. That is, preferably, the band gap BG4 of the first n-type layer 4A is closer to the band gap BG3 of the p-type light absorption layer 3 than the band gap BG5 of the second n-type layer 4B, and the difference between the band gap BG4 of the first n-type layer 4A and the band gap BG3 of the p-type light absorption layer 3 is relatively small compared with the difference between the band gap BG4 of the first n-type layer 4A and the band gap BG5 of the second n-type layer 4B.
[0211] The carrier concentration (electron concentration) of the first n-type layer 4A is preferably higher than the carrier concentration (hole concentration) of the p-type light-absorbing layer 3. The carrier concentration (electron concentration) of the first n-type layer 4A is preferably 100 times or more and 1,000,000 times or less, more preferably 500 times or more and 500,000 times or less, and even more preferably 1,000 times or more and 100,000 times or less. It is believed that by using the first n-type layer 4A, the influence caused by the low carrier concentration of the wide-bandgap semiconductor, where the carrier concentration of the p-type light-absorbing layer 3 tends to decrease, can be compensated for.
[0212] The band gap BG4 of the first n-type layer 4A of the solar cell 120, which uses a p-type light-absorbing layer 3 containing a cuprous oxide compound, is preferably 1.4 eV or more and less than 2.1 eV, more preferably 1.45 eV or more and less than 2.0 eV, and even more preferably 1.5 eV or more and less than 1.9 eV.
[0213] The first n-type layer 4A of the solar cell 120, which uses a p-type light-absorbing layer 3 containing a cuprous oxide compound, is preferably Cu3N or amorphous silicon. In addition to Cu3N and amorphous silicon, the first n-type layer 4A may also contain elements contained in the p-type light-absorbing layer 3 and the second n-type layer 4B.
[0214] Preferably, the first n-type layer 4A of the solar cell 120, which uses a p-type light-absorbing layer 3 containing a cuprous oxide compound, comprises 95 wt% to 100 wt% Cu3N or amorphous silicon. More preferably, the first n-type layer 4A comprises 98 wt% to 100 wt% Cu3N or amorphous silicon. Even more preferably, the first n-type layer 4A comprises 99 wt% to 100 wt% Cu3N or amorphous silicon. 100 wt% of the first n-type layer 4A may be composed of Cu3N or amorphous silicon.
[0215] From the viewpoint of repairing Cu defects in the first region 3a of the p-type light-absorbing layer 3 containing cuprous oxide compounds, it is preferable to use Cu3N in the first n-type layer 4A of the solar cell 120 that uses the p-type light-absorbing layer 3 containing cuprous oxide compounds.
[0216] The first n-type layer 4A of a solar cell 120 using a p-type light-absorbing layer 3 comprising a compound with a chalcopyrite-type structure and a band gap BG3 of 1.6 eV or higher and 2.4 eV or lower is preferably Cu3N, CdTe, or amorphous silicon. In addition to Cu3N, CdTe, or amorphous silicon, the first n-type layer 4A may also contain elements contained in the p-type light-absorbing layer 3 and the second n-type layer 4B.
[0217] In a solar cell 120 using a p-type light-absorbing layer 3 comprising a compound with a chalcopyrite-type structure, the first n-type layer 4A preferably comprises 95 wt% to 100 wt% Cu3N, CdTe, or amorphous silicon; more preferably, 98 wt% to 100 wt% Cu3N, CdTe, or amorphous silicon; and even more preferably, 99 wt% to 100 wt% Cu3N, CdTe, or amorphous silicon. The first n-type layer 4A may be composed of 100 wt% Cu3N, CdTe, or crystalline silicon.
[0218] The first n-type layer 4A of a solar cell 120 using a p-type light-absorbing layer 3 comprising a compound with a chalcopyrite-type structure and a band gap BG3 of 1.6 eV or higher and 2.4 eV or lower is preferably Cu3N, CdTe, or amorphous silicon. In addition to Cu3N, CdTe, or amorphous silicon, the first n-type layer 4A may also contain elements contained in the p-type light-absorbing layer 3 and the second n-type layer 4B.
[0219] In a solar cell 120 using a p-type light-absorbing layer 3 comprising a compound with a chalcopyrite-type structure, the bandgap BG4 of the first n-type layer 4A is preferably 1.4 eV or more and 2.1 eV or less, more preferably 1.45 eV or more and 2.0 eV or less, and even more preferably 1.5 eV or more and 1.9 eV or less. However, the bandgap BG4 of the first n-type layer 4A is necessarily smaller than the bandgap BG3 of the p-type light-absorbing layer.
[0220] The thickness of the first n-type layer 4A is preferably 1 nm or more and 50 nm or less, more preferably 2 nm or more and 40 nm or less, and even more preferably 3 nm or more and 30 nm or less.
[0221] The second n-type layer 4B of the solar cell 120, which uses a p-type light-absorbing layer 3 containing a cuprous oxide compound, preferably contains one or more elements selected from Ga oxides containing any element represented by M2, oxides containing Zn and any element represented by M3, Ti oxides containing any element represented by M4, and strontium titanate containing any element represented by M4. The element represented by M2 is selected from one or more elements selected from H, Sn, Sb, Cu, Ag, Li, Na, K, Cs, Rb, Al, In, Zn, Mg, Si, Ge, N, B, Ti, Hf, Zr, Ca, Ce, La, Pr, and Nd. The element represented by M3 is selected from one or more elements selected from Sn, Sb, Hf, Zr, Si, Al, and Mg. The element represented by M4 is selected from one or more elements selected from Nb, Ta, Mo, and W.
[0222] The second n-type layer 4B of the solar cell 120 using a p-type light-absorbing layer 3 containing a cuprous oxide compound is preferably a laminate containing an oxide layer containing Ga (on the side of the first n-type layer 4A) that arbitrarily contains the element shown in M2 and an oxide layer containing an oxide layer containing an element shown in M3 and Zn (on the side of the second electrode 5), a laminate containing an oxide layer containing an oxide layer containing an element shown in M3 and Zn, an oxide layer containing an oxide layer containing Ga (on the side of the first n-type layer 4A) that arbitrarily contains the element shown in M2 and an oxide layer containing ...
[0223] The second n-type layer 4B of the solar cell 120, which uses a p-type light-absorbing layer 3 containing a compound with a chalcopyrite-type structure, is CdS, Zn(O,S), ZnS, ZnMgO, or In2S3, and is not limited to these.
[0224] The preferred carrier concentration (electron concentration) of the first n-type layer 4A is 2.0 × 10⁻⁶. 16 cm -3 Above and 1.0×10 20 cm -3 Hereinafter, 5.0 × 10 is preferred. 16 cm -3 Above and 5.0×10 19 cm -3 Hereinafter, 1.0 × 10 is further preferred. 17 cm -3 Above and 1.0×10 19 cm -3 the following.
[0225] The second n-type layer 4B is the main n-type layer in the solar cell 120. The thickness of the second n-type layer 4B is preferably 1 nm or more and 50 nm or less, more preferably 2 nm or more and 40 nm or less, and even more preferably 3 nm or more and 30 nm or less.
[0226] The first n-type layer 4A is formed, for example, by atomic layer deposition (ALD), sputtering, pulsed laser deposition (PLD), chemical vapor deposition (CVD), or chemical bath deposition (CBD). The first n-type layer 4A is preferably crystalline, but may also contain amorphous material. Alternatively, a thin Cu layer may be formed on the surface of the p-type light-absorbing layer 3, and Cu3N may be formed by nitriding Cu in an atmosphere containing ammonia and oxygen.
[0227] The second n-type layer 4B is formed by methods such as atomic layer deposition, sputtering, pulsed laser deposition, chemical vapor deposition, and chemical bath deposition. The second n-type layer 4B is preferably crystalline, but may also contain amorphous material.
[0228] The valence band from the p-type light-absorbing layer 3 of the solar cell 120, which includes the first n-type layer 4A, to the second n-type layer 4B is preferably discontinuous.
[0229] Between the p-type light-absorbing layer 3 and the first n-type layer 4A, an intermediate layer may exist in an island-like manner, for example, containing one or more oxides selected from Al, Hf, Zr and B.
[0230] The n-type layer 4 of the third embodiment can be used in the first and second embodiments.
[0231] The second electrode 5 is disposed on the second n-type layer 4B. The second electrode 5 is an electrode on the side of the second n-type layer 4B that is transparent to visible light. The second electrode 5 is preferably disposed on the second n-type layer 4B. For the second electrode 5, an oxide transparent conductive film is preferably used. As the oxide transparent conductive film used in the second electrode 5, it is preferably a semiconductor conductive film selected from the group consisting of doped tin oxide, indium tin oxide, aluminum-doped zinc oxide, boron-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, titanium-doped indium oxide, indium gallium zinc oxide, and hydrogen-doped indium oxide. As the dopant in the tin oxide film, it is not particularly limited as long as it is selected from the group consisting of In, Si, Ge, Ti, Cu, Sb, Nb, Ta, W, Mo, F, and Cl. In order to reduce the resistance of the oxide transparent conductive film, the second electrode 5 may include a mesh or wire-shaped electrode. For the mesh or wire-shaped electrode, it is not particularly limited to Mo, Au, Cu, Ag, Al, Ta, or W. Graphene may also be used for the second electrode 5. Graphene is preferably stacked with silver nanowires.
[0232] The thickness of the second electrode 5 was determined by cross-sectional observation using an electron microscope and by using a height difference meter.
[0233] The thickness of the second electrode 5 is 30 nm or more and 2 μm or less, more preferably 30 nm or more and 1000 nm or less, and even more preferably 30 nm or more and 500 nm or less.
[0234] The second electrode 5 is preferably formed by, for example, ALD, sputtering, etc.
[0235] The composition of solar cell 120, for example, is analyzed... Figure 2 The analysis points A1 to A9 shown are used for confirmation. The center of each analysis point is determined by analyzing it in the thickness direction.
[0236] The carrier concentration of each layer contained in the solar cell 120 can be calculated, for example, by measuring the Hall effect at room temperature in an atmospheric atmosphere based on the van der Bauer method using an AC Hall effect measuring device manufactured by Toyo Technica.
[0237] The band gap of each layer in the solar cell 120 can be determined, for example, by measuring the absorbance using a spectrophotometer.
[0238] Next, examples of manufacturing methods for several configurations of solar cells 120 are shown.
[0239] The first example is a solar cell with the following configuration.
[0240] Substrate 1: White glass First electrode 2: A stack of ITO (on the substrate 1 side) and ATO (on the p-type light-absorbing layer 3 side). p-type light-absorbing layer 3: Cu2O First n-type layer 4A: Cu3N Second n-type layer 4B: Ga2O3 (side of first n-type layer 4A) and ZTO (side of second electrode 5 containing Zn Ti oxide) Second electrode 5: AZO First, ITO (In:Sn=80:20, film thickness 150 nm) and ATO (Sn:Sb=98:2, film thickness 100 nm) are deposited on a white glass substrate using CVD as the first electrode 2. A Cu2O film with a thickness of 6.6 μm is formed on the ATO substrate as a p-type light-absorbing layer 3 by sputtering in a nitrogen, oxygen, and argon atmosphere. Then, a Cu3N film with a thickness of 10 nm is formed on the Cu2O film by sputtering. Next, as the second n-type layer 4B, a Ga2O3 film with a thickness of 15 nm is formed on the Cu3N substrate by ALD, and a ZnSnO (Zn:Sn=80:20) film with a thickness of 14 nm is formed on the Ga2O3 substrate. Then, as the second electrode 5, AZO is formed on the ZnSnO substrate using ALD with a thickness of 40 nm and an Al content of 5% relative to Zn, resulting in a solar cell 120. Alternatively, in the final stage of sputtering the p-type light-absorbing layer 3, a 10 nm thick Cu film can be formed on Cu2O, and the film can be heated in an atmosphere containing ammonia and oxygen to dehydrogenate ammonia. The generated active nitrogen species can then be used to nitrid the Cu film, thereby forming Cu3N on Cu2O.
[0241] The second example is a solar cell with the following configuration.
[0242] Substrate 1: White glass First electrode 2: A stack of ITO (on the substrate 1 side) and ATO (on the p-type light-absorbing layer 3 side). p-type light-absorbing layer 3: Cu2O First n-type layer 4A: Amorphous silicon Second n-type layer 4B: ZTO Second electrode 5: AZO First, ITO (In:Sn=80:20, film thickness 150 nm) and ATO (Sn:Sb=98:2, film thickness 100 nm) are deposited on a white glass substrate using CVD as the first electrode 2. A 5 μm thick Cu₂O film is formed on the ATO substrate as a p-type light-absorbing layer 3 by sputtering in a nitrogen, oxygen, and argon atmosphere. Then, a 10 nm thick amorphous silicon film is formed on the Cu₂O film using plasma CVD with silane gas. Next, a 30 nm thick ZnSnO (Zn:Sn=80:20) film is formed on the amorphous silicon substrate as the second n-type layer 4B. Finally, as the second electrode 5, AZO is formed on the ZnSnO substrate using ALD with a thickness of 40 nm and an Al content of 5% relative to Zn, resulting in a solar cell 120.
[0243] The third example is a solar cell with the following configuration.
[0244] Substrate 1: White glass First electrode 2: Mo p-type light-absorbing layer 3: CuGaSe2 First n-type layer 4A: CdTe Second n-type layer 4B: CdS Second electrode 5: FTO First, a 1 μm thick Mo film is formed on a white glass substrate by DC magnetron sputtering as the first electrode 2. Then, a 2 μm thick CuGaSe2 film is formed on the Mo film as the p-type light-absorbing layer 3 using a three-stage method. Next, a 10 nm thick CdTe film is formed on the CuGaSe2 substrate as the first n-type layer 4A by sputtering. Next, a 30 nm thick CdS film is formed on the CdTe substrate as the second n-type layer 4B using the CBD method. Finally, a 100 nm thick FTO (Sn:F=95:5) film is formed on the CdS substrate as the second electrode 5 using CVD, resulting in a solar cell 120.
[0245] The fourth example is a solar cell with the following configuration.
[0246] Substrate 1: White glass First electrode 2: ITO p-type light-absorbing layer 3: Cu(Ga,In)(S,Se)2 Cu3N on the first n-type layer 4A CdS on the second n-type layer 4B FTO on the second electrode 5.
[0247] First, as the first electrode 2, an ITO (In:Sn=80:20, film thickness 150 nm) film is formed on a white glass substrate using CVD. Then, as the p-type light-absorbing layer 3, a 2 μm thick Cu(Ga,In)(S,Se)₂ film is formed on the ITO using a three-stage process. Next, as the first n-type layer 4A, a 10 nm thick Cu₃N film is formed on the Cu(Ga,In)(S,Se)₂ substrate using sputtering. Next, as the second n-type layer 4B, a 30 nm thick CdS film is formed on the Cu₃N substrate using CBD. Finally, as the second electrode 5, a 100 nm thick FTO (Sn:F=95:5) film is formed on the CdS substrate using CVD, resulting in a solar cell 120.
[0248] (Fourth Implementation) The fourth embodiment relates to a multijunction solar cell. Figure 6 The diagram shows a cross-sectional concept of a multi-junction solar cell according to the fourth embodiment. Figure 6 The multi-junction solar cell 200 has a solar cell (first solar cell) 100 of the first embodiment (or solar cell 110 of the second embodiment, or solar cell 120 of the third embodiment) and a second solar cell 201 on the light incident side. The band gap of the light-absorbing layer of the second solar cell 201 is smaller than that of the p-type light-absorbing layer 3 of the solar cell 100 of the first embodiment (or solar cell 110 of the second embodiment, or solar cell 120 of the third embodiment). It should be noted that the multi-junction solar cell 200 of the embodiments also includes solar cells obtained by joining three or more solar cells.
[0249] The band gap of the p-type light-absorbing layer (cuprous oxide) 3 of the first solar cell 100 of the fourth embodiment (or the solar cell 110 of the second embodiment, or the solar cell 120 of the third embodiment) is about 2.0 eV or more and 2.2 eV or less. Therefore, the band gap of the light-absorbing layer of the second solar cell 201 is preferably 1.0 eV or more and 1.6 eV or less. As the light-absorbing layer of the second solar cell 201, it is preferably selected from one of the following: a compound semiconductor layer composed of one or more of CIGS and CdTe compounds with high In content, crystalline silicon, and perovskite compounds.
[0250] (Fifth implementation method) The fifth embodiment relates to a solar cell module. Figure 7 A perspective view showing the solar cell module 300 according to the fifth embodiment. Figure 7The solar cell module 300 includes a first solar cell module 301 comprising a plurality of solar cells 100 or a first solar cell module 301 comprising a plurality of multi-junction solar cells 200. The solar cell module 300 may also be disposed on the light incident side of the configured solar cells.
[0251] Figure 8 This is a perspective view of the solar cell module 310 according to the fifth embodiment. The solar cell module 310 is a solar cell module (tandem solar cell module) formed by stacking a first solar cell module 301 and a second solar cell module 302, which include a plurality of solar cells 100. The first solar cell module 301 is the light incident side. For the second solar cell module 302, the second solar cell 201 is preferably used.
[0252] (Sixth Implementation Method) The sixth embodiment relates to a solar power generation system. The solar cell module of the fifth embodiment can be used as a generator in the solar power generation system of the sixth embodiment. The solar power generation system of this embodiment is a system that uses a solar cell module to generate electricity; specifically, it includes a solar cell module for generating electricity, a mechanism for converting the generated electricity into power, and an energy storage mechanism for storing the generated electricity or a load for consuming the generated electricity. Figure 9 The diagram shows the configuration of a solar power generation system 400 according to an embodiment. Figure 9 The solar power generation system includes a solar cell module 401 (300), a converter 402, a battery 403, and a load 404. Either the battery 403 or the load 404 may be omitted. The load 404 may also be configured to utilize the electrical energy stored in the battery 403. The converter 402 is a device containing circuits or components that perform power conversion, such as voltage transformation or DC-AC conversion, including DC-DC converters, DC-AC converters, and AC-AC converters. The configuration of the converter 402 can be optimized based on the generated voltage, the configuration of the battery 403, or the load 404.
[0253] The solar cell module 401 contains solar cells that generate electricity by receiving sunlight. This electricity is converted by a converter 402, stored in a battery 403, or consumed by a load 404. Preferably, the solar cell module 401 is equipped with a solar tracking drive to ensure it always faces the sun, a concentrator to focus sunlight, or additional devices to improve power generation efficiency. The load 404 can be an electrolysis device used for water electrolysis, CO2 electrolysis, ammonia electrolysis, ammonia synthesis, etc.
[0254] The solar power generation system 400 is preferably used in immovable properties such as residences, commercial facilities, or factories, or in movable properties such as vehicles, aircraft, or electronic equipment. By using solar cells with excellent conversion efficiency in the solar cell module, an increase in power generation can be expected.
[0255] As an example of the use of the solar power generation system 400, a vehicle is shown. Figure 10 The diagram shows a conceptual design of vehicle 500. Figure 10 The vehicle 500 includes a body 501, a solar cell module 502, a power conversion device 503, a battery 504, a motor 505, and tires (wheels) 506. The electricity generated by the solar cell module 502, located on the upper part of the body 501, is converted by the power conversion device 503, and either charged by the battery 504 or consumed by loads such as the motor 505. Using the electricity supplied by the solar cell module 502 or the battery 504, the motor 505 rotates the tires (wheels) 506, thereby enabling the vehicle 500 to operate. The solar cell module 502 may not be multi-junction type, but may consist only of a first solar cell module equipped with the solar cell 100 of the first embodiment (or the solar cell 110 of the second embodiment, or the solar cell 120 of the third embodiment). When using a transmissive solar cell module 502, it is preferable to use the solar cell module 502 as a power generation window on the side of the body 501, in addition to the upper part of the body 501.
[0256] As an example of the use of the solar power generation system 400, a drone (quadcopter drone) is shown. The drone uses a solar cell module 401. Figure 11 The schematic diagram of the drone 600 simply illustrates the configuration of the drone according to this embodiment. The drone 600 includes a solar cell module 601, a frame 602, a motor 603, a rotor 604, and a control unit 605. The solar cell module 601, motor 603, rotor 604, and control unit 605 are disposed on the frame 602. The control unit 605 converts or adjusts the power output from the solar cell module 601. The motor 603 uses the power output from the solar cell module 601 to rotate the rotor 604. By manufacturing the drone 600 of this configuration, which includes the solar cell module 601 of this embodiment, a drone capable of flying using more electricity can be provided.
[0257] An electrolysis apparatus is shown as an example of the use of the solar power generation system 400. The electrolysis apparatus uses a solar cell module 401. The electrolysis apparatus of the embodiment is used for water electrolysis, ammonia synthesis electrolysis, ammonia electrolysis to generate hydrogen, CO2 electrolysis to synthesize CO or hydrocarbons, etc. Figure 12This is a schematic diagram of an electrolysis apparatus 700. The electrolysis apparatus 700 includes an anode 701, a cathode 702, a diaphragm 703, an anode rectifier plate 704, a cathode rectifier plate 705, a power conversion device 706, and a solar cell module 707. The power conversion device 706 converts the electricity generated by the solar cell module 707 into a power source suitable for the electrolysis reaction. The electrolysis apparatus 700 is configured to use the anode 701, cathode 702, diaphragm 703, anode rectifier plate 704, and cathode rectifier plate 705 as the load 404 of a solar power generation system 400. The electrolysis reaction takes place at the anode 701, cathode 702, diaphragm 703, anode rectifier plate 704, and cathode rectifier plate 705. Preferably, a stack of components for the electrolysis reaction is used.
[0258] The present invention will now be described in more detail with reference to embodiments, but the present invention is not limited to the following embodiments. Embodiments A to D relate to a first embodiment. Embodiments E and F relate to a second embodiment. Embodiments G to I relate to a third embodiment.
[0259] (Example A) (Example A1) On a glass substrate 1, as the first electrode 2 on the back side, ITO (In:Sn=80:20, film thickness 150 nm) and ATO (Sn:Sb=98:2, film thickness 100 nm) are deposited on the upper surface of the side in contact with the glass phase. A Cu₂O layer with a thickness of 6 μm is formed on the ATO as a p-type light-absorbing layer 3 by sputtering in an oxygen and argon atmosphere. After the formation of the p-type light-absorbing layer 3, a trace amount of Cu is deposited. Then, a Ga₂O₃ film with a thickness of 10 nm is formed as an n-type layer 4. Finally, an AZO (ZnO:Al) film with a thickness of 0.1 μm is formed as the second electrode 5 to obtain a solar cell 100.
[0260] A solar simulator simulating an AM1.5G light source was used. Under this light source, Si cells were used as a reference, and the light intensity was adjusted to 1 sun. Measurements were performed at atmospheric pressure, with the indoor temperature set to 25°C. Voltage was scanned, and the short-circuit current density Jsc (the value obtained by dividing the current by the cell area) was measured. With the horizontal axis set to voltage and the vertical axis to current density, the point where the horizontal axis intersects the short-circuit voltage Voc is defined. On the measurement curve, the point where the voltage multiplied by the short-circuit current density reaches its maximum is set as Vmpp and Jmpp (maximum power point), respectively. The formula FF = (Vmpp) / (Jmpp) is used to calculate the maximum power. Jmpp) / (Voc) The fill factor is calculated using Jsc. Additionally, Eff. = Voc. Jsc FF calculates the conversion efficiency.
[0261] The evaluation assesses whether the highest luminous intensity value in the wavelength range of 900 nm to 950 nm in the first region is greater than or equal to 0 times but less than 2 times the highest luminous intensity value in the wavelength range of 900 nm to 950 nm in the second region. If it is greater than or equal to 0 times but less than 2 times, it is rated A; if it is greater than 2 times, it is rated B. The evaluation of luminous intensity is common in Examples A to D.
[0262] Regarding light transmittance, a transmittance of 75% or more for light in the wavelength band of 700nm to 1000nm is evaluated as A; a transmittance of 70% or more but less than 75% for light in the wavelength band of 700nm to 1000nm is evaluated as B; and a transmittance of less than 70% for light in the wavelength band of 700nm to 1000nm is evaluated as C. The evaluation of light transmittance is common in Examples A through D.
[0263] Regarding Jsc, cases where the Jsc relative to the comparison object is 1.01 times or more are evaluated as A, cases where the Jsc relative to the comparison object is 1.0 times or more but less than 1.01 times are evaluated as B, and cases where the Jsc relative to the comparison object is less than 1.0 times are evaluated as C. The evaluation of Jsc is common in Examples A to D.
[0264] Regarding Voc, cases where the Voc is 1.02 times or more relative to the comparison object are evaluated as A, cases where the Voc is 1.00 times or more but less than 1.02 times relative to the comparison object are evaluated as B, and cases where the Voc is less than 1.00 times relative to the comparison object are evaluated as C. The evaluation of Voc is common in Examples A to D.
[0265] Regarding FF, cases where the FF relative to the comparison object is 1.01 times or more are evaluated as A, cases where the FF relative to the comparison object is 1.00 times or more but less than 1.01 times are evaluated as B, and cases where the FF relative to the comparison object is less than 1.00 times are evaluated as C. The evaluation of FF is common in Examples A to D.
[0266] Regarding conversion efficiency, cases with a conversion efficiency of 1.04 times or more relative to the comparison object are evaluated as A, cases with a conversion efficiency of 1.00 times or more but less than 1.04 times relative to the comparison object are evaluated as B, and cases with a conversion efficiency of less than 1.00 times relative to the comparison object are evaluated as C. The evaluation of conversion efficiency is common in Examples A to D.
[0267] (Comparative Example A1) On a glass substrate 1, as the first electrode 2 on the back side, ITO (In:Sn=80:20, film thickness 150 nm) and ATO (Sn:Sb=98:2, film thickness 100 nm) are deposited on the upper surface of the side in contact with the glass phase. A Cu2O layer with a thickness of 6 μm is formed on the ATO as a p-type light-absorbing layer 3 by sputtering in an oxygen and argon atmosphere. After the formation of the p-type light-absorbing layer 3, a Ga2O3 film with a thickness of 10 nm is formed directly above the p-type light-absorbing layer 3 as an n-type layer 4. Then, an AZO (ZnO:Al) film with a thickness of 0.1 μm is formed as the second electrode 5 to obtain a solar cell. The solar cell of Comparative Example A1 is then evaluated in the same manner as in Example A1.
[0268] (Example A2) After the p-type light-absorbing layer 3 is formed, Zn is deposited instead of Cu, and otherwise, a solar cell is obtained in the same manner as in Example A1. Then, the solar cell of Example A2 is evaluated in the same manner as in Example A1.
[0269] (Example A3) After the p-type light-absorbing layer 3 is formed, Mg is deposited instead of Cu, and otherwise, a solar cell is obtained in the same manner as in Example A1. Then, the solar cell of Example A3 is evaluated in the same manner as in Example A1.
[0270] (Example A4) After the p-type light-absorbing layer 3 is formed, Li is deposited instead of Cu, and otherwise, a solar cell is obtained in the same manner as in Example A1. Then, the solar cell of Example A4 is evaluated in the same manner as in Example A1.
[0271] (Example A5) After the p-type light-absorbing layer 3 is formed, Na is deposited instead of Cu, and otherwise, a solar cell is obtained in the same manner as in Example A1. Then, the solar cell of Example A5 is evaluated in the same manner as in Example A1.
[0272] (Example A6) After the p-type light-absorbing layer 3 is formed, K is deposited instead of Cu, and otherwise, a solar cell is obtained in the same manner as in Example A1. Then, the solar cell of Example A6 is evaluated in the same manner as in Example A1.
[0273] (Example A7) After the p-type light-absorbing layer 3 is formed, Rb is deposited instead of Cu, and otherwise, a solar cell is obtained in the same manner as in Example A1. Then, the solar cell of Example A7 is evaluated in the same manner as in Example A1.
[0274] (Example A8) After the p-type light-absorbing layer 3 is formed, Cs is deposited instead of Cu, and otherwise, a solar cell is obtained in the same manner as in Example A1. Then, the solar cell of Example A8 is evaluated in the same manner as in Example A1.
[0275] (Example A9) After the p-type light-absorbing layer 3 is formed, Be is deposited instead of Cu, and otherwise, a solar cell is obtained in the same manner as in Example A1. Then, the solar cell of Example A9 is evaluated in the same manner as in Example A1.
[0276] (Example A10) After the p-type light-absorbing layer 3 is formed, Sr is deposited instead of Cu, and otherwise, a solar cell is obtained in the same manner as in Example A1. Then, the solar cell of Example A10 is evaluated in the same manner as in Example A1.
[0277] (Example A11) After the p-type light-absorbing layer 3 is formed, Ba is deposited instead of Cu, and otherwise, a solar cell is obtained in the same manner as in Example A1. Then, the solar cell of Example A11 is evaluated in the same manner as in Example A1.
[0278] The evaluation results of the solar cell of Example A are shown below. Figure 13 The results from Examples A1 to A11 show that by repairing Cu defects, Jsc, Voc, and FF are improved, which helps to improve conversion efficiency.
[0279] in addition, Figure 14 The photoluminescence spectra of Example A1 and Comparative Example A1 are shown. The photoluminescence spectra of the examples have all undergone data smoothing. Figure 14 The solid line (Example A1) and dashed line (Comparative Example A1) in the photoluminescence spectrum represent the luminescence intensity at a wavelength of 930 nm. For the solar cells of Example A1 and Comparative Example A1... Figure 2 The cross-section at position A5, with the interface between the p-type light-absorbing layer 3 and the n-type layer 4 as position 0 [μm], and the distance towards the first electrode 2 as the horizontal axis. From Figure 14 The photoluminescence spectrum shows that the wavelength of Example A1, represented by the solid line, is 930 nm, which is significantly reduced.
[0280] As can be seen from the above, the highest value of the luminous intensity in the wavelength range of 900 nm to 950 nm in the first region is 0 to 2 times the highest value of the luminous intensity in the wavelength range of 900 nm to 950 nm in the second region. Furthermore, in any embodiment, the highest value of the luminous intensity in the wavelength range of 900 nm to 950 nm in the first region is 0 to 2 times the highest value of the luminous intensity in the wavelength range of 900 nm to 950 nm in the second region.
[0281] in addition, Figure 15 The photoluminescence spectra of Example A1 (solid line) and Comparative Example A1 (dashed line) at position 0 [μm] are shown. No significant emission was observed in Example A1 at wavelengths above 900 [nm] and below 950 [nm], but in Comparative Example A1, a peak centered at approximately 930 [nm] was observed at wavelengths above 900 [nm] and below 950 [nm].
[0282] (Example B) (Example B1) On a glass substrate 1, as the first electrode 2 on the back side, ITO (In:Sn=80:20, film thickness 150 nm) and ATO (Sn:Sb=98:2, film thickness 100 nm) are deposited on the upper surface of the side in contact with the glass phase. A Cu₂O layer with a thickness of 6 μm is formed on the ATO as a p-type light-absorbing layer 3 by sputtering in an oxygen and argon atmosphere. After the formation of the p-type light-absorbing layer 3, a trace amount of Cu is deposited. Then, a Ga₂O₃ film with a thickness of 10 nm is formed as an n-type layer 4. Then, an AZO (ZnO:Al) film with a thickness of 0.1 μm is formed as the second electrode 5 to obtain a solar cell 100. The solar cell of Example B1 is then evaluated in the same manner as in Example A1.
[0283] (Comparative Example B1) Except that Cu was not deposited after the formation of the p-type light-absorbing layer 3, a solar cell was obtained in the same manner as in Example B1. Then, the solar cell of Comparative Example B1 was evaluated in the same manner as in Example A1.
[0284] (Example B2) After the p-type light-absorbing layer 3 was formed, a trace amount of Cu was deposited at a higher temperature than in Example B1. Otherwise, the solar cell was obtained in the same manner as in Example A1. Then, the solar cell of Example B2 was evaluated in the same manner as in Example A1.
[0285] (Example B3) After the p-type light-absorbing layer 3 was formed, a small amount of Cu was deposited at a lower temperature than in Example B1. Otherwise, the solar cell was obtained in the same manner as in Example A1. Then, the solar cell of Example B3 was evaluated in the same manner as in Example A1.
[0286] The evaluation results of the solar cell of Example B are shown below. Figure 16 The table shows that in Examples B1 to B3, the diffusion distance of Cu with repaired Cu defects changed. However, the results of Examples B1 to B3 show that in any of the solar cells, by repairing Cu defects, Jsc, Voc, and FF are improved, which helps to improve the conversion efficiency.
[0287] Furthermore, in any embodiment B, the highest value of the luminous intensity in the wavelength region of the first region ranging from 900 nm to 950 nm is 0 times to 2 times the highest value of the luminous intensity in the wavelength region of the second region ranging from 900 nm to 950 nm.
[0288] (Example C) (Example C1) A Cu2O layer as a p-type light-absorbing layer 3 was epitaxially grown on a substrate layer with a buffer layer between a NiW layer and an SRO (SrRuO3) layer using a PLD method. A trace amount of Zn was then deposited on the Cu2O layer. Next, a Ga2O3 film with a thickness of 10 nm was formed as an n-type layer 4. Then, an AZO (ZnO:Al) film with a thickness of 0.1 μm was formed as a second electrode 5 to obtain a solar cell 100. The solar cell of Example C1 was then evaluated in the same manner as in Example A1.
[0289] (Comparative Example C1) Except that no Zn was deposited after the Cu2O layer was formed, a solar cell was obtained in the same manner as in Example C1. Then, the solar cell of Comparative Example C1 was evaluated in the same manner as in Example A1.
[0290] In Example C, conversion efficiency is also improved by repairing Cu defects.
[0291] (Example D) (Example D1) A Cu plate was oxidized at approximately 1000°C, and an Au electrode was formed on one side of the resulting cuprous oxide plate as the first electrode 2. A trace amount of Zn was deposited on the opposite side of the resulting cuprous oxide plate. Then, a Ga₂O₃ film with a thickness of 10 nm was formed as an n-type layer 4. Then, an AZO (ZnO:Al) film with a thickness of 0.1 μm was formed as the second electrode 5 to obtain a solar cell 100. The solar cell of Example D1 was then evaluated in the same manner as in Example A1.
[0292] (Comparative Example D1) Except that no Zn is deposited after the formation of the cuprous oxide plate, a solar cell was obtained in the same manner as in Example D1. Then, the solar cell of Comparative Example D1 was evaluated in the same manner as in Example A1.
[0293] In Example D, conversion efficiency is also improved by repairing Cu defects.
[0294] In a multi-junction solar cell using a solar cell as the top unit and a Si solar cell as the bottom unit, it is beneficial to improve the conversion efficiency. If the p-type light-absorbing layer 3 of the solar cell 100 contains a region with Cu defects, the region with Cu defects tends to absorb light in the wavelength range generated by the Si solar cell. Therefore, from the viewpoint of using it as a multi-junction solar cell, the solar cell of the embodiment included in the example is preferred.
[0295] (Example E) (Example E1) On a glass substrate 1, as the first electrode 2 on the back side, ITO (In:Sn=80:20, film thickness 150 nm) and ATO (Sn:Sb=98:2, film thickness 100 nm) are deposited on the upper surface of the side in contact with the glass phase. A Cu₂O layer with a thickness of 6 μm is formed on the ATO as a layer mainly composed of cuprous oxide compound by sputtering in an oxygen / argon atmosphere. After the formation of the p-type light-absorbing layer 3, a trace amount of Cu is deposited. Then, a Ga₂O₃ film with a thickness of 10 nm is formed as the n-type layer 4, and a ZnSnO (Zn:Sn=80:20) film with a thickness of 14 nm is formed on the Ga₂O₃ film. Finally, an AZO (ZnO:Al) film with a thickness of 0.1 μm is formed as the second electrode 5 to obtain a solar cell 120.
[0296] A solar simulator simulating an AM1.5 G light source was used. Under this light source, Si cells were used as a reference, and the light intensity was adjusted to 1 sun. Measurements were performed at atmospheric pressure, with the indoor temperature set to 25°C. Voltage was scanned, and the short-circuit current density Jsc (the value obtained by dividing the current by the cell area) was measured. With the horizontal axis set to voltage and the vertical axis to current density, the point where the horizontal axis intersects the short-circuit voltage Voc is defined. On the measurement curve, the point where the voltage multiplied by the short-circuit current density reaches its maximum is set as Vmpp and Jmpp (maximum power point), respectively. The formula FF = (Vmpp) / (Jmpp) is used to calculate the maximum power. Jmpp) / (Voc) The fill factor is calculated using Jsc. Additionally, Eff. = Voc. Jsc FF calculates the conversion efficiency.
[0297] Regarding the FF (Fold Value), cases where the FF relative to the comparison object is 1.05 times or more are evaluated as A; cases where the FF relative to the comparison object is 1.01 times or more but less than 1.05 times are evaluated as B; cases where the FF relative to the comparison object is greater than 1.00 times but less than 1.01 times are evaluated as C; cases where the FF relative to the comparison object is 0.90 times or more but less than 1.00 times are evaluated as D; and cases where the FF relative to the comparison object is less than 0.90 times are evaluated as E. The evaluation of FF is common in Examples E to F.
[0298] Regarding conversion efficiency, cases with a conversion efficiency of 1.03 times or more relative to the comparison object are evaluated as A, cases with a conversion efficiency greater than 1.00 times but less than 1.03 times relative to the comparison object are evaluated as B, and cases with a conversion efficiency of less than 1.00 times relative to the comparison object are evaluated as C. The evaluation of conversion efficiency is common in Examples E to F.
[0299] The sputtering temperature of the Cu2O layer, the deposition temperature of Cu, the average thickness of the deposited Cu, the evaluation results of FF, and the evaluation results of conversion efficiency are shown in the figure. Figure 17 The table shows the SEM image of the p-type light-absorbing layer 3 before the formation of the n-type layer 4. Figure 18 middle.
[0300] (Comparative Example E1) On a glass substrate 1, as the first electrode 2 on the back side, ITO (In:Sn=80:20, film thickness 150 nm) and ATO (Sn:Sb=98:2, film thickness 100 nm) are deposited on the upper surface of the side in contact with the glass phase. A Cu2O layer with a thickness of 6 μm is formed on the ATO by sputtering in an oxygen and argon atmosphere. A Ga2O3 film with a thickness of 10 nm is formed directly above the Cu2O layer as an n-type layer 4, and a ZnSnO (Zn:Sn=80:20) film with a thickness of 14 nm is formed on the Ga2O3 film. Then, an AZO (ZnO:Al) film with a thickness of 0.1 μm is formed as the second electrode 5 to obtain a solar cell. Then, the solar cell of Comparative Example E1 is evaluated in the same manner as in Example E1.
[0301] (Examples E2-E6, Comparative Examples E2-E9) Cu was deposited by varying the thickness of the Cu deposited on the Cu2O layer (the amount of Cu ejected from the target), and otherwise, a solar cell was obtained in the same manner as in Example E1. These examples were then evaluated in the same manner as in Example E1. The sputtering temperature of the Cu2O layer, the Cu deposition temperature, the average thickness of the deposited Cu, the evaluation results of the flyback effect (FF), and the evaluation results of the conversion efficiency for these examples (comparative examples) are shown below. Figure 17 In the table.
[0302] like Figure 17 As shown in the table, the flow rate (FF) and conversion efficiency change by varying the Cu thickness. In Comparative Example E2, where the Cu deposition thickness is 0.01 nm, there is almost no difference compared to Comparative Example E1, where no Cu is deposited. In Comparative Example E2, where the Cu deposition thickness is 0.01 nm, and Example E2, where the Cu deposition thickness is 0.02 nm, the Cu thickness is small, but in Example E2, the FF and conversion efficiency are significantly improved. Furthermore, if the Cu deposition thickness exceeds 1 nm, although Cu diffuses into the interior of the cuprous oxide-dominated layer, undiffused Cu remains on the surface of the cuprous oxide-dominated layer and precipitates. In Comparative Examples E3 to E9, where varying amounts of Cu are deposited to the extent of precipitation, the more Cu is deposited, the lower the FF and conversion efficiency become.
[0303] like Figure 18 As shown in the SEM image, multiple recesses 3i are formed on the surface of the p-type light-absorbing layer 3. Cross-sections of three recesses 3i are captured in the SEM image. The depths of these recesses 3i from the left side of the SEM image are 42 nm, 31 nm, and 52 nm.
[0304] (Example F) (Example F1) Solar cell 120 was obtained in the same manner as in Example E1. These examples were then evaluated in the same manner as in Example E1. The sputtering temperature of the Cu2O layer, the deposition temperature of Cu, the average thickness of the deposited Cu, the evaluation results of FF, and the evaluation results of conversion efficiency are shown in... Figure 19 In the table.
[0305] (Comparative Example F1) Solar cell 120 was obtained in the same manner as Comparative Example E1. These examples were then evaluated in the same manner as Example E1. The sputtering temperature of the Cu2O layer, the deposition temperature of Cu, the average thickness of the deposited Cu, the evaluation results of FF, and the evaluation results of conversion efficiency are shown in... Figure 19 In the table.
[0306] (Examples F2-F6, Comparative Examples F2-F8) Without changing the thickness of Cu deposited on the Cu2O layer (Comparative Example F5 had no Cu deposition), the stage temperature during Cu2O sputtering and the stage temperature during Cu deposition were changed, and the solar cell was obtained in the same manner as in Example F1. These examples were then evaluated in the same manner as in Example E1. The stage temperatures during Cu2O sputtering, Cu deposition, average thickness of deposited Cu, evaluation results of FF, and evaluation results of conversion efficiency for these examples (comparative examples) are shown below. Figure 19 In the table.
[0307] like Figure 19 As shown in the table, no improvement in FF and conversion efficiency was observed under both low and high surface temperatures of the cuprous oxide-dominated layer during Cu deposition. However, Cu precipitation was observed on the surface of the cuprous oxide-dominated layer under both high and low deposition temperatures.
[0308] (Example G) (Examples G1-G2, Comparative Examples G1-G2) Simulation of Example G was conducted under the following conditions. The solar cell 120 is composed of a p-type light-absorbing layer 3, a first n-type layer 4A, a second n-type layer 4B, and a second electrode 5 stacked sequentially. Through simulation, the open-circuit voltage [V] and short-circuit current density [mA / cm²] were determined. 3The simulation included curvature factor FF and conversion efficiency Eff. Although substrate 1 was not considered in the simulation, its presence or absence was not taken into account; therefore, the same results as the following implementation could be obtained even with substrate 1 present. The first electrode 2 was not considered in the simulation. The simulation software has limitations on the number of layers in the solar cell. If the p-type light-absorbing layer 3 is ohmically bonded to the first electrode 2, the resistance value of the series resistance Rs of the solar cell 120 can be evaluated even without considering the specific layer composition of the first electrode 2. Therefore, a simulation of the solar cell 120 without the first electrode 2 was performed under the premise that the p-type light-absorbing layer 3 is ohmically bonded to the first electrode 2 (assuming that the surface resistance and interface resistance of the first electrode 2 are reflected in the series resistance Rs). The simulation method used SCAPS (a Solar Cell Capacitance Simulator) to solve the Poisson equation and the formula for current continuity.
[0309] The simulation conditions for the p-type light-absorbing layer 3, the first n-type layer 4A, the second n-type layer 4B, and the second electrode 5 are shown in the figure. Figure 20 The table shows the simulation results. Figure 21 In the table.
[0310] Regarding Jsc, Jsc[mA / cm] which is smaller than the comparison object 2 The evaluation for the case of ] is D, and the comparison object Jsc[mA / cm 2 The case where ] is 100% or more but less than 105% is rated as C, and Jsc[mA / cm] is used as the comparison object. 2 Cases where the percentage is 105% or higher but less than 110% are rated as B, and the comparison object Jsc[mA / cm] is used as the comparison object. 2 Cases where the percentage is over 110% are rated A. The Jsc rating is common in Examples G through I.
[0311] Regarding Voc, cases where it is less than the comparison object Voc[V] are rated as D; cases where it is 100% or more but less than 110% of the comparison object Voc[V] are rated as C; cases where it is 110% or more but less than 120% of the comparison object Voc[V] are rated as B; and cases where it is 120% or more of the comparison object Voc[V] are rated as A. The evaluation of Voc is common in Examples G to I.
[0312] Regarding FF, the case where it is less than the FF[-] of the comparison object is evaluated as D; the case where the FF[-] of the comparison object is 100% or more but less than 105% is evaluated as C; the case where the FF[-] of the comparison object is 105% or more but less than 110% is evaluated as B; and the case where the FF[-] of the comparison object is 110% or more is evaluated as A. The evaluation of FF is common in Examples G to I.
[0313] Regarding Eff, cases where Eff is less than that of the comparison object are rated as D; cases where Eff is 100% or more but less than 110% of the comparison object are rated as C; cases where Eff is 110% or more but less than 120% of the comparison object are rated as B; and cases where Eff is 120% or more of the comparison object are rated as A. The evaluation of Eff is common in Examples G to I.
[0314] As shown in the table of results, by depositing the first n-type layer 4A, which has a smaller band gap than the p-type light-absorbing layer 3, Voc, Jsc, FF and Eff are all improved.
[0315] (Example H) (Examples H1-H5, Comparative Examples H1-H3) A cuprous oxide compound was used in the p-type light-absorbing layer 3, and the first n-type layer 4A and / or the second n-type layer 4B were modified, and simulations were performed in the same manner as in Example G. The simulation conditions are shown below. Figure 22 The table shows the results. Additionally, the simulation results of Example H are presented in... Figure 23 In the table.
[0316] As shown in the table of results, by depositing a first n-type layer with a smaller band gap than the cuprous oxide compound in the p-type light-absorbing layer 3, Voc, Jsc, FF, and Eff are all improved.
[0317] (Example I) (Examples I1-I2, Comparative Examples I1-I2) The p-type light-absorbing layer 3 uses a compound with a chalcopyrite-type structure. The first n-type layer 4A and / or the second n-type layer 4B are modified, and simulations are performed in the same manner as in Example G. The simulation conditions are shown below. Figure 24 The table shows the results. Additionally, the simulation results of Example I are presented in... Figure 25 In the table.
[0318] As shown in the table of results, by depositing a first n-type layer with a chalcopyrite-type structure and a smaller band gap than the p-type light-absorbing layer 3, Voc, Jsc, FF, and Eff are all improved.
[0319] The embodiments of the present invention have been described above, but the present invention is not limited to the above embodiments. During implementation, the constituent elements can be modified and embodied without departing from its spirit. Furthermore, various inventions can be formed through suitable combinations of the multiple constituent elements disclosed in the above embodiments. For example, constituent elements from different embodiments can be appropriately combined as in the variations.
[0320] Some elements in the instruction manual are represented only by element symbols.
[0321] The technical solutions for the implementation methods are described below.
[0322] Technical Solution A1 A solar cell comprising: First electrode, p-type light-absorbing layer on the first electrode, The n-type layer on the p-type light-absorbing layer, and The second electrode on the n-type layer, When the photoluminescence spectrum of the p-type light-absorbing layer is measured at temperatures below 100K, The first region is defined as the area extending from the surface of the p-type light-absorbing layer on the n-type layer side towards the first electrode side to a depth of 100 nm. The second region is defined as the area extending from the center of the p-type light-absorbing layer in the thickness direction toward the first electrode side to a depth of 100 nm. The highest value of the luminous intensity in the wavelength range of the first region (above 900 nm and below 950 nm) is more than 0 times and less than 2 times the highest value of the luminous intensity in the wavelength range of the second region (above 900 nm and below 950 nm).
[0323] Technical Solution A2 According to the solar cell described in technical solution A1, the p-type light-absorbing layer is mainly composed of cuprous oxide compound. The p-type light-absorbing layer, mainly composed of the cuprous oxide compound, contains one or more first elements selected from Zn, Mg, Li, Na, K, Rb, Cs, Be, Ca, Sr, and Ba on the n-type layer side. The third region is defined as the area extending from the surface of the p-type light-absorbing layer on the n-type layer side toward the first electrode side to a depth of 1 μm. The concentration of the first element contained in the third region is more than 90 atomic% and less than 100 atomic% of the first element contained in the p-type light-absorbing layer.
[0324] Technical Solution A3 In the solar cell described in technical solutions A1 or A2, the p-type light-absorbing layer is mainly composed of cuprous oxide compound. Surface resistivity of the first region (Ω / cm) 2 The surface resistivity of the second region is Ω / cm 2 More than 0.3 times and less than 10,000 times.
[0325] Technical Solution A4 According to the solar cell described in technical solution A2, the p-type light-absorbing layer is mainly composed of cuprous oxide compound. The fourth region is defined as the area extending from the surface of the p-type light-absorbing layer on the n-type layer side towards the first electrode side to a depth of 50 nm. The concentration of the first element contained in the fourth region is more than 30 atomic% and less than 80 atomic% of the first element contained in the p-type light-absorbing layer.
[0326] Technical Solution A5 According to any one of technical solutions A1 to A4, the solar cell wherein the p-type light-absorbing layer is mainly composed of cuprous oxide compound. The carrier concentration in the first region is 1×10 11 cm -3 Above and 1×10 15 cm -3 the following, The carrier concentration in the second region is 1×10 12 cm -3 Above and 1×10 15 cm -3 the following.
[0327] Technical Solution A6 According to any one of technical solutions A1 to A5, the solar cell wherein the p-type light-absorbing layer is mainly composed of cuprous oxide compound. The carrier concentration in the first region is 1×10 11 cm -3 Above and 3×10 14 cm -3 the following, The carrier concentration in the second region is 1×10 13 cm -3 Above and 7.5×10 14 cm -3 the following, The carrier concentration in the first region is more than 0.0001 times and less than 3 times the carrier concentration in the second region.
[0328] Technical Solution A7 According to any one of the technical solutions A1 to A6, the wavelength region between 900nm and 950nm is defined as the first wavelength region. The wavelength range above 600nm and below 650nm is designated as the second wavelength region. The ratio of ([the highest value of luminous intensity in the first wavelength region of the first region] × [the highest value of luminous intensity in the second wavelength region of the second region]) / ([the highest value of luminous intensity in the second wavelength region of the first region] × [the highest value of luminous intensity in the first wavelength region of the second region]) is greater than 0 and less than 20.
[0329] Technical Solution A8 According to any one of the technical solutions A1 to A7, the solar cell wherein the p-type light-absorbing layer is polycrystalline.
[0330] Technical Solution A9 In the solar cell described in technical solutions A2 or A4, the p-type light-absorbing layer is a polycrystalline form of cuprous oxide compound. The first element is present in the grain boundaries contained in the first region.
[0331] Technical Solution A10 According to any one of technical solutions A1 to A9, the solar cell wherein the p-type light-absorbing layer is mainly composed of cuprous oxide compound. It also contains crystals of cuprous oxide compounds with a particle size that is more than 5 times the thickness of the p-type light-absorbing layer.
[0332] Technical Solution A11 In the solar cell described in any of technical solutions A1 to A10, the first electrode is a transparent electrode. The second electrode is a transparent electrode.
[0333] Technical Solution A12 According to any one of the technical solutions A1 to A11, the thickness of the p-type light-absorbing layer is 500 nm or more and 10 μm or less.
[0334] Technical Solution A13 A multi-junction solar cell uses the solar cell described in any one of technical solutions A1 to A12.
[0335] Technical Solution A14 A solar cell module that uses the solar cell described in any one of technical solutions A1 to A12.
[0336] Technical Solution A15 A solar power generation system that uses the solar cell module described in technical solution A14 to generate electricity.
[0337] Technical Solution B1 A solar cell comprising: First electrode, p-type light-absorbing layer on the first electrode, The n-type layer on the p-type light-absorbing layer, and The second electrode on the n-type layer, The surface of the p-type light-absorbing layer on the n-type layer side has a depression.
[0338] Technical Solution B2 According to the solar cell described in technical solution B1, the maximum diameter of the recess is greater than 15nm and less than 80nm.
[0339] Technical Solution B3 According to the solar cell described in technical solution B1 or B2, the maximum diameter of the recess is greater than 20 nm and less than 70 nm.
[0340] Technical Solution B4 According to any one of technical solutions B1 to B3, the depth of the recess is more than 15nm and less than 80nm.
[0341] Technical Solution B5 According to any one of technical solutions B1 to B4, the density of the recesses is more than 1 and less than 250 within a 500nm×500nm square area.
[0342] Technical Solution B6 According to any one of technical solutions B1 to B5, the density of the recesses is more than 10 and less than 200 within a 500nm×500nm square area.
[0343] Technical Solution B7 According to any one of technical solutions B1 to B6, in the case where the photoluminescence spectrum of the p-type light-absorbing layer is measured at a temperature below 100 K,... The first region is defined as the area extending from the surface of the p-type light-absorbing layer on the n-type layer side towards the first electrode side to a depth of 100 [nm]. The second region is defined as the area extending from the center of the p-type light-absorbing layer in the thickness direction toward the first electrode side to a depth of 100 [nm]. The highest value of the luminous intensity in the wavelength range of the first region above 900 nm and below 950 nm is more than 0 times and less than 2 times the highest value of the luminous intensity in the wavelength range of the second region above 900 nm and below 950 nm.
[0344] Technical Solution B8 According to any one of technical solutions B1 to B7, the wavelength region ranging from 900 nm to 950 nm is defined as the first wavelength region. The wavelength range between 600 nm and 650 nm is defined as the second wavelength region. The ratio of ([the highest value of luminous intensity in the first wavelength region of the first region] × [the highest value of luminous intensity in the second wavelength region of the second region]) / ([the highest value of luminous intensity in the second wavelength region of the first region] × [the highest value of luminous intensity in the first wavelength region of the second region]) is greater than 0 and less than 20.
[0345] Technical Solution B9 A method for manufacturing a solar cell includes the following steps: The process of forming a layer mainly composed of cuprous oxide compound on the first electrode by sputtering; The process of depositing Cu on the surface of the cuprous oxide-based layer opposite to the first electrode side after the film formation of the cuprous oxide-based layer is completed; The process of forming an n-type layer on the surface of the p-type light-absorbing layer on which Cu is deposited; and The process of forming a second electrode on the n-type layer.
[0346] Technical Solution B10 According to the manufacturing method of the solar cell described in technical solution B9, the average thickness of Cu deposited on the layer mainly composed of the cuprous oxide compound is 0.02 nm or more and 0.08 nm or less.
[0347] Technical Solution B11 According to the manufacturing method of the solar cell described in technical solution B9 or B10, the surface temperature of the layer mainly composed of cuprous oxide compound during Cu deposition is above 100°C and below 350°C.
[0348] Technical Solution B12 According to the manufacturing method of the solar cell described in any of technical solutions B9 to B11, the surface temperature of the layer mainly composed of cuprous oxide compound during Cu deposition is above 150°C and below 300°C.
[0349] Technical Solution B13 According to any one of technical solutions B9 to B12, in the method for manufacturing a solar cell, the deposited Cu diffuses inside the layer mainly composed of cuprous oxide compound, forming a depression on the surface of the p-type light-absorbing layer.
[0350] Technical Solution B14 According to the manufacturing method of the solar cell described in technical solution B13, the maximum diameter of the recess is more than 15 nm and less than 80 nm.
[0351] Technical Solution B15 According to the manufacturing method of the solar cell described in technical solution B13 or B14, the maximum diameter of the recess is 15 nm or more and 80 nm or less.
[0352] Technical Solution B16 According to any one of technical solutions B13 to B15, the method for manufacturing a solar cell is wherein the depth of the recess is more than 15 nm and less than 80 nm.
[0353] Technical Solution B17 According to any one of technical solutions B13 to B16, the manufacturing method of a solar cell, wherein the density of the recesses is more than 1 and less than 250 within a 500nm × 500nm square area.
[0354] Technical Solution B18 According to any one of the technical solutions B13 to B17, the manufacturing method of a solar cell, wherein the density of the recesses is more than 10 and less than 200 within a 500nm × 500nm square area.
[0355] Technical Solution B19 A multi-junction solar cell that uses the solar cell described in any one of technical solutions B1 to B8.
[0356] Technical Solution B20 A solar cell module that uses the solar cell described in any one of technical solutions B1 to B8.
[0357] Technical Solution B21 A solar power generation system that uses the solar cell module described in technical solution B20 to generate electricity.
[0358] Technical solution C1 A solar cell comprising: First electrode, p-type light-absorbing layer on the first electrode, The first n-type layer on the p-type light absorption layer, The second n-type layer on the first n-type layer, and The second electrode on the second n-type layer The band gap of the first n-type layer is smaller than the band gap of the p-type light-absorbing layer.
[0359] Technical solution C2 In the solar cell described in technical solution C1, the band gap of the second n-type layer is larger than the band gap of the first n-type layer. The band gap of the second n-type layer is larger than that of the p-type light-absorbing layer. Technical solution C3 According to the solar cell described in technical solution C1 or C2, the difference between the band gap of the first n-type layer and the band gap of the p-type light-absorbing layer is greater than 0.05 eV and less than 0.60 eV.
[0360] Technical solution C4 According to the solar cell described in technical solution C3, the difference between the band gap of the first n-type layer and the band gap of the second n-type layer is greater than 3.0 eV and less than 4.8 eV.
[0361] Technical solution C5 According to any one of technical solutions C2 to C4, the difference between the band gap of the p-type light-absorbing layer and the band gap of the second n-type layer is greater than 2.4 eV and less than 4.2 eV.
[0362] Technical solution C6 According to any one of technical solutions C3 to C5, the band gap of the first n-type layer is above 1.4 eV and below 2.1 eV. The band gap of the p-type light-absorbing layer is above 1.6 eV and below 2.4 eV.
[0363] Technical solution C7 According to any one of the technical solutions C1 to C6, the difference between the band gap of the first n-type layer and the band gap of the p-type light-absorbing layer is greater than 0.10 eV and less than 0.55 eV.
[0364] Technical solution C8 According to any one of the technical solutions C1 to C7, the solar cell wherein the first n-type layer comprises Cu3N, amorphous silicon, or CdTe.
[0365] Technical solution C9 According to any one of the technical solutions C1 to C8, the carrier concentration of the first n-type layer is higher than that of the second n-type layer.
[0366] Technical solution C10 According to any one of the technical solutions C1 to C9, the solar cell wherein the p-type light-absorbing layer comprises a cuprous oxide compound or a compound having a chalcopyrite-type structure.
[0367] Technical solution C11 According to any one of technical solutions C1 to C10, in the solar cell, the p-type light-absorbing layer comprises a cuprous oxide compound, and the first n-type layer comprises Cu3N. The p-type light-absorbing layer comprises a cuprous oxide compound, and the first n-type layer comprises amorphous silicon, or The p-type light-absorbing layer contains a chalcopyrite-type compound of the I-III-VI2 system containing Cu, and the first n-type layer contains CdTe.
[0368] Technical solution C12 According to any one of the technical solutions C1 to C11, the thickness of the first n-type layer is more than 1 nm and less than 50 nm.
[0369] Technical solution C13 According to any one of technical solutions C1 to C12, the thickness of the first n-type layer is more than 2 nm and less than 40 nm. The thickness of the first n-type layer is thinner than the thickness of the second n-type layer.
[0370] Technical solution C14 A multi-junction solar cell uses the solar cell described in any one of technical solutions C1 to C13.
[0371] Technical solution C15 A solar cell module that uses the solar cell described in any one of technical solutions C1 to C13.
[0372] Technical solution C16 A solar power generation system that uses the solar cell module described in technical solution C1 to generate electricity.
Claims
1. A solar cell, comprising: First electrode, p-type light-absorbing layer on the first electrode, The n-type layer on the p-type light-absorbing layer, and The second electrode on the n-type layer, When the photoluminescence spectrum of the p-type light-absorbing layer is measured at temperatures below 100K, The first region is defined as the area extending from the surface of the p-type light-absorbing layer on the n-type layer side towards the first electrode side to a depth of 100 nm. The second region is defined as the area extending from the center of the p-type light-absorbing layer in the thickness direction toward the first electrode side to a depth of 100 nm. The highest value of the luminous intensity in the wavelength range of the first region (above 900 nm and below 950 nm) is more than 0 times and less than 2 times the highest value of the luminous intensity in the wavelength range of the second region (above 900 nm and below 950 nm).
2. The solar cell according to claim 1, wherein, The p-type light-absorbing layer is mainly composed of cuprous oxide compounds. The p-type light-absorbing layer, mainly composed of the cuprous oxide compound, contains one or more first elements selected from Zn, Mg, Li, Na, K, Rb, Cs, Be, Ca, Sr, and Ba on the n-type layer side. The third region is defined as the area extending 1 μm from the surface of the p-type light-absorbing layer on the n-type layer side toward the first electrode side. The concentration of the first element contained in the third region is more than 90 atomic% and less than 100 atomic% of the first element contained in the p-type light-absorbing layer.
3. The solar cell according to claim 1, wherein, The p-type light-absorbing layer is mainly composed of cuprous oxide compounds. Surface resistivity of the first region (Ω / cm) 2 The surface resistivity of the second region is Ω / cm 2 More than 0.3 times and less than 10,000 times.
4. The solar cell according to claim 2, wherein, The p-type light-absorbing layer is mainly composed of cuprous oxide compounds. The fourth region is defined as the area extending from the surface of the p-type light-absorbing layer on the n-type layer side towards the first electrode side to a depth of 50 nm. The concentration of the first element contained in the fourth region is more than 30 atomic% and less than 80 atomic% of the first element contained in the p-type light-absorbing layer.
5. The solar cell according to claim 1, wherein, The p-type light-absorbing layer is mainly composed of cuprous oxide compounds. The carrier concentration in the first region is 1×10 11 cm -3 Above and 1×10 15 cm -3 the following, The carrier concentration in the second region is 1×10 12 cm -3 Above and 1×10 15 cm -3 the following.
6. The solar cell according to claim 1, wherein, The p-type light-absorbing layer is mainly composed of cuprous oxide compounds. The carrier concentration in the first region is 1×10 11 cm -3 Above and 3×10 14 cm -3 the following, The carrier concentration in the second region is 1×10 13 cm -3 Above and 7.5×10 14 cm -3 the following, The carrier concentration in the first region is more than 0.0001 times and less than 3 times the carrier concentration in the second region.
7. The solar cell according to claim 1, wherein, The wavelength range above 900nm and below 950nm is defined as the first wavelength region. The wavelength range above 600nm and below 650nm is designated as the second wavelength region. The ratio of ([the highest value of luminous intensity in the first wavelength region of the first region] × [the highest value of luminous intensity in the second wavelength region of the second region]) / ([the highest value of luminous intensity in the second wavelength region of the first region] × [the highest value of luminous intensity in the first wavelength region of the second region]) is greater than 0 and less than 20.
8. The solar cell according to claim 1, wherein, The p-type light-absorbing layer is polycrystalline.
9. The solar cell according to claim 2, wherein, The p-type light-absorbing layer is a polycrystalline form of cuprous oxide compound. The first element is present in the grain boundaries contained in the first region.
10. The solar cell according to claim 1, wherein, The p-type light-absorbing layer is mainly composed of cuprous oxide compounds. It also contains crystals of cuprous oxide compounds with a particle size that is more than 5 times the thickness of the p-type light-absorbing layer.
11. The solar cell according to claim 1, wherein, The first electrode is a transparent electrode. The second electrode is a transparent electrode.
12. The solar cell according to claim 1, wherein, The thickness of the p-type light-absorbing layer is greater than 500 nm and less than 10 μm.
13. A solar cell, comprising: First electrode, p-type light-absorbing layer on the first electrode, The n-type layer on the p-type light-absorbing layer, and The second electrode on the n-type layer, The surface of the p-type light-absorbing layer on the n-type layer side has a depression.
14. The solar cell according to claim 13, wherein, The maximum diameter of the depression is greater than 15 nm and less than 80 nm.
15. The solar cell according to claim 13, wherein, The depth of the depression is greater than 20 nm and less than 70 nm.
16. A solar cell comprising: First electrode, p-type light-absorbing layer on the first electrode, The first n-type layer on the p-type light absorption layer, The second n-type layer on the first n-type layer, and The second electrode on the second n-type layer The band gap of the first n-type layer is smaller than the band gap of the p-type light-absorbing layer.
17. The solar cell according to claim 16, wherein, The band gap of the second n-type layer is larger than that of the first n-type layer. The band gap of the second n-type layer is larger than that of the p-type light-absorbing layer. The difference between the band gap of the first n-type layer and the band gap of the p-type light-absorbing layer is greater than 0.05 eV and less than 0.60 eV.
18. A multijunction solar cell using the solar cell of claim 1.
19. A solar cell module that uses the solar cell of claim 1.
20. A solar power generation system that generates electricity using the solar cell module of claim 19.