A flexible gallium arsenide solar cell with a shape memory alloy substrate and its fabrication method
By enabling the NiTi shape memory alloy substrate to actively recover its shape under temperature changes, the warping and deformation problem of flexible gallium arsenide solar cells under thermal mismatch stress was solved, thereby improving photoelectric performance and simplifying the manufacturing process.
Patent Information
- Application Number
- CN202611619850.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
The substrate of existing flexible gallium arsenide solar cells cannot actively adjust its own mechanical state when the temperature changes, which leads to thermal mismatch stress between the epitaxial layer and the flexible substrate, causing device warping and deformation, and affecting photoelectric performance.
Using a NiTi shape memory alloy substrate, the structure is designed to allow it to actively recover its shape when the temperature changes, thus offsetting thermal stress. Furthermore, by changing the Ni/Ti ratio in the substrate thickness direction, a continuous NiTi gradient layer and a Ni-rich transition layer are formed, providing a metallurgical interface and thermal buffer function.
It effectively reduces device warpage and deformation, improves photoelectric performance, simplifies the manufacturing process, reduces the impact of thermal stress on the battery, and protects the brittle gallium arsenide epitaxial layer.
Smart Images

Figure CN123124504A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor technology, specifically to a flexible gallium arsenide solar cell with a shape memory alloy substrate and its fabrication method. Background Technology
[0002] Flexible gallium arsenide (GaAs) solar cells have become the primary choice in the space energy field due to their high conversion efficiency, good flexibility, and strong radiation resistance. The integration of epitaxial thin films with flexible substrates is a core requirement. However, the thermal mismatch stress between the epitaxial layer and the flexible substrate during bonding, alloying, and the significant temperature differences during space operations can cause overall device warping and deformation, leading to a decline in photoelectric performance. Currently, mainstream flexible substrates include organic polymer substrates represented by polyimide and inorganic metal substrates represented by electroplated copper and nickel foils. Organic polymer substrates offer good flexibility and light weight, but their coefficient of thermal expansion differs significantly from that of gallium arsenide. Furthermore, the polymer itself is insulating, requiring the fabrication of a back electrode and complex processes involving through-etching. Long-term temperature cycling also presents the problem of adhesion degradation between the polymer substrate and the metal layer. Inorganic metal substrates can also serve as back electrodes, but their coefficient of thermal expansion (CTE) is typically between 15 ppm / ℃ and 20 ppm / ℃, significantly different from gallium arsenide's 5.7 ppm / ℃. This results in substantial thermal stress during cooling, which is usually mitigated by adding a silicon dioxide stress film. However, traditional back-side stress films provide fixed, static compensation. Therefore, in existing technologies, none of the aforementioned flexible substrates can actively adjust their mechanical state according to temperature changes to release the thermal mismatch stress between the epitaxial layer and the flexible substrate.
[0003] This application aims to provide a flexible gallium arsenide solar cell with a shape memory alloy substrate and its fabrication method. By utilizing the characteristic of NiTi shape memory alloy to actively recover its shape with temperature changes, and using a structurally designed NiTi shape memory alloy as a substrate, this application solves the problem in the prior art that the substrate side of flexible gallium arsenide solar cells cannot actively adjust its own mechanical state according to temperature changes to release the thermal mismatch stress between the epitaxial layer and the flexible substrate. Summary of the Invention
[0004] To address the shortcomings of existing technologies, the present invention aims to provide a flexible gallium arsenide solar cell with a shape memory alloy substrate and its fabrication method. By using a structurally designed NiTi shape memory alloy as the substrate, the flexible gallium arsenide solar cell can actively adjust its mechanical state according to temperature changes to release the thermal stress caused by temperature changes, thereby improving the overall warping deformation of the device caused by thermal mismatch stress between the epitaxial layer and the substrate, which leads to a decrease in photoelectric performance.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: This invention provides a flexible gallium arsenide solar cell with a shape memory alloy substrate, comprising a NiTi shape memory alloy substrate, a first bonding layer, a second bonding layer, and a gallium arsenide epitaxial layer stacked sequentially from bottom to top; The NiTi shape memory alloy substrate is subjected to constrained state training so that the NiTi shape memory alloy remembers the planar shape at the alloy annealing temperature as a zero-stress state; The NiTi shape memory alloy substrate includes a NiTi gradient layer and a Ni-rich transition layer stacked sequentially from bottom to top. The Ni / Ti atomic ratio in the Ni-rich transition layer is a, and the Ni / Ti atomic ratio in the NiTi gradient layer gradually changes from b to c along the thickness direction from top to bottom. The values of a and b are both selected from 45:55 to 58:42, and the value of c is 49:51 to 50:50, and a ≥ b > c.
[0006] Furthermore, in the NiTi gradient layer, the Ni / Ti atomic ratio changes linearly from b to c along the thickness direction from top to bottom, with a ranging from 56:44 to 58:42, b ranging from 55:45 to 56:44, and c ranging from 49:51 to 50:50.
[0007] Furthermore, the thickness of the Ni-rich transition layer is 0.5 μm to 5 μm, and the thickness of the NiTi graded layer is 10 μm to 30 μm.
[0008] Furthermore, the NiTi shape memory alloy substrate also includes a near-backside transition layer, the upper surface of which is in contact with the lower surface of the NiTi gradient layer, the Ni / Ti atomic ratio in the near-backside transition layer is d, d≤c, and d takes a value of 49:51 to 50:50, and the thickness of the near-backside transition layer is 4μm to 6μm.
[0009] Furthermore, the constrained state training temperature of the NiTi shape memory alloy substrate is the alloy annealing temperature of the gallium arsenide solar cell, which is 250℃~350℃.
[0010] Furthermore, the gallium arsenide solar cell also includes a back metal stack, which is stacked on the surface of the NiTi shape memory alloy substrate away from the first bonding layer; The back metal stack comprises a NiAg transition layer, an Ag solderable layer, and an Au protective layer stacked sequentially from top to bottom; the NiAg transition layer is prepared from a NiAg alloy, wherein the mass ratio of Ni to Ag in the NiAg alloy is 10:90 to 50:50, and the thickness of the NiAg transition layer is 50 nm to 150 nm; the thickness of the Ag solderable layer is 0.8 μm to 1.2 μm, and the thickness of the Au protective layer is 200 nm to 300 nm.
[0011] Furthermore, the NiTi shape memory alloy substrate also includes a Ni-rich protective layer, the upper surface of which is in contact with the lower surface of the NiTi gradient layer, the Ni / Ti atomic ratio in the Ni-rich protective layer is 58:42, and the thickness of the Ni-rich protective layer is 0.4μm to 0.6μm.
[0012] The present invention also provides a method for fabricating the above-mentioned flexible gallium arsenide solar cell on a shape memory alloy substrate, comprising the following steps: S1. On the surface of the glass temporary carrier, a Ti adhesion layer, an Au protective layer, an Ag solderable layer and a NiAg transition layer are sequentially vapor-deposited. S2. A NiTi gradient layer and a Ni-rich transition layer are sequentially deposited on the surface of the NiAg transition layer using Ni and Ti dual-target co-sputtering. After deposition, constrained state training is performed at the gallium arsenide solar cell alloy annealing temperature to obtain a NiTi shape memory alloy substrate. The first bonding layer is then prepared on the surface of the NiTi shape memory alloy substrate. The constrained state training method involves fixing the prepared NiTi shape memory alloy substrate with a glass temporary carrier on a planar fixture, heating it to 250℃~350℃ and holding it for 1h~3h, then cooling it to room temperature, and repeating the heating and cooling process 2 to 4 times. S3. On the surface of a gallium arsenide substrate, an AlGaInP sacrificial layer, a gallium arsenide contact layer, and a gallium arsenide epitaxial layer are grown sequentially by MOCVD, and a second bonding layer is prepared on the surface of the gallium arsenide epitaxial layer. S4. Align the bonding surfaces of the first bonding layer on the NiTi shape memory alloy substrate side and the second bonding layer on the gallium arsenide epitaxial layer side, and perform wafer bonding. S5. After bonding, remove the gallium arsenide substrate and AlGaInP sacrificial layer to expose the gallium arsenide contact layer. Then, prepare the front electrode and anti-reflection film on the wafer surface after removing the gallium arsenide substrate and AlGaInP sacrificial layer. S6. The wafer prepared in S5 is subjected to alloy annealing at a temperature of 250℃~350℃. S7. Use an excimer laser to uniformly scan and irradiate the back of the glass temporary carrier. The laser passes through the glass temporary carrier, causing the Ti adhesion layer to vaporize under the laser energy. The Au protective layer, Ag solderable layer and NiAg transition layer are peeled off from the glass temporary carrier together with the NiTi shape memory alloy substrate. S8. The wafer is separated into individual battery chips using a wafer dicing machine, and then subjected to photoelectric performance testing and sorting.
[0013] Furthermore, the preparation method of the NiTi graded layer and the Ni-rich transition layer in S2 is as follows: Ni and Ti dual-target co-sputtering is used to deposit the NiTi graded layer on the surface of the NiAg transition layer. Ar atmosphere, substrate temperature 200℃~400℃, working pressure 0.3Pa~0.8Pa, initial stage control of Ni / Ti atomic ratio is c, linearly adjusted according to program to increase Ni target power and decrease Ti target power until Ni / Ti atomic ratio is b, thus completing the preparation of NiTi graded layer. Then, Ni and Ti dual-target co-sputtering is performed according to Ni / Ti atomic ratio a to complete the preparation of Ni-rich transition layer.
[0014] Furthermore, in S2, before preparing the NiTi gradient layer, a near-backside transition layer is also prepared. The near-backside transition layer is prepared by Ni and Ti dual-target co-sputtering to deposit the near-backside transition layer on the surface of the NiAg transition layer under Ar atmosphere, substrate temperature of 200℃~400℃, working pressure of 0.3Pa~0.8Pa, and controlling the Ni / Ti atomic ratio to d to complete the preparation of the near-backside transition layer.
[0015] Compared with the prior art, the beneficial effects of the present invention are: 1. The flexible gallium arsenide solar cell with a shape memory alloy substrate provided by this invention uses a NiTi shape memory alloy substrate as the substrate. Through training, the zero-stress state of the NiTi shape memory alloy is set at the alloy annealing temperature. When the temperature deviates from the annealing temperature, the NiTi shape memory alloy substrate actively counteracts the thermal stress through its shape memory restoring force. By continuously changing the Ni / Ti ratio in the substrate thickness direction, continuous NiTi gradient layers and Ni-rich transition layers are formed within the same thin film. The Ni-rich transition layer reduces thermal mismatch stress from the source, while utilizing Ni's oxidation resistance to protect the internal Ti from oxidation and providing a metallurgical interface for the first bonding layer. The NiTi gradient layer exhibits the strongest shape memory effect, with its restoring force automatically increasing with the degree of temperature deviation from the annealing temperature, dynamically canceling out the thermal mismatch warping force and improving the overall device warping deformation caused by thermal mismatch stress between the epitaxial layer and the substrate. Furthermore, the NiTi shape memory alloy substrate slows down the cooling / heating rate of the cell through phase transition heat absorption / release, forming a thermal buffer function, reducing the impact of drastic temperature differences on the solar cell device, and helping to protect the brittle gallium arsenide epitaxial layer.
[0016] 2. The fabrication method of the flexible gallium arsenide solar cell with shape memory alloy substrate provided in this application allows the NiTi shape memory alloy substrate to simultaneously perform four functions: flexible support, active stress compensation, thermal buffer, and vertical conductivity. The back metal stack solves the problem of poor solderability of NiTi shape memory alloy substrate, allowing it to be soldered to interconnect without additional processing, and simultaneously serving as the back electrode. This eliminates the need for traditional back stress film setup, simplifying the device structure, and eliminates the need for through-etching, simplifying the fabrication process. Attached Figure Description
[0017] The accompanying drawings, which are included to provide a further understanding of this application and form part of this application, illustrate exemplary embodiments and are used to explain this application, but do not constitute an undue limitation of this application. In the drawings: Figure 1 This is a schematic diagram showing the variation trends of Ni content, CTE, and martensitic phase transformation temperature along the thickness direction of the NiTi graded layer in some embodiments of this application; the black solid line in the figure represents the Ni content gradually increasing from the back side to the bonding surface along the thickness direction; the blue solid line represents the CTE gradually decreasing along the thickness direction and approaching GaAs; the red solid line represents the martensitic phase transformation temperature gradually decreasing from about +50°C to about -50°C along the thickness direction. Figure 2 This is a schematic diagram of the structure after the first bonding layer is prepared on a glass temporary slide, as shown in some embodiments of this application; Figure 3 This is a schematic diagram of the battery intermediate structure after bonding is completed, as shown in some embodiments of this application; Figure 4 This is a schematic diagram of the structure of a flexible gallium arsenide solar cell with a shape memory alloy substrate, as shown in some embodiments of this application. Figure 5 This is a schematic diagram of the structure after the first bonding layer is prepared on a glass temporary slide, as shown in some other embodiments of this application; Figure 6 This is a schematic diagram of the structure after the first bonding layer is prepared on a glass temporary substrate, as shown in some embodiments of this application; Figure descriptions: 1. Temporary glass substrate; 2. Backside metal stack; 3. NiTi shape memory alloy substrate; 31. NiTi gradient layer; 32. Ni-rich transition layer; 33. Near-backside transition layer; 34. Ni-rich protective layer; 4. First bonding layer; 5. Second bonding layer; 6. Gallium arsenide epitaxial layer; 7. Gallium arsenide contact layer; 8. Front electrode; 9. Anti-reflective coating. Detailed Implementation
[0018] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit this application or its application or use. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application.
[0019] Unless otherwise specifically stated, the relative arrangement, numerical expressions, and values of the components and steps described in these embodiments do not limit the scope of this application. It should also be understood that, for ease of description, the dimensions of the various parts shown in the drawings are not drawn to actual scale. Techniques, methods, and devices known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques, methods, and devices should be considered part of the specification. In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not as limitations. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters in the following drawings denote similar items; therefore, once an item is defined in one drawing, it need not be further discussed in subsequent drawings.
[0020] In the description of this application, it should be understood that the use of terms such as "first" and "second" to define components is merely for the purpose of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore should not be construed as limiting the scope of protection of this application.
[0021] In the description of this application, it should be understood that the orientation or positional relationship indicated by directional terms such as "front, back, up, down, left, right", "horizontal, vertical, horizontal" and "top, bottom" is usually based on the orientation or positional relationship shown in the accompanying drawings, and is only for the convenience of describing this application and simplifying the description. Unless otherwise stated, these directional terms do not indicate or imply that the device or element referred to must have a specific orientation or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation on the scope of protection of this application; the directional terms "inner" and "outer" refer to the inner and outer contours relative to the outline of each component itself.
[0022] The flexible gallium arsenide solar cell with a shape memory alloy substrate provided by this invention is based on the following core physical principles: NiTi shape memory alloys possess shape memory and superelasticity, enabling them to actively recover a preset shape or withstand large strains without permanent deformation in the face of temperature changes. The shape memory effect of NiTi shape memory alloys originates from the thermoelastic martensitic phase transformation. The high-temperature austenitic phase has a body-centered cubic structure with only one stable shape; the low-temperature martensitic phase has a monoclinic structure and can undergo macroscopic deformation through twin reorientation. Through constrained state training, NiTi shape memory alloys "remember" a specific shape in the austenitic state, corresponding to a zero-stress state. When the temperature drops from the austenitic region to the martensitic region, without constraint, the alloy maintains its memory shape; with constraint, the alloy generates a restoring force, directed towards the memory shape, with its magnitude increasing with the degree of constraint and temperature deviation. A core challenge of flexible gallium arsenide solar cells lies in the inability to effectively release thermal stress between the flexible substrate and the gallium arsenide epitaxial layer during temperature changes. This application utilizes the characteristic of NiTi shape memory alloys to actively recover their shape with temperature changes, addressing the need for actively mitigating thermal stress in this scenario.
[0023] The following combination Figures 1-6 The structural design of a flexible gallium arsenide solar cell with a shape memory alloy substrate provided in this application is further described. The flexible gallium arsenide solar cell includes a NiTi shape memory alloy substrate 3, a first bonding layer 4, a second bonding layer 5 and a gallium arsenide epitaxial layer 6 stacked from bottom to top. The NiTi shape memory alloy substrate 3 is subjected to constrained state training so that the NiTi shape memory alloy remembers the planar shape at the alloy annealing temperature as a zero-stress state. The NiTi shape memory alloy substrate 3 includes a NiTi gradient layer 31 and a Ni-rich transition layer 32 stacked sequentially from bottom to top. The Ni / Ti atomic ratio in the Ni-rich transition layer 32 is a, and the Ni / Ti atomic ratio in the NiTi gradient layer 31 gradually changes from b to c along the thickness direction from top to bottom. The values of a and b are both selected from 45:55 to 58:42, and the value of c is 49:51 to 50:50, and a ≥ b > c.
[0024] The flexible gallium arsenide solar cell with shape memory alloy substrate provided by the present invention uses a NiTi shape memory alloy substrate as the substrate. Through training, the zero-stress state of the NiTi shape memory alloy is set at the alloy annealing temperature. When the temperature deviates from the annealing temperature, the NiTi shape memory alloy substrate actively offsets the thermal stress through shape memory recovery force. By continuously changing the Ni / Ti ratio in the substrate thickness direction, continuous NiTi gradient layer and Ni-rich transition layer are formed in the same thin film. The Ni-rich transition layer has a high Ni / Ti atomic ratio and its thermal expansion coefficient is closer to that of the gallium arsenide epitaxial layer, which reduces thermal mismatch stress from the source. At the same time, the oxidation resistance of Ni is used to protect the internal Ti from oxidation and to provide a metallurgical interface for the first bonding layer. The Ni / Ti atomic ratio is reduced on the back side of the NiTi gradient layer, and the shape memory effect is strongest. After the NiTi shape memory alloy substrate is rigidly bonded to the gallium arsenide epitaxial layer, the shape recovery is constrained by the gallium arsenide epitaxial layer. The recovery force cannot be released through macroscopic deformation and is instead applied to the bonding surface. The restoring force automatically increases with the degree of temperature deviation from the annealing temperature, and its direction always points towards the planar state. It is opposite in direction and synchronous in magnitude with the thermal mismatch warping force, forming a dynamic cancellation and improving the overall device warping deformation caused by thermal mismatch stress between the epitaxial layer and the substrate. In addition, the martensitic phase transformation of NiTi shape memory alloy is a first-order phase transformation. During heating, the martensite to austenite phase transformation is endothermic, and during cooling, the reverse phase transformation is exothermic. The Joule heat generated during the operation of gallium arsenide solar cells is absorbed by the phase transition heat absorption portion of the NiTi shape memory alloy substrate. The substrate itself, as a metal, has good thermal conductivity, allowing heat to be quickly dissipated. The phase transition temperature range of a uniformly composed NiTi shape memory alloy is typically only 10℃ to 30℃. The functional gradient design of the NiTi shape memory alloy substrate allows the Ni / Ti ratio to change gradually along the thickness direction, thus widening the phase transition temperature range. The phase transition temperature is high near the back side of the NiTi gradient layer and low in the Ni-rich transition layer on the bonding surface side. When a satellite enters or exits Earth's shadow, the ambient temperature changes drastically, and the absorption and release of latent heat continue to occur within the widened phase transition temperature range. The NiTi shape memory alloy substrate slows down the cooling / heating rate of the cell through phase transition heat absorption / release, forming a thermal buffer function, reducing the impact of drastic temperature differences on solar cell devices, and helping to protect the brittle gallium arsenide epitaxial layer.
[0025] In a preferred embodiment, the Ni / Ti atomic ratio in the NiTi graded layer 31 linearly changes from b to c along the thickness direction from top to bottom, with a ranging from 56:44 to 58:42, b from 55:45 to 56:44, and c from 49:51 to 50:50. Preferably, the thickness of the NiTi graded layer 31 is 10 μm to 30 μm. In some preferred embodiments, the Ni / Ti atomic ratio in the NiTi graded layer 31 linearly changes from 55:45 to a near-equal atomic ratio of 50:50 along the thickness direction from top to bottom. Correspondingly, the CTE of the NiTi alloy material in the NiTi graded layer 31 gradually changes from approximately 8 ppm / ℃ to approximately 11 ppm / ℃ (austenitic state) along the thickness direction from top to bottom, the martensitic transformation temperature gradually changes from approximately -50℃ to approximately 50℃, and the transformation temperature range widens to approximately 100℃. This layer can simultaneously perform stress regulation and thermal buffering functions.
[0026] It should be noted that in the preferred embodiment described above, the phase transition temperature range is extended to approximately 100°C (-50°C to +50°C), but does not cover the entire service temperature range (-170°C to +120°C). Outside the phase transition temperature range, the restoring force remains zero or no longer changes with temperature. Within the service temperature range of -170°C to +120°C, the phase transition behavior of the NiTi graded layer 31 is divided into three states: In the temperature range of 120℃ to 50℃: the entire NiTi gradient layer is in the austenitic state with zero stress, and the substrate only serves as a flexible support and conductor.
[0027] Between 50℃ and -50℃: the phase transformation gradually progresses from the back side to the bonding surface, and the restoring force and latent heat are continuously released within this range. The greater the temperature deviates from the annealing temperature, the thicker the region where the phase transformation has occurred, and the greater the restoring force, which increases synchronously with the increase in thermal mismatch stress.
[0028] In the -50℃ to -170℃ range: the entire NiTi graded layer has completed the martensitic phase transformation and does not generate active restoring force. However, the elastic modulus of the martensitic phase is significantly lower than that of the austenitic phase, and it can passively absorb thermal mismatch strain through its own elastic deformation and twin reorientation, reducing the peak interfacial stress transmitted to the epitaxial layer. The latent heat of the phase transformation has been released, and the thermal buffering function has ended, but the interfacial stress is relieved through martensitic deformation, avoiding cracking caused by stress concentration.
[0029] In a preferred embodiment, the thickness of the Ni-rich transition layer 32 is 0.5 μm to 5 μm; in some preferred embodiments, the thickness of the Ni-rich transition layer 32 is 2 μm. The Ni content in the Ni-rich transition layer 32 is higher than that in the NiTi graded layer 31, and its CTE is closest to that of GaAs. The Ni-rich transition layer 32 is in direct contact with the first bonding layer 4, reducing the near-interface CTE to match GaAs, utilizing the oxidation resistance of Ni to protect the internal Ti from oxidation, and simultaneously providing a metallurgically compatible interface with the metal of the first bonding layer.
[0030] As a preferred embodiment, please refer to Figure 5 The NiTi shape memory alloy substrate 3 further includes a near-backside transition layer 33. The upper surface of the near-backside transition layer 33 is in contact with the lower surface of the NiTi gradient layer 31. The Ni / Ti atomic ratio in the near-backside transition layer 33 is d, where d ≤ c, and d takes a value of 49:51 to 50:50. The thickness of the near-backside transition layer 33 is 4 μm to 6 μm. The near-backside transition layer 33 allows sufficient shape memory effect to be retained on the backside.
[0031] In a preferred embodiment, the training temperature of the NiTi shape memory alloy substrate 3 in the constrained state is the alloy annealing temperature of gallium arsenide solar cells, which is 250℃~350℃. During training, the NiTi shape memory alloy is constrained in a planar state, and its austenitic "memory shape" is planar, with the zero-stress state consistent with the subsequent annealing state. During cooling, the shrinkage tendency of the NiTi shape memory alloy is constrained by the glass temporary carrier, and shape recovery stress accumulates inside the NiTi shape memory alloy; when heated again, the alloy returns to the austenitic planar state, and the shape recovery stress is released. This cycle is consistent with the mechanical conditions of the NiTi shape memory alloy constrained by the gallium arsenide epitaxial layer in the subsequent bonding state, and the direction of the training recovery force matches the actual constraint conditions in service. In a preferred implementation, the training temperature is set to 300℃, consistent with the alloy annealing temperature. During annealing, the NiTi shape memory alloy is in the austenitic state with zero stress, and the memory shape is planar. During cooling, the NiTi shape memory alloy transforms into martensite, and the recovery force always points towards the planar state. If the training temperature deviates from the alloy annealing temperature, the shape memory in the austenitic state is inconsistent with the actual shape in the annealed state. When the temperature drops, the direction of the restoring force deviates, and the stress compensation effect is weakened.
[0032] In a preferred embodiment, the gallium arsenide solar cell further includes a back metal stack 2, which is stacked on the surface of the NiTi shape memory alloy substrate 3 away from the first bonding layer 4. The back metal stack 2 includes a NiAg transition layer, an Ag solderable layer, and an Au protective layer stacked sequentially from top to bottom. In the NiAg transition layer, Ni is compatible with NiTi material, and Ag is compatible with the Ag solderable layer, serving as a transition connection and solving the problem of insufficient direct bonding between the Ag solderable layer and the NiTi shape memory alloy substrate. The Au protective layer is exposed on the outermost back surface after laser lift-off, utilizing Au's oxidation resistance and chemical stability to protect the inner Ag solderable layer from oxidation or sulfidation. The NiAg transition layer, Ag solderable layer, and Au protective layer together solve the problem of poor solderability of the NiTi shape memory alloy substrate, allowing it to be soldered to the interconnect without additional processing, and simultaneously serving as the back electrode.
[0033] In a preferred embodiment, the raw material for preparing the NiAg transition layer is a NiAg alloy, wherein the mass ratio of Ni to Ag in the NiAg alloy is 10:90 to 50:50, the thickness of the NiAg transition layer is 50 nm to 150 nm, the thickness of the Ag solderable layer is 0.8 μm to 1.2 μm, and the thickness of the Au protective layer is 200 nm to 300 nm.
[0034] As a preferred embodiment, please refer to Figure 6 The NiTi shape memory alloy substrate 3 further includes a Ni-rich protective layer 34, which is disposed on the upper surface of the NiAg transition layer, and the upper surface of the Ni-rich protective layer 34 is in contact with the lower surface of the NiTi gradient layer 31. The Ni / Ti atomic ratio in the Ni-rich protective layer 34 is 58:42, and the thickness of the Ni-rich protective layer 34 is 0.4 μm to 0.6 μm. The Ni-rich protective layer 34 is used to prevent the Ti-rich region from being oxidized during subsequent annealing and to enhance the adhesion between the NiAg transition layer and the NiTi shape memory alloy substrate 3.
[0035] In a preferred embodiment, the light-incident surface of the flexible gallium arsenide solar cell further includes a gallium arsenide contact layer 7, a front electrode 8, and an anti-reflection film 9; the gallium arsenide contact layer 7 is disposed on the surface of the gallium arsenide epitaxial layer 6 away from the second bonding layer 5, and the gallium arsenide contact layer 7 adopts a patterned structure to reduce light absorption; the front electrode 8 is disposed on the surface of the gallium arsenide contact layer 7, and the anti-reflection film 9 is disposed on the portion of the light-incident surface of the gallium arsenide epitaxial layer 6 excluding the area covered by the gallium arsenide contact layer 7.
[0036] Other preferred embodiments of the present invention provide a method for fabricating the above-described flexible gallium arsenide solar cell on a shape memory alloy substrate, the method comprising the following steps: S1. On the surface of the glass temporary carrier 1, a Ti adhesion layer, an Au protective layer, an Ag solderable layer and a NiAg transition layer are sequentially vapor-deposited. In a preferred embodiment, the Ti adhesion layer has a thickness of 10 nm to 15 nm, preferably 12 nm, and is deposited using electron beam evaporation. The Ti adhesion layer is chemically bonded to the glass temporary substrate, ensuring that the entire back metal stack does not detach in subsequent processes, and also serves as a laser absorption layer. During laser lift-off, a 308 nm excimer laser passes through the glass and irradiates the Ti adhesion layer. The Ti absorbs the energy and converts it into heat, causing a rapid increase in the interface temperature between the Ti adhesion layer and the glass temporary substrate. The Ti adhesion layer vaporizes, thus separating the glass temporary substrate from the back metal stack.
[0037] In a preferred embodiment, the thickness of the Au protective layer is 200nm to 300nm, preferably 250nm. It is deposited by electron beam evaporation, and the Au protective layer is reliably bonded to the Ti adhesion layer. After laser stripping, the Au protective layer is exposed to the outermost layer on the back side. The oxidation resistance and chemical stability of Au are used to protect the inner Ag solderable layer from oxidation or sulfidation.
[0038] In a preferred embodiment, the Ag solderable layer has a thickness of 0.8 μm to 1.2 μm, preferably 1 μm, and the solderable layer body is deposited by electron beam evaporation or resistance thermal evaporation.
[0039] In a preferred embodiment, the NiAg transition layer has a thickness of 50 nm to 150 nm, preferably 100 nm, and is prepared by electron beam evaporation deposition using a NiAg alloy target. The mass ratio of Ni to Ag in the NiAg alloy target is 10:90 to 50:50, preferably 30:70. In the NiAg transition layer, Ni is compatible with NiTi, and Ag is compatible with the Ag solderable layer, serving as a transitional connection and solving the problem of insufficient adhesion between the Ag solderable layer and the NiTi shape memory alloy substrate.
[0040] The glass temporary carrier acts as a rigid constraint mold during constrained training, restricting the NiTi shape memory alloy substrate to maintain its planar state. At the same time, it serves as a temporary support in bonding and subsequent processes to prevent film deformation or breakage.
[0041] S2. NiTi gradient layer 31 and Ni-rich transition layer 32 are sequentially deposited on the surface of NiAg transition layer by Ni and Ti dual-target co-sputtering. After deposition, constrained state training is performed at the gallium arsenide solar cell alloy annealing temperature to obtain NiTi shape memory alloy substrate 3. The first bonding layer 4 is prepared on the surface of NiTi shape memory alloy substrate 3. As a preferred embodiment, the preparation method of NiTi graded layer 31 and Ni-rich transition layer 32 in S2 is as follows: Ni and Ti dual-target co-sputtering is used to deposit NiTi graded layer 31 on the surface of NiAg transition layer under Ar atmosphere, substrate temperature of 200℃~400℃, working pressure of 0.3Pa~0.8Pa. In the initial stage, the Ni / Ti atomic ratio is controlled at c, and linearly adjusted according to the program to increase the Ni target power and decrease the Ti target power until the Ni / Ti atomic ratio is b, thus completing the preparation of NiTi graded layer 31. Then, Ni and Ti dual-target co-sputtering is performed at Ni / Ti atomic ratio a to complete the preparation of Ni-rich transition layer 32.
[0042] In a preferred embodiment, S2 further includes the preparation of a near-backside transition layer 33 before preparing the NiTi gradient layer 31. The near-backside transition layer 33 is prepared by Ni and Ti dual-target co-sputtering to deposit the near-backside transition layer 33 on the surface of the NiAg transition layer under an Ar atmosphere, with a substrate temperature of 200℃~400℃ and a working pressure of 0.3Pa~0.8Pa, and controlling the Ni / Ti atomic ratio to d to complete the preparation of the near-backside transition layer 33.
[0043] In a preferred embodiment, the constrained state training method involves fixing the prepared NiTi shape memory alloy substrate 3 with a glass temporary carrier 1 onto a planar fixture, heating it to 250℃~350℃ and holding it at that temperature for 1h~3h, then cooling it to room temperature, and repeating this heating and cooling process 2 to 4 times. In a preferred embodiment, the thickness of the prepared NiTi gradient layer 31 is 20μm~30μm, and the thickness of the prepared Ni-rich transition layer 32 is 0.5μm~3μm.
[0044] S3. On the surface of a gallium arsenide substrate, an AlGaInP sacrificial layer, a gallium arsenide contact layer 7, and a gallium arsenide epitaxial layer 6 are grown sequentially by MOCVD, and a second bonding layer 5 is prepared on the surface of the gallium arsenide epitaxial layer 6. S4. Align the bonding surfaces of the first bonding layer 4 on the NiTi shape memory alloy substrate 3 and the second bonding layer 5 on the gallium arsenide epitaxial layer 6, and perform wafer bonding. S5. After bonding, the gallium arsenide substrate and AlGaInP sacrificial layer are removed to expose the gallium arsenide contact layer 7. The front electrode 8 and anti-reflection film 9 are sequentially prepared on the wafer surface after removing the gallium arsenide substrate and AlGaInP sacrificial layer. S6. The wafer prepared in S5 is subjected to alloy annealing at a temperature of 250℃~350℃. S7. Use an excimer laser to uniformly scan and irradiate the back of the glass temporary carrier 1. The laser passes through the glass temporary carrier 1, causing the Ti adhesion layer to vaporize under the laser energy. The Au protective layer, Ag solderable layer and NiAg transition layer are peeled off from the glass temporary carrier 1 together with the NiTi shape memory alloy substrate 3. S8. The wafer is separated into individual battery chips using a wafer dicing machine, and then subjected to photoelectric performance testing and sorting.
[0045] The fabrication method of the flexible gallium arsenide solar cell with shape memory alloy substrate provided in this application allows the NiTi shape memory alloy substrate to simultaneously perform four functions: flexible support, active stress compensation, thermal buffering, and vertical conductivity. The back metal stack solves the problem of poor solderability of the NiTi shape memory alloy substrate, allowing it to be soldered to interconnects without additional processing, and simultaneously serving as the back electrode. This eliminates the need for traditional back stress film setups, simplifying the device structure, and eliminates the need for through-etching processes, simplifying the fabrication process. Since the flexible gallium arsenide solar cell fabrication method with shape memory alloy substrate provided in this application produces the aforementioned flexible gallium arsenide solar cell, it also possesses the advantages or beneficial effects of the aforementioned flexible gallium arsenide solar cell, which will not be elaborated further here.
[0046] The present application will be further described in detail below with reference to specific embodiments: Example 1 This embodiment provides a method for fabricating a flexible gallium arsenide solar cell on a shape memory alloy substrate, specifically including the following steps: Step (1): Select a glass temporary carrier and prepare a Ti adhesion layer, an Au protective layer, an Ag solderable layer and a NiAg transition layer on the surface of the glass temporary carrier by electron beam evaporation deposition. The thicknesses are 12nm, 250nm, 1μm and 100nm respectively. The mass ratio of Ni to Ag in the NiAg transition layer is 3:7. Step (2): Ni and Ti dual-target co-sputtering is used, and the chamber vacuum is greater than 5 × 10⁻⁶. -4 The sputtering atmosphere was high-purity Ar (99.999%), with a working pressure of 0.5 Pa and a substrate temperature of 300 °C. Initially, the Ni target power was 100 W and the Ti target power was 300 W; subsequently, the power was linearly adjusted to 300 W for Ni and 100 W for Ti. The NiTi graded layer thickness was 24 μm. Near the NiAg transition layer (back side of the substrate), the Ni / Ti atomic ratio was 50:50, with a CTE of approximately 11 ppm / °C and a martensitic transformation temperature of approximately +50 °C; near the bonding surface, the Ni / Ti atomic ratio was 55:45, with a CTE of approximately 8 ppm / °C and a martensitic transformation temperature of approximately -50 °C. Along the thickness direction, the CTE gradually decreased from approximately 11 ppm / °C to approximately 8 ppm / °C (austenite state), and the phase transformation temperature range broadened to approximately 100 °C.
[0047] While maintaining a Ni target power of 200W and a Ti target power of 50W, a Ni-rich transition layer with a thickness of 2μm was deposited on the surface of the NiTi graded layer. The Ni / Ti atomic ratio of the Ni-rich transition layer was 58:42, and the CTE was about 7 ppm / ℃, which is closer to GaAs's 5.7 ppm / ℃. At the same time, the internal Ti was protected from oxidation.
[0048] Step (3): The NiTi shape memory alloy film deposited on the glass temporary carrier is fixed onto a planar fixture and subjected to constrained training according to the following training procedure: heated to 300℃ and held for 2 hours, then rapidly cooled to room temperature, repeated 3 times. The glass temporary carrier serves as a rigid constraint mold during training. The training enables the NiTi shape memory alloy to remember the planar shape at 300℃ as a zero-stress state. The constraint conditions during training are consistent with the mechanical conditions under which the NiTi shape memory alloy substrate is constrained by the gallium arsenide epitaxial layer in service.
[0049] Step (4): On the surface of the gallium arsenide substrate, an AlGaInP sacrificial layer and a gallium arsenide contact layer are grown sequentially using an MOCVD device, followed by the growth of gallium arsenide epitaxial layers in flip-chip order. The gallium arsenide epitaxial layers include the sequentially grown GaInP top cell (containing an N-type AlInP window layer, an N-type GaInP emitter layer, a P-type GaInP base region, and a P-type GaInP back field layer), a first tunnel junction, a GaAs middle cell (containing an N-type InGaP window layer, an N-type GaAs emitter layer, a P-type GaAs base region, and a P-type InGaP back field layer), a second tunnel junction, and an InGaAs bottom cell (containing an N-type AlInP window layer, an N-type InGaAs emitter layer, a P-type InGaAs base region, a P-type InGaAs back field layer, and a P-type InGaAs contact layer).
[0050] Step (5): On the back side of the gallium arsenide epitaxial layer prepared in step (4), Au / Ag / Au were sequentially deposited by electron beam evaporation as the second bonding layer, with thicknesses of 50nm / 2000nm / 200nm respectively. On the NiTi shape memory alloy substrate side, Ti / Pt / Au were sequentially deposited by electron beam evaporation as the first bonding layer, with thicknesses of 20nm / 30nm / 100nm respectively. The trained NiTi shape memory alloy substrate and the triple-junction gallium arsenide epitaxial wafer were then bonded in a vacuum environment (<1Pa), at a temperature of 300℃ and a pressure of 1 MPa for 30 minutes.
[0051] The gallium arsenide substrate was thinned to approximately 120 μm by mechanical polishing. The residual GaAs was then selectively etched using an ammonia / hydrogen peroxide mixture (ammonia:hydrogen peroxide:water volume ratio 1:5:5) to expose the AlGaInP sacrificial layer.
[0052] Step (6): The AlGaInP sacrificial layer was removed at room temperature using concentrated hydrochloric acid (37%) to expose the gallium arsenide contact layer. The front electrode pattern was defined by photolithography. Au / AuGeNi / Au / Ag / Au metal stacks were deposited by electron beam evaporation, with thicknesses of 100nm, 50nm, 100nm, 4000nm, and 500nm respectively. The bottom layer Au served as the adhesion layer, and AuGeNi served as the ohmic contact layer. The AuGeNi alloy composition was 83wt% Au, 12wt% Ge, and 5wt% Ni. The middle layer Au served as the barrier layer, Ag served as the conductive host layer, and the top layer Au served as the anti-oxidation protective layer. The gallium arsenide contact layer outside the gate lines was selectively etched using a citric acid / hydrogen peroxide mixed solution (citric acid:hydrogen peroxide:water volume ratio of 1:1:2). A TiO2 / Al2O3 double-layer antireflection film was deposited with optical thicknesses of 350nm / 600nm. The antireflective coating on the pads was removed by photolithography etching, and then the alloy was annealed at 300°C for 30 minutes.
[0053] Step (7): Use a 308nm excimer laser to uniformly scan and irradiate the back of the glass temporary carrier. The laser light passes through the glass temporary carrier and is absorbed by the Ti adhesion layer. The Ti adhesion layer vaporizes, and the Au protective layer, Ag solderable layer, and NiAg transition layer detach from the glass temporary carrier along with the NiTi shape memory alloy substrate.
[0054] Step (8): Separate the wafer into individual chips along the preset cutting path using a wafer dicing machine, and perform optoelectronic performance testing and sorting.
[0055] Example 2 The only difference from Example 1 is that in step (2), the NiTi shape memory alloy substrate material is deposited by magnetron co-sputtering, which is prepared by Ni and Ti dual-target co-sputtering, and an equal atomic ratio near-backside transition layer is added, and the Ni / Ti atomic ratio and thickness of each layer are different: In S2, a near-backside transition layer with an equal atomic ratio is first formed on the side closest to the NiAg transition layer (back side of the substrate), with a Ni / Ti atomic ratio of 50:50 and a thickness of 4.8 μm. A constant Ni target power of 100 W and a Ti target power of 300 W are used, and the deposition time is determined based on the thickness. The Ni / Ti atomic ratio of the NiTi gradient layer linearly changes from 50:50 on the near-backside transition layer side to 55:45, with a thickness of 14.4 μm. Initially, the Ni target power is 100 W and the Ti target power is 300 W, then linearly adjusted according to the program to 300 W and 100 W, with the deposition time determined based on the thickness.
[0056] The Ni-rich transition layer has a Ni / Ti atomic ratio of 55:45 and a thickness of 4.8 μm. The Ni target power is 300 W and the Ti target power is 100 W, which are kept constant. The deposition time is determined according to the thickness.
[0057] In this embodiment, the total thickness of the NiTi shape memory alloy substrate is 24 μm, which is slightly different from the 26 μm in Example 1. This is achieved by adjusting the thickness distribution of each layer: the near-back transition layer and the Ni-rich transition layer each account for about 20%, and the NiTi gradient layer accounts for about 60%, so that the near-bonding surface maintains a low CTE over a larger thickness range, while the back side still retains sufficient shape memory effect.
[0058] Example 3 The only difference in Example 1 is that in step (2), the NiTi shape memory alloy substrate material is deposited by magnetron co-sputtering, with different Ni / Ti atomic ratios in each layer. In step (1), an additional Ni-rich protective layer of about 0.5 μm is deposited on the surface of the NiAg transition layer. The Ni-rich protective layer is a NiTi alloy with a Ni / Ti atomic ratio of 58:42, prepared by Ni and Ti dual-target co-sputtering. The Ni target power is 250W and the Ti target power is 50W during deposition. This Ni-rich protective layer is used to prevent the Ti-rich region from being oxidized during the subsequent annealing process and to enhance the bonding force between the NiAg transition layer and the NiTi shape memory alloy substrate. The Ni / Ti atomic ratio of the NiTi graded layer linearly changes from 49:51 to 56:44 near the back transition layer, with a thickness of 24 μm and a phase transition temperature of approximately +80℃. In the initial stage, the Ni target power is 80 W and the Ti target power is 320 W, which is then linearly adjusted to 320 W and 80 W respectively according to the program.
[0059] The Ni-rich transition layer has a Ni / Ti atomic ratio of 56:44, a thickness of 2 μm, a phase transition temperature of approximately -100℃, and a CTE of approximately 7.5 ppm / ℃. A constant Ni target power of 320 W and a Ti target power of 80 W were used.
[0060] Comparative Example 1 The method is the same as in Example 1, except that in step (2), the NiTi shape memory alloy substrate material is prepared by magnetron sputtering. A uniform NiTi substrate with an equal atomic ratio (Ni / Ti atomic ratio of 50:50) and a thickness of 26 μm is prepared with no compositional gradient. During co-sputtering, the Ni target power is kept constant at 100 W and the Ti target power at 300 W. Other sputtering conditions (cavity vacuum greater than 5 × 10⁻⁶) are also used. -4 The conditions (Pa, sputtering atmosphere: high-purity Ar, working pressure: 0.5 Pa, substrate temperature: 300 °C) were the same as in Example 1, and the film thickness was increased to 26 μm by controlling the deposition time.
[0061] Comparative Example 2 The method is the same as in Example 1, except that the constrained state training temperature in step (3) is changed to 200℃, while the alloy annealing temperature remains at 300℃. The constrained state training procedure is as follows: heat to 200℃, hold for 2 hours, then cool rapidly, repeating 3 times.
[0062] Comparative Example 3 On the surface of a gallium arsenide (GaAs) substrate, an AlGaInP sacrificial layer and a GaAs contact layer are sequentially grown using an MOCVD apparatus, followed by the growth of a GaAs epitaxial layer in flip-chip order. The GaAs epitaxial layer comprises, sequentially grown GaInP top cell (containing an N-type AlInP window layer, an N-type GaInP emitter layer, a P-type GaInP base region, and a P-type GaInP back field layer), a first tunnel junction, a GaAs middle cell (containing an N-type InGaP window layer, an N-type GaAs emitter layer, a P-type GaAs base region, and a P-type InGaP back field layer), a second tunnel junction, and an InGaAs bottom cell (containing an N-type AlInP window layer, an N-type InGaAs emitter layer, a P-type InGaAs base region, a P-type InGaAs back field layer, and a P-type InGaAs contact layer).
[0063] On the back side of the gallium arsenide epitaxial layer, an Au / Ag / Au / Ni stack was sequentially deposited by electron beam evaporation with thicknesses of 300nm / 1500nm / 100nm / 10nm, respectively. The bottom Au layer served as the ohmic contact layer, and the Ag layer served as the conductive layer. The top Au layer served as the protective layer, and the Ni layer served as the electroplating seed layer. Subsequently, a Ni layer with a thickness of 30μm was deposited by electroplating. The electroplating solution was a nickel sulfamate system with a current density of 2A / dm² and a temperature of 50℃. The electroplating time was controlled according to the target thickness. After electroplating, the gallium arsenide substrate was thinned to approximately 120μm by mechanical grinding. The residual GaAs was selectively etched using a mixture of ammonia and hydrogen peroxide (ammonia:hydrogen peroxide:water volume ratio 1:5:5) to expose the AlGaInP sacrificial layer. The AlGaInP sacrificial layer was removed according to the method of step (6) in Example 1, and the front electrode and antireflection film were fabricated. The lower electrode window area was defined using front-side photolithography. Cl-based ICP etching was employed, penetrating from top to bottom through the gallium arsenide epitaxial layer and the underlying Au layer until the Ag layer was exposed, with the exposed Ag layer serving as the lower electrode. A 2μm thick SiO2 stress-compensating film was deposited on the back side of the Ni layer using PECVD at a deposition temperature of 250℃, a SiH4 flow rate of 30 sccm, an N2O flow rate of 150 sccm, and an RF power of 80W. The wafer was then diced into individual chips along predetermined dicing paths using a wafer dicing machine for optoelectronic performance testing and sorting.
[0064] Comparative Example 4 The method of Example 1 is different in that the NiAg transition layer is not deposited in step (1). Instead, the Ti adhesion layer, Au protective layer and Ag solderable layer are deposited sequentially on the surface of the glass temporary substrate, with thicknesses of 12 nm, 250 nm and 1 μm, respectively. Then, the NiTi co-sputtering in step (2) is performed directly on the surface of the Ag solderable layer to deposit the NiTi gradient layer and the Ni-rich transition layer.
[0065] Test case The flexible gallium arsenide solar cells on shape memory alloy substrates prepared in the above embodiments and comparative examples were subjected to photoelectric performance and reliability tests. The photoelectric performance tests were conducted using a solar simulator under AM0 spectral conditions (AM0, 1000 W / m²). 2 The photoelectric parameters of the battery were measured at 25℃. Before testing, the spectral matching of the simulator was calibrated using a standard battery to control the spectral mismatch error within ±2%. During testing, the battery was placed on a temperature-controlled platform, and measurements were taken after the temperature stabilized at 25±0.5℃. The sample was placed in a thermal shock test chamber with a temperature range of -170℃ to +120℃, and held at both high and low temperatures for 20 minutes each, with a switching time not exceeding 1 minute, for a total of 10 cycles. After the test, the sample was removed and allowed to recover at room temperature for 2 hours before retesting the photoelectric performance and calculating the efficiency decay rate. Warpage was measured using a laser scanning rangefinder, and the maximum height difference on the sample surface was used as the measure. Measurements were performed at room temperature, with the sample placed freely without any external force applied. The test results are shown in Table 1. Table 1: Photoelectric performance parameters and reliability test results of each embodiment and comparative example
[0066] As shown in Table 1, the flexible gallium arsenide solar cell prepared in Example 1 exhibits the best overall performance, with an initial photoelectric conversion efficiency of 33.04%, an efficiency degradation of only 1.2% after thermal shock, and a warpage of 3.6 mm. Although Comparative Example 1 has a slightly higher fill factor (84.87%), its efficiency degradation after thermal shock is as high as 5.2%, and its warpage is 8.5 mm, resulting in a significantly lower overall reliability than Example 1. This indicates that this application achieves the best balance in key indicators such as efficiency, degradation, and warpage by setting a NiTi shape memory alloy substrate with a NiTi gradient layer and a Ni-rich transition layer.
[0067] Example 2 showed an initial photoelectric conversion efficiency of 32.29%, with an efficiency decrease of 1.3% after thermal shock and a warpage of 4.5 mm. While these figures were slightly lower than those of Example 1, they were still significantly better than the comparative example. This indicates that the NiTi shape memory alloy substrate fabrication in Example 1 already met the stress control requirements, and further adjustments to the thickness of each layer and the Ni / Ti ratio did not result in additional performance improvements.
[0068] Example 3 shows an initial photoelectric conversion efficiency of 32.67%, an efficiency decrease of 1.4% after thermal shock, and a warpage of 4.0 mm. The value of Example 3 lies in providing wider active control coverage for extreme temperature mission scenarios.
[0069] Comparative Example 1 had an initial photoelectric conversion efficiency of 32.59%, similar to Example 1, but its efficiency decreased by as much as 5.2% after thermal shock, with a warpage of 8.5 mm. This indicates that although the homogeneous composition shape memory alloy possesses shape memory effect, the near-bonding surface material CTE and GaAs have a large mismatch, and the phase transition temperature range is narrow. The restoring force is concentrated and released within the narrow temperature range, causing impact on the bonding interface. After temperature cycling, microcracks are generated in the epitaxial layer, leading to a significant decrease in photoelectric conversion efficiency.
[0070] Comparative Example 2 had an initial efficiency of 31.35%, and its efficiency decreased by 8.5% after thermal shock, with a warpage of 10.2 mm. All indicators were the worst, indicating that when the training temperature and the alloy annealing temperature were inconsistent, the direction of the restoring force deviated during cooling, and the stress compensation effect was impaired.
[0071] Comparative Example 3 showed a relatively low initial photoelectric conversion efficiency of 32.15% and a warpage of 5.8 mm, but its efficiency decreased by 6.0% after thermal shock. This indicates that static stress compensation cannot keep up with temperature changes in extreme temperature ranges, and the adhesion between the stress film and the Ni foil degrades during temperature cycling, leading to interface delamination and deterioration of electrical performance. This comparison demonstrates that active stress control on NiTi shape memory alloy substrates is superior to passive compensation schemes.
[0072] For the samples of Example 1 and Comparative Example 4, the adhesion between the Ag solderable layer and the NiTi shape memory alloy substrate was tested using the cross-cut method before laser lift-off. The test method involved using a knife tip to cut a 1mm × 1mm grid array on the sample surface, applying adhesive tape, and then quickly peeling it off. The percentage of the Ag solderable layer peeled off from the NiTi shape memory alloy substrate surface was observed. The test results showed that in Example 1, due to the presence of the NiAg transition layer, the adhesion between the Ag solderable layer and the NiTi shape memory alloy substrate was good, with a peeling area ratio of less than 1%. In Comparative Example 4, after removing the NiAg transition layer, the Ag solderable layer was in direct contact with the NiTi shape memory alloy substrate, resulting in a significant decrease in adhesion and a peeling area ratio greater than 40%. This indicates that Ni and NiTi are compatible in the NiAg transition layer, as are Ag and the Ag solderable layer, effectively solving the problem of insufficient direct adhesion between Ag and NiTi, and making it an indispensable component of the back metal stack.
[0073] Comparative Example 4 showed an initial photoelectric conversion efficiency of 32.33%, with an efficiency decrease of 3.5% and a warpage of 5.0 mm after thermal shock. Due to the lack of a NiAg transition layer, Comparative Example 4 exhibited poor adhesion between the Ag solderable layer and the NiTi shape memory alloy substrate. During laser lift-off or subsequent bonding annealing, localized peeling of the Ag solderable layer occurred, leading to increased contact resistance between the back metal stack and the NiTi shape memory alloy substrate, and a decrease in fill factor and efficiency. This comparison further demonstrates that the NiAg transition layer is not only a functional layer addressing the insufficient adhesion between Ag and NiTi, but also a necessary component ensuring the overall conductivity reliability of the back metal stack. Example 1, due to the inclusion of a NiAg transition layer, showed a strong bond between the back metal stack and the NiTi shape memory alloy substrate, low series resistance, and the highest initial photoelectric conversion efficiency of 33.04% among all samples. Its efficiency decrease of 1.2% and warpage of 3.6 mm after thermal shock were the lowest among all samples, demonstrating the best overall performance.
[0074] Regarding long-term temperature cycling stability, this application verifies the performance through thermal shock testing (-170℃ to +120℃, 10 cycles). Table 1 shows that Example 1 exhibits an efficiency degradation of only 1.2% and a warpage of 3.6 mm; Comparative Example 1 shows an efficiency degradation of 5.2% and a warpage of 8.5 mm. These data indicate that the NiTi shape memory alloy substrate effectively suppresses the accumulation of thermal mismatch stress, avoiding performance degradation caused by phase transformation fatigue and compositional segregation. The gradient design allows phase transformation to occur gradually over a wide temperature range, avoiding fatigue caused by localized concentrated phase transformations; the Ni-rich transition layer and Pt barrier layer suppress Ni diffusion and prevent compositional segregation.
[0075] To prevent Ni from diffusing from the NiTi shape memory alloy substrate to the gallium arsenide epitaxial layer, this application incorporates a diffusion barrier structure at the bonding interface. Pt in the first bonding layer serves as a diffusion barrier layer with a thickness of 30 nm to 50 nm. Pt has an extremely low diffusion coefficient in Ni and is chemically stable at annealing temperatures of 250 °C to 350 °C, effectively preventing Ni atoms from migrating towards the gallium arsenide epitaxial layer. A concentration gradient buffer is formed between the Ni-rich transition layer and the NiTi graded layer, further reducing the driving force for Ni diffusion into the epitaxial layer.
[0076] Outside the phase transition temperature range, this application still possesses stress management capabilities. In the range of -50℃ to -170℃, the NiTi shape memory alloy is entirely in the martensitic state, generating no active restoring force. However, the elastic modulus of the martensitic phase is significantly lower than that of the austenitic phase, allowing it to passively absorb thermal mismatch strain through its own elastic deformation and twin reorientation, reducing the peak interfacial stress transmitted to the epitaxial layer. In the range of 120℃ to 50℃, the low CTE characteristics of the Ni-rich transition layer reduce the generation of thermal mismatch stress from the source. These mechanisms complement the active restoring force within the phase transition temperature range, enabling the NiTi shape memory alloy substrate to possess stress management capabilities throughout its entire service temperature range.
[0077] This application achieves precise locking of the zero-stress point by setting the constrained-state training temperature to the alloy annealing temperature. In the NiTi gradient layer, the Ni / Ti atomic ratio gradually changes along the thickness direction, simultaneously managing CTE, phase transition temperature range, and restoring force. The NiAg transition layer, Ag solderable layer, and Au protective layer in the back metal stack jointly undertake the functions of solderability, conductivity, and laser lift-off bearing. As shown in Table 1, Example 1 has the highest initial photoelectric conversion efficiency of 33.04% among all samples, and the lowest efficiency degradation of 1.2% and warpage of 3.6 mm after thermal shock, indicating the best overall performance. Comparative Example 4, lacking the NiAg transition layer, has poor adhesion between the Ag solderable layer and the NiTi shape memory alloy substrate, resulting in lower efficiency than Example 1, further demonstrating the necessity of the back metal stack in this application. The above data fully demonstrate the synergistic effect between the various features.
[0078] For details not described in this embodiment, please refer to the relevant descriptions in the rest of this application.
[0079] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application and not to limit them; although this application has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications can still be made to the specific implementation of this application or equivalent substitutions can be made to some technical features, all of which should be covered within the scope of the technical solutions claimed in this application.
Claims
1. A shape memory alloy substrate flexible gallium arsenide solar cell, characterized by, It includes a NiTi shape memory alloy substrate, a first bonding layer, a second bonding layer, and a gallium arsenide epitaxial layer stacked sequentially from bottom to top; The NiTi shape memory alloy substrate is subjected to constrained state training so that the NiTi shape memory alloy remembers the planar shape at the alloy annealing temperature as a zero-stress state; The NiTi shape memory alloy substrate includes a NiTi gradient layer and a Ni-rich transition layer stacked sequentially from bottom to top. The Ni / Ti atomic ratio in the Ni-rich transition layer is a, and the Ni / Ti atomic ratio in the NiTi gradient layer gradually changes from b to c along the thickness direction from top to bottom. The values of a and b are both selected from 45:55 to 58:42, and the value of c is 49:51 to 50:50, and a ≥ b > c.
2. A shape memory alloy substrate flexible GaAs solar cell according to claim 1, characterized in that, In the NiTi gradient layer, the Ni / Ti atomic ratio changes linearly from b to c along the thickness direction from top to bottom, with a ranging from 56:44 to 58:42, b ranging from 55:45 to 56:44, and c ranging from 49:51 to 50:
50.
3. A shape memory alloy substrate flexible GaAs solar cell according to claim 1, wherein, The thickness of the Ni-rich transition layer is 0.5 μm to 5 μm, and the thickness of the NiTi graded layer is 10 μm to 30 μm.
4. A flexible GaAs solar cell with a shape memory alloy substrate according to any one of claims 1 to 3, characterized in that The NiTi shape memory alloy substrate further includes a near-back transition layer, the upper surface of which is in contact with the lower surface of the NiTi gradient layer. The Ni / Ti atomic ratio in the near-back transition layer is d, where d ≤ c, and d takes a value of 49:51 to 50:
50. The thickness of the near-back transition layer is 4 μm to 6 μm.
5. The shape memory alloy substrate flexible GaAs solar cell of claim 1, wherein, The constrained state training temperature of the NiTi shape memory alloy substrate is the alloy annealing temperature of the gallium arsenide solar cell, which is 250℃~350℃.
6. The shape memory alloy substrate flexible GaAs solar cell of claim 1, wherein, The gallium arsenide solar cell also includes a back metal stack, which is stacked on the surface of the NiTi shape memory alloy substrate away from the first bonding layer. The back metal stack comprises a NiAg transition layer, an Ag solderable layer, and an Au protective layer stacked sequentially from top to bottom; the NiAg transition layer is prepared from a NiAg alloy, wherein the mass ratio of Ni to Ag in the NiAg alloy is 10:90 to 50:50, and the thickness of the NiAg transition layer is 50 nm to 150 nm; the thickness of the Ag solderable layer is 0.8 μm to 1.2 μm, and the thickness of the Au protective layer is 200 nm to 300 nm.
7. The shape memory alloy substrate flexible GaAs solar cell of claim 1, wherein, The NiTi shape memory alloy substrate further includes a Ni-rich protective layer, the upper surface of which is in contact with the lower surface of the NiTi gradient layer, the Ni / Ti atomic ratio in the Ni-rich protective layer is 58:42, and the thickness of the Ni-rich protective layer is 0.4μm to 0.6μm.
8. The method of claim 1-7, wherein the method further comprises the step of: Includes the following steps: S1. On the surface of the glass temporary carrier, a Ti adhesion layer, an Au protective layer, an Ag solderable layer and a NiAg transition layer are sequentially vapor-deposited. S2. A NiTi gradient layer and a Ni-rich transition layer are sequentially deposited on the surface of the NiAg transition layer using Ni and Ti dual-target co-sputtering. After deposition, constrained state training is performed at the gallium arsenide solar cell alloy annealing temperature to obtain a NiTi shape memory alloy substrate. The first bonding layer is then prepared on the surface of the NiTi shape memory alloy substrate. The constrained state training method involves fixing the prepared NiTi shape memory alloy substrate with a glass temporary carrier on a planar fixture, heating it to 250℃~350℃ and holding it for 1h~3h, then cooling it to room temperature, and repeating the heating and cooling process 2 to 4 times. S3. On the surface of a gallium arsenide substrate, an AlGaInP sacrificial layer, a gallium arsenide contact layer, and a gallium arsenide epitaxial layer are grown sequentially by MOCVD, and a second bonding layer is prepared on the surface of the gallium arsenide epitaxial layer. S4. Align the bonding surfaces of the first bonding layer on the NiTi shape memory alloy substrate side and the second bonding layer on the gallium arsenide epitaxial layer side, and perform wafer bonding. S5. After bonding, remove the gallium arsenide substrate and AlGaInP sacrificial layer to expose the gallium arsenide contact layer. Then, prepare the front electrode and anti-reflection film on the wafer surface after removing the gallium arsenide substrate and AlGaInP sacrificial layer. S6. The wafer prepared in S5 is subjected to alloy annealing at a temperature of 250℃~350℃. S7. Use an excimer laser to uniformly scan and irradiate the back of the glass temporary carrier. The laser passes through the glass temporary carrier, causing the Ti adhesion layer to vaporize under the laser energy. The Au protective layer, Ag solderable layer and NiAg transition layer are peeled off from the glass temporary carrier together with the NiTi shape memory alloy substrate. S8. The wafer is separated into individual battery chips using a wafer dicing machine, and then subjected to photoelectric performance testing and sorting.
9. The method for fabricating a flexible gallium arsenide solar cell on a shape memory alloy substrate according to claim 8, characterized in that, The preparation method of NiTi graded layer and Ni-rich transition layer in S2 is as follows: Ni and Ti dual-target co-sputtering is used to deposit NiTi graded layer on NiAg transition layer surface. Ar atmosphere, substrate temperature 200℃~400℃, working pressure 0.3Pa~0.8Pa. In the initial stage, the Ni / Ti atomic ratio is controlled at c. The Ni target power is linearly adjusted according to the program to increase Ni target power and decrease Ti target power until Ni / Ti atomic ratio is b, thus completing the preparation of NiTi graded layer. Then, Ni and Ti dual-target co-sputtering is performed at Ni / Ti atomic ratio a to complete the preparation of Ni-rich transition layer.
10. A method for fabricating a flexible gallium arsenide solar cell on a shape memory alloy substrate according to claim 9, characterized in that, In S2, before preparing the NiTi gradient layer, a near-backside transition layer is also prepared. The preparation method of the near-backside transition layer is as follows: Ni and Ti dual-target co-sputtering is used to deposit the near-backside transition layer on the surface of the NiAg transition layer. Ar atmosphere, substrate temperature 200℃~400℃, working pressure 0.3Pa~0.8Pa, and the Ni / Ti atomic ratio is controlled to d to complete the preparation of the near-backside transition layer.