A perovskite solar cell, its fabrication method, and a photovoltaic module
By employing a gradient design of a NiOX dense layer and a NiOX buffer layer, the problems of small interfacial contact area and lattice mismatch caused by the compactness of the NiOx hole transport layer were solved, thereby improving the efficiency and stability of perovskite solar cells.
Patent Information
- Application Number
- CN202510624297.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-15
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, the compactness of the NiOx hole transport layer results in a small interfacial contact area and severe lattice mismatch, which limits the improvement of efficiency and stability of perovskite solar cells.
A hole transport gradient structure is constructed by synergistically building a NiOX dense layer and a NiOX buffer layer. By controlling the pore size, porosity and Li+ doping concentration, a gradient design is formed to enhance hole transport and interface charge extraction, thereby alleviating lattice mismatch.
This improves the photoelectric conversion efficiency and long-term stability of perovskite solar cells, reduces interface defects, enhances the contact area between the hole transport layer and the perovskite light-absorbing layer, and suppresses interface reactions.
Smart Images

Figure CN123124565A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photovoltaic technology, specifically relating to a perovskite solar cell, its preparation method, and a photovoltaic module. Background Technology
[0002] Perovskite solar cells have attracted widespread attention due to their high light absorption, larger defect capacity, and bipolar carrier transport. Perovskite solar cells are generally classified into formal nip structures and inverted pin structures. Inverted pin perovskite solar cells have become a focus of attention because they are more compatible with crystalline silicon solar cells in tandem cell fabrication processes. In inverted pin perovskite solar cells, NiOx hole transport layers are widely used due to their low production cost, high hole mobility, and high stability. In existing technologies, PVD magnetron sputtering is suitable for large-scale, large-area NiOx fabrication, enabling industrial manufacturing and use. However, magnetron sputtered NiOx is too dense, resulting in poor surface wettability and a small interfacial contact area. Furthermore, the large lattice difference between NiOx and perovskite means that the dense film cannot mitigate the mismatch through deformation, exacerbating interfacial defects. In addition, the low intrinsic hole mobility of NiOx limits the efficiency improvement of perovskite solar cells.
[0003] To address this, researchers have made technological improvements. For example, patent CN117979714A relates to a perovskite solar cell with a NiOx buffer layer and its fabrication method. The fabrication method includes the following steps: depositing a NiOx buffer layer on a pretreated TCO substrate using atomic layer deposition; depositing a nickel oxide hole transport layer on the NiOx buffer layer using spin coating; and sequentially fabricating a perovskite light-absorbing layer, an electron transport layer, a charge-blocking layer, and an electrode layer on the nickel oxide hole transport layer to obtain a perovskite solar cell with a NiOx buffer layer. Patent CN118102741A discloses an inverted perovskite solar cell based on an iron-doped nickel oxide hole transport layer, its preparation method, and its application. The inverted perovskite solar cell sequentially comprises a transparent conductive layer, an iron-doped nickel oxide hole transport layer, an electron transport layer, a perovskite layer, an electron transport layer, and a silver electrode layer. The transparent conductive layer is placed in a magnetron sputtering chamber, and iron-doped nickel oxide sputtering target is used to sputter the surface of the transparent conductive layer. The iron-doped nickel oxide hole transport layer is obtained by heat treatment. The inverted perovskite solar cell is obtained by spin-coating, annealing, and vapor deposition of perovskite solution on the iron-doped nickel oxide hole transport layer. Patent CN108063186A relates to a zinc-doped nickel oxide hole transport layer reverse perovskite solar cell and its fabrication method. The reverse perovskite solar cell comprises: (1) FTO glass; (2) fabrication of a zinc-doped nickel oxide hole transport layer; (3) fabrication of a perovskite heterojunction thin film; (4) fabrication of an electron transport layer on the perovskite layer; (5) an electrode modification layer; and (6) a metal electrode. However, although the above patent has made some progress in improving the NiOx layer, further exploration is still needed to solve problems such as interface reactions, improve cell efficiency, and long-term stability.
[0004] Therefore, how to effectively suppress interface reactions and defects, improve hole transport rate, and thus further improve battery efficiency and long-term stability is a technical problem that urgently needs to be solved. Summary of the Invention
[0005] To address the shortcomings of existing technologies, the present invention aims to provide a perovskite solar cell, its fabrication method, and a photovoltaic module. This invention utilizes the design of NiO... X dense layer and NiO X The buffer layer collaboratively constructs the hole transport gradient structure, using NiO on one hand. X The dense layer maintains the high conductivity of the hole transport layer and avoids excessive Li. + Introducing scattering centers ensures ohmic contact with the conductive substrate and reduces the risk of ion migration, thus improving the long-term stability of the battery. On the other hand, the use of NiO... XThe buffer layer provides more holes, enhancing the efficiency of interface charge extraction and improving the battery efficiency. Furthermore, this hole transport gradient structure increases the contact area between the hole transport layer and the perovskite light-absorbing layer, and alleviates lattice mismatch through deformation, helping to suppress interface reactions and reduce interface defects, thereby further improving battery efficiency and long-term stability.
[0006] To achieve this objective, the present invention adopts the following technical solution:
[0007] In a first aspect, the present invention provides a perovskite solar cell, the perovskite solar cell comprising a conductive substrate and NiO stacked thereon. X dense layer, NiO X Buffer layer, perovskite light-absorbing layer, electron transport layer and electrodes;
[0008] The NiO X The average pore size of the dense layer is smaller than that of the NiO X The average pore size of the buffer layer; the NiO X dense layer and NiO X The buffer layers are all doped with Li + And NiO X Li in the dense layer + The doping concentration is less than that of NiO X Li in the buffer layer + Doping concentration.
[0009] This invention designs NiO X dense layer and NiO X The buffer layer collaboratively constructs the hole transport gradient structure, using NiO on one hand. X The dense layer maintains the high conductivity of the hole transport layer and avoids excessive Li. + Introducing scattering centers ensures ohmic contact with the conductive substrate and reduces the risk of ion migration, thus improving the long-term stability of the battery. On the other hand, the use of NiO... X The buffer layer provides more holes, enhancing the efficiency of interface charge extraction and improving the battery efficiency. Furthermore, this hole transport gradient structure increases the contact area between the hole transport layer and the perovskite light-absorbing layer, and alleviates lattice mismatch through deformation, helping to suppress interface reactions and reduce interface defects, thereby further improving battery efficiency and long-term stability.
[0010] In this invention, NiO X The average pore size of the dense layer is smaller than that of NiO. X The average pore size of the buffer layer, combined with NiO X Li in the dense layer + Doping concentration less than NiO X Li in the buffer layer +Doping concentration, along with two other parameters, works synergistically to construct an efficient "implantation-transport-collection" pathway, which helps reduce the resistance to hole transport within the layer and improve charge separation efficiency. Furthermore, through pore size and Li... + Adjusting the doping concentration gradient allows for precise control of the energy levels in each layer (such as the valence band top and Fermi level), achieving energy level gradient matching between the doping layer and the conductive substrate and the perovskite light-absorbing layer. Furthermore, the synergistic effect of these two processes helps suppress interface defects, providing an important approach to improving the photoelectric conversion efficiency and long-term stability of perovskite solar cells.
[0011] In this invention, NiO X Li in the dense layer + Doping concentration less than NiO X Li in the buffer layer + The doping concentration gradient design enables holes to migrate directionally under the drive of the concentration gradient, reducing reverse electron transport and interface recombination. At the same time, it ensures efficient hole transport between layers, balancing the series and parallel resistance of the device. The band bending formed by this concentration gradient design can guide holes to pass through the interface quickly, while suppressing reverse electron injection caused by energy level mismatch, improving the interface charge separation efficiency. This concentration gradient design can enable the bilayer structure to maintain structural integrity during high-temperature annealing or long-term operation, delaying device aging and enhancing the stability of the battery device.
[0012] In this invention, NiO X The average pore size of the dense layer is smaller than that of the NiO X The average pore size of the buffer layer, through the design of pore size differences, achieves functional complementarity and synergy, effectively improving device performance. Among them, NiO... X The small average pore size in the dense layer gives it good compactness, effectively blocking the recombination of electrons and holes. Furthermore, as a transition layer between other functional layers and the conductive substrate, it can form good interfacial contact with conductive glass, improving the stability of the device structure. NiO X The larger average aperture in the buffer layer gives it a higher hole mobility, enabling it to transport holes more effectively. It can work synergistically with the perovskite light-absorbing layer to broaden the light absorption range and further improve the photoelectric conversion efficiency of the device.
[0013] It should be noted that NiO X In this context, x represents the stoichiometric ratio of oxygen atoms to nickel atoms. Since nickel oxide exists in multiple oxidation states, such as NiO (corresponding to x = 1), Ni2O3 (corresponding to x = 1.5), and Ni3O4 (corresponding to x = 1.33), NiOx is used to represent cases where the composition is uncertain or non-stoichiometric.
[0014] Preferably, the NiO XThe average pore size of the dense layer is ≤2nm, for example, it can be 2nm, 1.5nm or 1nm, etc.
[0015] Preferably, the NiO X The average pore size of the buffer layer is ≤20nm, for example, it can be 20nm, 15nm, 10nm or 5nm, etc.
[0016] Preferably, the NiO X The porosity of the dense layer is less than that of the NiO X Porosity of the buffer layer.
[0017] In this invention, NiO X The dense layer, located close to the conductive substrate, forms a dense barrier layer with low porosity, effectively preventing electrons from directly transporting from the conductive substrate to the perovskite light-absorbing layer. This reduces electron recombination at the interface, improves the open-circuit voltage and fill factor of the device, and thus enhances the photoelectric conversion efficiency of the battery. NiO... X The buffer layer is close to the perovskite light-absorbing layer. Its high porosity can increase the contact area with the perovskite light-absorbing layer and alleviate lattice mismatch through deformation, thereby reducing interface defects.
[0018] Preferably, the NiO X The porosity of the dense layer is ≤5%, for example, it can be 5%, 4%, 3%, 2% or 1%, etc.
[0019] Preferably, the NiO X The porosity of the buffer layer is ≤30%, for example, it can be 30%, 25%, 20%, 15% or 10%, etc.
[0020] Preferably, the NiO X The thickness of the buffer layer is 2-10nm, for example, it can be 2nm, 4nm, 6nm, 8nm or 10nm, etc.
[0021] Preferably, the NiO X dense layer and the NiO X The thickness ratio of the buffer layer is (1-7.5):1, for example, it can be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1 or 7.5:1, etc.
[0022] In this invention, NiO is synergistically controlled X dense layer and the NiO X The thickness ratio of the buffer layer can be combined with Li doping to improve hole transport and optimize energy level matching. It can also be combined with gradient-designed porosity changes to improve interface contact and reduce interface defects.
[0023] Preferably, the NiO X Li in the dense layer +The doping concentration is 0.046-0.28 wt%, for example, it can be 0.046 wt%, 0.05 wt%, 0.1 wt%, 0.15 wt%, 0.2 wt%, 0.25 wt%, or 0.046 wt%, etc.
[0024] Preferably, the NiO X Li in the buffer layer + The doping concentration is 0.46-1.15 wt%, for example, it can be 0.46 wt%, 0.5 wt%, 0.75 wt%, 1 wt%, or 1.15 wt%, etc.
[0025] Preferably, the conductive substrate is conductive glass. For example, it could be FTO (fluorine-doped tin oxide) conductive glass.
[0026] Preferably, the chemical formula of the perovskite light-absorbing layer is ABX3, wherein A includes any one or a combination of at least two of formamidinium ions, methylamine ions, or cesium ions, B includes lead ions and / or tin ions, and X is a halide ion.
[0027] Preferably, the thickness of the perovskite light-absorbing layer is 300-1000nm, for example, it can be 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm or 1000nm.
[0028] Preferably, the electron transport layer comprises a PCBM ([6,6]-phenyl-C61-isomethyl butyrate) layer, a SnO2 layer, a TiO2 layer, a ZnO layer, and a C 60 Any one or a combination of at least two of the following: layer or BCP (Bath Copper Essence) layer.
[0029] Preferably, the thickness of the electron transport layer is 20-50 nm, for example, it can be 20 nm, 30 nm, 40 nm or 50 nm.
[0030] Preferably, the electrode is a metal electrode. For example, it may be a Cu electrode, an Ag electrode, or an Au electrode.
[0031] Secondly, the present invention provides a method for preparing a perovskite solar cell, the method comprising the following steps:
[0032] NiO was sequentially prepared on a conductive substrate. X dense layer, NiO X The perovskite solar cell is obtained by comprising a buffer layer, a perovskite light-absorbing layer, an electron transport layer, and electrodes.
[0033] It should be noted that the perovskite solar cell prepared above is the perovskite solar cell described in the first aspect or the perovskite solar cell in the prior art.
[0034] Preferably, the NiO X dense layer and NiO X The methods for preparing the buffer layer can be independently categorized into magnetron sputtering.
[0035] Preferably, the NiO X When the dense layer is prepared by magnetron sputtering, the operating parameters include:
[0036] Target materials include NiO X Target and Li2O target, NiO X The sputtering power of the target is 5-8 kW (e.g., 5 kW, 6 kW, 7 kW or 8 kW, etc.), the sputtering power of the Li2O target is 0.05-0.15 kW (e.g., 0.05 kW, 0.1 kW or 0.15 kW, etc.), and the volume ratio of sputtering gas (e.g., argon, etc.) to reactant gas (e.g., oxygen, etc.) is (8-12):1 (e.g., 8:1, 9:1, 10:1, 11:1 or 12:1, etc.).
[0037] Preferably, the NiO X When the buffer layer is prepared by magnetron sputtering, the operating parameters include:
[0038] Target materials include NiO X Target and Li2O target, NiO X The sputtering power of the target is 1-4kW (e.g., 1kW, 2kW, 3kW or 4kW, etc.), the sputtering power of the Li2O target is 0.2-0.4kW (e.g., 0.2kW, 0.3kW or 0.4kW, etc.), and the volume ratio of sputtering gas (exemplarily, argon, etc.) to reactant gas (exemplarily, oxygen, etc.) is (2-5):1 (e.g., 2:1, 3:1, 4:1 or 5:1, etc.).
[0039] Preferably, the preparation steps of the perovskite light-absorbing layer include:
[0040] Coating a perovskite precursor solution onto NiO X After annealing, a perovskite light-absorbing layer is formed on the buffer layer. For example, the coating method can be a coating method or a spin coating method.
[0041] Preferably, the concentration of the perovskite precursor solution is 0.8-1.5 mol / L, for example, it can be 0.8 mol / L, 1 mol / L, 1.2 mol / L or 1.5 mol / L, etc.
[0042] Preferably, the electron transport layer is prepared by thermal evaporation or solution method.
[0043] Preferably, the electrode is prepared by magnetron sputtering or thermal evaporation.
[0044] Preferably, the preparation method includes the following steps:
[0045] (1) A NiO layer with a thickness of 10-15 nm was deposited on the conductive glass by magnetron sputtering. X Dense layer; wherein, the operating parameters of magnetron sputtering include:
[0046] Target materials include NiO X Target and Li2O target, NiO X The sputtering power of the target is 5-8 kW, the sputtering power of the Li2O target is 0.05-0.15 kW, and the volume ratio of sputtering gas to reactant gas is (8-12):1.
[0047] In NiO X A NiO layer with a thickness of 2-10 nm was deposited by magnetron sputtering on a dense layer. X Buffer layer; wherein, the operating parameters of magnetron sputtering include:
[0048] Target materials include NiO X Target and Li2O target, NiO X The sputtering power of the target is 1-4kW, the sputtering power of the Li2O target is 0.2-0.4kW, and the volume ratio of sputtering gas to reactant gas is (2-5):1.
[0049] (2) Coating the perovskite precursor solution onto NiO X After annealing, a perovskite light-absorbing layer with a thickness of 300-1000 nm is obtained on the buffer layer.
[0050] (3) An electron transport layer is deposited on the perovskite light-absorbing layer; wherein the deposition rate of the electron transport layer is (for example, it could be) or wait).
[0051] (4) Deposit a metal electrode with a thickness of 50-250 nm (e.g., 50 nm, 100 nm, 150 nm, 200 nm or 250 nm, etc.) on the electron transport layer.
[0052] Thirdly, the present invention provides a photovoltaic module, the photovoltaic module comprising the perovskite solar cell as described in the first aspect.
[0053] The numerical range described in this invention includes not only the point values listed above, but also any point values within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values included in the range.
[0054] Compared with the prior art, the present invention has the following beneficial effects:
[0055] This invention designs NiO X dense layer and NiO X The buffer layer collaboratively constructs the hole transport gradient structure, using NiO on one hand. X The dense layer maintains the high conductivity of the hole transport layer and avoids excessive Li. + Introducing scattering centers ensures ohmic contact with the conductive substrate and reduces the risk of ion migration, thus improving the long-term stability of the battery. On the other hand, the use of NiO... X The buffer layer provides more holes, enhancing the efficiency of interface charge extraction and improving the battery efficiency. Furthermore, this hole transport gradient structure increases the contact area between the hole transport layer and the perovskite light-absorbing layer, and alleviates lattice mismatch through deformation, helping to suppress interface reactions and reduce interface defects, thereby further improving battery efficiency and long-term stability. Attached Figure Description
[0056] Figure 1 This is a schematic diagram of the structure of the perovskite solar cell provided in Example 1 of the present invention.
[0057] Figure 2 NiO in the perovskite solar cell provided in Example 1 of this invention X dense layer and NiO X A schematic diagram of the buffer layer.
[0058] Among them, 1-FTO conductive glass; 2-NiO X Dense layer; 3-NiO X Buffer layer; 4-Perovskite light-absorbing layer; 5-Electron transport layer; 6-Metal electrode. Detailed Implementation
[0059] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0060] Example 1
[0061] This embodiment provides a perovskite solar cell, the structural schematic of which is shown below. Figure 1 As shown, the perovskite solar cell includes FTO conductive glass 1 and NiO stacked together. X Dense layer 2, NiO X Buffer layer 3, perovskite light-absorbing layer 4, electron transport layer 5, and metal electrode 6.
[0062] NiO X dense layer 2 and NiOX The structural diagram of buffer layer 3 is shown below. Figure 2 As shown, the NiO X The average pore size of the dense layer 2 is smaller than that of the NiO X Average pore size of buffer layer 3, NiO X The average pore size of the dense layer 2 is 2 nm, NiO X The average pore size of buffer layer 3 is 15 nm; the NiO X dense layer 2 and NiO X All of the buffer layers 3 are doped with Li + And NiO X Li in dense layer 2 + The doping concentration is less than that of NiO X Li in buffer layer 3 + Doping concentration, NiO X Li in dense layer 2 + The doping concentration is 0.046 wt%, NiO X Li in buffer layer 3 + The doping concentration is 0.46 wt%; the NiO X The porosity of the dense layer 2 is less than that of the NiO X Porosity of buffer layer 3, NiO X The porosity of the dense layer 2 is 3%, NiO X The porosity of buffer layer 3 is 25%; the NiO X The thickness of buffer layer 3 is 5nm, NiO X The thickness of the dense layer 2 is 15 nm, NiO X dense layer 2 and NiO X The thickness ratio of buffer layer 3 is 3:1.
[0063] The chemical formula of the perovskite light-absorbing layer 4 is Cs. 0.05 FA 0.85 MA 0.1 The PbI3 perovskite light-absorbing layer 4 has a thickness of 700 nm; the electron transport layer 5 includes C atoms stacked sequentially along the direction away from the perovskite light-absorbing layer 4. 60 Layer and BCP layer, C 60 The thickness of the layer is 40 nm, and the thickness of the BCP layer is 10 nm; the metal electrode 6 is a Cu electrode with a thickness of 200 nm.
[0064] This embodiment also provides a method for preparing the above-mentioned perovskite solar cell, the method comprising the following steps:
[0065] (1) Using 300mm×300mm FTO conductive glass as a substrate, the substrate is carried into the PVD magnetron sputtering cavity along with the carrier plate holder, and the vacuum level is evacuated to 1×10⁻⁶. -4Pa, using Ar and O2 with a purity of 99.999% as sputtering and reactant gases respectively, with a volume ratio of Ar to O2 of 10:1, co-sputtering was performed using NiOx and Li2O targets. X The sputtering power of the target was 6 kW, and the sputtering power of the Li2O target was 0.1 kW, resulting in a NiO layer with a thickness of 15 nm. X Dense layer.
[0066] Adjust the volume ratio of Ar and O2 to 3:1, NiO X The sputtering power of the target is 3kW, and the sputtering power of the Li2O target is 0.3kW. Magnetron sputtering is performed on NiO. X A 5 nm thick NiO layer was deposited on the dense layer. X Buffer layer.
[0067] (2) A 1.1 mol / L perovskite precursor solution (the solvent consisted of DMF (N,N-dimethylformamide) and DMSO (dimethyl sulfoxide) in a volume ratio of 4:1) was spin-coated onto NiO. X After annealing, a perovskite light-absorbing layer with a thickness of 700 nm and the chemical formula Cs was obtained on the buffer layer. 0.05 FA 0.85 MA 0.1 PbI3.
[0068] (3) Using a thermal evaporation method, C is sequentially deposited on the perovskite light-absorbing layer. 60 Layer and BCP layer; where, C 60 The deposition rate of the layer is The deposition rate of the BCP layer is
[0069] (4) Using magnetron sputtering, the vacuum level was reduced to 1×10⁻⁶. -4 Using Ar with a purity of 99.999% as the sputtering gas and a Cu target as the target material, a sputtering power of 0.5kW was used to deposit a Cu electrode with a thickness of 200nm on the BCP layer.
[0070] Example 2
[0071] This embodiment provides a perovskite solar cell, which includes FTO conductive glass and NiO stacked together. X dense layer, NiO X Buffer layer, perovskite light-absorbing layer, electron transport layer and metal electrode.
[0072] The NiO X The average pore size of the dense layer is smaller than that of the NiO X Average pore size of the buffer layer, NiO XThe average pore size of the dense layer is 1.5 nm, NiO X The average pore size of the buffer layer is 20 nm; the NiO X dense layer and NiO X The buffer layers are all doped with Li + And NiO X Li in the dense layer + The doping concentration is less than that of NiO X Li in the buffer layer + Doping concentration, NiO X Li in the dense layer + The doping concentration is 0.28 wt%, NiO X Li in the buffer layer + The doping concentration is 1.15 wt%; the NiO X The porosity of the dense layer is less than that of the NiO X Porosity of the buffer layer, NiO X The porosity of the dense layer is 1%, NiO X The porosity of the buffer layer is 20%; the NiO X The thickness of the buffer layer is 5nm, NiO X The thickness of the dense layer is 10 nm, NiO X dense layer and NiO X The thickness ratio of the buffer layer is 2:1.
[0073] The chemical formula of the perovskite light-absorbing layer is Cs. 0.05 FA 0.85 MA 0.1 The PbI3 perovskite light-absorbing layer has a thickness of 700 nm; the electron transport layer includes C atoms stacked sequentially along the direction away from the perovskite light-absorbing layer. 60 Layer and BCP layer, C 60 The thickness of the layer is 40 nm, the thickness of the BCP layer is 10 nm; the metal electrode is a Cu electrode with a thickness of 200 nm.
[0074] This embodiment also provides a method for preparing the above-mentioned perovskite solar cell, the method comprising the following steps:
[0075] (1) Using 300mm×300mm FTO conductive glass as a substrate, the substrate is carried into the PVD magnetron sputtering cavity along with the carrier plate holder, and the vacuum level is evacuated to 1×10⁻⁶. -4 Pa, using Ar and O2 with a purity of 99.999% as sputtering and reactant gases respectively, with an Ar to O2 volume ratio of 8:1, co-sputtering was performed using NiOx and Li2O targets. X The sputtering power of the target was 5 kW, and the sputtering power of the Li2O target was 0.05 kW, resulting in a NiO layer with a thickness of 10 nm.X Dense layer.
[0076] Adjust the volume ratio of Ar and O2 to 2:1, NiO X The sputtering power of the target is 1kW, and the sputtering power of the Li2O target is 0.2kW. Magnetron sputtering is performed on NiO. X A 5 nm thick NiO layer was deposited on the dense layer. X Buffer layer.
[0077] (2) A 1.1 mol / L perovskite precursor solution (the solvent consisted of DMF and DMSO in a volume ratio of 4:1) was spin-coated onto NiO. X After annealing, a perovskite light-absorbing layer with a thickness of 700 nm and the chemical formula Cs was obtained on the buffer layer. 0.05 FA 0.85 MA 0.1 PbI3.
[0078] (3) Using a thermal evaporation method, C is sequentially deposited on the perovskite light-absorbing layer. 60 Layer and BCP layer; where, C 60 The deposition rate of the layer is The deposition rate of the BCP layer is
[0079] (4) Using magnetron sputtering, the vacuum level was reduced to 1×10⁻⁶. -4 Using Ar with a purity of 99.999% as the sputtering gas and a Cu target as the target material, a sputtering power of 0.5kW was used to deposit a Cu electrode with a thickness of 200nm on the BCP layer.
[0080] Example 3
[0081] This embodiment provides a perovskite solar cell, which includes FTO conductive glass and NiO stacked together. X dense layer, NiO X Buffer layer, perovskite light-absorbing layer, electron transport layer and metal electrode.
[0082] The NiO X The average pore size of the dense layer is smaller than that of the NiO X Average pore size of the buffer layer, NiO X The average pore size of the dense layer is 1 nm, NiO X The average pore size of the buffer layer is 10 nm; the NiO X dense layer and NiO X The buffer layers are all doped with Li + And NiO X Li in the dense layer + The doping concentration is less than that of NiOX Li in the buffer layer + Doping concentration, NiO X Li in the dense layer + The doping concentration is 0.15 wt%, NiO X Li in the buffer layer + The doping concentration is 0.82 wt%; the NiO X The porosity of the dense layer is less than that of the NiO X Porosity of the buffer layer, NiO X The porosity of the dense layer is 5%, NiO X The porosity of the buffer layer is 30%; the NiO X The thickness of the buffer layer is 2nm, NiO X The thickness of the dense layer is 15 nm, NiO X dense layer and NiO X The thickness ratio of the buffer layer is 7.5:1.
[0083] The chemical formula of the perovskite light-absorbing layer is Cs. 0.05 FA 0.85 MA 0.1 The PbI3 perovskite light-absorbing layer has a thickness of 700 nm; the electron transport layer includes C atoms stacked sequentially along the direction away from the perovskite light-absorbing layer. 60 Layer and BCP layer, C 60 The thickness of the layer is 40 nm, the thickness of the BCP layer is 10 nm; the metal electrode is a Cu electrode with a thickness of 200 nm.
[0084] This embodiment also provides a method for preparing the above-mentioned perovskite solar cell, the method comprising the following steps:
[0085] (1) Using 300mm×300mm FTO conductive glass as a substrate, the substrate is carried into the PVD magnetron sputtering cavity along with the carrier plate holder, and the vacuum level is evacuated to 1×10⁻⁶. -4 Pa, using Ar and O2 with a purity of 99.999% as sputtering and reacting gases respectively, with an Ar to O2 volume ratio of 12:1, co-sputtering was performed using NiOx and Li2O targets. X The sputtering power of the target was 8 kW, and the sputtering power of the Li2O target was 0.15 kW, resulting in a NiO layer with a thickness of 15 nm. X Dense layer.
[0086] Adjust the volume ratio of Ar and O2 to 5:1, NiO X The sputtering power of the target is 4kW, and the sputtering power of the Li2O target is 0.4kW. Magnetron sputtering is performed on NiO. X A NiO layer with a thickness of 2 nm was deposited on the dense layer.X Buffer layer.
[0087] (2) A 1.1 mol / L perovskite precursor solution (the solvent consisted of DMF and DMSO in a volume ratio of 4:1) was spin-coated onto NiO. X After annealing, a perovskite light-absorbing layer with a thickness of 700 nm and the chemical formula Cs was obtained on the buffer layer. 0.05 FA 0.85 MA 0.1 PbI3.
[0088] (3) Using a thermal evaporation method, C is sequentially deposited on the perovskite light-absorbing layer. 60 Layer and BCP layer; where, C 60 The deposition rate of the layer is The deposition rate of the BCP layer is
[0089] (4) Using magnetron sputtering, the vacuum level was reduced to 1×10⁻⁶. -4 Using Ar with a purity of 99.999% as the sputtering gas and a Cu target as the target material, a sputtering power of 0.5kW was used to deposit a Cu electrode with a thickness of 200nm on the BCP layer.
[0090] Example 4
[0091] The difference between this embodiment and Embodiment 1 is that the NiO in step (1) is adjusted. X The magnetron sputtering parameters of the dense layer enable NiO X The average pore size of the dense layer is 5 nm.
[0092] The remaining preparation methods and parameters are consistent with those in Example 1.
[0093] Example 5
[0094] The difference between this embodiment and Embodiment 1 is that the NiO in step (1) is adjusted. X The magnetron sputtering parameters of the buffer layer enable NiO X The average pore size of the buffer layer is 25 nm.
[0095] The remaining preparation methods and parameters are consistent with those in Example 1.
[0096] Example 6
[0097] The difference between this embodiment and Embodiment 1 is that the NiO X The porosity of the dense layer is equal to that of the NiO X The porosity of the buffer layer is 5%.
[0098] The remaining preparation methods and parameters are consistent with those in Example 1.
[0099] Example 7
[0100] The difference between this embodiment and Embodiment 1 is that the NiO is adjusted. X The magnetron sputtering time of the dense layer makes NiO X dense layer and NiO X The thickness ratio of the buffer layer is 0.5:1.
[0101] The remaining preparation methods and parameters are consistent with those in Example 1.
[0102] Example 8
[0103] The difference between this embodiment and Embodiment 1 is that the NiO is adjusted. X The magnetron sputtering time of the dense layer makes NiO X dense layer and NiO X The thickness ratio of the buffer layer is 8:1.
[0104] The remaining preparation methods and parameters are consistent with those in Example 1.
[0105] Example 9
[0106] The difference between this embodiment and Embodiment 1 is that the NiO X Li in the dense layer + The doping concentration is 0.35 wt%.
[0107] The remaining preparation methods and parameters are consistent with those in Example 1.
[0108] Example 10
[0109] The difference between this embodiment and Embodiment 1 is that the NiO X Li in the buffer layer + The doping concentration is 0.4 wt%.
[0110] The remaining preparation methods and parameters are consistent with those in Example 1.
[0111] Comparative Example 1
[0112] The difference between this comparative example and Example 1 is that NiO is not included. X Buffer layer.
[0113] The remaining preparation methods and parameters are consistent with those in Example 1.
[0114] Comparative Example 2
[0115] The difference between this comparative example and Example 1 is that the NiO in step (1) is adjusted. X dense layer and NiO X The magnetron sputtering parameters of the buffer layer enable NiOX The average pore size of the dense layer is 15 nm, NiO X The average pore size of the buffer layer is 2 nm.
[0116] The remaining preparation methods and parameters are consistent with those in Example 1.
[0117] Comparative Example 3
[0118] The difference between this comparative example and Example 1 is that NiO X Li in the dense layer + The doping concentration is greater than that of NiO X Li in the buffer layer + Doping concentration, and NiO X Li in the dense layer + The doping concentration is 0.46 wt%, NiO X Li in the buffer layer + The doping concentration is 0.046 wt%.
[0119] The remaining preparation methods and parameters are consistent with those in Example 1.
[0120] Comparative Example 4
[0121] The difference between this comparative example and Example 1 is that NiO is first deposited on the FTO glass. X Buffer layer, then NiO deposition X Dense layer.
[0122] The remaining preparation methods and parameters are consistent with those in Example 1.
[0123] Performance testing
[0124] The photoelectric performance of the perovskite solar cells provided in the above embodiments and comparative examples was tested under the following conditions: AM1.5, 1000 W / m 2 , 25±2℃.
[0125] In addition, long-term stability tests were conducted under the following conditions: air environment, temperature of 25°C, relative humidity of 45%, and battery efficiency was recorded.
[0126] The test results are shown in Table 1.
[0127] Table 1
[0128]
[0129]
[0130] analyze:
[0131] This invention designs NiO X dense layer and NiOX The buffer layer collaboratively constructs the hole transport gradient structure, using NiO on one hand. X The dense layer maintains the high conductivity of the hole transport layer and avoids excessive Li. + Introducing scattering centers ensures ohmic contact with the conductive substrate and reduces the risk of ion migration, thus improving the long-term stability of the battery. On the other hand, the use of NiO... X The buffer layer provides more holes, enhancing the efficiency of interface charge extraction and improving the battery efficiency. Furthermore, this hole transport gradient structure increases the contact area between the hole transport layer and the perovskite light-absorbing layer, and alleviates lattice mismatch through deformation, helping to suppress interface reactions and reduce interface defects, thereby further improving battery efficiency and long-term stability.
[0132] A comparison of Example 1 and Examples 4-5 shows that, when NiO is satisfied... X The average pore size of the dense layer is smaller than that of NiO. X Given the average pore size of the buffer layer, if NiO X If the average pore size of the dense layer is too large, it will exacerbate water and oxygen permeation and ion migration, leading to a decrease in battery performance; if NiO X If the average pore size of the buffer layer is too large, the perovskite precursor cannot be completely covered, resulting in pinholes and a decrease in battery performance.
[0133] A comparison between Example 1 and Example 6 shows that if NiO X The porosity of the dense layer is equal to that of the NiO X The porosity of the buffer layer is significantly different from that of the perovskite lattice, making it impossible to alleviate the mismatch through deformation, which exacerbates interface defects and leads to a decline in battery performance.
[0134] A comparison of Example 1 and Examples 7-8 shows that if NiO X dense layer and NiO X If the thickness of the buffer layer is too small, it will increase the series resistance, reduce the hole extraction efficiency, and lead to a decrease in battery performance; if the NiO layer thickness is too small, it will increase the series resistance, reduce the hole extraction efficiency, and lead to a decrease in battery performance. X dense layer and NiO X If the thickness of the buffer layer is too large, internal stress will accumulate, increasing interface defects and leading to a decline in battery performance.
[0135] A comparison of Example 1 and Examples 9-10 shows that, when NiO is satisfied... X Li in the dense layer + Doping concentration less than NiO X Li in the buffer layer + Under the premise of doping concentration, if NiO X Li in the dense layer + Excessive doping concentration introduces carrier scattering, reducing carrier mobility and leading to decreased battery performance; if NiO...X Li in the buffer layer + If the doping concentration is too low, the improvement in energy level will be limited, the carrier mobility will be reduced, and the battery performance will decline.
[0136] A comparison of Example 1 and Comparative Example 1 shows that if only a single layer of NiO is provided... X In dense layers, the large lattice difference between NiOx and perovskite means that the dense film cannot alleviate the mismatch through deformation, exacerbating interface defects and leading to a decline in battery performance.
[0137] As can be seen from the comparison between Example 1 and Comparative Example 2, if NiO X The average pore size of the dense layer is greater than that of NiO. X The average pore size of the buffer layer increases the series resistance, reduces the hole extraction efficiency, and leads to a decrease in battery performance.
[0138] As can be seen from the comparison between Example 1 and Comparative Example 3, if NiO X Li in the dense layer + Doping concentration greater than NiO X Li in the buffer layer + Doping concentration, then excess Li + Introducing scattering centers reduces carrier mobility, increases contact resistance with the bottom electrode, and increases the risk of ion migration, leading to a decline in battery performance.
[0139] As can be seen from the comparison between Example 1 and Comparative Example 4, if NiO X dense layer and NiO X If the position of the buffer layer is reversed, the difference between the NiOx dense layer and the perovskite lattice will be large. The dense film cannot alleviate the mismatch through deformation, which will aggravate the interface defects and lead to a decrease in battery performance.
[0140] It should be noted that the present invention is illustrated through the above embodiments, but the present invention is not limited to the above process steps, that is, it does not mean that the present invention must rely on the above process steps to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials used in the present invention, additions of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A perovskite solar cell, characterized in that, The perovskite solar cell includes a conductive substrate and NiO stacked together. X dense layer, NiO X Buffer layer, perovskite light-absorbing layer, electron transport layer and electrodes; The NiO X The average pore size of the dense layer is smaller than that of the NiO X The average pore size of the buffer layer; the NiO X dense layer and NiO X The buffer layers are all doped with Li + And NiO X Li in the dense layer + The doping concentration is less than that of NiO X Li in the buffer layer + Doping concentration.
2. The perovskite solar cell according to claim 1, characterized in that, The NiO X The average pore size of the dense layer is ≤2nm; The NiO X The average pore size of the buffer layer is ≤20nm.
3. The perovskite solar cell according to claim 1, characterized in that, The NiO X The porosity of the dense layer is less than that of the NiO X Porosity of the buffer layer; The NiO X The porosity of the dense layer is ≤5%; The NiO X The porosity of the buffer layer is ≤30%.
4. The perovskite solar cell according to claim 1, characterized in that, The NiO X The thickness of the buffer layer is 2-10 nm; The NiO X dense layer and the NiO X The thickness ratio of the buffer layer is (1-7.5):
1.
5. The perovskite solar cell according to claim 1, characterized in that, The NiO X Li in the dense layer + The doping concentration is 0.046-0.28 wt%. The NiO X Li in the buffer layer + The doping concentration is 0.46-1.15 wt%.
6. The perovskite solar cell according to any one of claims 1-5, characterized in that, The conductive substrate is conductive glass; The chemical formula of the perovskite light-absorbing layer is ABX3, wherein A includes any one or a combination of at least two of formamidinium ions, methylamine ions or cesium ions, B includes lead ions and / or tin ions, and X is a halide ion. The electron transport layer includes a PCBM layer, a SnO2 layer, a TiO2 layer, a ZnO layer, and a C layer. 60 Any one or at least two of the layers or BCP layers; The electrode is a metal electrode.
7. A method for fabricating a perovskite solar cell, characterized in that, The preparation method includes the following steps: NiO was sequentially prepared on a conductive substrate. X dense layer, NiO X The perovskite solar cell is obtained by comprising a buffer layer, a perovskite light-absorbing layer, an electron transport layer, and electrodes.
8. The preparation method according to claim 7, characterized in that, The NiO X dense layer and NiO X The methods for preparing the buffer layer can be independently categorized into magnetron sputtering; The NiO X When the dense layer is prepared by magnetron sputtering, the operating parameters include: Target materials include NiO X Target and Li2O target, NiO X The sputtering power of the target is 5-8kW, the sputtering power of the Li2O target is 0.05-0.15kW, and the volume ratio of sputtering gas to reactant gas is (8-12):
1. The NiO X When the buffer layer is prepared by magnetron sputtering, the operating parameters include: Target materials include NiO X Target and Li2O target, NiO X The sputtering power of the target is 1-4kW, the sputtering power of the Li2O target is 0.2-0.4kW, and the volume ratio of sputtering gas to reactant gas is (2-5):
1.
9. The preparation method according to claim 7 or 8, characterized in that, The preparation method includes the following steps: A NiO layer with a thickness of 10-15 nm was deposited on conductive glass by magnetron sputtering. X Dense layer; wherein, the operating parameters of magnetron sputtering include: Target materials include NiO X Target and Li2O target, NiO X The sputtering power of the target is 5-8kW, the sputtering power of the Li2O target is 0.05-0.15kW, and the volume ratio of sputtering gas to reactant gas is (8-12):
1. In NiO X A NiO layer with a thickness of 2-10 nm was deposited by magnetron sputtering on a dense layer. X Buffer layer; wherein, the operating parameters of magnetron sputtering include: Target materials include NiO X Target and Li2O target, NiO X The sputtering power of the target is 1-4kW, the sputtering power of the Li2O target is 0.2-0.4kW, and the volume ratio of sputtering gas to reactant gas is (2-5):
1. Coating a perovskite precursor solution onto NiO X After annealing, a perovskite light-absorbing layer with a thickness of 300-1000 nm is obtained on the buffer layer; An electron transport layer is deposited on a perovskite light-absorbing layer; wherein the deposition rate of the electron transport layer is... A metal electrode with a thickness of 50-250 nm is deposited on the electron transport layer.
10. A photovoltaic module, characterized in that, The photovoltaic module includes a perovskite solar cell as described in any one of claims 1-6, or a perovskite solar cell prepared by the preparation method as described in any one of claims 7-9.
Citation Information
Patent Citations
Zinc-doped nickel oxide hole transport layer reserve perovskite solar cell and preparation method
CN108063186A
Inverse perovskite solar cell based on iron-doped nickel oxide hole transport layer, preparation method and application thereof