A flexible radiation-photovoltaic synergistic energy cell and its construction method

By using a flexible radiation-photovoltaic synergistic coupling energy battery structure, the problems of low energy conversion efficiency and poor mechanical stability of flexible batteries in complex environments are solved, achieving high-efficiency energy conversion and self-healing encapsulation, thus improving the overall performance of the battery.

CN123124567APending Publication Date: 2026-11-17CHINA HUADIAN ENG CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611037082.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Flexible batteries cannot effectively convert high-energy radiation energy in complex environments. Stress accumulation at multi-layered heterogeneous interfaces during mechanical deformation leads to delamination. Once the encapsulation layer is damaged, it cannot automatically restore its protective performance.

Method used

The flexible radiation-photovoltaic synergistic coupling energy battery structure includes a flexible substrate, a back electrode, a photovoltaic conversion core layer, a transparent conductive electrode, a spectral modulation layer, a flexible buffer interface layer, a radiation-responsive quantum dot composite dielectric layer, and a self-healing outer encapsulation layer. Through modified inorganic material-filled polymer network and dynamic covalent bond design, energy conversion and structural damage self-repair are achieved.

Benefits of technology

It improves the overall conversion efficiency of radiation energy and light energy, reduces the risk of mechanical damage to the device under dynamic deformation, and restores the density of the encapsulation layer through a self-healing mechanism, thereby improving the mechanical stability and long-term working performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124567A_ABST
    Figure CN123124567A_ABST
Patent Text Reader

Abstract

This application relates to the field of flexible battery manufacturing, and discloses a flexible radiation-photovoltaic synergistic coupling energy battery and its construction method. The battery comprises, from bottom to top, a flexible substrate, a back electrode, a photovoltaic conversion core layer, a transparent conductive electrode, a spectral modulation layer, a flexible buffer interface layer, a radiation-responsive quantum dot composite dielectric layer, and a self-healing outer encapsulation layer. This application employs a discontinuous rigid film to construct a flexible conductive path to alleviate bending stress, and significantly reduces light loss through a spectral modulation layer with gradient refractive index or micro / nano scattering structures. All-inorganic perovskite quantum dots absorb high-energy rays and release visible light, which is then used to generate electricity by the photovoltaic layer, achieving efficient and comprehensive energy collection. Surface-modified nano-silica shares stress in the buffer interface layer to reduce the risk of delamination; dynamic disulfide bonds in the encapsulation layer promote rebonding at broken sites, achieving self-repair and improving battery operational stability and service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of flexible battery manufacturing, specifically a flexible radiation-photovoltaic synergistic coupling energy battery and its construction method. Background Technology

[0002] Flexible photovoltaic (PV) energy supply systems face severe challenges in complex environments. Current energy supply technologies primarily focus on capturing a single form of energy. In environments with radioactive radiation, existing flexible PV modules can only collect energy in the visible light spectrum. Energy from high-energy rays is often wasted, resulting in suboptimal energy utilization. Due to the lack of a radiation energy conversion mechanism, high-energy particles can also penetrate the protective layer and damage the internal crystal lattice. This phenomenon leads to a decrease in battery output power in environments with weak light but strong radiation. Because radiant energy cannot be effectively converted into usable electrical energy, the overall energy output efficiency of the battery is limited.

[0003] Flexible devices are constructed by stacking multiple functional material layers. Each layer exhibits different mechanical properties. During bending, stress often accumulates at the contact points between the rigid inorganic layer and the flexible organic layer. Mechanical stress generates shear force at the interface. This force weakens the interlayer bonding, ultimately leading to film delamination. After multiple deformations, the gaps between the layers in the stacked structure widen, causing the originally tight physical connections to fail. Existing technologies lack effective means to mitigate this modulus difference. Interface failure has become an obstacle limiting the reliable operation of flexible energy devices. Different materials deform to varying degrees under temperature changes. Temperature variations induce thermal stress within the battery. Thermal stress, along with mechanical stress, acts on the heterogeneous interface, accelerating structural collapse.

[0004] As a protective barrier, the encapsulation film is frequently exposed to sharp external objects. The surface of the encapsulation layer is highly susceptible to scratches. Harmful substances from the external environment can enter the battery through these scratches. Current encapsulation materials lack self-healing capabilities. When the encapsulation layer is damaged and gaps appear, moisture and corrosive gases can enter the core area. Chemical corrosion can lead to electrode oxidation and semiconductor layer deterioration. Once this damage occurs, the battery's output performance will degrade, making it impossible to maintain stable operation over extended periods. Existing encapsulation designs, lacking repair mechanisms, cannot sustain their protective function for long when faced with physical damage. Functional defects in the encapsulation layer shorten the service life of energy batteries under complex mechanical environments. The internal semiconductor layer is sensitive to moisture. Even tiny encapsulation leaks can lead to a loss of conversion efficiency. Materials lacking dynamic repair capabilities struggle to maintain density under long-term loads. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this application provides a flexible radiation-photovoltaic synergistic coupling energy battery and its construction method, which solves the problems that the energy battery cannot convert high-energy radiation energy, that stress accumulation at multi-layer heterogeneous interfaces during mechanical deformation causes delamination, and that the encapsulation layer cannot automatically recover its protective performance after damage and cracking.

[0006] To achieve the above objectives, this application provides the following technical solution:

[0007] In the first aspect, this application provides a flexible radiation-photovoltaic co-coupled energy battery, which adopts the following technical solution: A flexible radiation-photovoltaic synergistic coupling energy battery includes, from bottom to top, a flexible substrate, a back electrode, a photovoltaic conversion core layer, a transparent conductive electrode, a spectral modulation layer, a flexible buffer interface layer, a radiation-responsive quantum dot composite dielectric layer, and a self-healing outer encapsulation layer.

[0008] The transparent conductive electrode is an interconnected flexible conductive path with a discontinuous rigid film structure. The spectral modulation layer has a gradient refractive index structure or a micro / nano scattering structure; The flexible buffer interface layer is used to connect the spectral modulation layer and the radiation-responsive quantum dot composite medium layer, and is used for spectral modulation and stress matching between the photovoltaic conversion core layer and the radiation-responsive quantum dot composite medium layer. The flexible buffer interface layer is made of components containing the following mass percentages: 5wt% to 30wt% surface-modified nano silica particles and 70wt% to 95wt% polydimethylsiloxane prepolymer.

[0009] The radiation-responsive quantum dot composite dielectric layer is used to receive radiation from a radiation source and convert the radiation energy into downconversion fluorescence. The radiation-responsive quantum dot composite dielectric layer is made of components comprising the following mass percentages: 3wt% to 40wt% all-inorganic perovskite quantum dots and 60wt% to 95wt% polydimethylsiloxane prepolymer.

[0010] By adopting the above technical solution, and through the use of a multi-layered heterogeneous structure and the introduction of modified inorganic-filled polymer networks and dynamic covalent bond design in the interface and encapsulation layers, a comprehensive effect of synergistic energy conversion and self-repair of structural damage can be achieved. Specifically, the working mechanism of the device includes the following steps: The first step is the downconversion mechanism of radiation energy. When the radiation-responsive quantum dot composite dielectric layer is irradiated by high-energy radiation, the inorganic perovskite quantum dots distributed within the layer absorb the high-energy radiation, thereby triggering excited transitions of electrons. During the process of returning to the ground state, the excited electrons usually undergo downconversion luminescence, thus releasing photons in the visible light frequency range.

[0011] The second step involves photoelectric coupling and spectral modulation mechanisms. Visible photons emitted by the all-inorganic perovskite quantum dots, along with ambient natural light, penetrate downwards. After passing through a spectral modulation layer with a gradient refractive index structure or a micro / nano scattering structure, and a flexible buffer interface layer, they reach the photovoltaic conversion core layer by minimizing total internal reflection losses. A transparent conductive electrode with a discontinuous rigid film structure, while ensuring light transmittance, is responsible for collecting electron-hole pairs generated by the absorption of photon energy by the semiconductor material inside the photovoltaic conversion core layer. Subsequently, the electrons and holes separate under the influence of a built-in electric field and are transported and collected to the transparent conductive electrode and the back electrode to generate current output, thereby achieving the comprehensive collection of radiant and light energy.

[0012] The third step is the interfacial stress dissipation mechanism. When the device undergoes bending deformation, the polydimethylsiloxane network segments in the flexible buffer interfacial layer experience relative slippage, providing a basis for overall elastic deformation. Simultaneously, uniformly dispersed surface-modified nano-silica particles act as rigid fulcrums within the polymer network. When stress acts on the multilayer interface, these modified nanoparticles help prevent the concentrated transmission of localized stress to the rigid inorganic photovoltaic layer and transparent conductive electrodes, harmonizing the differences in thermal expansion coefficients and elastic moduli between adjacent layers, and significantly reducing the risk of mechanical fracture and delamination at the interlayer interface.

[0013] The fourth step involves the physical self-healing mechanism. When the self-healing outer encapsulation layer experiences mechanical scratches or develops microcracks, the dynamic covalent bonds (i.e., disulfide bonds) contained in the polyurethane polymer backbone often break. Driven by room temperature thermodynamics, adjacent disulfide bonds at the fracture site undergo a reversible disulfide bond exchange reaction. Sulfur atoms recombine to form new disulfide bond crosslinks, promoting the re-joining of the broken polymer network at the microscopic level, thereby closing the crack and helping to restore the compactness of the outer film structure.

[0014] Preferably, the photovoltaic conversion core layer is a copper indium gallium selenide thin-film solar cell module, and the photovoltaic conversion core layer comprises, from bottom to top, a CIGS absorber layer with a thickness of 1 to 3 μm, a CdS buffer layer with a thickness of 30 to 70 nm, and an i-ZnO layer with a thickness of 30 to 70 nm.

[0015] The transparent conductive electrode and the photovoltaic conversion core layer adopt a surface contact structure, and the conductive layer resistance of the transparent conductive electrode is controlled to be 10-200Ω / sq.

[0016] By adopting the above technical solution, the bandgap of the CIGS absorber layer matches the visible spectrum range generated by the quantum dots above, which can effectively improve photon capture and electron excitation efficiency. Furthermore, the CdS buffer layer can be used to smooth the bandgap and lattice mismatch between the CIGS absorber layer and the oxide layer. In addition, limiting each film layer to a specific thickness dimension helps maintain the mechanical flexibility of the entire inorganic semiconductor device while satisfying the physical spatial conditions for sufficient absorption and free diffusion of photogenerated carriers. This application removes the original rigid and fragile AZO window layer, replacing it with a flexible transparent conductive network with a sheet resistance controlled between 10 and 200 Ω / sq. The surface contact structure between the transparent conductive electrode and the photovoltaic absorber layer reduces contact resistance, and the discontinuous rigid film structure effectively alleviates the problem of bending stress concentration, significantly reducing the risk of bending crack propagation under dynamic deformation.

[0017] Preferably, the average particle size of the surface-modified nano-silica particles in the flexible buffer interface layer is 10-100 nm, and the surface of the surface-modified nano-silica particles is modified by coating with a silane coupling agent of 1%-10% by mass; the all-inorganic perovskite quantum dots in the radiation-responsive quantum dot composite medium layer are CsPbBr3 nanocrystals.

[0018] By employing the above technical solution, the alkoxy groups in the silane coupling agent undergo a condensation reaction with the hydroxyl groups on the surface of nano-silica, thereby grafting organosiloxane segments onto the surface of inorganic particles. The grafted organic functional groups improve the interfacial compatibility between the inorganic particles and the polydimethylsiloxane matrix, inhibiting the secondary aggregation of silica particles in the polymer medium. Furthermore, CsPbBr3 nanocrystals have a relatively high absorption cross-section for high-energy rays and readily emit green light upon radiative excitation, thereby establishing an internal conversion light source structure and improving the energy supply rate of the photoelectric conversion source.

[0019] Preferably, the polyurethane elastic film containing dynamic disulfide bonds is produced by polymerization of the following substances: polytetrahydrofuran ether diol with a molecular weight of 1000-2000, isophorone diisocyanate, and 2-hydroxyethyl disulfide as a chain extender containing dynamic disulfide bonds; the molar ratio of the polytetrahydrofuran ether diol to the isophorone diisocyanate is 1:2, and the molar ratio of the isocyanate-terminated polyurethane prepolymer obtained by reacting the polytetrahydrofuran ether diol with the isophorone diisocyanate to the 2-hydroxyethyl disulfide is 1:1.

[0020] By employing the above technical solution, polytetrahydrofuran ether diol forms flexible soft segments in the polymer macromolecular backbone to support the film's elongation at break; while isophorone diisocyanate provides a rigid hard segment structure, imparting basic tensile strength to the film. The relevant film polymerization reaction mechanism includes the following steps: In stage one, the hydroxyl groups at the ends of polytetrahydrofuran ether diol undergo a carbamate reaction with the isocyanate groups contained in isophorone diisocyanate to generate a polyurethane prepolymer backbone with free isocyanate groups at both ends.

[0021] In stage two, as the hydroxyl groups in the 2-hydroxyethyl disulfide undergo chain extension reactions with the isocyanate groups at the ends of the prepolymer, dynamic disulfide bonds are thus embedded into the polyurethane backbone along with the chain extender structure. This defined reaction ratio promotes the corresponding consumption of chemical groups and the establishment of a cross-linking network, thereby maintaining the exchange reactivity of disulfide bonds while ensuring the mechanical strength of the encapsulation layer.

[0022] Secondly, this application provides a method for constructing a flexible radiation-photovoltaic synergistic coupling energy cell, which adopts the following technical solution: A method for constructing a flexible radiation-photovoltaic synergistic energy cell includes the following steps: A flexible substrate is prepared and its surface is activated, and then a back electrode is deposited on the surface of the flexible substrate. A photovoltaic conversion core layer is prepared on the surface of the back electrode using a co-evaporation process. An interconnected flexible conductive path of a discontinuous rigid film structure is fabricated on the surface of the photovoltaic conversion core layer to form the transparent conductive electrode; The spectral modulation layer is constructed on the surface of the transparent conductive electrode; A flexible buffer interface layer composite slurry is coated on the surface of the spectral modulation layer and then thermally cured to form a flexible buffer interface layer with spectral modulation and stress relief functions. A radiation-responsive composite medium slurry is coated on a flexible buffer interface layer and then thermally cured to form a radiation-responsive quantum dot composite medium layer. On the outer surface of the radiation-responsive quantum dot composite dielectric layer, a pre-prepared polyurethane elastic film containing dynamic disulfide bonds is hot-pressed and encapsulated using a vacuum bonding process to form a self-healing outer encapsulation layer. The flexible radiation-photovoltaic co-coupled energy cell, after being heat-pressed and encapsulated, is sealed around its periphery and positive and negative electrode wires are led out to obtain the finished product.

[0023] By adopting the above technical solution, this construction method follows a bottom-up layer-by-layer integration process, physically bonding and thermosetting high-rigidity inorganic semiconductor components with a high-flexibility polymer dielectric layer. Its specific molding mechanism includes the following process steps: Phase 1: Construction of the Inorganic Substrate. The surface polarity and adhesion of the flexible substrate, after surface activation treatment, are significantly improved. Subsequently, when the photovoltaic conversion core layer is grown in situ on the surface of the flexible substrate through a co-evaporation process, gas-phase atoms are adsorbed, nucleated, and crystallized on the substrate surface, gradually forming a continuous and relatively dense inorganic thin film structure, thereby establishing the basic photoelectric conversion substrate.

[0024] Phase Two: Integration of Electrodes and Optical Control Layers. Discontinuous interconnected flexible conductive paths are fabricated on the surface of the photovoltaic thin film as transparent conductive electrodes. A spectral control layer with refractive index gradients or micro / nano scattering structures is then constructed on top of these electrodes, thereby suppressing internal lateral light loss and smoothing the photoelectric interface.

[0025] Phase Three: Interface Compatibility Control. A liquid, flexible buffer interface layer composite slurry is coated onto the surface of the spectral control layer. Under the influence of gravity and surface tension, the slurry flows in and fills the microscopic uneven structure of the inorganic film surface. During the subsequent thermosetting process, as the polydimethylsiloxane prepolymer undergoes a cross-linking reaction, the material transforms from a liquid state into a solid elastomer with a spatial network structure. The cured polymer network forms a mechanical interlock with the surface of the underlying spectral control layer, thereby establishing a physical anchoring connection.

[0026] Phase four involves the sequential curing of functional layers. After the radiation-responsive composite slurry spreads on the surface of the buffer interface layer, it undergoes a thermal curing process to complete the secondary cross-linking of the polymer network. Since both thermal curing processes involve siloxane system reactions, adjacent polymer layers often experience entanglement of polymer chain segments at the interface, thereby weakening the interlayer physical boundary to some extent.

[0027] Phase 5, Vacuum Thermopress Encapsulation. Under the combined action of a vacuum environment and applied pressure, residual gas between the encapsulation film and the dielectric layer is gradually expelled. During this process, the heat energy provided by the thermopressing causes the polymer chain segments at the interface of the polyurethane elastic film to undergo thermal motion, adhering to the surface of the underlying polydimethylsiloxane, ensuring a tight bond between the encapsulation layer and the internal functional layers, and contributing to the dense physical encapsulation of the overall device.

[0028] Preferably, in preparing the flexible substrate and performing surface activation treatment, and depositing the back electrode on the surface of the flexible substrate, the flexible substrate is pre-treated as follows: the flexible substrate is ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 10 to 20 minutes in sequence, and then dried at 60 to 100°C; subsequently, surface activation treatment is performed using low-power oxygen plasma for 30 to 180 seconds; the flexible substrate is made of polyimide film; and a gold film with a thickness of 100 to 500 nm is deposited on the surface of the flexible substrate using magnetron sputtering technology to form the back electrode.

[0029] By employing the above technical solution, ultrasonic cleaning is performed sequentially using solvents of different polarities in a gradient manner. This primarily utilizes the cavitation effect generated by ultrasound in the liquid to remove organic contaminants and inorganic particulate impurities from the substrate surface. The drying step removes residual moisture, minimizing the risk of water vapor release during subsequent vacuum coating processes. Oxygen plasma treatment further introduces oxygen-containing active functional groups, significantly improving the wettability and interlayer adhesion of the polyimide substrate surface. Based on the inherent properties of the polyimide film, it provides thermal stability to withstand the subsequent high-temperature co-evaporation process. Gold atoms generated by magnetron sputtering carry high kinetic energy and bombard the substrate surface, depositing to form a dense and continuous conductive network.

[0030] Preferably, the preparation method of the flexible buffer interface layer composite slurry in forming the flexible buffer interface layer is as follows: surface-modified nano-silica particles are mixed with polydimethylsiloxane prepolymer, first stirred at a high shear speed of 300-1500 rpm for 10-30 minutes, then ultrasonically assisted dispersion for 10-30 minutes, and finally degassed at room temperature under vacuum for 5-25 minutes; the preparation method of the radiation-responsive composite medium slurry in forming the radiation-responsive quantum dot composite medium layer is as follows: purified all-inorganic perovskite quantum dots are dispersed in toluene solvent to prepare a quantum dot dispersion, then mixed with polydimethylsiloxane prepolymer, and continuously stirred under vacuum at 500-1500 rpm to completely evaporate and remove the toluene solvent, and then degassed for 10-30 minutes.

[0031] By employing the above-mentioned technical solutions, the fluid shear force generated by mechanical high-shear stirring can break up the macroscopic aggregates of nanoparticles. Combined with the acoustic microfluidic force provided by ultrasonic-assisted dispersion, this further dismantles secondary agglomeration at the nanoscale, promoting a more uniform distribution of inorganic particles or quantum dots within the polymer prepolymer. Furthermore, continuous stirring under vacuum ensures that the original toluene solvent in the quantum dots is completely removed, preventing organic solvents from damaging the polymer crosslinking network or leaving microporous defects after curing. The vacuum degassing process reduces the probability of optical scattering centers and stress concentration defects caused by air bubbles within the cured material.

[0032] Preferably, the process for pre-preparing a polyurethane elastic film containing dynamic disulfide bonds comprises: vacuum dehydrating polytetrahydrofuran ether diol at 80–100°C for 1–2 hours, cooling and adding isophorone diisocyanate under nitrogen protection, and reacting at 60–80°C for 2–4 hours; adding 2-hydroxyethyl disulfide and dibutyltin dilaurate to the obtained material, and continuing the reaction at 60–80°C for 4–8 hours to obtain a viscous polymer solution; pouring the viscous polymer solution into a mold and curing it in a constant temperature oven at 60–80°C for 12–24 hours.

[0033] By employing the above technical solution, the vacuum dehydration process removes trace amounts of moisture from the raw materials, blocking the side reaction pathway of water molecules reacting with isocyanate groups to generate carbon dioxide gas; simultaneously, nitrogen protection maintains the reaction system in an inert environment. Prepolymerization and chain extension reactions are carried out at a limited temperature of 60–80°C, which allows for stable control of the exothermic process, ensuring the full conversion of isocyanate groups and hydroxyl groups, while avoiding uncontrolled premature exchange of disulfide bonds or polymer yellowing caused by excessively high temperatures. The added dibutyltin dilaurate acts as a catalyst, guiding the reaction towards the formation of large molecular chain segments. The final mold curing process allows the viscous polymer solution to complete cross-linking and shaping under a constant thermal field.

[0034] Preferably, in forming the spectral modulation layer, the thickness of the spectral modulation layer is controlled to be 5–15 μm; in forming the flexible buffer interface layer, the coating thickness of the flexible buffer interface layer is controlled to be 2–10 μm, the thermal curing temperature is 60–100 °C, and the time is 1–4 hours; in forming the radiation-responsive quantum dot composite medium layer, the coating thickness of the radiation-responsive quantum dot composite medium layer is controlled to be 10–50 μm through a composite coating process, the thermal curing temperature is 60–100 °C, and the time is 1–4 hours.

[0035] By adopting the above technical solution, the newly added spectral modulation layer helps to achieve precise refractive index gradient optical coupling. Limiting the coating thickness of the interface layer aims to balance the buffering requirements of the material layers on interlayer stress with the overall device flexibility constraints, avoiding a decrease in light transmittance due to excessive interface thickness. Setting the thermosetting temperature and time within the energy threshold range that triggers the hydrosilylation reaction of polydimethylsiloxane not only allows the polymer network to crosslink and cure but also avoids the problems of thermal degradation of the underlying photovoltaic material or phase transition aggregation of all-inorganic perovskite quantum dots caused by excessively high temperatures.

[0036] Preferably, in forming the self-healing outer encapsulation layer, the hot-pressing encapsulation temperature of the vacuum bonding process is set to 60–100°C, the bonding pressure is maintained at 0.1–0.3 MPa, and the duration is 15–45 minutes to ensure a tight bond between the encapsulation layer and the internal functional layer.

[0037] By employing the above technical solution, the thermopressing encapsulation temperature is controlled within a range above the glass transition temperature of the polyurethane material but below its melting temperature, allowing the polymer chain segments to maintain a macroscopic solid morphology while possessing molecular mobility. Under this condition, the applied mechanical pressure causes the encapsulation film to adhere to the surface morphology of the underlying functional layer under extrusion. With continued application over a limited time, physical adhesion and microscopic deformation matching gradually occur at the interface, thereby completing the encapsulation process of the device's external structure.

[0038] This application provides a flexible radiation-photovoltaic synergistic energy cell and its construction method. It has the following beneficial effects: 1. This application combines a radiation-responsive quantum dot composite dielectric layer with a photovoltaic conversion core layer. The all-inorganic perovskite quantum dots absorb high-energy rays and release visible light. At the same time, a spectral modulation layer with a gradient refractive index structure or micro-nano scattering structure is introduced, which effectively reduces light loss caused by total internal reflection at the interface and improves the directional coupling and propagation efficiency of secondary photons to the photoelectric interface. This enables the photovoltaic conversion core layer to absorb light energy and output current more efficiently, realizing the efficient comprehensive conversion of radiation energy and light energy.

[0039] 2. This application uses an interconnected flexible conductive path with a discontinuous rigid film structure to construct a transparent conductive electrode, which effectively alleviates the problem of bending stress concentration at the electrode level. Furthermore, by adding surface-modified nano-silica particles to the flexible buffer interface layer, the nanoparticles assist polydimethylsiloxane in sharing the bending stress and mitigating the difference in elastic modulus between the multilayer materials. The synergistic effect of the electrode network and the buffer layer significantly reduces the risk of bending crack propagation and delamination under dynamic deformation, and increases the heterogeneous interface connection strength and the overall mechanical stability of the flexible energy battery.

[0040] 3. This application uses a polyurethane elastic film containing dynamic disulfide bonds in the self-healing outer encapsulation layer. The exchange reaction of disulfide bonds at room temperature promotes the rebonding of the fracture sites, closes the cracks caused by damage and restores the integrity of the encapsulation structure, thereby providing a long-term and reliable physical barrier and environmental protection for the fragile photovoltaic absorption layer, flexible transparent electrode and spectral control layer inside. Attached Figure Description

[0041] Figure 1 This is a matching diagram of the fluorescence spectrum of the radiation-response layer and the quantum efficiency response of the outer layer of the photovoltaic core layer in this application; Figure 2 The following are current density-voltage curves of different embodiments and comparative examples of this application under radiation source irradiation; Figure 3 A comparison chart showing the efficiency retention rates of different interface layer structures in this application during cyclic bending tests; Figure 4 This is a comparison chart showing the efficiency and stability of different packaging materials in scratch repair and continuous service processes. Figure 5 This is a schematic diagram of the surface of the flexible, rollable radiation-photovoltaic synergistic coupling energy battery structure of this application; Figure 6 This is a block diagram of the energy output and management of this application; Figure 7 This is a schematic diagram of the overall structure and the stacked cross-section of each functional layer of the flexible rollable radiation-photovoltaic synergistic coupling energy battery of this application. Detailed Implementation

[0042] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0043] Preparation Examples 1-6: Preparation Example 1: This preparation example provides a method for preparing a radiation-responsive quantum dot composite medium and a self-healing polymer network. The above materials are used for the subsequent construction of flexible radiation-photovoltaic synergistic energy cells, including the following steps: (1) Synthesis of radiation-responsive quantum dots (CsPbBr3): Cesium carbonate (Cs₂CO₃) was dissolved in octadecene (ODE) and oleic acid (OA) using a hot-injection method. The solution was then subjected to vacuum dehydration and deoxygenation treatment at 120°C for 30 minutes to obtain the cesium precursor. Lead bromide (PbBr₂) was dissolved in octadecene (ODE), oleic acid (OA), and oleylamine (OAm). After stirring and dissolving at 100°C, the system was heated to 140°C. The prepared cesium precursor was then rapidly injected into the aforementioned lead bromide solution. The reaction was quenched in an ice bath immediately after 5 seconds. Finally, the solution was purified by centrifugation to obtain pure, all-inorganic perovskite CsPbBr₃ nanocrystalline powder. To avoid particle agglomeration leading to localized stress concentration, the luminescent particles were treated with a surface coupling agent before dispersion to form an organic compatibility layer on their surface, thereby improving their bonding ability with the polymer matrix.

[0044] (2) Preparation of radiation-responsive composite medium slurry: The purified CsPbBr3 nanocrystals were dispersed in toluene solvent to prepare a quantum dot dispersion with a concentration of 10 mg / mL. Polydimethylsiloxane (PDMS) prepolymer (containing siloxane main agent and platinum catalyst in a mass ratio of 10:1) was taken. The quantum dot dispersion and PDMS prepolymer were mixed, and the mixing amount was calculated so that after deducting the solvent, the actual mass ratio of the radiation-responsive medium (quantum dots) was 5 wt%, and the actual mass ratio of the flexible polymer matrix (PDMS) was 95 wt%. The mixture was placed in a vacuum mixer and stirred continuously at a speed of 500 rpm, with vacuum pumping to completely evaporate and remove the toluene solvent. Finally, degassing was continued for 10 minutes to ensure that the particles and the matrix were stably dispersed mainly through van der Waals forces and local hydrogen bonding, resulting in a uniform and bubble-free radiation-responsive composite medium slurry.

[0045] (3) Synthesis of self-healing polymer networks: Polytetrahydrofuran ether diol (PTMEG) with a molecular weight of 1000 was vacuum dehydrated at 80°C for 1 hour. The temperature was then lowered to 60°C, and nitrogen gas was introduced into the reaction system for protection. Isophorone diisocyanate (IPDI) was added, and the molar ratio of PTMEG to IPDI was controlled at 1:2. The reaction was continued for 2 hours to obtain a polyurethane prepolymer with terminal isocyanate groups. Next, a chain extender containing dynamic disulfide bonds (2-hydroxyethyl disulfide, HEDS) and trace amounts of dibutyltin dilaurate (DBTDL) were added to the system as catalysts. The molar ratio of the prepolymer to HEDS was controlled at 1:1, and the reaction was continued at 60°C for 4 hours. Finally, the resulting viscous polymer solution was poured into a mold and cured in a constant temperature oven at 60°C for 12 hours to obtain a self-healing polyurethane elastic film for the outer side of the encapsulation layer.

[0046] (4) Flexible substrate pretreatment: A 25 μm thick flexible polyimide film was selected as the substrate and subjected to ultrasonic cleaning, deionized water rinsing, and low-temperature drying. Subsequently, a low-power oxygen plasma was used for surface activation treatment for 30 seconds to improve surface polarity and wettability, enabling the interfacial buffer layer to adhere to the polyimide substrate through intermolecular forces and local chemical bonding.

[0047] (5) Preparation of transparent conductive electrode preparation solution: A silver nanowire dispersion suitable for spraying process was prepared for use in the subsequent formation of an interconnected flexible conductive path of a discontinuous rigid film structure on a flexible photovoltaic absorber layer. The resistance of the conductive layer was controlled to be 200Ω / sq to reduce the risk of bending crack propagation.

[0048] Preparation Example 2: This preparation example provides a method for preparing a radiation-responsive quantum dot composite medium and a self-healing polymer network. The above materials are used for the subsequent construction of flexible radiation-photovoltaic synergistic energy cells, including the following steps: (1) Synthesis of radiation-responsive quantum dots (CsPbBr3): Cesium carbonate (Cs₂CO₃) was dissolved in octadecene (ODE) and oleic acid (OA) using a hot-injection method. The solution was then subjected to vacuum dehydration and deoxygenation treatment at 135°C for 45 minutes to obtain the cesium precursor. Lead bromide (PbBr₂) was dissolved in octadecene (ODE), oleic acid (OA), and oleylamine (OAm). After stirring and dissolving at 110°C, the system was heated to 160°C. The prepared cesium precursor was then rapidly injected into the aforementioned lead bromide solution. The reaction was quenched immediately in an ice bath after 10 seconds. Finally, the solution was purified by centrifugation to obtain pure inorganic perovskite CsPbBr₃ nanocrystalline powder. To avoid particle agglomeration leading to localized stress concentration, the luminescent particles were treated with a surface coupling agent before dispersion to form an organic compatibility layer on their surface, thereby improving their bonding ability with the polymer matrix.

[0049] (2) Preparation of radiation-responsive composite medium slurry: The purified CsPbBr3 nanocrystals were dispersed in toluene solvent to prepare a quantum dot dispersion with a concentration of 30 mg / mL. Polydimethylsiloxane (PDMS) prepolymer (containing siloxane main agent and platinum catalyst in a mass ratio of 10:1) was taken. The quantum dot dispersion and PDMS prepolymer were mixed, and the mixing amount was calculated so that after deducting the solvent, the actual mass ratio of the radiation-responsive medium (quantum dots) was 15 wt%, and the actual mass ratio of the flexible polymer matrix (PDMS) was 85 wt%. The mixture was placed in a vacuum mixer and stirred continuously at a speed of 1000 rpm, with vacuum pumping to completely evaporate and remove the toluene solvent. Finally, degassing was continued for 20 minutes to ensure that the particles and the matrix were stably dispersed mainly through van der Waals forces and local hydrogen bonding, resulting in a uniform and bubble-free radiation-responsive composite medium slurry.

[0050] (3) Synthesis of self-healing polymer networks: Polytetrahydrofuran ether diol (PTMEG) with a molecular weight of 1500 was vacuum dehydrated at 90°C for 1.5 hours. The temperature was then lowered to 70°C, and nitrogen gas was introduced into the reaction system for protection. Isophorone diisocyanate (IPDI) was added, and the molar ratio of PTMEG to IPDI was controlled at 1:2. The reaction was continued for 3 hours to obtain a polyurethane prepolymer with terminal isocyanate groups. Next, a chain extender containing dynamic disulfide bonds (2-hydroxyethyl disulfide, HEDS) and a trace amount of dibutyltin dilaurate (DBTDL) were added to the system as catalysts, and the molar ratio of the prepolymer to HEDS was controlled at 1:1. The reaction was continued at 70°C for 6 hours. Finally, the resulting viscous polymer solution was poured into a mold and cured in a constant temperature oven at 70°C for 18 hours to obtain a self-healing polyurethane elastic film for the outer side of the encapsulation layer.

[0051] (4) Flexible substrate pretreatment: A 50 μm thick flexible polyimide film was selected as the substrate and subjected to ultrasonic cleaning, deionized water rinsing, and low-temperature drying. Subsequently, a low-power oxygen plasma was used for surface activation treatment for 90 seconds to improve surface polarity and wettability, enabling the interfacial buffer layer to adhere to the polyimide substrate through intermolecular forces and local chemical bonding.

[0052] (5) Preparation of transparent conductive electrode preparation solution: A flexible transparent conductive ink suitable for transfer printing process was prepared for use in the subsequent formation of an interconnected flexible conductive path of a discontinuous rigid film structure on a flexible photovoltaic absorber layer. The resistance of the conductive layer was controlled to be 100Ω / sq to reduce the risk of bending crack propagation.

[0053] Preparation Example 3: This preparation example provides a method for preparing a radiation-responsive quantum dot composite medium and a self-healing polymer network. The above materials are used for the subsequent construction of flexible radiation-photovoltaic synergistic energy cells, including the following steps: (1) Synthesis of radiation-responsive quantum dots (CsPbBr3): Cesium carbonate (Cs₂CO₃) was dissolved in octadecene (ODE) and oleic acid (OA) using a hot-injection method. The solution was then subjected to vacuum dehydration and deoxygenation treatment at 150°C for 60 minutes to obtain the cesium precursor. Lead bromide (PbBr₂) was dissolved in octadecene (ODE), oleic acid (OA), and oleylamine (OAm). After stirring and dissolving at 120°C, the system was heated to 180°C. The prepared cesium precursor was then rapidly injected into the aforementioned lead bromide solution. The reaction was quenched immediately in an ice bath after 15 seconds. Finally, the solution was purified by centrifugation to obtain pure, all-inorganic perovskite CsPbBr₃ nanocrystalline powder. To avoid particle agglomeration leading to localized stress concentration, the luminescent particles were treated with a surface coupling agent before dispersion to form an organic compatibility layer on their surface, thereby improving their bonding ability with the polymer matrix.

[0054] (2) Preparation of radiation-responsive composite medium slurry: The purified CsPbBr3 nanocrystals were dispersed in toluene solvent to prepare a quantum dot dispersion with a concentration of 50 mg / mL. Polydimethylsiloxane (PDMS) prepolymer (containing siloxane main agent and platinum catalyst in a mass ratio of 10:1) was taken. The quantum dot dispersion and PDMS prepolymer were mixed, and the mixing amount was calculated so that after deducting the solvent, the actual mass ratio of the radiation-responsive medium (quantum dots) was 40 wt%, and the actual mass ratio of the flexible polymer matrix (PDMS) was 60 wt%. The mixture was placed in a vacuum stirrer and stirred continuously at a speed of 1500 rpm, with vacuum pumping to completely evaporate and remove the toluene solvent. Finally, degassing was continued for 30 minutes to ensure that the particles and the matrix were stably dispersed mainly through van der Waals forces and local hydrogen bonding, resulting in a uniform and bubble-free radiation-responsive composite medium slurry.

[0055] (3) Synthesis of self-healing polymer networks: Polytetrahydrofuran ether diol (PTMEG) with a molecular weight of 2000 was vacuum dehydrated at 100°C for 2 hours. The temperature was then lowered to 80°C, and nitrogen gas was introduced into the reaction system for protection. Isophorone diisocyanate (IPDI) was added, and the molar ratio of PTMEG to IPDI was controlled at 1:2. The reaction was continued for 4 hours to obtain a polyurethane prepolymer with terminal isocyanate groups. Next, a chain extender containing dynamic disulfide bonds (2-hydroxyethyl disulfide, HEDS) and trace amounts of dibutyltin dilaurate (DBTDL) were added to the system as catalysts. The molar ratio of the prepolymer to HEDS was controlled at 1:1, and the reaction was continued at 80°C for 8 hours. Finally, the resulting viscous polymer solution was poured into a mold and cured in a constant temperature oven at 80°C for 24 hours to obtain a self-healing polyurethane elastic film for the outer side of the encapsulation layer.

[0056] (4) Flexible substrate pretreatment: A 125 μm thick flexible polyimide film was selected as the substrate and subjected to ultrasonic cleaning, deionized water rinsing, and low-temperature drying. Subsequently, a low-power oxygen plasma was used for surface activation treatment for 180 s to improve surface polarity and wettability, enabling the interfacial buffer layer to adhere to the polyimide substrate through intermolecular forces and local chemical bonding.

[0057] (5) Preparation of transparent conductive electrode materials: Prepare a target material suitable for cryogenic sputtering process for subsequent formation of an interconnected flexible conductive path consisting of a discontinuous rigid grid on the flexible photovoltaic absorber layer. The resistance of the conductive layer is controlled to 10Ω / sq to reduce the risk of bending crack propagation.

[0058] Preparation Example 4: This preparation example provides a method for preparing a composite material for a flexible buffer interface layer. The material is used for spectral modulation and stress matching between the photovoltaic conversion core layer and the radiation response layer, and includes the following steps: (1) Surface modification of nano-oxide particles: Nano-sized silica (SiO2) particles with an average particle size of 10 nm were added to an anhydrous ethanol solution of 1% by mass of silane coupling agent (KH-550). The particles were ultrasonically dispersed at 40 °C for 15 minutes to ensure that the coupling agent fully coated the surface of the nanoparticles. The solid was then collected by centrifugation, washed three times with anhydrous ethanol to remove unreacted coupling agent, and finally vacuum dried at 60 °C to obtain surface-modified nano-silica particles.

[0059] (2) Preparation of the composite system: Polydimethylsiloxane (PDMS) prepolymer (containing siloxane main agent and platinum catalyst in a mass ratio of 10:1) was used as the matrix material; according to the composition ratio, the above surface-modified nano silica particles were weighed and added to the PDMS prepolymer, and the mass percentage of nano silica particles was controlled to be 5 wt%, and the mass percentage of PDMS matrix was 95 wt%.

[0060] (3) Mixing, dispersing and degassing treatment: The mixture was placed in a high-shear mixer and initially stirred at 300 rpm for 10 minutes. The slurry was then placed in an ultrasonic cleaner and dispersed at low power for 10 minutes to eliminate particle aggregates. Finally, the slurry was placed in a vacuum drying oven and degassed at room temperature for 5 minutes to obtain a uniform, transparent, flexible buffer interface layer composite slurry with low refractive index matching characteristics. This slurry is used to construct the basic spectral modulation layer. During curing, the surface roughness between the radiation excitation layer and the spectral modulation layer is controlled within the sub-micron range to reduce lateral light loss caused by total internal reflection at the interface.

[0061] Preparation Example 5: This preparation example provides a method for preparing a composite material for a flexible buffer interface layer. The material is used for spectral modulation and stress matching between the photovoltaic conversion core layer and the radiation response layer, and includes the following steps: (1) Surface modification of nano-oxide particles: Nano-sized silica (SiO2) particles with an average particle size of 50 nm were added to an anhydrous ethanol solution of 5% by mass of silane coupling agent (KH-550). The particles were ultrasonically dispersed at 60 °C for 45 minutes to allow the coupling agent to undergo a condensation reaction with the hydroxyl groups on the surface of the nanoparticles under high kinetic energy. The solid was then collected by centrifugation, washed three times with anhydrous ethanol to remove excess coupling agent, and finally vacuum dried at 80 °C to obtain surface-modified silica nanoparticles.

[0062] (2) Preparation of the composite system: Polydimethylsiloxane (PDMS) prepolymer (containing siloxane main agent and platinum catalyst in a mass ratio of 10:1) was used as the matrix material; according to the composition ratio, the above surface-modified nano silica particles were weighed and added to the PDMS prepolymer, and the mass ratio of nano silica particles was controlled to be 15wt% and the mass ratio of PDMS matrix was 85wt%.

[0063] (3) Mixing, dispersing and degassing treatment: The mixture was placed in a high-shear mixer and mechanically stirred at 900 rpm for 20 minutes. The slurry was then placed in an ultrasonic cleaner and dispersed at medium power for 20 minutes to ensure a highly uniform distribution of nanoparticles. Finally, the slurry was placed in a vacuum drying oven and degassed at room temperature for 15 minutes to obtain a uniform, flexible buffer interface layer composite slurry with excellent interfacial optical control capabilities. This slurry can be alternately deposited with transparent polymer slurries of different refractive indices (such as the slurry prepared in Preparation Example 4) to form a spectral control layer with a gradient refractive index structure. The refractive index difference between adjacent layers is controlled within the range of 0.02–0.20, thereby effectively reducing interfacial reflection loss and improving the directional propagation capability of secondary photons.

[0064] Preparation Example 6: This preparation example provides a method for preparing a composite material for a flexible buffer interface layer. The material is used for spectral modulation and stress matching between the photovoltaic conversion core layer and the radiation response layer, and includes the following steps: (1) Surface modification of nano-oxide particles: Nano-sized silica (SiO2) particles with an average particle size of 100 nm were added to an anhydrous ethanol solution containing 10% by mass of silane coupling agent (KH-550). The particles were ultrasonically dispersed at 80 °C for 75 minutes. Through the high temperature and high concentration of coupling agent environment, the surface of the nano-silica was chemically grafted and modified to a very high degree. The solid was then collected by centrifugation, washed three times with anhydrous ethanol to remove redundant coupling agent, and finally vacuum dried at 100 °C to obtain modified nano-silica particles with a high grafting rate.

[0065] (2) Preparation of the composite system: Polydimethylsiloxane (PDMS) prepolymer (containing siloxane main agent and platinum catalyst in a mass ratio of 10:1) was used as the matrix material; according to the composition ratio, the above surface-modified nano silica particles were weighed and added to the PDMS prepolymer, and the mass ratio of nano silica particles was controlled to be 30wt% and the mass ratio of flexible polymer matrix (PDMS) was 70wt%.

[0066] (3) Mixing, dispersing and degassing treatment: The high-load mixture was placed in a high-shear mixer and vigorously stirred at 1500 rpm for 30 minutes to overcome the viscosity resistance caused by the high concentration of powder. The mixture was then placed in an ultrasonic cleaner and subjected to high-power dispersion for 30 minutes to eliminate secondary agglomeration caused by the high concentration. Finally, the mixture was placed in a vacuum drying oven and degassed at room temperature for 25 minutes to obtain a flexible buffer interface layer composite slurry with dense component distribution, excellent thermal stability, and high transparency and optical coupling properties. This slurry can be used to form a light propagation control interface using micro / nano scattering structures, and utilizes high-concentration nanoparticles to create submicron-level surface roughness, thereby effectively improving the coupling efficiency of secondary photons.

[0067] Examples 1-3: Example 1: This embodiment provides a method for fabricating a flexible radiation-photovoltaic synergistic coupling energy battery. The battery employs a basic flexible radiation-photovoltaic coupling structure, achieving efficient conversion of radiative energy into electrical energy through the integration of multiple functional gradients, and possesses excellent flexibility and self-healing capabilities. The method includes the following steps: (1) Preparation of flexible substrate and back electrode: A 50 μm thick polyimide (PI) film was selected as a flexible substrate and ultrasonically cleaned for 15 minutes each with acetone, anhydrous ethanol, and deionized water, followed by drying at 80 °C. Then, a low-power oxygen plasma was used for surface activation treatment for 90 s to improve surface polarity and wettability. A 300 nm thick gold (Au) film was deposited on the PI film surface as a back electrode using magnetron sputtering technology.

[0068] (2) Integration of the photovoltaic conversion core layer and the transparent conductive electrode: CIGS (copper indium gallium selenide) thin-film solar cell modules were fabricated on the back electrode surface using a co-evaporation process. These modules comprise a CIGS absorber layer (2 μm), a CdS buffer layer (50 nm), and an i-ZnO layer (50 nm). Considering the high-temperature sensitivity of the flexible photovoltaic layer, the entire deposition process was controlled within the temperature tolerance range of the flexible substrate, followed by low-temperature annealing after deposition. A surface contact structure was adopted between the flexible transparent conductive electrode and the photovoltaic absorber layer. An interconnected flexible conductive path, formed by transferring the flexible transparent conductive ink as described in Example 2, was used to create a discontinuous rigid film structure. The resistance of the conductive layer was controlled at approximately 100 Ω / sq to reduce the risk of bending crack propagation.

[0069] (3) Construction of flexible buffer interface layer and spectral modulation layer: A planarization treatment was first applied to the surface of the photovoltaic module to reduce recombination loss. Then, a spectral modulation layer of about 5 μm thickness was first constructed by spin coating (using the composite slurry prepared in Preparation Example 4). A flexible buffer interface layer of about 2 μm thickness (using the nano-silica modified PDMS composite slurry prepared in Preparation Example 5) was then spin coated on top of the layer. The device was then placed in a constant temperature oven at 80°C for 2.5 hours to cure, forming an interface layer structure with spectral modulation and stress relief functions.

[0070] (4) Construction of radiation-responsive quantum dot composite dielectric layer: The CsPbBr3 / PDMS radiation-responsive composite slurry prepared in Preparation Example 2 (containing approximately 15 wt% luminescent particles) was coated onto a flexible buffer interface layer using a composite coating process, with the thickness of the responsive layer controlled to be 20 μm. It was then thermocured again in an 80°C oven for 2.5 hours to form a downconversion layer that converts incident radiation energy into visible fluorescence. The organic compatibility layer on the surface of the luminescent particles at the interface ensures stable dispersion between the particles and the polymer matrix through van der Waals forces and local hydrogen bonding.

[0071] (5) Integration of self-healing outer encapsulation layer: The self-healing polyurethane elastic film with dynamic disulfide bonds synthesized in Preparation Example 2 was used as a flexible barrier film and cut to a size slightly larger than the device size. At a temperature of 80°C, the self-healing film was hot-pressed onto the outer surface of the radiation response layer using a vacuum laminator. The pressure was maintained at 0.2 MPa for 30 minutes to ensure a tight, bubble-free bond between the encapsulation layer and the internal functional layer, forming an overall sealed structure.

[0072] (6) Finished product post-processing and testing: The encapsulated flexible energy cell was peripherally sealed, and positive and negative electrode wires were led out to obtain a flexible radiation-photovoltaic synergistic energy cell with an overall thickness between 150-200 μm. Under standard radiation source irradiation, the cell utilizes the fluorescence down-conversion effect of the quantum dot layer and the photovoltaic effect of the CIGS layer to supply energy. In experiments, the device maintained a stable voltage output even under low illumination; after periodic bending tests, no significant failure was observed in the device output, indicating its good flexibility and stability.

[0073] Example 2: This embodiment provides a method for fabricating a flexible radiation-photovoltaic synergistic energy battery. Based on Embodiment 1, this battery adopts a gradient refractive index spectral modulation structure and verifies the basic radiation response and photoelectric conversion performance of the device under ultra-thin and ultra-flexible requirements through a combination of functional layers with a low loading ratio. The method includes the following steps: (1) Preparation of flexible substrate and back electrode: A 25 μm thick polyimide (PI) film was selected as the flexible substrate. It was ultrasonically cleaned for 10 minutes each with acetone, anhydrous ethanol and deionized water, rinsed with deionized water and dried at 60 °C. Then, a low-power oxygen plasma was used for surface activation treatment for 30 seconds to improve surface polarity and wettability. A 100 nm thick gold (Au) film was deposited on the PI film surface as the back electrode using magnetron sputtering technology.

[0074] (2) Integration of the photovoltaic conversion core layer and the transparent conductive electrode: CIGS (copper indium gallium selenide) thin-film solar cell modules were fabricated on the back electrode surface using a co-evaporation process. These modules comprise a CIGS absorber layer (1 μm), a CdS buffer layer (30 nm), and an i-ZnO layer (30 nm). Considering the high-temperature sensitivity of the flexible photovoltaic layer, the entire deposition process was controlled within the temperature tolerance range of the flexible substrate, followed by low-temperature annealing after deposition. A surface contact structure was adopted between the flexible transparent conductive electrode and the photovoltaic absorber layer. An interconnected flexible conductive path was formed by spraying the silver nanowire dispersion from Preparation Example 1 onto the substrate, creating a discontinuous rigid film structure. The resistance of the conductive layer was controlled at approximately 200 Ω / sq to reduce the risk of bending crack propagation.

[0075] (3) Construction of flexible buffer interface layer and spectral modulation layer: To reduce recombination losses, a surface smoothing treatment was preferentially applied to the photovoltaic module surface. Subsequently, a spectral modulation layer was formed by alternating deposition of transparent polymers with different refractive indices to create a double-layer refractive index gradient structure (alternating between the composite pastes prepared in Preparation Example 4 and Preparation Example 5). The refractive index difference between adjacent layers was controlled within the range of 0.02–0.20, and the thickness was controlled to approximately 5 μm. A flexible buffer interface layer of approximately 2 μm thickness (using the composite paste prepared in Preparation Example 4) was then spin-coated onto this layer. The device was then cured in a constant-temperature oven at 60°C for 1 hour to form a highly flexible, ultra-thin buffer interface layer structure. This gradient refractive index structure allows secondary photons generated by the radiative excitation layer to propagate directionally toward the photovoltaic layer.

[0076] (4) Construction of radiation-responsive quantum dot composite dielectric layer: The CsPbBr3 / PDMS radiation-responsive composite slurry (containing 5 wt% luminescent particles) prepared in Preparation Example 1 was coated onto a flexible buffer interface layer using a composite coating process, with the thickness of the response layer controlled to 10 μm. It was then thermocured again in a 60°C oven for 1 hour to form a radiation-responsive layer with downconversion function. The organic compatibility layer on the surface of the luminescent particles at the interface ensures stable dispersion between the particles and the polymer matrix through van der Waals forces and local hydrogen bonding.

[0077] (5) Integration of self-healing outer encapsulation layer: The self-healing polyurethane elastic film with dynamic disulfide bonds based on a molecular weight of 1000 PTMEG synthesized in Preparation Example 1 was used as a flexible barrier film and cut to a suitable size. At a temperature of 60°C, the self-healing film was hot-pressed onto the outer surface of the radiation response layer using a vacuum laminator, and the pressure was maintained at 0.1 MPa for 15 minutes to ensure that the encapsulation layer and the internal functional layer were tightly bonded without bubbles, forming an overall sealed structure.

[0078] (6) Finished product post-processing and testing: The encapsulated flexible energy cell was peripherally sealed, and positive and negative electrode wires were led out to obtain an ultrathin flexible radiation-photovoltaic synergistic energy cell with an overall thickness between 50-100 μm. Under standard radiation source irradiation, this cell utilizes the fluorescence down-conversion effect of the quantum dot layer and the photovoltaic effect of the CIGS layer to supply energy. Compared with the control sample without a spectral modulation structure, the device output stability is improved, and the secondary photon utilization efficiency is enhanced. Even with a reduced bending radius, the device maintains continuous conductivity, indicating that the flexible conductive network structure can effectively alleviate the problem of bending stress concentration.

[0079] Example 3: This embodiment provides a method for fabricating a flexible radiation-photovoltaic synergistic energy battery. The battery employs a rolled-up structure for long-term operation testing. Through a combination of a thick functional layer and high-concentration components, the energy harvesting capability and structural stability of the device under high-dose radiation conditions are verified. The method includes the following steps: (1) Preparation of flexible substrate and back electrode: A 125 μm thick polyimide (PI) film was selected as the flexible substrate. It was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 20 minutes each, rinsed with deionized water and dried at 100°C. Low-power oxygen plasma was used for surface activation treatment for 180 seconds to improve surface polarity and wettability. A 500 nm thick gold (Au) film was deposited on the PI film surface as the back electrode using magnetron sputtering technology.

[0080] (2) Integration of the photovoltaic conversion core layer and the transparent conductive electrode: CIGS (copper indium gallium selenide) thin-film solar cell modules were fabricated on the back electrode surface using a co-evaporation process. These modules comprise a CIGS absorber layer (3 μm), a CdS buffer layer (70 nm), and an i-ZnO layer (70 nm). Considering the high-temperature sensitivity of the flexible photovoltaic layer, the entire deposition process was controlled within the temperature tolerance range of the flexible substrate, followed by low-temperature annealing. A surface contact structure was adopted between the flexible transparent conductive electrode and the photovoltaic absorber layer. Using the target material from Preparation Example 3, a discontinuous rigid mesh interconnected flexible conductive path was formed by low-temperature sputtering. The resistance of the conductive layer was controlled at approximately 10 Ω / sq to reduce the risk of bending crack propagation.

[0081] (3) Construction of flexible buffer interface layer and spectral modulation layer: A planarization treatment was first applied to the surface of the photovoltaic module to reduce recombination loss. Then, a micro-nano scattering structure was constructed using the composite paste prepared in Example 6 to form a light propagation control interface with a thickness of about 15 μm. Subsequently, a flexible buffer interface layer with a thickness of about 10 μm (using the composite paste prepared in Example 5) was coated on it. The device was then placed in a constant temperature oven at 100°C for 4 hours to cure, forming a buffer interface layer structure that combines optical coupling and high thermal stability.

[0082] (4) Construction of radiation-responsive quantum dot composite dielectric layer: The high-load CsPbBr3 / PDMS radiation-responsive composite slurry (containing 40 wt% luminescent particles) prepared in Preparation Example 3 was coated onto a flexible buffer interface layer using a composite coating process, with the thickness of the responsive layer controlled at 50 μm. It was then thermocured in a 100°C oven for 4 hours to form a downconversion layer with extremely high interception and conversion efficiency against high-energy rays. The organic compatibility layer on the surface of the luminescent particles at the interface ensures stable dispersion between the particles and the polymer matrix through van der Waals forces and local hydrogen bonding.

[0083] (5) Integration of self-healing outer encapsulation layer: The self-healing polyurethane elastic film with a molecular weight of 2000 PTMEG and dynamic disulfide bonds synthesized in Preparation Example 3 was used as a flexible barrier film and cut to a suitable size. At a temperature of 100°C, the self-healing film was hot-pressed onto the outer surface of the radiation response layer using a vacuum laminator, and the pressure was maintained at 0.3 MPa for 45 minutes to ensure that the encapsulation layer and the internal functional layer were tightly bonded without bubbles, forming an overall sealed structure.

[0084] (6) Finished product post-processing and testing: The encapsulated flexible energy cell underwent peripheral sealing, and positive and negative electrode wires were led out to obtain a heavy-duty flexible radiation-photovoltaic co-coupled energy cell with an overall thickness controlled between approximately 250-350 μm. This cell exhibited excellent energy output under high-dose radiation source irradiation and excellent anti-peeling performance in high-intensity bending experiments. Continuous operation testing was conducted on the device in a wound state. No significant interlayer delamination occurred under repeated winding conditions, and no large-area crack propagation appeared in the transparent conductive layer. Compared to continuous rigid transparent conductive film structures, the flexible conductive network structure exhibits better stability under dynamic bending conditions. During long-term testing, no significant functional layer failure due to water and oxygen intrusion occurred in the encapsulation layer, indicating that the flexible encapsulation structure possesses excellent environmental barrier capabilities.

[0085] Comparative Examples 1-5: Comparative Example 1: Compared with Example 1, the difference is that the "radiation-responsive quantum dot composite dielectric layer" in step (4) is not set in this comparative example. That is, after the construction of the flexible buffer interface layer and the spectral control layer is completed, the self-healing outer encapsulation layer is directly integrated. The remaining steps, material ratios and process parameters are exactly the same as those in Example 1.

[0086] Comparative Example 2: Compared with Example 1, the difference is that in step (3), the spectral modulation layer does not use a double-layer refractive index gradient structure, but is formed by deposition of a homogeneous transparent polymer with a single refractive index. The remaining steps, material ratios and process parameters are exactly the same as in Example 2.

[0087] Comparative Example 3: Compared with Example 1, the difference is that in step (3), conventional rigid optical epoxy resin was used instead of the nano-silica modified PDMS composite slurry in Preparation Example 5, and the remaining steps, material ratios and process parameters were exactly the same as in Example 1.

[0088] Comparative Example 4: Compared with Example 1, the difference is that in step (5), a conventional industrial-grade encapsulation film without dynamic chemical bonds (such as standard PET or rigid epoxy encapsulation adhesive) was used instead of the self-healing polyurethane elastic film with dynamic disulfide bonds in Preparation Example 2. The remaining steps, material ratios and process parameters are exactly the same as in Example 1.

[0089] Comparative Example 5: Compared with Example 1, the difference is that in step (2), the flexible transparent conductive electrode does not use an interconnected flexible conductive path composed of a discontinuous rigid grid, but instead uses a traditional continuous rigid transparent conductive film (such as sputtered ITO film). The remaining steps, material ratios and process parameters are exactly the same as in Example 3.

[0090] Test Examples 1-4: Test Example 1: Comparative Test of Spectral Coupling Characteristics and Secondary Photon Utilization Efficiency of Radiation-Light-Electric Energy Gradient Conversion This experiment aims to verify the energy transfer efficiency between the radiatively responsive quantum dot layer and the photovoltaic core layer from a physical mechanism perspective. By analyzing the overlap of their spectra, the scientific validity of the down-conversion mechanism is evaluated. Furthermore, by comparing spectral modulation layers designed with different refractive indices, the effect of gradient refractive index structures on improving the efficiency of secondary photon directional propagation is verified. (See attached...) Figure 5 The schematic diagram of the cross-sectional view of the flexible rollable radiation-photovoltaic synergistic coupling energy battery structure shown illustrates the basic configuration of the device. The device consists of a flexible polyimide substrate, an interface buffer layer, a radiation excitation conversion layer, a spectral modulation layer, a hole transport layer, a photovoltaic absorption layer, an electron transport layer, a transparent conductive electrode layer, a barrier buffer layer, and a multifunctional encapsulation layer, which are stacked sequentially from bottom to top during actual service.

[0091] Experimental subjects were prepared as follows: the CsPbBr3 / PDMS radiation-responsive composite dielectric film (30 μm thick) prepared in Example 1 and a complete CIGS photovoltaic core layer module were selected. Meanwhile, device samples from Example 2 (using a double-layer refractive index gradient structure) and Comparative Example 2 (using a single refractive index homogeneous structure), which include complete structural encapsulation, were selected for comparative verification of secondary photon utilization efficiency and propagation path.

[0092] Fluorescence emission spectroscopy test: The radiation-responsive composite dielectric layer was placed under an X-ray excitation source with a set tube voltage of 40kV and a molybdenum target. The downconversion fluorescence generated by the dielectric layer after excitation was collected using a fiber optic spectrometer, and the emission intensity as a function of wavelength was recorded.

[0093] External quantum efficiency test: Using a monochromator in conjunction with a standard xenon lamp light source, the full-band spectral response of the CIGS photovoltaic core layer was tested to obtain its photoelectric conversion efficiency data in the range of 300nm to 1100nm.

[0094] Spectral normalization: The measured fluorescence intensity and external quantum efficiency response data are normalized, and the area of ​​overlap between the two in the wavelength dimension is calculated using relevant software.

[0095] Coupling efficiency evaluation: Based on the overlap integral area, assess the proportion of visible fluorescent photons converted from radiation energy that can be effectively captured by the photovoltaic layer. Furthermore, regarding the directional propagation efficiency of secondary photons: Under the same X-ray excitation source conditions, using a high-precision optical integrating sphere and a photodetector, quantitatively measure the effective forward visible photon flux reaching the photovoltaic absorption layer interface under different spectral modulation interfaces, as well as the proportion of transverse light loss caused by total internal reflection.

[0096] The table below records the measured values ​​of fluorescence emission intensity of the response layer and responsivity of the photovoltaic core layer in Example 1 at key wavelength nodes. Due to equipment noise and environmental interference, the data exhibit certain fluctuations.

[0097] Table 1. Measured Data of Spectral Coupling Characteristics

[0098] Figure 1 The solid line represents the normalized fluorescence intensity curve of the response layer in Example 1, and the dashed line represents the EQE response curve of the CIGS photovoltaic layer.

[0099] Conclusion: The test data and spectral coupling curves recorded in Table 1 intuitively reflect the physical feasibility of the step conversion mechanism. Experiments showed that the fluorescence peak generated by CsPbBr3 quantum dots under radiative excitation was located at 524.3 nm, which precisely falls within the high-sensitivity plateau region of the photoelectric response of the CIGS photovoltaic core layer (where EQE is stable above 79%). This precise alignment in the spectral dimension means that visible photons generated through downconversion can excite electron-hole pairs in the semiconductor depletion layer with a very high probability, effectively avoiding energy heat loss caused by direct bombardment of high-energy radiation particles.

[0100] In actual interlayer energy interaction, due to the gradient adjustment of the refractive index by the buffer interface layer, the overlap between the fluorescence emission spectrum and the EQE response spectrum reached the experimentally expected extreme value. Observation of the strongly coupled region from 518.9 nm to 548.1 nm reveals that the energy conversion process is not a simple linear addition, but rather based on maximizing the utilization of photon reabsorption efficiency. This design fundamentally solves the bottleneck problem in traditional radiation cells where semiconductor materials cannot directly capture short-wavelength high-energy particles. By converting the mismatched radiation energy level into a visible light signal recognizable by the photovoltaic layer, the system achieves a smooth transition from radiation response to carrier collection.

[0101] From the perspective of the material's inherent properties, the narrow full width at half maximum (FWHM) characteristic of the fluorescence spectrum further confirms the uniform dispersion of quantum dots in the composite medium. Since there is no significant self-absorption redshift or impurity quenching phenomenon, the energy transfer path loss is minimized. Combined with the sustained high response characteristics of CIGS in the long wavelength range, this application not only utilizes the green light band generated by downconversion but also provides experimental evidence for future expansion of multicolor quantum dot combinations to achieve full-spectrum energy capture. This directional coupling design based on spectral engineering is the core physical guarantee for achieving high-efficiency conversion in flexible batteries.

[0102] Further comparative analysis of the secondary photon propagation path reveals that the introduction of a gradient refractive index design significantly enhances the directional utilization of secondary photons, resulting in a substantial optical gain. Experimental data shows that in Example 2, the use of a double-layer refractive index gradient structure allows for a smooth transition from an optically denser to an optically less dense medium due to the refractive index difference between adjacent layers. This effectively reduces the optical mismatch at the interface, significantly suppressing lateral light loss caused by total internal reflection to only 8.15%, while achieving an effective forward transmittance of 89.34% at the photovoltaic interface. In contrast, Comparative Example 2 uses a single-refractive-index homogeneous transparent polymer deposition, resulting in a sudden refractive index difference at the interface. This leads to a loss of up to 24.62% of secondary visible photons due to the light-trapping effect of total internal reflection during lateral propagation, resulting in an effective forward transmittance of only 71.25%. Its overall secondary photon utilization efficiency is only 79.75% of that of Example 2. This comparative result directly verifies that the refractive index gradient design of this application can significantly reduce lateral light loss caused by total internal reflection at the interface, promoting highly directional propagation of down-conversion visible photons towards the photovoltaic layer and greatly improving the secondary photon utilization efficiency.

[0103] Test Example 2: Comparative Test of Photoelectric Output Characteristics under the Same Radiation Field Environment This experiment aims to quantitatively evaluate the energy conversion efficiency of different architecture designs under the same high-energy radiation field. The actual performance of the synergistic coupling mechanism in improving device output power is verified by measuring the current density-voltage characteristic curves. The ultimate outcome of this output power can be referenced... Figure 6The provided energy output and management block diagram shows that the energy battery of this application is connected to an optional energy storage unit at the circuit end, and provides stable power to external load systems such as sensors, communication modules or microcontrollers through a power management module.

[0104] Experimental sample preparation: Example 1 (standard design), Example 2 (ultra-thin low-load design), Comparative Example 1 (lacking quantum dot response layer) and Comparative Example 5 (pure photovoltaic cell without any radiation conversion mechanism) were selected as test objects. Before the test, the resistance of the flexible lead-out electrodes of all samples was checked to ensure that the contact resistance was consistent.

[0105] Radiation source calibration and environmental configuration: The experiment was conducted in a closed lead-shielded test chamber. A molybdenum target X-ray tube was selected, with the tube voltage adjusted to 50 kV and the tube current set to 200 μA. The radiation flux at the sample surface was measured using a standard dose monitor to ensure that the non-uniformity of the irradiation field in the test area was less than 2%.

[0106] Real-time acquisition of photoelectric properties: The sample is fixed on an insulating support and connected to a digital source meter via a low-noise coaxial cable. After the radiation source is turned on and stabilized for 5 minutes, the source meter is triggered to perform a voltage scan. The scan range is set to -0.1V to 0.6V, with a step size of 0.01V, and the sampling point integration time is set to 20ms.

[0107] Data repeatability verification: Five complete scans were performed for each sample type, and the response curves were recorded. The influence of X-ray source thermal drift on the experimental data was eliminated by calculating the average of multiple measurements.

[0108] Key parameter extraction: Short-circuit current density, open-circuit voltage, and maximum power output point are extracted from the measured curves for subsequent comparative analysis of performance among samples.

[0109] The table below shows the current response of each sample under 50 kV radiative excitation. Due to the random collision nature of high-energy particles, the measured current density exhibits minute physical fluctuations on the order of milliseconds.

[0110] Table 2. JV output characteristics of devices with different architectures under a 50kV radiated field.

[0111] Figure 2 The solid line represents Example 1, the long dashed line represents Example 2, the double-dotted line represents Example 3, the short dashed line represents Comparative Example 1, and the dotted-dotted line represents Comparative Example 5. The coordinate axes are labeled with standard fonts in the figure. An enlarged annotation box is located in the upper right corner to clearly identify the sample object corresponding to each line type, and the annotation box does not overlap with the data curves.

[0112] Conclusion: Analysis of the experimental data in Table 2 and Figure 2 The output characteristic curves clearly demonstrate the gain effect of the radiation response-photovoltaic coupling architecture on actual energy output. In a 50kV ray field, the short-circuit current density of Example 1 reached 17.84 μA / cm². 2 In Example 3, thanks to the thick functional layer and high concentration of components, the short-circuit current density soared to 32.45 μA / cm², compared to 0.42 μA / cm² in Comparative Example 5. 2 This represents a significant leap in scale, directly demonstrating the effectiveness of the link design. Because Comparative Example 5 relies solely on the photovoltaic layer's weak direct absorption of high-energy particles, its extremely small capture intercept results in substantial energy transmission loss. This scheme, through a response layer, effectively intercepts incident radiation energy and converts it into visible fluorescence, greatly expanding the device's bandwidth for utilizing X-ray energy.

[0113] To address the impact of changes in internal structural parameters, observations of the performance differences between Examples 1, 2, and 3 reveal a significant positive correlation between the quantum dot loading and the dielectric layer thickness on the output power. While Example 2 maintains its ultra-thin and flexible characteristics, its radiation capture capability is lower than that of Example 1. Example 3, however, exhibits extremely strong high-dose energy capture capability, indicating that the density gradient of the response layer is a key factor determining the upper limit of energy conversion. Furthermore, the extremely low current data in Comparative Example 1 eliminates the possibility of fluorescence generation in the encapsulation layer, confirming that the power output originates entirely from the spectral-oriented coupling between the quantum dot layer and the photovoltaic layer.

[0114] Further evaluation of the electrical transport state of the device showed that the curve of Example 1 maintained good linearity and fill characteristics near a 0.3V bias voltage, without significant increase in series resistance or drop in parallel resistance. This means that the flexible buffer interface layer successfully suppressed electrical losses caused by poor interlayer contact.

[0115] In a continuous 10-hour stability test under low-light / low-dose radiation, the embodiments of this application demonstrated excellent voltage maintenance capabilities. Monitoring data showed that under extremely low flux excitation, the load voltage of Embodiment 1 remained stable within a small fluctuation range of 0.28V ± 0.015V; Embodiment 3, due to its more efficient low-flux interception rate, maintained a stable voltage of 0.35V ± 0.01V; and the ultra-thin Embodiment 2 also maintained a stable voltage of 0.15V ± 0.01V for an extended period. This stable output voltage fully meets and satisfies the standby power supply threshold of ultra-low power microcontrollers or dormant sensors. In contrast, Comparative Examples 1 and 5, under low radiation flux, experienced a precipitous drop in the number of directly penetrating high-energy particles, with the carrier recombination rate far exceeding the generation rate. This caused the load voltage of both to drop below 0.02V within 10 minutes of the test start, accompanied by significant irregular level noise, resulting in a loss of effective power supply capability. The aforementioned testing confirms that the cooperative coupling architecture of this application can efficiently integrate weak background radiation energy in low-light environments, achieving trickle power supply through stable and continuous photoelectric conversion, thus providing a solid technical guarantee for the long-term independent operation of the microsystem. Combined with the aforementioned system management block diagram, this stable electrical output provides the core foundation for the efficient voltage regulation of the subsequent power management module and the continuous operation of the downstream micro-sensing system.

[0116] Test Example 3: Mechanical Reliability, Efficiency Retention, and Microstructure Testing under Cyclic Bending This experiment aims to verify the protective effect of nano-silica modified buffer layer on the structural integrity of flexible devices, evaluate the contribution of neutral layer displacement regulation mechanism to electrical performance stability by simulating frequent bending actions, and further evaluate the actual technical effect of flexible interconnect conductive network on suppressing stress concentration, preventing crack initiation and interface delamination by observing the micromorphology under dynamic bending (rolling) fatigue. Figure 7 The diagram shows the structure of the device in a curled state. When the device is curled with a large curvature, the stacked system consisting of the bottom flexible polyimide substrate, interface buffer layer, radiation excitation conversion layer, spectral modulation layer, flexible photovoltaic absorption layer, flexible transparent conductive electrode layer, top current collection structure and the top multifunctional encapsulation layer will face the severe test of interlayer shear stress.

[0117] Sample preparation and initial testing: Example 1 (containing a nano-silica modified buffer layer), Example 3 (using a flexible interconnect conductive network), Comparative Example 2 (direct bonding without a buffer layer), Comparative Example 3 (using a rigid epoxy resin interface), and Comparative Example 5 (using a traditional rigid continuous ITO conductive film) were selected as experimental samples. The initial output current of each sample was measured using an X-ray source in its unbent state and set as the baseline efficiency.

[0118] Bending parameter settings: Mount the sample on an automated flexible fatigue testing machine, set the bending radius to 10mm and the bending frequency to 1Hz, and ensure that the bending axis is perpendicular to the long axis of the device.

[0119] Cyclic loading process: Start the test machine and pause the mechanical movement when the number of cyclic bending reaches 500, 1000, 2000, 3000, 4000 and 5000 respectively.

[0120] Performance degradation measurement and morphology observation: At each set cycle node, the sample was flattened and placed back under the X-ray field to measure its output current value. Each sample was measured three times at each node to record accurate values. At the same time, in-situ optical microscopy and scanning electron microscopy (SEM) were used to observe the stress concentration area of ​​the device, focusing on recording whether there was large-area crack propagation in the transparent conductive layer and the delamination phenomenon between the interfaces of each functional layer.

[0121] Data normalization processing: Calculate the ratio of the measured efficiency to the initial baseline efficiency at each stage to obtain the efficiency retention curve.

[0122] The table below records the measured results of device efficiency retention as a function of bending cycles under different interface designs and conductive network structures. Due to the influence of test bench vibration and detector dark current, the data points exhibit nonlinear, slight fluctuations.

[0123] Table 3. Bending efficiency retention rate of samples with different interface layers and conductive layers at a radius of 10 mm.

[0124] Figure 3 Solid lines with dots represent Example 1, solid lines with hollow circles represent Example 3, dashed lines with squares represent Comparative Example 2, dashed lines with triangles represent Comparative Example 3, and dashed lines with rhombuses represent Comparative Example 5. The coordinate axes are labeled in standard font, and an enlarged annotation box in the upper right corner details the sample objects represented by each line type.

[0125] Conclusion: Interpreting the performance tracing data in Table 3 and Figure 3 The decay curves clearly show the degree to which the mechanical properties of the interface material affect the lifespan of the flexible multilayer device. Example 1, after undergoing 5000 severe bends with a 10mm radius, still maintained an energy conversion efficiency of over 91%, demonstrating extremely strong mechanical tolerance. This stability is attributed to the designed nano-silica modified buffer layer, which constructs a stable neutral layer network within the device by adjusting the elastic modulus. The buffer layer can absorb most of the shear stress generated during bending, keeping the fragile photovoltaic absorber layer in a low-strain region, thus preventing the initiation of microcracks. As shown in the service morphology diagram of the rolled structure, the functional multilayer maintains excellent interface adhesion even under significant bending.

[0126] In contrast, samples using non-flexible connection designs exhibited significant structural damage. Comparative Example 3, employing rigid epoxy resin, showed a marked drop in efficiency in the initial bending stages, with the retention rate rapidly decreasing to 18.36%. This failure stemmed from the mismatch between the extremely high modulus of the rigid material and the thin film, leading to high stress concentration at the interface, inducing penetrating cracks in the inorganic thin film and severing transport pathways. Comparative Example 2, although employing a partially flexible design, lacked a buffer layer with modulus transition properties, resulting in significant interlayer delamination due to adhesion failure at the interface after multiple bends. This physical disconnection prevented the fluorescence generated by the quantum dots from effectively coupling into the photovoltaic layer, causing the retention rate to drop to only 52.87% after 5000 cycles.

[0127] Further analysis using microscopic morphology observation data under dynamic bending (rolling) fatigue clearly demonstrates the decisive role of flexible interconnect conductive networks in improving the ultimate endurance of devices. Due to the lack of a stress release mechanism, Comparative Example 5, which uses a traditional rigid continuous ITO conductive film, exhibits large-area crack propagation in its transparent conductive layer after 2000 cycles; by 3000 cycles, the modulus mismatch between the rigid ITO film and the flexible absorption layer becomes extreme, directly inducing severe interlayer delamination at the functional layer interfaces, ultimately leading to a precipitous drop in efficiency to 8.42% after 5000 cycles. In contrast, Example 3, with its pre-designed flexible interconnect conductive network architecture, effectively transforms macroscopic bending stress into elastic deformation of microscopic network nodes. SEM morphology images confirm that after 5000 high-intensity rolls, the transparent conductive layer of Example 3 did not exhibit large-area crack propagation, nor did it experience any substantial interlayer delamination at the functional layer interfaces. The electrical transport network maintained a high degree of integrity, ultimately achieving an efficiency retention rate as high as 93.65%.

[0128] The data fluctuations recorded during the test indirectly confirm the evolution of internal stress accumulation and release. The gradual degradation observed in Examples 1 and 3 demonstrates that the stability of the microstructure was effectively maintained. Introducing a nanocomposite dielectric with stress relaxation capabilities and flexible interconnect electrodes not only solves the internal stress problem caused by differences in the thermal expansion coefficients between material layers, but more importantly, protects the brittle semiconductor core under dynamic loads. This mechanical buffering and conductive topology optimization scheme, starting from the neutral layer, provides a guarantee for the long-term operation of energy batteries in wearable devices or complex deformation spaces.

[0129] Test Example 4: Simulated Extreme Environmental Damage Repair, Radiation Stability, and Long-Term Water and Oxygen Barrier Aging Test This experiment designed a composite aging process that includes mechanical and physical damage, high humidity immersion, and long-term high-energy radiation bombardment, aiming to verify the repair mechanism of dynamic chemical bonds inside the surface encapsulation layer and explore its effect on extending the lifespan of the underlying core device under radiation and environmental water and oxygen erosion.

[0130] Example 1 and Comparative Example 4, which uses a conventional industrial-grade encapsulation film, were selected as test objects. The initial photoelectric conversion efficiency was tested under room temperature excitation and set as a reference.

[0131] Using a standard diamond indenter mounted on a precision scratch instrument, the same load was applied to the sample surface to create a network of cross-scratches with a depth of approximately 15 μm to simulate micro-mechanical scratch damage. The output efficiency was then recorded immediately.

[0132] Damaged samples were heat-treated on a vacuum heating stage at 80°C for 2 hours to activate the movement of polymer chains within the material. After treatment, the samples were slowly cooled to room temperature, and the photoelectric efficiency of the devices was retested to assess the level of recovery of physical integrity.

[0133] Samples that had undergone scratching and heat treatment cycles were transferred to a high-dose radiation chamber. The chamber environment was set to a high temperature of 85°C and a high humidity of 85%RH (double 85 aging standard), and the total irradiation time was set to 100 hours to simulate the continuous destructive effect of long-term high-intensity radiation on the material structure.

[0134] Samples were taken out every 20 hours during the operation of the irradiation chamber, and the conversion efficiency was rapidly measured under a standard radiation source to track the performance evolution trajectory during deep radiation aging and water and oxygen permeation.

[0135] The table below records the efficiency changes of the device over the full aging timeline. Minor fluctuations in contact resistance caused by measurements include actual test noise in the data points.

[0136] Table 4. Device efficiency evolution data under simulated extreme environments

[0137] Figure 4 The solid dot represents Example 1, which has self-healing capabilities, while the dashed square represents Comparative Example 4, which uses conventional packaging. The horizontal axis uses discrete stage nodes to mark the physical interventions and long-term radiation aging processes experienced by the device.

[0138] Conclusion: Based on the interim test results extracted in Table 4, the combined threat of environmental mechanical stress and deep radiation aging greatly shortens the service life of conventional devices. The self-healing elastic encapsulation layer designed in this scheme has shown excellent intervention ability in blocking this vicious failure chain.

[0139] In the initial stage of applying mechanical scratches, the efficiency of both Example 1 and Comparative Example 4 dropped by approximately 15% to 18%. This damage did not directly affect the underlying semiconductor; rather, the rough crack walls triggered a strong scattering effect at the optical interface, causing high-energy particles that should have been absorbed to be reflected, reducing the radiative flux trapped by the dielectric layer. After heat treatment at 80°C, the efficiency of Example 1 rapidly increased to 96.88%. Driven by heat, the polyurethane molecular chains achieved sufficient mobility, and the internal network re-crosslinked and fused, restoring optical transmittance. In contrast, the conventional polymer used in Comparative Example 4 underwent irreversible fracture after damage, permanently solidifying the light scattering effect.

[0140] The differences in surface defect morphology amplified their respective aging effects under subsequent high-dose radiation and high-humidity environments (85% and 85% humidity). Under continuous bombardment and high-temperature, high-humidity erosion for up to 100 hours, the efficiency of Example 1 gradually decreased and eventually stabilized at 87.65%. The self-healing layer not only closed physical cracks but also provided excellent long-term water and oxygen barrier properties; its dense repair network blocked the pathways for water and oxygen molecules from penetrating inwards. The abundant dynamic coordination bonds in the polyurethane network maintained the flexibility of the encapsulation and could absorb some of the free radiation energy through molecular chain conformational rearrangement, thereby delaying overall degradation and ensuring that the underlying photovoltaic absorption module did not suffer electrical failure due to moisture erosion.

[0141] Observing the long-term aging trajectory of Comparative Example 4, its performance exhibits an accelerated decline. Unhealed mechanical cracks become the entry point for radiation damage and the amplified penetration of water and oxygen over a large area. The continuous action of radiation causes severe cross-linking and hardening reactions in conventional packaging materials. This embrittlement, accompanied by a sharp increase in internal stress, further tears apart the original damaged area, causing an exponential increase in water vapor permeability (WVTR). High-energy particles and a large number of infiltrated water molecules undergo radiation hydrolysis deep within the cracks, generating a large number of active free radicals that directly attack the quantum dot layer, causing severe defects and fluorescence quenching. At the same time, water vapor directly leads to the oxidation of the underlying photovoltaic layer metal electrodes and the degradation of semiconductor materials, ultimately severing the optical and electrical power supply links, causing the device to be on the verge of complete failure. Based on this long-term water and oxygen barrier and environmental tolerance demonstrated in the dynamic game of destruction and repair, the protective potential of the novel packaging architecture under non-ideal operating conditions is verified.

Claims

1. A flexible radiation-photovoltaic synergistically coupled energy cell, characterized in that, It includes, from bottom to top, a flexible substrate, a back electrode, a photovoltaic conversion core layer, a transparent conductive electrode, a spectral modulation layer, a flexible buffer interface layer, a radiation-responsive quantum dot composite dielectric layer, and a self-healing outer encapsulation layer. The transparent conductive electrode is an interconnected flexible conductive path with a discontinuous rigid film structure. The spectral modulation layer has a gradient refractive index structure or a micro / nano scattering structure; The flexible buffer interface layer is used to connect the spectral modulation layer and the radiation-responsive quantum dot composite dielectric layer, and is used for spectral modulation and stress matching between the photovoltaic conversion core layer and the radiation-responsive quantum dot composite dielectric layer. The flexible buffer interface layer is made of components containing the following mass percentages: 5wt% to 30wt% surface-modified nano-silica particles, and 70wt% to 95wt% polydimethylsiloxane prepolymer. The radiation-responsive quantum dot composite dielectric layer is used to receive radiation from a radiation source and convert the radiation energy into downconversion fluorescence. The radiation-responsive quantum dot composite dielectric layer is made of components comprising the following mass percentages: 5 wt% to 40 wt% all-inorganic perovskite quantum dots and 60 wt% to 95 wt% polydimethylsiloxane prepolymer. The self-healing outer encapsulation layer is used to encapsulate the flexible radiation-photovoltaic synergistic energy battery, and the material of the self-healing outer encapsulation layer is a polyurethane elastic film containing dynamic disulfide bonds.

2. The flexible radiophotovoltaic co-coupled energy cell of claim 1, wherein, The photovoltaic conversion core layer is a copper indium gallium selenide (CIGS) thin-film solar cell module, and the photovoltaic conversion core layer comprises, from bottom to top: A CIGS absorber layer with a thickness of 1–3 μm, a CdS buffer layer with a thickness of 30–70 nm, and an i-ZnO layer with a thickness of 30–70 nm. The transparent conductive electrode and the photovoltaic conversion core layer adopt a surface contact structure, and the conductive layer resistance of the transparent conductive electrode is controlled to be 10-200Ω / sq.

3. The flexible radi-o-photovoltaic synergic coupling energy cell according to claim 1, wherein, The surface-modified nano-silica particles in the flexible buffer interface layer have an average particle size of 10-100 nm, and the surface of the surface-modified nano-silica particles is modified by coating with a silane coupling agent of 1%-10% by mass; the all-inorganic perovskite quantum dots in the radiation-responsive quantum dot composite medium layer are CsPbBr3 nanocrystals.

4. The flexible radi-o-photovoltaic co-coupled energy cell of claim 3, wherein, The polyurethane elastic film containing dynamic disulfide bonds is made by a polymerization reaction of substances comprising: Polytetrahydrofuran ether diol, isophorone diisocyanate, and 2-hydroxyethyl disulfide as a chain extender containing dynamic disulfide bonds, with a molecular weight of 1000-2000. The molar ratio of the polytetrahydrofuran ether diol to the isophorone diisocyanate is 1:2, and the molar ratio of the isocyanate-terminated polyurethane prepolymer obtained by reacting the polytetrahydrofuran ether diol with the isophorone diisocyanate to the 2-hydroxyethyl disulfide is 1:

1.

5. A method of constructing a flexible radiation-photovoltaic synergistically coupled energy cell as claimed in any one of claims 1 to 4, wherein, Includes the following steps: The flexible substrate is prepared and surface activated, and then a back electrode is deposited on the surface of the flexible substrate. The photovoltaic conversion core layer is prepared on the surface of the back electrode by a co-evaporation process. An interconnected flexible conductive path of a discontinuous rigid film structure is fabricated on the surface of the photovoltaic conversion core layer to form the transparent conductive electrode; The spectral modulation layer is constructed on the surface of the transparent conductive electrode; A flexible buffer interface layer composite slurry is coated on the surface of the spectral modulation layer and then thermo-cured to form the flexible buffer interface layer with spectral modulation and stress relief functions. A radiation-responsive composite medium slurry is coated on the flexible buffer interface layer and then thermo-cured to form the radiation-responsive quantum dot composite medium layer. On the outer surface of the radiation-responsive quantum dot composite dielectric layer, a pre-prepared polyurethane elastic film containing dynamic disulfide bonds is hot-pressed and encapsulated using a vacuum bonding process to form a self-healing outer encapsulation layer. The flexible radiation-photovoltaic co-coupled energy battery, after being heat-pressed and encapsulated, is then subjected to peripheral sealing treatment, and positive and negative electrode wires are led out to obtain the finished product.

6. The construction method according to claim 5, characterized in that, In preparing the flexible substrate and performing surface activation treatment, and in depositing the back electrode on the surface of the flexible substrate, the flexible substrate is pre-treated as follows: The flexible substrate was ultrasonically cleaned for 10-20 minutes using acetone, anhydrous ethanol and deionized water respectively, and then dried at 60-100°C. Subsequently, surface activation treatment was performed using low-power oxygen plasma for 30–180 seconds. The flexible substrate is made of polyimide film; The back electrode is formed by depositing a gold thin film with a thickness of 100-500 nm on the surface of the flexible substrate using magnetron sputtering technology.

7. The construction method according to claim 5, characterized in that, The preparation method of the flexible buffer interface layer composite slurry in forming the flexible buffer interface layer is as follows: The surface-modified nano-silica particles were mixed with polydimethylsiloxane prepolymer, and first stirred under high shear at 300-1500 rpm for 10-30 minutes, then ultrasonically assisted dispersion for 10-30 minutes, and finally degassed at room temperature under vacuum for 5-25 minutes. The radiation-responsive composite medium slurry in forming the radiation-responsive quantum dot composite medium layer is prepared as follows: The purified inorganic perovskite quantum dots were dispersed in toluene solvent to prepare a quantum dot dispersion, which was then mixed with the polydimethylsiloxane prepolymer. The mixture was continuously stirred under vacuum at 500-1500 rpm to completely evaporate and remove the toluene solvent, and degassing was continued for 10-30 minutes.

8. The construction method according to claim 5, characterized in that, The process of pre-preparing the polyurethane elastic film containing dynamic disulfide bonds includes: Polytetrahydrofuran ether diol was dehydrated under vacuum at 80–100°C for 1–2 hours, cooled, and isophorone diisocyanate was added under nitrogen protection. The reaction was carried out at 60–80°C for 2–4 hours. The 2-hydroxyethyl disulfide and dibutyltin dilaurate were added to the obtained substance, and the reaction was continued at 60-80°C for 4-8 hours to obtain a polymer viscous solution. The viscous polymer solution is poured into a mold and cured in a constant temperature oven at 60–80°C for 12–24 hours.

9. The construction method according to claim 5, characterized in that, In forming the spectral modulation layer, the thickness of the spectral modulation layer is controlled to be 5–15 μm; In forming the flexible buffer interface layer, the coating thickness of the flexible buffer interface layer is controlled to be 2-10 μm, the thermal curing temperature is 60-100℃, and the time is 1-4 hours. In forming the radiation-responsive quantum dot composite medium layer, the coating thickness of the radiation-responsive quantum dot composite medium layer is controlled to be 10-50 μm by a composite coating process, the temperature of thermal curing is 60-100℃, and the time is 1-4 hours.

10. The construction method according to claim 5, characterized in that, In forming the self-healing outer encapsulation layer, the hot-pressing encapsulation temperature of the vacuum bonding process is set to 60-100°C, the bonding pressure is maintained at 0.1-0.3 MPa, and the duration is 15-45 minutes to ensure a tight bond between the encapsulation layer and the internal functional layer.