A perovskite solar cell, its fabrication method and application
By using a wide-width ultrasonic atomization spraying process to prepare a nickel oxide hole transport layer and a composite interface passivation layer, the problem of poor interface compatibility in the traditional slit spraying process is solved, enabling high-efficiency, stable, and low-cost large-area production of perovskite solar cells, which is suitable for both rigid and flexible substrates.
Patent Information
- Application Number
- CN202611489172.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional slot spraying composite processes for perovskite solar cells suffer from problems such as poor interface compatibility, uneven performance of sub-cells in large-area modules, and insufficient stability, making it difficult to achieve low-cost, wide-area mass production and flexible substrate adaptation.
A nickel oxide hole transport layer and a composite interface passivation layer were prepared using a wide-width ultrasonic atomization spraying process. By optimizing specific parameters, including ultrasonic power, atomization pressure, feed flow rate, nozzle liquid slit opening, and substrate running speed, a nickel oxide layer and a composite interface passivation layer with a thickness of 5-45 nm were formed.
This technology achieves high efficiency, stability, and uniformity in perovskite solar cells, reduces production costs, is applicable to both rigid and flexible substrates, and improves the feasibility of large-area production and cell performance.
Smart Images

Figure SMS_1 
Figure SMS_4
Abstract
Description
Technical Field
[0001] This invention belongs to the field of perovskite photovoltaic device technology, specifically, it relates to a perovskite solar cell, its fabrication method, and its application. More specifically, it relates to a perovskite solar cell fabricated using a fully sprayed composite interface, its fabrication method, and its application. Background Technology
[0002] With the ever-increasing energy demands of human society and the dwindling availability of traditional fossil fuels, a major challenge for the future is finding a renewable energy source to replace traditional fossil fuels. Solar energy, with its inexhaustible, environmentally friendly characteristics, has gained significant attention. Currently, silicon-based solar cells dominate the market, but due to their high manufacturing costs and complex processes, their ability to become a primary clean energy source for humanity in the future is constantly questioned. Therefore, it is essential to find new types of solar cells that are inexpensive and have simple manufacturing processes.
[0003] Perovskite solar cells have become a research hotspot for next-generation photovoltaic technology due to their advantages such as high photoelectric conversion efficiency, low cost, and solution-processability. Flexible perovskite modules combine lightweight, bendability, and portability, and are used in wearable devices, building-integrated photovoltaics, and mobile energy.
[0004] In inverted perovskite photovoltaic modules, the NiOx hole transport layer, the SAM self-assembled modification layer, and the perovskite top interface passivation layer are the three key interfacial functional films that determine the device's open-circuit voltage, non-radiative recombination, and long-term damp-heat stability. Currently, the mainstream technologies for large-area industrial-scale fabrication are slit coating, single-point reciprocating air spraying, and spin coating. Among them, slit coating has become the preferred solution for mass production by major manufacturers due to its precise metering and high material utilization. However, it has unavoidable industrialization shortcomings in areas such as continuous integrated fabrication of NiOx, ultra-thin SAM (self-assembled monolayer), and top interface three layers, flexible substrate adaptation, and open-air mass production. Traditional single-point fan-shaped spraying has defects such as spliced film formation, large thickness dispersion, and poor large-area consistency. Existing processes cannot simultaneously meet the four requirements of continuous co-line fabrication of three layers, open production at atmospheric pressure, compatibility with flexible / rigid substrates, and low-cost wide-area mass production. The specific defects of existing technologies are described below: The SAM layer coating process window is extremely narrow, making it difficult to achieve uniform anchoring of single molecules in the narrow slits. The target film thickness of the SAM layer is only 1-10 nm, the ink concentration is as low as 0.2-0.8 mg / mL, and the solid content is extremely low. The film is spread by continuous liquid bridges in the narrow slits, and low concentration solutions are prone to film breakage, pinholes, and localized missing coating. At the same time, the wet film thickness in the narrow slits is relatively large, which easily leads to SAM multilayer agglomeration and local stacking after annealing. This results in uneven density of SAM molecules on the NiOx surface, with some areas exposing NiOx oxygen vacancies and some areas having excessively thick SAM that hinders hole extraction, directly increasing the efficiency dispersion between modules.
[0005] The processing, maintenance, and debugging of wide-width slit heads have extremely high barriers to entry, resulting in low tolerance for errors in mass production. The parallelism and flatness of the lip of a 400mm full-width slit head must be less than 3μm. The procurement cost of imported custom slit heads is 3-5 times that of linear atomizing printheads. During mass production, fluctuations in the flow rate of the feed pump, changes in ambient temperature, and slight changes in ink viscosity caused by solvent evaporation can all lead to a film thickness gradient defect with a thicker middle and thinner edges. The debugging cycle for a single 400mm slit production line can easily take tens of days. The tolerance range for mass production parameters is narrow, and even slight modifications to the formula require the re-customization of gaskets and optimization of the process. The costs of R&D and mass production iterations are high.
[0006] The process suffers from poor repeatability and stability, resulting in high equipment and energy costs. The stability of the liquid outlet bend in the slit coating die is highly susceptible to environmental temperature and humidity, as well as air convection disturbances. The NiOx precursor alcohol solution and low-concentration SAM ethanol solution evaporate rapidly, and in open air, the rapid evaporation of solvents easily crystallizes and clogs the lip, causing stringing streaks and localized film defects. Furthermore, the solvent systems of the three ink layers—NiOx, SAM, and the upper interface—are significantly different, requiring each layer to be replaced and purged in an independent, sealed chamber, which multiplies the production line footprint, energy consumption, and maintenance costs.
[0007] A patent document published in China, publication number CN121888855A, on July 20, 2026, discloses a method for preparing a hole transport layer for perovskite solar cells based on a digital spraying method. This method, targeting digital spraying equipment, uses a mixed solvent composed of DMF and ethanol. The strong dipole and hydrogen bonding of DMF are utilized to improve the aggregation of SAM molecules in a single ethanol solvent and resist the influence of moisture. Simultaneously, the low boiling point of ethanol enables rapid spreading of the sprayed droplets, achieving large-area uniform deposition of the hole transport layer under a non-inert gas atmosphere and high humidity. However, specific digital spraying equipment is required to achieve large-area spraying, addressing the issues of SAM formation from multiple spraying processes, low photoelectric conversion efficiency, and high cost.
[0008] A patent document published in China, publication number CN108417739A, on August 17, 2018, discloses a perovskite light-emitting diode (LED) based on a spray coating process and its fabrication method. The method includes the following steps: preparing a substrate; sequentially fabricating an anode layer, a hole transport layer, a perovskite light-emitting layer, an electron transport layer, and a cathode layer on the substrate; and finally encapsulating the obtained substrate to complete device fabrication. Specifically, the step of preparing the perovskite light-emitting layer involves placing the substrate on a low-temperature plate for cooling, spraying a perovskite material solution onto the hole transport layer in a single operation to obtain the perovskite light-emitting layer, and then directly placing the low-temperature substrate on a hot plate for annealing to complete the perovskite light-emitting layer preparation. However, achieving this solution requires precise control of the low-temperature environment, which increases the complexity and cost of the process and places higher demands on large-scale production. Summary of the Invention
[0009] The purpose of this invention is to provide: A perovskite solar cell, its preparation method and application, and related technologies are disclosed to solve technical problems such as poor interface compatibility, uneven performance of sub-cells in large-area modules, and insufficient stability in traditional slot spraying composite processes, or combinations thereof.
[0010] Terminology Explanation: Unless otherwise defined, all technical terms used herein have the same meanings as commonly understood by one of ordinary skill in the art. Unless otherwise stated, all patents, patent inventions, and publications cited throughout this document are incorporated herein by reference in their entirety. If multiple definitions exist for terms in this document, the definitions provided in this chapter shall prevail.
[0011] It should be understood that the above brief description and the following detailed description are exemplary and for illustrative purposes only, and do not limit the subject matter of the invention in any way. In this invention, the singular is used in conjunction with the plural unless otherwise specifically stated. It should also be noted that, unless otherwise stated, the use of “or” or “or” means “and / or”. Furthermore, the use of the term “comprising” and other forms such as “including,” “containing,” and “contains” are not limiting.
[0012] Unless specifically defined herein, the use of all commercially available products herein employs standard techniques. For example, it may be carried out using the manufacturer's instructions for use with the kit, or in accordance with methods known in the art or the description of this invention. The techniques and methods described herein can generally be implemented according to conventional methods well known in the art, based on the descriptions in the various summary and more specific documents cited and discussed in this specification.
[0013] The terms “optional / arbitrary” or “optionally / arbitrarily” mean that the event or situation described below may or may not occur, including both the occurrence and non-occurrence of the event or situation.
[0014] The term "rigid ITO glass" as used in this article refers to a composite material with an inorganic glass (such as soda-lime glass, borosilicate glass, or quartz glass) as a rigid substrate, on which a transparent, conductive indium tin oxide (ITO) thin film is formed through physical or chemical deposition processes (such as magnetron sputtering, chemical vapor deposition, etc.). This material has high light transmittance, low resistivity, excellent surface flatness, and high temperature resistance, and the substrate does not deform. It is suitable for high-temperature processes and optoelectronic devices requiring high mechanical strength (such as liquid crystal displays, touch screens, thin-film solar cells, etc.), but it does not have bending or rolling properties.
[0015] The term "flexible ITO-PET / ITO-PEN substrate" as used in this article refers to a transparent conductive film made by depositing an indium tin oxide (ITO) conductive layer on the surface of a flexible substrate—polyethylene terephthalate (PET) or polyethylene naphthalate (PEN)—using low-temperature sputtering or roll-to-roll deposition processes. This type of substrate is characterized by its flexibility, light weight, resistance to certain deformations, and suitability for winding processing. However, its processing temperature is limited by the glass transition temperature of the polymer substrate, resulting in relatively low processing temperatures. Furthermore, the ITO layer is prone to cracking and increased resistance under repeated bending or humid and hot environments. It is mainly used in flexible displays, wearable electronics, flexible sensors, and organic photovoltaic devices.
[0016] The term "atomized spraying" as used in this article refers to a spraying technology that uses principles such as ultrasonic atomization and compressed air atomization to disperse liquid materials (sols, sols, suspensions, etc.) into fine droplets, which are then guided by a carrier gas or airflow to be uniformly deposited on the surface of a substrate to form a coating or film.
[0017] The term "Voc" used in this article refers to Open-circuit Voltage, which is the potential difference between the positive and negative terminals of a solar cell under no-load (open-circuit) conditions. Voc is one of the key parameters that determines the maximum power output of a solar cell.
[0018] The term "FF" used in this article refers to the fill factor, which is the ratio of the maximum output power of a solar cell to the product of its open-circuit voltage and short-circuit current. It is used to measure the "rectangularity" of the cell's output characteristics. A higher FF indicates a smaller series resistance and a higher carrier extraction efficiency.
[0019] The term "Jsc" used in this article refers to Short-circuit Current Density, which is the photocurrent generated per unit effective area when the device is in a short-circuit state (voltage is zero) under standard test conditions. It is a key parameter for measuring the efficiency of photogenerated carrier generation and collection in a battery, and its value directly reflects the battery's ability to utilize incident photons.
[0020] The term "PCE" used in this article refers to Power Conversion Efficiency, which is the ratio of the maximum electrical power output by a cell to the total solar power incident on the effective area of the cell under standard test conditions. It is the most core and direct macroscopic indicator for measuring the overall performance of photovoltaic devices, and its value is determined by the open-circuit voltage (Voc), short-circuit current density (Jsc), and fill factor (FF).
[0021] As used herein, the term "slot coating" refers to a coating technique for applying solutions, slurries, or extruded films onto a flat substrate. This process involves dissolving or suspending the desired coating material in a precursor solution or slurry and delivering it to the substrate surface through a slot die. Controlled delivery of the coating liquid allows for the continuous production of wide coating materials on the substrate. By controlling the solution deposition rate and the relative velocity between the solution and the substrate, thin material coatings ranging from 10 nanometers to 100 micrometers in thickness can be obtained.
[0022] The term "substrate" as used in this article refers to the base material that serves as a support or starting layer during the material preparation or device manufacturing process. Other materials are usually deposited, grown, or coated on the substrate, such as glass and silicon wafers.
[0023] The term "hole transport layer" used in this article refers to the layer located between the active layer and the anode, which promotes hole transport while suppressing reverse flow between holes and the cathode. It is one of the key components affecting the performance of solar cells. Commonly used hole transport layer materials include conductive polymers such as PEDOT and PSS.
[0024] The term "perovskite active layer" used in this article refers to the key functional layer in a perovskite solar cell that absorbs photons and generates electron-hole pairs. It is usually composed of materials with a perovskite structure, such as ABX3 type (A is an organic cation, B is a metal cation, and X is a halogen element) perovskite materials, and its performance directly affects the photoelectric conversion efficiency of the cell.
[0025] The term "electron transport layer" as used in this article refers to a layer of material located between the perovskite active layer and the cathode in a solar cell. Its main function is to collect and transport electrons generated in the perovskite active layer, while preventing holes from transporting to the cathode, so as to achieve effective separation and transport of electrons and holes and improve the photoelectric performance of the cell.
[0026] The term "metal top electrode" as used in this article refers to an important component of a solar cell, usually located at the top of the cell structure. It is generally made of a metal material with good conductivity and stability, such as silver or aluminum. Its function is to collect the current generated in the cell and lead the current out for external power supply.
[0027] In a first aspect, the present invention provides: a perovskite solar cell, comprising, from bottom to top, a transparent conductive substrate, a nickel oxide hole transport layer, a composite interface passivation layer, a CsFAPbI3 perovskite layer, an electron transport layer, and a metal back electrode. The nickel oxide hole transport layer is prepared using a wide-width ultrasonic atomization spraying process; The thickness of the nickel oxide hole transport layer is 5-45 nm.
[0028] Preferably, the effective spraying area of the wide-width ultrasonic atomization spraying is 400×400mm.
[0029] Preferably, the thickness of the nickel oxide hole transport layer is selected from any value or range between 5 and 45 nm, specifically from: 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm or any two of them.
[0030] More preferably, the thickness of the nickel oxide hole transport layer is 20 nm.
[0031] Preferably, the specific parameters of the wide-width ultrasonic atomization spraying process for the nickel oxide hole transport layer are as follows: The ultrasonic power is 22-45W; the upper atomizing pressure is 0.14-0.22MPa, and the lower atomizing pressure is 0.12-0.19MPa; the carrier gas pressure is 0.2-0.6MPa; the feed flow rate is 1.5-3.0mL / min; the nozzle liquid slit opening is 0.10-0.15mm, and the distance between the nozzle and the substrate is 35-55mm; the substrate running speed is 180-260mm / s; pre-anneal at 70-90℃ for 3-8min, followed by high-temperature annealing at 120-160℃ for 15-25min; and then allow to cool naturally to room temperature.
[0032] Preferably, the ultrasonic power is selected from any value or range between 22-45W, specifically from: 22W, 25W, 28W, 30W, 35W, 38W, 40W, 42W, 45W or any two of them.
[0033] More preferably, the ultrasonic power is selected from any value or range between 28-42W, specifically from: 28W, 30W, 35W, 38W, 40W, 42W or any two of them.
[0034] More preferably, the ultrasonic power is 35W.
[0035] Preferably, the upper atomizing pressure is selected from any value or range between 0.14 and 0.22 MPa, specifically from: 0.14 MPa, 0.15 MPa, 0.16 MPa, 0.17 MPa, 0.18 MPa, 0.19 MPa, 0.20 MPa, 0.21 MPa, 0.22 MPa, or any two of them.
[0036] More preferably, the upper atomizing pressure is selected from any value or range between 0.14-0.21 MPa, specifically from: 0.14 MPa, 0.15 MPa, 0.16 MPa, 0.17 MPa, 0.18 MPa, 0.19 MPa, 0.20 MPa, 0.21 MPa or any two of them.
[0037] More preferably, the upper atomizing pressure is 0.18 MPa.
[0038] Preferably, the lower atomizing pressure is selected from any value or range between 0.12 and 0.19 MPa, specifically from: 0.12 MPa, 0.13 MPa, 0.14 MPa, 0.15 MPa, 0.16 MPa, 0.17 MPa, 0.18 MPa, 0.19 MPa or any two of them.
[0039] More preferably, the lower atomizing pressure is selected from any value or range between 0.12-0.18 MPa, specifically from: 0.12 MPa, 0.13 MPa, 0.14 MPa, 0.15 MPa, 0.16 MPa, 0.17 MPa, 0.18 MPa or any two of them.
[0040] More preferably, the lower atomizing pressure is 0.15 MPa.
[0041] Preferably, the carrier gas pressure is selected from any value or range between 0.2-0.6 MPa, specifically from: 0.2 MPa, 0.3 MPa, 0.4 MPa, 0.5 MPa, 0.6 MPa or any two of them.
[0042] More preferably, the carrier gas pressure is 0.2 MPa.
[0043] Preferably, the feed flow rate is selected from any value or range between 1.5 and 3.0 mL / min, specifically from: 1.5 mL / min, 1.6 mL / min, 1.7 mL / min, 1.8 mL / min, 1.9 mL / min, 2.0 mL / min, 2.1 mL / min, 2.2 mL / min, 2.3 mL / min, 2.4 mL / min, 2.5 mL / min, 2.6 mL / min, 2.7 mL / min, 2.8 mL / min, 2.9 mL / min, 3.0 mL / min, or any range between two of them.
[0044] More preferably, the feed flow rate is selected from any value or range between 1.6 and 2.9 mL / min, specifically from: 1.6 mL / min, 1.7 mL / min, 1.8 mL / min, 1.9 mL / min, 2.0 mL / min, 2.1 mL / min, 2.2 mL / min, 2.3 mL / min, 2.4 mL / min, 2.5 mL / min, 2.6 mL / min, 2.7 mL / min, 2.8 mL / min, 2.9 mL / min or any two of them.
[0045] More preferably, the feed flow rate is 2.2 mL / min.
[0046] Preferably, the nozzle liquid slit opening is selected from any value or range between 0.10-0.15mm, specifically from: 0.1mm, 0.11mm, 0.12mm, 0.13mm, 0.14mm, 0.15mm or any two of them.
[0047] More preferably, the nozzle liquid slit opening is 0.12 mm.
[0048] Preferably, the distance between the nozzle and the substrate is selected from any value or range between 35-55mm, specifically from: 35mm, 36mm, 37mm, 38mm, 39mm, 40mm, 41mm, 45mm, 50mm, 55mm or any two of them.
[0049] More preferably, the distance between the nozzle and the substrate is 45mm.
[0050] Preferably, the operating speed of the substrate is selected from any value or range between 180-260 mm / s, specifically from: 180 mm / s, 185 mm / s, 190 mm / s, 195 mm / s, 200 mm / s, 205 mm / s, 210 mm / s, 215 mm / s, 220 mm / s, 230 mm / s, 240 mm / s, 250 mm / s, 260 mm / s or any two of them.
[0051] More preferably, the operating speed of the substrate is selected from any value or range between 185-240 mm / s, specifically from: 185 mm / s, 190 mm / s, 195 mm / s, 200 mm / s, 205 mm / s, 210 mm / s, 215 mm / s, 220 mm / s, 230 mm / s, 240 mm / s or any two of them.
[0052] More preferably, the substrate operates at a speed of 220 mm / s.
[0053] Preferably, the pre-annealing temperature is selected from any value or range between 70-90℃, specifically from: 70℃, 75℃, 80℃, 85℃, 90℃ or any two of them.
[0054] More preferably, the pre-annealing temperature is 80°C.
[0055] Preferably, the pre-annealing time is selected from any value or range between 3 and 8 minutes, specifically from: 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes or any two of them.
[0056] More preferably, the pre-annealing time is 5 minutes.
[0057] Preferably, the high-temperature annealing temperature is selected from any value or range between 120-160℃, specifically from: 120℃, 130℃, 140℃, 150℃, 160℃ or any two of them.
[0058] More preferably, the high-temperature annealing temperature is 140°C.
[0059] Preferably, the high-temperature annealing time is selected from any value or range between 15 and 25 min, specifically from: 15 min, 16 min, 17 min, 18 min, 19 min, 20 min, 21 min, 22 min, 23 min, 24 min, 25 min or any two of them.
[0060] More preferably, the high-temperature annealing time is 20 minutes.
[0061] Preferably, the composite interface passivation layer is prepared using a wide-width ultrasonic atomization spraying process, and the composite interface passivation layer includes a SAM monolayer and a passivation interface upper layer.
[0062] Preferably, the specific parameters of the wide-width ultrasonic atomization spraying process for a single layer of SAM are as follows: The ultrasonic power is reduced to 18-26W; the upper atomizing pressure is 0.08-0.15MPa; the lower atomizing pressure is 0.07-0.13MPa; the feed flow rate is 0.5-1.2mL / min; the liquid slit opening is 0.10-0.15mm; the nozzle-substrate spacing is increased to 50-65mm; the substrate running speed is 180-260mm / s; and annealing is carried out at 85-110℃ for 5-15min.
[0063] Preferably, the ultrasonic power is selected from any value or range between 18-26W, specifically from: 18W, 19W, 20W, 21W, 22W, 23W, 24W, 25W, 26W or any two of them.
[0064] More preferably, the ultrasonic power is 22W.
[0065] Preferably, the upper atomizing pressure is selected from any value or range between 0.08 and 0.15 MPa, specifically from: 0.08 MPa, 0.09 MPa, 0.10 MPa, 0.11 MPa, 0.12 MPa, 0.13 MPa, 0.14 MPa, 0.15 MPa or any two of them.
[0066] More preferably, the upper atomizing pressure is 0.12 MPa.
[0067] Preferably, the lower atomizing pressure is selected from any value or range between 0.07 and 0.13 MPa, specifically from: 0.07 MPa, 0.08 MPa, 0.09 MPa, 0.10 MPa, 0.11 MPa, 0.12 MPa, 0.13 MPa or any two of them.
[0068] More preferably, the lower atomizing pressure is 0.10 MPa.
[0069] Preferably, the feed flow rate is selected from any value or range between 0.5 and 1.2 mL / min, specifically from: 0.5 mL / min, 0.6 mL / min, 0.7 mL / min, 0.8 mL / min, 0.9 mL / min, 1.0 mL / min, 1.1 mL / min, 1.2 mL / min or any two of them.
[0070] More preferably, the feed flow rate is 0.8 mL / min.
[0071] Preferably, the nozzle liquid slit opening is selected from any value or range between 0.10-0.15 mm, specifically from: 0.10 mm, 0.11 mm, 0.12 mm, 0.13 mm, 0.14 mm, 0.15 mm or any two of them.
[0072] More preferably, the nozzle liquid slit opening is 0.12 mm.
[0073] Preferably, the distance between the nozzle and the substrate is selected from any value or range between 50-65mm, specifically from: 50mm, 51mm, 52mm, 53mm, 54mm, 55mm, 56mm, 57mm, 58mm, 59mm, 60mm, 61mm, 62mm, 63mm, 64mm, 65mm or any two of them.
[0074] More preferably, the distance between the nozzle and the substrate is 55mm.
[0075] Preferably, the operating speed of the substrate is selected from any value or range between 180-260 mm / s, specifically from: 180 mm / s, 190 mm / s, 200 mm / s, 210 mm / s, 220 mm / s, 230 mm / s, 240 mm / s, 250 mm / s, 260 mm / s or any two of them.
[0076] More preferably, the substrate operates at a speed of 220 mm / s.
[0077] Preferably, the annealing temperature is selected from any value or range between 85-110℃, specifically from: 85℃, 90℃, 95℃, 100℃, 105℃, 110℃ or any two of them.
[0078] More preferably, the annealing temperature is 100°C.
[0079] Preferably, the annealing time is selected from any value or range between 5 and 15 minutes, specifically from: 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 15 minutes or any two of them.
[0080] More preferably, the annealing time is 10 minutes.
[0081] Preferably, the specific parameters of the wide-width ultrasonic atomization spraying process on the passivation interface upper layer are as follows: The ultrasonic power is 22-34W; the upper atomizing pressure is 0.10-0.18MPa; the lower atomizing pressure is 0.08-0.15MPa; the feed flow rate is 0.7-1.5mL / min; the liquid slit opening is 0.10-0.15mm; the nozzle-substrate spacing is 40-60mm; the substrate running speed is 180-260mm / s; and annealing is carried out at 85-110℃ for 5-12min.
[0082] Preferably, the ultrasonic power is selected from any value or range between 22-34W, specifically from: 22W, 23W, 24W, 25W, 26W, 27W, 28W, 29W, 30W, 31W, 32W, 33W, 34W or any two of them.
[0083] More preferably, the ultrasonic power is 28W.
[0084] Preferably, the upper atomizing pressure is selected from any value or range between 0.10-0.18 MPa, specifically from: 0.10 MPa, 0.11 MPa, 0.12 MPa, 0.13 MPa, 0.14 MPa, 0.15 MPa, 0.16 MPa, 0.17 MPa, 0.18 MPa, or any two of them.
[0085] More preferably, the upper atomizing pressure is 0.14 MPa.
[0086] Preferably, the lower atomizing pressure is selected from any value or range between 0.08 and 0.15 MPa, specifically from: 0.08 MPa, 0.09 MPa, 0.10 MPa, 0.11 MPa, 0.12 MPa, 0.13 MPa, 0.14 MPa, 0.15 MPa or any two of them.
[0087] More preferably, the lower atomizing pressure is 0.12 MPa.
[0088] Preferably, the feed flow rate is selected from any value or range between 0.7 and 1.5 mL / min, specifically from: 0.7 mL / min, 0.8 mL / min, 0.9 mL / min, 1.0 mL / min, 1.1 mL / min, 1.2 mL / min, 1.3 mL / min, 1.4 mL / min, 1.5 mL / min or any two of them.
[0089] More preferably, the feed flow rate is 1.0 mL / min.
[0090] Preferably, the liquid gap opening is selected from any value or range between 0.10-0.15 mm, specifically from: 0.10 mm, 0.11 mm, 0.12 mm, 0.13 mm, 0.14 mm, 0.15 mm or any two of them.
[0091] More preferably, the liquid slit opening is 0.12 mm.
[0092] Preferably, the nozzle substrate spacing is selected from any value or range between 40-60mm, specifically from: 40mm, 45mm, 50mm, 55mm, 60mm or any two of them.
[0093] More preferably, the nozzle substrate spacing is 50mm.
[0094] Preferably, the operating speed of the substrate is selected from any value or range between 180-260 mm / s, specifically from: 180 mm / s, 190 mm / s, 200 mm / s, 210 mm / s, 220 mm / s, 230 mm / s, 240 mm / s, 250 mm / s, 260 mm / s or any two of them.
[0095] More preferably, the substrate operates at a speed of 200 mm / s.
[0096] Preferably, the annealing temperature is selected from any value or range between 85-110℃, specifically from: 85℃, 90℃, 95℃, 100℃, 105℃, 110℃ or any two of them.
[0097] More preferably, the annealing temperature is 100°C.
[0098] Preferably, the annealing time is selected from any value or range between 5 and 12 minutes, specifically from: 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes or any two of them.
[0099] More preferably, the annealing time is 10 minutes.
[0100] Preferably, the transparent conductive substrate is rigid ITO glass or a flexible ITO-PET / ITO-PEN substrate.
[0101] More preferably, the transparent conductive substrate is ITO-PET.
[0102] Preferably, the electron transport layer is C 60 .
[0103] Preferably, the metal back electrode is a copper electrode.
[0104] Preferably, the effective area of a single module of the perovskite solar cell is 840 cm². 2 .
[0105] Secondly, the present invention provides a method for preparing the above-mentioned perovskite solar cell, comprising the following steps: (1) Preparation of transparent conductive substrate; (2) Preparation of nickel oxide hole transport layer; (3) Preparation of composite interface passivation layer; (4) Preparation of CsFAPbI3 perovskite layer; (5) Fabrication of an electron transport layer; (6) Prepare metal electrodes to obtain perovskite solar cells.
[0106] Preferably, the specific operation for preparing the transparent conductive substrate in step (1) is as follows: after P1 is scratched in PET / ITO, the substrate is sequentially cleaned by spraying, brushing, ultrasonic cleaning, two-fluid cleaning, spraying again, and air knife drying to obtain the transparent conductive substrate.
[0107] Preferably, the specific operation for preparing nickel oxide (NiOx) holes via transport in step (2) is as follows: S1. Prepare an organic solvent, stir, add a rheology modifier, stir again, add a wetting agent, and continue stirring to obtain the material; S2. Preparation of nickel salt basic solution: Add nickel salt to the material prepared in step S1 and stir to obtain nickel salt basic solution; S3. Binary composite doping agent doping modification: Cesium acetate and potassium formate are added sequentially to the nickel salt base solution prepared in step S2, stirred, allowed to stand, and filtered to obtain the precursor solution. S4. The nickel oxide hole transport layer is coated by wide-width ultrasonic atomization spraying using the precursor liquid prepared in step S3 to obtain the nickel oxide hole transport layer.
[0108] Preferably, the organic solvent in step S1 is a mixture of anhydrous ethanol and acetonitrile in a volume ratio of 7:3.
[0109] Preferably, the stirring operation in step S1 is as follows: stirring until a uniform and transparent mixed solvent system is obtained.
[0110] Preferably, the re-stirring time in step S1 is 5 minutes.
[0111] Preferably, the rheology modifier in step S1 is diethylene glycol methyl ether acetate.
[0112] Preferably, the wetting aid mentioned in step S1 is a fluorocarbon nonionic surfactant.
[0113] Preferably, the amount of rheology modifier added in step S1 is any value or range between 3% and 5% of the volume of the organic solvent, specifically selected from: 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5%, or any range between two of them.
[0114] More preferably, the amount of rheology modifier added in step S1 is 4% of the volume of the organic solvent.
[0115] Preferably, the amount of wetting agent added in step S1 is selected from any value or range between 0.01% and 0.05% of the nickel salt mass, specifically from: 0.01%, 0.02%, 0.03%, 0.04%, 0.05% or any two of them.
[0116] More preferably, the amount of wetting aid added in step S1 is 0.03% of the mass of the nickel salt.
[0117] Preferably, the nickel salt described in step S2 is nickel acetate tetrahydrate.
[0118] Preferably, the molar concentration of the nickel salt in step S2 is selected from any value or range between 0.35 and 0.45 mol / L, specifically from: 0.35 mol / L, 0.36 mol / L, 0.37 mol / L, 0.38 mol / L, 0.39 mol / L, 0.40 mol / L, 0.41 mol / L, 0.42 mol / L, 0.43 mol / L, 0.44 mol / L, 0.45 mol / L, or any range between two of them.
[0119] More preferably, the molar concentration of the nickel salt in step S2 is 0.4 mol / L.
[0120] Preferably, the stirring in step S2 is magnetic stirring.
[0121] Preferably, the magnetic stirring time is 30 minutes.
[0122] Preferably, the amount of cesium acetate added in step S3 is selected from any value or range between 1% and 6% of the amount of nickel salt, specifically from: 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6% or any two of them.
[0123] More preferably, the amount of cesium acetate added in step S3 is 2 mol of the amount of nickel salt.
[0124] Preferably, the amount of potassium formate added in step S3 is selected from any value or range between 1% and 8% of the amount of nickel salt, specifically from: 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8% or any two of them.
[0125] More preferably, the amount of potassium formate added in step S3 is 4 mol of the nickel salt substance.
[0126] Preferably, the molar ratio of cesium acetate to potassium formate is selected from any value or range between 1:1 and 3, specifically from: 1:1, 1:1.5, 1:1.7, 1:8, 1:2, 1:2.5, 1:3 or any two of them.
[0127] More preferably, the molar ratio of cesium acetate to potassium formate is 1:2.
[0128] Preferably, the stirring in step S3 is magnetic stirring.
[0129] Preferably, the magnetic stirring time is 2 hours.
[0130] Preferably, the stirring described in step S3 needs to be carried out in a dark environment at room temperature.
[0131] Preferably, the settling time in step S3 is 10 minutes.
[0132] Preferably, the mesh size of the filter in step S3 is 0.45 μm.
[0133] Preferably, the filtration in step S3 is negative pressure filtration, the purpose of which is to thoroughly remove trace amounts of undissolved impurities, tiny agglomerated particles and flocculent matter, ensuring that the precursor liquid is free of particles, sediment and suspended impurities.
[0134] Preferably, the preparation of the composite interface passivation layer in step (3) includes preparing a single layer of SAM and / or a passivation interface upper layer by wide-width ultrasonic atomization spraying.
[0135] Preferably, the preparation of the SAM monolayer is as follows: preparing a SAM monolayer solution and using the SAM monolayer solution for wide-width ultrasonic atomization spraying.
[0136] Preferably, the SAM monolayer solution is a [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz) solution.
[0137] Preferably, the SAM monolayer solution is prepared by dissolving Me-4PACz in anhydrous ethanol, stirring at room temperature in the dark for 4 hours, and the solution concentration is 0.5 mg / mL.
[0138] Preferably, the passivation interface upper layer is prepared by: preparing a passivation interface upper layer solution, and using the passivation interface upper layer solution for wide-width ultrasonic atomization spraying.
[0139] Preferably, the upper solution of the passivation interface is a phenylethyl ammonium iodide (PEAI) solution.
[0140] Preferably, the PEAI solution is prepared by dissolving PEAI in isopropanol, stirring at room temperature in the dark for 3 hours, resulting in a PEAI solution concentration of 2 mg / mL.
[0141] Preferably, the specific operation for preparing the CsFAPbI3 perovskite layer in step (4) is as follows: using CsFAPbI3 perovskite precursor liquid, a wide-width slit coating is formed, and annealing is performed at 135°C for 25 minutes to obtain a perovskite light-absorbing layer with a thickness of 650-750 nm.
[0142] More preferably, the specific operation for preparing the CsFAPbI3 perovskite layer in step (4) is as follows: a perovskite precursor solution composed of 10% CsPbI3 and 90% FAPbI3 is dissolved in a solvent of N,N-dimethylformamide (DMF):N-methylpyrrolidone (NMP) = 8:2 to obtain a Cs0.1FA0.9PbI3 perovskite layer solution, which is then coated with a wide-slit coating and annealed at 135°C for 25 min to obtain a perovskite light-absorbing layer with a thickness of 700 nm.
[0143] Preferably, the specific operation for preparing the electron transport layer in step (5) is as follows: vacuum thermal evaporation of C 60 The evaporation rate is 0.05-0.1 nm / s, and the film thickness is 22-28 nm; the BCP buffer layer is then deposited with a thickness of 6-8 nm.
[0144] More preferably, the specific operation for preparing the electron transport layer in step (5) is as follows: vacuum thermal evaporation of C 60The evaporation rate was 0.08 nm / s, and the film thickness was 25 nm; a BCP buffer layer with a thickness of 7 nm was then deposited.
[0145] Preferably, the specific operation for preparing the metal electrode in step (6) is: vacuum thermal evaporation of copper metal back electrode with a thickness of 90-110 nm.
[0146] More preferably, the specific operation for preparing the metal electrode in step (6) is: vacuum thermal evaporation of copper metal back electrode with a thickness of 100 nm.
[0147] Thirdly, the present invention provides the application of the above-mentioned perovskite solar cells in the field of photovoltaic power generation.
[0148] Based on further solutions to the technical problems of the present invention, or simultaneous solutions to multiple technical problems, the preferred solution in the technical solution provided in the first aspect of the present invention includes: The first priority solution is perovskite solar cells fabricated using a fully sprayed composite interface. This solution addresses the technical problem of poor interface compatibility in traditional slot spraying composite processes, and further solves the technical problem of uneven performance and insufficient stability of sub-cells in large-area modules.
[0149] The beneficial effects of this invention are as follows: 1. The perovskite solar cells prepared by this invention can avoid the defects of ultra-thin leakage and thick film poor light transmission. The consistency of large-area cell modules is greatly improved. The fully sprayed SAM+passivated double-layer composite interface solves the interface mismatch problem of spraying and slit mixing process, significantly reduces interface recombination loss, and improves the open circuit voltage and photoelectric conversion efficiency of the device simultaneously.
[0150] 2. Advantages of large-area modules: 400×400mm wide linear spraying forms a film in one pass, and the 840cm² module has uniform thickness and low performance dispersion; the full spraying process does not require equipment switching, is suitable for continuous mass production of flexible roll materials, and has significantly improved long-term light exposure stability, with significant industrialization advantages. Detailed Implementation
[0151] The following non-limiting embodiments are intended to enable those skilled in the art to gain a more comprehensive understanding of the present invention, but do not limit the invention in any way. The following content is merely an exemplary description of the scope of protection claimed by the present invention, and those skilled in the art can make various changes and modifications to the present invention based on the disclosed content, and such changes should also fall within the scope of protection claimed by the present invention.
[0152] The present invention will be further described below by way of specific embodiments. Unless otherwise specified, all instruments, devices, equipment, reagents, products, etc., used in the embodiments of the present invention are obtained through conventional commercial means.
[0153] Table 1
[0154] Example 1 (1) Preparation of transparent conductive substrate: After P1 is scratched in PET / ITO, the substrate is sequentially cleaned by spraying, brushing, ultrasonic cleaning, two-fluid cleaning, spraying, and air knife drying to obtain a transparent conductive substrate; (2) Preparation of nickel oxide hole transport layer: S1. Prepare 10 mL of organic solvent according to the volume ratio of anhydrous ethanol: acetonitrile = 7:3. After stirring until a homogeneous and transparent mixed solvent system is obtained, add diethylene glycol methyl ether acetate at a volume of 4% of the organic solvent. Stir for 5 min, then add fluorocarbon nonionic surfactant (the amount of fluorocarbon nonionic surfactant added is 0.03% of the mass of nickel salt) and continue stirring until the fluorocarbon nonionic surfactant is completely dispersed to obtain the material. S2. Preparation of nickel salt basic solution: Add nickel acetate tetrahydrate to the material prepared in step S1 and stir magnetically for 30 min at room temperature to obtain nickel acetate tetrahydrate basic solution, wherein the molar concentration of nickel acetate tetrahydrate is 0.4 mol / L. S3. Binary composite doping agent modification: Cesium acetate and potassium formate were added sequentially to the nickel acetate tetrahydrate base solution prepared in step S2 (the amount of cesium acetate added was 2% of the amount of nickel salt, the amount of potassium formate added was 4% of the amount of nickel salt, and the molar ratio of cesium acetate to potassium formate was 1:2). After stirring magnetically for 2 hours at room temperature in the dark, the solution was allowed to stand for 10 minutes to remove microbubbles. The solution was then filtered under negative pressure using a 0.45μm organic microporous filter membrane to thoroughly remove trace amounts of undissolved impurities, small agglomerates, and flocculents, ensuring that the precursor solution was free of particles, precipitates, and suspended impurities. The precursor solution was then sealed and stored at room temperature in the dark. S4. The nickel oxide hole transport layer is coated with the precursor solution prepared in step S3 using wide-width ultrasonic atomization spraying. The parameters for wide-width ultrasonic atomization spraying are as follows: Ultrasonic power: 35W; upper atomizing pressure: 0.18MPa, lower atomizing pressure: 0.15MPa; carrier gas pressure: 0.2MPa; feed flow rate: 2.2mL / min; nozzle liquid slit opening: 0.12mm, nozzle-substrate distance: 45mm; substrate running speed: 220mm / s; pre-annealing at 80℃ for 5min (to remove surface solvent), followed by high-temperature annealing at 140℃ for 20min; then naturally cooled to room temperature to obtain a nickel oxide hole transport layer with a thickness of 20nm. (3) Preparation of composite interface passivation layer: SAM monolayers were prepared using wide-width ultrasonic atomization spraying, specifically as follows: Preparation of SAM monolayer solution: Dissolve 10 mg of Me-PACz in 20 mL of anhydrous ethanol, stir at room temperature in the dark for 4 h to obtain a SAM monolayer solution with a concentration of 0.5 mg / mL; Wide-width ultrasonic atomization spraying was performed using a SAM monolayer solution. The specific parameters for wide-width ultrasonic atomization spraying were as follows: ultrasonic power was reduced to 22W (low power avoids single-molecule breakage); upper atomization pressure: 0.12MPa; lower atomization pressure: 0.10MPa; feed flow rate: 0.8mL / min; liquid slit opening: 0.12mm; nozzle-substrate spacing was increased to 55mm to extend the droplet pre-evaporation path in the air; substrate running speed: 220mm / s; annealing at 100℃ for 10min yielded a SAM monolayer with a thickness of 1.5nm. The passivation interface upper layer is prepared by wide-width ultrasonic atomization spraying, specifically as follows: Preparation of passivation interface upper layer solution: Dissolve 40 mg of PEAI in 20 mL of isopropanol, stir at room temperature in the dark for 3 h to obtain a passivation interface upper layer solution with a concentration of 2 mg / mL. Wide-width ultrasonic atomization spraying was performed using a passivation interface upper layer solution. The specific parameters for wide-width ultrasonic atomization spraying were as follows: ultrasonic power: 28W; upper atomization pressure: 0.14MPa, lower atomization pressure: 0.12MPa; feed flow rate: 1.0mL / min; nozzle liquid slit opening: 0.12mm; nozzle-to-substrate distance: 50mm; substrate running speed: 220mm / s; annealing at 100℃ for 10min; and natural cooling to room temperature to obtain a passivation interface upper layer with a thickness of 2.5nm. (4) Cs 0.1 FA 0.9 Preparation of PbI3 perovskite layer: Formulating Cs 0.1 FA 0.9 PbI3 perovskite precursor solution: A perovskite precursor solution consisting of 10% CsPbI3 and 90% FAPbI3 was dissolved in a solvent of N,N-dimethylformamide (DMF):N-methylpyrrolidone (NMP) = 8:2 to obtain CsPbI3. 0.1 FA 0.9 PbI3 perovskite layer solution; A perovskite light-absorbing layer with a thickness of 700 nm was obtained by wide-slit coating and annealing at 135℃ for 25 min. (5) Preparation of electron transport layer: vacuum thermal evaporation of C 60 The evaporation rate was 0.08 nm / s, and the film thickness was 25 nm; a BCP buffer layer with a thickness of 7 nm was then deposited. (6) Preparation of metal electrodes: Vacuum thermal evaporation of copper metal back electrode with a thickness of 100 nm to obtain flexible perovskite solar cell.
[0155] Example 2 The only difference from Example 1 is that the method for preparing the upper passivation interface layer in step (3) of the composite interface passivation layer is changed, specifically: (3) Preparation of composite interface passivation layer: The passivation interface upper layer was prepared by slit coating. Specifically, the passivation interface upper layer solution was deposited on the perovskite active layer by slit coating at a coating speed of 10 mm / s, a liquid injection speed of 10 μL / s, and a gap of 100 μm. The passivation interface upper layer was obtained by annealing at 95℃ for 8 min. The remaining dosages and steps are the same as in Example 1.
[0156] Example 3 The only difference from Example 1 is that the preparation method of the SAM monolayer in the composite interface passivation layer in step (3) is changed, specifically: (3) Preparation of composite interface passivation layer: SAM monolayers were prepared using slits, specifically as follows: SAM monolayer solution was deposited on NiOx transport layer by slit coating at a coating speed of 5 mm / s, a liquid injection speed of 8 μL / s, and a gap of 100 μm; annealing at 100 °C for 10 min yielded SAM monolayer. The remaining dosages and steps are the same as in Example 1.
[0157] Example 4 The only difference from Example 1 is that the method of preparing the S4 wide-width ultrasonic atomization spraying in step (2) of the nickel oxide hole transport layer is changed, specifically: S4. The nickel oxide hole transport layer is coated with the precursor solution prepared in step S3 using wide-width ultrasonic atomization spraying. The parameters for wide-width ultrasonic atomization spraying are as follows: Ultrasonic power: 28W; upper atomizing pressure: 0.14MPa, lower atomizing pressure: 0.12MPa; carrier gas pressure: 0.2MPa; feed flow rate: 1.6mL / min; nozzle liquid slit opening: 0.12mm, nozzle-substrate distance: 45mm; substrate running speed: 240mm / s; pre-annealing at 80℃ for 5min (to remove surface solvent), followed by high-temperature annealing at 140℃ for 20min; then naturally cooled to room temperature to obtain a nickel oxide hole transport layer with a thickness of 10nm. The remaining dosages and steps are the same as in Example 1.
[0158] Example 5 The only difference from Example 1 is that the method of preparing the S4 wide-width ultrasonic atomization spraying in step (2) of the nickel oxide hole transport layer is changed, specifically: S4. The nickel oxide hole transport layer is coated with the precursor solution prepared in step S3 using wide-width ultrasonic atomization spraying. The parameters for wide-width ultrasonic atomization spraying are as follows: Ultrasonic power: 38W; upper atomizing pressure: 0.20MPa, lower atomizing pressure: 0.17MPa; carrier gas pressure: 0.2MPa; feed flow rate: 2.6mL / min; nozzle liquid slit opening: 0.12mm; nozzle-to-substrate distance: 45mm; substrate running speed: 200mm / s; pre-annealing at 80℃ for 5min, followed by high-temperature annealing at 140℃ for 20min; then naturally cooled to room temperature to obtain a nickel oxide hole transport layer with a thickness of 30nm. The remaining dosages and steps are the same as in Example 1.
[0159] Example 6 The only difference from Example 1 is that the method of preparing the S4 wide-width ultrasonic atomization spraying in step (2) of the nickel oxide hole transport layer is changed, specifically: S4. The nickel oxide hole transport layer is coated with the precursor solution prepared in step S3 using wide-width ultrasonic atomization spraying. The parameters for wide-width ultrasonic atomization spraying are as follows: Ultrasonic power: 42W; upper atomizing pressure: 0.21MPa, lower atomizing pressure: 0.18MPa; carrier gas pressure: 0.2MPa; feed flow rate: 2.9mL / min; nozzle liquid slit opening: 0.12mm; nozzle-to-substrate distance: 45mm; substrate running speed: 185mm / s; pre-annealing at 80℃ for 5min, followed by high-temperature annealing at 140℃ for 20min; then naturally cooled to room temperature to obtain a nickel oxide hole transport layer with a thickness of 45nm. The remaining dosages and steps are the same as in Example 1.
[0160] Example 7 The only difference from Example 1 is that the wide-width ultrasonic atomization spraying parameters in step (3) of the composite interface passivation layer are changed, specifically: Wide-width ultrasonic atomization spraying was performed using a SAM monolayer solution. The specific parameters for wide-width ultrasonic atomization spraying were as follows: ultrasonic power was reduced to 18W (low power avoids single-molecule breakage); upper atomization pressure: 0.08MPa; lower atomization pressure: 0.07MPa; feed flow rate: 0.5mL / min; liquid slit opening: 0.10mm; nozzle-substrate spacing was increased to 65mm to extend the droplet pre-evaporation path in the air; substrate running speed: 260mm / s; annealing at 100℃ for 10min yielded a SAM monolayer with a thickness of 0.75nm. Wide-width ultrasonic atomization spraying was performed using a passivation interface upper layer solution. The specific parameters for wide-width ultrasonic atomization spraying were as follows: ultrasonic power: 22W; upper atomization pressure: 0.10MPa, lower atomization pressure: 0.08MPa; feed flow rate: 0.7mL / min; nozzle liquid slit opening: 0.10mm; nozzle-to-substrate distance: 60mm; substrate running speed: 260mm / s; annealing at 100℃ for 10min; and natural cooling to room temperature to obtain a passivation interface upper layer with a thickness of 1.5nm. The remaining dosages and steps are the same as in Example 1.
[0161] Example 8 The only difference from Example 1 is that the wide-width ultrasonic atomization spraying parameters in step (3) of the composite interface passivation layer are changed, specifically: Wide-width ultrasonic atomization spraying was performed using a SAM monolayer solution. The specific parameters for wide-width ultrasonic atomization spraying were as follows: ultrasonic power was reduced to 26W (low power avoids single-molecule breakage); upper atomization pressure: 0.15MPa; lower atomization pressure: 0.13MPa; feed flow rate: 1.2mL / min; liquid slit opening: 0.15mm; nozzle-substrate spacing was increased to 50mm to extend the droplet pre-evaporation path in the air; substrate running speed: 180mm / s; annealing at 100℃ for 10min yielded a SAM monolayer with a thickness of 2.5nm. Wide-width ultrasonic atomization spraying was performed using a passivation interface upper layer solution. The specific parameters for wide-width ultrasonic atomization spraying were as follows: ultrasonic power: 34W; upper atomization pressure: 0.18MPa, lower atomization pressure: 0.15MPa; feed flow rate: 1.5mL / min; nozzle liquid slit opening: 0.15mm; nozzle-to-substrate distance: 40mm; substrate running speed: 180mm / s; annealing at 100℃ for 10min; and natural cooling to room temperature to obtain a passivation interface upper layer with a thickness of 4.5nm. The remaining dosages and steps are the same as in Example 1.
[0162] Example 9 The only difference from Example 1 is that the method of preparing the S4 wide-width ultrasonic atomization spraying in step (2) of the nickel oxide hole transport layer is changed, specifically: S4. The nickel oxide hole transport layer is coated with the precursor solution prepared in step S3 using wide-width ultrasonic atomization spraying. The parameters for wide-width ultrasonic atomization spraying are as follows: Ultrasonic power: 22W; upper atomizing pressure: 0.18MPa, lower atomizing pressure: 0.15MPa; carrier gas pressure: 0.2MPa; feed flow rate: 2.2mL / min; nozzle liquid slit opening: 0.12mm; nozzle-to-substrate distance: 45mm; substrate running speed: 220mm / s; pre-annealing at 80℃ for 5min (to remove surface solvent), followed by high-temperature annealing at 140℃ for 20min; then naturally cooled to room temperature to obtain a nickel oxide hole transport layer with a thickness of 5nm. The remaining dosages and steps are the same as in Example 1.
[0163] Comparative Example 1 Perovskite solar cells were prepared according to Example 1 of CN121888855A.
[0164] Comparative Example 2 The only difference from Example 1 is that the preparation method of the SAM monolayer in the composite interface passivation layer in step (3) is changed, specifically: SAM monolayers were prepared using a slit coating method with a SAM monolayer solution. The specific parameters for the slit coating method were: slit die gap of 100 μm, feed flow rate of 1.2 mL / min, substrate travel speed of 80 mm / s, and annealing at 100 °C for 10 min. The remaining dosages and steps are the same as in Example 1.
[0165] Comparative Example 3 The only difference from Example 1 is that the preparation method of the passivation interface upper layer in step (3) of the composite interface passivation layer is changed, specifically: The passivation interface upper layer was prepared by slit coating method using a passivation interface upper layer solution. The specific parameters of the slit coating method were: slit head gap of 50 μm, feed flow rate of 1.0 mL / min, substrate speed of 80 mm / s, and annealing at 100℃ for 10 min. The remaining dosages and steps are the same as in Example 1.
[0166] Comparative Example 4 The only difference from Example 1 is that the preparation method of the composite interface passivation layer in step (3) is changed, specifically: (3) Preparation of composite interface passivation layer: Preparation of SAM monolayer solution: Dissolve 10 mg of Me-PACz in 20 mL of anhydrous ethanol, stir at room temperature in the dark for 4 h to obtain a SAM monolayer solution with a concentration of 0.5 mg / mL; SAM monolayers were prepared using a slit coating method with a SAM monolayer solution. The specific parameters for the slit coating method were: slit die gap of 100 μm, feed flow rate of 1.2 mL / min, substrate travel speed of 80 mm / s, and annealing at 100 °C for 10 min. Preparation of passivation interface upper layer solution: Dissolve 40 mg of PEAI in 20 mL of isopropanol, stir at room temperature in the dark for 3 h to obtain a passivation interface upper layer solution with a concentration of 2 mg / mL. The passivation interface upper layer was prepared by slit coating method using a passivation interface upper layer solution. The specific parameters of the slit coating method were: slit head gap of 50 μm, feed flow rate of 1.0 mL / min, substrate speed of 80 mm / s, and annealing at 100℃ for 10 min. The remaining dosages and steps are the same as in Example 1.
[0167] Comparative Example 5 The only difference from Example 1 is that the method of preparing the S4 wide-width ultrasonic atomization spraying in step (2) of the nickel oxide hole transport layer is changed, specifically: S4. The nickel oxide hole transport layer is coated with the precursor solution prepared in step S3 using wide-width ultrasonic atomization spraying. The parameters for wide-width ultrasonic atomization spraying are as follows: Ultrasonic power: 45W; upper atomizing pressure: 0.22MPa, lower atomizing pressure: 0.19MPa; feed flow rate: 3.0mL / min; nozzle liquid slit opening: 0.12mm; nozzle-to-substrate distance: 45mm; substrate running speed: 175mm / s; pre-annealing at 80℃ for 5min, followed by high-temperature annealing at 140℃ for 20min; then naturally cooled to room temperature to obtain a nickel oxide hole transport layer with a thickness of 50nm. The remaining dosages and steps are the same as in Example 1.
[0168] Comparative Example 6 The only difference from Example 1 is that the ultrasonic power of the wide-width ultrasonic atomization spraying in step S4 is changed to 20W, specifically: S4. The nickel oxide hole transport layer is coated with the precursor solution prepared in step S3 using wide-width ultrasonic atomization spraying. The parameters for wide-width ultrasonic atomization spraying are as follows: Ultrasonic power: 20W; upper atomizing pressure: 0.18MPa, lower atomizing pressure: 0.15MPa; feed flow rate: 2.2mL / min; nozzle liquid slit opening: 0.12mm; nozzle-to-substrate distance: 45mm; substrate running speed: 220mm / s; pre-annealing at 80℃ for 5min (to remove surface solvent), followed by high-temperature annealing at 140℃ for 20min; then naturally cooled to room temperature to obtain a nickel oxide hole transport layer with a thickness of 7nm. The remaining dosages and steps are the same as in Example 1.
[0169] Comparative Example 7 The only difference from Example 1 is that the feed flow rate of the wide-width ultrasonic atomization spraying in step S4 is changed to 1 mL / min, specifically: S4. The nickel oxide hole transport layer is coated with the precursor solution prepared in step S3 using wide-width ultrasonic atomization spraying. The parameters for wide-width ultrasonic atomization spraying are as follows: Ultrasonic power: 35W; upper atomizing pressure: 0.18MPa, lower atomizing pressure: 0.15MPa; carrier gas pressure: 0.2MPa; feed flow rate: 1mL / min; nozzle liquid slit opening: 0.12mm, nozzle-to-substrate distance: 45mm; substrate running speed: 220mm / s; pre-annealing at 80℃ for 5min (to remove surface solvent), followed by high-temperature annealing at 140℃ for 20min; then naturally cooled to room temperature to obtain a nickel oxide hole transport layer with a thickness of 3nm. The remaining dosages and steps are the same as in Example 1.
[0170] Comparative Example 8 The only difference from Example 1 is that the distance between the nozzle and the substrate in step S4, wide-width ultrasonic atomization spraying, is changed to 70mm. Specifically: S4. The nickel oxide hole transport layer is coated with the precursor solution prepared in step S3 using wide-width ultrasonic atomization spraying. The parameters for wide-width ultrasonic atomization spraying are as follows: Ultrasonic power: 35W; upper atomizing pressure: 0.18MPa, lower atomizing pressure: 0.15MPa; carrier gas pressure: 0.2MPa; feed flow rate: 2.2mL / min; nozzle liquid slit opening: 0.12mm, nozzle-substrate distance: 70mm; substrate running speed: 220mm / s; pre-annealing at 80℃ for 5min (to remove surface solvent), followed by high-temperature annealing at 140℃ for 20min; then naturally cooled to room temperature to obtain a nickel oxide hole transport layer with a thickness of 9nm. The remaining dosages and steps are the same as in Example 1.
[0171] Detection Example 1 1. Experimental Methods A transport layer and a perovskite layer were prepared by atomization spraying to produce a single piece with an area of 35 mm. 35cm 2 Flexible components, 35 35cm 2 The aperture area of the component is 840 cm². 2 By simulating strong outdoor light, the photoelectric conversion efficiency of the prepared perovskite solar cells was tested using an AAA-level steady-state solar simulator (AM1.5G, light spot ≥35cm×35cm). The test indicators included 1500h photoelectric conversion efficiency, open circuit voltage, short circuit current, and fill factor.
[0172] Photoelectric conversion efficiency over 1500 hours = (illuminance measured after 1000 hours of continuous illumination / initial illumination efficiency) × 100%.
[0173] 2. Experimental Results The perovskite solar cells prepared in Examples 1-9 all had a light efficiency retention rate of over 76% after 1500 hours of illumination, and their performance was better than that of the perovskite solar cells prepared in Comparative Examples 1-8.
[0174] In Example 1, a three-layer thin film was deposited stepwise using a 400mm wide-width spraying equipment. A 20nm dense NiOx substrate was used, and SAM (Surface Atomizing Agent) was sprayed onto the NiOx substrate to regulate the interface energy levels. A passivation layer was sprayed onto the perovskite surface to passivate perovskite defects. The synergistic effect of the two layers minimized non-radiative recombination at the interface, resulting in highly uniform performance and optimal light-induced stability in the 840cm² module battery.
[0175] Table 2
[0176] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, and is not intended to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions made by those skilled in the art to the technical solution of the present invention do not depart from the essence and scope of the technical solution of the present invention.
Claims
1. A perovskite solar cell, characterized in that, From bottom to top, it includes a transparent conductive substrate, a nickel oxide hole transport layer, a composite interface passivation layer, a CsFAPbI3 perovskite layer, an electron transport layer, and a metal back electrode. The nickel oxide hole transport layer is prepared using a wide-width ultrasonic atomization spraying process; The specific parameters of the wide-width ultrasonic atomization spraying process for the nickel oxide hole transport layer are as follows: The ultrasonic power is 22-45W; the upper atomizing pressure is 0.14-0.22MPa, and the lower atomizing pressure is 0.12-0.19MPa; the carrier gas pressure is 0.2-0.6MPa; the feed flow rate is 1.5-3.0mL / min; the nozzle liquid slit opening is 0.10-0.15mm, and the distance between the nozzle and the substrate is 35-55mm; the substrate running speed is 180-260mm / s; pre-anneal at 70-90℃ for 3-8min, followed by high-temperature annealing at 120-160℃ for 15-25min; and then allow to cool naturally to room temperature. The composite interface passivation layer is prepared using a wide-width ultrasonic atomization spraying process, and the composite interface passivation layer includes a SAM monolayer and a passivation interface upper layer. The specific parameters of the aforementioned SAM single-layer wide-width ultrasonic atomization spraying process are as follows: The ultrasonic power was reduced to 18-26W; the upper atomizing gas pressure was 0.08-0.15MPa; the lower atomizing gas pressure was 0.07-0.13MPa; the feed flow rate was 0.5-1.2mL / min; the liquid slit opening was 0.10-0.15mm; the nozzle-substrate spacing was increased to 50-65mm; the substrate running speed was 180-260mm / s; and annealing was performed at 85-110℃ for 5-15min. The specific parameters of the wide-width ultrasonic atomization spraying process on the upper layer of the passivation interface are as follows: The ultrasonic power is 22-34W; the upper atomizing pressure is 0.10-0.18MPa; the lower atomizing pressure is 0.08-0.15MPa; the feed flow rate is 0.7-1.5mL / min; the liquid slit opening is 0.10-0.15mm; the nozzle-substrate spacing is 40-60mm; the substrate running speed is 180-260mm / s; and annealing is carried out at 85-110℃ for 5-12min.
2. The perovskite solar cell according to claim 1, characterized in that, The thickness of the nickel oxide hole transport layer is 5-45 nm.
3. The perovskite solar cell according to claim 1, characterized in that, The thickness of the nickel oxide hole transport layer is 20 nm.
4. The perovskite solar cell according to claim 1, characterized in that, The transparent conductive substrate is a rigid ITO glass or a flexible ITO-PET / ITO-PEN substrate.
5. The perovskite solar cell according to claim 1, characterized in that, The electron transport layer is C 60 The metal back electrode is a copper electrode.
6. The perovskite solar cell according to claim 1, characterized in that, The effective area of a single module of the perovskite solar cell is 840 cm². 2 .
7. The method for preparing a perovskite solar cell according to any one of claims 1-6, characterized in that, Includes the following steps: (1) Preparation of transparent conductive substrate; (2) Preparation of nickel oxide hole transport layer; (3) Preparation of composite interface passivation layer; (4) Preparation of CsFAPbI3 perovskite layer; (5) Fabrication of an electron transport layer; (6) Prepare metal electrodes to obtain perovskite solar cells.
8. The preparation method according to claim 7, characterized in that, The specific operation for preparing the nickel oxide hole transport layer in step (2) is as follows: S1. Prepare an organic solvent, stir, add a rheology modifier, stir again, add a wetting agent, and continue stirring to obtain the material; S2. Preparation of nickel salt basic solution: Add nickel salt to the material prepared in step S1 and stir to obtain nickel salt basic solution; S3. Binary composite doping agent doping modification: Cesium acetate and potassium formate are added sequentially to the nickel salt base solution prepared in step S2, stirred, allowed to stand, and filtered to obtain the precursor solution. S4. The nickel oxide hole transport layer is coated by wide-width ultrasonic atomization spraying using the precursor liquid prepared in step S3 to obtain the nickel oxide hole transport layer.
9. The preparation method according to claim 7, characterized in that, Step (3) involves preparing a composite interface passivation layer by using wide-width ultrasonic atomization spraying to prepare a single layer of SAM and a passivation interface upper layer. The preparation of the SAM monolayer is as follows: a SAM monolayer solution is prepared, and the SAM monolayer solution is used for wide-width ultrasonic atomization spraying. The passivation interface upper layer is prepared by: preparing a passivation interface upper layer solution, and using the passivation interface upper layer solution for wide-width ultrasonic atomization spraying.
10. The application of the perovskite solar cell according to any one of claims 1-6 in the field of photovoltaic power generation.
Citation Information
Patent Citations
Perovskite light-emitting diode based on spraying process and preparation method of light-emitting diode
CN108417739A
Method for preparing perovskite solar cell hole transport layer based on digital spraying method
CN121888855A