A vertical deep ultraviolet LED with a light emission morphology control structure
By setting an Al composition gradient-modulated light extraction morphology control layer in the N-type doped region, the problem of low light extraction efficiency of vertical deep ultraviolet LEDs is solved, the controllability and consistency of the light extraction morphology are achieved, and the light extraction efficiency and device performance are improved.
Patent Information
- Application Number
- CN202611229323.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-13
- Publication Date
- 2026-11-17
AI Technical Summary
The light extraction efficiency of existing vertical deep ultraviolet LEDs is low, mainly due to the poor uniformity and controllability of the coarsening morphology on the main light-emitting side, making it difficult to form an inclined light-emitting structure that is conducive to deep ultraviolet light emission.
An Al composition gradient control layer is set near the main light-emitting side in the N-type doped region. The Al composition gradient distribution is constructed through the epitaxial growth stage, so that the main light-emitting side forms an inclined light-emitting microstructure during the etching process. The difference in etching response of AlGaN materials with different Al compositions is used to form an inclined side to reduce total reflection.
It significantly improves light extraction efficiency and the consistency of light output morphology, reduces total internal reflection loss, and enhances the stability and repeatability of device performance.
Smart Images

Figure CN123124525A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor optoelectronics, and more particularly to a vertical deep ultraviolet LED with a light emission morphology control structure. Background Technology
[0002] Deep ultraviolet light-emitting diodes (LEDs) are semiconductor light-emitting devices with emission wavelengths in the deep ultraviolet band. They have advantages such as small size, fast response speed, easy integration, mercury-free and environmentally friendly, and low-voltage driving capability. They have important application value in fields such as sterilization and disinfection, air purification, water treatment, biomedicine, photopolymerization and high-end testing.
[0003] Currently, deep ultraviolet (DUV) LED chips commonly employ AlGaN-based epitaxial structures, primarily consisting of an n-type AlGaN layer, a multi-quantum-well active region, and a p-type AlGaN layer. Due to the short wavelength of DUV emission, the Al content in the epitaxial material is typically high. High-Al-content AlGaN presents significant challenges in doping activation, carrier transport, ohmic contacts, and crystal quality control. To improve current distribution and heat dissipation, vertical structures have become an important development direction for DUV LEDs. Vertical structure DUV LEDs are achieved through substrate bonding and laser lift-off (LLO) processes, effectively improving chip heat dissipation and light extraction efficiency, making it a crucial development direction in the current DUV LED field. Existing vertical structure DUV LEDs typically employ surface roughening processes such as dry etching, wet etching, or photoelectrochemical etching on the exposed N-type AlGaN main emission side after laser lift-off to reduce total internal reflection loss at the emission interface, thereby improving DUV light extraction efficiency.
[0004] However, in existing technologies, the roughening morphology of the main light-emitting side mainly relies on etching process parameters for control. The roughening effect is greatly affected by etching conditions, making it difficult to ensure the consistency and controllability of the roughening morphology. At the same time, existing epitaxial structures are usually not pre-designed for the main light-emitting side after laser ablation. The surface morphology formed during the etching process has a large degree of randomness, making it difficult to obtain an inclined light-emitting structure that is conducive to deep ultraviolet light emission, thus greatly limiting the improvement of light extraction efficiency.
[0005] Therefore, there is an urgent need to provide an epitaxial structure design scheme suitable for vertical deep ultraviolet LEDs. By pre-designing the main light-emitting side after laser stripping during the epitaxial growth stage, the expected light-emitting microstructure can be formed on this side during the subsequent etching process, thereby improving the consistency and controllability of the light-emitting morphology, further reducing the total internal reflection loss of the main light-emitting side, and improving the light extraction efficiency of vertical deep ultraviolet LEDs. Summary of the Invention
[0006] The purpose of this invention is to provide a vertical deep ultraviolet LED with a light-emitting morphology control structure to solve the technical problem of low light extraction efficiency in existing vertical deep ultraviolet LEDs. This invention sets a light-emitting morphology control layer with an Al composition gradient near the main light-emitting side in the N-type doped region. Utilizing the difference in etching response between AlGaN materials with different Al compositions, an Al composition gradient distribution is pre-constructed during the epitaxial growth stage, causing the main light-emitting side to automatically form an inclined light-emitting microstructure during etching. This reduces total internal reflection of deep ultraviolet light on the main light-emitting side and improves light extraction efficiency.
[0007] Specifically, the technical solution provided by this invention is as follows: This invention provides a vertical deep ultraviolet LED with a light emission morphology control structure, which, from top to bottom, comprises an N-type electrode, an N-type semiconductor layer, a multi-quantum-well active layer, a P-type semiconductor layer, a P-type electrode, and a supporting substrate. Among them, a light-emitting morphology control layer is provided between the N-type electrode and the N-type semiconductor layer; the light-emitting morphology control layer is made of AlGaN material, and its Al molar composition decreases continuously or stepwise along the direction away from the multi-quantum-well active layer; a light-emitting microstructure with an inclined side is formed on the surface of the light-emitting morphology control layer away from the multi-quantum-well active layer.
[0008] Specifically, this invention provides a light-emitting morphology control layer near the main light-emitting side of the N-type semiconductor layer, where the Al composition decreases continuously or in a stepwise manner away from the active layer. Utilizing the difference in etching response of AlGaN materials with different Al compositions, this light-emitting morphology control layer can self-form a light-emitting microstructure with tilted sides based on the composition gradient during subsequent etching processes. On the one hand, the tilted sides can effectively change the incident angle of deep ultraviolet light at the light-emitting interface, reducing the probability of total internal reflection and thus significantly improving light extraction efficiency. On the other hand, since the morphology of the light-emitting microstructure is determined by the Al composition gradient distribution pre-designed during the epitaxial stage, rather than solely relying on etching process parameters, it can effectively improve the consistency and controllability of the light-emitting morphology, overcoming the shortcomings of existing technologies where the coarsening morphology is highly random and it is difficult to stably obtain tilted light-emitting structures.
[0009] Preferably, the thickness of the light-emitting morphology control layer is 100–800 nm, and the total variation of its Al molar composition is 0.2–0.5.
[0010] Specifically, this thickness range ensures sufficient variation in the Al composition gradient, allowing for a significant rate difference along the thickness direction during etching to induce a light-emitting microstructure with distinct tilting characteristics. It also avoids increasing epitaxial growth time and material defect density due to an excessively thick light-emitting morphology control layer, while preventing insufficient gradient variation and indistinct tilting side morphology due to excessive thinness. On the other hand, the total Al composition variation of 0.2–0.5 ensures a sufficiently significant difference in etching rate between different layers, resulting in a clearly discernible tilting side profile. It also avoids introducing large lattice mismatch stress due to excessive composition variation, reducing epitaxial layer dislocation density and interface defect risk, and ensuring crystal quality and device reliability.
[0011] Preferably, the Al molar composition content of the light-emitting morphology control layer on the surface near the multi-quantum-well active layer is a, and the Al molar composition on the surface near the N-type electrode is b; wherein a and b satisfy the following relationship: 0.55≤a≤0.85, 0.35≤b≤0.60, and a>b.
[0012] Specifically, the aforementioned Al composition design ensures that the side near the multi-quantum-well active layer has a higher Al composition to match the Al composition of the underlying N-type semiconductor layer and the multi-quantum-well active layer, reducing lattice mismatch and band break at the interface and lowering carrier transport resistance. It also enables the low-Al composition region near the light-emitting side to exhibit a faster etching response rate during etching, thus forming a significant rate difference with the high-Al composition region and inducing the formation of a tilted side profile that gradually narrows or expands from bottom to top. At the same time, a and b are respectively limited within the aforementioned composition range, and by limiting a > b, it is ensured that the Al composition of the light-emitting morphology control layer decreases overall along the direction away from the multi-quantum-well active layer, thereby ensuring the certainty of the composition gradient direction and the predictability of the etching morphology, which is beneficial for stably obtaining the light-emitting microstructure with the expected tilt angle.
[0013] Preferably, the light-emitting morphology control layer is made of Si-doped AlGaN material, with a Si doping concentration of 1×10⁻⁶. 17 ~5×10 19 cm -3 .
[0014] Specifically, Si doping can effectively improve the conductivity of the control layer, reduce the transport resistance of N-type current in the vertical direction, and ensure that the current can smoothly pass through the light-emitting morphology control layer and be injected into the multi-quantum-well active layer, avoiding the increase in device series resistance or the current crowding effect caused by the introduction of the light-emitting morphology control layer. At the same time, the above-mentioned Si doping concentration range can ensure sufficient carrier concentration to meet the current expansion requirements, while avoiding the introduction of impurity scattering and free carrier absorption loss due to excessive doping concentration.
[0015] Preferably, after laser stripping, the surface of the light-emitting morphology control layer is exposed on the side away from the multi-quantum-well active layer, and the light-emitting microstructure is formed by etching the surface; the etching is selected from inductively coupled plasma (ICP) dry etching, photoelectrochemical etching, wet etching, and combinations thereof.
[0016] Specifically, laser lift-off can precisely remove the original growth substrate and expose the predetermined surface of the light morphology control layer, so that the etching start surface of the light-emitting microstructure corresponds precisely to the starting position of the composition gradient. This ensures that the etching process can fully utilize the composition gradient distribution of the entire control layer to induce the formation of tilted sides. On the other hand, the selection and combination of various etching methods can adapt to different Al composition gradient distributions and different microstructure morphology requirements. Among them, dry etching can achieve precise morphology control with high anisotropy, photoelectrochemical etching can achieve highly selective etching based on the differences in the electrical properties of materials, and wet etching has the advantages of simple process and low damage. By combining these methods, the smoothness, tilt angle uniformity and etching damage of the tilted sides can be further optimized, thereby obtaining a light-emitting morphology that is more conducive to light extraction.
[0017] Preferably, the light-emitting microstructure is selected from slope structure, cone structure, step structure, pit structure and combination thereof.
[0018] Specifically, the ramp structure provides a continuous and gradual refractive index transition, effectively reducing Fresnel reflection at the interface; the conical structure can change the incident direction of light within a wide angle range, allowing more light to exit at an angle less than the critical angle; the stepped structure can gradually reduce light reflection through multiple refractive index steps; and the pit structure can increase the number of light scatterings at the light-emitting surface and provide multiple exit windows, further improving light extraction efficiency. The combined use of multiple structures can also achieve synergistic effects, simultaneously enhancing light output on light rays at different angles and in different modes, thereby maximizing the extraction efficiency of deep ultraviolet light.
[0019] Preferably, the angle between the inclined side and the thickness direction of the light-emitting morphology control layer is 10° to 75°.
[0020] Specifically, since the refractive index of AlGaN material is about 2.0 to 2.5, the critical angle for total internal reflection on the air side is about 24° to 30°. When the angle between the tilted side and the thickness direction is in the range of 10° to 75°, the light that was originally incident at a large angle to the light-emitting interface can be converted into effective emitted light with an incident angle less than the critical angle. The smaller tilt angle is suitable for improving the light emission in the near-normal direction, while the larger tilt angle has a more significant effect on enhancing the emission of large-angle light. By controlling the angle within this range, the effective refraction of the tilted side for total internal reflection can be guaranteed, while avoiding the morphology being close to a plane and the light emission enhancement effect being insignificant due to the tilt angle being too small. At the same time, it is prevented that the duty cycle of the microstructure is too high due to the tilt angle being too large, which would affect the electrical contact performance and mechanical stability of the device.
[0021] Preferably, the thickness of the N-type semiconductor layer is 500–4000 nm, and the N-type semiconductor layer includes at least one of an N-type contact layer and a current spreading layer; both the N-type contact layer and the current spreading layer are Si-doped AlGaN materials, with an Al molar composition of 0.40–0.90 and a Si doping concentration of 1 × 10⁻⁶. 18 ~5×10 19 cm -3 .
[0022] Specifically, the aforementioned thickness range ensures that the N-type semiconductor layer has sufficient current spreading capability, allowing the current to spread laterally before being injected into the multi-quantum-well active layer to improve current distribution uniformity, while avoiding increased series resistance and light absorption loss due to excessive thickness. On the other hand, the Al composition range of 0.40–0.90 can achieve good matching with the Al composition of the multi-quantum-well active layer and the light-emitting morphology control layer, reducing interface bandgap and lattice mismatch, while 1×10⁻⁶… 18 ~5×10 19 cm -3 The Si doping concentration ensures good ohmic contact and low resistance while effectively controlling the free carrier absorption loss in the deep ultraviolet band, thus balancing the electrical and optical performance of the device.
[0023] More preferably, the N-type semiconductor layer includes an N-type contact layer and a current spreading layer from top to bottom.
[0024] Specifically, the upper N-type contact layer can use a higher doping concentration or an AlGaN material with an appropriate Al composition to reduce contact resistance; while the lower current spreading layer can optimize the Al composition and doping concentration to achieve sufficient lateral current spreading while maintaining good conductivity, so that the current is evenly distributed throughout the active region, avoiding local overheating and efficiency degradation caused by current crowding effect.
[0025] Preferably, the P-type semiconductor layer comprises, from top to bottom, a carrier control layer and a P-type contact layer, wherein the P-type contact layer is directly or indirectly electrically connected to the P-type electrode, and both the carrier control layer and the P-type contact layer are P-type doped AlGaN materials; the carrier control layer comprises at least one of a P-type AlGaN electron blocking layer, a P-type AlGaN superlattice layer, and a P-type AlGaN composition gradient layer.
[0026] Specifically, the carrier control layer is positioned close to the active region, which can block electron leakage and improve hole injection, thereby improving the carrier distribution and recombination efficiency in the active region; the P-type contact layer ensures good ohmic contact with the P-type electrode, thus achieving the dual goals of carrier control and low contact resistance on the P-type side.
[0027] Furthermore, the P-type AlGaN electron blocking layer utilizes the conduction band barrier formed by the high Al composition to effectively prevent electrons in the active region from overflowing to the P-type side, reducing electron leakage losses and improving the recombination efficiency of charge carriers in the active region; the P-type AlGaN superlattice layer forms microstrip transport channels through periodically alternating AlGaN structures, which can enhance hole transport and injection efficiency, and also utilize the effective barrier of the superlattice to block electron leakage, thus having the dual functions of hole injection enhancement and electron blocking; the P-type AlGaN composition gradient layer forms a gradient valence band through the gradient change of Al composition, reducing the potential peak of hole injection, making hole injection smoother and more uniform, and at the same time, it can also block electron overflow to a certain extent, thereby improving the carrier distribution and recombination uniformity in the active region.
[0028] Preferably, the P-type electrode is a reflective electrode material, which is used to reflect the deep ultraviolet light propagating toward the P-type electrode side to the main light-emitting side of the vertical deep ultraviolet LED.
[0029] Specifically, the P-type electrode adopts a reflective electrode structure, which can reflect the deep ultraviolet light propagating towards the P-type electrode side back into the device and finally emit it from the main light-emitting side, effectively reducing the light absorption loss on the P-type side and the substrate side and significantly improving the light extraction efficiency. The reflective electrode combined with the vertical structure can give full play to the advantages of the vertical structure in heat dissipation and current distribution, while improving the external quantum efficiency through optical design.
[0030] The beneficial effects of this invention are as follows: Unlike existing technologies, this invention provides a vertical deep ultraviolet LED with a light-emitting morphology control structure. It utilizes a light-emitting morphology control layer formed near the main light-emitting side of the N-type semiconductor layer, where the Al molar composition decreases continuously or in a stepped manner along the direction away from the multi-quantum-well active layer. Taking advantage of the significant differences in etching response rates of AlGaN materials with different Al compositions, this light-emitting morphology control layer, during the etching process to form the light-emitting microstructure, induces the formation of a microstructure with tilted sides along the thickness direction due to the gradient etching rate. This tilted side alters the incident angle of deep ultraviolet light at the light-emitting interface, allowing more light to escape from the chip at an angle less than the critical angle of total internal reflection. Furthermore, the pre-set composition gradient template in the epitaxial stage enables active control of the light-emitting morphology, fundamentally solving the problems of high randomness and poor consistency in existing roughening processes. Ultimately, this significantly improves the light extraction efficiency of deep ultraviolet LEDs and the stability and repeatability of device performance. Attached Figure Description
[0031] Figure 1 This is a schematic diagram of the cross-sectional structure of the vertical deep ultraviolet LED provided in Embodiment 1; In the accompanying drawings: 11—N-type electrode; 12—N-type semiconductor layer; 13—Multi-quantum well active layer; 14—P-type semiconductor layer; 141—Carrier control layer; 142—P-type contact layer; 15—P-type electrode; 16—Supporting substrate; 17—Light emission morphology control layer. Detailed Implementation
[0032] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0033] The technical solution of this application will now be described in conjunction with specific embodiments.
[0034] Example 1 (The thickness of the light-emitting morphology control layer 17 is 300 nm, and its Al composition has a continuously decreasing gradient): Please see Figure 1 , Figure 1 This is a schematic diagram of the cross-sectional structure of the vertical deep ultraviolet LED provided in Embodiment 1; the vertical deep ultraviolet LED with the light emission morphology control structure includes, from top to bottom, an N-type electrode 11, an N-type semiconductor layer 12, a multi-quantum well active layer 13, a P-type semiconductor layer 14, a P-type electrode 15 and a supporting substrate 16. Among them, a light-emitting morphology control layer 17 is provided between the N-type electrode 11 and the N-type semiconductor layer 12; the light-emitting morphology control layer 17 is made of AlGaN material, and its Al molar composition decreases continuously or stepwise along the direction away from the multi-quantum-well active layer 13; a light-emitting microstructure with an inclined side is formed on the surface of the light-emitting morphology control layer 17 away from the multi-quantum-well active layer 13.
[0035] In Example 1, the N-type electrode 11 can adopt a single-layer or multi-layer metal structure, and the metal material is selected from one or more of Ti, Al, Ni, Au, Cr, Pt, Ta, Cu, and Ag. Preferably, the N-type electrode 11 adopts a Ti / Al / Ni / Au multi-layer metal structure, wherein the Ti layer is in contact with the N-type AlGaN layer to form an ohmic contact, and the Au layer serves as a conductive and connecting metal layer. The thickness of the Au layer is 1 to 4 μm, preferably 2 μm.
[0036] In Example 1, the light emission morphology control layer 17 is made of Si-doped AlGaN material with a thickness of 300 nm and a Si doping concentration of 5 × 10⁻⁶. 18 cm -3 The Al molar composition of the light-emitting morphology control layer 17 decreases continuously along the direction away from the multi-quantum-well active layer 13; the Al molar composition of the light-emitting morphology control layer 17 is 0.7 on the side closer to the multi-quantum-well active layer and 0.4 on the side closer to the laser stripping interface and the main light-emitting side, with a change in Al molar composition of 0.30.
[0037] In Example 1, the N-type semiconductor layer 12 is located on the lower surface of the light emission morphology control layer 17. The N-type semiconductor layer 12 is an N-type AlGaN current spreading layer used to realize vertical current transport and lateral current spreading. The Al molar composition of the N-type semiconductor layer 12 is 0.65, the thickness is 1500 nm, and the Si doping concentration is 8 × 10⁻⁶. 18 cm -3 .
[0038] In this embodiment 1, the multi-quantum-well active layer 13 is located on the lower surface of the N-type semiconductor layer 12 and is composed of 2 to 20 cycles of AlGaN quantum well / quantum barrier structures (5 cycles in this embodiment 1). The thickness of the AlGaN quantum well is 0.1 to 5 nm (approximately 2 nm in this embodiment 1), and the Al composition is 0 to 0.8 (0.45 in this embodiment 1); the thickness of the AlGaN quantum barrier is 5 to 30 nm (approximately 10 nm in this embodiment 1), and the Al composition is 0.2 to 1 (0.65 in this embodiment 1). In this embodiment 1, by adjusting the Al molar composition in the AlGaN quantum well, deep ultraviolet light emission in the 200 to 310 nm wavelength band can be achieved (the emission wavelength in this embodiment 1 is 275 nm).
[0039] In this embodiment 1, the P-type semiconductor layer 14 is located on the lower surface of the multi-quantum-well active layer 13; the P-type semiconductor layer 14 includes a carrier control layer 141 and a P-type contact layer 142 from top to bottom, and the P-type contact layer 142 is directly or indirectly electrically connected to the P-type electrode 15. Both the carrier control layer 141 and the P-type contact layer 142 are P-type doped AlGaN materials.
[0040] Specifically, the carrier control layer 141 is a p-type AlGaN electron blocking layer made of Mg-doped AlGaN material, with a thickness of 20 nm, an Al molar composition of 0.80, and a Mg doping concentration of 5 × 10⁻⁶. 19 cm -3 .
[0041] Specifically, the P-type contact layer 142 is used to realize hole injection and to make ohmic contact with the P-type electrode 15; the P-type contact layer 142 is made of Mg-doped AlGaN material with a thickness of 1-100 nm (approximately 20 nm in this embodiment 1), an Al molar composition of 0.45, and a Mg doping concentration of 1×10⁻⁶. 19 ~1×10 21 cm -3 (This Example 1 is 8×10) 19 cm -3 ).
[0042] In this embodiment 1, the P-type electrode 15 is an electrode material that reflects deep ultraviolet light and serves as the second electrode of a vertical deep ultraviolet LED. The material of the P-type electrode 15 is selected from one or more of Rh, Ru, Ir, Os, Cr, W, Al, Au, Ni, Ti, Pt, and ITO. It can be a single-layer structure or a multi-layer stacked structure with a thickness of 5–70 nm (in this embodiment 1, a single-layer Rh structure with a thickness of approximately 30 nm is used). The Rh material has a high reflectivity to deep ultraviolet light and can form a good ohmic contact with the P-type contact layer 142.
[0043] In this embodiment 1, the support substrate 16 is used to support the chip and conduct current. The material can be a doped semiconductor material (such as an N-type or P-type Si substrate) or a metal substrate with a thickness of 100 to 2000 μm (in this embodiment 1, an N-type Si substrate with a thickness of about 300 μm is used).
[0044] In this embodiment 1, the fabrication method of the vertical deep ultraviolet LED includes the following steps: Step (1) Surface Cleaning: The epitaxial wafer with the light-emitting morphology control structure is placed in a cleaning basket and ultrasonically cleaned sequentially with acetone, isopropanol, and SPM solution (sulfuric acid-hydrogen peroxide mixture) to remove organic impurities from the surface of the epitaxial wafer. Then, it is rinsed with deionized water for 5 minutes to ensure no residual reagents remain on the surface. Finally, it is placed in a spin dryer to obtain a clean epitaxial wafer. The epitaxial wafer, from bottom to top, comprises a sapphire substrate, an AlN low-temperature buffer layer, an intrinsic layer, a sacrificial layer, a light-emitting morphology control layer 17, an N-type semiconductor layer 12, a multi-quantum-well active layer 13, and a P-type semiconductor layer 14, and is epitaxially grown using MOCVD technology. The SPM solution is a mixture of concentrated sulfuric acid and hydrogen peroxide, with a mixing ratio typically between 3:1 and 7:1 (4:1 in Example 1), which effectively removes organic matter and metallic impurities from the surface.
[0045] Specifically, the aforementioned MOCVD technology is mainly implemented in the VeecoK 465i MOCVD equipment. High-purity H2, high-purity N2, or a mixture of high-purity H2 and high-purity N2 are used as the carrier gas, high-purity NH3 as the N source, trimethylgallium (TMGa) as the gallium source, trimethylaluminum (TMAl) as the Al source, silane (SiH4) as the N-type dopant, and magnesium dicthene (CP2Mg) as the P-type dopant. The pressure in the reaction chamber of the MOCVD equipment is controlled between 20 and 100 torr.
[0046] Specifically, the epitaxial growth steps of the epitaxial wafer with a light-emitting morphology control structure are as follows: Step (1.1): Place the sapphire substrate in the MOCVD equipment and grow an AlN low-temperature buffer layer on the sapphire substrate at 400℃~800℃ (650℃ in this embodiment 1), with a thickness of 10~50nm (25nm in this embodiment 1).
[0047] Step (1.2): Heat to 1200-1400℃ (1300℃ in this example 1) to grow an intrinsic AlN layer (AlN high-temperature buffer layer) with a thickness of 500-4000nm (2000nm in this example 1) to alleviate the lattice mismatch between the sapphire substrate and the AlGaN material and improve the quality of the epitaxial crystal.
[0048] Step (1.3): Cool down to 600℃~1100℃ (1100℃ in this embodiment 1) and grow a sacrificial layer (lifting aid layer). The sacrificial layer is a single layer or multiple layers of AlGaN or GaN (a single layer AlGaN structure in this embodiment 1). The Al composition of the sacrificial layer is 0.01~0.95 (0.35 in this embodiment 1) and the thickness is 1~300nm (80nm in this embodiment 1). It is used for subsequent substrate lift-off or epitaxial structure transfer and reduces damage to the N-type semiconductor layer 12 and the light emission morphology control layer 17 during laser lift-off.
[0049] Step (1.4): Maintaining a constant temperature, grow a light morphology control layer 17 on the sacrificial layer; the light morphology control layer 17 is made of Si-doped AlGaN material, with a thickness of 300 nm and a Si doping concentration of 5 × 10⁻⁶. 18 cm -3 The Al molar composition of the light-emitting morphology control layer 17 is 0.7 on the side near the multi-quantum well active layer and 0.4 on the side near the laser lift-off interface and the main light-emitting side, with a change of 0.30 in Al molar composition. The Al molar composition of the light-emitting morphology control layer 17 decreases continuously along the direction away from the multi-quantum well active layer 13, so that the main light-emitting side exposed after laser lift-off has pre-designed etching response characteristics, improving the controllability of subsequent formation of tilted light-emitting microstructures.
[0050] Step (1.5): Cool to 800–1200℃ (1000℃ in Example 1), and grow an N-type semiconductor layer 12 on the light-emitting morphology control layer 17; wherein, the N-type semiconductor layer 12 is an N-type AlGaN current spreading layer, used to realize vertical current transport and lateral current spreading; the Al molar composition of the N-type semiconductor layer 12 is 0.65, the thickness is 1500 nm, and the Si doping concentration is 8 × 10⁻⁶. 18 cm -3 .
[0051] Step (1.6): Cool down to 700℃~1100℃ (900℃ in this example 1) to grow a multi-quantum-well active layer 13, which consists of 5 periods of AlGaN quantum well / quantum barrier structure: the thickness of AlGaN quantum well is 2nm and the Al composition is 0.45; the thickness of AlGaN quantum barrier is 10nm and the Al composition is 0.65.
[0052] Step (1.7): Maintaining a constant temperature, grow a carrier control layer 141 on the multi-quantum-well active layer 13. The carrier control layer 141 includes a p-type AlGaN electron blocking layer to suppress electron leakage to the p-side and improve hole injection. The p-type AlGaN electron blocking layer is made of Mg-doped AlGaN material with a thickness of 20 nm, an Al molar composition of 0.8, and a Mg doping concentration of 5 × 10⁻⁶.19 cm -3 .
[0053] Step (1.8): Maintaining a constant temperature, grow a P-type contact layer 142 on the carrier control layer 141; the P-type contact layer 142 is made of Mg-doped AlGaN material, with a thickness of 20 nm, an Al molar composition of 0.45, and a Mg doping concentration of 8 × 10⁻⁶. 19 cm -3 .
[0054] Step (2) Fabrication of P-type electrode 15: After epitaxial growth, P-type electrode 15 is fabricated on the surface of the P-type contact layer 142 away from the multi-quantum-well active layer 13 using electron beam evaporation or sputtering technology. The P-type electrode 15 is a deep ultraviolet reflective electrode, used to form an electrical connection with the P-type contact layer 142 and reflect the deep ultraviolet light propagating towards the P-type electrode 15 to the main light-emitting side. The material of the P-type electrode 15 is selected from one or more of Rh, Ru, Ir, Os, Cr, W, Al, Au, Ni, Ti, Pt, and ITO. It can be a single-layer structure or a multi-layer stacked structure with a thickness of 5-70 nm (in this embodiment 1, a single-layer Rh structure with a thickness of approximately 30 nm is used). The evaporation / sputtering rate is 0.1-10 nm / s (in this embodiment 1, the evaporation rate is 0.5 nm / s).
[0055] Step (3) Bonding of the epitaxial structure to the support substrate 16: Using electron beam evaporation or sputtering technology, a bonding layer is simultaneously prepared on the surface of the P-type electrode 15 away from the multi-quantum-well active layer 13 and on the surface of the support substrate 16. The material mainly includes at least one of Cr, Ni, Pt, Ti, Au, Sn, Cu, Ag, and Ta, with Au-Sn alloy preferred. The thickness is 100-3000 nm (Au-Sn alloy with a thickness of 1000 nm is used in Example 1), and the evaporation / sputtering rate is 0.1-5 nm / s (evaporation rate of 0.5 nm / s in Example 1). The support substrate 16 can be a doped semiconductor material (such as an N-type or P-type Si substrate) or a metal substrate. The thickness of the support substrate 16 is 100-2000 μm (N-type Si substrate with a thickness of 300 μm is used in Example 1) to support the chip and conduct current.
[0056] Step (4) Sapphire substrate stripping: Align the epitaxial chip with the bonding layer with the support substrate 16, and bond it in a vacuum environment at a temperature of 100-500℃ and a pressure of 1-5MPa (bonding is performed at 300℃ and 3MPa in this embodiment 1). The bonding time is 10-120min (60min in this embodiment 1) to ensure a firm bond and no bubbles. After bonding, the sapphire substrate, AlN low-temperature buffer layer and AlN intrinsic layer used for epitaxial growth are completely stripped and removed by laser stripping process to expose the surface of the light-emitting morphology control layer 17 away from the multi-quantum-well active layer 13. If there is a residual sacrificial layer on the surface of the light-emitting morphology control layer 17 away from the multi-quantum-well active layer 13, the residual sacrificial layer can be removed by short-term etching pretreatment to expose at least part of the light-emitting morphology control layer 17.
[0057] Step (5) Etching of the main light-emitting side surface of the light-emitting morphology control layer 17: ICP dry etching is performed on the exposed main light-emitting side of the light-emitting morphology control layer 17. Since the light-emitting morphology control layer 17 has an Al composition gradient along the thickness direction, and the side closer to the main light-emitting side is a region with a lower Al composition and the side closer to the multi-quantum well active layer 13 is a region with a higher Al composition, different Al composition regions have different etching rates and etching responses during the etching process, so that the main light-emitting side forms an inclined light-emitting microstructure composed of a ramp structure, a step structure and a pit structure; wherein, the angle between the inclined surface of the inclined light-emitting microstructure and the thickness direction of the light-emitting morphology control layer 17 is 35° to 55°.
[0058] Step (6) Fabrication of N-type electrode 11: An N-type electrode 11 is fabricated in a localized area on the main light-emitting side using electron beam evaporation technology, so that the N-type electrode 11 forms an electrical connection with the N-type conductive region. The N-type electrode 11 adopts a multilayer metal structure, with each metal layer sequentially deposited on the surface of the N-type conductive region. In this embodiment 1, the N-type electrode 11 adopts a Ti / Al / Ni / Au multilayer metal structure, wherein the thickness of the Ti layer is 10-100 nm, the thickness of the Al layer is 50-500 nm, the thickness of the Ni layer is 10-100 nm, and the thickness of the Au layer is 1-4 μm, preferably about 2 μm.
[0059] Step (7) Chip dicing and testing: The prepared chip wafer is diced into individual chips using a dicing machine. The dicing width is 20-100μm (50μm in Example 1). After dicing, the individual chips are subjected to electrical performance, optical performance and reliability tests. If the tests are qualified, they are the finished vertical deep ultraviolet LED chips.
[0060] Examples 2A-2D (the thicknesses of the light-emitting morphology control layer 17 are 100 nm, 200 nm, 500 nm, and 800 nm, respectively, and its Al composition has a continuously decreasing gradient): Examples 2A to 2D provide four vertical deep ultraviolet LEDs with light emission morphology control structures. Their specific structural parameters and preparation methods are roughly the same as those of Example 1, with the only difference being that the thickness of the light emission morphology control layer 17 in Example 2A is 100 nm; the thickness of the light emission morphology control layer 17 in Example 2B is 200 nm; the thickness of the light emission morphology control layer 17 in Example 2C is 500 nm; and the thickness of the light emission morphology control layer 17 in Example 2D is 800 nm.
[0061] Example 3 (the thickness of the light-emitting morphology control layer 17 is 300 nm, and its Al composition has a stepwise gradient reduction): Example 3 provides a vertical deep ultraviolet LED with a light emission morphology control structure. Its specific structural parameters and fabrication method are largely the same as those of Example 1, except that the light emission morphology control layer 17 in Example 3 comprises, from top to bottom, a first sublayer, a second sublayer, and a third sublayer stacked together. The first sublayer is made of Si-doped AlGaN material with a thickness of 100 nm and a Si doping concentration of 5 × 10⁻⁶. 18 cm -3 The Al molar composition is 0.4; the second sublayer is Si-doped AlGaN material with a thickness of 100 nm and a Si doping concentration of 5 × 10⁻⁶. 18 cm -3 The Al molar composition is 0.55; the third sublayer is Si-doped AlGaN material with a thickness of 100 nm and a Si doping concentration of 5 × 10⁻⁶. 18 cm -3 The molar composition of Al is 0.7.
[0062] Comparative Example 1 (Vertical deep ultraviolet LED without light emission morphology control structure): Comparative Example 1 provides a vertical deep ultraviolet LED 100 without a light emission morphology control structure. Its specific structural parameters and preparation method are roughly the same as those of Example 1. The only difference is that the light emission morphology control layer 17 is not provided between the N-type electrode 11 and the N-type semiconductor layer 12. The rest of the structure and preparation process are the same as those of Example 1.
[0063] Comparative Example 2 (the thickness of the light-emitting morphology control layer 17 is 300 nm, and its Al composition is constant): Comparative Example 2 provides a vertical deep ultraviolet LED, whose specific structural parameters and preparation method are largely the same as those of Example 1. The only difference is that the light emission morphology control layer 17 in Comparative Example 2 is made of Si-doped AlGaN material with a thickness of 300 nm and a Si doping concentration of 5 × 10⁻⁶. 18 cm -3The Al molar composition is constant at 0.55.
[0064] Results and Analysis: The samples from Examples 1, 2A-2D, 3, and Comparative Examples 1-2 were tested for forward voltage, optical output power, electro-optical conversion efficiency, and average tilt angle at room temperature and an injection current of 100mA. The test results are shown in Tables 1 and 2 below: Table 1. Test results of Examples 1, 2A-2D and Comparative Example 1
[0065] Table 2 Test results of Example 1, Example 3 and Comparative Example 2
[0066] Specifically, the vertical deep ultraviolet LED chip prepared in Example 1 was tested. Under the conditions of room temperature and injection current of 100mA, the device forward voltage was 5.59V, the peak wavelength was 275nm, the light output power was 98.1mW, and the electro-optical conversion efficiency was 17.55%. Compared with Comparative Example 1 without a light-emitting morphology control layer, the vertical deep ultraviolet LED chip prepared in Example 1 has a more uniform tilted light-emitting microstructure on the main light-emitting side, and the light output power and electro-optical conversion efficiency are significantly improved.
[0067] As can be seen from the relative performance test results in Table 1, when the light-emitting morphology control layer 17 is not set, the etching morphology on the main light-emitting side is mainly formed randomly by the etching process, with a small average tilt angle and insufficient tilted light-emitting microstructures. Strong total internal reflection still exists on the main light-emitting side for deep ultraviolet light. With the addition of the light-emitting morphology control layer 17, as the thickness of the layer increases, the control effect of the Al composition gradient on the etching morphology is enhanced. It becomes easier to form light-emitting microstructures with tilted surfaces on the main light-emitting side, thereby improving the light output power and electro-optical conversion efficiency.
[0068] Furthermore, when the thickness of the light-emitting morphology control layer 17 is 200–500 nm, it can balance morphology control and current transport performance, resulting in high device optical output power and electro-optical conversion efficiency. When the thickness of the light-emitting morphology control layer 17 is further increased to 800 nm, although the tilted light-emitting microstructure can still be formed, the larger thickness of the light-emitting morphology control layer 17 may introduce additional series resistance or epitaxial stress, leading to a slight increase in forward voltage and limiting the improvement in device efficiency. Therefore, the thickness of the light-emitting morphology control layer 17 in this invention is preferably 200–500 nm.
[0069] As can be seen from the relative performance test results in Table 2, when the light-emitting morphology control layer 17 does not have an Al composition gradient, even with the same etching process, the microstructure formed on the main light-emitting side is still relatively random, with a low proportion of tilted surfaces, resulting in limited improvement in light extraction efficiency. When the light-emitting morphology control layer 17 adopts a continuous gradient or stepped gradient structure, due to the different Al compositions near the main light-emitting side and near the multi-quantum-well active layer 13, different depth regions produce different etching responses during the etching process. The main light-emitting side is more likely to form light-emitting microstructures with predetermined tilted surfaces, thereby increasing the probability of deep ultraviolet light emanating from the main light-emitting side. The continuous gradient structure in Example 1 has a smoother etching response, while the stepped gradient structure in Example 3 is easier to achieve through multilayer epitaxial growth. Both can achieve the light-emitting morphology control effect of the present invention.
[0070] In summary, this invention, by pre-setting a light-emitting morphology control layer 17 with an Al composition gradient on the main light-emitting side of a vertical deep ultraviolet LED, and by reducing the Al composition along the direction away from the multi-quantum-well active layer 13, enables the formation of a light-emitting microstructure with an inclined surface on the main light-emitting side during the etching process after laser stripping. Compared with structures without a light-emitting morphology control layer 17 or without an Al composition gradient, this invention can improve the consistency and controllability of the light-emitting morphology on the main light-emitting side, reduce total internal reflection of deep ultraviolet light on the main light-emitting side, and improve light output power and electro-optical conversion efficiency.
[0071] It should be noted that all the above embodiments belong to the same inventive concept, and the descriptions of each embodiment have different focuses. Where the description in a particular embodiment is not detailed, please refer to the description in other embodiments.
[0072] The above embodiments merely illustrate implementation methods of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A vertical deep ultraviolet LED with a light emission morphology control structure, characterized in that, From top to bottom, it includes an N-type electrode, an N-type semiconductor layer, a multi-quantum-well active layer, a P-type semiconductor layer, a P-type electrode, and a supporting substrate; The light-emitting morphology control layer is provided between the N-type electrode and the N-type semiconductor layer; the light-emitting morphology control layer is made of AlGaN material, and its Al molar composition decreases continuously or stepwise along the direction away from the multi-quantum-well active layer; the surface of the light-emitting morphology control layer away from the multi-quantum-well active layer has a light-emitting microstructure with an inclined side.
2. The vertical deep ultraviolet LED with light emission morphology control structure according to claim 1, characterized in that, The thickness of the light-emitting morphology control layer is 100–800 nm, and the total variation of its Al molar composition is 0.2–0.
5.
3. The vertical deep ultraviolet LED with light emission morphology control structure according to claim 2, characterized in that, The Al molar composition content of the light-emitting morphology control layer on the surface near the multi-quantum well active layer is a, and the Al molar composition on the surface near the N-type electrode is b; wherein a and b satisfy the following relationship: 0.55≤a≤0.85, 0.35≤b≤0.60, and a>b.
4. The vertical deep ultraviolet LED with a light emission morphology control structure according to claim 1, characterized in that, The light emission morphology control layer is made of Si-doped AlGaN material, with a Si doping concentration of 1×10⁻⁶. 17 ~5×10 19 cm -3 .
5. The vertical deep ultraviolet LED with light emission morphology control structure according to claim 1, characterized in that, After laser ablation, the surface of the light-emitting morphology control layer is exposed on the side away from the multi-quantum-well active layer. The light-emitting microstructure is formed by etching the surface. The etching is selected from inductively coupled plasma dry etching, photoelectrochemical etching, wet etching, and combinations thereof.
6. The vertical deep ultraviolet LED with light emission morphology control structure according to claim 5, characterized in that, The light-emitting microstructure is selected from slope structure, cone structure, step structure, pit structure and combination thereof.
7. The vertical deep ultraviolet LED with light emission morphology control structure according to claim 5, characterized in that, The angle between the inclined side and the thickness direction of the light-emitting morphology control layer is 10° to 75°.
8. The vertical deep ultraviolet LED with light emission morphology control structure according to claim 1, characterized in that, The thickness of the N-type semiconductor layer is 500–4000 nm, and the N-type semiconductor layer includes at least one of an N-type contact layer and a current spreading layer; both the N-type contact layer and the current spreading layer are Si-doped AlGaN materials, with an Al molar composition of 0.40–0.90 and a Si doping concentration of 1 × 10⁻⁶. 18 ~5×10 19 cm -3 .
9. The vertical deep ultraviolet LED with a light emission morphology control structure according to claim 1, characterized in that, The P-type semiconductor layer comprises, from top to bottom, a carrier control layer and a P-type contact layer. The P-type contact layer is directly or indirectly electrically connected to the P-type electrode. Both the carrier control layer and the P-type contact layer are P-type doped AlGaN materials. The carrier control layer includes at least one of the following: a P-type AlGaN electron blocking layer, a P-type AlGaN superlattice layer, and a P-type AlGaN composition gradient layer.
10. The vertical deep ultraviolet LED with a light emission morphology control structure according to claim 1, characterized in that, The P-type electrode is a reflective electrode material, which is used to reflect deep ultraviolet light propagating toward the P-type electrode to the main light-emitting side of the vertical deep ultraviolet LED.