Semiconductor device and method of forming thereof
By first forming a dielectric layer in a three-dimensional stacked semiconductor memory, then removing the sacrificial layer and forming an electrode plate, and finally forming an electrode pillar, the problem of low product yield in the prior art is solved, and higher electrical connection reliability and simplified process steps are achieved.
Patent Information
- Application Number
- CN202610903616.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-22
- Publication Date
- 2026-11-17
AI Technical Summary
In the formation of semiconductor memory with a three-dimensional stacked architecture, the existing technology suffers from low product yield, mainly due to the damage and morphological inhomogeneity of the electrode pillars during wet etching, which affects the reliability of electrical connections and manufacturing yield.
A first dielectric layer is first formed in the via, then the sacrificial layer is removed to form an opening, an electrode plate is then formed in the opening, and an electrode post is formed after the first dielectric layer is removed. This decouples the formation process sequence of the electrode plate and the electrode post, avoids damage to the electrode post caused by wet etching, and simplifies the process steps.
By decoupling the formation process sequence of electrode plates and electrode posts, damage to the electrode posts caused by etching is avoided, thereby improving the product yield of semiconductor structures and the reliability of electrical connections, and simplifying the process steps.
Smart Images

Figure CN123124661A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor manufacturing, and more particularly to a semiconductor device and a method for forming the same. Background Technology
[0002] Semiconductor memory, as a fundamental device type in the integrated circuit industry, is widely used in various electronic devices, undertaking the core functions of data storage and retrieval. As electronic devices continue to evolve towards higher performance, miniaturization, and lower power consumption, semiconductor memory needs to achieve higher storage density and larger storage capacity within a limited chip area. To meet this demand, three-dimensional stacked architecture has gradually become an important development direction for semiconductor memory technology. By stacking multiple layers of memory cells vertically perpendicular to the chip surface, storage density can be increased exponentially within a unit chip area. The formation process of a three-dimensional semiconductor memory involves constructing conductive channels and functional regions within the vertically stacked dielectric structure, and defining the space and structure of each functional layer through the sequential filling and selective removal of various materials. As the number of vertically stacked layers continues to increase, the formation sequence of each functional layer, the interaction between material removal steps, and the precise control of the structural morphology throughout the process all have a significant impact on the electrical performance and manufacturing yield of the final device.
[0003] In the fabrication of three-dimensional semiconductor devices, the formation sequence of each functional layer (e.g., electrode plates and electrode pillars), the etching selectivity of the material removal process in each step, and the process compatibility between temporary filling materials and permanent functional materials are important factors affecting the uniformity of the final device structure morphology, the reliability of electrical connections, and the product yield.
[0004] Currently, the yield rate of semiconductor devices still needs to be improved. Summary of the Invention
[0005] The problem solved by the embodiments of the present invention is to provide a semiconductor device and a method for forming the same, thereby improving the product yield of the semiconductor device.
[0006] To address the aforementioned problems, embodiments of the present invention provide a method for forming a semiconductor device, comprising: providing a substrate, wherein a dielectric structure layer is formed on the top of the substrate, the dielectric structure layer including a sacrificial layer and an insulating layer alternately stacked in a longitudinal direction, and a via is formed on the top of the substrate penetrating the dielectric structure layer, the via exposing the top surface of the substrate; forming a first dielectric layer in the via; removing the sacrificial layer to form an opening corresponding to the sacrificial layer; forming a filling electrode plate in the opening, the electrode plate including a storage dielectric layer surrounding and covering the inner wall of the opening and a conductive layer filling the remaining space of the opening; removing the first dielectric layer to use the space released by the first dielectric layer as a first through-groove; and forming an electrode post in the first through-groove, the electrode post covering the sidewalls of the storage dielectric layer and the insulating layer.
[0007] Optionally, the material of the first dielectric layer includes one or more of silicon nitride, polycrystalline silicon, amorphous silicon, silicon carbonitride, silicon oxide, monocrystalline silicon, silicon oxynitride, spin-coated organic carbon, spin-coated inorganic carbon, and amorphous carbon.
[0008] Optionally, before forming the first dielectric layer, the forming method further includes: forming a second dielectric layer on the sidewall and bottom of the through hole; in the step of forming the first through groove, the first through groove exposes the second dielectric layer; after removing the first dielectric layer to form the first through groove, and before forming the electrode post, the forming method further includes: removing the second dielectric layer and using the space area released by the second dielectric layer as the second through groove, the second through groove exposing the sidewall of the insulating layer and the electrode plate, and the second through groove communicating with the first through groove; in the step of forming the electrode post, the electrode post is also formed in the second through groove.
[0009] Optionally, after removing the second dielectric layer and before forming the electrode post, the method further includes: removing a portion of the insulating layer exposed by the second through groove, so that the sidewall of the electrode plate protrudes beyond the sidewall of the remaining insulating layer, and using the space released by the removed insulating layer as a horizontal groove, wherein the horizontal groove communicates with the second through groove; in the step of forming the electrode post, the electrode post is also formed in the horizontal groove.
[0010] Optionally, the thickness of the second dielectric layer covering the sidewall of the through hole gradually increases in the direction along the longitudinal direction and gradually away from the substrate.
[0011] Optionally, the sidewall of the electrode plate protrudes from the sidewall of the insulating layer by a size ranging from 0.5 nanometers to 10 nanometers.
[0012] Optionally, the material of the second dielectric layer includes one or more of silicon nitride, polycrystalline silicon, amorphous silicon, silicon carbonitride, silicon oxide, monocrystalline silicon, silicon oxynitride, spin-coated organic carbon, spin-coated inorganic carbon, and amorphous carbon.
[0013] Optionally, in the step of providing the substrate, the substrate includes a conductive connector located on the top surface, and the through-hole exposes the conductive connector.
[0014] Optionally, the storage medium layer includes a variable resistance layer that stores data by changing resistance under the action of current or voltage, or a polarization layer that stores data by changing polarization state under the action of voltage.
[0015] Accordingly, embodiments of the present invention also provide a semiconductor device formed using the formation method provided by the present invention.
[0016] Compared with the prior art, the technical solution of the embodiments of the present invention has the following advantages: The semiconductor device formation method provided in this invention first forms a first dielectric layer in a via and then removes a sacrificial layer to form an opening. During the removal of the sacrificial layer, the first dielectric layer occupies the entire space of the via, thus avoiding erosion or damage to the electrode posts caused by the sacrificial layer removal process. After forming an electrode plate in the opening, the first dielectric layer is then removed to form a first through-hole. In other words, the formation of the electrode plate and the electrode posts are decoupled in terms of process sequence. This allows the electrode plate to be filled before the electrode posts without worrying about damage to the electrode posts during the removal of the sacrificial layer, or the difficulty of etching the electrode plate material layer to form an opening to accommodate the electrode posts. Simultaneously, the first dielectric layer is removed after the electrode plate is formed, releasing a regular first through-hole. When the electrode posts are formed in the first through-hole, they can directly cover the sidewalls of the storage dielectric layer and the insulating layer, eliminating the need for an additional protective layer on the via sidewalls to avoid damage to the electrode posts. This also prevents the thickness of the protective layer from affecting the critical dimensions of the via for accommodating the electrode posts, thereby simplifying the process steps and improving the product yield of the semiconductor structure. Attached Figure Description
[0017] Figures 1 to 7 This is a schematic diagram of the structure corresponding to each step in a method for forming a semiconductor device; Figures 8 to 13 This is a schematic diagram of the structure corresponding to each step of an embodiment of the semiconductor device formation method of the present invention; Figures 14 to 18 This is a schematic diagram of the structure corresponding to each step in the second embodiment of the semiconductor device formation method of the present invention. Detailed Implementation
[0018] Currently, the performance of semiconductor devices still needs improvement. This paper analyzes the reasons why the performance of a semiconductor device still needs improvement, using a semiconductor device fabrication method as an example.
[0019] in, Figures 1 to 7 This is a schematic diagram of the structure corresponding to each step in the formation method of a semiconductor device.
[0020] refer to Figure 1 A substrate 16 is provided, and a dielectric structure layer 10 is formed on the top of the substrate 16. The dielectric structure layer 10 includes a first sacrificial layer 20 and an insulating layer 12 that are alternately stacked in the longitudinal direction. A through hole 26 is formed on the top of the substrate 16, penetrating the dielectric structure layer 10, and the through hole 26 exposes the top surface of the substrate 16.
[0021] refer to Figure 2 A second sacrificial layer 50 is formed at the bottom and sidewalls of the through hole 26 and at the top of the dielectric structure layer 10, and a protective layer 51 is formed to conformally cover the second sacrificial layer 50.
[0022] refer to Figure 3 Remove the protective layer 51 and the second sacrificial layer 50 at the bottom of the through hole 26.
[0023] refer to Figure 4 Remove the remaining protective layer 51.
[0024] refer to Figure 5 A conductive material layer is formed on top of the second sacrificial layer 50 and in the remaining space of the via 26; the conductive material layer on top of the dielectric structure layer 10 is planarized with the top of the dielectric structure layer 10 as the stop position, and the remaining conductive material layer in the via 26 is used as the electrode post 66.
[0025] refer to Figure 6 ,in, Figure 6 (b) is Figure 6 (a) An enlarged schematic diagram of reference numeral A, after forming the electrode post 66, the first sacrificial layer 20 is removed to form an opening 70 that exposes part of the sidewall of the second sacrificial layer 50.
[0026] refer to Figure 7 Wet etching removes the second sacrificial layer 50 exposed by the opening 70, forming a horizontal groove 90 that exposes the sidewall of the electrode post 66. The horizontal groove 90 is connected to the opening 70.
[0027] Research has revealed that in the process step of removing the first sacrificial layer 20 to form the opening 70, the wet etching solution used to remove the first sacrificial layer 20 comes into contact with the second sacrificial layer 50 on the sidewall of the via 26. The exposed portion of the second sacrificial layer 50 at the sidewall is subjected to lateral erosion by the wet etching solution. In the step of wet etching to remove the exposed second sacrificial layer 50 of the opening 70 to form the horizontal trench 90, due to the isotropic nature of wet etching, the second sacrificial layer 50 is also eroded by the etching solution in the vertical direction, resulting in irregular and uncontrollable morphological loss in the vertical direction. This affects the morphological accuracy and dimensional uniformity of the finally formed horizontal trench 90, thus adversely affecting the overall yield and reliability of the semiconductor device. Furthermore, as a thin film material, the second sacrificial layer 50 itself has pinhole defects (such as...). Figure 6 (b) As shown, when removing the first sacrificial layer 20 in the dielectric structure layer 10, the wet etching solution may penetrate into the via 26 through the pinhole position on the second sacrificial layer 50 film, causing interface damage to the surface of the electrode pillar 66 already formed in the via 26, thereby affecting the product yield of the semiconductor device; and the second sacrificial layer 50 will occupy part of the volume of the via 26, causing a contradiction between the critical dimensions of the via 26 and the conductivity of the electrode pillar 66.
[0028] To address the technical problem, embodiments of the present invention provide a method for forming a semiconductor device, comprising: providing a substrate, wherein a dielectric structure layer is formed on the top of the substrate, the dielectric structure layer including a sacrificial layer and an insulating layer alternately stacked in a longitudinal direction, and a via is formed on the top of the substrate penetrating the dielectric structure layer, the via exposing the top surface of the substrate; forming a first dielectric layer in the via; removing the sacrificial layer to form an opening corresponding to the sacrificial layer; forming a filling electrode plate in the opening, the electrode plate including a storage dielectric layer surrounding and covering the inner wall of the opening and a conductive layer filling the remaining space of the opening; removing the first dielectric layer, the space area released by the first dielectric layer serving as a first through-groove; and forming an electrode post in the first through-groove, the electrode post covering the sidewalls of the storage dielectric layer and the insulating layer.
[0029] The semiconductor device formation method provided in this invention first forms a first dielectric layer in a via and then removes a sacrificial layer to form an opening. During the removal of the sacrificial layer, the first dielectric layer occupies the entire space of the via, thus avoiding erosion or damage to the electrode posts caused by the sacrificial layer removal process. After forming an electrode plate in the opening, the first dielectric layer is then removed to form a first through-hole. In other words, the formation of the electrode plate and the electrode posts are decoupled in terms of process sequence. This allows the electrode plate to be filled before the electrode posts without worrying about damage to the electrode posts during the removal of the sacrificial layer, or the difficulty of etching the electrode plate material layer to form an opening to accommodate the electrode posts. Simultaneously, the first dielectric layer is removed after the electrode plate is formed, releasing a regular first through-hole. When the electrode posts are formed in the first through-hole, they can directly cover the sidewalls of the storage dielectric layer and the insulating layer, avoiding damage to the electrode posts without the need for an additional protective layer on the via sidewalls. This also prevents the thickness of the protective layer from affecting the critical dimensions of the via for accommodating the electrode posts, thereby simplifying the process steps and improving the product yield of the semiconductor structure.
[0030] To make the above-mentioned objects, features and advantages of the embodiments of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0031] in, Figures 8 to 13 This is a schematic diagram of the structure corresponding to each step of the first embodiment of the semiconductor device formation method of the present invention.
[0032] refer to Figure 8 A substrate 106 is provided, and a dielectric structure layer 100 is formed on the top of the substrate 106. The dielectric structure layer 100 includes a sacrificial layer 101 and an insulating layer 102 that are alternately stacked in the longitudinal direction. A through hole 116 is formed on the top of the substrate 106, penetrating the dielectric structure layer 100, and the through hole 116 exposes the top surface of the substrate 106.
[0033] The substrate 106 serves to provide a support base for the dielectric structure layer 100 and subsequently formed electrode plates and electrode posts, and to provide structural support for the entire semiconductor device. The substrate 106 may include at least one of an insulating material, a conductive material, and a semiconductor material. For example, the substrate 106 includes a silicon wafer with an insulating film layer formed on its top surface.
[0034] Specifically, the longitudinally alternating stacked sacrificial layer 101 and insulating layer 102 provide the structural prerequisite for the subsequent selective removal of sacrificial layer 101 to form an opening.
[0035] The alternating arrangement of the sacrificial layer 101 and the insulating layer 102 in the longitudinal direction ensures that after the sacrificial layer 101 is removed, the openings are separated in the longitudinal direction by the insulating layer 102, thereby providing space for the independent formation of electrode plates in each opening. It also ensures that the multiple electrode plates formed in the end are electrically isolated from each other in the longitudinal direction by the insulating layer 102.
[0036] The sacrificial layer 101 is removed in subsequent processes to create openings, thereby providing space for the formation of the electrode plate. In other words, the thickness and position of the sacrificial layer 101 directly define the longitudinal position and thickness of the final formed electrode plate.
[0037] The insulating layer 102, on the one hand, cooperates with the first dielectric layer to support the entire dielectric structure layer 100 to maintain the mechanical stability of the structure after the sacrificial layer 101 is removed, and on the other hand, serves as an insulating isolation medium between adjacent electrode plates to prevent electrical short circuits or signal crosstalk between electrode plates of different levels.
[0038] There is etching selectivity between the materials of the sacrificial layer 101 and the insulating layer 102. For example, the sacrificial layer 101 includes silicon nitride and the insulating layer 102 includes silicon oxide, but it is not limited to these, as long as the etching selectivity requirement can be met between the two.
[0039] It should be noted that the through-hole 116 penetrates the dielectric structure layer 100 and exposes the top surface of the substrate 106, providing a longitudinally extending spatial channel for the subsequent formation of electrode pillars within the dielectric structure layer 100. The fact that the through-hole 116 exposes the top surface of the substrate 106 means that the material filling the through-hole 116 can form direct contact with the substrate 106. When the first dielectric layer is subsequently formed in the through-hole 116 and the electrode pillar is formed after the first dielectric layer is removed, the electrode pillar can extend along the longitudinal path defined by the through-hole 116 to the top surface of the substrate 106, thereby achieving a reliable electrical connection with the top surface of the substrate 106.
[0040] It should also be noted that the position and horizontal cross-sectional dimensions of the through hole 116 directly determine the position and radial dimensions of the final electrode post. Therefore, when forming the through hole 116, the layout and key dimensions of the electrode post can be controlled by controlling the pattern and size of the through hole 116.
[0041] In this embodiment, during the step of providing the substrate 106, the substrate 106 includes a conductive connector 110 located on the top surface, and a through hole 116 exposes the conductive connector 110.
[0042] Specifically, the conductive connector 110 is located on the top surface of the substrate 106 and exposed by the through-hole 116, so that the bottom end of the subsequently formed electrode post can directly contact the conductive connector 110 and form an electrical connection. As an electrical connector between the internal circuit of the substrate 106 and the electrode post, the conductive connector 110 conducts the electrical signal or current of the electrode post to the functional circuit area inside the substrate 106, thereby enabling the semiconductor device to read or write the stored data associated with the electrode post through the electrode post during operation.
[0043] refer to Figure 9 A first dielectric layer 130 is formed in the through hole 116.
[0044] Specifically, the first dielectric layer 130 fills the through-hole 116 as a temporary filler material occupying the space of the through-hole 116. During the process of removing the sacrificial layer 101 to form an opening, the first dielectric layer 130 occupies the entire space of the through-hole 116, replacing the electrode post to support the insulating layer 102, thus preventing damage to the electrode post and maintaining structural stability during the removal of the sacrificial layer 101. Simultaneously, during the process of forming the electrode plate, the first dielectric layer 130 occupies the space of the through-hole 116, ensuring that the material filling the electrode plate can only fill the opening released after the sacrificial layer 101 is removed, and will not enter the interior of the through-hole 116. After the subsequent electrode plate is formed, the first dielectric layer 130 is removed to release the space of the through-hole 116 (i.e., forming the first through-groove), providing space for the subsequent formation of the electrode post.
[0045] In this embodiment, the material of the first dielectric layer 130 includes one or more of silicon nitride, polycrystalline silicon, amorphous silicon, silicon carbonitride, silicon oxide, monocrystalline silicon, silicon oxynitride, spin-coated organic carbon, spin-coated inorganic carbon, and amorphous carbon.
[0046] In the process of removing the sacrificial layer 101, the first dielectric layer 130 needs to have etching resistance, that is, the material of the first dielectric layer 130 should have a lower etching rate than the chemical reagent used to remove the sacrificial layer 101, so as to maintain structural integrity during the removal of the sacrificial layer 101 and continuously occupy the space of the via 116 to achieve physical isolation function; at the same time, the first dielectric layer 130 needs to have a high etching selectivity relative to the insulating layer 102 and the storage dielectric layer, so that when the first dielectric layer 130 is subsequently removed to form the first via, the first dielectric layer 130 can be removed cleanly without significantly eroding the sidewalls of the insulating layer 102 and the sidewalls of the electrode plate; and the material of the first dielectric layer 130 should also have good filling ability, and be able to fully fill the entire space of the via 116 through processes such as CVD (Chemical Vapor Deposition), ALD (Atomic Layer Deposition), or spin coating, so as to avoid the generation of voids or gaps in the via 116. Specifically, the material of the first dielectric layer 130 can be selected from the group consisting of silicon nitride, polycrystalline silicon, amorphous silicon, silicon carbonitride, silicon oxide, monocrystalline silicon, silicon oxynitride, spin-coated organic carbon, spin-coated inorganic carbon, and amorphous carbon, according to the above requirements.
[0047] refer to Figure 10 The sacrificial layer 101 is removed to form an opening 136 corresponding to the sacrificial layer 101. In this embodiment, the opening 136 exposes a portion of the sidewall of the first dielectric layer 130.
[0048] It should be noted that opening 136 provides space for the subsequent formation of the electrode plate.
[0049] In this embodiment, a wet etching process is used to remove the sacrificial layer 101.
[0050] For example, phosphoric acid can be used as an etchant when the sacrificial layer 101 is made of silicon nitride, or a wet etchant with an appropriate etching selectivity can be selected depending on the specific material of the sacrificial layer 101.
[0051] refer to Figure 11 A filling electrode plate 162 is formed in the opening 136. The electrode plate 162 includes a storage medium layer 160 surrounding and covering the inner wall of the opening 136 and a conductive layer 161 filling the remaining space of the opening 136.
[0052] Specifically, the electrode plate 162 is composed of a storage medium layer 160 and a conductive layer 161, wherein the storage medium layer 160 surrounds the inner wall covering the opening 136, meaning that the storage medium layer 160 first forms a continuous thin film on all the inner wall surfaces of the opening 136, thereby forming electrical isolation between the insulating layer 102 and the subsequently filled conductive layer 161, and between the sidewall of the subsequently formed electrode post and the conductive layer 161.
[0053] It should be noted that the storage medium layer 160, such as a variable resistance layer or a polarization layer, is a core functional thin film in a semiconductor device that realizes data storage. It stores data by changing resistance under the action of current or voltage (e.g., resistive random access memory), or by changing polarization state under the action of voltage (i.e., ferroelectric memory). The conductive layer 161 fills the remaining space of the opening 136 (i.e., the space inside the opening 136 that is not occupied after the storage medium layer 160 covers the inner wall of the opening 136). The conductive layer 161 serves as the conductive material part in the electrode plate 162, and together with the storage medium layer 160 and the electrode post, it forms a complete storage cell structure. The conductive layer 161 plays the role of transmitting electrical signals when the semiconductor device is working.
[0054] It should also be noted that in the process of forming electrode plate 162, since the first dielectric layer 130 occupies the entire space of the through hole 116, the material forming electrode plate 162 can only be deposited in the space of opening 136 and cannot enter the interior of through hole 116, thereby limiting electrode plate 162 to the area defined by opening 136.
[0055] In this embodiment, the storage medium layer 160 includes a variable resistance layer that stores data by changing resistance under the action of current or voltage, or a polarization layer that stores data by changing polarization state under the action of voltage.
[0056] It should be noted that the storage medium layer serves as the core functional layer of the memory. This storage medium layer includes a variable resistance layer that stores data through resistance changes under the influence of current or voltage, such as one or more of a magnetic tunnel junction material layer, a phase change material layer, or a resistive switching material layer. Alternatively, the storage medium layer may include a polarization layer that stores data through polarization state changes under the influence of voltage, such as a ferroelectric material layer. The resistive switching material layer may include, for example, metal oxides, such as hafnium oxide (HfO2) or tantalum oxide (TaO). xData storage methods include: 1) By applying voltage or current, conductive filaments are formed or broken within the layer, causing it to switch between low-resistivity and high-resistivity states; 2) Phase change material layers, such as chalcogenides like germanium-antimony-tellurium (GST), rapidly switch between crystalline and amorphous states by applying current pulses of varying amplitudes and widths, utilizing the resistance difference between the two states to store data; 3) Ferroelectric material layers, such as zirconium oxide (ZrO2), hafnium oxide (HfO2), zirconium-hafnium oxide (HZO), barium strontium titanate (SBT), or lead zirconate titanate (PZT), reverse the spontaneous polarization direction of the ferroelectric material during operation by applying an external electric field, utilizing different polarization states to store data.
[0057] Specifically, the storage medium layer includes a magnetic tunnel junction material layer, a ferroelectric material layer, a phase change material layer, or a resistive switching material layer, enabling the memory to be implemented as a magnetic random access memory (MRAM), a ferroelectric random access memory (FeRAM), a phase change random access memory (PCRAM), or a resistive random access memory (RRAM). However, it is not limited to these; as mentioned earlier, the materials filling the pillar structure 400 and the trench 170 can be set according to actual needs to achieve different memory structures.
[0058] The storage medium layer 160 surrounds the inner wall covering the opening 136, meaning that in this embodiment, it extends continuously in the opening 136 along the surface of the insulating layer 102 and the surface of the sidewall of the first medium layer 130, forming a continuous thin film layer that partially surrounds the conductive layer 161.
[0059] refer to Figure 12 Remove the first dielectric layer 130 and use the space area released by the first dielectric layer 130 as the first through groove 170.
[0060] Specifically, the first through groove 170 provides space for the subsequent formation of the electrode post 190.
[0061] In this embodiment, the process for removing the first dielectric layer 130 includes a wet etching process or a dry etching process.
[0062] refer to Figure 13 Electrode posts 190 are formed in the first through groove 170, and the electrode posts 190 cover the sidewalls of the storage medium layer 160 and the insulating layer 102.
[0063] Specifically, the electrode post 190 covers the sidewalls of the storage medium layer 160 and the insulating layer 102, which means that the electrode post 190 fills the entire space area of the first through slot 170 and is in direct contact with the sidewall of the storage medium layer 160. The electrode post 190 extends through the entire longitudinal height of the dielectric structure layer 100, so that it is electrically connected to the conductive connector 110 on the top surface of the substrate 106.
[0064] When the semiconductor device is operating, a memory cell structure is formed between the electrode post 190 and the conductive layer 161 of the electrode plate 162 through the memory medium layer 160. Electrical signals are transmitted to the memory medium layer 160 through the electrode post 190. In conjunction with the electrical signals provided by the conductive layer 161 of the electrode plate 162, write or read operations on the data state in the memory medium layer 160 are realized. Since the electrode post 190 is formed in the regular spatial channel released after the first dielectric layer 130 is removed, the morphology of the electrode post 190 is directly determined by the morphology of the first through-slot 170 and is not damaged by the etching process of removing the sacrificial layer. Therefore, the final electrode post 190 has a uniform morphology and a complete surface, avoiding the risk of irregular sidewall morphology and surface defects caused by the isotropic wet etching in traditional processes.
[0065] In this embodiment, the material of the electrode post 190 includes one or more of tungsten, titanium, titanium nitride, ruthenium, copper and aluminum.
[0066] Figures 14 to 18 This is a schematic diagram of the structure corresponding to each step in the second embodiment of the semiconductor device formation method of the present invention.
[0067] The similarities between the embodiments of the present invention and the first embodiment will not be repeated here. The differences between the embodiments of the present invention and the first embodiment are as follows: refer to Figure 14 A second dielectric layer 140 is formed on the sidewall and bottom of the through hole 116.
[0068] It should be noted that the second dielectric layer 140 is formed on the sidewall and bottom of the via 116, providing an isolation liner between the subsequently formed first dielectric layer 130 and the sidewall of the via 116. During the subsequent removal of the sacrificial layer 101 to form an opening, the first dielectric layer occupies the space of the via 116, while the second dielectric layer 140 is located between the first dielectric layer and the sidewall of the insulating layer 102. During the subsequent removal of the sacrificial layer 101, the second dielectric layer 140 can protect the first dielectric layer and prevent the chemical reagents used to remove the sacrificial layer 101 from corroding the sidewall of the first dielectric layer. Therefore, as long as the second dielectric layer 140 has etching selectivity relative to the sacrificial layer 101, the material requirements for the first dielectric layer can be reduced, and the filling and subsequent removal processes of the first dielectric layer can be simplified.
[0069] It should also be noted that in the subsequent process step of removing the first dielectric layer 130 to form the first through groove, the first dielectric layer 130 has a large volume and is removed from top to bottom. Therefore, the material located outside the sidewall of the first dielectric layer 130 will be in contact with the etchant used to remove the first dielectric layer 130 for a long time, and the contact time increases from bottom to top. This results in the material located outside the sidewall of the first dielectric layer 130 being eroded to varying degrees. The longer the contact time, the greater the degree of erosion. After removing the first dielectric layer 130, there is a risk of uneven lateral push of the material located outside the sidewall of the first dielectric layer 130. The presence of the second dielectric layer 140 ensures that when the first dielectric layer 130 is removed, the first through-hole exposes the second dielectric layer 140 first, rather than directly exposing the insulating layer 102 and the sidewall of the electrode plate 162. This prevents the process of removing the first dielectric layer from directly contacting and eroding the sidewall surfaces of the insulating layer 102 and the electrode plate. In other words, during the subsequent wet etching process to remove the first dielectric layer, the second dielectric layer 140 can block the wet etching solution from eroding the sidewalls of the insulating layer 102 and the electrode plate 162. At the same time, the second dielectric layer 140 is also formed at the bottom of the through-hole 116, covering the top surface of the substrate 106 exposed by the through-hole 116, thus protecting the exposed top surface of the substrate 106 during the subsequent removal of the first dielectric layer.
[0070] Furthermore, during the removal of the second dielectric layer 140, the etchant used for removal can simultaneously contact both the upper and lower parts of the second dielectric layer 140, rather than being removed gradually from top to bottom. Therefore, even when the etchant contacts the material outside the sidewalls of the second dielectric layer 140 during removal, the degree of erosion on the material outside the sidewalls of the second dielectric layer 140 tends to be uniform. Moreover, the thickness of the second dielectric layer 140 can be relatively thin, thus eliminating the need for excessive immersion in the etchant during removal, further reducing the erosion on the material outside the sidewalls of the second dielectric layer 140 and the resulting unevenness in transverse penetration. For example, the thickness of the second dielectric layer 140 is less than 20% of the critical dimension of the via 116.
[0071] In this embodiment, the thickness of the second dielectric layer 140 covering the sidewall of the through hole 116 gradually increases in the longitudinal direction and gradually away from the substrate 106.
[0072] Specifically, as mentioned above, the material located outside the sidewall of the first dielectric layer 130 will be in contact with the etchant used to remove the first dielectric layer 130 for a longer period of time, and the contact time increases from bottom to top, which in turn leads to an increase in the lateral thrust from bottom to top. In the subsequent removal of the first dielectric layer, the second dielectric layer 140, which is thicker in the top region, can absorb more lateral thrust, while the second dielectric layer 140, which is thinner in the bottom region, absorbs relatively less lateral thrust. Thus, after the first dielectric layer is removed, the remaining second dielectric layer 140 has a thickness that tends to be uniform in the longitudinal direction. The uniform thickness of the second dielectric layer 140 in the longitudinal direction enables the process of removing the second dielectric layer 140 to form the second through groove to have a consistent action time on the sidewalls of the insulating layer 102 and the electrode plate 162 at various locations in the longitudinal direction. This avoids the insulation layer 102 and the sidewalls of the electrode plate 162 being eroded to different degrees in the longitudinal direction due to the uneven thickness of the second dielectric layer 140, thereby ensuring the uniformity of the morphology of the first through groove and the second through groove formed in the longitudinal direction.
[0073] In this embodiment, the material of the second dielectric layer 140 includes one or more of silicon nitride, polycrystalline silicon, amorphous silicon, silicon carbonitride, silicon oxide, monocrystalline silicon, silicon oxynitride, spin-coated organic carbon, spin-coated inorganic carbon, and amorphous carbon.
[0074] It should be noted that the second dielectric layer 140 needs to have sufficient etching resistance in the process of removing the sacrificial layer 101. That is, the material of the second dielectric layer 140 should have a lower etching rate than the chemical reagent used to remove the sacrificial layer 101, so as to effectively protect the insulating layer 102 on the sidewall of the via 116 from being eroded during the removal of the sacrificial layer 101. At the same time, the second dielectric layer 140 also needs to have sufficient etching resistance in the process of removing the first dielectric layer. That is, the material of the second dielectric layer 140 should have a lower etching rate than the chemical reagent used to remove the first dielectric layer, so as to act as a barrier layer for lateral pushing during the removal of the first dielectric layer. Furthermore, the material of the second dielectric layer 140 should have a sufficiently high etching selectivity than the material of the insulating layer 102 and the sidewall material of the electrode plate 162, so that when the second dielectric layer 140 is subsequently removed to form the second via, the second dielectric layer 140 can be removed cleanly without significantly eroding the insulating layer 102 and the electrode plate 162. The specific material of the second dielectric layer 140 can be selected from the group of silicon nitride, polycrystalline silicon, amorphous silicon, silicon carbonitride, silicon oxide, monocrystalline silicon, silicon oxynitride, spin-coated organic carbon, spin-coated inorganic carbon, and amorphous carbon, depending on the actual materials of the first dielectric layer, insulating layer 102, and electrode plate 162.
[0075] refer to Figure 15 The first through groove 170 exposes the second dielectric layer 140.
[0076] It should be noted that when the second dielectric layer 140 is formed on the sidewall of the via 116 before the first dielectric layer is formed, the first through-groove formed after the first dielectric layer is removed exposes the surface of the second dielectric layer 140, rather than directly exposing the sidewalls of the insulating layer 102 and the electrode plate 162. During the removal of the first dielectric layer, the second dielectric layer 140 serves as a protective layer for the sidewalls of the insulating layer 102 and the electrode plate 162, reducing the probability that the sidewalls of the insulating layer 102 and the electrode plate 162 will be eroded by the etching process of removing the first dielectric layer. When the step of removing the first dielectric layer is completed, the surface of the second dielectric layer 140 exposed in the first through-groove is the etching starting surface for the subsequent removal of the second dielectric layer 140 to form the second through-groove.
[0077] refer to Figure 16 Remove the second dielectric layer 140 and use the space released by the second dielectric layer 140 as the second through groove 144. The second through groove 144 exposes the sidewalls of the insulating layer 102 and the electrode plate 162, and the second through groove 144 is connected to the first through groove 170.
[0078] Specifically, the second through-slot 144 is connected to the first through-slot 170, meaning that the first through-slot 170 and the second through-slot 144 together form a through-slot longitudinal spatial channel. The second through-slot 144 exposes the sidewalls of the insulating layer 102 and the electrode plate 162, providing a technological basis for the electrode post 190 to directly cover the sidewalls of the insulating layer 102 and the sidewalls of the electrode plate 162 (storage medium layer 160) when the electrode post 190 is subsequently formed in the first through-slot 170 and the second through-slot 144.
[0079] It should be noted that, since the second dielectric layer 140 has a relatively uniform thickness in the longitudinal direction, the process of removing the second dielectric layer 140 to form the second through groove 144 has a relatively uniform effect on the insulating layer 102 and the sidewall of the electrode plate 162 in the longitudinal direction, thereby making the final formed second through groove 144 have a uniform radial dimension in the longitudinal direction, thus ensuring that the subsequently formed electrode post 190 has a uniform radial dimension in the longitudinal direction.
[0080] In this embodiment, the process of removing the second dielectric layer 140 includes wet etching or dry etching.
[0081] refer to Figure 17 Remove the portion of the insulation layer 102 exposed in the second through groove 144 so that the sidewall of the electrode plate 162 protrudes beyond the sidewall of the remaining insulation layer 102, and use the space area freed by the removed insulation layer 102 as a horizontal groove 148, and the horizontal groove 148 communicates with the second through groove 144.
[0082] Specifically, based on the second through groove 144 exposing the insulating layer 102 and the sidewall of the electrode plate 162, a portion of the insulating layer 102 exposed in the second through groove 144 (i.e., the portion of the insulating layer 102 at the position of the sidewall of the second through groove 144) is further removed, so that the sidewall of the insulating layer 102 at the second through groove 144 is retracted inward relative to the sidewall of the electrode plate 162 (i.e., retracted radially away from the central axis of the second through groove 144), thereby causing the sidewall of the electrode plate 162 to protrude from the sidewall of the insulating layer 102.
[0083] It should be noted that the space released by the removed insulating layer 102 is the horizontal groove 148. The horizontal groove 148 is located radially on both the upper and lower sides of the protruding portion of the electrode plate 162's sidewall (i.e., the space formed between the remaining surface of the insulating layer 102 and the protruding portion of the electrode plate 162's sidewall after the insulating layer 102 has retracted). The horizontal groove 148 communicates with the second through groove 144, thereby increasing the contact area between the sidewall of the electrode plate 162 and the subsequently formed electrode pillars. In other words, the sidewall of the electrode plate 162 protrudes from the sidewall of the insulating layer 102, making... The increased exposed surface area of the electrode plate 162 in the second through groove 144 (including the side wall end face and the upper and lower surfaces of the protruding portion) allows the electrode pillars subsequently formed in the first through groove 170, the second through groove 144, and the horizontal groove 148 to simultaneously cover the side wall end face and the upper and lower surfaces of the protruding portion of the side wall of the electrode plate 162, thereby increasing the total contact area between the electrode pillars and the electrode plate 162. This increases the area of the memory cell without increasing the total thickness of the dielectric structure layer, and without increasing the difficulty of the etching process or the deposition process.
[0084] It should also be noted that the size of the sidewall of electrode plate 162 protruding from the sidewall of insulating layer 102 should not be too large or too small. If the size of the sidewall of electrode plate 162 protruding from the sidewall of insulating layer 102 is too large, it will increase the difficulty of filling the electrode pillar in horizontal groove 148 during the subsequent formation of electrode pillars, and increase the risk of voids in the electrode pillar formed in horizontal groove 148. At the same time, if the size of the sidewall of electrode plate 162 protruding from the sidewall of insulating layer 102 is too large, it means that too much of insulating layer 102 is removed, and the remaining thickness of insulating layer 102 is correspondingly reduced, which may weaken the electrical isolation capability of insulating layer 102 between adjacent electrode plates 162, and increase the risk of leakage or breakdown between adjacent electrode plates 162. If the size of the sidewall of electrode plate 162 protruding from the sidewall of insulating layer 102 is too small, it is not enough to significantly increase the contact interface between electrode pillar and electrode plate 162, resulting in the electrical performance of semiconductor device not being improved. Therefore, in this embodiment, the sidewall of the electrode plate 162 protrudes from the sidewall of the insulating layer 102 by a size ranging from 0.5 nanometers to 10 nanometers. For example, the sidewall of the electrode plate 162 protrudes from the sidewall of the insulating layer 102 by a size of 3 nanometers, 5 nanometers, or 7 nanometers.
[0085] refer to Figure 18 In the step of forming electrode post 190, electrode post 190 is also formed in second through groove 144.
[0086] Specifically, when the second dielectric layer 140 is present and removed to form the second through groove 144, the second through groove 144 is connected to the first through groove 170. When the electrode post 190 is formed, it not only fills the space of the first through groove 170, but also fills the space of the second through groove 144.
[0087] It should be noted that the electrode post 190 is formed in the second through groove 144, so that the electrode post 190 covers the surface of the storage medium layer 160 sidewall of the electrode plate 162. At the same time, the electrode post 190 is formed in the second through groove 144, which means that the cross-sectional size of the electrode post 190 in the radial direction is increased, so that the final electrode post 190 has a larger radial size and reduces the overall resistance of the electrode post 190.
[0088] In this embodiment, during the step of forming the electrode post 190, the electrode post 190 is also formed in the horizontal groove 148.
[0089] The electrode post 190 fills the horizontal groove 148, so that the electrode post 190 can wrap the upper and lower surfaces of the protruding part of the side wall of the electrode plate 162 and the end face of the protruding part, thereby significantly increasing the contact area between the electrode post 190 and the electrode plate 162. Without increasing the total thickness of the dielectric structure layer, the area of the memory cell is increased without increasing the difficulty of the etching process and the deposition process.
[0090] Accordingly, embodiments of the present invention also provide a semiconductor device.
[0091] The semiconductor device is formed by the semiconductor device formation method provided by the present invention.
[0092] For a detailed description of the semiconductor device, please refer to the preceding description; it will not be repeated here.
[0093] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.
Claims
1. A method for forming a semiconductor device, characterized in that, include: A substrate is provided, on top of which a dielectric structure layer is formed, the dielectric structure layer including sacrificial layers and insulating layers alternately stacked in a longitudinal direction, and a through-hole is formed on top of the substrate through the dielectric structure layer, the through-hole exposing the top surface of the substrate; A first dielectric layer is formed in the through hole; Remove the sacrificial layer to form an opening corresponding to the sacrificial layer; A filling electrode plate is formed in the opening, the electrode plate including a storage medium layer surrounding and covering the inner wall of the opening and a conductive layer filling the remaining space of the opening; Remove the first dielectric layer and use the space released by the first dielectric layer as the first through slot; An electrode post is formed in the first through-slot, the electrode post covering the sidewalls of the storage medium layer and the insulating layer.
2. The method for forming a semiconductor device as claimed in claim 1, characterized in that, The material of the first dielectric layer includes one or more of silicon nitride, polycrystalline silicon, amorphous silicon, silicon carbonitride, silicon oxide, monocrystalline silicon, silicon oxynitride, spin-coated organic carbon, spin-coated inorganic carbon, and amorphous carbon.
3. The method for forming a semiconductor device as claimed in claim 1, characterized in that, Before forming the first dielectric layer, the forming method further includes: A second dielectric layer is formed on the sidewall and bottom of the through hole; In the step of forming the first through groove, the first through groove exposes the second dielectric layer; After removing the first dielectric layer to form the first through-groove and before forming the electrode post, the forming method further includes: Remove the second dielectric layer and use the space released by the second dielectric layer as a second through groove. The second through groove exposes the sidewalls of the insulating layer and the electrode plate, and the second through groove communicates with the first through groove. In the step of forming the electrode post, the electrode post is also formed in the second through groove.
4. The method for forming a semiconductor device as claimed in claim 3, characterized in that, After removing the second dielectric layer and before forming the electrode post, the method further includes: removing a portion of the insulating layer exposed by the second through groove, so that the sidewall of the electrode plate protrudes beyond the sidewall of the remaining insulating layer, and using the space area released by the removed insulating layer as a horizontal groove, wherein the horizontal groove communicates with the second through groove; In the step of forming the electrode post, the electrode post is also formed in the horizontal groove.
5. The method for forming a semiconductor device as claimed in claim 3, characterized in that, The thickness of the second dielectric layer covering the sidewall of the through hole gradually increases in the direction along the longitudinal direction and gradually away from the substrate.
6. The method for forming a semiconductor device as claimed in claim 4, characterized in that, The sidewall of the electrode plate protrudes from the sidewall of the insulating layer in the range of 0.5 nanometers to 10 nanometers.
7. The method for forming a semiconductor device as claimed in claim 4, characterized in that, The material of the second dielectric layer includes one or more of silicon nitride, polycrystalline silicon, amorphous silicon, silicon carbonitride, silicon oxide, monocrystalline silicon, silicon oxynitride, spin-coated organic carbon, spin-coated inorganic carbon, and amorphous carbon.
8. The method for forming a semiconductor device as claimed in claim 1, characterized in that, In the step of providing the substrate, the substrate includes a conductive connector located on the top surface, and the through-hole exposes the conductive connector.
9. The method for forming a semiconductor device as claimed in claim 1, characterized in that, The storage medium layer includes a variable resistance layer that stores data by changing resistance under the action of current or voltage, or a polarization layer that stores data by changing polarization state under the action of voltage.
10. A semiconductor device, characterized in that, Formed using the method described in any one of claims 1 to 9.