Spherical silver powder and its manufacturing method, as well as conductive paste.

By preparing spherical silver powder with specific structure and particle size, and combining it with a surface treatment agent, the problem of the difficulty in sintering conductive paste at low temperature was solved, and the formation of a conductive film with low resistance and low damage was achieved.

CN123125064APending Publication Date: 2026-11-17DOWA ELECTRONICS MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580028930.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-22
Filing Date
2025-05-23
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing conductive pastes are difficult to sinter at low temperatures with low resistance and low damage, which cannot meet the high-performance requirements of electronic devices.

Method used

Spherical silver powder is used, and in XRD analysis, the ratio of the intensity of the hexagonal Ag peak to the intensity of the cubic Ag peak is greater than 0.5%, the crystallite diameter is less than 28 nm, the BET specific surface area is greater than 0.1 m2/g and less than 1.8 m2/g, the particle size meets a specific relationship, and it is manufactured through silver complex formation and reduction processes, with the addition of surface treatment agents to improve low-temperature sintering properties.

Benefits of technology

It provides spherical silver powder and conductive paste that can achieve excellent sintering properties at low temperatures, reducing the resistivity of the conductive film and minimizing substrate damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125064A_ABST
    Figure CN123125064A_ABST
Patent Text Reader

Abstract

The purpose of this invention is to provide spherical silver powder capable of imparting excellent low-temperature sintering properties to conductive pastes. This invention provides a spherical silver powder that exhibits cubic Ag peaks and hexagonal Ag peaks in XRD analysis, wherein the intensity of the hexagonal Ag peak is at least 0.5% higher than the intensity of the cubic Ag peak.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to spherical silver powder, a method for manufacturing spherical silver powder, and a conductive paste. Background Technology

[0002] The method of forming conductive films such as electrodes and electrical wiring by coating or printing conductive paste containing conductive metal powder onto substrates such as thin films, substrates, and electronic components, and then heating and drying or firing them, has been widely used for a long time. However, with the increasing performance of electronic devices in recent years, there is a growing demand for lower resistance in conductive films formed using conductive pastes, and this demand is becoming more stringent year by year.

[0003] To address the aforementioned requirements, for example, Patent Document 1 proposes a silver powder with an apparent density of 8.2 g / cm³, which has a lower volume resistivity than conventional silver powder used as a conductive paste. 3 Above and 9.2g / cm 3 Silver powder whose ratio of the length of the outer perimeter of the cross-section of the silver particle to the length of the line circumferentially connected to the outer perimeter of the particle cross-section is 1.1 or more and 1.4 or less.

[0004] Existing technical documents

[0005] Patent documents

[0006] Patent Document 1: International Publication No. 2023 / 054405 Summary of the Invention

[0007] The problem the invention aims to solve

[0008] In recent years, in addition to reducing the resistance of conductive films, it has been desirable to sinter conductive pastes at low temperatures (e.g., below 200°C) to reduce damage to substrates and other materials.

[0009] Therefore, the object of the present invention is to provide spherical silver powder that can impart excellent low-temperature sintering properties to conductive pastes.

[0010] In addition, the present invention aims to provide a method for manufacturing spherical silver powder that can impart excellent low-temperature sintering properties to conductive pastes.

[0011] In addition, the present invention aims to provide a conductive paste with excellent low-temperature sintering properties.

[0012] Solution for solving the problem

[0013] In order to solve the above-mentioned problems, the inventors have repeatedly conducted in-depth research, and as a result, completed the present invention as described below.

[0014] That is, the main structure of the present invention for solving the above-mentioned problems is as follows.

[0015] [1] A spherical silver powder, which exhibits cubic Ag peaks and hexagonal Ag peaks in XRD analysis.

[0016] The ratio of the intensity of the hexagonal Ag peak to the intensity of the cubic Ag peak is greater than 0.5%.

[0017] [2] According to the spherical silver powder described in [1], the crystallite diameter is less than 28 nm.

[0018] [3] The spherical silver powder according to [1] or [2] has a BET specific surface area of ​​0.1 m². 2 / g or more and 1.8m 2 / g or less.

[0019] [4] Spherical silver powder according to any one of [1] to [3], wherein the cumulative 10% particle size D based on the volume reference of laser diffraction is... 10 50% cumulative particle size D 50 and cumulative 90% particle size D 90 The following relationship (1) must be satisfied:

[0020] 0.5≤(D 90 -D 10 ) / D 50 ≤2.5…(1).

[0021] [5] Spherical silver powder according to any one of [1] to [4], wherein the cumulative 50% particle size D based on the volume reference of laser diffraction is... 50 It is between 0.5μm and 6μm.

[0022] [6] The spherical silver powder according to any one of [1] to [5], wherein the cumulative 100% particle size D based on the volume reference of laser diffraction is... MAX It is below 15μm.

[0023] [7] A method for manufacturing spherical silver powder as described in any one of [1] to [6], comprising:

[0024] The silver complex formation process involves adding ammonia and a first chelating agent formed from ethylenediaminetetraacetic acid to an aqueous silver-containing solution to obtain an aqueous silver complex solution; and...

[0025] In the reduction process, a reducing agent is added to the aqueous solution of the silver complex to reduce and precipitate the silver particles.

[0026] The amount of the first chelating agent added is more than 3 parts by mass and less than 40 parts by mass relative to 100 parts by mass of silver in the silver-containing aqueous solution.

[0027] [8] In the method for manufacturing spherical silver powder according to [7], a second chelating agent formed of a polymer is further added to the silver-containing aqueous solution or the silver complex solution.

[0028] [9] According to the method for manufacturing spherical silver powder described in [8], the amount of the second chelating agent added is 0.1 parts by mass or more relative to 100 parts by mass of silver in the silver-containing aqueous solution.

[0029]

[10] A method for manufacturing spherical silver powder according to any one of [7] to [9], wherein a surface treatment agent is added to a slurry containing silver particles precipitated after the reduction step.

[0030]

[11] A conductive paste comprising, as described in any one of [1] to [6], spherical silver powder as a conductive filler.

[0031] The effects of the invention

[0032] According to the present invention, spherical silver powder capable of imparting excellent low-temperature sintering properties to conductive pastes can be provided.

[0033] In addition, according to the present invention, a method for manufacturing spherical silver powder capable of imparting excellent low-temperature sintering properties to conductive pastes can be provided.

[0034] Furthermore, according to the present invention, a conductive paste with excellent low-temperature sintering properties can be provided. Attached Figure Description

[0035] Figure 1 This is a magnified graph showing the XRD analysis of the spherical silver powder of Example 1.

[0036] Figure 2 This is a magnified graph showing the XRD analysis of the spherical silver powder of Example 2.

[0037] Figure 3 This is a magnified graph showing the XRD analysis of the spherical silver powder of Example 3.

[0038] Figure 4 This is a magnified graph showing the XRD analysis of the spherical silver powder of Example 4.

[0039] Figure 5 This is a magnified graph showing the XRD analysis of the spherical silver powder of Example 5.

[0040] Figure 6 This is a magnified graph showing the XRD analysis results of the spherical silver powder in Comparative Example 1.

[0041] Figure 7 This is a magnified graph showing the XRD analysis results of the spherical silver powder in Comparative Example 2.

[0042] Figure 8 This is a magnified graph showing the XRD analysis results of the spherical silver powder in Comparative Example 3.

[0043] Figure 9 This is a graph showing the XRD analysis results of the spherical silver powders from Examples 1-5 and Comparative Examples 1-3.

[0044] Figure 10 This is a 50,000x SEM image of the crushed spherical silver powder from the separation process in Example 1.

[0045] Figure 11 This is a 50,000x SEM image of the crushed spherical silver powder from the separation process in Comparative Example 1.

[0046] Figure 12 This is a 50,000x SEM image of the crushed spherical silver powder from the separation process in Comparative Example 2. Detailed Implementation

[0047] The spherical silver powder of the present invention is suitable as a conductive filler for use in conductive pastes. Conductive pastes using the spherical silver powder of the present invention can be used for forming conductive patterns, forming electrodes, or bonding applications on substrates. Conductive pastes using the spherical silver powder of the present invention can be printed onto substrates, for example, by screen printing, offset printing, photolithography, etc., thereby forming conductive patterns, electrodes, and other conductive films. Furthermore, components can be bonded using the paste printed on the substrate.

[0048] (Terminology and Measurement Methods)

[0049] First, before describing the implementation method, the terminology and measurement methods used in this specification will be explained.

[0050] <Confirmation of spherical silver powder (particle shape)>

[0051] In this specification, spherical silver powder refers to silver powder in which the average shape factor of 100 or more particles observed through image analysis based on scanning electron microscopy (SEM) images is in the range of 1.0 or higher and less than 1.7. It should be noted that the shape factor in this specification refers to the ratio of the area of ​​an imaginary circle with an average maximum length as its diameter for 100 or more particles observed through the aforementioned image analysis to the average particle area obtained by depicting the shape of the particles; it is the value obtained by dividing the area of ​​the imaginary circle by the average particle area. The shape factor is calculated using the formula π(average maximum length / 2). 2 / Average particle area is represented.

[0052] <X-ray Diffraction (XRD) Analysis>

[0053] In this manual, X-ray diffraction (XRD) analysis was performed using an X-ray diffraction apparatus (SmartLab manufactured by Rigaku Corporation, Japan). The measurement conditions are as follows.

[0054] Target material: Cu

[0055] Target voltage: 45kV

[0056] Target current: 200mA

[0057] Measurement method: θ-2θ

[0058] Scanning speed: 1deg / min

[0059] Scan step size: 0.02 deg

[0060] Scan range: 30°≤2θ≤50°

[0061] <Cubic Ag Peak>

[0062] In this specification, the "cubic Ag peak" refers to the X-ray diffraction peak originating from the 3C(111) plane, typically a peak with a apex (the point where the X-ray diffraction intensity distribution is maximized) around 2θ = 38.14°. Furthermore, in this specification, the "intensity of the cubic Ag peak" refers to the numerical value (count) of the intensity at the peak apex of the cubic Ag peak. It should be noted that this specification uses the intensity value at 38.14°.

[0063] <Hexagonal Ag Peak>

[0064] In this specification, the "hexagonal Ag peak" refers to an X-ray diffraction peak originating from the 4H(0004) plane, typically apexed near 2θ = 36.00°. Considering the influence of the peak tail of the cubic Ag peak, a point where the difference between the intensity at 35.60° and the intensity at 36.40° is maximized when a straight line is connected to the baseline is also considered a hexagonal Ag peak. Furthermore, in this specification, the "intensity of the hexagonal Ag peak" refers to the difference between the numerical value (count) of the hexagonal Ag peak intensity when a straight line is connected to the intensity at 35.60° and the intensity at 36.40° as the baseline, and the count at the baseline at the 2θ position of the peak apex.

[0065] Here, a magnified plot of the XRD analysis of the spherical silver powder from Example 1 described later is shown. Figure 1 When specifically describing the intensity of the hexagonal Ag peak, Figure 1 The dashed line in the diagram represents the baseline connecting the intensities at 35.60° and 36.40°. The intensity of the hexagonal Ag peak is at 36.00° with a 2θ value of [missing value]. Figure 1The range indicated by the middle arrow. It should be noted that in this specification, the intensity calculation of the hexagonal Ag peak in Examples 1-4 was performed with the 2θ position set to 36.00°. Furthermore, the intensity calculation of the hexagonal Ag peak in Example 5 was performed with the 2θ position set to 35.92°, and the intensity calculation of the hexagonal Ag peak in Comparative Example 3 was performed with the 2θ position set to 36.04°.

[0066] <BET specific surface area>

[0067] The BET specific surface area is calculated as follows: Using a specific surface area measuring device employing the BET method (Macsorb HM-model 1210 manufactured by MOUNTECH), 3g of spherical silver powder is placed in the measuring chamber, and a carrier gas mixture of 70% by volume He and 30% by volume Nitrogen is circulated in the measuring chamber at 25mL / min. The chamber is degassed at 60℃ for 10 minutes, and then the BET 1-point method is used to calculate the specific surface area.

[0068] <Particle Size Distribution>

[0069] In this specification, the cumulative 10% particle size D of the spherical silver powder is defined on a volume basis. 10 50% cumulative particle size D 50 90% cumulative particle size D 90 and cumulative 100% particle size D MAX The particle size distribution was measured using a laser diffraction / scattering particle size distribution measuring device (MicrotracBEL Co., Ltd., Microtrac MT-3300 EXII). During the measurement, 0.1 g of the sample (spherical silver powder) was added to 40 mL of isopropanol (IPA) for dispersion. Dispersion was performed using an ultrasonic homogenizer (Nippon Seiki Co., Ltd., device name: US-150T; 19.5 kHz, front end diameter 18 mm). The dispersion time was set to 2 minutes. The dispersed sample was then fed into the aforementioned device, and the particle size distribution was determined using the accompanying analysis software. It should be noted that the circulator used in the laser diffraction / scattering particle size distribution measuring device was an SDC device, and the "flow rate (%)" setting of this circulator was set to 60. Furthermore, the post-measurement calculation mode of the MT-3300 EXII used the HRA mode. It should be noted that, hereinafter, the cumulative 10% particle size D based on the volumetric standard of laser diffraction will sometimes be used. 10 50% cumulative particle size D 50 90% cumulative particle size D 90 and cumulative 100% particle size D MAX They are abbreviated as "D" 10 “D” 50 “D” 90 "and "D MAX ".

[0070] <Ig-loss>

[0071] In this specification, "Ig-loss" refers to the change in mass when heated from room temperature to 800°C. Specifically, it is an indicator of the amount of the composition other than silver in the spherical silver powder, and an indicator of the amount of residual components in the spherical silver powder, such as processing agents and additives used in the manufacturing process of the spherical silver powder. Moreover, in this specification, "Ig-loss" is calculated by accurately weighing a spherical silver powder sample (weighing value: w1) and placing it in a magnetic crucible, heating it to 800°C, then maintaining it at 800°C for 30 minutes as long as a sufficient time to reach constant weight, then cooling and weighing it again (weighing value: w2), and then calculating it using "Ig-loss (mass%) = (w1-w2) / w1×100".

[0072] <Crystal diameter Dx>

[0073] The crystallite diameter Dx was determined using an X-ray diffraction apparatus (SmartLab manufactured by Rigaku Corporation, Japan), and the half-width of the (111) peak appearing near 2θ = 38.14° was obtained by Scherrer equation (D... hkl =Kλ / βcosθ) is obtained. Here, in the Scherrer equation, D hkl λ refers to the size of the crystallite diameter (the size of the crystallite in the direction perpendicular to hkl) (unit: nm), λ refers to the wavelength of the X-rays measured (0.15405 nm when using a Cu target), β refers to the width of the diffraction line based on the size of the crystallite (rad) (expressed using half-value width), θ refers to the Bragg angle of the diffraction angle (rad) (the angle when the incident angle and the reflection angle are equal, using the angle of the peak), and K refers to the Scherrer constant (K=0.94).

[0074] (Spherical silver powder)

[0075] The spherical silver powder of the present invention has a cubic Ag peak with a 2θ of around 38.14° and a hexagonal Ag peak with a 2θ of around 36.00° in XRD analysis. The ratio of the intensity of the hexagonal Ag peak to the intensity of the cubic Ag peak (intensity of hexagonal Ag peak / intensity of cubic Ag peak × 100) is more than 0.5%.

[0076] As described above, spherical silver powder can impart excellent low-temperature sintering properties to conductive pastes. The reason for this is presumably due to a possible transformation from a hexagonal to a cubic crystal structure during low-temperature sintering, but the reason is not necessarily clear. However, as shown in the results of the following examples and comparative examples, spherical silver powder that meets the above requirements can impart excellent low-temperature sintering properties to conductive pastes.

[0077] It should be noted that the spherical silver powder of the present invention can be obtained by the manufacturing method of the spherical silver powder of the present invention described later.

[0078] The ratio of the intensity of the hexagonal Ag peak to the intensity of the cubic Ag peak is 0.5% or more, preferably 0.8% or more, and more preferably 1% or more.

[0079] It should be noted that the ratio of the intensity of the hexagonal Ag peak to the intensity of the cubic Ag peak can be, for example, less than 30%, less than 15%, or less than 9%.

[0080] The preferred BET specific surface area of ​​spherical silver powder is 0.1 m². 2 / g or more, preferably 0.2m 2 / g or more, and preferably 1.8m 2 / g or less, more preferably 1.5m 2 / g or less.

[0081] If the BET specific surface area of ​​spherical silver powder is 0.1 m² 2 A concentration of / g or higher can improve low-temperature sintering properties.

[0082] On the other hand, if the BET specific surface area of ​​spherical silver powder is 1.8 m² 2 When spherical silver powder is used in conductive pastes or similar products, it can effectively reduce the viscosity of the resulting conductive pastes or similar products when the powder is below a certain size (e.g., g).

[0083] D of spherical silver powder 10 Preferably, the micrometer is 0.2 μm or more, more preferably 0.5 μm or more, and preferably 3 μm or less, more preferably 2 μm or less.

[0084] D of spherical silver powder 50 Preferably, the micrometer is 0.5 μm or more, more preferably 0.8 μm or more, and preferably 6 μm or less, more preferably 3 μm or less.

[0085] D of spherical silver powder 90 Preferably, the micrometer is 1 μm or more, more preferably 2 μm or more, and preferably 8 μm or less, more preferably 5 μm or less.

[0086] D of spherical silver powder MAX Preferably, the micrometer is 2μm or larger, more preferably 3μm or larger, and preferably 15μm or smaller, more preferably 10μm or smaller.

[0087] If the D of spherical silver powder 10 D 50 D 90 D MAXIf the values ​​are above the aforementioned lower limit, then when spherical silver powder is used in conductive pastes, the viscosity of the resulting conductive pastes can be effectively reduced.

[0088] On the other hand, if the D of spherical silver powder 10 D 50 D 90 D MAX If the particle size is below the aforementioned upper limit, the spherical silver powder becomes a good size, which can improve the low-temperature sintering properties.

[0089] In spherical silver powder, the cumulative 10% particle size D based on a volumetric standard using laser diffraction. 10 50% cumulative particle size D 50 and cumulative 90% particle size D 90 Preferably, the following relationship (1) is satisfied:

[0090] 0.5≤(D 90 -D 10 ) / D 50 ≤2.5…(1).

[0091] If (D) 90 -D 10 ) / D 50 Within the aforementioned range, when spherical silver powder is used in conductive pastes, the stability of the resulting conductive paste can be improved.

[0092] Here, the spherical silver powder (D) 90 -D 10 ) / D 50 More preferably, it is 2.0 or less, and even more preferably 1.5 or less. If (D 90 -D 10 ) / D 50 If the particle size is below 2.5, the uniformity of the silver particles is high, and conductive pastes can be easily prepared when using spherical silver powder.

[0093] The loss on ignition (Ig-loss) value of the spherical silver powder is preferably 0.05% by mass or more, more preferably 0.2% by mass or more. Furthermore, it is preferably 10% by mass or less, more preferably 5% by mass or less.

[0094] If the weight loss on ignition of spherical silver powder is 0.05% by mass or higher, then when spherical silver powder is used in conductive pastes, it can effectively inhibit the aggregation of spherical silver powder in conductive pastes.

[0095] On the other hand, if the weight loss on ignition of the spherical silver powder is less than 10% by mass, there are few impurities. Therefore, when a conductive film is obtained by using a conductive paste containing spherical silver powder, the increase in the resistance of the obtained conductive film can be effectively suppressed.

[0096] The crystallite diameter Dx of the spherical silver powder is preferably less than 28 nm, and more preferably less than 20 nm.

[0097] If the crystallite diameter Dx of the spherical silver powder is below 28 nm, it can improve the low-temperature sintering properties.

[0098] It should be noted that the crystallite diameter Dx of the spherical silver powder can be, for example, greater than 1 nm or greater than 10 nm.

[0099] In one embodiment, the spherical silver powder of the present invention preferably contains a surface treatment agent. As a surface treatment agent, there are no particular limitations as long as the spherical silver powder meets the above-mentioned requirements; examples include fatty acids, compounds having an azole structure, fatty acid salts, surfactants, organometallic chelate forming agents, protective colloids, etc.

[0100] From the viewpoint of being able to uniformly adhere to the surface of spherical silver powder and obtain high dispersibility, the surface treatment agent is preferably one or more selected from the group consisting of fatty acids, compounds having an azole structure and fatty acid salts.

[0101] Examples of fatty acids include benzyl acid, stearic acid, palmitic acid, myristic acid, lauric acid, ricinoleic acid, oleic acid, linoleic acid, and linolenic acid. They can be used individually or in combination of two or more.

[0102] As fatty acid salts, examples include salts of the fatty acids listed above. Examples of salts include sodium salts and potassium salts.

[0103] Examples of compounds with an azole structure include benzotriazole, sodium salts of benzotriazole, and potassium salts of benzotriazole. They can be used alone or in combination of two or more.

[0104] (Method for manufacturing spherical silver powder)

[0105] The method for manufacturing spherical silver powder of the present invention (hereinafter, sometimes simply referred to as the "manufacturing method") includes: a silver complex formation step, in which ammonia and a first chelating agent formed by ethylenediaminetetraacetic acid are added to a silver-containing aqueous solution to obtain a silver complex aqueous solution; and a reduction step, in which a reducing agent is added to the silver complex aqueous solution to reduce and precipitate silver particles, wherein the amount of the first chelating agent added is 3 parts by mass or more and 40 parts by mass or less relative to 100 parts by mass of silver (Ag) in the silver-containing aqueous solution.

[0106] If the manufacturing method described above is used, the spherical silver powder of the present invention, which can impart excellent low-temperature sintering properties to conductive pastes, can be obtained.

[0107] It should be noted that the manufacturing method of the present invention may optionally include steps other than the silver complex formation step and the reduction step described above (hereinafter sometimes referred to as "other steps"). Examples of other steps include: a pH adjustment agent addition step, in which a pH adjustment agent is added to an aqueous solution of the silver complex before reduction; a surface treatment agent addition step, in which a surface treatment agent is added to a mixture containing precipitated silver particles; and a separation step, in which the silver particles or surface treatment agent-coated silver particles (silver particles coated with surface treatment agent) are separated and dried from a mixture containing silver particles or surface treatment agent-coated silver particles (silver particles coated with surface treatment agent) obtained in the surface treatment agent addition step.

[0108] <Silver Complex Formation Process>

[0109] In the silver complex formation process, ammonia and a first chelating agent formed from ethylenediaminetetraacetic acid are added to an aqueous solution containing silver to obtain an aqueous solution containing silver complex. The order in which ammonia and the first chelating agent are added to the aqueous solution containing silver can be: ammonia first, the first chelating agent first, or both ammonia and the first chelating agent can be added simultaneously. Both ammonia and the first chelating agent can form complexes with silver, but it is preferable to stir and mix until they are complexed.

[0110] In the silver complex formation process, a second chelating agent formed by the polymer may be further added to the silver-containing aqueous solution or the silver complex aqueous solution. There are no particular restrictions on the timing of the addition of the second chelating agent; it can be added before the addition of ammonia, before the addition of the first chelating agent, after the addition of ammonia, after the addition of the first chelating agent, or simultaneously with ammonia and the first chelating agent.

[0111] There are no particular limitations on the type of silver-containing aqueous solution; silver nitrate aqueous solution, silver oxide aqueous solution, etc., can be used. Among them, silver nitrate aqueous solution is preferred.

[0112] Examples of ammonia added to silver-containing aqueous solutions include ammonia water and ammonium salts.

[0113] The amount of ammonia added is not particularly limited as long as it is sufficient to obtain a silver ammonia complex that constitutes the silver complex aqueous solution. It is preferably 38 parts by mass or more, more preferably 47 parts by mass or more, and more preferably 78 parts by mass or less, more preferably 62 parts by mass or less, relative to 100 parts by mass of silver in the silver-containing aqueous solution.

[0114] The first chelating agent added to the silver-containing aqueous solution is ethylenediaminetetraacetic acid (EDTA). Here, EDTA also includes EDTA in the form of an alkali metal salt. That is, some or all of the four carboxylic acids in EDTA can be alkali metal salts. Moreover, from the viewpoint of solubility in the silver-containing aqueous solution, EDTA in the form of an alkali metal salt is preferred. It should be noted that EDTA in the form of an alkali metal salt can be a hydrate.

[0115] Examples of ethylenediaminetetraacetic acid (EDTA) as alkali metal salts include disodium EDTA, trisodium EDTA, tetrasodium EDTA, dipotassium EDTA, tripotassium EDTA, and tetrapotassium EDTA. Disodium EDTA is preferred. It should be noted that EDTA can be used alone or in combination with two or more of the above-mentioned substances.

[0116] The amount of the first chelating agent added is 3 parts by mass or more, preferably 3.5 parts by mass or more, and also 40 parts by mass or less, preferably 36 parts by mass or less, relative to 100 parts by mass of silver in the silver-containing aqueous solution.

[0117] If the amount of the first chelating agent added is less than 3 parts by mass, the proportion of hexagonal Ag in the resulting silver powder becomes very low, which may prevent the invention from achieving its intended effect. However, if the amount is within the above range, silver powder in which the ratio of the intensity of the hexagonal Ag peak to the intensity of the cubic Ag peak is within the range of this invention can be obtained effectively and easily. Although the reason is not yet certain, it is believed that because the first chelating agent can also form a complex with silver, the anisotropy of silver precipitation is affected by allowing ammonia, which can form a complex with silver, to coexist with the first chelating agent.

[0118] It should be noted that, in this invention, the amount of the first chelating agent added is preferably 5 parts by mass or more, more preferably 6 parts by mass or more, more preferably 70 parts by mass or less, and more preferably 65 parts by mass or less, relative to 100 parts by mass of ammonia in the silver-containing aqueous solution.

[0119] The second chelating agent added to the silver-containing aqueous solution is formed from a polymer. Using a polymer-formed second chelating agent effectively inhibits the aggregation of silver particles obtained during the reduction process.

[0120] Specific examples of preferred second chelating agents include amino compounds and imine compounds. Among them, polyethyleneimine (PEI) is preferred. In particular, PEI, as an imine compound, has a network structure in which both primary amine (-NH2) and secondary amine (=NH) are present in the molecule, which provides preferred results in the present invention.

[0121] The weight-average molecular weight of the second chelating agent is preferably 600 or less, more preferably 145 or more and 600 or less. This is because when the weight-average molecular weight of the second chelating agent is 145 or more, it is possible to obtain silver particles with high dispersibility. On the other hand, it is believed that by making the weight-average molecular weight of the polymeric amine 600 or less, the water solubility of the polymeric amine can be ensured, and the polymeric amine will hardly remain on the surface and inside the generated silver particles.

[0122] It should be noted that the weight-average molecular weight of the second chelating agent can be determined by the GPC-MALS method.

[0123] The amount of the second chelating agent added is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, relative to 100 parts by mass of silver in the silver-containing aqueous solution.

[0124] It is speculated that if the amount of the second chelating agent added is 0.1 parts by mass or more relative to 100 parts by mass of silver in the silver-containing aqueous solution, the silver particles will be uniform and grow into spherical shapes, effectively inhibiting aggregation. There is no particular upper limit to the amount added, but in the case of excessive addition, the growth of silver will be significantly hindered, so for example, it should be 10 parts by mass or less, preferably 3 parts by mass or less.

[0125] The temperature of the aqueous solution of the silver complex is preferably 5°C or higher, more preferably 20°C or higher, and preferably 50°C or lower, more preferably 40°C or lower.

[0126] If the temperature of the aqueous solution of the silver complex is above 5°C, the reduction reaction can be carried out effectively.

[0127] On the other hand, if the temperature of the silver complex aqueous solution is below 50°C, the excessive reaction rate of the reduction reaction described later can be effectively suppressed, and the deviation in the particle size of the silver particles can be effectively suppressed.

[0128] In addition, if the temperature of the silver complex aqueous solution is within the above range, the increase in energy cost can be effectively suppressed.

[0129] <pH Adjuster Addition Process>

[0130] As a pH adjusting step, a pH adjuster can be added to the silver complex aqueous solution before the reducing agent is added. Adding a pH adjuster to the silver complex aqueous solution before reduction allows for easy adjustment of the resulting silver powder particle size. Common acids and bases can be used as pH adjusters, such as nitric acid and sodium hydroxide. It should be noted that the amount of pH adjuster added can be appropriately adjusted based on the amount of silver nitrate aqueous solution used and the desired silver powder particle size. One method for adjustment is to conduct level tests on the silver powder particle size based on the amount of pH adjuster added to adjust the amount.

[0131] <Reduction Process>

[0132] In the reduction process, a reducing agent is added to the stirred aqueous solution of the silver complex, causing the silver particles to be reduced and precipitated. This yields a slurry containing silver particles dispersed in a mixture.

[0133] The reducing agent added to the aqueous solution of the silver complex is not particularly limited, and can include hydrazine, formalin, sodium borohydride, glucose, hypophosphite, etc. Among these, hydrazine is preferred.

[0134] To improve the reaction yield of silver, the amount of reducing agent added is preferably 1 equivalent or more relative to the amount of silver in the reaction. Here, "equivalent" refers to molar equivalents, which express the quantitative relationship between silver and the reducing agent in the chemical reaction. For example, in the case of hydrazine reduction, 1 equivalent of hydrazine is 0.25 moles relative to 1 mole of silver. When using a reducing agent with weak reducing power, such as formalin or glucose, it is preferably 2 equivalents or more relative to silver, more preferably 10 equivalents or more and 20 equivalents or less.

[0135] <Surface treatment agent addition process>

[0136] In the case of a surface treatment agent addition step, a surface treatment agent is added to a mixture containing silver particles precipitated during the reduction step. This results in silver particles coated with the surface treatment agent.

[0137] It should be noted that the mixture containing silver particles coated with a surface treatment agent is usually a slurry in which silver particles coated with a surface treatment agent are dispersed.

[0138] Surface treatment agents added to mixtures containing precipitated silver particles include, for example, fatty acids, compounds with azole structures, fatty acid salts, surfactants, organometallic chelate forming agents, and protective colloids.

[0139] From the viewpoint of easily and uniformly adhering to the surface of silver powder, the surface treatment agent is preferably one or more selected from the group consisting of fatty acids, compounds having an azole structure, and fatty acid salts.

[0140] Examples of fatty acids include benzyl acid, stearic acid, palmitic acid, myristic acid, lauric acid, ricinoleic acid, oleic acid, linoleic acid, and linolenic acid. They can be used individually or in combination of two or more.

[0141] As fatty acid salts, salts of the fatty acids listed above can be included. Examples of salts include sodium salts and potassium salts.

[0142] Examples of compounds with an azole structure include benzotriazole, sodium salts of benzotriazole, and potassium salts of benzotriazole. They can be used alone or in combination of two or more.

[0143] The amount of surface treatment agent added to the mixture containing silver particles is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and preferably 3 parts by mass or less, more preferably 1 part by mass or less, relative to 100 parts by mass of silver in the silver-containing aqueous solution.

[0144] If the amount of surface treatment agent added is more than 0.05 parts by mass relative to 100 parts by mass of silver in the silver-containing aqueous solution, the dispersibility of silver particles can be improved.

[0145] On the other hand, if the amount of surface treatment agent added is less than 3 parts by mass relative to 100 parts by mass of silver in the silver-containing aqueous solution, the risk of reduced low-temperature sinterability can be effectively suppressed.

[0146] For the addition of the surface treatment agent to the mixture containing silver particles, it is preferable to add it after a specific time has elapsed since the reducing agent was added to the aqueous solution of the silver complex. In this invention, the grain growth of the silver particles stops upon the addition of the surface treatment agent; therefore, the timing of addition can be arbitrarily determined to ensure that the silver in the mixture is sufficiently used for the precipitation of silver particles.

[0147] <Separation Process>

[0148] In the separation process, silver particles are separated from a mixture containing silver particles or silver particles coated with a surface treatment agent.

[0149] It should be noted that the washing and recycling process can be carried out after the separation process, or the drying process can be carried out without the washing and recycling process.

[0150] In the cleaning and recovery process, for example, the separated silver particles or the cake-like aggregates of silver particles coated with a surface treatment agent are cleaned. Cleaning in the cleaning and recovery process can be performed, for example, using pure water. Dehydration in the cleaning and recovery process can be performed, for example, by decanting or using a filter press. The endpoint of cleaning can be determined using the conductivity of the cleaning water. Specifically, cleaning can be considered complete when the conductivity of the cleaning water falls below a specified value. The cleaned silver particles or the silver particles coated with the surface treatment agent can be fed into the drying process in an aggregated state such as a cake.

[0151] In the drying process, silver particles containing moisture and in an aggregated state, or aggregates of silver particles coated with a surface treatment agent, are dried. The drying process can utilize vacuum drying or airflow drying equipment. During the drying process, high-pressure airflow can be blown onto the silver particles or aggregates of silver particles coated with a surface treatment agent, or the filter cake or spherical silver powder from the drying process can be fed into a mixer with a stirring rotor for stirring, thereby imparting a dispersing force to the filter cake or spherical silver powder from the drying process, promoting dispersion and drying.

[0152] In the drying process, the temperature of the spherical silver powder is not particularly limited as long as the aggregate of silver particles is fully dried. It is preferably 40°C or higher, more preferably 70°C or higher, preferably 120°C or lower, and more preferably 100°C or lower.

[0153] If the temperature of the spherical silver powder is above 40°C, the drying efficiency can be improved.

[0154] On the other hand, if the temperature of the spherical silver powder is below 120°C, the transformation from hexagonal to cubic crystal structure in silver particles or silver particles coated with a surface treatment agent can be effectively suppressed.

[0155] Since dried spherical silver powder sometimes becomes lumpy, it is preferable to perform dry crushing or grading operations during or after the drying process to improve the workability of the spherical silver powder. Here, improving the workability of the spherical silver powder means, for example, appropriately loosening the spherical silver powder to ensure sufficient flowability for supplying it into the equipment, or to enable efficient processing within the equipment.

[0156] There are no particular restrictions on the dry crushing process; it can be selected appropriately according to the purpose. It is preferable to use a crusher that uses rotating stirring blades to crush and flow the spherical silver powder, such as a sample mill, blender, or coffee mill.

[0157] (Conductive paste)

[0158] The conductive paste of the present invention comprises the spherical silver powder of the present invention as a conductive filler. Preferably, the conductive paste contains, in addition to the spherical silver powder, a solvent and a binder, and further may contain other components as needed. The solvent and binder, etc., can be appropriately selected according to the method of use.

[0159] Example

[0160] The present invention will be further described in detail below using examples, but the present invention is by no means limited to the following examples.

[0161] It should be noted that the XRD analysis, the intensity of the cubic Ag peak, the intensity of the hexagonal Ag peak, the BET specific surface area, the particle size distribution, the weight loss on ignition (Ig-loss), and the crystallite diameter Dx are determined or calculated using the methods described above.

[0162] (Example 1)

[0163] <Silver Complex Formation Process>

[0164] First, while stirring 3436g of a silver nitrate aqueous solution containing 50.84g of silver at 174rpm, 103.2g of 28% (w / w) ammonia solution (manufactured by Junsei Kagaku Co., Ltd.) was added. Then, while continuing stirring, 4.17g of 43% (w / w) EDTA aqueous solution (manufactured by CHELEST, CHELEST OD-50) as the first chelating agent was added 30 seconds after the addition of ammonia solution (EDTA addition amount relative to 100 parts by weight of silver: 3.53 parts by weight), to obtain a silver complex aqueous solution. Next, 60 seconds after the addition of ammonia solution, 10.17g of 5% (w / w) PEI aqueous solution (manufactured by Nippon Shokubai Co., Ltd., weight average molecular weight 600) as the second chelating agent was added (PEI addition amount relative to 100 parts by weight of silver: 1.00 parts by weight), and the liquid temperature was adjusted to 35°C.

[0165] <Reduction Process>

[0166] For the obtained silver complex aqueous solution, 302.8 g of a 2.43% by mass hydrazine (manufactured by Mitsubishi Gas Chemical Co., Ltd.) aqueous solution (hydrazine addition amount relative to 100 parts by mass of silver: 14.47 parts by mass) was added all at once after 180 seconds following the addition of ammonia to obtain a slurry containing silver particles.

[0167] <Surface treatment agent addition process>

[0168] Next, for the resulting slurry containing silver particles, stirring was temporarily stopped after 5 seconds of stirring following the addition of hydrazine, and then resumed after 130 seconds. Simultaneously, 5.12 g of a 1.55% stearic acid emulsion (stearic acid to silver content of 0.16 parts by mass per 100 parts by mass) was added as a surface treatment agent, and stirring was continued for 75 seconds to obtain a slurry containing silver particles coated with the surface treatment agent. It should be noted that the reaction utilized a baffled reaction layer and a second-stage turbine blade.

[0169] <Separation Process>

[0170] Then, stirring was stopped, and the silver particles coated with the surface treatment agent were allowed to settle. The liquid after the silver particles coated with the surface treatment agent were filtered and washed with water until the conductivity of the liquid after water flow was below 0.5 mS / m. The liquid was then vacuum dried at 73°C. The resulting dried silver powder was then fed into a sample mill (SK-M10 manufactured by Kyoritsu Riko Co., Ltd.) with 50 g of silver added. The mill was crushed twice for 30 seconds at a scale of 100 to obtain the spherical silver powder of Example 1.

[0171] Using the obtained spherical silver powder, the intensity of the cubic Ag peak, the intensity of the hexagonal Ag peak, the ratio of the intensity of the hexagonal Ag peak to the intensity of the cubic Ag peak, the BET specific surface area, particle size distribution, weight loss on ignition (Ig-loss), and crystallite diameter Dx were determined or calculated. The results are shown in Table 2.

[0172] In addition, the magnified XRD analysis curves of the spherical silver powder of Example 1 in the range of 2θ from 35.00° to 37.00° are illustrated in the figure. Figure 1 The XRD analysis curves for the range of 2θ from 35.00 to 40.00° are plotted in the figure. Figure 9 A 50,000x SEM image of the crushed spherical silver powder from the separation process is shown. Figure 10 It should be noted that the intensity of the cubic Ag peak, the intensity of the hexagonal Ag peak, and the ratio of the intensity of the hexagonal Ag peak to the intensity of the cubic Ag peak of the spherical silver powder after vacuum drying (before crushing) in the separation process are shown in Table 2 as reference examples.

[0173] <Resistance Measurement>

[0174] The above-obtained spherical silver powder (93.01 parts by weight), ethyl cellulose (0.25 parts by weight), TEXANOL (1.59 parts by weight), butyl carbitol acetate (3.86 parts by weight), tributyl citrate (0.26 parts by weight), oleic acid (0.25 parts by weight), triacetin (0.26 parts by weight), and methylphenyl polysiloxane (KF96-100) (0.51 parts by weight) were mixed to obtain a mixture. Next, the mixture was premixed in a rotary mixer (1000 rpm) and then kneaded using a three-roll mill (EXAKT) with the roller gap decreasing from 100 μm to 20 μm to obtain a conductive paste.

[0175] Using the conductive paste obtained above, linear shapes were printed by screen printing. The linear shapes were designed with a line width of 500 μm and a length of 128 mm. Printing was performed using a Microtec printer at a squeegee speed of 80 mm / s. A silicon substrate with a thickness of approximately 170 μm (for solar cells, to complete texture formation, SiN) was used for printing. x (film formation).

[0176] After printing, the material is dried in a dryer set to 100°C for 10 minutes to form a conductive film. The resistivity (in Ω) of the formed conductive film is measured using a high-temperature microscope (manufactured by Yonekura Manufacturing Co., Ltd.) at a heating rate of 10°C / min, from room temperature to 300°C. The resistivity values ​​at 100°C, 140°C, 160°C, 180°C, 190°C, 195°C, and 200°C are shown in Table 3. Lower resistivity values ​​as shown in Table 3 indicate better low-temperature sintering properties of the conductive paste.

[0177] (Examples 2-4)

[0178] Except that the amounts of the first chelating agent and the second chelating agent added are as shown in Table 1, the spherical silver powders of Examples 2 to 4 were obtained in the same manner as in Example 1.

[0179] Using the obtained spherical silver powder, XRD analysis, BET specific surface area, particle size distribution, loss on ignition (Ig-loss), and crystallite diameter Dx were determined or calculated. The results are shown in Table 2.

[0180] In addition, the resistance value was measured using the obtained spherical silver powder. The results are shown in Table 3.

[0181] Furthermore, the magnified XRD analysis curves of the spherical silver powders from Examples 2-4 in the range of 2θ (35.00° to 37.00°) are illustrated in the figure below. Figures 2-4 The XRD analysis curves for the range of 2θ from 35.00° to 40.00° are plotted in the figure. Figure 9 .

[0182] (Example 5)

[0183] The resulting dried silver powder was fed with 50g of silver using a coffee mill (Made by Melitta Japan Ltd.) and crushed twice for 30 seconds. Otherwise, the spherical silver powder of Example 5 was obtained in the same manner as in Example 1.

[0184] Using the obtained spherical silver powder, XRD analysis, BET specific surface area, particle size distribution, loss on ignition (Ig-loss), and crystallite diameter Dx were determined or calculated. The results are shown in Table 2.

[0185] In addition, the resistance value was measured using the obtained spherical silver powder. The results are shown in Table 3.

[0186] Furthermore, the magnified XRD analysis curves of the spherical silver powder of Example 5 in the range of 2θ (35.00°~37.00°) are illustrated in the figure below. Figure 5 The XRD analysis curves for the range of 2θ from 35.00° to 40.00° are plotted in the figure. Figure 9 .

[0187] (Comparative Example 1)

[0188] <Silver Complex Formation Process>

[0189] First, while stirring 3489g of an aqueous solution of silver nitrate containing 53.71g of silver at 332rpm, 113.2g of ammonia water (manufactured by Junsei Chemical Co., Ltd.) with a concentration of 28% by mass was added to obtain an aqueous solution of silver complex.

[0190] Next, while continuing to stir, 4.98 g of 20% by mass sodium hydroxide aqueous solution was added to the resulting silver complex aqueous solution as a pH adjuster to adjust the liquid temperature to 28°C.

[0191] <Reduction Process>

[0192] For the pH-adjusted solution, 251.3 g of a 26% (w / w) formaldehyde aqueous solution (formalin) was added all at once 180 seconds after the addition of ammonia (the amount of formaldehyde added relative to 100 parts by weight of silver was 121.11 parts by weight) to obtain a slurry containing silver particles.

[0193] <Surface treatment agent addition process>

[0194] Next, for the obtained slurry containing silver particles, 6.13 g of a 1.55% stearic acid emulsion (stearic acid to silver content of 0.18 parts by mass per 100 parts by mass) was added as a surface treatment agent 15 seconds after the addition of the reducing agent, and the mixture was stirred for another 180 seconds to obtain a slurry containing silver particles coated with the surface treatment agent. It should be noted that the reaction used a baffled reaction layer and a second-stage turbine blade.

[0195] <Separation Process>

[0196] Then, stirring was stopped, and the silver particles coated with the surface treatment agent were allowed to settle. The liquid after the silver particles coated with the surface treatment agent were filtered and washed with water until the conductivity of the liquid after water flow was below 0.5 mS / m. The liquid was then vacuum dried at 73°C. The resulting dried silver powder was then fed into a sample mill (SK-M10 manufactured by Kyoritsu Riko Co., Ltd.) with 50 g of silver added. The mill was crushed twice for 30 seconds at a scale of 100 on the dial to obtain the spherical silver powder of Comparative Example 1.

[0197] Using the obtained spherical silver powder, XRD analysis, BET specific surface area, particle size distribution, loss on ignition (Ig-loss), and crystallite diameter Dx were determined or calculated. The results are shown in Table 2.

[0198] In addition, the resistance value was measured using the obtained spherical silver powder. The results are shown in Table 3.

[0199] Furthermore, the magnified XRD analysis curves of the spherical silver powder of Comparative Example 1 in the range of 2θ from 35.00° to 37.00° are illustrated in the figure below. Figure 6 The XRD analysis curves for the range of 2θ from 35.00° to 40.00° are plotted in the figure. Figure 9 A 50,000x SEM image of the crushed spherical silver powder from the separation process is shown. Figure 11 .

[0200] (Comparative Example 2)

[0201] <Silver Complex Formation Process>

[0202] First, while stirring 3448g of an aqueous solution of silver nitrate containing 50.84g of silver at 174rpm, 103.2g of ammonia water (manufactured by Junsei Chemical Co., Ltd.) with a concentration of 28% by mass was added to obtain an aqueous solution of silver complex.

[0203] Next, while continuing to stir, 1.02 g of sodium carbonate aqueous solution with a concentration of 5% by mass was added to the resulting silver complex aqueous solution as a pH adjuster. 60 seconds after adding ammonia, 0.508 g of PEI aqueous solution with a concentration of 5% by mass (manufactured by Nippon Shokubai Co., Ltd., weight average molecular weight 600) was added (the amount of PEI added relative to 100 parts by mass of silver: 0.05 parts by mass). The liquid temperature was then adjusted to 35°C.

[0204] <Reduction Process>

[0205] For the obtained silver complex aqueous solution, 302.8 g of a 2.43% by mass hydrazine (manufactured by Mitsubishi Gas Chemical Co., Ltd.) aqueous solution (hydrazine addition amount relative to 100 parts by mass of silver: 14.47 parts by mass) was added all at once after 180 seconds following the addition of ammonia to obtain a slurry containing silver particles.

[0206] <Surface treatment agent addition process>

[0207] Next, for the obtained slurry containing silver particles, 5.12 g of a 1.55% stearic acid emulsion (stearic acid to silver concentration: 0.16 parts by mass per 100 parts by mass) was added as a surface treatment agent 15 seconds after the addition of the reducing agent, and the mixture was stirred for another 180 seconds to obtain a slurry containing silver particles coated with the surface treatment agent. It should be noted that the reaction used a baffled reaction layer and a second-stage turbine blade.

[0208] <Separation Process>

[0209] Then, stirring was stopped, and the silver particles coated with the surface treatment agent were allowed to settle. The liquid after the silver particles coated with the surface treatment agent were filtered and washed with water until the conductivity of the liquid after water flow was below 0.5 mS / m. Vacuum drying was then carried out at 73°C. The resulting dried silver powder was then fed into a sample mill (SK-M10 manufactured by Kyoritsu Riko Co., Ltd.) with 50 g of silver added. The mill was crushed twice for 30 seconds at a scale of 100 on the dial to obtain spherical silver powder of Comparative Example 2.

[0210] Using the obtained spherical silver powder, XRD analysis, BET specific surface area, particle size distribution, loss on ignition (Ig-loss), and crystallite diameter Dx were determined or calculated. The results are shown in Table 2.

[0211] In addition, the resistance value was measured using the obtained spherical silver powder. The results are shown in Table 3.

[0212] Furthermore, the magnified XRD analysis curves of the spherical silver powder of Comparative Example 2 in the range of 2θ (35.00° to 37.00°) are illustrated in the figure below. Figure 7 The XRD analysis curves for the range of 2θ from 35.00° to 40.00° are plotted in the figure. Figure 9 A 50,000x SEM image of the crushed spherical silver powder from the separation process is shown. Figure 12 .

[0213] (Comparative Example 3)

[0214] Except that the amounts of the first chelating agent and the second chelating agent added are as shown in Table 1, the spherical silver powder of Comparative Example 3 was obtained in the same manner as in Example 1.

[0215] Using the obtained spherical silver powder, XRD analysis, BET specific surface area, particle size distribution, loss on ignition (Ig-loss), and crystallite diameter Dx were determined or calculated. The results are shown in Table 2.

[0216] In addition, the resistance value was measured using the obtained spherical silver powder. The results are shown in Table 3.

[0217] Furthermore, the magnified XRD analysis curves of the spherical silver powder of Comparative Example 3 in the range of 2θ (35.00° to 37.00°) are illustrated in the figure below. Figure 8 The XRD analysis curves for the range of 2θ from 35.00° to 40.00° are plotted in the figure. Figure 9 .

[0218] [Table 1]

[0219]

[0220] [Table 2]

[0221]

[0222] [Table 3]

[0223]

[0224] The results in Table 3 clearly show that the spherical silver powder used in Examples 1-5 imparts excellent low-temperature sintering properties to the conductive paste. As can be seen from Comparative Examples 1-3, the conductive paste using spherical silver powder with a ratio of hexagonal Ag peak intensity to cubic Ag peak intensity of less than 0.5% exhibits poor low-temperature sintering properties.

[0225] Furthermore, the results in Table 3 clearly show that spherical silver powder obtained by the manufacturing methods of Examples 1-5 can impart excellent low-temperature sintering properties to the conductive paste. As shown in Comparative Examples 1-3, it can be seen that the conductive paste obtained by using spherical silver powder without adding the specified amount of the first chelating agent has poor low-temperature sintering properties.

[0226] Industrial availability

[0227] According to the present invention, spherical silver powder capable of imparting excellent low-temperature sintering properties to conductive pastes can be provided.

[0228] In addition, according to the present invention, a method for manufacturing spherical silver powder capable of imparting excellent low-temperature sintering properties to conductive pastes can be provided.

[0229] Furthermore, according to the present invention, a conductive paste with excellent low-temperature sintering properties can be provided.

Claims

1. A spherical silver powder, which exhibits cubic Ag peaks and hexagonal Ag peaks in XRD analysis. The ratio of the intensity of the hexagonal Ag peak to the intensity of the cubic Ag peak is greater than 0.5%.

2. The spherical silver powder according to claim 1, wherein, The crystallite diameter is less than 28 nm.

3. The spherical silver powder according to claim 1, having a BET specific surface area of ​​0.1 m². 2 / g or more and 1.8m 2 / g or less.

4. The spherical silver powder according to claim 1, wherein, Cumulative 10% particle size D based on volumetric standard using laser diffraction 10 50% cumulative particle size D 50 and cumulative 90% particle size D 90 The following relationship (1) must be satisfied: 0.5≤(D 90 -D 10 ) / D 50 ≤2.5…(1)。 5. The spherical silver powder according to claim 1, wherein, Cumulative 50% particle size D based on volumetric reference using laser diffraction 50 It is between 0.5μm and 6μm.

6. The spherical silver powder according to claim 1, wherein, Cumulative 100% particle size D based on volume standard using laser diffraction MAX It is below 15μm.

7. A method for manufacturing the spherical silver powder according to claim 1, comprising: The silver complex formation process involves adding ammonia and a first chelating agent formed from ethylenediaminetetraacetic acid to a silver-containing aqueous solution to obtain a silver complex aqueous solution. as well as In the reduction process, a reducing agent is added to the aqueous solution of the silver complex to reduce and precipitate the silver particles. The amount of the first chelating agent added is more than 3 parts by mass and less than 40 parts by mass relative to 100 parts by mass of silver in the silver-containing aqueous solution.

8. The method for manufacturing spherical silver powder according to claim 7, wherein, A second chelating agent formed from a polymer is also added to the silver-containing aqueous solution or the silver complex aqueous solution.

9. The method for manufacturing spherical silver powder according to claim 8, wherein, The amount of the second chelating agent added is 0.1 parts by mass or more relative to 100 parts by mass of silver in the silver-containing aqueous solution.

10. The method for manufacturing spherical silver powder according to any one of claims 7 to 9, wherein, A surface treatment agent is added to the slurry containing the silver particles precipitated after the reduction process.

11. A conductive paste comprising spherical silver powder as any one of claims 1 to 6 as a conductive filler.

Citation Information

Patent Citations

  • Silver powder, electroconductive paste, method for producing silver powder, and mixed silver powder

    WO2023054405A1