A Brightening Structure for a Micro-LED Vertical Chip and Its Fabrication Method

By setting a highly reflective metal fence in the inter-pixel grooves of the Micro-LED vertical chip, the problems of light crosstalk and low light extraction efficiency are solved, thereby improving the display contrast and brightness, making it suitable for mass production.

CN123124555APending Publication Date: 2026-11-17WEIJIU (SUZHOU) OPTOELECTRONICS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611619003.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing Micro-LED vertical chips suffer from optical crosstalk and low light extraction efficiency during manufacturing. Existing dielectric layers cannot effectively isolate optical crosstalk between pixels and have complex fabrication processes, which cannot meet the needs of mass production.

Method used

A highly reflective metal fence is set in the trench between pixels, and a metal fence reflective layer is formed by eutectic bonding and etching processes to achieve optical crosstalk isolation between pixels and improve the output brightness.

Benefits of technology

It effectively suppresses optical crosstalk, improves display contrast and light extraction efficiency, and is compatible with existing semiconductor manufacturing processes, making it suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124555A_ABST
    Figure CN123124555A_ABST
Patent Text Reader

Abstract

This application discloses a brightness enhancement structure for a vertical Micro-LED chip and its fabrication method, belonging to the field of semiconductor display technology. The structure features a highly reflective metal fence within the trenches between periodically arrayed LED pixel units, surrounding the sidewalls of each pixel. This simultaneously achieves physical isolation of inter-pixel crosstalk and reflection and recovery of lateral light emission, effectively suppressing crosstalk and significantly improving chip brightness and display contrast. The invention provides two fabrication methods: a double-layer positive adhesive undercut process and a negative adhesive undercut process. Both can form adhesive hole patterns with undercut morphology. Combined with metal evaporation and stripping processes, a well-defined metal fence is obtained. The process is fully compatible with existing semiconductor mass production processes. This invention is adaptable to high-reliability scenarios, high-resolution small-size pixels, and 12-inch wafer mass production requirements. It boasts high yield, controllable cost, and can be widely applied to the manufacturing of various Micro-LED display chips.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor optoelectronic device technology, and in particular to a brightness enhancement structure for a Micro-LED vertical chip and its fabrication method. Background Technology

[0002] Micro-LED (micro-light-emitting diode) display technology boasts advantages such as high brightness, high contrast, low power consumption, and long lifespan, making it a core development direction for next-generation display technology. Vertical-structure Micro-LED chips, which bond gallium nitride epitaxial wafers to a silicon substrate with driving circuitry and then peel off a sapphire growth substrate, exhibit characteristics such as uniform current distribution, excellent heat dissipation, and high luminous efficiency, and have become the mainstream technology solution for high-resolution Micro-LED displays.

[0003] In the manufacturing process of vertical Micro-LED chips, after the growth substrate is peeled off, the buffer layer needs to be removed to expose the n-type gallium nitride layer, and then an etch process is used to form a periodic array of LED pixels. However, the existing chip structure has two core problems in practical applications: first, there is optical crosstalk between pixels, with the lateral emission of adjacent pixels penetrating each other, which seriously reduces the display contrast; second, the lateral emission of a single pixel cannot be effectively exported, resulting in low light extraction efficiency and insufficient brightness of a single pixel.

[0004] In existing technologies, isolation is usually achieved by filling the pixels with dielectric layers such as silicon oxide and silicon nitride. However, the dielectric can only perform electrical isolation and has no reflective effect on lateral light emission, so it cannot improve the brightness problem. Some solutions use distributed Bragg reflector layers as isolation structures, but the fabrication process of this structure is complex and it is difficult to grow uniformly in pixel trenches with high aspect ratios. The manufacturing cost is high and the yield is low, which cannot meet the needs of mass production. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a brightening structure for a Micro-LED vertical chip and its preparation method. By setting a high-reflectivity metal fence in the trench between pixels, it can simultaneously achieve optical crosstalk isolation between pixels and improve the output brightness. Moreover, the process is compatible with existing semiconductor manufacturing processes and can be mass-produced.

[0006] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: A brightness enhancement structure for a vertical Micro-LED chip includes a driving substrate, a bonding metal layer, a gallium nitride epitaxial wafer, and a metal fence reflective layer. The gallium nitride epitaxial wafer is eutectic bonded to the driving substrate through the bonding metal layer; the gallium nitride epitaxial wafer is etched to form periodically arrayed LED pixel units, and trenches are formed between adjacent LED pixel units; The metal fence reflective layer fills the trench and surrounds the sidewalls of each LED pixel unit to reflect the lateral light emitted by the LED pixel unit, thereby isolating light crosstalk between pixels and improving the brightness of the chip.

[0007] In a preferred embodiment, the metal fence reflective layer comprises an adhesive layer and a highly reflective metal layer; the adhesive layer is a chromium layer or a titanium layer with a thickness of 5~50nm; the highly reflective metal layer is a silver-aluminum alloy layer with a thickness of 800~1200nm.

[0008] In a preferred embodiment, the height of the metal fence reflective layer is not lower than the height of the upper surface of the quantum well layer within the LED pixel unit.

[0009] In a preferred embodiment, the LED pixel unit comprises, from the side closest to the driving substrate to the light-emitting side, a p-type gallium nitride layer, a quantum well layer, and an n-type gallium nitride layer in sequence; the bonding metal layer comprises a first bonding metal layer and a second bonding metal layer, the first bonding metal layer being disposed on the surface of the driving substrate, and the second bonding metal layer being disposed on the p-type side of the gallium nitride epitaxial wafer, and the two being eutectic bonded.

[0010] A preferred embodiment further includes a passivation layer and a common n-type transparent conductive layer; The passivation layer covers the light-emitting surface of the LED pixel unit and the surface of the metal fence reflective layer; the passivation layer has contact holes corresponding to the light-emitting area of ​​each LED pixel unit; The common n-type transparent conductive layer is disposed on the surface of the passivation layer and is electrically connected to the n-type gallium nitride layer of each LED pixel unit through the contact hole, thereby realizing the common cathode connection of all LED pixel units.

[0011] This invention also provides a method for fabricating a Micro-LED vertical chip brightening structure, comprising the following steps: S1. A first bonding metal layer is prepared on the surface of the driving substrate, and a transparent conductive film layer and a second bonding metal layer are prepared on the p-type side of the gallium nitride epitaxial wafer. S2. The driving substrate and the gallium nitride epitaxial wafer are bonded together by eutectic bonding to form a bond body. The growth substrate of the gallium nitride epitaxial wafer is peeled off, and the gallium nitride epitaxial wafer is thinned. S3. Photolithography and etching are performed on the thinned gallium nitride epitaxial wafer to form periodically arrayed LED pixel units, with trenches formed between adjacent pixel units; S4. Etch away the bonding metal layer between pixel units to achieve independent anodes for each LED pixel unit; S5. Prepare a photoresist pattern on the chip surface, and form a photoresist hole with an undercut morphology corresponding to the trench position of the photoresist pattern; deposit a high-reflectivity metal layer on the chip surface; remove the photoresist and the surface metal by a stripping process, retaining the metal in the trench to form a metal fence reflective layer; S6. Deposit a passivation layer on the chip surface and etch to form contact holes; prepare a common n-type transparent conductive layer on the passivation layer surface to complete chip fabrication.

[0012] In a preferred embodiment, step S5 involves preparing the photoresist pattern using a double-layer positive resist process, specifically including: S511. Spin-coat a photoresist base coat onto the chip surface after the anode independent etching is completed, and form a base coat layer with a thickness of 200~500nm after soft baking. S512. Spin-coat positive photoresist onto the surface of the base layer, and after soft baking, form a positive photoresist layer with a thickness of 800~1000nm. S513. Exposure is performed through a mask, followed by development with a developer. The positive resist layer in the exposed area reacts with the developer and is removed, while the underlying resist layer in the corresponding position is also dissolved by the developer. The positive resist layer and the underlying resist layer in the unexposed area are retained, forming a resist hole pattern with an undercut morphology.

[0013] In a preferred embodiment, step S5 involves preparing the photoresist pattern using a negative resist process, specifically including: S521. Spin-coat negative photoresist onto the chip surface after independent anodic etching, and form a negative photoresist layer with a thickness of 1000~1500nm after soft baking. S522. Exposure is performed through a mask, followed by development with a developer; the negative adhesive layer in the unexposed area is dissolved and removed by the developer, while the negative adhesive layer in the exposed area is retained, forming an adhesive hole pattern with an undercut morphology.

[0014] In a preferred embodiment, in step S2, the eutectic bonding temperature is 260~350℃, the pressure is 25~80KN, and the bonding time is 10~30min; the growth substrate is removed by laser lift-off, with a laser wavelength of 200~300nm and a frequency of 800~1200Hz, and the stage temperature during lift-off is 20~50℃, using a ring lift-off method from the outside in; after lift-off, the gallium nitride epitaxial wafer is thinned to 1~1.5μm by chemical polishing.

[0015] In a preferred embodiment, in step S3, the gallium nitride epitaxial wafer is etched using inductively coupled plasma etching, and the etching gases are chlorine and boron trichloride, with a gas flow rate of 20~100 sccm. In step S4, the bonding metal layer is etched using an ion beam etching process with an etching angle of 0°~15° and an etching voltage of 300~500V. In step S6, the passivation layer is a silicon oxide layer with a thickness of 300~500nm, prepared by chemical vapor deposition; the common n-type transparent conductive layer is an indium tin oxide layer with a thickness of 300~500nm, prepared by reactive plasma deposition or magnetron sputtering.

[0016] Due to the application of the above technical solution, the beneficial effects of this application compared with the prior art are as follows: 1. Enhanced light efficiency and contrast: The metal fence can physically block the lateral emission of adjacent pixels, effectively suppressing light crosstalk and improving display contrast; at the same time, it reflects and recovers the lateral dissipated light to the light-emitting surface, significantly improving the brightness of a single pixel and the overall light extraction efficiency.

[0017] 2. Strong process compatibility: It provides two photolithography solutions, namely double-layer positive resist and negative resist, both of which can form resist holes with undercut morphology, ensuring complete metal stripping and neat pattern edges. It is fully compatible with existing semiconductor mass production lines and requires no additional special equipment.

[0018] 3. Controllable process and low cost: The height of the metal fence is precisely matched to the quantum well light-emitting area, maximizing the reflection efficiency; the overall process is seamlessly connected with standard processes such as vertical chip bonding, laser lift-off, and etching, with simple process steps, enabling mass production. Attached Figure Description

[0019] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0020] Figure 1 This is a schematic diagram of the structure of step S11 in embodiment S1 of the present invention; Figure 2 This is a schematic diagram of the structure of S12 in step S1 of embodiment one of the present invention; Figure 3 This is a schematic diagram of step S2 in Embodiment 1 of the present invention; Figure 4 This is a schematic diagram of the structure of S3 in step S1 of embodiment one of the present invention; Figure 5 This is a schematic diagram of the structure of S4 in step S1 of embodiment one of the present invention; Figure 6 This is a schematic diagram of the structure of S5 in step S1 of embodiment one of the present invention; Figure 7 This is a schematic diagram of the structure of step S61 in embodiment S6 of the present invention; Figure 8This is a schematic diagram of the structure of step S62 in step S6 of embodiment one of the present invention; Figure 9 This is a flowchart of the fabrication method of the Micro-LED vertical chip brightening structure described in this invention; Among them, 1. driving substrate; 2. first bonding metal layer; 3. second bonding metal layer; 4. transparent conductive film layer; 5. gallium nitride epitaxial wafer; 6. metal fence reflective layer; 7. passivation layer; 8. common n-type transparent conductive layer. Detailed Implementation

[0021] To enable those skilled in the art to better understand the present application, the technical solutions in the embodiments of the present application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present application, and not all embodiments. Based on the embodiments in the present application, all other embodiments obtained by those of ordinary skill in the art without creative effort should fall within the scope of protection of the present application.

[0022] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate for the embodiments of this application described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.

[0023] In this application, the terms "upper," "lower," "left," "right," "front," "rear," "top," "bottom," "inner," "outer," "middle," "vertical," "horizontal," "lateral," and "longitudinal" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. These terms are primarily for the purpose of better describing the invention and its embodiments, and are not intended to limit the indicated device, element, or component to having a specific orientation, or to be constructed and operated in a specific orientation.

[0024] Furthermore, in addition to indicating direction or positional relationship, some of the aforementioned terms may also have other meanings. For example, the term "above" may also be used in certain situations to indicate a dependency or connection. Those skilled in the art can understand the specific meaning of these terms in this invention based on the specific circumstances.

[0025] Furthermore, the terms "installation," "setup," "equipped with," "connection," "linking," and "socketing" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral structure; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium, or an internal connection between two devices, components, or parts. Those skilled in the art can understand the specific meaning of these terms in this invention based on the specific circumstances.

[0026] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. This application will now be described in detail with reference to the accompanying drawings and embodiments.

[0027] Example 1 See appendix Figure 1-9 This embodiment is a standard basic structure, including a silicon-based CMOS driving substrate 1, a eutectic bonding metal layer, a gallium nitride epitaxial wafer 5, and a silver-aluminum alloy metal fence reflective layer 6; the gallium nitride epitaxial wafer 5 is mechanically and electrically connected to the driving substrate 1 through the Au-Au eutectic bonding layer, and the epitaxial layer is etched to form an LED pixel array with a period of 15μm, a single pixel diameter of 10μm, and a trench width of 5μm and a depth of 1.2μm between adjacent pixels.

[0028] The metal fence reflective layer 6 is completely filled in the trench and surrounds the sidewalls of each LED pixel. It is composed of a 20nm Cr adhesive layer and a 1μm Ag-Al alloy reflective layer. The top surface of the metal fence is flush with the upper surface of the quantum well layer inside the pixel.

[0029] The light-emitting surface of the pixel and the surface of the metal fence are covered with a 400nm silicon oxide passivation layer 7. The passivation layer 7 has a contact hole in the center of each pixel. The top 400nm thick ITO common n electrode layer is electrically connected to the n-type gallium nitride of all pixels through the contact hole.

[0030] This embodiment can achieve an inter-pixel optical crosstalk suppression rate of ≥85% and a single pixel light output brightness increase of more than 20%, making it suitable for conventional consumer display scenarios.

[0031] This embodiment details the complete process of fabricating a Micro-LED vertical chip brightening structure using a double-layer positive adhesive process: S1. A first bonding metal layer 2 is prepared on the surface of the driving substrate 1, and a transparent conductive film layer 4 and a second bonding metal layer 3 are prepared on the p-type side of the gallium nitride epitaxial wafer 5. S11, Fabrication of bonding metal layer on drive substrate 1: A silicon-based CMOS substrate containing pixel circuits, driving circuits, and interface circuits is used as the driving substrate 1. An electron beam evaporation process is used to prepare a first bonding metal layer 2 on its surface. The evaporation rate is 1~2 nm / s. The metal layer has a three-layer structure: the first layer is a Cr adhesion layer with a thickness of 20 nm; the second layer is a Pt transition layer with a thickness of 200 nm; and the third layer is an Au layer with a thickness of 200 nm.

[0032] S12, Preparation of transparent conductive film and bonding metal layer on epitaxial wafer: Take gallium nitride epitaxial wafer 5 on a sapphire substrate. The epitaxial structure from the sapphire side consists of an n-type gallium nitride layer, a quantum well layer, and a p-type gallium nitride layer.

[0033] A p-type ITO transparent conductive film layer 4 with a thickness of 100 nm was prepared on the p-type surface of an epitaxial wafer using magnetron sputtering at a sputtering rate of 1.5 nm / s. The epitaxial wafer was then annealed in a rapid annealing furnace at a temperature of 550 °C for 5 min under an oxygen atmosphere of 5 sccm to improve the conductivity and transmittance of the ITO.

[0034] After annealing, the second bonded metal layer 3 was prepared by electron beam evaporation at a rate of 1 nm / s. The structure consisted of a 5 nm Cr adhesion layer, a 20 nm Pt transition layer, and a 200 nm Au layer.

[0035] S2, eutectic bonding and epitaxial thinning: After aligning the driving substrate 1 and the gallium nitride epitaxial wafer 5, they are placed in a metal bonding machine for eutectic bonding. The bonding temperature is 300℃, the pressure is 50KN, and the bonding time is 20min.

[0036] After bonding, the sapphire substrate was removed by laser lift-off with a laser wavelength of 266 nm, a frequency of 1000 Hz, and a stage temperature of 30 °C, using a circular scanning method from the outside in. After lift-off, the gallium nitride epitaxial wafer 5 was thinned to 1.2 μm by chemical polishing.

[0037] S3, Epitaxial etching forms a pixel array: A 500 nm thick silicon oxide hard mask was deposited on the surface of an epitaxial wafer using PECVD process at a deposition temperature of 300 °C, with SiH4 and N2O as the reaction gases.

[0038] A 1.5μm positive photoresist is spin-coated, and the image is exposed and developed using a stepper lithography machine to transfer the frustum array pattern. Silicon oxide is first etched using ICP etching with CF4 etching gas at a flow rate of 80 sccm, with the upper electrode power at 300W and the lower electrode power at 80W. Then, gallium nitride epitaxial wafer 5 is further etched using Cl2+BCl3 etching gases at a total flow rate of 60 sccm, forming periodic LED pixel units with trenches between adjacent pixels.

[0039] S4, Independent Anode Etching: A 2μm positive photoresist is spin-coated, and after exposure and development, a frustum mask covering each pixel is formed. The transparent conductive film layer 4 and the bonding metal layer in the exposed area are etched using the IBE process to achieve independent anodes for each pixel; the etching angle is 8° and the etching voltage is 400V.

[0040] S5, Preparation of metal fences using the double-layer positive adhesive method: (1) Spin coating of primer: spin coating of LOR-812 photoresist at 1500r / min for 25s; soft baking at 190℃ for 180s to form a 300nm thick primer layer.

[0041] (2) Spin coating of positive photoresist: Spin coating of AZ5214 positive photoresist onto the base coat at a speed of 4000 r / min; soft baking at 100℃ for 100 s to form a 900 nm thick positive photoresist layer.

[0042] (3) Exposure and development: Expose through a grooved pattern mask and develop with 2.38% TMAH developer for 70 seconds. The positive resist in the exposed area is dissolved, and the underresist is simultaneously etched by the developer, forming resist holes with an undercut morphology.

[0043] (4) Metal vapor deposition: Electron beam vapor deposition first deposits a 10 nm Cr adhesion layer, then deposits a 1 μm silver aluminum alloy reflective layer, and the vapor deposition height covers the quantum well region.

[0044] (5) Metal stripping: Immersion in NMP solution to strip the photoresist and surface metal, leaving only the metal fence reflective layer 6 in the trench.

[0045] S6. Deposit a passivation layer 7 on the chip surface and etch to form contact holes; prepare a common n-type transparent conductive layer 8 on the surface of the passivation layer 7 to complete the chip fabrication; S61, Deposited passivation layer 7: PECVD was used to deposit 400nm silicon oxide as a passivation layer 7, covering the top surface of the pixel and the surface of the metal fence. Photolithography was used to etch the contact hole in the center of the pixel, exposing the n-type gallium nitride surface.

[0046] S62, Preparation of n-type transparent conductive layer 8: The RPD process deposits 400nm ITO as a common n-type transparent conductive layer 8, and photolithography etches it to form a common cathode pattern, so that all pixel n-electrodes are interconnected, thus completing the chip fabrication.

[0047] Example 2 The only difference between this embodiment and Embodiment 1 is that the metal fence is prepared using a negative adhesive process; the other steps are exactly the same. (1) Spin-coat negative photoresist at 2000 r / min for 25 s; then bake at 100 ℃ for 80 s to form a 1200 nm thick negative photoresist layer.

[0048] (2) Expose through a grooved mask, develop with 2.38% TMAH developer for 70s, dissolve the negative adhesive in the unexposed area, and form an adhesive hole pattern with undercut.

[0049] The subsequent metal vapor deposition and stripping processes are the same as in Example 1, ultimately forming the metal fence reflective layer 6.

[0050] Example 3 This embodiment addresses the reliability issues of silver-aluminum alloys being prone to oxidation and electromigration in high-temperature and high-humidity environments. It optimizes the layered structure of the metal fence by adopting a sandwich stacked structure of "adhesive layer-high reflectivity layer-blocking layer", which significantly improves the environmental stability of the device while maintaining high reflectivity.

[0051] The specific preparation steps are as follows: (1) The preceding process is the same as in Example 1. The bonding metal preparation of the driving substrate 1, the preparation of the transparent conductive film and bonding metal of the epitaxial wafer, eutectic bonding, laser lift-off, epitaxial thinning, pixel etching and anode independent etching are completed in sequence to obtain an LED pixel array structure with a period of 15μm, a pixel diameter of 10μm, a trench width of 5μm and a depth of 1.2μm.

[0052] (2) Preparation of double-layer positive adhesive pattern: Same as step (1)-(3) of step S5 in Example 1, forming an array of adhesive holes with undercut morphology, with the undercut amount controlled at 200~250nm to ensure that the subsequent peeling boundary is neat.

[0053] (3) Sandwich metal layer evaporation: Three functional metal layers are deposited sequentially using electron beam evaporation. The substrate is kept at a constant temperature of 30°C during the evaporation process to avoid excessive temperature causing softening and deformation of the photoresist. The first layer is a Ti adhesion layer with a thickness of 15nm and a deposition rate of 0.8nm / s, which strengthens the interfacial bonding between the metal and the gallium nitride sidewalls and the silicon oxide at the bottom of the trench. The second layer is an Ag high-reflectivity layer with a thickness of 950nm and a deposition rate of 1.2nm / s. As the core reflective structure, it has a reflectivity of ≥95% for the 450nm blue light band. The third layer is a Ti barrier layer with a thickness of 35nm and a deposition rate of 0.8nm / s. It completely covers the sidewalls and top surface of the silver layer, blocking the intrusion of oxygen and water vapor and inhibiting the oxidation and electromigration of silver atoms.

[0054] (4) Metal stripping: NMP solution was used in conjunction with low-frequency ultrasound to assist stripping. The ultrasound power was 80W, the solution temperature was 40℃, and the stripping time was 120s. Then, the metal fence with titanium-silver-titanium sandwich structure was obtained by rinsing with isopropanol, rinsing with deionized water, and high-speed spin drying.

[0055] (5) The subsequent passivation layer 7 deposition, contact hole etching and common n-type ITO preparation process are the same as step S6 in Example 1.

[0056] The technical effects of this embodiment are as follows: With the protection of the surface titanium barrier layer, the high temperature oxidation resistance of the metal fence is improved by more than 3 times. After 1000 hours of high temperature and high humidity reliability testing at 85℃ / 85%RH, the reflectivity decay is less than 2%, which can meet the usage requirements of high reliability scenarios such as vehicle display and outdoor high brightness screen.

[0057] Example 4 This embodiment targets the 5μm-level small pixel scenario of high-resolution Micro-LED displays, corresponding to a trench depth-to-width ratio of 1.8:1 or higher. It optimizes the photoresist coating, development, and evaporation parameters to solve the process problems of uneven photoresist layer filling and poor metal sidewall coverage in deep trenches.

[0058] The specific preparation steps are as follows: (1) Pre-epi-epitaxy etching: Same as steps S1-S3 in Example 1, to prepare an LED pixel array with a 5μm period, a pixel diameter of 3μm, a trench width of 2μm, an ICP etching depth of 1.1μm, and a trench depth-to-width ratio of approximately 1.8:1.

[0059] (2) Negative photoresist pattern preparation: A negative photoresist process is used to adapt to the deep trench morphology, and the stress of the photoresist layer is controlled by segmented spin coating and programmed baking. ① Three-stage spin coating of negative photoresist: spin coating at low speed of 500r / min for 10s to lay the photoresist, spin coating at high speed of 3500r / min for 30s to form the film, and spin coating at low speed of 800r / min for 5s to remove the edge, ensuring uniform filling of the photoresist layer in the trench. ②Programmed temperature-controlled soft baking: Pre-bake at 70℃ for 60s, main bake at 100℃ for 90s, and slowly cool down to room temperature to avoid stress concentration in the adhesive layer that could cause cracking in the grooves; the final total thickness of the adhesive layer is 1.4μm, and the adhesive thickness at the bottom of the groove is ≥300nm; ③ Stepper lithography machine overlay exposure, exposure dose 120mJ / cm², multiple exposure mode is used to ensure full exposure of the bottom of the trench; ④ Spray development with 2.38% TMAH developer for 90 seconds, rinse with deionized water, and gently spin dry with nitrogen; the final undercut depth of the adhesive wells is controlled at 150~200nm, and the undercut uniformity deviation of the whole piece is ≤10%.

[0060] (3) Directional metal evaporation: Electron beam evaporation with ion assistance is used. The substrate is tilted at 15° and kept in planetary rotation. The evaporation rate is 0.6 nm / s. First, a 10 nm Cr adhesion layer is deposited, and then a 900 nm Al reflection layer is deposited. The tilted rotation evaporation ensures that the metal coverage of the trench sidewalls is uniform and the thickness deviation of the upper and lower sidewalls is ≤15%.

[0061] (4) Low temperature and low pressure peeling: Immerse in 35℃ NMP solution and use low pressure spray to assist peeling. Peeling time is 150s. Avoid adhesive layer expansion caused by high temperature. After peeling, the metal fence edge is neat, without burrs or residual adhesive.

[0062] (5) The subsequent passivation layer 7 and the common n-type transparent conductive layer 8 are prepared in the same way as in Example 1.

[0063] The technical effects of this embodiment are: it can stably realize the fabrication of metal fences with small-sized, high aspect ratio pixels at the 5μm level, with a metal coverage rate of ≥95% on the trench sidewalls, an inter-pixel light crosstalk suppression rate of over 90%, and a single pixel light output brightness increase of over 25%, making it compatible with high-definition Micro-LED display panels with resolutions of 4K and above.

[0064] Example 5 This embodiment describes the entire process parameters of a 12-inch wafer-level metal fence for industrial mass production, and verifies the adaptability and economy of this solution for large-scale mass production.

[0065] The specific preparation steps are as follows: (1) Pre-wafer level process: complete the eutectic bonding, laser lift-off, epitaxial thinning and pixel ICP etching of 12-inch silicon-based driver wafer and gallium nitride epitaxial wafer, and the depth uniformity deviation of the whole wafer pixel array is ≤3%.

[0066] (2) Wafer-level double-layer positive adhesive coating: The entire surface is uniformly coated using a track-type adhesive coater. ① Base coat coating: spin coater speed 1800r / min, spin coating time 30s, hot plate soft baking at 195℃ for 190s, base coat thickness of 350nm across the entire wafer, thickness uniformity within the wafer ≤5%; ② Positive adhesive coating: main rotation speed 4200r / min, spin coating time 30s, hot plate soft baking at 105℃ for 110s, positive adhesive thickness 950nm, thickness deviation within the wafer ≤3%.

[0067] (3) Wafer-level step-scan exposure: An ArF step-scan lithography machine was used, with an exposure dose of 180 mJ / cm². 2 Overlay accuracy ±50nm, total exposure time for the entire 12-inch wafer ≤90s.

[0068] (4) Full-wave spray development: A fully automatic spray developer is used. 2.38% TMAH developer solution is sprayed at constant pressure for 75s, followed by gradient rinsing with deionized water and drying with nitrogen air knife. The bottom cut of the whole wafer is stably controlled at 200~250nm, and the pattern yield is ≥99%.

[0069] (5) Magnetron sputtering of metal on the whole surface: a long stroke planar magnetron sputtering stage is used. The 12-inch wafer is rotated and revolved. First, a 15nm Ti adhesion layer is sputtered, and then a 1050nm silver aluminum alloy reflective layer is sputtered. The sputtering power is 8kW, and the uniformity of the film thickness on the whole wafer is ≤4%.

[0070] (6) Wafer-level batch stripping: A multi-tank stripping machine is used, with NMP solution circulating and filtered, solution temperature 45℃, and low-frequency ultrasonic-assisted stripping for 180s; then the wafers are discharged through an isopropanol cleaning tank, a deionized water rinsing tank, and a hot air drying tank; the whole metal stripping yield is ≥98.5%, with no residual adhesive and no metal burrs.

[0071] (7) Subsequent passivation layer 7 deposition, contact hole etching, and common n-type ITO fabrication were all completed using 12-inch wafer-level semiconductor processes.

[0072] The technical effects of this embodiment are: to achieve 12-inch wafer-level batch production, to shorten the processing cycle of the single wafer metal fence process by 30%, to achieve a final device yield of ≥95%, to achieve chip brightness uniformity of ≥92%, and to achieve full compatibility with existing semiconductor mass production lines, thus meeting the cost and yield requirements of large-scale mass production.

[0073] Finally, it should be noted that the above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A brightness enhancement structure for a Micro-LED vertical chip, characterized in that, It includes a driving substrate, a bonding metal layer, a gallium nitride epitaxial wafer, and a metal fence reflective layer; The gallium nitride epitaxial wafer is eutectic bonded to the driving substrate through the bonding metal layer; the gallium nitride epitaxial wafer is etched to form periodically arrayed LED pixel units, and trenches are formed between adjacent LED pixel units; The metal fence reflective layer fills the trench and surrounds the sidewalls of each LED pixel unit to reflect the lateral light emitted by the LED pixel unit, thereby isolating light crosstalk between pixels and improving the brightness of the chip.

2. The brightness enhancement structure of the Micro-LED vertical chip according to claim 1, characterized in that, The metal fence reflective layer includes an adhesive layer and a highly reflective metal layer; the adhesive layer is a chromium layer or a titanium layer with a thickness of 5~50nm; the highly reflective metal layer is a silver-aluminum alloy layer with a thickness of 800~1200nm.

3. The brightness enhancement structure of the Micro-LED vertical chip according to claim 1, characterized in that, The height of the metal fence reflective layer is not lower than the height of the upper surface of the quantum well layer inside the LED pixel unit.

4. The brightness enhancement structure of the Micro-LED vertical chip according to claim 1, characterized in that, The LED pixel unit includes a p-type gallium nitride layer, a quantum well layer, and an n-type gallium nitride layer in sequence from the side closest to the driving substrate to the light-emitting side; the bonding metal layer includes a first bonding metal layer and a second bonding metal layer, the first bonding metal layer is disposed on the surface of the driving substrate, and the second bonding metal layer is disposed on the p-type side of the gallium nitride epitaxial wafer, and the two are eutectic bonded.

5. The brightness enhancement structure of the Micro-LED vertical chip according to claim 1, characterized in that, It also includes a passivation layer and a common n-type transparent conductive layer; The passivation layer covers the light-emitting surface of the LED pixel unit and the surface of the metal fence reflective layer; the passivation layer has contact holes corresponding to the light-emitting area of ​​each LED pixel unit; The common n-type transparent conductive layer is disposed on the surface of the passivation layer and is electrically connected to the n-type gallium nitride layer of each LED pixel unit through the contact hole, thereby realizing the common cathode connection of all LED pixel units.

6. A method for fabricating a Micro-LED vertical chip brightening structure as described in any one of claims 1-5, characterized in that, Includes the following steps: S1. A first bonding metal layer is prepared on the surface of the driving substrate, and a transparent conductive film layer and a second bonding metal layer are prepared on the p-type side of the gallium nitride epitaxial wafer. S2. The driving substrate and the gallium nitride epitaxial wafer are bonded together by eutectic bonding to form a bond body. The growth substrate of the gallium nitride epitaxial wafer is peeled off, and the gallium nitride epitaxial wafer is thinned. S3. Photolithography and etching are performed on the thinned gallium nitride epitaxial wafer to form periodically arrayed LED pixel units, with trenches formed between adjacent pixel units; S4. Etch away the bonding metal layer between pixel units to achieve independent anodes for each LED pixel unit; S5. A photoresist pattern is prepared on the chip surface, and a photoresist hole with an undercut morphology is formed at the trench position corresponding to the photoresist pattern; A highly reflective metal layer is deposited on the chip surface by vapor deposition; The photoresist and surface metal are removed by a stripping process, leaving the metal in the trenches to form a metal fence reflective layer. S6. Deposit a passivation layer on the chip surface and etch to form contact holes; A common n-type transparent conductive layer is prepared on the surface of the passivation layer to complete the chip fabrication.

7. The preparation method according to claim 6, characterized in that, Step S5 involves preparing the photoresist pattern using a double-layer positive resist process, specifically including: S511. Spin-coat a photoresist base coat onto the chip surface after the anode independent etching is completed, and form a base coat layer with a thickness of 200~500nm after soft baking. S512. Spin-coat positive photoresist onto the surface of the base layer, and after soft baking, form a positive photoresist layer with a thickness of 800~1000nm. S513. Exposure is performed through a mask, followed by development with a developer. The positive resist layer in the exposed area reacts with the developer and is removed, while the underlying resist layer in the corresponding position is also dissolved by the developer. The positive resist layer and the underlying resist layer in the unexposed area are retained, forming a resist hole pattern with an undercut morphology.

8. The preparation method according to claim 6, characterized in that, Step S5 involves preparing the photoresist pattern using a negative resist process, specifically including: S521. Spin-coat negative photoresist onto the chip surface after independent anodic etching, and form a negative photoresist layer with a thickness of 1000~1500nm after soft baking. S522. Exposure is performed through a mask, followed by development with a developer; the negative adhesive layer in the unexposed area is dissolved and removed by the developer, while the negative adhesive layer in the exposed area is retained, forming an adhesive hole pattern with an undercut morphology.

9. The preparation method according to claim 6, characterized in that, In step S2, the eutectic bonding temperature is 260~350℃, the pressure is 25~80KN, and the bonding time is 10~30min; the growth substrate is removed by laser lift-off with a laser wavelength of 200~300nm and a frequency of 800~1200Hz. The stage temperature during lift-off is 20~50℃, and a ring lift-off method from the outside to the inside is adopted; after lift-off, the gallium nitride epitaxial wafer is thinned to 1~1.5μm by chemical polishing.

10. The preparation method according to claim 6, characterized in that, In step S3, the gallium nitride epitaxial wafer is etched using inductively coupled plasma etching (ICP-C) with chlorine and boron trichloride as the etching gases and a gas flow rate of 20-100 sccm. In step S4, the bonding metal layer is etched using an ion beam etching process with an etching angle of 0°~15° and an etching voltage of 300~500V. In step S6, the passivation layer is a silicon oxide layer with a thickness of 300~500nm, prepared by chemical vapor deposition; the common n-type transparent conductive layer is an indium tin oxide layer with a thickness of 300~500nm, prepared by reactive plasma deposition or magnetron sputtering.