Layered modeling system
By controlling the AC frequency and EN ratio in consumable electrode arc welding, the instability problem of stacked weld beads was solved, and stable stacking and shape control of weld beads were achieved.
Patent Information
- Application Number
- CN202580028389.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-18
- Filing Date
- 2025-04-11
- Publication Date
- 2026-11-17
AI Technical Summary
In the process of stacked fusion deposition welding, the existing technology fails to take into account both deposition amount and heat input at the same time, resulting in unstable weld shape, especially when using consumable electrodes, where there is a problem of excessive or insufficient heat input.
The consumable electrode arc welding method with short-circuit transition is adopted. By controlling the AC frequency and EN ratio, the welding current is supplied to the consumable electrode welding wire, and the heat input is adjusted to ensure the stable stacking of the weld bead.
By changing the EN ratio under the same welding current, the heat input can be finely adjusted to ensure stable stacking of weld beads and improve the stability of the stacking direction.
Smart Images

Figure CN123125070A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to a layered modeling system. Background Technology
[0002] Japanese Patent Application Publication No. 2022-106172 (Patent Document 1) discloses a method for shaping an object by stacking weld beads, and for changing welding conditions when the height of the weld beads deviates from the planned height. In Japanese Patent Application Publication No. 2022-106172 (Patent Document 1), a consumable electrode is used when stacking weld beads, and the welding speed is changed according to the stacking height.
[0003] Existing technical documents
[0004] Patent documents
[0005] Patent Document 1: Japanese Patent Application Publication No. 2022-106172 Summary of the Invention
[0006] The problem that the invention aims to solve
[0007] In the case of stacked weld beads, if not only the amount of weld deposited but also the heat input (i.e., the heat imparted from the outside to the molten portion) is not considered simultaneously, the shape of the stacked weld beads may be unstable. Japanese Patent Application Publication No. 2022-106172 (Patent Document 1) states that when using consumable electrodes, if the amount of weld deposited is changed to alter the height of the weld bead, the magnitude of the welding current affecting the heat input also changes simultaneously. Therefore, there is a possibility of excessive or insufficient heat input to the weld bead, and it cannot be said to be sufficient for stacking weld beads with a stable shape.
[0008] The purpose of this disclosure is to provide a technique for stably depositing weld beads in consumable electrode arc welding with short-circuit transition.
[0009] Methods for solving problems
[0010] This disclosure relates to a stacked molding system that uses a consumable electrode arc welding method with short-circuit transition to supply welding current to a consumable electrode wire and stack weld beads to shape an object. The stacked molding system includes: a welding torch that performs the stacking of weld beads using the consumable electrode wire; a drive device that moves the welding torch; a welding power source that supplies alternating current (AC) to the consumable electrode wire as welding current; and a control device that controls the frequency and EN ratio of the AC. The control device sets the AC frequency to a value of 2 Hz or higher and 30 Hz or lower.
[0011] Invention Effects
[0012] The amount of weld deposited can be easily varied by changing the heat input through the change of the EN ratio, even under the same welding current. The stacking system of this disclosure sets the AC frequency to a value between 2 Hz and 30 Hz. Therefore, the stacking system of this disclosure can ensure the stability of the stacking direction and finely adjust the EN ratio, thus enabling stable stacking of weld beads when using consumable electrode wire. Attached Figure Description
[0013] Figure 1 This is a diagram that schematically illustrates the layered modeling system of Implementation Method 1.
[0014] Figure 2 This is a graph used to illustrate the EN ratio.
[0015] Figure 3 It is a graph used to illustrate the difference in the EN ratio during one cycle of the AC circuit.
[0016] Figure 4 This diagram is used to illustrate the layering state of weld beads at lower frequencies.
[0017] Figure 5 This is a diagram illustrating an example of the welding conditions for Embodiment 1.
[0018] Figure 6 It is a diagram showing the cross-sectional shape of stacked weld beads.
[0019] Figure 7 This is a diagram used to illustrate the appropriate range of frequencies in Embodiment 1.
[0020] Figure 8 This is a flowchart illustrating the control content of Implementation Method 1.
[0021] Figure 9 This is a diagram that schematically illustrates the layered modeling system of Embodiment 2. Detailed Implementation
[0022] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. It should be noted that the same or equivalent parts in the drawings are labeled with the same reference numerals, and their descriptions will not be repeated.
[0023] [Implementation Method 1]
[0024] Figure 1 This is a schematic diagram illustrating the stacked modeling system 1 of Embodiment 1. The stacked modeling system 1 includes a robotic arm 40, a welding torch 20, a welding power source 10, a welding wire feed device 50, and a control device 30.
[0025] The robotic arm 40 is a multi-jointed arm, such as a six-axis multi-joint arm. The robotic arm 40 functions as a drive device to move the welding torch 20 at a set welding speed. By moving the welding torch 20 with the robotic arm 40, weld beads 70 containing molten consumable electrode wire 51 are stacked. The robotic arm 40 operates in a manner that shapes the object by stacking the weld beads 70. It should be noted that the layer preceding the currently stacked layer of weld beads 70 is called the preceding layer.
[0026] In the welding torch 20, a welding current is supplied to the consumable electrode wire 51 through a power supply nozzle (not shown) located inside the nozzle 21. The consumable electrode wire 51 melts due to the electric arc 22 generated between it and the base material 80 or the already stacked weld beads 70, as well as the resistance heating caused by the current supply. The melting of the consumable electrode wire 51 forms the weld beads 70. The welding torch 20 performs the stacking of weld beads 70 using the consumable electrode wire 51. A shielding gas is supplied to the welding torch 20 through a shielding gas supply section (not shown), which exits from the nozzle 21 and reaches the electric arc 22 and the melting section. The shielding gas may be, for example, argon, CO2, or a mixture thereof.
[0027] The welding torch cable 11 connected to the welding torch 20 contains a cable for current supplied from the welding power source 10, a consumable electrode welding wire 51 fed from the welding wire feed device 50, and a shielding gas supply unit (not shown) for shielding gas.
[0028] The welding power source 10 supplies alternating current (AC) as the welding current to the consumable electrode welding wire 51. The magnitude of the welding current output from the welding power source 10 and the EN ratio are set by the control device 30. Here, the EN ratio refers to the proportion of the time of the welding wire's negative polarity period in one AC cycle to the total time. Alternatively, the EN ratio can also be set as the ratio of the value obtained by integrating the negative polarity current in one AC cycle to the value obtained by integrating the current in one AC cycle (the sum of the values obtained by integrating the positive polarity current and the negative polarity current).
[0029] Figure 2 This is a graph used to illustrate the EN ratio. In Figure 2The waveform of short-circuit welding accompanied by short-circuit transition is shown in the figure. The welding power source 10 switches the polarity of the electrode positive polarity (also known as EP polarity) and electrode negative polarity (also known as EN polarity) supplied to the consumable electrode wire 51 in the welding torch 20. Electrode positive polarity (EP polarity) refers to the polarity state in which the consumable electrode wire 51 side in the current path supplied from the welding power source 10 is the anode and the base material 80 or weld bead 70 side is the cathode. Electrode negative polarity (EN polarity) refers to the polarity state in which the base material 80 or weld bead 70 side in the current path supplied from the welding power source 10 is the anode and the consumable electrode wire 51 side is the cathode.
[0030] The cycle of alternating current is defined as the time when the electrode switches from negative to positive polarity, and the time from switching back to positive polarity. Within one cycle, the ratio of electrodes that become positive is called the EP ratio, and the ratio that becomes negative is called the EN ratio. For example... Figure 2 As shown, the welding power source 10 can output welding current with alternating positive and negative electrode polarities in one cycle.
[0031] It is known that during the period of negative electrode polarity, the melting rate of the welding wire 51 consumed by the electrode increases. This is because, during the period of negative electrode polarity, the amount of heat input from the arc 22 to the welding wire 51 consumed by the electrode increases compared to the period of positive electrode polarity. Conversely, during the period of positive electrode polarity, the amount of heat input from the arc 22 to the base material 80 or the weld bead 70 increases compared to the period of negative electrode polarity, thus increasing the amount of heat input to the molten portion. Therefore, the heat input to the molten portion can be adjusted by changing the EN ratio.
[0032] Here, the shape formed by stacking weld beads 70 is in the following relationship: the lower the layer, the closer it is to the base material 80, so heat dissipates easily; the higher the layer, the further it is from the base material 80, so heat dissipates more difficultly. Under such circumstances, if the stacking is performed with the same welding current, the temperature of the upper weld bead 70 becomes too high, and the weld bead 70 may burn through. The stacking shaping system 1 of Embodiment 1 adjusts the amount of heat input to the molten part by setting an appropriate EN ratio.
[0033] return Figure 1 The wire feed device 50 includes a roller (not shown) and a motor. The wire feed device 50 feeds the consumable electrode wire 51 onto the welding torch 20 by driving the motor and rotating the roller. The operation of the wire feed device 50 is controlled by the welding power source 10 based on commands from the control device 30. The operation of the wire feed device 50 can also be directly controlled by the welding power source 10.
[0034] The control device 30 includes a computing unit 31, a memory 32, a storage device 33, and an input / output interface 34. These components are connected via a bus.
[0035] The arithmetic unit 31 is a computing entity (computer) that performs the prescribed processing. The arithmetic unit 31 may be composed of processors such as CPU (Central Processing Unit), MPU (Micro-Processing Unit), TPU (Tensor Processing Unit), or GPU (Graphics Processing Unit). The arithmetic unit 31 may also be read as a processing circuitry that performs the prescribed processing.
[0036] The memory 32 includes a storage area (e.g., a working area) for storing program code or working memory when the computing device 31 executes various programs.
[0037] The storage device 33 functions as a storage unit for storing various programs or data executed by the arithmetic unit 31. For example, the storage device 33 stores the control program 330 executed by the arithmetic unit 31.
[0038] The input / output interface 34 accepts various types of data input. Following the instructions of the arithmetic unit 31, the input / output interface 34 outputs data obtained through various processing steps.
[0039] Here, the control device 30 controls, for example, the movement of the robotic arm 40. The control device 30 calculates the AC EN ratio, frequency, etc., and displays them on a display device (not shown). The calculation and display of the AC EN ratio, frequency, etc., can also be performed by the welding power source 10. Thus, a condition setting device for setting the AC conditions can be assembled in either the control device 30 or the welding power source 10.
[0040] Next, the differences in the EN ratio during one cycle of AC at different frequencies will be explained. Figure 3 It is a graph used to illustrate the difference in the EN ratio during one cycle of the AC circuit. Figure 3 (A) is a graph used to illustrate the EN ratio in one cycle of an AC when the frequency of the AC is low. Figure 3 (B) is a graph used to illustrate the EN ratio in one cycle of an AC when the frequency of the AC is high. Figure 3 (C) is used to explain the change. Figure 3 A graph showing the state of the EN ratio during a cycle of (B) exchange.
[0041] Low-frequency communication is an example of a frequency lower than 2Hz. High-frequency communication is an example of a frequency higher than 30Hz. In cases of low-frequency communication, such as... Figure 3 As shown in (A), the duration of one cycle of the alternation becomes longer. Conversely, at higher alternation frequencies, such as Figure 3 As shown in (B) and (C), the duration of one cycle of the exchange becomes shorter.
[0042] Here, arc welding accompanied by short-circuit transition refers to welding during the arc period when arc discharges repeatedly occur between the electrodes, and the short-circuit period when the electrodes are in contact, resulting in an electrical short circuit. One cycle of this short-circuit period and arc period is called the short-circuit-arc cycle. The short-circuit-arc cycle is the minimum period required to change the EN ratio (change polarity state). The short-circuit-arc cycle is the same period as the transition cycle for performing the melting of the consuming electrode wire 51 and the transfer of molten droplets to the base material 80 or the already stacked weld beads 70.
[0043] like Figure 3 As shown, the short-circuit-arc cycle of polarity EP is repeated during EP, and the short-circuit-arc cycle of polarity EN is repeated during EN. To change the EN ratio, the time ratio of EN polarity can be changed within one AC cycle. That is, if the EN ratio is increased, the number of short-circuit-arc cycles during EP decreases, and the number of short-circuit-arc cycles during EN increases.
[0044] The frequency of communication is Figure 3 As shown in (A), at lower frequencies, the total number of short-circuit-arc cycles in one AC cycle increases, thus requiring more methods to allocate the EP and EN periods, compared to the AC frequency of... Figure 3 Compared to the higher frequency cases shown in (B) and (C), the EN ratio has a greater degree of freedom in variation. That is, the number of possible variations of the EN ratio when the frequency is lower in a cycle of alternating current is greater than the number of possible variations of the EN ratio when the frequency is higher in a cycle of alternating current.
[0045] Specifically, when you want to increase the variable number of the EN ratio and finely adjust the EN ratio (or when you want to decrease the adjustment unit of the EN ratio), such as Figure 3 As shown in (A), the frequency of the exchange can be reduced by lengthening the period of one exchange cycle. Conversely, if one wants to reduce the variable number of the EN ratio and increase the adjustment unit of the EN ratio, as... Figure 3 As shown in (B) and (C), the frequency of communication can be increased by shortening the period of one communication cycle.
[0046] However, if the frequency of communication is increased excessively, the duration of a communication cycle becomes too short, therefore... Figure 3 As shown in (B) and (C), adjustments during EN are almost impossible. For example, in Figure 3 In (B) and (C), adjustments to the EN period can only be made during the three-cycle change period. Therefore, the number of possible changes to the EN ratio becomes extremely small.
[0047] Figure 4 This diagram illustrates the layering state of weld beads 70 under low-frequency conditions. (Example) Figure 4 As shown, when the frequency of the AC is reduced to an extreme (e.g., 1 Hz), the EP period or EN period that can be set becomes too long, due to the increased duration of one AC cycle.
[0048] Therefore, as Figure 4 As shown, the temperature of the molten portion is different, therefore the shape of the stacking direction of the weld bead 70, which is approximately perpendicular to the welding direction indicated by the arrow, is unstable. Based on the above, it is desirable to change the EN ratio within a suitable range of AC frequency. The stacking modeling system 1 sets the AC frequency to a value suitable for stacking by controlling the AC frequency and the EN ratio control device 30, and changes the EN ratio within the set range.
[0049] Under the following welding conditions, verify the range of AC frequencies suitable for stacking. Figure 5 This is a diagram illustrating an example of the welding conditions in Embodiment 1. (As shown...) Figure 5 As shown, in Embodiment 1, during the EP polarity period, the welding conditions are set as follows: the feed speed of the consuming electrode welding wire 51 is 450 (cm / min), the welding speed of the driving welding torch 20 is 50 (cm / min), the current is 110 (A), and the voltage is 16.4 (V). Figure 5 As shown, in Embodiment 1, during the EN polarity period, the welding conditions are set as follows: the feed speed of the consuming electrode welding wire 51 is set to 450 (cm / min), the welding speed of the driving welding torch 20 is set to 50 (cm / min), the current is set to 75 (A), and the voltage is set to 14.4 (V). Figure 5 The welding conditions described are just one example; they could also be AC conditions where the current is fixed during EP and EN periods and the feed rate of the electrode wire 51 is varied.
[0050] The cross-sectional shape of the multi-layered weld bead 70 when welding current is supplied to the consumable electrode wire 51 under the above welding conditions will be described. Figure 6 This is a diagram showing the cross-sectional shape of the stacked weld beads 70. Figure 6 In the middle, weld beads 70 are stacked in a stacking direction (height direction) that is approximately perpendicular to the base material 80.
[0051] Figure 6 (A) is a comparative example showing the cross-sectional shape of the laminated weld bead 70 when a DC current of only EP polarity is supplied to the consuming electrode welding wire 51. Figure 6 (B) is a diagram showing the cross-sectional shape of the stacked weld beads 70 when AC at a frequency of 2Hz is supplied to the consuming electrode wire 51. Figure 6 (C) is a diagram showing the cross-sectional shape of the stacked weld beads 70 when AC at a frequency of 30 Hz is supplied to the consuming electrode wire 51.
[0052] like Figure 6 As shown in (A), when the weld beads 70 are stacked by direct current, the temperature of the molten portion increases as it becomes the upper layer, and the shape becomes unstable due to burn-through of the weld beads 70. Thus, direct current is not suitable for stacking weld beads 70.
[0053] On the other hand, such as Figure 6 As shown in (B) and (C), if AC is used, the deformation caused by burn-through is mitigated compared to DC. Under these conditions, a higher EN ratio results in a better weld bead shape. However, in reality, if the EN ratio is too high when the weld bead 70 has cooled sufficiently, the heat input to the weld bead 70 becomes smaller, resulting in a smaller molten portion and an unstable shape of the weld bead 70. Therefore, it is desirable to select an appropriate EN ratio that matches the state of the weld bead 70.
[0054] At a frequency of 2Hz, if the short-circuit-arc period is set to 10ms, then the number of short-circuit-arc periods in one AC cycle is 50, and the adjustment unit for the EN ratio is 2%. As an example, in... Figure 6 (B) shows five cross-sectional shapes: 20%, 30%, 50%, 70%, and 80%. For example... Figure 6 As shown in (B), the stack shape can be adjusted by finely changing the EN ratio (reducing the change unit). Thus, AC at a frequency of 2Hz is suitable for the stack of weld beads 70.
[0055] At a frequency of 30Hz, if the short-circuit-arc period is set to 10ms, the number of short-circuit-arc periods in one AC cycle is 3~4, and the adjustment unit for the EN ratio is approximately 25~33%. Figure 6 In (C), the variation of the short-circuit-arc period is shown, and the cross-sectional shapes with EN ratios of 20%, 50%, and 80% can be selected under these conditions. Figure 6 As shown in (C), the unit of change for the EN ratio increases, but the stack shape can be adjusted. Thus, AC at a frequency of 30Hz is suitable for the stack of weld beads 70.
[0056] The verification results indicate that the appropriate frequencies for cascaded communication are as follows. Figure 7 This is a diagram used to illustrate a suitable frequency range for Embodiment 1. In the case where the AC frequency is less than 2Hz, such as... Figure 3 (A) Figure 4 As shown, the heat input differs depending on the length of the EP or EN period. Therefore, as... Figure 7 As shown, the stability of the stacking direction is low when the frequency of the AC is less than 2Hz.
[0057] When the frequency of the exchange exceeds 30Hz, such as Figure 3 As shown in (B) and (C), the duration of one cycle of the AC becomes shorter, thus the variable number of the EN ratio becomes very small. Therefore, as Figure 7 As shown, when the frequency of the AC exceeds 30Hz, the adjustment unit of the EN ratio becomes too large and is not suitable for adjusting the stacking shape based on changes in the EN ratio.
[0058] Based on the above, the suitable AC frequency for stacking is a value of 2Hz or higher and 30Hz or lower. The control device 30 stably stacks and deposits weld beads 70 when using consumable electrode welding wire 51 by controlling the AC frequency to a value of 2Hz or higher and 30Hz or lower.
[0059] The processing performed by the control device 30 in Embodiment 1 will be described in detail. Figure 8 This is a flowchart illustrating the control content of Implementation Method 1. Figure 8 The flowchart processing is repeatedly called up and executed as a subroutine from the main routine in the control of the control device 30. The control device 30 first confirms the stacked data pre-stored in the storage device 33 in step S (hereinafter referred to as "S") 1.
[0060] Next, the control device 30 is set. Figure 5 The welding conditions are as shown in S2. Next, the control device 30 sets the AC frequency and EN ratio corresponding to the layering data in S1 and the welding conditions in S2 (S3). In S3, the control device 30 sets the AC frequency to a value of 2Hz or higher and 30Hz or lower. The AC frequency and EN ratio can be directly input by the user via an input unit such as a touch panel or keyboard (not shown), or the arithmetic device 31 can calculate appropriate values. The AC frequency and EN ratio can also be extracted from data predetermined by the control device 30.
[0061] Next, the control device 30 sends information on the AC frequency, EN ratio, current, and voltage to the welding power source 10 (S4). Next, the control device 30 sends information on the welding wire feed speed to the welding wire feed device 50 (S5). Next, the control device 30 sends information on the welding speed to the robotic arm 40 (S6), causing the process to return from the subroutine to the main routine. It should be noted that part or all of the control device 30 can also be integrated into the control device of the welding power source 10 or the robotic arm 40.
[0062] In the layered modeling system 1 of Embodiment 1, the control device 30 sets the AC frequency to a value of 2Hz or higher and 30Hz or lower. For example... Figure 7 As shown, the stability of the stacking direction is improved within the frequency range of 2Hz to 30Hz. The EN ratio can be finely adjusted within the range of 2Hz to 30Hz. Therefore, the stacking modeling system 1 of this disclosure can ensure the stability of the stacking direction and finely adjust the EN ratio, thus enabling stable stacking of weld beads 70 when using consumable electrode welding wire 51.
[0063] [Implementation Method 2]
[0064] Next, the layered modeling system 1A of Embodiment 2 will be described. Figure 9 This is a diagram that schematically illustrates the stacked modeling system 1A of Embodiment 2. The stacked modeling system 1A of Embodiment 2 differs from the stacked modeling system 1 of Embodiment 1 in that it includes a detection device 61.
[0065] The detection device 61 is, for example, a shape sensor. The shape sensor (detection device 61) is used to detect when the weld beads 70 are stacked, relative to... Figure 9 The shape sensor (detection device 61) detects the shape of the weld bead 70 at position H preceding the currently stacked layer, according to the welding direction indicated by the arrow. A non-contact sensor, such as a laser scanner, is preferably used. Position H corresponds to the layer preceding the currently stacked layer (also called the previous layer). The shape sensor (detection device 61) sends the height information of the weld bead 70 as shape information to the control device 30.
[0066] The control device 30 controls at least one of the frequency and EN ratio based on the height information of the weld bead 70 received from the shape sensor (detection device 61). For example, the control device 30 performs the following processing: When the height of the previous layer is high, the control device 30 decreases the EN ratio to make the currently stacked layer lower. When the height of the previous layer is low, the control device 30 increases the EN ratio to make the currently stacked layer higher. When the previous layer is unstable, the control device 30 increases the frequency to stabilize the currently stacked layer. When the control device 30 wants to change the EN ratio from the previous layer at finer intervals, it decreases the frequency to narrow the adjustment range of the EN ratio.
[0067] The detection device 61 can also be, for example, a temperature sensor. The temperature sensor (detection device 61) measures the temperature relative to the weld beads 70 as the weld beads are stacked. Figure 9 The temperature of the weld bead 70 at position H in front of the layered weld bead, indicated by the arrow in the diagram, is detected in the welding direction. The temperature sensor (detection device 61) is preferably a non-contact sensor such as a thermal imager. The temperature information of the weld bead 70 detected by the temperature sensor (detection device 61) is sent to the control device 30. Alternatively, the temperature sensor (detection device 61) may be a pyrometer that takes point-based images, rather than a thermal imager that takes area-based images.
[0068] The control device 30 controls at least one of the AC frequency and the EN ratio based on the temperature information of the weld bead 70 received from the temperature sensor (detection device 61). For example, the control device 30 performs the following processing: When the temperature of the previous layer is high, the control device 30 increases the EN ratio to lower the temperature of the currently stacked layer. When the temperature of the previous layer is low, the control device 30 decreases the EN ratio to raise the temperature of the currently stacked layer.
[0069] It should be noted that the detection device 61 may also include both a shape sensor and a temperature sensor. The control device 30 controls at least one of the AC frequency and the EN ratio based on the information obtained from the detection device 61, thereby enabling the execution of a layer stack corresponding to the state of the previous layer.
[0070] [Variation Example]
[0071] In the above embodiments, the welding torch 20 may also be moved by an orthogonal robot instead of a multi-jointed robotic arm 40.
[0072] [Summarize]
[0073] (1) This disclosure relates to a stacked molding system 1, which uses a consumable electrode arc welding method with short-circuit transition to supply welding current to a consumable electrode welding wire 51 and stack weld beads 70 to shape an object. The stacked molding system 1 includes: a welding torch 20, which performs the stacking of weld beads 70 using consumable electrode welding wire 51; a drive device (robotic arm 40) that moves the welding torch 20; a welding power source 10 that supplies alternating current as welding current to the consumable electrode welding wire 51; and a control device 30 that controls the frequency of the alternating current and the EN ratio. The change period of the EN ratio is constant and independent of the frequency of the alternating current. The control device 30 sets the frequency of the alternating current to a value of 2 Hz or higher and 30 Hz or lower.
[0074] According to the stack-up system 1 of this disclosure, the control device 30 sets the AC frequency to a value of 2 Hz or higher and 30 Hz or lower. The stability of the stacking direction is improved when the AC frequency is within the range of 2 Hz or higher and 30 Hz or lower. The EN ratio can be finely adjusted within the range of 2 Hz or higher and 30 Hz or lower. Therefore, the stack-up system 1 of this disclosure can ensure the stability of the stacking direction and finely adjust the EN ratio, thus enabling stable stacking of weld beads 70 when using consumable electrode wire 51.
[0075] (2) Based on the stacked modeling system 1 in (1), the adjustment unit of the EN ratio (e.g., 2%) when the AC frequency is a first frequency (e.g., 2Hz) is set to be smaller than the adjustment unit of the EN ratio (e.g., 25%~33%) when the AC frequency is a second frequency higher than the first frequency (e.g., 30Hz).
[0076] According to the layered modeling system 1 disclosed herein, the adjustment unit of the EN ratio can be adjusted by changing the frequency of the communication.
[0077] (3) Based on the stacking modeling system 1 of (1) or (2), the control device 30 increases the EN ratio while increasing the stacking height of the weld bead 70.
[0078] According to the stacking modeling system 1 disclosed herein, the stacking height can be easily increased by increasing the EN ratio.
[0079] (4) Based on the stacking modeling system 1A described in any one of (1) to (3), the system further includes a shape sensor (detection device 61) which detects the shape of the weld bead 70 in front of it during the stacking process. The control device 30 controls at least one of the AC frequency and the EN ratio based on the shape of the weld bead 70 detected by the shape sensor (detection device 61).
[0080] According to the stacking modeling system 1A of this disclosure, it is possible to perform stacking that corresponds to the shape of the weld bead 70 preceding the stacking detected by the shape sensor (detection device 61).
[0081] (5) Based on the stacking molding system 1A described in any one of (1) to (4), the system further includes a temperature sensor (detection device 61) that detects the temperature of the weld bead preceding the weld bead being stacked when the weld bead 70 is being stacked. The control device 30 controls at least one of the AC frequency and the EN ratio based on the temperature of the weld bead 70 detected by the temperature sensor (detection device 61).
[0082] According to the stacking modeling system 1A disclosed herein, stacking can be performed in accordance with the temperature of the weld bead 70 preceding the stacking process detected by the temperature sensor (detection device 61).
[0083] The embodiments disclosed herein should be considered illustrative in all respects and not restrictive. The scope of this disclosure is not defined by the description of the embodiments above, but by the technical solutions, and is intended to include all equivalents and modifications within the scope of the technical solutions.
[0084] Explanation of reference numerals in the attached figures
[0085] 1.1A Layered Modeling System, 10 Welding Power Source, 20 Welding Torch, 21 Nozzle, 30 Control Device, 31 Computing Device, 32 Memory, 33 Storage Device, 34 Input / Output Interface, 40 Robotic Arm, 50 Welding Wire Feeding Device, 51 Consumable Electrode Welding Wire, 61 Detection Device, 70 Weld Beads, 80 Base Material, 330 Control Program.
Claims
1. A layered molding system that uses a consumable electrode arc welding method with short-circuit transition, supplies welding current to a consumable electrode welding wire, and layers weld beads to shape the object, wherein, The layered modeling system has the following features: A welding torch that performs a stacking of weld beads using the consumable electrode wire; A drive device that moves the welding torch; A welding power source that supplies alternating current as the welding current to the consumable electrode wire; and Control device, which controls the frequency and EN ratio of the AC signal. The EN ratio changes periodically and is constant regardless of the frequency of the AC. The control device sets the frequency of the AC signal to a value between 2 Hz and 30 Hz.
2. The layered modeling system according to claim 1, wherein, The adjustment unit for the EN ratio when the frequency of the AC is a first frequency is set to be smaller than the adjustment unit for the EN ratio when the frequency of the AC is a second frequency higher than the first frequency.
3. The layered modeling system according to claim 1 or 2, wherein, The control device increases the EN ratio by increasing the stack height of the weld bead.
4. The layered modeling system according to claim 1 or 2, wherein, The stacking system also includes a shape sensor, which detects the shape of the weld bead preceding it during the stacking process. The control device controls at least one of the AC frequency and the EN ratio based on the shape of the weld bead detected by the shape sensor.
5. The layered modeling system according to claim 1 or 2, wherein, The stacking system also includes a temperature sensor that detects the temperature of the weld bead preceding it during the stacking process. The control device controls at least one of the AC frequency and the EN ratio based on the temperature of the weld bead detected by the temperature sensor.
Citation Information
Patent Citations
Laminate molded article manufacturing method
JP2022106172A