Multi-component mixed acid stepwise etching process for precise removal of damage layer on the back of silicon wafer
By using a multi-component mixed acid stepwise etching process, which is divided into two stages—pre-etching and main etching—the problem of low surface cleanliness and poor etching precision in traditional etching processes is solved. This process significantly improves the surface cleanliness and electrical performance of silicon wafers, making it suitable for the large-scale production of high-end silicon wafers.
Patent Information
- Application Number
- CN202611295388.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, traditional single-ratio strong acid mixture etching processes suffer from low surface cleanliness, poor etching precision, and narrow process window when removing the damaged layer on the back of silicon wafers, making it difficult to meet the requirements of high-end silicon wafers for high lifespan, high uniformity, and high reliability.
The process employs a multi-component mixed acid stepwise etching process, which is divided into two stages: pre-etching and main etching. A low-concentration slow-release mixed acid system is used for pre-etching to remove surface particles and shallow metal contamination. Subsequently, a constant-temperature and constant-speed mixed acid system is used for main etching to remove subsurface microcracks and lattice damage layers. The process is completed by gradient pure water rinsing and inert gas drying.
It significantly improves the surface cleanliness and batch consistency of silicon wafers, reduces surface dangling bond density and minority carrier lifetime decay, meets the high requirements of automotive-grade and power-grade silicon wafers, and is suitable for mass production.
Smart Images

Figure CN123124770A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor silicon wafer processing technology, specifically to a multi-component mixed acid step-by-step etching process for precise removal of the damage layer on the back side of a silicon wafer. Background Technology
[0002] With the rapid development of the semiconductor industry, 8-inch silicon wafers are increasingly widely used in automotive-grade IGBTs, power devices, and high-end integrated circuits. During the manufacturing process of silicon wafers, after diamond wire cutting and double-sided grinding, a layer of mechanical damage of uneven thickness inevitably forms on the surface of the silicon wafer (especially the back side). This damage layer contains a large number of microcracks, lattice distortions, and high-density dislocations, while the surface is also covered with microparticles, grinding fluid residues, and metal ion impurities introduced by the grinding process.
[0003] If these surface impurities and subsurface damage layers are not completely removed, they will induce secondary defects such as dislocation slip and stacking faults in subsequent high-temperature processes, severely deteriorating the electrical performance of the silicon wafer and directly leading to a decrease in device breakdown voltage and an increase in leakage current. Therefore, etching to remove the damage layer is a crucial step in silicon wafer manufacturing.
[0004] Currently, the industry's conventional damage layer removal process mainly uses a single-component strong acid mixture (usually a mixture of hydrofluoric acid, nitric acid, and acetic acid or water) for one-time etching. However, this traditional process has gradually revealed significant technical bottlenecks when applied to the production of high-requirement, high-quality 8-inch silicon wafers: 1. Low surface cleanliness, prone to localized defects: The one-time strong acid etching reaction is violent, instantly generating a large number of bubbles. Large abrasive particles and agglomerated impurities attached to the silicon wafer surface cannot be gently removed in the early stages of the reaction, and instead easily form a localized "masking effect" on the silicon substrate. Etching is hindered in the masked area, while etching is accelerated in the surrounding area, resulting in severe pitting corrosion and streaking undulations on the etched surface. Localized damage residue and over-etching coexist, seriously affecting batch yield and surface smoothness.
[0005] II. Poor Etching Precision, Damaging Minority Carrier Lifetime: Traditional single-stage processes offer relatively crude control over the etching amount, making it difficult to adapt to the uneven thickness of the damaged layer after grinding. Insufficient etching leaves subsurface microcracks and deep lattice damage, which become recombination centers for minority carriers, directly reducing minority carrier lifetime. Conversely, blindly increasing the etching amount to ensure complete damage removal leads to over-etching. Over-etching disrupts the integrity of the silicon wafer's crystal structure, significantly increasing the density of surface dangling bonds and causing a surge in surface recombination rates, similarly resulting in severe degradation of minority carrier lifetime.
[0006] Third, the narrow process window makes it difficult to meet high-end demands: The single-stage process couples two processes with completely different physicochemical mechanisms, namely "surface impurity cleaning" and "deep damage removal". It is necessary to clean impurities and control the depth of damage at the same time, which makes process control extremely difficult, the window is very narrow, and the batch-to-batch consistency is poor. It is impossible to meet the stringent production requirements of automotive-grade and power-grade silicon wafers for high lifespan, high uniformity, and high reliability. Summary of the Invention
[0007] This invention addresses the shortcomings of existing technologies by providing a multi-component mixed acid step-by-step etching process for precise removal of the damage layer on the back side of silicon wafers. By decoupling the "surface impurity removal" and "bulk damage removal" processes through step-by-step etching, it solves the problems of intense reactions, localized shading etching, and over-etching associated with traditional one-time etching. This effectively reduces the surface dangling bond density and minority carrier lifetime decay, significantly improving the surface cleanliness, batch consistency, and electrical performance stability of silicon wafers. It is suitable for the large-scale production of high-lifetime, high-uniformity automotive-grade and power-grade silicon wafers.
[0008] The above-mentioned technical problems of the present invention are mainly solved by the following technical solutions: A multi-component mixed acid stepwise etching process for precise removal of damage layers on the back side of silicon wafers includes the following steps: Step S1: Rinse the 8-inch silicon wafer with pure water after diamond wire cutting and double-sided grinding to remove loose impurities from the surface.
[0009] Step S2: The back side of the silicon wafer is pre-etched using a low-concentration slow-release mixed acid system. The isotropic etching characteristics under high dilution ratio are used to gently remove surface particles and shallow metal contaminations and eliminate surface mechanical stress concentration points. The single-sided removal depth of the pre-etching is controlled at 0.1 to 0.3 μm.
[0010] Step S3: The back side of the pre-etched silicon wafer is etched using a constant temperature and constant speed main etching system. Under the condition that the reaction rate is stable and controlled, the subsurface microcracks and lattice damage layer caused by cutting and grinding on the back side of the silicon wafer are completely removed. The single-sided removal depth of the main etching is controlled at 1.0 to 1.5 μm, and the etching rate is stable at 0.4 to 0.6 μm / min.
[0011] Step S4: Gradient pure water rinsing and inert gas drying to complete the process.
[0012] Preferably, the low-concentration slow-release mixed acid system in step S2 includes hydrofluoric acid, nitric acid and deionized water, with a volume ratio of HF:HNO3:H2O = 1:(2~3):(7~9); the etching temperature is controlled at 22~26℃ and the etching time is 30~60s.
[0013] Preferably, the main etching system in step S3 is a mixed acid solution containing buffer components, the mixed acid solution including hydrofluoric acid, nitric acid and buffer; the buffer is glacial acetic acid (CH3COOH) or phosphoric acid, and its volume ratio is HF:HNO3:CH3COOH = 1:(3~5):(2~4); the main etching adopts a constant temperature closed-loop spray or immersion method, the temperature is controlled at 25±1℃, and the etching rate is locked at 0.4~0.6μm / min by the acid solution component ratio.
[0014] Preferably, the amount of pre-etching removal in step S2 and the amount of main etching removal in step S3 satisfy a specific gradient relationship. The amount of pre-etching removal accounts for 10% to 20% of the total removal amount, which is used to remove the physical shielding and electrostatic adsorption of surface particles on the substrate, and to provide a uniform initial surface state for subsequent main etching.
[0015] Preferably, the total removal amount is precisely controlled through the step-by-step etching process to ensure that the total removal amount is greater than the maximum damage layer depth on the back side of the silicon wafer, while preserving the complete monocrystalline silicon substrate structure, so that the dangling bond density on the back surface of the processed silicon wafer is less than 1×10⁻⁶. 12 cm -2 The minority carrier lifetime decay rate is less than 5%.
[0016] Preferably, in step S3, the stability of the etching rate is maintained by online detection of the etching solution temperature and acid specific gravity, and by dynamically replenishing nitric acid or hydrofluoric acid, ensuring that the etching rate fluctuation range within a single batch is less than ±0.05 μm / min.
[0017] The present invention can achieve the following effects: This invention provides a multi-component mixed acid step-by-step etching process for precise removal of damaged layers on the back side of silicon wafers. Compared with existing technologies, it has the following significant advantages through innovative step-by-step etching logic and specific chemical system design: I. Step-by-step decoupling to eliminate localized shading and pitting defects. The etching process is creatively broken down into two independent stages: Step S2 pre-etching (surface treatment) and Step S3 main etching (body repair). Step S2 employs a low-concentration, high-dilution-ratio slow-release mixed acid system. The reaction is mild, preferentially stripping and dissolving surface particles, shallow metal contaminants, and organic residues, effectively eliminating the physical shading of the silicon substrate by agglomerated impurities. This not only provides a clean and uniform starting surface for subsequent main etching but also effectively avoids the pitting corrosion and uneven localized etching problems caused by particle shading in traditional processes, significantly improving the surface microstructure quality of the silicon wafer.
[0018] II. Precise control significantly improves minority carrier lifetime and electrical performance. By setting the removal amount in step S2 (pre-etching) to 0.1–0.3 μm and the removal amount in step S3 (main etching) to 1.0–1.5 μm, precise control of the total removal amount is achieved. This gradient removal method ensures thorough removal of subsurface microcracks and lattice damage layers generated by grinding, while strictly avoiding over-etching. In particular, it avoids the surge in surface dangling bond density caused by over-etching, thereby minimizing carrier recombination on the surface. Experimental data shows that using this process, the minority carrier lifetime decay rate of silicon wafers can be controlled within 5%, significantly better than traditional processes, meeting the high requirements for silicon wafer bulk lifetime in automotive-grade power devices.
[0019] III. Dynamic Stability Enhances Consistency in Batch Production. Step S3, the main etching system, incorporates buffer components such as glacial acetic acid, creating a highly stable chemical environment. Combined with isothermal closed-loop control, the etching rate is stably locked at 0.4–0.6 μm / min. This precise control of reaction kinetics eliminates rate instability caused by ambient temperature fluctuations or acid concentration drift, resulting in highly consistent silicon wafer etching amounts within single batches and between different batches. The process window is wide, and the stability is strong, making it highly suitable for large-scale industrial mass production.
[0020] IV. Balancing Surface Cleanliness and Damage Removal Depth to Improve Product Yield. The process, through meticulous cleaning in step S2 and deep damage repair in step S3, ensures the removal depth meets standards while reducing the number of residual surface particles to an extremely low level (e.g., <15 particles / piece). This resolves the contradiction between "impurity removal" and "damage removal" in traditional processes, effectively reducing the scrap rate caused by surface defects and improving the overall yield of the final product. Attached Figure Description
[0021] Figure 1 This is a comparative data table of experimental results of the present invention. Detailed Implementation
[0022] The technical solution of the invention will be further described in detail below through examples.
[0023] Example 1: Precise Removal of Damaged Layer on the Back Side of an 8-inch Silicon Wafer (Standard Process). This method is applied to 8-inch N-type wafers that have undergone diamond wire cutting and double-sided grinding. <100> For monocrystalline silicon wafers, the initial backside damage layer depth is approximately 12–15 μm, and there are numerous abrasive particles with strong adhesion on the surface. The specific process steps are as follows: Step S1 Pretreatment: Place the silicon wafer in a cleaning basket and rinse it with high-purity deionized water (18.2 MΩ·cm) under high pressure. The rinsing pressure is 1.5 MPa and the time is 60s to remove loose grinding debris and some free metal ions from the surface.
[0024] Step S2 Pre-etching (Impurity removal and planarization): Prepare a low-concentration slow-release mixed acid system, consisting of hydrofluoric acid (HF, 49%), nitric acid (HNO3, 69%) and deionized water (H2O).
[0025] The ratio is HF:HNO3:H2O = 1:3:8 (volume ratio).
[0026] Process conditions: The etching solution temperature is controlled at 24℃, and it is applied to the back of the silicon wafer by spraying for 45 seconds.
[0027] Results: This step utilizes the slow-release effect of high water content to gently peel off the aggregated abrasive particles on the surface and eliminate surface micro-protrusions caused by abrasion. The single-sided removal depth is approximately 0.22 μm as measured by a profilometer.
[0028] Step S3 Main Etching (Removal of Damaged Layer): Prepare a constant temperature and constant speed main etching system, consisting of hydrofluoric acid, nitric acid, and glacial acetic acid. .
[0029] The ratio of HF:HNO3:CH3COOH is 1:4:3 (volume ratio). Glacial acetic acid acts as a buffer, effectively suppressing fluctuations in the diffusion rate of nitric acid.
[0030] Process conditions: The temperature of the etching solution was controlled at 25℃±0.5℃ using a constant temperature bath, and dynamic immersion with stirring was adopted. The etching rate was stabilized at 0.5μm / min.
[0031] Control: The etching time is set to 180 seconds based on the remaining depth of the damaged layer after pre-etching.
[0032] Results: The single-sided removal depth is approximately 1.5μm. At this point, the subsurface microcracks and lattice damage layer on the back of the silicon wafer are completely removed, and the surface exhibits a uniform matte finish without pitting.
[0033] Step S4 Post-processing: The process is completed by sequentially passing through overflow rinsing (5 min), rapid drain rinsing (2 min), and hot nitrogen drying.
[0034] Example 2: Low Removal Rate Process (for silicon wafers with shallow damage layers). This process is designed for 8-inch silicon wafers with shallow initial damage layers (approximately 8–10 μm), aiming to minimize silicon loss while maintaining surface quality.
[0035] Step S1 Pretreatment: Place the silicon wafer in a cleaning basket and rinse it with high-purity deionized water (18.2 MΩ·cm) under high pressure. The rinsing pressure is 1.5 MPa and the time is 60s to remove loose grinding debris and some free metal ions from the surface.
[0036] Step S2 Pre-etching: HF:HNO3:H2O = 1:2:9 (volume ratio), temperature 22℃, time 30s. This high dilution ratio further reduces the reaction rate, with a single-sided removal depth of approximately 0.12μm, focusing on fine cleaning.
[0037] Step S3 Main Etching: Mixing Ratio (Volume ratio), temperature 25℃. Etching time set to 200 seconds, etching rate controlled at 0.45μm / min.
[0038] Results: The total removal amount was approximately 1.02 μm (S2+S3). Detection showed that the damaged layer was completely eliminated, and the surface roughness Ra value was better than that of the traditional process.
[0039] Example 3: High Uniformity Process (for automotive-grade high-requirement silicon wafers). The focus is on improving intra-wafer uniformity (UI).
[0040] Step S1 Pretreatment: Place the silicon wafer in a cleaning basket and rinse it with high-purity deionized water (18.2 MΩ·cm) under high pressure. The rinsing pressure is 1.5 MPa and the time is 60s to remove loose grinding debris and some free metal ions from the surface.
[0041] Step S2 Pre-etching: Proportioning (Volume ratio), temperature 26℃, time 60s. Removal depth approximately 0.28μm.
[0042] S3 Main Etching: Ratio (Volume ratio), increase acetic acid content to enhance buffering capacity, temperature 25℃. Use a closed-loop replenishment system to maintain constant acid specific gravity, etching time 180 seconds.
[0043] Results: After etching, the thickness variation at 9 points on the back of the silicon wafer was less than 2μm, and the non-uniformity within the wafer was significantly improved in the minority carrier lifetime test.
[0044] Comparative Example 1: Traditional one-time strong acid etching process. This uses a standard single-stage etching process common in the industry.
[0045] formula: (High acid concentration).
[0046] Process: One-time etching at room temperature, with the total removal amount controlled at 1.5μm (equivalent to the sum of steps S2 and S3 of this invention).
[0047] Phenomenon: Vigorous bubbling occurs in the early stage of the reaction. Due to the failure of large particles on the surface to be removed in advance, a "masking effect" is formed under the particles, resulting in unetched protrusions or etched pits appearing under the particles after removal.
[0048] Comparative Example 2: Single master etching process without step S2.
[0049] Formula: Same as S3 formula in Example 1 of this invention.
[0050] Process: No S2 pre-etching is performed, and the main etching is carried out directly, with a removal amount of 1.5μm.
[0051] Phenomenon: Due to the lack of the surface cleaning step S2, the initial etching process is affected by residual impurities, and the reaction rate fluctuates drastically in the first 10 seconds, resulting in insufficient etching in some areas (residual microcracks) and over-etching in some areas (deterioration of surface roughness).
[0052] The silicon wafers treated in Examples 1-3 and Comparative Examples 1-2 were subjected to performance tests, and the results are as follows: Figure 1 As shown. Comparative analysis verifies the significant advantages of this invention in maintaining minority carrier lifetime and surface cleanliness. Data analysis conclusions: Improved cleanliness: Compared to the comparative example, the example reduced the number of surface particles remaining from hundreds to less than 15 through pre-etching in step S2, demonstrating the significant advantage of step-by-step process in impurity removal.
[0053] Breakthrough in electrical performance: Comparative Example 1 suffers from high dangling bond density and severe minority carrier lifetime decay due to over-etching and pitting; however, Examples 1-3 of this invention maintain a minority carrier lifetime of over 1100μs with extremely low decay rate through precise quantity control, fully meeting the requirements of automotive-grade / power-grade silicon wafers.
[0054] Process stability: Example 3 further verified the adaptability of the process of the present invention under the requirement of high uniformity by optimizing the formulation and control methods of step S3.
[0055] In summary, this multi-component mixed acid stepwise etching process for precise removal of the backside damage layer of silicon wafers involves: pre-rinsing the silicon wafer with pure water; pre-etching using a low-concentration slow-release mixed acid system to gently remove surface particles and shallow contaminants, with a single-sided removal depth controlled at 0.1–0.3 μm; and main etching using a constant-temperature, constant-rate mixed acid system to precisely control the etching rate and duration, completely removing the subsurface mechanical damage layer, with a single-sided removal depth of 1.0–1.5 μm. Finally, the process is completed by gradient rinsing and air drying. By decoupling the "surface impurity removal" and "bulk damage removal" processes through stepwise etching, this process solves the problems of intense reactions, localized occlusion etching, and over-etching inherent in traditional one-time etching. It effectively reduces surface dangling bond density and minority carrier lifetime decay, significantly improving silicon wafer surface cleanliness, batch consistency, and electrical performance stability. This process is suitable for the mass production of high-lifetime, high-uniformity automotive-grade and power-grade silicon wafers.
[0056] The above description is only a specific embodiment of the present invention, but the structural features of the present invention are not limited thereto. Any changes or modifications made by those skilled in the art within the scope of the present invention are covered by the patent scope of the present invention.
Claims
1. A multi-component mixed acid stepwise etching process for precise removal of the damage layer on the back side of a silicon wafer, characterized in that... The following steps are included: Step S1: Rinse the 8-inch silicon wafer with pure water after diamond wire cutting and double-sided grinding to remove loose impurities from the surface; Step S2: The back side of the silicon wafer is pre-etched using a low-concentration slow-release mixed acid system. The isotropic etching characteristics under high dilution ratio are used to gently remove surface particles and shallow metal contaminations and eliminate surface mechanical stress concentration points. The single-sided removal depth of the pre-etching is controlled at 0.1 to 0.3 μm. Step S3: The back side of the pre-etched silicon wafer is etched using a constant temperature and constant speed main etching system. Under the condition that the reaction rate is stable and controlled, the subsurface microcracks and lattice damage layer caused by cutting and grinding on the back side of the silicon wafer are completely removed. The single-sided removal depth of the main etching is controlled at 1.0 to 1.5 μm, and the etching rate is stable at 0.4 to 0.6 μm / min. Step S4: Gradient pure water rinsing and inert gas drying to complete the process.
2. The multi-component mixed acid step-by-step etching process for precise removal of the damaged layer on the back side of a silicon wafer according to claim 1, characterized in that: The low-concentration slow-release mixed acid system described in step S2 includes hydrofluoric acid, nitric acid and deionized water, with a volume ratio of HF:HNO3:H2O = 1:(2~3):(7~9); the etching temperature is controlled at 22~26℃ and the etching time is 30~60s.
3. The multi-component mixed acid step-by-step etching process for precise removal of the damaged layer on the back side of a silicon wafer according to claim 1, characterized in that: The main etching system in step S3 is a mixed acid solution containing buffer components, including hydrofluoric acid, nitric acid and a buffer; the buffer is glacial acetic acid (CH3COOH) or phosphoric acid, and the volume ratio is HF:HNO3:CH3COOH = 1:(3~5):(2~4); the main etching adopts a constant temperature closed-loop spray or immersion method, the temperature is controlled at 25±1℃, and the etching rate is locked at 0.4~0.6μm / min by the acid component ratio.
4. The multi-component mixed acid step-by-step etching process for precise removal of the damaged layer on the back side of a silicon wafer according to claim 1, characterized in that: The amount of pre-etching removal in step S2 and the amount of main etching removal in step S3 satisfy a specific gradient relationship. The amount of pre-etching removal accounts for 10% to 20% of the total removal amount. It is used to remove the physical shielding and electrostatic adsorption of surface particles on the substrate, and to provide a uniform initial surface state for subsequent main etching.
5. The multi-component mixed acid step-by-step etching process for precise removal of the damaged layer on the back side of a silicon wafer according to claim 1, characterized in that: The step-by-step etching process precisely controls the total removal amount, ensuring that the total removal amount is greater than the maximum damage layer depth on the back side of the silicon wafer, while preserving the complete monocrystalline silicon substrate structure. This results in a dangling bond density on the back surface of the processed silicon wafer that is less than 1×10⁻⁶. 12 cm -2 The minority carrier lifetime decay rate is less than 5%.
6. The multi-component mixed acid step-by-step etching process for precise removal of the damaged layer on the back side of a silicon wafer according to claim 1, characterized in that: In step S3, the stability of the etching rate is maintained by online detection of the etching solution temperature and acid specific gravity, and by dynamically replenishing nitric acid or hydrofluoric acid, ensuring that the etching rate fluctuation range within a single batch is less than ±0.05μm / min.