A printing ink system for perovskite thin film cells, an inkjet printing method

By developing a printing ink system and an ultra-fine inkjet printing method for perovskite thin-film solar cells, the problems of resolution, solvent evaporation, and thermal sensitivity in perovskite solar cell fabrication using inkjet printing technology have been solved. This has enabled efficient and stable fabrication of 1μm-level patterning and spherical arrays, thereby improving the photoelectric conversion efficiency and industrialization potential of perovskite solar cells.

CN123124572APending Publication Date: 2026-11-17CHANGZHOU S C EXACT EQUIP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611305814.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing inkjet printing technology has problems in perovskite solar cell fabrication, including physical limitations in resolution, poor controllability of solvent evaporation and crystallization, high ink thermal sensitivity, and poor compatibility with all functional layers. It cannot achieve ultra-fine patterning at the 1μm level and continuous printing stability, thus failing to meet industrialization requirements.

Method used

A printing ink system for perovskite thin-film batteries is provided, comprising a hole transport layer, a perovskite light absorption layer, an electron transport layer, and a back electrode printing ink. The system achieves precise temperature control of droplets and solvent evaporation through synergistic regulation of a colloidal binder and a mixed solvent system, combined with a graphene infrared heater. An ultra-fine inkjet printing method is used to prepare 1μm-level patterns and spherical arrays.

Benefits of technology

It achieves an order-of-magnitude improvement in 1μm-level patterned printing resolution, a continuous printing yield of ≥99%, adjustable film properties, significantly improved process compatibility, applicability to various substrates, and has industrial application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124572A_ABST
    Figure CN123124572A_ABST
Patent Text Reader

Abstract

This invention discloses a printing ink system and inkjet printing method for perovskite thin-film batteries. The printing ink system includes inks for printing hole transport layers, perovskite light-absorbing layers, electron transport layers, back electrodes, and spherical arrays. All printing inks have a viscosity of 2-10 mPa·s and a surface tension of 25-35 mN / m at 25°C. Compared to existing technologies, this invention achieves an order-of-magnitude improvement in resolution, overcoming the physical limitations of nozzle orifice size; it also enables precise and controllable droplet formation, with droplet formation stability far superior to existing technologies; it significantly improves process compatibility, solving the problem that existing technologies cannot simultaneously meet two preparation requirements; the film properties are tunable over a wide range, satisfying application needs in different fields such as microelectronics, optoelectronics, and biosensing; it has significant advantages in engineering applications, enabling large-scale fabrication and possessing extremely high industrial application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solar cell fabrication technology, and in particular to an inkjet printing ink system for perovskite thin-film batteries and an ultra-fine inkjet printing method for perovskite thin-film batteries using the ink system. Background Technology

[0002] Perovskite thin-film solar cells possess significant advantages such as high photoelectric conversion efficiency, simple fabrication process, low raw material cost, and flexible fabrication capabilities, making them a core development direction for next-generation photovoltaic technology. Inkjet printing technology, as a non-contact, digital, maskless, large-area additive manufacturing technology, is one of the core fabrication processes for perovskite solar cells to move from the laboratory to industrialization. It enables large-area, patterned, and automated fabrication of various functional layers of perovskite solar cells, significantly reducing production costs.

[0003] However, existing inkjet printing technology faces four major insurmountable industry challenges in perovskite solar cell fabrication, and there are no targeted solutions: Printing resolution has a physical ceiling, resulting in significant area efficiency loss: Limited by the minimum stable mass production nozzle aperture and minimum stable jet droplet volume of existing commercial piezoelectric printheads, the linewidth after droplet deposition in traditional processes is generally ≥20μm, making it impossible to fabricate ultra-fine patterns at the 1μm level. In the fabrication of perovskite tandem solar cells and large-area modules, the linewidth of the interconnect pattern of sub-cells directly determines the proportion of dead area. The proportion of dead area in traditional inkjet printing is ≥5%, leading to a relative loss of more than 10% in the photoelectric conversion efficiency of large-area modules, failing to leverage the efficiency advantages of perovskite solar cells. Forcibly reducing the nozzle aperture to below 10μm will face engineering challenges such as a sharp increase in nozzle processing difficulty, easy clogging of perovskite ink, continuous printing yield ≤60%, and a drastic reduction in printhead lifespan, completely failing to meet mass production requirements.

[0004] The solvent evaporation and crystallization are extremely uncontrollable, resulting in numerous film defects: Perovskite precursor inks are extremely sensitive to the solvent evaporation rate. Existing technologies mostly use substrate heating or overall chamber heating, which makes solvent evaporation uncontrollable. This easily leads to uneven perovskite crystallization, numerous pinholes and grain boundary defects, and a significant coffee ring effect. This directly results in low open-circuit voltage, poor fill factor, and poor stability of the battery, which is the core bottleneck restricting the breakthrough of inkjet-printed perovskite battery efficiency.

[0005] Perovskite inks are highly thermally sensitive, and existing heating methods are incompatible with them: perovskite precursors are prone to decomposition and premature crystallization at high temperatures. Existing infrared-assisted inkjet technologies mostly use traditional infrared heating tubes to heat the substrate or chamber as a whole, which cannot accurately focus infrared radiation onto the millimeter-level droplet flight channel, and cannot achieve precise temperature control within the 0.1-0.4 ms microsecond flight time of a 4 pL droplet. Furthermore, the wavelength of traditional infrared heating tubes has a low matching degree with perovskite solvents, which can easily lead to premature crystallization of the precursor in the nozzle, causing nozzle blockage and a continuous printing yield of ≤80%, which cannot meet the needs of industrial continuous production.

[0006] Poor compatibility of all functional layers makes it impossible to achieve targeted performance optimization through adhesive-solvent control: The ink characteristics and photoelectric performance requirements of the hole transport layer, light absorption layer, electron transport layer, and back electrode layer of perovskite solar cells vary greatly. Existing technologies cannot achieve both in-flight droplet process adaptation and targeted performance optimization of each functional layer through the synergistic control of colloidal binders and solvents using the same set of equipment. This requires multiple sets of equipment and multiple processes, resulting in high production costs and poor process compatibility.

[0007] Furthermore, existing publicly available side-heated inkjet printing technologies are all designed for ordinary polymer and metallic inks, without considering the thermal sensitivity and crystallization control requirements of perovskite inks, without designing a matching heating system for the microsecond-level flight time of tiny droplets, and without establishing a coupled control system of adhesive-solvent-infrared heating, making them completely unsuitable for the fabrication requirements of perovskite thin-film batteries.

[0008] In summary, existing technologies cannot simultaneously solve the four core problems of achieving 1μm-level patterning with a 50μm diameter nozzle; precise temperature control of microdroplet flight time at the microsecond level; continuous printing stability of perovskite inks; and adapting the adhesive-solvent control to the performance of the entire film layer. There is an urgent need to develop a new ultra-fine inkjet printing technology solution that is fully adapted to the characteristics of perovskite batteries. Summary of the Invention

[0009] In view of the above-mentioned defects and shortcomings of existing inkjet printing technology in the preparation of perovskite solar cells, the purpose of this invention is to provide a printing ink system for perovskite thin-film solar cells and a printing method for preparing perovskite thin-film solar cells using the ink system.

[0010] To address the aforementioned problems, this invention provides a printing ink system for perovskite thin-film batteries, comprising hole transport layer printing ink, perovskite light absorption layer printing ink, electron transport layer printing ink, back electrode printing ink, and spherical array printing ink. All printing inks have a viscosity of 2-10 mPa・s at 25°C and a surface tension of 25-35 mN / m. They simultaneously meet the requirements for piezoelectric jet stability, in-flight infrared droplet technology, and the performance requirements of the corresponding functional layers in perovskite thin-film batteries. These requirements are synergistically controlled by the colloidal binder and mixed solvent system in the printing ink.

[0011] Preferably, the hole transport layer printing ink comprises the following raw materials formulated in a weight percentage: Hole transport functional material 0.5%-5%, mixed solvent system 90%-98%, colloidal binder 0.5%-3%, infrared absorber 0.05%-0.3%, surfactant 0.05%-0.5%; wherein: The hole transport functional material is any one of Spiro-OMeTAD, PTAA, PEDOT:PSS, or NiOx nanoparticles. The mixed solvent system is prepared by any two solvents of chlorobenzene, toluene, anhydrous ethanol or acetonitrile through a high-low boiling point solvent volume ratio of 95:5 to 80:20, thereby controlling the solvent evaporation rate. The colloidal binder is any one of polyvinylidene fluoride, acrylic resin, or ethyl cellulose, and is used to control the viscoelasticity of the ink, the adhesion of the film layer, and the cell migration rate.

[0012] Preferably, the perovskite light-absorbing layer printing ink comprises the following raw materials formulated in the following weight percentages: The composition includes: 10%-25% perovskite precursor, 70%-88% mixed solvent system, 0.5%-2% colloidal binder, 0.1%-1% crystallization regulator, 0.05%-0.2% infrared absorber, and 0.05%-0.3% surfactant, wherein: The perovskite precursor is at least one of formamidine cesium lead iodine, formamidine methylamine lead iodine, or all-inorganic cesium lead bromine; The mixed solvent system is a ternary system prepared by mixing DMF, DMSO and NMP in a volume ratio of 7:2:1 to 4:5:1. The infrared absorption efficiency and perovskite crystallization rate are controlled by the ratio of this mixed solvent system. The colloidal binder is either polyethylene oxide or polyvinylpyrrolidone, and is used to suppress precursor phase separation during flight, regulate grain growth, and reduce grain boundary defects.

[0013] Preferably, the electron transport layer printing ink comprises the following raw materials formulated in weight percentages: The composition includes: 1%-8% electron transport functional materials, 90%-97% mixed solvent system, 0.5%-2% colloidal binder, 0.05%-0.3% infrared absorber, and 0.05%-0.5% surfactant; among which: The electron transport functional material is any one of C60, PCBM, SnO2 nanoparticles, TiO2 nanoparticles, or ZnO nanoparticles. The mixed solvent system is any binary mixture of chlorobenzene, anhydrous ethanol, isopropanol or ethyl acetate; The colloidal binder is PMMA or acrylic resin, used to regulate the film density and interfacial contact characteristics, and reduce leakage current.

[0014] Preferably, the back electrode printing ink and the spherical array printing ink comprise the following raw materials formulated in weight percentages: Functional materials 5%-15%, mixed solvent system 80%-92%, colloidal binder 1%-5%, infrared absorber 0.1%-0.5%, surfactant 0.1%-0.5%; wherein: The functional material of the back electrode printing ink is any one of silver, copper, or gold nanoparticles with a particle size ≤30nm, used for fabricating 1μm-level sub-cell interconnect patterns; the mixed solvent system is a binary compound system of main solvent and co-solvent, the main solvent is any one of anhydrous ethanol, isopropanol, or acetone; the co-solvent is any one of ethylene glycol butyl ether, propylene glycol methyl ether, or diethylene glycol dimethyl ether, and the mass ratio of main solvent to co-solvent is 90:10~80:20; the colloidal binder is any one of acrylic resin, ethyl cellulose, or polyvinylpyrrolidone.

[0015] The functional material of the spherical array printing ink is PMMA or silica nanoparticles, used for the fabrication of perovskite solar cell photomanagement microsphere arrays. The mixed solvent system is divided into two categories based on the type of functional material, both using a combination of high and low boiling point solvents. For the PMMA microsphere system, the mixed solvent system is any binary mixed solvent from chlorobenzene, toluene, ethyl acetate, or isopropanol, with the high-boiling-point component accounting for 10%–25%. For the silica microsphere system, the mixed solvent system is any binary mixed solvent from anhydrous ethanol, ethylene glycol, deionized water, or isopropanol, with the high-boiling-point component accounting for 5%–15%. The colloidal binder is matched according to the selected functional material. For the PMMA microsphere system, the colloidal binder uses PMMA itself as the main sphere-forming component and the binding component, compounded with polyethylene glycol as an auxiliary binder. For the silica microsphere system, the colloidal binder uses silica sol and tetraethyl orthosilicate hydrolyzed prepolymer as binders, undergoing a condensation reaction during microsphere curing to improve the mechanical strength of the microspheres and the adhesion to the substrate.

[0016] This invention also provides an ultra-fine inkjet printing method for perovskite thin-film batteries, comprising a three-part printing process. The first part of the printing process involves printing the target functional layer of the perovskite thin-film battery on the surface of a conductive substrate, including the following steps: S1 Pre-printing preparation: Fix the conductive substrate onto the ultra-fine inkjet printing equipment, inject the printing ink system of each functional layer of the perovskite thin film battery provided by the present invention into the printing equipment, and adjust the printing equipment. S2 heating system preset: Start the printer heating, set the target heating temperature, and control the nozzle temperature to be stable at 25-30℃; S3 Injection Parameter Calibration: Edit the multi-segment bipolar pulse drive waveform, set the drive amplitude, pulse width, and injection frequency, observe the droplet injection status in real time, optimize the drive waveform, and achieve stable single droplet injection without satellite droplets or tails. The 4pL droplet injection speed is controlled at 8-15m / s, and the flight time is 0.1-0.4ms. S4 Controllable Droplet Printing: Select the corresponding printing ink and printing mode, and start the three-axis motion platform and printhead of the device to print synchronously on the conductive substrate; S5 Post-processing annealing: The conductive substrate with the printed target functional layer is subjected to programmed temperature annealing to complete film crystallization, solvent removal and performance optimization, and obtain the target functional layer of the perovskite solar cell.

[0017] Preferably, when the uniform film printing mode is selected, the heater temperature of the printing equipment is controlled at 80-120℃ and the heater power density is 3-10W / cm², so that the solvent evaporation rate of the droplets reaches 60%-80% during the flight process, the particle size shrinks to 5-10μm and completes semi-curing. After the semi-cured droplets are deposited, they spread and overlap evenly to form a dense film without pinholes or coffee rings.

[0018] The second part of the printing process involves printing a back electrode on the surface of a perovskite thin-film battery with the target functional layer. The steps are as follows: 1) Setting up the printing device: Set the parameters for printing the back electrode, adjust the printing equipment, and prepare to print the back electrode; 2) Printing of the back electrode S1 Printing Preparation: Fix the perovskite thin-film battery with the target functional layer onto the ultra-fine inkjet printing equipment and adjust the printing equipment; S2 heating system preset: Start the printer heating, set the heating temperature, and control the nozzle temperature to be stable at 28℃; S3 jet parameter calibration: Edit the three-segment bipolar pulse drive waveform, set the drive amplitude, pulse width, and jet frequency, observe the droplet jet status in real time, optimize the drive waveform, and achieve stable jetting of a single droplet without satellite droplets or tails. The jetting speed of a 4pL droplet is controlled at 10m / s, and the flight time is 0.15ms. S4 Ultra-fine graphic printing: Select the ultra-fine graphic printing ink and printing mode, start the three-axis motion platform and printhead of the device to synchronously print the back electrode of the perovskite thin film battery with the target functional layer. S5 Post-processing: After the back electrode is printed, the sample is placed in a forced-air oven and sintered at 150°C for 30 minutes to remove residual solvent and obtain a perovskite thin-film battery with a printed back electrode. 3) The performance of the perovskite thin-film battery with the printed back electrode was tested. SEM and profilometer tests showed that the average line width of the printed conductive lines was 1.02 μm, the line width uniformity CV ≤ 4.0%, the edge roughness ≤ 0.2 μm, and there were no coffee ring effect or broken pen defects.

[0019] Preferably, the power density of the heater in the printing equipment is controlled to be 2-12W / cm², so that the solvent evaporation rate of 2-4pL droplets reaches 80%-95% during flight, the particle size shrinks from the initial 20-50μm to 2-5μm and completes gelation and pre-curing. After the pre-cured droplets are deposited on the substrate, they have no flowability, the spreading coefficient is ≤1.2, and the curing forms an ultra-fine pattern at the 1±0.2μm level.

[0020] The third part of the printing process involves printing a spherical array on the surface of a perovskite thin-film battery with a back electrode. The steps are as follows: 1) Setting up the printing device: Set the parameters for printing the spherical array, adjust the printing equipment, and prepare to print the spherical array; 2) Printing of spherical arrays S1 Printing Preparation: Fix the perovskite thin-film battery with the back electrode onto the ultra-fine inkjet printing equipment and adjust the printing equipment; S2 heating system preset: Start the printer heating, set the heating temperature, and control the nozzle temperature to be stable at 28℃; S3 Injection Parameter Calibration: Edit the two-segment bipolar pulse drive waveform, set the drive amplitude, pulse width, and jet frequency, observe the droplet jet state in real time, optimize the drive waveform, and achieve stable jetting of a single droplet without satellite droplets or tails. The jetting speed of a 4pL droplet is controlled at 8~12m / s, and the flight time is 0.2ms. S4 Printed Spherical Array: Select the printing ink and printing mode for the spherical array, and start the three-axis motion platform and printhead of the device to simultaneously print the spherical array for the perovskite thin film battery with the back electrode. S5 Post-processing: After the spherical array is printed, the sample is placed in a vacuum oven and annealed at 80°C for 20 minutes to remove trace amounts of residual solvent inside the microspheres and strengthen the interfacial bonding force between the microspheres and the back electrode layer, thus completing the preparation of the light-management spherical microsphere array. 3) Performance testing of perovskite thin-film solar cells with printed spherical arrays. SEM and step profile tests showed that the microsphere array prepared by PMMA microsphere array had a controllable particle size of 2-5μm, a particle size uniformity CV≤2.5%, a sphericity ≥95%, an array position accuracy of ±0.8μm, and no deformation or adhesion defects.

[0021] Preferably, the power density of the heater in the printing equipment is controlled to be 12-20W / cm², so that the solvent evaporation rate of the droplets reaches 100% during flight, and the solid microspheres are formed after complete curing. After deposition on the substrate, they are not deformed or spread, forming a high-precision spherical array with a controllable particle size of 1-10μm.

[0022] Compared with the prior art, the present invention has the following significant advantages: 1. Breakthrough in resolution: Using a 50μm orifice nozzle (4pL initial droplet), it can stably achieve a feature linewidth / dot diameter of 1±0.2μm, which is more than an order of magnitude higher than traditional inkjet printing, breaking through the physical limitations of nozzle orifice size; no ultra-small nozzle is required, there is no risk of nozzle clogging during the printing process, and the yield of printing 10,000 droplets continuously is ≥99%, which greatly improves the long-term stability and service life of inkjet printing.

[0023] 2. Precise and controllable droplet shrinkage process: The 8-14μm far-infrared radiation of the graphene infrared heater matches the infrared absorption peak of the organic solvent by ≥90%, the heating uniformity of the droplet bulk phase is ≥95%, the heating response rate is ≥50℃ / s, and the temperature control accuracy is ±1℃. It can achieve continuous and precise control of solvent evaporation rate of 80%-100% within the droplet flight time of 0.1-0.4ms, and the droplet size shrinkage rate can reach up to 95%. There are no defects such as droplet breakage, satellite droplets, or trajectory deviation. The stability of the droplet shrinkage process is far superior to that of existing technologies.

[0024] 3. Significantly improved process compatibility: The same device can seamlessly switch between two core functional modes by simply changing the formula and process parameters: ① Ultra-fine pattern printing mode, which can prepare high-precision patterns with linewidth of 1μm, edge roughness ≤0.2μm, no coffee ring effect, and linewidth uniformity CV≤5%; ② Spherical array preparation mode, which can prepare microsphere arrays with continuously adjustable particle size of 1-10μm, sphericity ≥95%, and positional accuracy ±1μm, with particle size uniformity CV≤3%, solving the problem that existing technologies cannot meet the two preparation requirements at the same time.

[0025] 4. Wide range of adjustable film properties: Through targeted optimization of ink formulation and control of post-processing, the properties of the printed film can be precisely controlled over a wide range: the resistivity of the conductive system can reach 10⁻ 6 -10⁻ 4 Ω・cm, dielectric constant of insulating system adjustable from 3.0 to 10.0, optical thin film transmittance up to ≥90%, can meet the application needs of different fields such as microelectronics, optoelectronics, and biosensing.

[0026] 5. Significant advantages in engineering applications: The device of this invention has a simple structure and can be upgraded and modified to be compatible with existing commercial inkjet printing equipment. It does not require a complex high-voltage electric field or vacuum system, and the equipment modification cost is low. It has a wide process window and can achieve stable printing at room temperature and pressure. It is compatible with a variety of substrates such as glass, silicon wafers, PI, PET, and ceramics. The process flow is short, without masks or subsequent etching processes. It is green and environmentally friendly and can achieve large-scale preparation, which has extremely high industrial application value. Attached Figure Description

[0027] Figure 1 This is a schematic diagram of the perovskite thin-film battery fabricated by inkjet printing according to the present invention. Detailed Implementation

[0028] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0029] The printing ink system for perovskite thin-film batteries provided by this invention includes printing ink for hole transport layers, perovskite light absorption layers, electron transport layers, back electrodes, and spherical arrays. All printing inks have a viscosity of 2-10 mPa·s and a surface tension of 25-35 mN / m at 25°C, simultaneously meeting the requirements for piezoelectric jet stability, in-flight infrared droplet formation, and the performance requirements of the corresponding functional layers in the perovskite thin-film battery. Through synergistic regulation of the colloidal binder and mixed solvent system in the printing inks, it is possible to: match the solvent evaporation and droplet formation requirements of 2-4 pL droplets within a flight time of hundreds of microseconds; suppress perovskite precursor precipitation, phase separation, and nozzle clogging during flight; and directionally optimize the photoelectric performance, crystal quality, and interfacial contact characteristics of the corresponding functional layers. The printing ink formulations for each functional layer are as follows: 1. The hole transport layer printing ink comprises the following raw materials prepared in weight percentages: Hole transport functional material 0.5%-5%, mixed solvent system 90%-98%, colloidal binder 0.5%-3%, infrared absorber 0.05%-0.3%, surfactant 0.05%-0.5%; wherein: The hole transport functional material is any one of Spiro-OMeTAD, PTAA, PEDOT:PSS, or NiOx nanoparticles; the mixed solvent system is any binary solvent of chlorobenzene, toluene, anhydrous ethanol, or acetonitrile, prepared by a high-low boiling point solvent volume ratio of 95:5 to 80:20 to control the solvent evaporation rate; the colloidal binder is any one of polyvinylidene fluoride, acrylic resin, or ethyl cellulose, used to control the ink viscoelasticity, film adhesion, and hole mobility; the infrared absorber is any one of phthalocyanine infrared dyes, ATO nanoparticles, or nanographene; the surfactant is any one of organosilicon surfactants, sodium dodecylbenzenesulfonate, or fluorocarbon nonionic surfactants.

[0030] 2. The perovskite light-absorbing layer printing ink comprises the following raw materials formulated in the following weight percentages: The composition includes: 10%-25% perovskite precursor, 70%-88% mixed solvent system, 0.5%-2% colloidal binder, 0.1%-1% crystallization regulator, 0.05%-0.2% infrared absorber, and 0.05%-0.3% surfactant, wherein: The perovskite precursor is at least one of formamidine cesium lead iodine, formamidine methylamine lead iodine, or all-inorganic cesium lead bromine; the mixed solvent system is DMF, DMSO, and NMP in a volume ratio of 7:2:1 to 4:5:1. The prepared ternary system controls the infrared absorption efficiency and perovskite crystallization rate through the ratio of the mixed solvent system; the colloidal binder is any one of polyethylene oxide and polyvinylpyrrolidone, used to suppress precursor phase separation during flight, regulate grain growth, and reduce grain boundary defects; the crystallization regulator is any one of polyethylene oxide (PEO), polyvinylpyrrolidone (PVP), lead chloride (PbCl2), cesium bromide (CsBr), and methylammonium chloride (MACl), which can passivate grain boundary defects, suppress precursor phase separation during flight, and optimize crystallization kinetics by regulating the crystal phase structure and band gap through halogen components; the infrared absorber is any one of phthalocyanine infrared dyes and nano-graphene; the surfactant is any one of polyether-modified siloxanes and fluorocarbon nonionic surfactants.

[0031] 3. The electron transport layer printing ink comprises the following raw materials formulated in the following weight percentages: The composition includes: 1%-8% electron transport functional materials, 90%-97% mixed solvent system, 0.5%-2% colloidal binder, 0.05%-0.3% infrared absorber, and 0.05%-0.5% surfactant; among which: The electron transport functional material is any one of C60, PCBM, SnO2 nanoparticles, TiO2 nanoparticles, or ZnO nanoparticles; the mixed solvent system is any binary mixture system of chlorobenzene, anhydrous ethanol, isopropanol, or ethyl acetate; the colloidal binder is PMMA or acrylic resin, used to regulate the film density and interfacial contact characteristics, and reduce leakage current; the infrared absorber is any one of phthalocyanine infrared dyes, indium tin oxide nanoparticles, or nanographene; the surfactant is any one of hexadecyltrimethylammonium bromide or fluorocarbon nonionic surfactants.

[0032] 4. The back electrode printing ink and the spherical array printing ink comprise the following raw materials formulated in percentage by mass: Functional materials 5%-15%, mixed solvent system 80%-92%, colloidal binder 1%-5%, infrared absorber 0.1%-0.5%, surfactant 0.1%-0.5%; wherein: The functional material of the back electrode printing ink is any one of silver, copper, or gold nanoparticles with a particle size ≤30nm, used for fabricating 1μm-level sub-cell interconnect patterns; the mixed solvent system adopts a binary compound system of "low-boiling-point main solvent + medium-high-boiling-point co-solvent". The main solvent is selected from any one of anhydrous ethanol, isopropanol, and acetone, possessing low boiling point and high volatility, supporting the rapid evaporation and droplet shrinkage of droplets within a flight time of hundreds of microseconds; the co-solvent is selected from any one of ethylene glycol butyl ether, propylene glycol methyl ether, and diethylene glycol dimethyl ether, slowing down the solvent evaporation rate at the nozzle orifice and inhibiting ink drying and clogging. The mass ratio of the main solvent to the co-solvent is 90:10~80:20, which can be flexibly adjusted according to the temperature and humidity of the printing environment. The colloidal binder is selected from any one of acrylic resin, ethyl cellulose, and polyvinylpyrrolidone. On the one hand, it controls the viscoelasticity of the ink to match the droplet gelation and pre-curing process during flight. On the other hand, it improves the adhesion between the metal conductive layer and the substrate after sintering, while inhibiting the aggregation of metal nanoparticles during flight and ensuring the uniformity of the graphic line width. The infrared absorber is one of graphene nanosheets or carbon nanotubes. The surfactant is preferably a fluorocarbon nonionic type, with polyether-modified siloxane as an alternative. The core selection considers both infrared response efficiency and low residue and high conductivity after sintering.

[0033] The functional material of the spherical array printing ink is PMMA or silica nanoparticles, used for the fabrication of perovskite solar cell photomanagement microsphere arrays. The mixed solvent system is divided into two types based on the functional material, both using a combination of high and low boiling point solvents: PMMA microsphere system: using a binary mixed solvent of chlorobenzene + toluene and ethyl acetate + isopropanol, with the high-boiling point component accounting for 10%~25%. The main solvent is used to dissolve the PMMA polymer, and the co-solvent is used to control the evaporation rate and prevent droplet deformation after deposition. Silica microsphere system: using a binary mixed solvent of anhydrous ethanol + ethylene glycol and deionized water + isopropanol, with the high-boiling point component accounting for 5%~15%, ensuring uniform dispersion of silica nanoparticles while meeting the evaporation rate requirements for full-fledged curing. The colloidal binder is selected and matched according to the functional material: PMMA microsphere system: using PMMA itself as the main sphere-forming component and binder, with a small amount of polyethylene glycol (PEG) can be added. 2000) is used as an auxiliary binder to enhance the interfacial bonding between microspheres and the substrate, while also regulating the viscoelasticity of the ink to ensure stable spherical morphology during the curing process. For the silica microsphere system, silica sol and tetraethyl orthosilicate (TEOS) hydrolyzed prepolymer are used as binders, which can undergo a condensation reaction during microsphere curing, improving the mechanical strength of the microspheres and the adhesion to the substrate. The spherical array printing ink is selected based on the functional material system. For the PMMA system, cyanine-based near-infrared dyes are preferred as infrared absorbers, and fluorocarbon nonionic surfactants are preferred. For the silica system, antimony-doped tin dioxide (ATO) nanoparticles are preferred as infrared absorbers, and polyether-modified siloxanes are preferred as surfactants, prioritizing the sphericity of the microspheres and visible light transmittance.

[0034] Please combine Figure 1 The embodiment of the ultra-fine inkjet printing method for perovskite thin-film batteries provided by this invention involves the fabrication of the battery in three main process parts. The first part, the printing process, is the fabrication of the target functional layer of the perovskite thin-film battery, and includes the following steps: S1 Pre-printing preparation: Fix the ITO / FTO conductive substrate onto the precision substrate stage of the printing equipment, and complete cleaning and surface pretreatment; inject the prepared target functional layer ink (the printing ink system provided by this invention) into the constant temperature ink supply system of the equipment, and set the ink constant temperature parameters after vacuum degassing; seal the printing chamber of the equipment, introduce nitrogen gas to replace it until the water and oxygen content is ≤1ppm, and set the chamber temperature and humidity parameters; calibrate the relative position of the three-axis motion platform of the equipment and the printhead, and set the distance between the nozzle of the equipment and the conductive substrate to 1-3mm.

[0035] S2 Heating System Pre-adjustment: Activate the graphene infrared heating module in the printing equipment. Based on the characteristics of the target functional layer ink, set the target temperature of the graphene infrared heater to 60-200℃ through the temperature control unit of the equipment. Monitor the temperature field of the heating area in real time through the infrared thermal imager. After the temperature stabilizes, activate the end water cooling heat dissipation unit of the printhead to stabilize the nozzle temperature at 25-30℃.

[0036] S3 Ejection Parameter Calibration: Edit the multi-segment bipolar pulse drive waveform of the printing equipment, set the drive amplitude to 20-40V, pulse width to 5-20μs, and ejection frequency to 1-30kHz. Observe the droplet ejection status in real time through the droplet observer, optimize the drive waveform, and achieve stable single-droplet ejection without satellite droplets or tails. The 4pL droplet ejection speed is controlled at 8-15m / s, and the flight time is 0.1-0.4ms.

[0037] S4 Controlled Droplet Printing: Based on the requirements of perovskite thin-film battery fabrication, select the corresponding functional layer printing ink and printing mode, and start the three-axis motion platform and printhead for synchronous printing. The uniform film printing mode is selected to prepare large-area functional layers for perovskite solar cells. The power density of the graphene infrared heater is controlled to be 3-10 W / cm², so that the solvent evaporation rate of the droplets reaches 60%-80% during flight, the particle size shrinks to 5-10 μm and completes semi-curing. After the semi-cured droplets are deposited, they spread and overlap evenly to form a dense film without pinholes or coffee rings. When using uniform film printing to prepare perovskite light-absorbing layers, it is preferable to control the heater temperature at 80-120℃, the power density at 5-8W / cm², and the solvent evaporation rate during droplet flight at 70%-75%. After deposition, the perovskite film is annealed by programmed temperature rise, resulting in a grain size ≥1μm and a defect state density ≤1×10¹. 5 cm⁻³.

[0038] like Figure 1 As shown, inkjet printing is performed sequentially from bottom to top on the upper surface of the ITO conductive glass substrate, consisting of an electron transport functional layer, a perovskite light absorption functional layer, a hole transport functional layer, and a back electrode functional layer.

[0039] S5 Post-processing annealing: After printing, the substrate is subjected to programmed temperature annealing according to the characteristics of the target functional layer to complete film crystallization, solvent removal and performance optimization, and obtain the target functional layer of the perovskite thin film battery.

[0040] The second part of the printing process involves printing the back electrode on the surface of a perovskite thin-film battery with the target functional layer, specifically ultra-fine inkjet printing of 1μm-level metallic conductive interconnect patterns. The steps are as follows: 1. Setting up the printing device An ultra-fine inkjet printer is used, with the following parameters set: Piezoelectric inkjet printhead: Adopts industrial-grade DOD piezoelectric printhead with a nozzle orifice diameter of 50μm, a minimum stable droplet volume of 4pL, and a driving frequency of 1-10kHz. Graphene infrared heating module: Two sets of CVD single-layer graphene infrared heaters with a surface resistivity of 150Ω / sq, rated power density of 5-15W / cm², radiation wavelength of 8-14μm, and intelligent temperature control accuracy of ±1℃. They are symmetrically arranged on both sides of the droplet flight channel, and the heating area covers the entire flight path of 1.5mm. A water-cooled heat dissipation unit is set at the nozzle end to control the nozzle temperature to be stable at 28±1℃. Three-axis motion platform: X / Y axis positioning accuracy ±0.5μm, repeatability ±0.2μm, Z axis adjustment accuracy 1μm; Sealed printing chamber: chamber temperature controlled at 25℃, relative humidity at 20%, nitrogen atmosphere; Online monitoring module for flight process: Ink droplet observer, which collects the flight status of droplets in real time.

[0041] 2. Special ink formulation for ultra-fine graphic printing The ink formulation, by mass percentage, is as follows: 2% 20nm silver nanoparticles, 88% anhydrous ethanol (main solvent), 8% ethylene glycol butyl ether (co-solvent), 1.5% acrylic resin (binder), 0.3% nano-graphene (infrared absorber), and 0.2% fluorocarbon nonionic surfactant. After mixing the above components, the mixture was ultrasonically dispersed for 30 min and vacuum degassed for 15 min to obtain the target ink. Testing showed that the ink had a viscosity of 3.2 mPa·s and a surface tension of 29.5 mN / m at 25°C, meeting the requirements for stable ejection by the piezoelectric printhead.

[0042] 3. Printing process S1 Printing Preparation: Fix a 100μm thick PI flexible substrate onto a precision substrate stage, perform fluorine-modified hydrophobic pretreatment on the substrate to make the static contact angle of the silver ink on the substrate surface 90°~95°; inject the prepared ink into the constant temperature ink supply system and set the ink temperature to 25℃; set the nozzle-substrate distance to 1.5mm and calibrate the relative position of the three-axis motion platform and the printhead. S2 heating system pre-adjustment: Activate the graphene infrared heating module and set the segmented gradient heating parameters: inlet section temperature 100℃, middle section temperature 180℃, outlet section temperature 90℃. After the temperature field is stabilized by monitoring with an infrared thermal imager, activate the nozzle end water cooling heat dissipation unit to maintain the nozzle temperature at 28℃. S3 injection parameter calibration: Edit the three-segment bipolar pulse drive waveform, drive amplitude 30V, main pulse width 10μs, injection frequency 5kHz, observe the droplet injection state through a high-speed camera, and optimize the waveform to achieve stable injection without satellite droplets or trailing, with droplet injection velocity of 10m / s and droplet flight time of about 0.15ms; S4 Ultra-Fine Graphic Printing: The three-axis motion platform and printhead are synchronized during printing. The heater power density is controlled at 10W / cm². Real-time monitoring is conducted using a high-speed camera. During the droplet flight, the solvent evaporation rate reaches 90%, and the droplets with an initial particle size of 19.7μm shrink to 3.2μm, completing the gelation and pre-curing process. After the pre-cured droplets are deposited on the PI substrate, the spreading factor is 1.15, with no flowability and no spreading. When printing continuous lines, the overlap rate between adjacent droplets is controlled at 12%~15%. The target pattern printed is a conductive interconnect line and array of dots with a line width of 1μm. In the ultra-fine pattern printing mode, it is used to prepare interconnect patterns and patterned functional layers for perovskite solar cells. The power density of the graphene infrared heater is controlled at 2-12W / cm², so that the solvent evaporation rate of 2-4pL droplets reaches 80%-95% during flight, and the particle size shrinks from the initial 20-50μm to 2-5μm and completes gelation and pre-curing. After the pre-cured droplets are deposited on the substrate, they have no flowability and a spreading coefficient ≤1.2. Finally, they are cured to form ultra-fine patterns at the 1±0.2μm level.

[0043] The ultra-fine pattern printing mode is used for interconnecting sub-cells of perovskite tandem solar cells. A segmented gradient heating process is adopted: the inlet section of the droplet flight channel is heated at 60-100℃, the middle section at 120-180℃, and the outlet section at 60-90℃; the linewidth of the prepared interconnect pattern is 1±0.2μm.

[0044] S5 Post-processing: After printing, the sample is placed in a forced-air oven and sintered at 150℃ for 30 minutes to remove residual solvent and improve the density and conductivity of silver nanoparticles.

[0045] 4. Performance Test Results SEM and profilometer tests showed that the average line width of the printed conductive lines was 1.02 μm, the line width uniformity CV ≤ 4.0%, the edge roughness ≤ 0.2 μm, and there were no coffee ring effect or broken pen defects.

[0046] The third part of the printing process involves in-situ printing an array of light management microspheres on the surface of the battery after the back electrode functional layer has been fabricated, thereby improving the battery's light capture efficiency. The steps are as follows: 1. Setting up the printing device Utilizing the core configuration of an ultra-fine inkjet printer, parameters have been optimized for spherical array printing requirements: Piezoelectric inkjet printhead: Adopts industrial-grade DOD piezoelectric printhead with a nozzle orifice diameter of 50μm, a minimum stable droplet volume of 4pL, and a driving frequency of 1-20kHz; Graphene infrared heating module: Two sets of CVD single-layer graphene infrared heaters, with a surface resistivity of 150Ω / sq, rated power density of 12-20W / cm², radiation wavelength of 8-14μm, and intelligent temperature control accuracy of ±1℃. They are symmetrically arranged on both sides of the droplet flight channel, and the heating area covers the entire flight path of 1.5mm. A water-cooled heat dissipation unit is set at the nozzle end to control the nozzle temperature to be stable at 28±1℃. Three-axis motion platform: X / Y axis positioning accuracy ±0.5μm, repeatability ±0.2μm, Z axis adjustment accuracy 1μm; Sealed printing chamber: chamber temperature controlled at 25℃, relative humidity ≤20%, nitrogen atmosphere; Online monitoring module for flight process: Ink droplet observer, which collects the flight status of droplets in real time.

[0047] 2. Formulation of special ink for spherical array printing Taking PMMA light-management microsphere ink as an example, the ink formulation by mass percentage is as follows: 10% PMMA polymer powder (molecular weight 15000), 85% chlorobenzene (main solvent), 3% toluene (co-solvent), 1.5% acrylic resin (colloidal binder), 0.3% nano-graphene (infrared absorber), and 0.2% fluorocarbon nonionic surfactant. After mixing the above components, the mixture is magnetically stirred for 60 minutes until completely dissolved, ultrasonically dispersed for 20 minutes, and vacuum degassed for 15 minutes to obtain the target ink. Testing shows that the ink has a viscosity of 4.1 mPa·s and a surface tension of 30.2 mN / m at 25°C, meeting the requirements for stable spraying by piezoelectric nozzles and on-flight curing processes.

[0048] If a silica microsphere system is used, the formula is adjusted to: 8% silica nanoparticles with a particle size of 30nm, 87% anhydrous ethanol, 3% ethylene glycol, 1.2% silica sol (binder), 0.4% ATO nanoparticles (infrared absorber), and 0.4% polyether-modified siloxane surfactant. The preparation process is the same as above.

[0049] 3. Printing process Preparation before S1 printing: Fix the perovskite battery substrate with the back electrode fabricated onto a precision substrate stage, and perform appropriate hydrophobic modification treatment on the substrate surface to ensure that the static contact angle of the microsphere ink on the substrate surface is ≥100°, so as to ensure that there is no spreading deformation after the microspheres are deposited; inject the prepared spherical array ink into the constant temperature ink supply system and set the ink temperature to 25°C; set the nozzle-substrate distance to 2mm, calibrate the relative position of the three-axis motion platform and the printhead, and plan the array arrangement path.

[0050] S2 Heating System Pre-adjustment: Activate the graphene infrared heating module, set a constant heating temperature of 160~200℃, corresponding to a power density of 12~20W / cm², and after monitoring the uniformity and stability of the temperature field in the heating area by the infrared thermal imager, activate the water-cooled heat dissipation unit at the printhead end to maintain the nozzle temperature at 28℃ and prevent the ink in the nozzle from drying out prematurely.

[0051] S3 injection parameter calibration: Edit the two-segment bipolar pulse drive waveform, drive amplitude 25~35V, main pulse width 8~12μs, injection frequency 3~10kHz, observe the droplet injection state through a high-speed camera, and optimize the waveform to achieve stable single droplet injection without satellite droplets or tails. The 4pL droplet injection velocity is controlled at 8~12m / s, and the flight time is about 0.2ms.

[0052] S4 Spherical Array Printing: A three-axis motion platform and nozzle are synchronously printed, using a fixed-point spraying mode to prepare periodic microsphere arrays. The heater power density is controlled at 15 W / cm², and real-time monitoring is conducted using a high-speed camera. During droplet flight, the solvent evaporation rate reaches 100%, and droplets with an initial diameter of approximately 20 μm complete full solidification during flight, shrinking to form solid polymer microspheres. After deposition on the substrate, the microspheres exhibit no deformation or spreading, maintaining their sphericity. By adjusting the droplet spray volume and array spacing, microsphere arrays with particle sizes of 1–10 μm and spacing of 2–20 μm can be controllably prepared.

[0053] S5 Post-processing: After printing, the sample is placed in a vacuum oven and annealed at 80℃ for 20 minutes to remove trace amounts of residual solvent inside the microspheres, while strengthening the interfacial bonding force between the microspheres and the back electrode layer, thus completing the preparation of the light-management spherical microsphere array.

[0054] 4. Performance Test Results SEM and profilometry tests revealed that the prepared PMMA microsphere array exhibited a controllable particle size of 2-5 μm, a particle size uniformity (CV) ≤ 2.5%, sphericity ≥ 95%, and array position accuracy ± 0.8 μm, with no deformation or adhesion defects. When applied to the surface of a perovskite thin-film solar cell, photoelectric performance tests showed an increase in short-circuit current density from 19.07 mA / cm² to 20.32 mA / cm², and a photoelectric conversion efficiency from 21.05% to 24.12%, thus achieving a significant light management gain effect.

[0055] like Figure 1 As shown, the perovskite thin-film battery of the present invention was finally printed (printing completed).

[0056] The performance of the battery prepared by this invention and the battery prepared by conventional technology were tested. The test indicators included photoelectric conversion efficiency, open-circuit voltage, short-circuit current density, fill factor, film defect state density, interconnect dead zone area ratio, continuous printing yield, and line edge roughness. The test results are shown in the table below:

[0057] As shown in the test results above, the battery printed by this invention outperforms batteries prepared by existing technologies in all aspects. The battery of this invention exhibits significantly improved photoelectric conversion efficiency, higher open-circuit voltage, shorter-circuit current density, and fill factor. Continuous printing yield is greatly improved, pattern accuracy is significantly optimized, film defect state density is significantly reduced, and interconnect dead zone loss is reduced by more than 73%. Therefore, this invention demonstrates that the printing ink and printing method provided by this invention can effectively improve the photoelectric performance of perovskite thin-film batteries, overcome the defects of traditional processes, and possess significant technical advantages and application value.

[0058] This invention effectively achieves its objective through the following technical solutions: By designing a dedicated perovskite ink system, it pioneers a four-in-one formulation design logic integrating adhesive, solvent, infrared response, and photoelectric performance, developing a dedicated ink system for the full-functional layer of perovskite batteries adapted to the fly-drop process. Through the control of the type and content of the colloidal binder, it simultaneously achieves matching of ink viscoelasticity with the fly-drop process, and directional optimization of film density and photoelectric performance. Through the precise control of the ratio of the mixed solvent system, it accurately matches infrared radiation absorption efficiency, solvent evaporation rate, and perovskite crystallization rate, solving the technical challenge that existing perovskite inkjet inks cannot simultaneously meet the requirements of ultra-fine printing suitability and device photoelectric performance. A perovskite-specific printing method was designed to establish a three-stage printing process adapted to the entire perovskite solar cell fabrication process. Through the coordinated control of heating power, ink formulation, and jetting parameters, seamless switching between three core process modes is achieved: ① A 1μm-level ultra-fine pattern printing mode for fabricating sub-cell interconnect patterns, significantly reducing dead zone area; ② A uniform film layer printing mode for fabricating large-area defect-free perovskite functional layers, achieving precise control of solvent gradient evaporation and crystallization; ③ A spherical array printing mode for in-situ fabrication of light management microsphere arrays, improving the cell's light capture efficiency. The same equipment can achieve integrated printing fabrication of all functional layers and light management structures for perovskite solar cells.

[0059] The core innovation of this invention lies in: 1. Mechanism Innovation: Targeting the flight dynamics of 2-4 pL droplets in 20-50 μm nozzles, a novel gradient infrared droplet-pre-curing-crystallization control printing mechanism at the microsecond level during flight was pioneered. This mechanism overturns the traditional process logic of droplet deposition-solvent evaporation-high-temperature annealing and crystallization in perovskite inkjet printing. By bringing the solvent evaporation and pre-curing processes forward to the flight stage, low-temperature, uniform, and controllable solvent evaporation of perovskite ink is achieved. This overcomes the physical limitations of nozzle aperture and can stably prepare ultra-fine patterns at the 1±0.2 μm level. At the same time, it avoids problems such as precursor decomposition, uneven crystallization, and pinhole defects caused by high-temperature heating of the substrate in traditional printing, fundamentally solving the core pain points of perovskite inkjet printing.

[0060] 2. Material Innovation: A dedicated ink system for perovskite full-function layers, deeply coupled with the flying droplet mechanism, was developed. A synergistic control model of colloidal binder and mixed solvent was established: the viscoelasticity of the ink is controlled by the colloidal binder to match the flying droplet requirements of 4pL droplets, while suppressing precursor phase separation during flight and controlling perovskite grain growth; the infrared absorption efficiency and solvent evaporation rate are controlled by the ratio of mixed solvents, and precisely matched with the side-mounted infrared heating system. This can fill the technical gap that existing perovskite inks cannot simultaneously meet the three major requirements of ultra-fine jetting, flying droplet formation, and device performance.

[0061] 3. Process Innovation: An integrated printing process system for the entire perovskite solar cell process has been established. Through the coordinated control of heating power and formula parameters, three core processes can be seamlessly switched on the same set of equipment: 1μm-level interconnect pattern preparation, large-area functional layer uniform printing, and in-situ preparation of light management spherical array. For the first time, integrated inkjet printing of the full functional layer and light management structure of perovskite solar cells has been achieved, eliminating the need for multiple equipment and multiple processes. The preparation process is shortened by more than 60%, and the production cost is significantly reduced.

[0062] This invention pioneers a gradient infrared droplet-pre-curing-crystallization control mechanism for 2-4 pL droplets in flight at the microsecond level, overcoming the physical limitations of 20-50 μm nozzle orifice diameter on printing resolution. It also solves the technical problems of perovskite ink's thermal sensitivity, poor crystallization controllability, and low continuous printing stability. Through the synergistic control of adhesive and solvent, it achieves performance-oriented optimization of the full functional layer of perovskite solar cells, significantly improving the conversion efficiency, stability, and industrial feasibility of perovskite solar cells.

Claims

1. A printing ink system for perovskite thin-film batteries, characterized in that, It includes hole transport layer printing ink, perovskite light absorption layer printing ink, electron transport layer printing ink, back electrode printing ink, and spherical array printing ink; all printing inks have a viscosity of 2-10 mPa・s and a surface tension of 25-35 mN / m at 25°C.

2. The printing ink system as described in claim 1, characterized in that, The hole transport layer printing ink comprises the following raw materials formulated in weight percentages: Hole transport functional material 0.5%-5%, mixed solvent system 90%-98%, colloidal binder 0.5%-3%, infrared absorber 0.05%-0.3%, surfactant 0.05%-0.5%.

3. The printing ink system as described in claim 2, characterized in that, The hole transport functional material is any one of Spiro-OMeTAD, PTAA, PEDOT:PSS, or NiOx nanoparticles. The mixed solvent system is prepared by any two solvents of chlorobenzene, toluene, anhydrous ethanol or acetonitrile at a volume ratio of 95:5 to 80:20, thereby controlling the solvent evaporation rate. The colloidal binder is any one of polyvinylidene fluoride, acrylic resin, or ethyl cellulose, and is used to control the viscoelasticity of the ink, the adhesion of the film layer, and the cell migration rate.

4. The printing ink system as described in claim 1, characterized in that, The perovskite light-absorbing layer printing ink comprises the following raw materials formulated in the following weight percentages: The composition includes 10%-25% perovskite precursor, 70%-88% mixed solvent system, 0.5%-2% colloidal binder, 0.1%-1% crystallization regulator, 0.05%-0.2% infrared absorber, and 0.05%-0.3% surfactant.

5. The printing ink system as described in claim 4, characterized in that, The perovskite precursor is at least one of formamidine cesium lead iodine, formamidine methylamine lead iodine, or all-inorganic cesium lead bromine; The mixed solvent system is a ternary system prepared by mixing DMF, DMSO and NMP in a volume ratio of 7:2:1 to 4:5:

1. The infrared absorption efficiency and perovskite crystallization rate are controlled by the ratio of this mixed solvent system. The colloidal binder is either polyethylene oxide or polyvinylpyrrolidone, and is used to suppress precursor phase separation during flight, regulate grain growth, and reduce grain boundary defects.

6. The printing ink system as described in claim 1, characterized in that, The electron transport layer printing ink comprises the following raw materials formulated in weight percentages: Electron transport functional materials 1%-8%, mixed solvent system 90%-97%, colloidal binder 0.5%-2%, infrared absorber 0.05%-0.3%, surfactant 0.05%-0.5%.

7. The printing ink system as described in claim 6, characterized in that, The electron transport functional material is any one of C60, PCBM, SnO2 nanoparticles, TiO2 nanoparticles, or ZnO nanoparticles. The mixed solvent system is any binary mixture of chlorobenzene, anhydrous ethanol, isopropanol or ethyl acetate; The colloidal binder is PMMA or acrylic resin, used to regulate the film density and interfacial contact characteristics, and reduce leakage current.

8. The printing ink system as described in claim 1, characterized in that, The back electrode printing ink and the spherical array printing ink comprise the following raw materials formulated in percentage by mass: Functional materials 5%-15%, mixed solvent system 80%-92%, colloidal binder 1%-5%, infrared absorber 0.1%-0.5%, surfactant 0.1%-0.5%.

9. The printing ink system as described in claim 8, characterized in that, The functional material in the back electrode printing ink is any one of silver, copper, or gold nanoparticles with a particle size ≤30nm, used for fabricating 1μm-level sub-cell interconnect patterns; the mixed solvent system is a binary compound system of main solvent and co-solvent, the main solvent is any one of anhydrous ethanol, isopropanol, or acetone; the co-solvent is any one of ethylene glycol butyl ether, propylene glycol methyl ether, or diethylene glycol dimethyl ether, and the mass ratio of main solvent to co-solvent is 90:10~80:20; the colloidal binder is any one of acrylic resin, ethyl cellulose, or polyvinylpyrrolidone.

10. The printing ink system as described in claim 8, characterized in that, The functional material in the spherical array printing ink is PMMA or silica nanoparticles, used for the fabrication of perovskite solar cell photomanagement microsphere arrays. The mixed solvent system is divided into two categories based on the type of functional material, both using a combination of high and low boiling point solvents. For the PMMA microsphere system, the mixed solvent system is any binary mixed solvent from chlorobenzene, toluene, ethyl acetate, or isopropanol, with the high-boiling-point component accounting for 10%–25%. For the silica microsphere system, the mixed solvent system is any binary mixed solvent from anhydrous ethanol, ethylene glycol, deionized water, or isopropanol, with the high-boiling-point component accounting for 5%–15%. The colloidal binder is matched according to the selected functional material. For the PMMA microsphere system, the colloidal binder uses PMMA itself as the main sphere-forming component and the binding component, compounded with polyethylene glycol as an auxiliary binder. For the silica microsphere system, the colloidal binder uses silica sol and tetraethyl orthosilicate hydrolyzed prepolymer as binders, undergoing a condensation reaction during microsphere curing to improve the mechanical strength of the microspheres and the adhesion to the substrate.

11. A method for ultra-fine inkjet printing of perovskite thin-film batteries, comprising a three-part printing process, the first part of which involves printing the target functional layer of the perovskite thin-film battery on the surface of a conductive substrate, including the following steps: S1 Printing Preparation: Fix the conductive substrate onto the ultra-fine inkjet printer, inject the printing ink system of the perovskite thin film battery into the printer, and adjust the printer. S2 heating system preset: Start the printer heating, set the target heating temperature, and control the nozzle temperature to be stable at 25-30℃; S3 jet parameter calibration: Edit the multi-segment bipolar pulse drive waveform, set the drive amplitude, pulse width, and jet frequency, observe the droplet jet status in real time, optimize the drive waveform, and achieve stable jetting of a single droplet without satellite droplets or tails. The jetting speed of a 4pL droplet is controlled at 8-15m / s, and the flight time is 0.1-0.4ms. S4 Controllable Droplet Printing: Select the corresponding printing ink and printing mode, and start the three-axis motion platform and printhead of the device to print synchronously on the conductive substrate; S5 Post-processing annealing: The conductive substrate with the printed target functional layer is subjected to programmed temperature annealing to complete film crystallization, solvent removal and performance optimization, and obtain the target functional layer of the perovskite solar cell.

12. The printing method as described in claim 11, characterized in that, When the uniform film printing mode is selected, it is used to prepare large-area functional layers for perovskite solar cells. The heater temperature of the printing equipment is controlled at 80-120℃ and the heater power density is 3-10W / cm². This allows the solvent evaporation rate of the droplets to reach 60%-80% during flight, the particle size to shrink to 5-10μm and complete semi-curing. After the semi-cured droplets are deposited, they spread and overlap evenly to form a dense film without pinholes or coffee rings.

13. The printing method as described in claim 11, characterized in that, The second part of the printing process involves printing a back electrode on the surface of a perovskite thin-film battery with the target functional layer. The steps are as follows: 1) Setting up the printing device: Set the parameters for printing the back electrode, adjust the printing equipment, and prepare to print the back electrode; 2) Printing of the back electrode S1 Printing Preparation: Fix the perovskite thin-film battery with the target functional layer onto the ultra-fine inkjet printing equipment and adjust the printing equipment; S2 heating system preset: Start the printer heating, set the heating temperature, and control the nozzle temperature to be stable at 28℃; S3 jet parameter calibration: Edit the three-segment bipolar pulse drive waveform, set the drive amplitude, pulse width, and jet frequency, observe the droplet jet status in real time, optimize the drive waveform, and achieve stable jetting of a single droplet without satellite droplets or tails. The jetting speed of a 4pL droplet is controlled at 10m / s, and the flight time is 0.15ms. S4 Ultra-fine graphic printing: Select the ultra-fine graphic printing ink and printing mode, start the three-axis motion platform and printhead of the device to synchronously print the back electrode of the perovskite thin film battery with the target functional layer. S5 Post-processing: After the back electrode is printed, the sample is placed in a forced-air oven and sintered at 150°C for 30 minutes to remove residual solvent and obtain a perovskite thin-film battery with a printed back electrode. 3) The performance of the perovskite thin-film battery with the printed back electrode was tested. SEM and profilometer tests showed that the average line width of the printed conductive lines was 1.02 μm, the line width uniformity CV ≤ 4.0%, the edge roughness ≤ 0.2 μm, and there were no coffee ring effect or broken pen defects.

14. The printing method as described in claim 13, characterized in that, The power density of the heater in the printing equipment is controlled to be 2-12W / cm², so that the solvent evaporation rate of 2-4pL droplets reaches 80%-95% during flight, the particle size shrinks from the initial 20-50μm to 2-5μm and completes gelation and pre-curing. After the pre-cured droplets are deposited on the substrate, they have no flowability and a spreading coefficient ≤1.

2. After curing, they form ultra-fine patterns at the 1±0.2μm level.

15. The printing method as described in claim 11, characterized in that, The third part of the printing process involves printing a spherical array on the surface of a perovskite thin-film battery with a back electrode. The steps are as follows: 1) Setting up the printing device: Set the parameters for printing the spherical array, adjust the printing equipment, and prepare to print the spherical array; 2) Printing of spherical arrays S1 Printing Preparation: Fix the perovskite thin-film battery with the back electrode onto the ultra-fine inkjet printing equipment and adjust the printing equipment; S2 heating system preset: Start the printer heating, set the heating temperature, and control the nozzle temperature to be stable at 28℃; S3 Injection Parameter Calibration: Edit the two-segment bipolar pulse drive waveform, set the drive amplitude, pulse width, and jet frequency, observe the droplet jet state in real time, optimize the drive waveform, and achieve stable jetting of a single droplet without satellite droplets or tails. The jetting speed of a 4pL droplet is controlled at 8~12m / s, and the flight time is 0.2ms. S4 Printed Spherical Array: Select the printing ink and printing mode for the spherical array, and start the three-axis motion platform and printhead of the device to simultaneously print the spherical array for the perovskite thin film battery with the back electrode. S5 Post-processing: After the spherical array is printed, the sample is placed in a vacuum oven and annealed at 80°C for 20 minutes to remove trace amounts of residual solvent inside the microspheres and strengthen the interfacial bonding force between the microspheres and the back electrode layer, thus completing the preparation of the light-management spherical microsphere array. 3) Performance testing of perovskite thin-film solar cells with printed spherical arrays. SEM and step profile tests showed that the microsphere array prepared by PMMA microsphere array had a controllable particle size of 2-5μm, a particle size uniformity CV≤2.5%, a sphericity ≥95%, an array position accuracy of ±0.8μm, and no deformation or adhesion defects.

16. The printing method as described in claim 15, characterized in that, The power density of the heater in the printing equipment is controlled to be 12-20W / cm², so that the solvent evaporation rate of the droplets reaches 100% during flight, and the solid microspheres are formed after complete curing. After deposition on the substrate, they are not deformed or spread, forming a high-precision spherical array with a controllable particle size of 1-10μm.