A method for fabricating silicon heterojunction solar cells based on laser crystallization and low-temperature ion implantation, and the silicon heterojunction solar cells.

By employing excimer laser crystallization and low-temperature ion implantation techniques, combined with an IGZO buffer layer, the problems of low carrier mobility and high contact resistance in HJT cells were solved, achieving efficient low-temperature processing and high photoelectric conversion efficiency.

CN123124491APending Publication Date: 2026-11-17CANNNOVATION LOW CARBON NEW ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611359154.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing HJT battery fabrication technologies suffer from low carrier mobility, high doping process temperatures, and high contact resistance between the TCO and the silicon substrate, which limits the improvement of battery performance.

Method used

By employing excimer laser crystallization and low-temperature ion implantation, a microcrystalline silicon layer is formed on the surface of a silicon wafer, and IGZO is used as a buffer layer. Combined with low-temperature ion implantation and laser annealing, a high-quality PN junction and low contact resistance are formed.

Benefits of technology

It significantly improves carrier mobility, reduces contact resistance, enables efficient low-temperature processing, and enhances the photoelectric conversion efficiency and industrialization potential of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124491A_ABST
    Figure CN123124491A_ABST
Patent Text Reader

Abstract

This invention discloses a silicon heterojunction solar cell based on laser crystallization and low-temperature ion implantation, and its fabrication method, belonging to the field of solar cell manufacturing technology. The invention involves sequentially depositing an intrinsic amorphous silicon passivation first layer and an intrinsic amorphous silicon second layer on both sides of an N-type silicon wafer. An excimer laser is then used to crystallize the intrinsic amorphous silicon second layer, transforming it into a microcrystalline silicon structure, followed by hydrogen passivation to repair grain boundary defects. Subsequently, an IGZO buffer layer is deposited, and then low-temperature ion implantation allows dopant ions to penetrate the IGZO layer and implant into the microcrystalline silicon layer to form a heavily doped region. Low-temperature laser annealing is then used to activate the dopant ions. Finally, a transparent conductive layer is deposited and metal electrodes are printed. This invention increases the electron mobility of microcrystalline silicon to 50–100 cm² / V·s, achieves high-quality PN junction fabrication at temperatures not exceeding 450°C, and reduces the contact resistivity to below 1 mΩ·cm², making it suitable for the large-scale production of high-efficiency silicon heterojunction solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solar cell manufacturing technology, specifically relating to a method for preparing silicon heterojunction cells based on laser crystallization and low-temperature ion implantation, and the silicon heterojunction cell itself. Background Technology

[0002] Silicon heterojunction (HJT) cells, due to their excellent surface passivation and high open-circuit voltage, have become one of the mainstream technologies for next-generation high-efficiency crystalline silicon cells. For example... Figure 1 As shown, conventional HJT cells currently mainly use plasma-enhanced chemical vapor deposition (PECVD) to deposit amorphous silicon (a-Si:H) thin films on both sides of an N-type silicon wafer, where intrinsic amorphous silicon serves as a passivation layer and doped amorphous silicon serves as the emitter and back field.

[0003] However, existing HJT battery fabrication technology suffers from the following insurmountable drawbacks:

[0004] 1. Extremely low carrier mobility: The atomic arrangement of amorphous silicon thin films deposited by PECVD is in a short-range ordered and long-range disordered state, and the electron mobility is usually less than 1 cm² / Vs, resulting in a large lateral transport resistance of the battery, which severely restricts the further improvement of the fill factor (FF).

[0005] 2. Excessive doping temperature: To achieve efficient doping of amorphous silicon layers, traditional processes often require high-temperature diffusion (>600℃) or in-situ heavy doping during deposition. However, high temperatures can damage the passivation properties of intrinsic amorphous silicon, increase the interface state density (Dit), and exacerbate carrier recombination losses.

[0006] 3. High contact resistance between transparent conductive layer (TCO) and silicon substrate: TCO (such as ITO, AZO) is directly deposited on amorphous silicon layer. There is a large barrier height at the interface between the two, resulting in high contact resistivity and affecting the overall photoelectric conversion efficiency.

[0007] Therefore, there is an urgent need to develop a method for fabricating silicon heterojunction solar cells that can simultaneously achieve a high mobility transport layer, a high-quality PN junction, and low contact resistance under low-temperature conditions. Summary of the Invention

[0008] This invention provides a method for preparing silicon heterojunction solar cells based on laser crystallization and low-temperature ion implantation, as well as the silicon heterojunction solar cells themselves. This method eliminates the need for high-temperature furnace tube annealing, significantly improves the electron mobility of the prepared microcrystalline silicon thin films, and effectively reduces the contact resistance.

[0009] To achieve the above objectives, the present invention adopts the following technical solution:

[0010] A method for fabricating silicon heterojunction solar cells based on laser crystallization and low-temperature ion implantation includes the following steps:

[0011] S1: The intrinsic amorphous silicon deposited on the front and back surfaces of a silicon wafer is crystallized using an excimer laser to transform it into microcrystalline silicon (μc-Si).

[0012] S2: An IGZO (indium gallium zinc oxide) thin film is deposited on the microcrystalline silicon layer after crystallization on both sides as an intermediate buffer layer; the IGZO layer serves as a buffer layer for carrier transport, taking into account both high transmittance (visible light region >85%) and lateral conductivity.

[0013] S3: A penetrating low-temperature ion implantation method is used to penetrate the IGZO layer to form a P+ heavily doped region in the front microcrystalline silicon layer, forming a PN junction with the N-type silicon substrate; and to penetrate the IGZO layer to form an N+ heavily doped region in the back microcrystalline silicon layer, forming a high-low junction (same-type high-low doped junction) with the N-type substrate; after implantation, annealing is performed to activate the implanted dopants and repair the lattice damage caused by implantation.

[0014] S4: Deposit conductive layers on both sides;

[0015] S5: Prepare metal electrodes on both sides to obtain a silicon heterojunction cell.

[0016] In the steps described above, S1 involves pre-treating the silicon wafer to form a pyramid light-trapping structure on the wafer surface to enhance the incident light capture efficiency. Then, two intrinsic amorphous silicon layers (ia-Si) are deposited on the front and back sides of the silicon wafer, respectively. The inner intrinsic amorphous silicon layer is not doped and serves only as a high-quality chemical passivation layer to reduce the dangling bond density on the silicon substrate surface. The outer intrinsic amorphous silicon layer serves as a precursor layer for subsequent laser crystallization.

[0017] The crystallization process of S1 is performed on the outer intrinsic amorphous silicon layer; the crystallization process is performed using an excimer laser with a wavelength of 308 nm (XeCl), a pulse width of less than 50 ns, and a laser energy density set to 200~400 mJ / cm². 2 The overlap rate of light spots is 30%~50%;

[0018] After crystallization, the temperature of the reaction chamber is reduced to 200~300℃, and high-purity hydrogen is introduced for in-situ plasma hydrogen passivation treatment for 5~15 minutes. The dangling bonds at the grain boundaries of hydrogen-saturated microcrystalline silicon are used to ensure that the crystallized film still has good interface passivation performance.

[0019] In S2, magnetron sputtering is used for deposition, with the thickness controlled at 10~30nm and the Ar / O2 flow ratio controlled at 20:1 to 30:1.

[0020] Boron (B) is injected into S3 from the front. + ) or boron trifluoride (BF2) + Phosphorus (P) ions, with phosphorus (P) implanted on the back side.+ Ions; after implantation, annealing is performed at a temperature of 350~450℃ for 1~5 minutes to activate the implanted doped ions and repair the lattice damage caused by implantation, while avoiding high temperature damage to IGZO and passivation layer.

[0021] Beneficial effects: This invention provides a method for fabricating silicon heterojunction solar cells based on laser crystallization and low-temperature ion implantation, and the silicon heterojunction solar cell itself, which has the following advantages compared with the prior art:

[0022] 1. This invention utilizes the high single-photon energy of an excimer laser (308nm XeCl) to melt and rapidly recrystallize amorphous a-Si within nanoseconds, forming a microcrystalline silicon structure containing nanoscale grains, significantly improving the atomic arrangement order. After crystallization, hydrogen gas is introduced for plasma hydrogen passivation, dangling bonds at saturated grain boundaries. The electron mobility of the prepared microcrystalline silicon thin film is increased from <1cm² / Vs to 50~100 cm² / Vs. 2 / Vs, significantly reducing lateral transport resistance; hydrogen passivation repairs defects, maintaining the interface state density (Dit) at 10. 10 cm -2 eV -1 The magnitude is such that the passivation effect does not need to be sacrificed;

[0023] 2. This invention employs an integrated process of "penetrating low-temperature ion implantation + laser-induced annealing," controlling the energy of dopant ions (B implanted on the front and P implanted on the back) at a low level (10~30keV), allowing them to penetrate the surface-deposited IGZO buffer layer and be implanted at the microcrystalline silicon / monocrystalline silicon interface; subsequently, rapid annealing is performed, with the temperature strictly controlled at 350~450℃, eliminating the need for high-temperature furnace tube annealing and completely avoiding thermal damage to the bottom passivation layer and the top TCO; thus achieving high-quality PN junction fabrication under low-temperature (<450℃) conditions;

[0024] 3. This invention introduces high carrier concentration IGZO (indium gallium zinc oxide) as an intermediate buffer layer. During ion implantation, a small number of ions bombarding the IGZO layer will generate oxygen vacancies, naturally increasing the carrier concentration of the IGZO (>10). 20 cm -3 This allows it to form a good tunneling ohmic contact with microcrystalline silicon, effectively reducing the contact resistivity (ρc) to <1 mΩ·cm. 2 This improved the battery fill factor (FF) and short-circuit current (Jsc).

[0025] 4. Good process compatibility. The overall process temperature of this invention does not exceed 450℃, which is fully compatible with the low-temperature process route of HJT batteries. It can be upgraded and transformed on the basis of existing HJT production lines by adding laser crystallization and ion implantation modules, and has good industrialization prospects. Attached Figure Description

[0026] Figure 1 This is a schematic diagram of an existing heterojunction battery structure in the prior art;

[0027] Figure 2 This is a schematic diagram of the improved heterojunction battery structure of the present invention;

[0028] Figure 3 This is a schematic diagram of the crystallization process in an embodiment of the present invention. Detailed Implementation

[0029] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments:

[0030] A method for fabricating silicon heterojunction solar cells based on laser crystallization and low-temperature ion implantation specifically includes the following steps:

[0031] Step 1: Silicon substrate preparation and pre-cleaning

[0032] We provide N-type monocrystalline silicon wafers (thickness 130~180μm, resistivity 1~10 Ω·cm), which undergo standard RCA cleaning and surface texturing to form a pyramid light-trapping structure on the silicon wafer surface to enhance the incident light capture efficiency.

[0033] Step 2: Deposition of intrinsic amorphous silicon (ia-Si) passivation layer

[0034] Using PECVD, intrinsic amorphous silicon layer 1 (ia-Si) is deposited on both sides of a silicon wafer, with a thickness strictly controlled between 5 and 10 nm. Then, another 5-10 nm intrinsic amorphous silicon layer 2 (ia-Si) is deposited on top of the intrinsic amorphous silicon layer 1 on both sides. The intrinsic amorphous silicon layer 1 is not doped and serves solely as a high-quality chemical passivation layer to reduce the dangling bond density on the silicon substrate surface (target interface state density Dit < 5 × 10⁻⁶). 10 cm -2 eV -1 ).

[0035] Step 3: Excimer laser crystallization and hydrogen passivation

[0036] The intrinsic amorphous silicon layer 2 on both sides was scanned and irradiated using an excimer laser (wavelength 308 nm, pulse width < 50 ns). The laser energy density was set to 200–400 mJ / cm². 2 The overlap rate of light spots is 30%~50%.

[0037] like Figure 3 As shown, the intrinsic amorphous silicon layer 2 (ia-Si) melts and recrystallizes instantaneously after being irradiated by laser, transforming from a disordered amorphous state into a microcrystalline silicon (μc-Si) structure containing fine grains (while still maintaining its intrinsic conductivity type).

[0038] After crystallization, the temperature of the reaction chamber is lowered to 200~300℃, and high-purity hydrogen gas (H2) is introduced for in-situ plasma hydrogen passivation treatment for 5~15 minutes. By utilizing the dangling bonds at the grain boundaries of hydrogen-saturated microcrystalline silicon, the crystallized film still has good interface passivation performance.

[0039] Step 4: Deposition of IGZO buffer layer

[0040] Using magnetron sputtering (RF power supply, power density 2~5 W / cm²) 2 An IGZO (indium gallium zinc oxide) thin film is deposited on a microcrystalline silicon layer after crystallization on both sides, with the thickness controlled at 10~30nm and the Ar / O2 flow ratio controlled at 20:1 to 30:1. This IGZO layer serves as a buffer layer for carrier transport, taking into account both high transmittance (visible light region >85%) and lateral conductivity.

[0041] Step 5: Low-temperature ion implantation penetration doping and laser annealing

[0042] An ion implanter was used, with the implantation energy set to 10-30 keV (sufficient to penetrate the IGZO layer in step 4, controlled within the shallow junction range on the silicon substrate surface), and the implantation dose controlled at 1×10⁻⁶. 15 ~ 5×10 15 ions / cm 2 .

[0043] Frontal implantation: implanted boron (B + ) or boron trifluoride (BF2) + The ions penetrate the IGZO layer, forming a P+ heavily doped region on the front microcrystalline silicon layer, and forming a PN junction with the N-type substrate.

[0044] Backside injection: Injection of phosphorus (P) + The N+ ions penetrate the IGZO layer and form an N+ heavily doped region on the back microcrystalline silicon layer, forming a high-low junction (homogeneous high-low doped junction) with the N-type substrate.

[0045] After injection, the low-power output mode (energy density <150 mJ / cm²) of the excimer laser from step 3 is used. 2 Large-area scanning can be performed, or rapid thermal annealing (RTA) can be performed using residual heat from the cavity. The annealing temperature is controlled at 350~450℃ for 1~5 minutes to activate the implanted dopant ions and repair the lattice damage caused by the implantation, while avoiding high temperature damage to IGZO and passivation layer.

[0046] Step 6: Deposition of Transparent Conductive Layer (TCO)

[0047] ITO (indium tin oxide) or AZO (aluminum-doped zinc oxide) thin films were deposited on both sides using magnetron sputtering, with a thickness of 70–100 nm and a sheet resistance of <30 Ω / sq, serving as the electrode collection layer for the battery. This TCO layer has a wide bandgap (approximately 3.5–4.3 eV) and high transmittance in the visible light region.

[0048] Step 7: Screen printing and low-temperature sintering

[0049] Low-temperature silver paste grid line electrodes are printed on both sides using screen printing. The electrodes are then sintered in a sintering furnace at 200~250℃ for 30 minutes to form metal electrodes with good ohmic contact, thus completing the fabrication of silicon heterojunction solar cells.

[0050] Example 1:

[0051] This embodiment provides a method for fabricating silicon heterojunction solar cells based on laser crystallization and low-temperature ion implantation. The specific steps are as follows:

[0052] (1) Silicon substrate preparation and pre-cleaning: Provide an N-type single crystal silicon wafer with a thickness of 150 μm and a resistivity of 3 Ω·cm. Perform standard RCA cleaning and surface texturing to form a pyramid light trapping structure on the silicon wafer surface. The pyramid size is 3 to 8 μm.

[0053] (2) Deposition of intrinsic amorphous silicon passivation layer: Using PECVD, an intrinsic amorphous silicon first layer (ia-Si) with a thickness of 7nm is deposited on the front and back sides of the silicon wafer as a chemical passivation layer; then an intrinsic amorphous silicon second layer (ia-Si) with a thickness of 50nm is deposited on the intrinsic amorphous silicon first layer on the front and back sides as a precursor layer for subsequent laser crystallization; PECVD process parameters: substrate temperature 200℃, SiH4 flow rate 20sccm, H2 flow rate 200sccm, power 20W, pressure 0.5Torr.

[0054] (3) Excimer laser crystallization and hydrogen passivation: The intrinsic amorphous silicon second layer on both sides was scanned and irradiated using a XeCl excimer laser (wavelength 308 nm, pulse width 25 ns). The laser energy density was 300 mJ / cm², the spot overlap rate was 40%, and the scanning speed was 10 mm / s. After laser irradiation, the intrinsic amorphous silicon second layer melted and recrystallized instantly, transforming from a disordered amorphous state into a microcrystalline silicon (μc-Si) structure containing nanoscale grains (grain size approximately 10–50 nm). After crystallization, the temperature of the reaction chamber was lowered to 250 °C, and high-purity hydrogen gas (flow rate 100 sccm) was introduced for 10 minutes of in-situ plasma hydrogen passivation treatment (power 50 W), utilizing the dangling bonds at the grain boundaries of the hydrogen-saturated microcrystalline silicon.

[0055] (4) IGZO buffer layer deposition: An IGZO thin film with a thickness of 20 nm was deposited on the microcrystalline silicon layer after crystallization on both sides using magnetron sputtering (RF power supply, power density 3 W / cm²), with an Ar / O2 flux ratio of 25:1 and a substrate temperature of room temperature. The visible light transmittance of this IGZO layer is >88%.

[0056] (5) Low-temperature ion implantation penetration doping and laser annealing: An ion implanter was used, with an implantation energy of 15 keV and an implantation dose of 3 × 10⁻⁶. 15 ions / cm 2 Frontal injection of B + Ions are implanted to penetrate the IGZO layer (20 nm) and form a heavily P+ doped region (junction depth approximately 30–50 nm) in the front-side microcrystalline silicon layer, forming a PN junction with the N-type substrate; P+ is implanted on the back side. + Ions are introduced to penetrate the IGZO layer and form an N+ heavily doped region in the back microcrystalline silicon layer.

[0057] After implantation, large-area scanning annealing was performed using the same excimer laser in low-power output mode (energy density 100 mJ / cm²) at a temperature of approximately 400°C for 3 minutes to activate the implanted dopant ions and repair the lattice damage caused by implantation, while avoiding high-temperature damage to the IGZO and passivation layer.

[0058] (6) Deposition of transparent conductive layer: ITO thin film with a thickness of 85 nm and a sheet resistance of about 20 Ω / sq is deposited on the front and back sides by magnetron sputtering, which serves as the electrode collection layer of the battery.

[0059] (7) Screen printing and low-temperature sintering: Low-temperature silver paste grid line electrodes (main grid line width 1.5 mm, fine grid line width 40 μm, spacing 1.5 mm) are printed on the front and back sides by screen printing. The electrodes are then placed in a sintering furnace at 220°C for 30 minutes to form metal electrodes with good ohmic contact, thus completing the preparation of silicon heterojunction cells.

[0060] Example 2

[0061] This embodiment is basically the same as Embodiment 1, except that the laser energy density in step (3) is 250 mJ / cm². 2 The spot overlap rate is 35%; in step (5), the ion implantation energy is 10 keV and the implantation dose is 2 × 10⁻⁶. 15 ions / cm 2 The annealing method was rapid thermal annealing (RTA) at a temperature of 380°C for 5 minutes. All other process parameters were the same as in Example 1.

[0062] Example 3

[0063] This embodiment is basically the same as Embodiment 1, except that: the thickness of the intrinsic amorphous silicon second layer in step (2) is 30 nm; and the laser energy density in step (3) is 350 mJ / cm². 2 The spot overlap rate is 45%, and the hydrogen passivation time is 8 minutes; the IGZO film thickness in step (4) is 15 nm; the ion implantation energy in step (5) is 20 keV, and the implantation dose is 4 × 10⁻⁶. 15 ions / cm 2 BF2 injected from the front + Ions. The remaining process parameters are the same as in Example 1.

[0064] Comparative Example 1 (Traditional HJT process)

[0065] Prepared using traditional PECVD method, such as Figure 1 The HJT cell shown is constructed as follows: After depositing intrinsic amorphous silicon passivation layers (7nm) on both sides of an N-type silicon wafer, a P-type doped amorphous silicon emitter (10nm) is deposited on the front side, and an N-type doped amorphous silicon back field (10nm) is deposited on the back side at a deposition temperature of 200℃. Subsequently, an ITO transparent conductive layer (85nm) is directly deposited, and a low-temperature silver paste electrode is screen-printed. The wafer is then sintered at 220℃ for 30 minutes. Laser crystallization, hydrogen passivation, IGZO buffer layer deposition, and ion implantation processes are not performed.

[0066] Comparative Example 2 (without laser crystallization)

[0067] The process is basically the same as in Example 1, except that the excimer laser crystallization process in step (3) is not performed, the intrinsic amorphous silicon second layer remains amorphous, and the remaining steps are the same as in Example 1.

[0068] Comparative Example 3 (without IGZO buffer layer)

[0069] The process is basically the same as in Example 1, except that: step (4) of depositing the IGZO buffer layer is not performed, ion implantation is directly applied to the surface of the microcrystalline silicon layer, and TCO is directly deposited on the microcrystalline silicon layer. The remaining steps are the same as in Example 1.

[0070] Performance Testing and Comparison

[0071] The battery samples prepared in Example 1 and Comparative Examples 1-3 were tested under standard test conditions (AM 1.5G, 100mW / cm²). 2 Photoelectric performance tests were conducted at 25°C. Battery samples prepared in Example 1, Comparative Example 1 (conventional HJT), Comparative Example 2 (without laser crystallization), and Comparative Example 3 (without IGZO buffer layer) were placed under standard test conditions (AM1.5G, 100mW / cm²). 2The tests were conducted at 25℃, and the thin film electron mobility, contact resistivity ρc, open circuit voltage Voc, short circuit current density Jsc, fill factor FF, and photoelectric conversion efficiency η were measured respectively. The experimental results are shown in Table 1.

[0072] Table 1. Comparison of photoelectric performance test results of battery samples prepared in the examples and comparative examples.

[0073] sample Electron mobility cm² / (V⋅s) <![CDATA[Contact resistivity mΩ·cm 2 > Voc (V) <![CDATA[Jsc (mA / cm 2 )]]> FF (%) Conversion efficiency η (%) Example 1 72 0.72 0.742 41.30 84.1 25.75 Comparative Example 1 0.75 3.85 0.734 40.22 78.3 23.03 Comparative Example 2 0.82 2.94 0.736 40.41 79.2 23.46 Comparative Example 3 70 2.77 0.738 40.65 80.4 24.13

[0074] In summary, this invention effectively solves the technical problems of low mobility, high doping temperature, and high contact resistance in existing HJT cells through the synergistic effect of three core technologies: excimer laser crystallization and hydrogen passivation, penetrating low-temperature ion implantation and laser annealing, and IGZO buffer layer. It significantly improves the photoelectric conversion efficiency of the cells and has important industrial application value.

[0075] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for fabricating silicon heterojunction solar cells based on laser crystallization and low-temperature ion implantation, characterized in that, Includes the following steps: S1: Crystallize the intrinsic amorphous silicon deposited on the front and back surfaces of the silicon wafer substrate to transform it into microcrystalline silicon; S2: Deposit an indium gallium zinc oxide thin film as an intermediate buffer layer on the microcrystalline silicon layer after crystallization on both sides; S3: Using a penetrating low-temperature ion implantation method, a P+ heavily doped region is formed in the front microcrystalline silicon layer through the IGZO layer, forming a PN junction with the N-type silicon substrate; an N+ heavily doped region is formed in the back microcrystalline silicon layer through the IGZO layer, forming a high-low junction with the N-type substrate. After implantation, annealing is performed to activate the implanted dopant ions and repair the lattice damage caused by implantation. S4: Deposit conductive layers on both sides; S5: Prepare metal electrodes on both sides to obtain a silicon heterojunction cell.

2. The method for fabricating silicon heterojunction solar cells based on laser crystallization and low-temperature ion implantation according to claim 1, characterized in that, Crystallization was performed using an excimer laser with a wavelength of 308 nm, a pulse width of less than 50 ns, a laser energy density of 200~400 mJ / cm², and a spot overlap rate of 30%~50%.

3. The method for fabricating silicon heterojunction solar cells based on laser crystallization and low-temperature ion implantation according to claim 1 or 2, characterized in that, After crystallization, the temperature of the reaction chamber is lowered to 200-300℃, and high-purity hydrogen is introduced for in-situ plasma hydrogen passivation treatment for 5-15 minutes.

4. The method for fabricating silicon heterojunction solar cells based on laser crystallization and low-temperature ion implantation according to claim 1, characterized in that, In S2, magnetron sputtering is used for deposition, with the thickness controlled at 10~30nm and the Ar / O2 flow ratio controlled at 20:1 to 30:

1.

5. The method for fabricating silicon heterojunction solar cells based on laser crystallization and low-temperature ion implantation according to claim 1, characterized in that, In S3, boron or boron trifluoride ions are implanted on the front side, and phosphorus ions are implanted on the back side.

6. The method for fabricating silicon heterojunction solar cells based on laser crystallization and low-temperature ion implantation according to claim 1, characterized in that, After injection, the annealing temperature is controlled at 350~450℃ for 1~5 minutes.

7. The method for fabricating silicon heterojunction solar cells based on laser crystallization and low-temperature ion implantation according to claim 1, characterized in that, Before S1, the silicon wafer is pretreated to form a pyramid light-trapping structure on the surface of the silicon wafer to enhance the capture efficiency of incident light. Then, two intrinsic amorphous silicon layers are deposited on the front and back sides of the silicon wafer respectively. The inner intrinsic amorphous silicon layer is not doped and serves only as a high-quality chemical passivation layer to reduce the dangling bond density on the silicon substrate surface. The outer intrinsic amorphous silicon layer serves as a precursor layer for subsequent laser crystallization.

8. A silicon heterojunction solar cell, characterized in that, The substrate includes an N-type monocrystalline silicon substrate. On the front side of the N-type monocrystalline silicon substrate, an intrinsic amorphous silicon passivation layer, a microcrystalline silicon layer, an IGZO buffer layer, and a transparent conductive layer are stacked sequentially from the inside out. On the back side of the N-type monocrystalline silicon substrate, an intrinsic amorphous silicon passivation layer, a microcrystalline silicon layer, an IGZO buffer layer, and a transparent conductive layer are stacked sequentially from the inside out. The microcrystalline silicon layer on the front side has a P+ heavily doped region, and the microcrystalline silicon layer on the back side has an N+ heavily doped region. Metal electrodes are disposed on the transparent conductive layers on both the front and back sides.

9. The silicon heterojunction solar cell according to claim 8, characterized in that, The intrinsic amorphous silicon passivation layer has a thickness of 5–10 nm; the microcrystalline silicon layer has a thickness of 20–80 nm and is composed of nanoscale grains with a grain size of 10–50 nm; the IGZO buffer layer has a thickness of 10–30 nm; and the transparent conductive layer has a thickness of 70–100 nm.

10. The silicon heterojunction solar cell according to claim 8 or 9, characterized in that, A tunneling ohmic contact is formed between the IGZO buffer layer and the microcrystalline silicon layer, with a contact resistivity of less than 1 mΩ·cm².