Solar cells and their preparation methods

By introducing a self-assembled monomolecule material layer on the surface of NiOx thin film, the surface defect problem of NiOx thin film is solved, the NiOx/perovskite interface contact is optimized, charge transfer and hole transport are promoted, and the photoelectric conversion efficiency of perovskite solar cells is improved.

CN123124577APending Publication Date: 2026-11-17CHINT NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611591687.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the prior art, the high surface defect density of NiOx thin films leads to poor contact quality at the NiOx/perovskite interface, hindering hole extraction and charge transfer, increasing charge transport resistance, and causing severe non-radiative recombination effects, which limits the photoelectric conversion efficiency of perovskite solar cells.

Method used

A self-assembled monomolecular material layer is introduced on the surface of NiOx thin film. The self-assembled monomolecular material has a D-π-A structure, which forms stable covalent bonds through anchoring groups, reduces surface defects, and promotes charge transfer and hole transport by optimizing interfacial contact through molecular structure.

Benefits of technology

It significantly reduced nonradiative recombination at the NiOx/perovskite interface, reduced defects in the perovskite light-absorbing layer, improved photoelectric conversion efficiency, and increased open-circuit voltage, short-circuit current density, and fill factor, achieving a photoelectric conversion efficiency of over 23.72%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124577A_ABST
    Figure CN123124577A_ABST
Patent Text Reader

Abstract

This application discloses a solar cell and its fabrication method. In the composite hole transport layer of the solar cell described in this application, the introduction of self-assembled monomolecule materials can reduce surface defects in the nickel oxide layer and promote charge transfer, while also reducing the NiO content. x Non-radiative recombination at the perovskite interface significantly reduces defects in the perovskite light-absorbing layer, thereby improving device efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of solar cell technology, and more specifically, to a solar cell and a method for its fabrication. Background Technology

[0002] With the rapid development of photovoltaic technology, perovskite solar cells, with their outstanding advantages such as simple fabrication process, low production cost, high light absorption coefficient, and excellent carrier mobility, have become a core research direction for next-generation photovoltaic devices, and have broad application prospects in flexible photovoltaics, distributed power generation, and other fields. After years of technological iteration, the photoelectric conversion efficiency of perovskite solar cells has been significantly improved, and they are gradually showing potential for industrial application. As the core functional layer of perovskite solar cells, the hole transport layer plays a crucial role in extracting and transporting photogenerated holes, blocking electrons, and suppressing carrier recombination. Its interface characteristics, thin film quality, and band structure directly determine the photoelectric conversion efficiency and long-term operational stability of the device, and are one of the core key factors restricting the development of high-performance perovskite solar cells.

[0003] Among numerous hole transport materials, nickel oxide (NiO) x NiO₂, as a typical inorganic p-type semiconductor material, possesses excellent light transmittance, high hole mobility, good chemical stability, excellent energy level matching, and high compatibility with fabrication processes. It is widely used in inverted perovskite solar cells. Compared to organic hole transport materials, it also has advantages such as low cost, strong weather resistance, and ease of failure without doping. However, in existing technologies, NiO₂ obtained through conventional fabrication processes... x Thin films generally suffer from high surface defect density. The surface of thin films contains a large number of intrinsic defects such as coordination unsaturated nickel sites and oxygen vacancies. These surface defects can form a large number of carrier trap energy levels, which become active centers for photogenerated carrier recombination.

[0004] Specifically, NiO x Surface defects in the layer can severely damage NiO. x The quality of the interfacial contact between the perovskite light-absorbing layer and the perovskite layer will, on the one hand, hinder hole extraction and charge transfer processes at the interface, increasing charge transport resistance and preventing effective separation and transport of photogenerated carriers; on the other hand, it will significantly exacerbate the NiO… x Nonradiative recombination at the perovskite heterojunction interface is a trap-assisted form of carrier loss in devices. Its recombination rate is much higher than bulk recombination and direct radiative recombination, causing severe open-circuit voltage loss and photocurrent loss. Meanwhile, NiO... xSurface defects on the substrate can further affect the crystal growth behavior of the upper perovskite film, inducing secondary defects such as grain boundary defects and vacancy defects in the perovskite light-absorbing layer. This further exacerbates carrier recombination losses, greatly limiting the further improvement of the photoelectric conversion efficiency of perovskite solar cells, and becoming a constraint on NiO. x The core technological bottleneck for achieving high performance in perovskite solar cells. Summary of the Invention

[0005] This application provides a solar cell and its fabrication method. In the composite hole transport layer of the solar cell described in this application, the introduction of self-assembled monomolecule materials can reduce surface defects in the nickel oxide layer and promote charge transfer, while also reducing the NiO content. x Non-radiative recombination at the perovskite interface significantly reduces defects in the perovskite light-absorbing layer, thereby improving device efficiency.

[0006] In a first aspect, a solar cell is provided, comprising a transparent conductive glass, a composite hole transport layer, a perovskite light-absorbing layer, an electron transport layer, and a back electrode stacked sequentially, wherein the composite hole transport layer comprises a nickel oxide layer and a self-assembled monomolecule material layer, and the self-assembled monomolecule material layer comprises a structure of the self-assembled monomolecule material having the following structural formula: and / or R includes any one or a combination of at least two of carboxyl groups, sulfonic acid groups, phosphonic acid groups, or boric acid groups, and the self-assembled monomolecular material layer of the composite hole transport layer is disposed on the side close to the perovskite light-absorbing layer.

[0007] In the composite hole transport layer of the solar cell provided in this application embodiment, the self-assembled monomolecule material has a D-π-A (donor-π-bridge-acceptor) molecular structure, which contains electron-withdrawing chalcone units and electron-donating groups. An anchoring group (carboxyl group) at one end of the self-assembled monomolecule material can anchor to NiO. x Strong and stable covalent bonds are formed on the thin film surface, enabling selective contact to mitigate interfacial recombination and reduce NiO. x Thin film surface defects; meanwhile, the carbazole group and / or triphenylamine unit at the other end of the molecule have strong hole transport capabilities. The planarized molecular structure and enhanced π-π stacking can further improve hole mobility.

[0008] In some embodiments, R is -(CH2). n -COOH, where n is an integer from 0 to 3.

[0009] In some embodiments, the thickness of the nickel oxide layer is 10 nm to 20 nm.

[0010] In some embodiments, the thickness of the self-assembled monomolecular material layer is 1 nm to 3 nm.

[0011] In some embodiments, the material of the perovskite light-absorbing layer includes ABX3, wherein A includes CH3NH3. + CH(NH2)2 + Cs + or Rb + B includes any one or at least two of the following, where B includes Pb. 2+ Sn 2+ Or Ge 2+ X includes any one or at least two of the following, X including Cl - ,Br - Or I - Any one or at least two of them.

[0012] In some embodiments, the thickness of the perovskite light-absorbing layer is 200 nm to 900 nm.

[0013] In some embodiments, the material of the electron transport layer includes C 60 Any one or at least two of the following: PCBM, TiO2, SnO2, ZnO, or ZnO-ZnS.

[0014] In some embodiments, the back electrode material includes any one or a combination of at least two of Au, Ag, Al, Cu, or carbon.

[0015] In a second aspect, a method for preparing a solar cell as described in the first aspect is provided, the method comprising the following steps: Depositing a nickel oxide layer on transparent conductive glass; The self-assembled monomolecule material is dispersed in a solvent to obtain a self-assembled monomolecule material solution. The self-assembled monomolecule material solution is coated on a nickel oxide layer and then annealed to obtain a composite hole transport layer. The solar cell is obtained by sequentially fabricating a perovskite light-absorbing layer, an electron transport layer, and a back electrode on the surface of the composite hole transport layer.

[0016] In this embodiment, a self-assembled monomolecular material solution is coated onto a nickel oxide layer. The self-assembled monomolecular material is uniformly distributed on the nickel oxide layer. The self-assembled monomolecular material layer can be obtained after simple annealing. The thickness of the self-assembled monomolecular material layer can be controlled by the concentration of the self-assembled monomolecular material solution.

[0017] In some embodiments, the solvent includes any one or a combination of at least two of isopropanol, ethanol, or DMF.

[0018] In some embodiments, the mass concentration of the self-assembled monomolecular material solution is 0.2 mg / mL to 1.2 mg / mL.

[0019] In some embodiments, the annealing temperature is 80°C to 120°C.

[0020] In some embodiments, the annealing process takes 5 to 15 minutes.

[0021] In the solar cell provided in this application embodiment, the anchoring groups in the self-assembled molecular structure of the composite hole transport layer are anchored to NiO. x Strong and stable covalent bonds are formed on the surface of the thin film, enabling selective contact to reduce surface defects and promote charge transfer in NiO. x The large number of charge carriers accumulated at the perovskite interface are highly selectively extracted through self-assembled molecular layers, reducing nonradiative recombination at the interface. Simultaneously, the carboxyl groups at the other end of the molecule can interact with uncoordinated Pb on the perovskite surface. 2+ This combination significantly reduces defects in the perovskite light-absorbing layer, thereby improving device efficiency. Attached Figure Description

[0022] Figure 1 This is a comparison chart of the JV curves of the perovskite solar cells described in Example 1 and Comparative Example 1.

[0023] Figure 2 The images show a comparison of the fluorescence lifetime of the perovskite thin film in the perovskite solar cells described in Example 1 and Comparative Example 1. Detailed Implementation

[0024] The descriptions of specific structures or functions implemented according to the concept of this application disclosed in this specification are merely illustrative examples for explaining embodiments based on the concept of this application. Those skilled in the art will understand that embodiments based on the concept of this application can have various variations and forms, and are not limited to the embodiments described in this specification, but also include various modifications, equivalents, or substitutions made within the scope of the purpose, concept, and technology of this application.

[0025] In the description of this application, it should be understood that the use of terms such as "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", "axial", "radial", and "circumferential" indicates the relative orientation or positional relationship between different components, and is only for the convenience of describing this application and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.

[0026] Although the terms "first" or "second" may be used to describe various components or components, the components or components should not be limited by the terms. The terms above are used only for the purpose of distinguishing one component or component from another. For example, without departing from the scope of the claims according to the concept of this application, a first battery cell may be referred to as a second battery cell, and similarly, a second battery cell may be referred to as a first battery cell.

[0027] In this application, unless otherwise expressly specified and limited, the terms "connected," "fixed," "set," etc., should be interpreted broadly. For example, when one component is said to "connect" another component, it should be understood that it can be directly or indirectly connected to the other component, meaning that other components may also be present in between. Similarly, the terms "fixed" and "set" should be interpreted broadly in a similar way. Furthermore, the term "connected" can refer to a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can refer to the internal communication of two components or the interaction between two components, unless otherwise expressly limited. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances. In this application, unless otherwise expressly specified and limited, the description of "above" or "below" the second feature can mean that the first and second features are in direct contact, or that the first and second features are in indirect contact through an intermediate medium. Moreover, "above," "on top of," and "over" the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. The first feature being "below", "under", or "below" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.

[0028] To make the above-mentioned objectives, features and advantages of this application more apparent and understandable, the specific embodiments of this application will be described in detail below with reference to the accompanying drawings.

[0029] This application provides a photovoltaic system that can be used in photovoltaic power plants, such as ground-mounted power plants, rooftop power plants, and water-based power plants, as well as in equipment or devices that use solar energy to generate electricity, such as user solar power supplies, solar streetlights, solar cars, and solar buildings.

[0030] It is understandable that the application scenarios of photovoltaic (PV) systems are not limited to this; that is to say, PV systems can be applied in all fields that require solar energy for power generation. Taking a PV power generation system as an example, a PV system can include a PV array, a combiner box, and an inverter. The PV array can be an array combination of multiple PV modules; for example, multiple PV modules can form multiple PV arrays. The PV array is connected to the combiner box, which can collect the current generated by the PV array. The collected current flows through the inverter and is converted into AC power required by the mains power grid before being connected to the mains power grid to realize solar power supply.

[0031] A photovoltaic (PV) module is a device that directly converts light energy into electrical energy through the photoelectric effect or photochemical effect. A PV module typically has a stacked encapsulation structure, comprising at least the following from the light-facing side to the back-light-facing side: a front cover, a first encapsulating film, a cell string layer, a second encapsulating film, and a back cover, as well as a frame surrounding the stacked structure and a junction box located on one side of the back cover.

[0032] The front cover can be made of a material with excellent light transmittance, impact resistance, corrosion resistance, and weather resistance, and may optionally include at least one of the following materials: tempered glass, plexiglass, transparent ceramics, organic fibers, or polymers. In some embodiments, the front cover may include at least one of an insulating barrier layer, a fluorinated weather-resistant layer, and a transition adhesive layer.

[0033] Back cover plates typically need to possess insulation, water resistance, aging resistance, weather resistance, and corrosion resistance. They can optionally include at least one of the following composite back covers as the substrate: tempered glass, acrylic glass, metal back cover, or PET film. The PET-based composite back cover can be selected from various types, such as composite (e.g., TPT / KPK, TPE / KPE), coated (e.g., TPC, KPC, CPC), and co-extruded (e.g., PO), depending on the needs of different scenarios.

[0034] Understandably, the choice of materials for the front cover and the back cover does not affect each other, and the same or different materials can be selected depending on the different application scenarios of the components (such as residential photovoltaics and building-integrated photovoltaics).

[0035] The first and second encapsulating films can be selected from at least one of ethylene-vinyl acetate copolymer (EVA) film, polyvinyl octene coelastomer (POE) film, EVA-POE-EVA co-extruded film (EPE), PVB (polyvinyl butyral), polyethylene terephthalate (PET) film, or liquid silicone. In some embodiments, the first and second encapsulating films may further include one or more functional additives selected from the group consisting of crosslinking agents, coupling agents, antioxidants, and ultraviolet absorbers to improve the degree of crosslinking, weather resistance, adhesive strength, and anti-aging properties of the films. It is understood that the first and second encapsulating films can be made of the same or different materials.

[0036] The battery string layer comprises multiple battery strings, which can be combined in series, parallel, or series-parallel configurations to achieve current collection and output. Further, each battery string is formed by sequentially connecting multiple battery cells via connectors. In some embodiments, at least a portion of the connector is electrically connected to the back electrode of one battery cell, and at least another portion of the connector is electrically connected to the front or back electrode of another battery cell to form a battery string. The connector may optionally include conductive elements such as solder strips, busbars, or metal clips. In some embodiments, to improve welding performance, oxidation resistance, and weather resistance, the connector material may preferably be a highly conductive metal material, such as at least one of silver, copper, tin, and nickel, or an alloy thereof. In some embodiments, to balance conductivity and cost control, the connector material may also be at least one of metal-clad composite materials such as silver-coated copper, copper-coated silver, copper-coated aluminum, aluminum-coated copper, tin-plated copper, or nickel-plated copper. The electrical connection may be selected from one of the following methods: laser welding, spot welding, bonding, ultrasonic welding, resistance welding, or brazing.

[0037] The solar cell may include a semiconductor substrate, a first emitter of a first conductivity type, and a second emitter of a second conductivity type. It is understood that one of the first and second conductivity types is P-type, and the other is N-type. The semiconductor substrate may include an N-type silicon substrate or a P-type silicon substrate. N-type silicon substrates are typically formed by doping with Group V elements such as phosphorus, arsenic, or antimony, and have the characteristic that the majority charge carriers are electrons; P-type silicon substrates are typically formed by doping with Group III elements such as boron, gallium, or aluminum, and have the characteristic that the majority charge carriers are holes.

[0038] The solar cell can employ a grid line design with no main grid (OBB), multiple main grid (MBB), or super-multiple main grid (SMBB). In some embodiments, the grid line material can be selected as at least one of silver-based conductive paste or silver-coated copper composite paste. The paste uses highly conductive metal powder as the conductive substrate, and the substrate can be at least one of silver powder, copper powder, or silver-coated copper composite powder. To improve the ohmic contact performance, conductivity, and long-term weather resistance of the electrodes, a composite functional layer can be formed on the surface of the substrate or in the grid line structure. The functional layer material includes at least one of glass powder, organic carrier, nickel-based barrier layer, tin-based alloy layer, or anti-oxidation and corrosion-resistant coating.

[0039] It is understood that the solar cell can be at least one of the following commonly used in the field: TOPCon (Tunnel Oxide Passivated Contact) cell, HJT (Heterojunction with Intrinsic Thin-film) cell, BC (Back Contact) cell, perovskite / tandem cell, etc.

[0040] The frame surrounds the periphery of the stacked structure and is typically made of aluminum alloy or steel alloy. In some embodiments, the frame may also be a fiberglass frame or a plastic frame. The inner side of the frame usually has grooves for filling with sealant to achieve a sealed bond with the stacked components formed by the front cover, the first encapsulating film, the battery string layers, the second encapsulating film, and the back cover, thereby blocking moisture and buffering external impacts. In some embodiments, the frame can be assembled using corner brackets.

[0041] The junction box is located on one side of the rear cover and is electrically connected to the terminals of the bus electrodes in the battery string layer via a lead-out busbar for energy extraction. The junction box typically includes a housing and cover made of weather-resistant insulating material, conductive connecting tabs disposed within the housing, and one or more bypass diodes. The bypass diodes are connected in parallel with sub-units of the battery string. The electrical leads of the junction box include photovoltaic-specific connectors and cables. The cables preferably use cross-linked polyethylene insulation sheaths and tinned copper core wires. In some embodiments, the interior of the junction box may also be filled and encapsulated with potting compound to achieve insulation, thermal conductivity, moisture protection, and fixation.

[0042] The performance of the solar cells was tested in the following ways: I. Preparatory work before testing 1. Battery cell cleaning, including: Wipe the surface of the battery cells with ultrapure water, ethanol or isopropanol to remove fingerprints, dust and organic residues; After drying the solar cells with nitrogen, let them stand for 10 minutes to avoid surface contamination affecting their optical properties.

[0043] 2. Electrode contact inspection, including Use a four-wire probe (such as the Keithley 2400 series) to perform electrical measurements on the solar cells, ensuring that the contact resistance between the metal electrodes of the solar cells and the probe is <0.1Ω; Use silver paste or spring probes to secure the battery cells and avoid pressure damage.

[0044] 3. Stabilization treatment, including: Place the solar cells under standard lighting (1000W / m²). 2 Aging for 1 hour under light-induced degradation (LID) to eliminate light-induced degradation. The temperature of the solar cells was maintained at 25℃±0.5℃ using a constant temperature stage to avoid the impact of thermal effects on carrier mobility.

[0045] 4. Equipment calibration, including: The light source spectrum was calibrated using a standard reference cell to conform to the AM1.5G standard spectral conditions, with a calibration wavelength range of 300 nm to 1200 nm. The irradiance uniformity deviation in the test area does not exceed ±2%, and the measurement error of the temperature sensor used is less than ±0.1℃.

[0046] II. Testing Equipment and Conditions 1. Core equipment IV tester: Keysight B2900A series, with a voltage resolution of 0.1mV and a current resolution of 0.1μA; Solar simulator: Class AAA compliant, with selectable pulsed or steady-state light source (e.g., Wacom WXS-200S-20). Temperature control console: Temperature regulation is achieved based on a thermoelectric cooling (TEC) module, with a control accuracy of ±0.2℃; Spectral response instrument: equipped with a quantum efficiency (QE) testing system (such as Bentham PVE300).

[0047] 2. Standard Test Conditions (STC) Irradiance: 1000 W / m 2 (AM1.5G standard spectrum); Temperature: 25℃±1℃ (real-time monitoring via TEC module); Light spot uniformity: The uniformity of the light spot covering the effective area of ​​the battery is >95%.

[0048] III. Key Parameter Testing Procedures 1. Conversion efficiency (Eta) and IV characteristics (Voc, Isc, FF) testing Test equipment: solar simulator, IV tester and four-wire probe.

[0049] step: (1) Sample placement: Place the battery cell in the center of the light spot of the simulator, and use a light shield to block the edge of the battery cell by 5mm to avoid light leakage at the edge; (2) IV scan: Apply a scan voltage from -0.5V to Voc+0.5V through an IV tester, set the scan step size to 10mV, and record the IV characteristic curve of the battery simultaneously; (3) Parameter extraction: Extract the open-circuit voltage Voc (voltage when current = 0) and short-circuit current Isc (current when voltage = 0) from the IV curve; (4) Calculation of power and fill factor: Calculate the maximum power point (Pmax = Vmpp×Impp) and fill factor FF = Pmax / (Voc×Isc) on the IV curve; (5) Efficiency calculation: The conversion efficiency Eta = (Pmax / Pin) × 100% is calculated, where the incident light power Pin is calibrated by a calibrated standard cell.

[0050] 2. Series resistance (Rs) test Method 1: Dual-light illumination method (1) Curve measurement: at 1000W / m 2 and 800W / m 2 The IV curves of the battery were measured under two irradiance conditions; (2) Resistance calculation: Calculate the slope of ΔV / ΔI of the two IV curves in the region near the short-circuit current Isc, and calculate the series resistance Rs using the formula Rs = (Voc1 - Voc2) / (Isc1 - Isc2).

[0051] Method 2: Four-wire pulse measurement (1) Pulse application: Use an IV tester to apply a short current pulse with a pulse width of 1ms to the battery cell to eliminate the influence of battery self-heating on the measurement. (2) Resistance back calculation: According to Ohm's law ΔV=I×Rs, the series resistance Rs = ΔV / I is calculated from the measured voltage drop ΔV. It should be noted that the inherent contact resistance of the system needs to be deducted during the calculation.

[0052] 3. Parallel Resistance (Rsh) Test Method 1: Dark Current Method (1) Dark-state bias scanning: Under completely dark conditions, apply a reverse bias voltage from -1V to 0V to the solar cell and perform scanning; (2) Resistance calculation: Measure the slope of the IV characteristic in the reverse saturation current region, and the parallel resistance Rsh = ΔV / ΔI. Usually, the data point is taken at a bias voltage of -0.5V.

[0053] Method 2: Low-intensity IV analysis (1) Low light measurement: at 50W / m 2 The IV curve of the battery was measured under low irradiance. (2) Resistance estimation: The parallel resistance Rsh can be approximated as the reciprocal of the slope of the IV curve in the region near the open-circuit voltage Voc.

[0054] The researchers of this application have discovered that: Traditional technologies using NiO... x As a hole transport layer, NiO has serious drawbacks, including low intrinsic conductivity, high defect density, energy level mismatch with the perovskite interface, and reaction with perovskite precursors. Even though perovskite materials themselves have relatively high defect tolerance, untreated NiO... x Numerous defects and deep potential wells at the NiO-perovskite interface induce high levels of nonradiative recombination, thus limiting the potential of NiO. x The photovoltaic performance of NiO-based perovskite solar cells. Introducing an interface layer for modification and alteration is key to optimizing NiO. x One of the main methods for improving the photovoltaic performance of perovskite solar cells.

[0055] Based on this, this application provides a solar cell and its fabrication method, wherein the composite hole transport layer of the solar cell contains a self-assembled monomolecule material with anchoring groups and groups with strong hole transport capabilities, and the self-assembled monomolecule material is anchored to NiO. x Strong and stable covalent bonds are formed on the surface of the thin film, enabling selective contact to reduce interfacial recombination and promote charge transfer. Meanwhile, groups with strong hole transport capabilities can further improve hole mobility, thereby enhancing device efficiency.

[0056] In a first aspect, a solar cell is provided, comprising a transparent conductive glass, a composite hole transport layer, a perovskite light-absorbing layer, an electron transport layer, and a back electrode stacked sequentially, wherein the composite hole transport layer comprises a nickel oxide layer and a self-assembled monomolecule material layer, and the self-assembled monomolecule material layer comprises a structure of the self-assembled monomolecule material having the following structural formula: and / or R includes any one or a combination of at least two of carboxyl groups, sulfonic acid groups, phosphonic acid groups, or boric acid groups, and the self-assembled monomolecular material layer of the composite hole transport layer is disposed on the side close to the perovskite light-absorbing layer.

[0057] In the composite hole transport layer of the solar cell provided in this application embodiment, the self-assembled single-molecule material has a D-π-A molecular structure that can passivate NiO through molecular dipole and charge transfer. x Surface defects reduce the density of trapped states and suppress nonradiative recombination. One end of the self-assembled monomolecule material is anchored to NiO. x One end faces the perovskite, forming a hole-selective channel that blocks the back diffusion of electrons, further reducing interfacial recombination.

[0058] The solar cells described in this application include perovskite solar cells and / or crystalline silicon perovskite tandem cells.

[0059] In the solar cell provided in this application embodiment, the self-assembled monomolecule material within the composite hole transport layer is stably bonded to the surface of the nickel oxide thin film by means of end carboxyl anchoring groups, forming strong covalent bonds. This effectively repairs and reduces substrate surface defects, constructing an interfacial contact structure with selective conductivity, and significantly promoting efficient interfacial charge migration. The self-assembled monomolecule material layer can selectively and rapidly extract NiO. x The large number of charge carriers stacked at the perovskite interface significantly suppresses nonradiative recombination losses at the interface. At the same time, the terminal groups of the molecular structure can also interact with uncoordinated lead ions on the surface of the perovskite layer, effectively passivating defect sites inside the light-absorbing layer and reducing charge trapping losses. Combined with the excellent hole transport framework and tight π-π stacking structure of the molecule itself, the hole transport capability is further enhanced. Under the synergistic effect of multiple actions, the photoelectric conversion efficiency of the battery is effectively improved, while the stability of the device is optimized.

[0060] In some embodiments, R is -(CH2). n -COOH, where n is an integer from 0 to 3.

[0061] In some embodiments, the thickness of the nickel oxide layer is 10nm to 20nm, for example: 10nm, 12nm, 15nm, 18nm or 20nm.

[0062] In some embodiments, the thickness of the self-assembled monomolecular material layer is 1 nm to 3 nm, for example: 1 nm, 1.5 nm, 2 nm, 2.5 nm or 3 nm, etc.

[0063] This application controls the thickness of the self-assembled monomolecular material layer within the above-mentioned range, which can not only fully cover and passivate defects, stabilize interface bonding, and optimize energy levels, but also ensure smooth hole transport, thus balancing device efficiency and lifespan.

[0064] In some embodiments, the material of the perovskite light-absorbing layer includes ABX3, wherein A includes CH3NH3. + CH(NH2)2 + Cs+ or Rb + B includes any one or at least two of the following, where B includes Pb. 2+ Sn 2+ Or Ge 2+ X includes any one or at least two of the following, X including Cl - ,Br - Or I - Any one or at least two of them.

[0065] In some embodiments, the thickness of the perovskite light-absorbing layer is 200 nm to 900 nm.

[0066] In some embodiments, the material of the electron transport layer includes C 60 Any one or at least two of the following: PCBM, TiO2, SnO2, ZnO, or ZnO-ZnS.

[0067] In some embodiments, the back electrode material includes any one or a combination of at least two of Au, Ag, Al, Cu, or carbon.

[0068] In a second aspect, a method for preparing a solar cell as described in the first aspect is provided, the method comprising the following steps: Depositing a nickel oxide layer on transparent conductive glass; The self-assembled monomolecule material is dispersed in a solvent to obtain a self-assembled monomolecule material solution. The self-assembled monomolecule material solution is coated on a nickel oxide layer and then annealed to obtain a composite hole transport layer. The solar cell is obtained by sequentially fabricating a perovskite light-absorbing layer, an electron transport layer, and a back electrode on the surface of the composite hole transport layer.

[0069] In this embodiment, a self-assembled monomolecular material solution is coated onto a nickel oxide layer. The self-assembled monomolecular material is uniformly distributed on the nickel oxide layer, with a regular molecular arrangement and good consistency in defect passivation. Annealing then promotes bonding between carboxyl groups and the nickel oxide surface, resulting in stable molecular anchoring and preventing the film from easily peeling off.

[0070] In some embodiments, the solvent includes any one or a combination of at least two of isopropanol, ethanol, or DMF.

[0071] In some embodiments, the mass concentration of the self-assembled monomolecular material solution is 0.2 mg / mL to 1.2 mg / mL, for example: 0.2 mg / mL, 0.5 mg / mL, 0.8 mg / mL, 1 mg / mL or 1.2 mg / mL, etc.

[0072] This application can control the thickness of the self-assembled monomolecular material layer by controlling the mass concentration of the self-assembled monomolecular material solution, thereby obtaining optimal hole transport performance.

[0073] In some embodiments, the annealing temperature is 80°C to 120°C, for example: 80°C, 90°C, 100°C, 110°C or 120°C.

[0074] In some embodiments, the annealing time is 5 min to 15 min, for example: 5 min, 8 min, 10 min, 12 min or 15 min.

[0075] The numerical range described in this application includes not only the point values ​​listed above, but also any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values ​​included in the range.

[0076] Compared with the prior art, this application has the following advantages: (1) In the composite hole transport layer of the solar cell described in this application, the introduction of self-assembled monomolecule materials can reduce surface defects in the nickel oxide layer and promote charge transfer, and also reduce the NiO content. x Non-radiative recombination at the perovskite interface significantly reduces defects in the perovskite light-absorbing layer, thereby improving device efficiency.

[0077] (2) The open-circuit voltage Voc of the solar cell described in this application can reach above 1.17V, and the short-circuit current density Jsc can reach 24.8 mA / cm². 2 The fill factor FF can reach over 80.6%, and the photoelectric conversion efficiency can reach over 23.72%.

[0078] The self-assembled monomolecule materials used in the embodiments and comparative examples of this application were prepared by the following method: A solution containing 5.0% NaOH (4.0 mL) and ethanol (20 mL) was mixed with a substance of formula I (4.48 mmol) and N-ethylcarbazole-3-carbaldehyde (1.0 g, 4.48 mmol) and stirred. The mixture was then reacted overnight at room temperature. The reaction progress was monitored by thin-layer chromatography (TLC). The developing solvent for TLC was a 1:1 mixture of dichloromethane and petroleum ether, and the elution process used a 1:3 mixture of dichloromethane and petroleum ether. Once the reaction was complete, the resulting precipitate was filtered off. The crude product was purified by column chromatography (silica gel) and then recrystallized in a 1:1 mixture of dichloromethane and petroleum ether to give the final product. A solution containing 5.0% NaOH (4.0 mL) and ethanol (20 mL) was mixed with the substance of formula II (4.48 mmol) and 4-diphenylaminobenzaldehyde (1.0 g, 3.66 mmol) and stirred. The mixture was then reacted overnight at room temperature. The reaction progress was monitored by thin-layer chromatography (TLC). The developing solvent for TLC was a dichloromethane / petroleum ether mixture (v / v, 1:2), and the elution process used a dichloromethane / petroleum ether mixture (v / v, 1:4). Once the reaction was complete, the resulting precipitate was filtered off. The crude product was purified by column chromatography (silica gel) and then recrystallized in a dichloromethane and petroleum ether mixture (v / v, 1:1) to give the final product.

[0079] Example 1 This embodiment provides a solar cell, which includes a transparent conductive glass, a composite hole transport layer, a perovskite light-absorbing layer, an electron transport layer, and a back electrode stacked sequentially. The composite hole transport layer comprises a 15 nm thick nickel oxide layer and a 2 nm thick self-assembled monomolecule material layer. The structural formula of the self-assembled monomolecule material in the self-assembled monomolecule material layer is as follows: The self-assembled monomolecular material layer of the composite hole transport layer is disposed on the side close to the perovskite light-absorbing layer, and the solar cell is fabricated by the following method: The ITO transparent conductive glass was cleaned, specifically by ultrasonic cleaning with detergent, deionized water, acetone, and anhydrous ethanol, followed by drying with a nitrogen gun. The ultrasonic cleaning power was 100 Hz, and the ultrasonic cleaning time was 15 minutes. A hole transport layer was then deposited on the conductive glass surface by spin-coating; specifically, NiO was applied... x The solution (20 mg / mL, deionized water) was spin-coated onto conductive glass at 3000 rpm for 30 seconds, and then annealed at 200 °C for 15 minutes to form NiO. x Layer; mg / mL The self-assembled monomolecule was dispersed in DMF and stirred at room temperature for 4 hours to ensure complete dissolution, resulting in a concentration of 0.5 mg / mL. Then, 150 μL of this solution was spin-coated onto NiO at 3000 rpm. x The composite hole transport layer is obtained by spin coating for 30 seconds and then annealing at 100°C for 10 minutes. 108.33 mg CsI, 1218.34 mg FAI, 132.50 mg MAI, 4033.76 mg PbI2, and 83.27 mg MCl were added to a vial containing 4200 μL DMF and 840 μL DMSO, and stirred thoroughly for at least 12 hours to form a 1.67 mol / L CsI solution. 0.05 MA 0.1 FA 0.85 PbI3 perovskite precursor solution. The perovskite precursor solution was spin-coated onto the self-assembled layer at 5000 rpm for 50 s with an acceleration of 1000 rpm. At the 35th s mark, 200 μL of chlorobenzene was added dropwise. Finally, annealing was performed at 120 °C for 15 min to crystallize and form a Cs layer with a thickness of approximately 450 nm. 0.05 MA 0.1 FA 0.85 A PbI3 perovskite light-absorbing layer was then deposited on the surface of the perovskite layer using a vacuum evaporation method to form an electron transport layer (C). 60 The evaporation is carried out under a vacuum of 5×10⁻⁶. -4 The process was carried out under Pa conditions at an evaporation rate of 0.15 A / s, with a thickness of 20 nm. An electron transport layer of SnO2 was then deposited on the surface of the electron transport layer via atomic layer deposition (ALD), with the tin source extraction rate and purge time being 0.5 s and 5 s respectively, and the water source extraction rate and purge time being 0.5 s and 5 s respectively. The reaction temperature was 85 °C, the number of cycles was 120, and the thickness was 12 nm. A 100 nm thick silver electrode was then formed in a metal evaporation chamber via thermal evaporation, with a vacuum level of 5 × 10⁻⁶. -4 A solar cell was obtained by evaporating at a rate of 2 A / s using Pa.

[0080] Example 2 This embodiment provides a solar cell, which includes a transparent conductive glass, a composite hole transport layer, a perovskite light-absorbing layer, an electron transport layer, and a back electrode stacked sequentially. The composite hole transport layer comprises a 15 nm thick nickel oxide layer and a 2 nm thick self-assembled monomolecule material layer. The structural formula of the self-assembled monomolecule material in the self-assembled monomolecule material layer is as follows: The self-assembled monomolecular material layer of the composite hole transport layer is disposed near the perovskite light-absorbing layer, and the composite hole transport layer is prepared by the following method: The transparent conductive glass was cleaned, specifically by ultrasonic cleaning with detergent, deionized water, acetone, and anhydrous ethanol, followed by drying with a nitrogen gun. The ultrasonic cleaning power was 100 Hz, and the cleaning time was 15 minutes. A hole transport layer was then deposited on the conductive glass surface via spin coating; specifically, NiO was applied. x The solution (20 mg / mL, deionized water) was spin-coated onto conductive glass at 3000 rpm for 30 seconds, and then annealed at 200 °C for 15 minutes to form NiO. x layer; The self-assembled monomolecule was dispersed in isopropanol and stirred at room temperature for 4 hours to ensure complete dissolution, resulting in a concentration of 0.5 mg / mL. Then, 150 μL of this solution was spin-coated onto NiO at 3000 rpm. x The composite hole transport layer is obtained by spin coating for 30 seconds and then annealing at 80°C for 15 minutes. 108.33 mg CsI, 1218.34 mg FAI, 132.50 mg MAI, 4033.76 mg PbI2, and 83.27 mg MCl were added to a vial containing 4200 μL DMF and 840 μL DMSO, and stirred thoroughly for at least 12 hours to form a 1.67 mol / L CsI solution. 0.05 MA 0.1 FA 0.85 PbI3 perovskite precursor solution. The perovskite precursor solution was spin-coated onto the self-assembled layer at 5000 rpm for 50 s with an acceleration of 1000 rpm. At the 35th s mark, 200 μL of chlorobenzene was added dropwise. Finally, annealing was performed at 120 °C for 15 min to crystallize and form a Cs layer with a thickness of approximately 450 nm. 0.05 MA 0.1 FA 0.85 A PbI3 perovskite light-absorbing layer was then deposited on the surface of the perovskite layer using a vacuum evaporation method to form an electron transport layer (C). 60 The evaporation is carried out under a vacuum of 5×10⁻⁶. -4 The process was carried out under Pa conditions at an evaporation rate of 0.15 A / s, with a thickness of 20 nm. An electron transport layer of SnO2 was then deposited on the surface of the electron transport layer via atomic layer deposition (ALD), with the tin source extraction rate and purge time being 0.5 s and 5 s respectively, and the water source extraction rate and purge time being 0.5 s and 5 s respectively. The reaction temperature was 85 °C, the number of cycles was 120, and the thickness was 12 nm. A 100 nm thick silver electrode was then formed in a metal evaporation chamber via thermal evaporation, with a vacuum level of 5 × 10⁻⁶. -4 A solar cell was obtained by evaporating at a rate of 2 A / s using Pa.

[0081] Example 3 This embodiment provides a solar cell, which includes a transparent conductive glass, a composite hole transport layer, a perovskite light-absorbing layer, an electron transport layer, and a back electrode stacked sequentially. The composite hole transport layer comprises a 15 nm thick nickel oxide layer and a 2 nm thick self-assembled monomolecule material layer. The structural formula of the self-assembled monomolecule material in the self-assembled monomolecule material layer is as follows: The self-assembled monomolecular material layer of the composite hole transport layer is disposed near the perovskite light-absorbing layer, and the composite hole transport layer is prepared by the following method: The transparent conductive glass was cleaned, specifically by ultrasonic cleaning with detergent, deionized water, acetone, and anhydrous ethanol, followed by drying with a nitrogen gun. The ultrasonic cleaning power was 100 Hz, and the cleaning time was 15 minutes. A hole transport layer was then deposited on the conductive glass surface via spin coating; specifically, NiO was applied. x The solution (20 mg / mL, deionized water) was spin-coated onto conductive glass at 3000 rpm for 30 seconds, and then annealed at 200 °C for 15 minutes to form NiO. x layer; The self-assembled monomolecule was dispersed in ethanol and stirred at room temperature for 4 hours to ensure complete dissolution, resulting in a concentration of 0.5 mg / mL. Then, 150 μL of this solution was spin-coated onto NiO at 3000 rpm. x The composite hole transport layer is obtained by spin-coating the layer for 30 seconds and then annealing it at 120°C for 5 minutes. 108.33 mg CsI, 1218.34 mg FAI, 132.50 mg MAI, 4033.76 mg PbI2, and 83.27 mg MCl were added to a vial containing 4200 μL DMF and 840 μL DMSO, and stirred thoroughly for at least 12 hours to form a 1.67 mol / L CsI solution. 0.05 MA 0.1 FA 0.85 PbI3 perovskite precursor solution. The perovskite precursor solution was spin-coated onto the self-assembled layer at 5000 rpm for 50 s with an acceleration of 1000 rpm. At the 35th s mark, 200 μL of chlorobenzene was added dropwise. Finally, annealing was performed at 120 °C for 15 min to crystallize and form a Cs layer with a thickness of approximately 450 nm. 0.05 MA 0.1 FA 0.85 A PbI3 perovskite light-absorbing layer was then deposited on the surface of the perovskite layer using a vacuum evaporation method to form an electron transport layer (C).60 The evaporation is carried out under a vacuum of 5×10⁻⁶. -4 The process was carried out under Pa conditions at an evaporation rate of 0.15 A / s, with a thickness of 20 nm. An electron transport layer of SnO2 was then deposited on the surface of the electron transport layer via atomic layer deposition (ALD), with the tin source extraction rate and purge time being 0.5 s and 5 s respectively, and the water source extraction rate and purge time being 0.5 s and 5 s respectively. The reaction temperature was 85 °C, the number of cycles was 120, and the thickness was 12 nm. A 100 nm thick silver electrode was then formed in a metal evaporation chamber via thermal evaporation, with a vacuum level of 5 × 10⁻⁶. -4 A solar cell was obtained by evaporating at a rate of 2 A / s using Pa.

[0082] Example 4 This embodiment provides a solar cell, which includes a transparent conductive glass, a composite hole transport layer, a perovskite light-absorbing layer, an electron transport layer, and a back electrode stacked sequentially. The composite hole transport layer comprises a 15 nm thick nickel oxide layer and a 2 nm thick self-assembled monomolecule material layer. The structural formula of the self-assembled monomolecule material in the self-assembled monomolecule material layer is as follows: The self-assembled monomolecular material layer of the composite hole transport layer is disposed near the perovskite light-absorbing layer, and the composite hole transport layer is prepared by the following method: The transparent conductive glass was cleaned, specifically by ultrasonic cleaning with detergent, deionized water, acetone, and anhydrous ethanol, followed by drying with a nitrogen gun. The ultrasonic cleaning power was 100 Hz, and the cleaning time was 15 minutes. A hole transport layer was then deposited on the conductive glass surface via spin coating; specifically, NiO was applied. x The solution (20 mg / mL, deionized water) was spin-coated onto conductive glass at 3000 rpm for 30 seconds, and then annealed at 200 °C for 15 minutes to form NiO. x layer; The self-assembled monomolecule was dispersed in DMF and stirred at room temperature for 4 hours to ensure complete dissolution, resulting in a concentration of 0.5 mg / mL. Then, 150 μL of this solution was spin-coated onto NiO at 3000 rpm. x The composite hole transport layer is obtained by spin coating for 30 seconds and then annealing at 100°C for 10 minutes. 108.33 mg CsI, 1218.34 mg FAI, 132.50 mg MAI, 4033.76 mg PbI2, and 83.27 mg MCl were added to a vial containing 4200 μL DMF and 840 μL DMSO, and stirred thoroughly for at least 12 hours to form a 1.67 mol / L CsI solution. 0.05 MA 0.1 FA 0.85 PbI3 perovskite precursor solution. The perovskite precursor solution was spin-coated onto the self-assembled layer at 5000 rpm for 50 s with an acceleration of 1000 rpm. At the 35th s mark, 200 μL of chlorobenzene was added dropwise. Finally, annealing was performed at 120 °C for 15 min to crystallize and form a Cs layer with a thickness of approximately 450 nm. 0.05 MA 0.1 FA 0.85 A PbI3 perovskite light-absorbing layer was then deposited on the surface of the perovskite layer using a vacuum evaporation method to form an electron transport layer (C). 60 The evaporation is carried out under a vacuum of 5×10⁻⁶. -4 The process was carried out under Pa conditions at an evaporation rate of 0.15 A / s, with a thickness of 20 nm. An electron transport layer of SnO2 was then deposited on the surface of the electron transport layer via atomic layer deposition (ALD), with the tin source extraction rate and purge time being 0.5 s and 5 s respectively, and the water source extraction rate and purge time being 0.5 s and 5 s respectively. The reaction temperature was 85 °C, the number of cycles was 120, and the thickness was 12 nm. A 100 nm thick silver electrode was then formed in a metal evaporation chamber via thermal evaporation, with a vacuum level of 5 × 10⁻⁶. -4 A solar cell was obtained by evaporating at a rate of 2 A / s using Pa.

[0083] Example 5 The only difference between this embodiment and Example 1 is that the mass concentration of the self-assembled monomolecule material dispersed in DMF is 0.2 mg / mL, and the thickness of the self-assembled monomolecule material layer is 1 nm. All other conditions and parameters are exactly the same as in Example 1.

[0084] Example 6 The only difference between this embodiment and Example 1 is that the mass concentration of the self-assembled monomolecule material dispersed in DMF is 1.2 mg / mL, and the thickness of the self-assembled monomolecule material layer is 3 nm. All other conditions and parameters are exactly the same as in Example 1.

[0085] Example 7 The only difference between this embodiment and Example 1 is that the mass concentration of the self-assembled monomolecule material dispersed in DMF is 0.1 mg / mL, and the thickness of the self-assembled monomolecule material layer is 0.5 nm. All other conditions and parameters are exactly the same as in Example 1.

[0086] Example 8 The only difference between this embodiment and Example 1 is that the mass concentration of the self-assembled monomolecule material dispersed in DMF is 1.5 mg / mL, and the thickness of the self-assembled monomolecule material layer is 4 nm. All other conditions and parameters are exactly the same as in Example 1.

[0087] Comparative Example 1 The only difference between this comparative example and Example 1 is that no self-assembled monomolecule material layer is set; all other conditions and parameters are exactly the same as in Example 1.

[0088] Performance testing: The solar cells obtained in the examples and comparative examples were tested, and the test results are shown in Table 1: Table 1 As shown in Table 1, based on Examples 1 to 8, the open-circuit voltage Voc of the solar cell described in this application can reach over 1.14V, and the short-circuit current density Jsc can reach 23.7 mA / cm². 2 The fill factor (FF) can reach over 78.4%, and the photoelectric conversion efficiency can reach over 21.37%. By adjusting the thickness of the self-assembled monomolecular material layer in the composite hole transport layer, the open-circuit voltage (Voc) of the solar cell can reach over 1.17V, and the short-circuit current density (Jsc) can reach 24.8 mA / cm². 2 The fill factor FF can reach over 80.6%, and the photoelectric conversion efficiency can reach over 23.72%.

[0089] A comparison of Examples 1 and 5-8 shows that the thickness of the self-assembled monomolecular material layer (the concentration of the self-assembled monomolecular material solution during preparation) affects the performance of the solar cell described in this application. Controlling the thickness of the self-assembled monomolecular material layer to 1 nm to 3 nm (the concentration of the self-assembled monomolecular material solution during preparation to 0.2 mg / mL to 1.2 mg / mL) results in a composite hole transport layer with better performance. If the thickness of the self-assembled monomolecular material layer is too thick, molecules are prone to stacking, which obstructs the charge transport path and further affects the efficiency. If the thickness of the self-assembled monomolecular material layer is too thin, effective charge transport cannot be formed, leading to a decrease in efficiency.

[0090] The JV curves of the perovskite solar cells described in Example 1 and Comparative Example 1 are compared as follows: Figure 1As shown, a comparison between Example 1 and Comparative Example 1 reveals that the solar cell with the addition of the self-assembled molecular layer in this application exhibits significant improvements in open-circuit voltage, short-circuit current, fill factor, and photoelectric conversion efficiency. The improved battery performance is attributed to the anchoring groups in the self-assembled molecular structure anchoring to NiO. x Strong and stable covalent bonds form on the thin film surface, enabling selective contact to reduce surface defects and promote charge transfer. A key reason for the increased Voc is the formation of a more favorable energy level arrangement in NiO. x The large number of charge carriers accumulated at the perovskite interface are highly selectively extracted through self-assembled molecular layers, reducing nonradiative recombination at the interface. Simultaneously, the carboxyl groups at the other end of the molecule can interact with uncoordinated Pb on the perovskite surface. 2+ This combination significantly reduces defects in the perovskite light-absorbing layer, thereby improving device efficiency.

[0091] The fluorescence lifetime comparison spectra of the perovskite thin films in the solar cells prepared in Example 1 and Comparative Example 1 are shown below. Figure 2 As shown, by Figure 2 It can be seen that the average carrier lifetime of the perovskite film modified with the self-assembled molecular layer is shorter than that of the perovskite film without the self-assembled molecular layer. The reduced lifetime indicates that the introduction of the self-assembled molecular layer effectively promotes the carrier lifetime of NiO. x Hole separation at the perovskite interface.

[0092] The applicant declares that the above description is only a specific implementation of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. A solar cell, characterized in that, The solar cell comprises, in sequence, a transparent conductive glass, a composite hole transport layer, a perovskite light-absorbing layer, an electron transport layer, and a back electrode. The composite hole transport layer comprises a nickel oxide layer and a self-assembled monomolecule material layer. The structural formula of the self-assembled monomolecule material in the self-assembled monomolecule material layer includes... and / or R includes any one or a combination of at least two of carboxyl groups, sulfonic acid groups, phosphonic acid groups, or boric acid groups, and the self-assembled monomolecular material layer of the composite hole transport layer is disposed on the side close to the perovskite light-absorbing layer.

2. The solar cell as described in claim 1, characterized in that, The R is -(CH2). n -COOH, where n is an integer from 0 to 3.

3. The solar cell as described in claim 1 or 2, characterized in that, The thickness of the nickel oxide layer is 10 nm to 20 nm.

4. The solar cell according to any one of claims 1-3, characterized in that, The thickness of the self-assembled monomolecular material layer is 1 nm to 3 nm.

5. The solar cell according to any one of claims 1-4, characterized in that, The perovskite light-absorbing layer is made of ABX3, wherein A includes CH3NH3. + CH(NH2)2 + Cs + or Rb + B includes any one or at least two of the following, where B includes Pb. 2+ Sn 2+ Or Ge 2+ X includes any one or at least two of the following, X including Cl - ,Br - or I - Any one or at least two of them; And / or, the thickness of the perovskite light-absorbing layer is 200nm~900nm.

6. The solar cell according to any one of claims 1-5, characterized in that, The material of the electron transport layer includes C. 60 Any one or at least two of the following: PCBM, TiO2, SnO2, ZnO, or ZnO-ZnS.

7. The solar cell according to any one of claims 1-6, characterized in that, The back electrode material includes any one or a combination of at least two of Au, Ag, Al, Cu, or carbon.

8. A method for preparing a solar cell according to any one of claims 1-4, characterized in that, The preparation method includes the following steps: Depositing a nickel oxide layer on transparent conductive glass; The self-assembled monomolecule material is dispersed in a solvent to obtain a self-assembled monomolecule material solution. The self-assembled monomolecule material solution is coated on a nickel oxide layer and then annealed to obtain a composite hole transport layer. The solar cell is obtained by sequentially fabricating a perovskite light-absorbing layer, an electron transport layer, and a back electrode on the surface of the composite hole transport layer.

9. The preparation method according to claim 8, characterized in that, The solvent includes any one or a combination of at least two of isopropanol, ethanol, or DMF. And / or, the mass concentration of the self-assembled monomolecular material solution is 0.2 mg / mL to 1.2 mg / L.