A silicon wafer cleaning and etching integrated thickness removal measurement system and method

By using a six-slot integrated process layout and a multi-element composite calibration model, combined with constant pressure airflow shearing and intelligent weighing, the problem of non-destructive and high-precision measurement of silicon wafer etching removal was solved, realizing continuous flow and efficient measurement of silicon wafers in the rotating drum.

CN123124757APending Publication Date: 2026-11-17ZHEJIANG HAINA SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611128147.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot achieve non-destructive, high-precision online measurement of silicon wafer etching removal. Traditional methods are prone to causing scratches and breakage of silicon wafers, and the measurement results are subject to significant drift, making it difficult to meet the micron-level accuracy requirements.

Method used

By adopting a six-slot integrated process layout, a constant pressure airflow shearing mechanism, and a multi-element composite calibration model, combined with an intelligent weighing and lifting mechanism, the silicon wafers are continuously rotated in the rotating cage, the liquid film is peeled off, and the error is corrected by the algorithm to achieve high-precision measurement.

Benefits of technology

It achieves non-destructive, high-precision online measurement of silicon wafer etching thickness removal, improving measurement accuracy to the micrometer level, avoiding mechanical scratches and secondary contamination, and improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124757A_ABST
    Figure CN123124757A_ABST
Patent Text Reader

Abstract

This invention discloses an integrated thickness removal measurement system and method for silicon wafer cleaning and etching, belonging to the field of semiconductor manufacturing technology. The system includes an intelligent weighing hanger with embedded high-precision tensile and compressive sensors, a horizontal rotating cage, an intelligent weighing hanger mechanism, a constant-pressure airflow shearing mechanism, a six-tank process tank group, and a data processing and control system. The process tank group adopts a six-tank parallel architecture, consisting sequentially of a pre-etching chemical cleaning tank, a pre-etching QDR tank, a chemical etching tank, a post-etching QDR tank, a post-etching chemical cleaning tank, and a post-etching cleaning and post-QDR tank. This invention uses the weighing hanger to vertically lift the silicon wafer from the liquid surface through the second and sixth tanks and sweep it with an air knife, online collecting the static weight difference before and after etching. The control system then calls a pre-set multivariate calibration model to deduct the liquid film volume difference caused by microscopic morphology changes and the trace chemical residue density drift caused by multi-tank flow, accurately calculating the average thickness removal of the silicon wafer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor silicon wafer manufacturing and testing technology, specifically relating to an integrated thickness removal measurement system and method for silicon wafer cleaning and etching. Background Technology

[0002] In the manufacturing process of monocrystalline silicon wafers, the surface of the polished wafers contains a large number of mechanical damage layers, organic contaminants, and traces of metal ions. To remove these damage layers, acidic mixed acid solutions or strong alkaline solutions are typically used to chemically etch and thin the silicon wafers. Accurately monitoring the amount of silicon wafer removed during the chemical etching process is a crucial step in ensuring the stability of the batch process window.

[0003] Traditional thickness measurement methods often employ optical or mechanical contact methods. These methods cannot achieve full inspection, only sampling measurements of a small number of silicon wafers, making it difficult to accurately reflect the average thickness removal of the entire batch. Furthermore, the need to remove each wafer individually from the tumbler, with frequent mechanical handling and manual operation easily causing scratches, breakage, and secondary contamination. If weighing is performed directly in a wet state, a liquid film and suspended water droplets will adhere to the surface of the wafer when it is vertically lifted from the liquid surface. More importantly, the corrosion process fundamentally alters the microstructure of the silicon wafer surface, resulting in a significant difference in the volume of water droplets before and after corrosion. This causes severe drift in traditional wet weighing results, making it impossible to achieve micron-level thickness measurement accuracy.

[0004] Therefore, developing an integrated cleaning and corrosion thickness removal measurement system that is non-destructive, can automatically eliminate interference from residual liquid film mass drift, and achieves online high-precision measurement is an engineering problem that urgently needs to be solved in this field. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide an integrated silicon wafer cleaning and etching thickness removal measurement system and method. By combining a six-tank integrated process layout, constant pressure airflow to homogenize the liquid film, and a multi-component composite calibration model, the system eliminates quality interference caused by microscopic morphology evolution and chemical residues, and achieves online, non-destructive, and high-precision measurement of silicon wafer etching thickness removal.

[0006] An integrated thickness removal measurement system for silicon wafer cleaning and etching is used to process and measure the thickness of polished silicon wafers. The system includes a horizontal rotating drum, an intelligent weighing and lifting mechanism, a constant pressure airflow shearing mechanism, a six-slot process tank group, and a data processing and control system.

[0007] The horizontal rotating drum is arranged axially and has multiple sets of vertical parallel limiting slots inside, which can load multiple polished silicon wafers vertically in sequence along the horizontal direction, reducing the spacing between silicon wafers and increasing the production capacity of a single batch.

[0008] The intelligent weighing lifting device mechanism is used to grab, lift, move laterally and release the horizontal rotating cage. It is embedded with a high-precision tensile and compressive sensor, which can collect the overall gravity signal of the rotating cage in situ in a static hovering state. The high-precision tensile and compressive sensor is surrounded by a fully enclosed polytetrafluoroethylene protective shell, which can work stably for a long time in acid and alkali mist environments.

[0009] The vehicle drive system adopts a composite architecture of horizontal and vertical arms. Both the intelligent weighing lifting device and the constant-pressure airflow shearing mechanism are mounted on the vertical arm, employing a spatially coaxial but force-decoupled design. The constant-pressure airflow shearing mechanism is fixed to the vertical arm and located above the force reference plane of the weighing sensor. This mechanical isolation ensures that the weight of the air blade, the reaction force of the high-pressure airflow, and the drag stress of the air supply pipeline are all borne by the vertical arm, fundamentally eliminating physical interference with the sensor's micron-level weighing accuracy.

[0010] The constant pressure airflow shearing mechanism has a multi-angle rotation function. When the rotating drum is vertically lifted, the air knife can rotate and blow within a set angle range. Through the dynamic cross airflow shearing force, it can more efficiently peel off the microscopic residual droplets between the silicon wafers, ensuring the formation of an extremely uniform residual liquid film.

[0011] The six-tank process tank group is arranged compactly side by side according to the process sequence, as follows: the first tank is a pre-etching chemical cleaning tank, used to remove organic matter and metal contaminants from the silicon wafer surface to ensure uniform surface wetting; the second tank is a pre-etching QDR rapid flushing tank, used for rapid pure water replacement rinsing, and also serves as the initial wet weight measurement environment; the third tank is a chemical etching tank, used for chemical thinning or texturing etching of the silicon wafer; the fourth tank is a post-etching QDR rapid flushing tank, used for rapid pure water replacement to instantly terminate the etching reaction and prevent over-etching; the fifth tank is a post-etching chemical cleaning tank, used to remove microscopic byproducts, insoluble substances, and residual particles generated by the etching reaction; and the sixth tank is a post-etching QDR rapid flushing tank, used for final pure water rinsing and replacement, and also serves as the final wet weight measurement environment.

[0012] The data processing and control system is communicatively connected to the intelligent weighing and lifting device mechanism and the control components of each process tank. It is used to control the rotation of the robotic arm, process parameters and tank operation, and process gravity sensor data. Based on the difference between the static gravity signals before and after corrosion, combined with the preset multi-element residual composite calibration model, the system uses an algorithm to eliminate the mass drift of the residual liquid film and accurately calculate the average thickness removal amount of the batch of silicon wafers.

[0013] Furthermore, the six-slot process tank assembly is available in two material configurations to adapt to different process routes: When adapting to the acid etching process route, the first and fifth tanks are made of PVDF or PTFE material; the second, fourth and sixth tanks are made of PVDF material; the third tank is made of PTFE or PVDF material. The entire tank is free of quartz glass material and can withstand the corrosion of the hydrofluoric acid mixed acid system.

[0014] When adapting to the alkaline corrosion process route, the first, second, fourth, fifth and sixth tanks are made of high-purity quartz or PFA material; the third tank is made of stainless steel lined with PFA material or high-purity quartz material, which can withstand high temperature and high concentration of strong alkaline solution corrosion, while eliminating the risk of leaching of metal ions and additives.

[0015] The axial length of the constant pressure airflow shearing mechanism covers the entire axial length of the horizontal rotating cage, and the spray medium is high-pressure nitrogen. The constant pressure airflow shearing mechanism is arranged parallel to the horizontal axis of the horizontal rotating cage and is configured such that, during the synchronous lifting and lowering process with the vertical lifting arm, its spraying part always maintains a preset lateral purging distance from the horizontal rotating cage.

[0016] Furthermore, the present invention also provides a method for measuring the thickness removal amount of silicon wafers through integrated cleaning and etching using the above system. This method employs a continuous flow process, eliminating the need for intermediate drying of the silicon wafers during the process. Specifically, it includes the following steps: S1: Silicon wafer loading and pre-cleaning: Multiple silicon wafers to be processed and ground are vertically inserted into a horizontal rotating drum. The rotating drum is picked up by an intelligent weighing and lifting mechanism and sent to the first tank for chemical cleaning. Then it is transferred to the second tank for pure water rapid rinsing and surface pre-wetting.

[0017] S2: Initial Weighing Before Corrosion: After the second tank rinsing is completed, the lifting device is controlled to vertically lift the rotating cage out of the liquid surface at a preset first speed. After being swept and blown away by the constant pressure airflow shearing mechanism above the liquid surface to remove suspended water droplets, it is statically suspended at a preset height until the liquid flow stabilizes. The static total weight at this time is collected and recorded as the initial weight. .

[0018] S3: Etching and post-cleaning: Keep the silicon wafer fully wet and transfer the rotating drum to the third tank for chemical etching; after the set etching time is reached, transfer it sequentially to the fourth tank for QDR rinsing to terminate the reaction, the fifth tank for post-etching chemical cleaning to remove residue, and the sixth tank for final pure water rapid rinsing.

[0019] S4: Final Weighing After Corrosion: After rinsing the sixth tank, the lifting device is used to vertically lift the rotating cage out of the liquid surface at a second speed identical to the first speed. After being purged by a constant-pressure airflow shearing mechanism with the same parameters, it is statically suspended at the same height for the same duration. The static overall weight at this time is collected and recorded as the final weight. .

[0020] S5: Thickness Removal Calculation: The data processing and control system retrieves the corresponding multi-element residual composite calibration model based on the current process type, and calculates the gravity difference value. Excluding total residual quality error throughout the entire process Then, the total mass of the silicon wafer etched is taken into account, combined with the number of silicon wafers loaded. single silicon wafer area and single crystal silicon density The average thickness removal amount of this batch of silicon wafers was calculated. .

[0021] Furthermore, the total residual mass error throughout the entire process satisfies ,in The composite correction coefficient is a characteristic constant that is pre-stored through a multi-dimensional calibration experiment of the entire process before the process is run. It can correct two types of errors at the same time: one is the difference in the volume of the retained liquid film caused by the evolution of the surface micromorphology before and after corrosion, and the other is the liquid film density drift caused by the flow and adsorption of the liquid in multiple tanks.

[0022] Furthermore, the composite correction coefficient takes different values ​​for different corrosion processes: Under acid corrosion route, the acid corrosion composite correction factor is used. .

[0023] Under the alkaline corrosion route, an alkaline corrosion composite correction factor is adopted. .

[0024] Furthermore, the aforementioned pre-process multivariate calibration experiment is performed before the machine leaves the factory or before the formula is changed. The specific steps are as follows: a) Initial state calibration: Take several ( Unetched and ground silicon wafers (area: ), determine the absolute dry total mass ( The silicon wafers are loaded into a rotating drum (1) and sequentially cleaned with a chemical solution in the first tank (51) and rinsed with pure water in the second tank (52). They are then lifted out of the liquid at the first speed and swept by an air knife and suspended for stabilization. The initial total weight in the fully wet state is then measured. The difference between the two ( ) divided by the total surface area ( ) Obtain the initial state cutoff coefficient ; b) Final state calibration: After the silicon wafer is sent into the third tank (53) to complete the target etching, it is continuously wet-state flowed through the fourth tank (54), the fifth tank (55), and the sixth tank (56) to complete the cleaning. After being lifted out of the liquid surface at the second speed and subjected to the same purging and suspension, the final total weight of the whole wet state is measured. Then, thoroughly dry the silicon wafers and measure the total drying mass. The difference between the two ( ) divided by the total surface area ( ), to obtain the final state cutoff coefficient ; c) Calculate the composite correction factor , and store it as a characteristic constant of the corresponding process in the control system (6).

[0025] Furthermore, the formula for calculating the average thickness removal amount is: ; In the formula: This represents the theoretical density of current monocrystalline silicon wafers; Furthermore, the polished silicon wafers are 4-8 inch monocrystalline silicon wafers with an initial nominal thickness of 500-1200 μm, and the number of wafers loaded in the horizontal rotary drum is [not specified]. The number of pieces is 100, and the process target is an average thickness removal of 20-60 μm.

[0026] Beneficial effects:

[0027] This invention integrates cleaning, etching, and measurement into a compact six-slot layout. The silicon wafers continuously rotate within the rotating drum throughout the process, eliminating the need for individual wafer removal and completely avoiding the risks of scratches, fragments, and secondary contamination caused by mechanical gripping. At the same time, it enables full-batch online measurement, which more accurately reflects the overall quality of the batch compared to sampling inspection, resulting in higher production efficiency. This invention uses a constant-pressure airflow air knife to peel suspended water droplets into a uniform liquid film. Combined with a multi-component composite calibration model, it simultaneously deducts the liquid film volume change caused by microscopic morphology evolution and the density drift caused by drug residue from the algorithm level, improving the accuracy of wet weighing to the micrometer level and meeting the monitoring requirements of precision processing of semiconductor silicon wafers. The core weighing sensor of this invention uses PTFE fully enclosed protection, which does not directly contact acid and alkali mist; the tank material is specially selected for corrosion protection for acid and alkali processes, the system has a long service life and low maintenance cost in harsh wet chemical environments; at the same time, the measurement link has no complex optical or contact moving parts, so the reliability is high. Attached Figure Description

[0028] The invention will now be further described with reference to the accompanying drawings; Figure 1 This is a schematic diagram of the overall three-dimensional structure of the thickness removal measurement system of the present invention; Figure 2 This is a schematic diagram of the horizontal rotating cage of the present invention in a suspended weighing state; Figure 3 This is a schematic diagram of the six-slot process tank assembly in this invention. Figure 4 This is a block diagram illustrating the data processing principle of the multivariate composite calibration model of the present invention. Figure 5This is a complete process flow diagram of the thickness removal measurement method of the present invention; Figure 6 This is a screenshot of the system's operating interface.

[0029] (1) Horizontal rotating cage; (2) Grinding silicon wafer; (3) Intelligent weighing and lifting mechanism; (4) Constant pressure airflow shearing mechanism; (5) Six-slot process tank group; (6) Data processing and control system; (7) Sliding bracket; (8) Overhead crane boom; (9) Vertical arm; (51) First slot; (52) Second slot; (53) Third slot; (54) Fourth slot; (55) Fifth slot; (56) Sixth slot. Detailed Implementation

[0030] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0031] The technical solutions of this application will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are merely some embodiments of this application, and not all embodiments. The components of this application described and shown in the drawings can generally be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of this application provided in the drawings is not intended to limit the scope of the claimed application, but merely to illustrate selected embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application.

[0032] It should be noted that similar reference numerals and letters in the following figures indicate similar items; therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures. Furthermore, in the description of this application, terms such as "first," "second," etc., are used only to distinguish descriptions and should not be construed as indicating or implying relative importance.

[0033] Example 1

[0034] like Figure 1 - Figure 3 As shown, Example 1 discloses an integrated thickness removal measurement system for silicon wafer cleaning and etching. This system is an integrated measurement system adapted to the alkaline etching texture process of 4-8 inch polished silicon wafers.

[0035] The system includes a horizontal rotating cage 1, an intelligent weighing and lifting device mechanism 3, a constant pressure airflow shearing mechanism 4, a six-slot process tank group 5, and a data processing and control system 6.

[0036] The horizontal rotating drum 1 is arranged horizontally along the axis and has 100 sets of parallel and vertical limiting slots inside, which can load 100 8-inch polished silicon wafers 2 vertically in sequence along the horizontal direction, with the silicon wafer spacing maintained at 2mm, maximizing the single batch production capacity in a limited space.

[0037] The system's traveling and driving architecture adopts an XY-axis orthogonal motion system. Specifically, a sliding bracket 7 is installed on the rear side of the six-slot process tank group 5, and the horizontal traveling crane boom 8 is slidably connected to the sliding bracket 7, preferably driven by an electric telescopic rod for translation; a downwardly extending vertical lifting arm 9 is slidably connected to the horizontal traveling crane boom 8.

[0038] In the specific mechanical connection and control structure, the intelligent weighing lifting device 3 and the constant pressure airflow shearing mechanism 4 are jointly installed on the vertical lifting arm 9, used for gripping, lifting, lateralizing, and releasing the horizontal rotating cage 1. To balance the high-precision weighing and efficient purging of the silicon wafer grinding group 2, this embodiment employs a special force-measuring decoupling design for the installation position and operation mode of the constant pressure airflow shearing mechanism 4: The intelligent weighing lifting device 3 contains a high-precision tensile and compressive force sensor with a precision of 0.01%. A horizontal rotating cage 1 is suspended below it, allowing for real-time acquisition of the overall gravity signal of the horizontal rotating cage 1 and the polished silicon wafer 2 in a static, suspended state. To resist corrosion from high-temperature, high-concentration alkaline mist, the high-precision tensile and compressive force sensor is encased in a fully sealed PTFE protective shell. Precision leads are led out through fully sealed PTFE flexible tubing and connected to an external data processing and control system 6.

[0039] The constant pressure airflow shearing mechanism 4 is rigidly fixed to the vertical lifting arm 9, and its physical installation position is above the force transmission path of the high-precision tension and compression sensor. This decoupled design ensures that during static hovering and weighing, the weight of the shearing air knife and the drag stress generated by the external connecting air pipe are directly transmitted to the rigid vertical lifting arm 9, completely bypassing the high-precision tension and compression sensor below, thus achieving precise mechanical isolation.

[0040] Secondly, the end exhaust air knife of the constant pressure airflow shearing mechanism 4 integrates a rotary drive component, such as a rotary drive servo component or a stepping cylinder, which can rotate and oscillate at a certain angle according to a preset program. When the vertical lifting arm 9 drives the horizontal rotating cage 1 to lift the liquid surface at a preset speed, the constant pressure airflow shearing mechanism 4 not only rises synchronously with the vertical lifting arm 9, but its air knife also dynamically rotates and sweeps at a set angle (e.g., within a 90° range). The multi-angle airflow directly cuts into the gap of the polished silicon wafer 2 with a spacing of only 2mm, which can effectively destroy the surface tension of the liquid, completely peel off the suspended droplets at the lower edge, and greatly improve the consistency of the residual liquid film in the initial and final states.

[0041] The six-tank process tank group 5 adopts a compact, side-by-side linear layout of six tanks, which are arranged in the following order according to the process flow: the first tank 51 is the pre-corrosion chemical cleaning tank, the second tank 52 is the pre-corrosion QDR quick flushing tank, the third tank 53 is the chemical corrosion tank, the fourth tank 54 is the post-corrosion QDR quick flushing tank, the fifth tank 55 is the post-corrosion chemical cleaning tank, and the sixth tank 56 is the post-corrosion QDR quick flushing tank.

[0042] This embodiment is adapted to high-temperature strong alkali corrosion process, therefore the tank material adopts special configuration for alkali corrosion: the tank body, pipeline and spray head of the first tank 51, the second tank 52, the fourth tank 54, the fifth tank 55 and the sixth tank 56 are all made of high-purity quartz glass or high-temperature resistant PFA material; the third tank 53 is the core corrosion reaction zone, which uses stainless steel as the load-bearing shell, and is lined with a high-density PFA coating with a thickness of more than 5mm. It contains a 15% KOH strong alkali solution and adds isopropanol to adjust the surface tension. The tank body is equipped with a heating cable to keep the temperature of the solution constant at 80℃.

[0043] The data processing and control system 6 communicates with the lifting device drive, sensors, tank valves, heating components, etc., and can automatically control the process flow, parameter adjustment, and data calculation. It has a built-in multi-element composite calibration model database, which can automatically retrieve the corresponding correction coefficients according to the process formula to accurately calculate the thickness removal amount. When the system switches to an acid etching process route, only the tank material configuration needs to be changed: the first tank 51 and the fifth tank 55 are made of PVDF or PTFE; the second tank 52, the fourth tank 54, and the sixth tank 56 are made of PVDF; the third tank 53 is made of PTFE or PVDF. The entire system does not use quartz glass components, thus withstanding the corrosion of the hydrofluoric acid mixed acid system and adapting to different process requirements.

[0044] Example 2

[0045] like Figure 4 - Figure 6As shown, a method for measuring the thickness removal amount of silicon wafers through integrated cleaning and etching is disclosed. This embodiment is based on the system implementation of Embodiment 1 and includes two stages: pre-process multivariate calibration and mass production online measurement. The complete data processing logic and process flow are as follows: Figure 3 , Figure 4 As shown.

[0046] Phase 1: Pre-production multi-component calibration experiment. This calibration experiment is performed before the machine is put into mass production or when the process formula is changed to determine the composite correction coefficient of the corresponding process. This example uses the alkaline corrosion process as an example: S1. Initial State Calibration: Select 100 standard 8-inch polished silicon wafers 2, and measure the absolute total mass of dried material offline using a high-precision balance, denoted as . The silicon wafer 2 is loaded into the horizontal rotating drum 1 and sent to the first tank 51 for surface cleaning and activation with SC-1 solution via the intelligent weighing and lifting mechanism 3. It is then transferred to the second tank 52 for pure water rinsing. After rinsing, the vertical lifting arm 9 is controlled to lift vertically upwards at a uniform speed of 10mm / s, hovering at a height of 20cm above the liquid surface. During the lifting process, the constant pressure airflow shearing mechanism 4, which moves synchronously with the vertical lifting arm 9, activates the air knife and performs dynamic rotational sweeping and blowing twice within a 90° range via the rotation drive component. After the droplets stabilize, the static weight signal from the high-precision tensile and compressive sensor is read to obtain the initial total weight in the fully wet state, denoted as [missing value]. .

[0047] The initial state cutoff coefficient is calculated using the following formula: ; In the formula, =100 represents the number of polished silicon wafers loaded. The value represents the macroscopic area of ​​a single side of a single polished silicon wafer, and the coefficient 2 corresponds to the two surfaces of the polished silicon wafer.

[0048] S2. Final State Calibration: Maintaining the silicon wafer 2 in a fully wet state, directly immerse the horizontal rotating drum 1 into the high-temperature KOH etching solution in the third tank 53 for a set reaction time, allowing a regular microscopic pyramid texture to form on the surface of the silicon wafer 2. After the etching time is reached, remove the horizontal rotating drum 1 and sequentially send it to the fourth tank 54 for pure water rinsing to terminate the reaction, the fifth tank 55 for neutralizing and cleaning residual alkali with dilute hydrochloric acid, and the sixth tank 56 for final pure water rapid rinsing. After rinsing, the vertical lifting arm 9 vertically lifts the horizontal rotating drum 1 at a uniform speed of 10mm / s to 20cm above the liquid surface. The constant pressure airflow shearing mechanism 4 performs dynamic rotational sweeping and blowing twice with the same parameters. After stabilization, read the static weight signal from the high-precision tensile and compressive sensor to obtain the final total weight in the fully wet state, denoted as [missing value]. The rotating drum is then transferred to the drying chamber for thorough drying. The polished silicon wafer 2 is removed and weighed to obtain the final total dried mass, denoted as [missing information]. .

[0049] The final state cutoff coefficient is calculated using the following formula:

[0050] This coefficient simultaneously incorporates the capillary water-locking effect of micromorphological evolution, as well as the influence of density changes in residual drug solution in multiple tanks.

[0051] S3. Calculation of Composite Correction Coefficient: The composite correction coefficient for the alkaline corrosion process is calculated according to the following formula:

[0052] This coefficient is used as a characteristic constant of the alkaline corrosion formulation and permanently stored in the database of the data processing and control system 6. For acid corrosion processes, the acid corrosion composite correction coefficient is obtained through the same calibration procedure. This value is positive, corresponding to the liquid film reduction effect caused by surface smoothing after acid polishing.

[0053] Phase Two: When the online measurement system is officially put into mass production, online measurement is performed according to the following steps. In this embodiment, the target corrosion removal amount is 30µm: S4: Silicon Wafer Loading and Pre-Cleaning: The wafer decoupling machine vertically loads 100 8-inch polished silicon wafers 2 into the horizontal rotating drum 1. The single-sided area of ​​a single wafer is approximately S≈314cm². 2 The initial nominal thickness is 800um. The intelligent weighing and lifting device 3 grabs the horizontal rotating cage 1 and sends it into the first tank 51 for chemical cleaning, and then transfers it to the second tank 52 for QDR rinsing and wetting.

[0054] S5: Initial Weighing and Sweeping: After the second tank 52 is rinsed, the vertical lifting arm 9 lifts the horizontal rotating cage 1 vertically out of the liquid surface at a uniform speed of 10mm / s, and suspends it statically 20cm above the liquid surface; during this process, the constant pressure airflow shearing mechanism 4 activates the air knife to perform 90° dynamic rotation sweeping and blowing twice; after the liquid flow stabilizes, the high-precision tension and pressure sensor, due to its decoupling from the shearing mechanism, can accurately collect the pure static total gravity signal, which is recorded as the initial weight by the data processing and control system 6. .

[0055] S6: Chemical corrosion and post-cleaning: The vertical lifting arm 9 directly puts the wet horizontal rotating cage 1 into the KOH corrosion solution in the third tank 53 for chemical corrosion with a target removal amount of 30um; after the set reaction time is reached, it is taken out and sequentially sent to the fourth tank 54 for quick flushing to terminate the reaction, the fifth tank 55 for chemical cleaning to remove particulate residue, and the sixth tank 56 for final quick flushing with ultrapure water.

[0056] S7: Final Weighing and Sweeping: After rinsing the sixth tank 56, the vertical lifting arm 9 lifts the horizontal rotating cage 1 vertically out of the liquid surface at a uniform speed of 10mm / s, suspending it at the same height. The constant pressure airflow shearing mechanism 4 performs dynamic rotation sweeping and purging twice with the same parameters. After stabilization, the static total gravity signal is collected, and the data processing and control system 6 records it as the final weight, denoted as [missing value]. .

[0057] S8: Thickness Removal Calculation: The data processing and control system 6 automatically retrieves the pre-stored alkaline corrosion composite correction coefficient. The coefficient is negative, corresponding to the weight gain effect caused by water retention due to surface texture after corrosion. Substituting the weight difference into the calculation formula:

[0058] Among them, the theoretical density of single-crystal silicon r =2.33g / cm 3 , N =100, S =314cm 2 By subtracting the composite residual error term, the net mass of the silicon wafer 2 that was etched and dissolved is accurately restored, and the average thickness removal amount of this batch of silicon wafer 2 is finally calculated. This method requires no intermediate drying throughout the process. The silicon wafer 2 is continuously rotated within the horizontal rotating drum 1 without any additional mechanical contact. Through the combination of hardware isolation decoupling, dynamic homogenization of the liquid film, and software calibration correction, micron-level measurement accuracy can be achieved, fully meeting the online monitoring requirements of the batch etching process for semiconductor silicon wafers.

[0059] Those skilled in the art will understand that the above embodiments are merely preferred embodiments of the present invention. When switching to an acid etching process, only the tank material needs to be changed accordingly, and the acid etching composite correction coefficient needs to be adjusted. All equivalent substitutions and partial improvements made within the six-tank integrated architecture and multi-element composite calibration logic of the present invention fall within the protection scope of the present invention.

[0060] The above are merely embodiments of this application and are not intended to limit the scope of protection of this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of protection of this application.

[0061] The above formulas are all derived from software simulation using a large amount of data, and are selected to be close to the actual values. The coefficients in the formulas are set by those skilled in the art based on the actual situation. The above are only preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or changes made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A system for measuring the thickness removal of a silicon wafer cleaning and etching integrated system for processing and measuring a ground silicon wafer (2), characterized by, The system includes a horizontal rotating drum (1), an intelligent weighing lifting device mechanism (3), a constant pressure airflow shearing mechanism (4), a six-slot process tank group (5), and a data processing and control system (6). The horizontal rotating cage (1) is arranged horizontally along the axis and has several sets of vertically parallel limiting slots inside, which are used to vertically insert and load multiple polishing silicon wafers (2) in sequence along the transverse direction. The intelligent weighing lifting device mechanism (3) is used to grab, lift, move laterally and release the horizontal rotating cage (1), and a high-precision tensile and compressive sensor is nested inside it; The system also includes a horizontal overhead crane boom (8) and a vertical lifting boom (9) connected to the horizontal overhead crane boom (8); the intelligent weighing lifting device (3) and the constant pressure airflow shearing mechanism (4) are both mounted on the vertical lifting boom (9); The constant pressure airflow shearing mechanism (4) is fixed on the vertical lifting arm (9) and located above the force transmission path of the high-precision tension and pressure sensor. The constant pressure airflow shearing mechanism (4) is equipped with an angle-adjustable rotary drive component at the injection part, which is used to perform rotary sweeping and blowing on the surface of the horizontal rotating cage (1) and the polishing silicon wafer (2) that are lifted out of the liquid surface within a preset angle range. The six-tank process tank group (5) is arranged side by side according to the process flow sequence, including: the first tank (51) is the pre-corrosion cleaning tank; the second tank (52) is the pre-corrosion QDR quick flushing tank; the third tank (53) is the chemical corrosion tank; the fourth tank (54) is the post-corrosion QDR quick flushing tank; the fifth tank (55) is the post-corrosion cleaning tank; and the sixth tank (56) is the post-corrosion QDR quick flushing tank. The data processing and control system (6) is connected to the intelligent weighing hoist mechanism (3) and the control components of each process tank, respectively, and is used to calculate the average thickness removal amount of the polished silicon wafer (2) based on the difference between two static gravity signals collected by the intelligent weighing hoist mechanism (3) at the second tank (52) and the sixth tank (56) and the preset multi-element residual composite calibration model.

2. The integrated silicon wafer cleaning and etch thickness removal measurement system of claim 1, wherein: When adapting to the acid corrosion process route, the material configuration of the six-tank process tank group (5) is as follows: the first tank (51) and the fifth tank (55) are made of PVDF or PTFE; the second tank (52), the fourth tank (54) and the sixth tank (56) are made of PVDF; the third tank (53) is made of PTFE or PVDF to withstand corrosion of the nitric acid / hydrofluoric acid mixed acid system.

3. The integrated silicon wafer cleaning and etch thickness removal measurement system of claim 1, wherein: When adapting to the alkaline corrosion process route, the material configuration of the six-tank process tank group (5) is as follows: the first tank (51), the second tank (52), the fourth tank (54), the fifth tank (55) and the sixth tank (56) are made of high-purity quartz or PFA material; the third tank (53) is made of stainless steel lined with PFA material or high-purity quartz material, which is used to withstand the corrosion of high temperature and high concentration of strong alkaline solution and reduce the risk of leaching.

4. The integrated etch and thickness removal measurement system for cleaning a silicon wafer of claim 1, wherein, The axial length of the constant pressure airflow shearing mechanism (4) covers the entire axial length of the horizontal rotating cage (1), and the spray medium is high pressure nitrogen. The constant pressure airflow shearing mechanism (4) is arranged parallel to the horizontal axis of the horizontal rotating cage (1) and is configured such that during the synchronous lifting and lowering process with the vertical lifting arm (9), its spraying part always maintains a preset lateral purging distance with the horizontal rotating cage (1).

5. A method for measuring the thickness removal of a silicon wafer by cleaning and etching in an integrated system according to any one of claims 1 to 4, characterized in that, The continuous flow process eliminates the need for intermediate drying of silicon wafers throughout the entire process, including the following steps: S1: Vertically insert multiple silicon wafers to be processed into a horizontal rotating cage (1), and send the rotating cage (1) into the first tank (51) for cleaning with chemical solution through the intelligent weighing and lifting mechanism (3), and then transfer it to the second tank (52) for quick flushing with pure water and surface pre-wetting. S2: After the second tank (52) is rinsed, the intelligent weighing lifting device (3) is controlled to vertically lift the rotating cage (1) out of the liquid surface at a preset first speed. After the constant pressure airflow shearing mechanism (4) sprays high-pressure gas to sweep away and peel off the residual liquid, it is statically suspended at a preset height above the liquid surface for a first preset time. The static weight at this time is collected and recorded as the initial weight. ; S3: Transfer the rotating drum (1) to the third tank (53) for chemical corrosion. After the set corrosion time is reached, transfer it to the fourth tank (54) to stop corrosion rinsing, the fifth tank (55) for chemical cleaning after corrosion, and the sixth tank (56) for final pure water fast flushing. S4: After the sixth tank (56) is rinsed, the intelligent weighing lifting device (3) is controlled to lift the rotating cage (1) vertically out of the liquid surface at a second speed with the same first speed. After being purged by the constant pressure airflow shearing mechanism (4) with the same parameters, it is statically suspended at the same height for the same second preset time as the first preset time. The static weight at this time is collected and recorded as the final weight. ; S5: Data Processing and Control System (6) Retrieves the corresponding multi-element residual composite calibration model according to the current corrosion process type, and calculates the gravity difference value. Excluding total residual quality error throughout the entire process Then, the total mass of the silicon wafer etched is taken into account, combined with the number of silicon wafers loaded. single silicon wafer area and single crystal silicon density The average thickness removal amount of this batch of silicon wafers was calculated. .

6. The method for determining the thickness removal amount of silicon wafers through integrated cleaning and etching according to claim 5, characterized in that, The total residual mass error of the whole process satisfies: ; In the formula, The composite correction coefficient is a characteristic constant pre-stored through a multivariate calibration experiment before process operation. It is used to simultaneously correct for differences in the volume of the retained liquid film caused by surface micromorphology evolution, and for liquid film density drift caused by multi-tank liquid flow and adsorption. The composite correction coefficient under acid corrosion circuitry is... The composite correction factor for alkaline corrosion circuits is: .

7. The method for determining the thickness removal amount of silicon wafers through integrated cleaning and etching according to claim 6, characterized in that, When the process is acid corrosion, the third tank (53) uses an HF / HNO3 / CH3COOH mixed acid system for isotropic chemical corrosion; the composite correction coefficient is obtained from the acid corrosion pre-calibration. It is used to compensate for the weight loss interference caused by the reduction in liquid film volume due to the smoothing of the silicon wafer surface after acid polishing.

8. The method for determining the thickness removal amount of silicon wafers through integrated cleaning and etching according to claim 6, characterized in that, When the process is alkaline corrosion, the third tank (53) uses a strong alkaline solution system of KOH or NaOH to perform anisotropic corrosion to form a pyramid texture; the composite correction coefficient is obtained by referring to the alkaline corrosion composite correction coefficient obtained by pre-calibration of alkaline corrosion. It is used to deduct the weight gain interference caused by the increase in volume of capillary water-locking in the microstructure and the increase in liquid film density due to drug residue.

9. The method for determining the thickness removal amount of silicon wafers through integrated cleaning and etching according to claim 7 or 8, characterized in that, The pre-process multivariate calibration experiment includes the following steps: a) Initial state calibration: Take several ( Unetched and ground silicon wafers (area: ), determine the absolute dry total mass ( The silicon wafers are loaded into a rotating drum (1) and sequentially cleaned with a chemical solution in the first tank (51) and rinsed with pure water in the second tank (52). They are then lifted out of the liquid at the first speed and swept by an air knife and suspended for stabilization. The initial total weight in the fully wet state is then measured. The difference between the two ( ) divided by the total surface area ( ) Obtain the initial state cutoff coefficient ; b) Final state calibration: After the silicon wafer is sent into the third tank (53) to complete the target etching, it is continuously wet-state flowed through the fourth tank (54), the fifth tank (55), and the sixth tank (56) to complete the cleaning. After being lifted out of the liquid surface at the second speed and subjected to the same purging and suspension, the final total weight of the whole wet state is measured. Then, thoroughly dry the silicon wafers and measure the total drying mass. The difference between the two ( ) divided by the total surface area ( ), to obtain the final state cutoff coefficient ; c) calculating a complex correction factor which are stored in the control system (6) as characteristic constants of the corresponding process.

10. The method of claim 6 wherein the thickness removal is determined by the equation: ###0001### where: t = thickness removal, A = area of the wafer, t = thickness of the wafer, and t = thickness of the wafer after cleaning. The average thickness removal amount The calculation formula is: ; In the formula: is the theoretical density of the current single crystal silicon wafer.