Polycarbonate compositions with good ductility and flame retardant properties

By incorporating a combination of polycarbonate-siloxane copolymer, bisphenol A bis(diphenyl phosphate), and polytetrafluoroethylene into polycarbonate, the problem of decreased mechanical properties of polycarbonate after the addition of flame retardants has been solved. This has enabled the use of high-recycled polycarbonate in consumer electronics products to achieve both flame retardancy and impact resistance, thus meeting sustainability requirements.

CN123125280APending Publication Date: 2026-11-17SHPP GLOBAL TECH BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202580027888.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-19
Filing Date
2025-04-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

When flame retardants are added to existing polycarbonates in consumer electronics, their mechanical properties, especially impact strength, decrease. At the same time, PCR plastic compositions with high recycled content cannot provide sufficient flame retardancy and mechanical properties, making it difficult to meet sustainability requirements.

Method used

The polymer's flame retardancy and impact resistance are enhanced by a combination of about 10 wt% to about 90 wt% of polycarbonate component, about 2 wt% to about 40 wt% of polycarbonate-siloxane copolymer (PC-Si), about 2 wt% to about 15 wt% of bisphenol A bis(diphenyl phosphate) flame retardant (BPADP) and about 0.05 wt% to about 2 wt% of polytetrafluoroethylene (PTFE) flame retardant, and it contains a high loading of mechanically recycled polycarbonate.

Benefits of technology

This technology enables polymers to maintain good ductility while possessing excellent impact resistance and flame retardant properties, meeting the sustainability requirements of consumer electronics products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The thermoplastic composition comprises: (a) about 10 wt% to about 90 wt% of a polycarbonate component; (b) about 2 wt% to about 40 wt% of a polycarbonate-siloxane (PC-Si) copolymer, wherein the siloxane content of the PC-Si copolymer is at least 25 wt%; (c) about 2 wt% to about 15 wt% of a bisphenol A bis(diphenyl phosphate) (BPADP) flame retardant; and (d) about 0.05 wt% to about 2 wt% of a polytetrafluoroethylene (PTFE) flame retardant. The combined weight percentage of all components does not exceed 100 wt%, and all weight percentages are based on the total weight of the composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to polycarbonate compositions, and more particularly to polycarbonate compositions comprising polycarbonate-siloxane copolymers, said polycarbonate compositions having good ductility and flame retardant properties. Background Technology

[0002] Polycarbonate is a popular plastic in the consumer electronics (CE) market due to its flexibility. Flame retardant additives are incorporated to improve the flame retardancy (FR) of the polymer in CE applications. However, additional flame retardant additives can reduce some mechanical properties of polycarbonate, especially impact strength.

[0003] Furthermore, more customers in the CE market are seeking sustainable components to improve the green footprint of their products. Using post-consumer recycled (PCR) plastics could potentially meet the expectations of these customers. However, compositions including PCR plastics, especially those with high recycling content, do not provide sufficient FR and mechanical properties for many CE applications.

[0004] These and other disadvantages are addressed through various aspects of this disclosure. Summary of the Invention

[0005] Various aspects of this disclosure relate to thermoplastic compositions comprising: (a) about 10 wt% to about 90 wt% of a polycarbonate component; (b) about 2 wt% to about 40 wt% of a polycarbonate-siloxane (PC-Si) copolymer, wherein the siloxane content of the PC-Si copolymer is at least 25 wt%; (c) about 2 wt% to about 15 wt% of a bisphenol A bis(diphenyl phosphate) (BPADP) flame retardant; and (d) about 0.05 wt% to about 2 wt% of a polytetrafluoroethylene (PTFE) flame retardant. The combined weight percentage of all components does not exceed 100 wt%, and all weight percentages are based on the total weight of the composition. Detailed Implementation

[0006] This disclosure relates to a novel composition of an impact-modified FR polycarbonate (PC) compound that may include a high loading of mechanically recycled post-consumer PC. The composition provides a balance between FR and excellent impact resistance, and the recycled contents meet customer expectations for sustainability. Specifically, determining that a siloxane-based PC copolymer (polycarbonate-siloxane copolymer) with a siloxane content of about 25-65 wt% enhances the FR and ductility properties of the PC blend.

[0007] Before disclosing and describing the compounds, compositions, articles, systems, devices, and / or methods of this disclosure, it should be understood that, unless otherwise specified, they are not limited to specific synthetic methods, or, unless otherwise specified, are not limited to specific reagents, and therefore, they can certainly be varied. It should also be understood that the terminology used herein is for descriptive purposes only and is not intended to be limiting.

[0008] This disclosure covers various combinations of elements of this disclosure, such as combinations of elements from supplementary claims attached to the same independent claim.

[0009] Furthermore, it should be understood that, unless otherwise expressly stated, any method described herein is not intended to be construed as requiring its steps to be performed in a specific order. Therefore, in no way is an order intended to be inferred unless a method claim actually describes the order in which its steps are followed, or unless the claims or description specifically state that the steps are limited to a specific order. This applies to any possible non-expressive basis for interpretation, including: matters concerning the logic of the arrangement of steps or the flow of operations; literal meaning derived from grammatical organization or punctuation; or the number or type of aspects described in the description.

[0010] All publications mentioned herein are incorporated herein by reference to disclose and describe the methods and / or materials in connection with the cited publications.

[0011] definition

[0012] It should also be understood that the terminology used herein is for descriptive purposes only and is not intended to be limiting. As used in the specification and claims, the term "comprising" can include aspects "consisting of" and "consisting essentially of". Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure pertains. Reference will be made to numerous terms that should be defined herein in this specification and the following claims.

[0013] As used in the specification and appended claims, unless the context clearly specifies otherwise, the singular forms “a”, “an”, and “the” include plural indicators. Thus, for example, reference to “polycarbonate” includes a mixture of two or more polycarbonate polymers.

[0014] As used herein, the term "composite" includes blends, mixtures, alloys, reaction products, etc.

[0015] A range may be expressed herein as a range from one value (first value) to another value (second value). When expressing such a range, the range includes, in some respects, one or both of the first and second values. Similarly, when a value is expressed as an approximation using the antecedent “about,” it should be understood that a particular value forms another aspect. It should be further understood that the endpoints of each range are significant relative to and independent of the other endpoint. It should also be understood that many values ​​are disclosed herein, and each value is disclosed herein as “about” the particular value in addition to the value itself. For example, if the value “10” is disclosed, “about 10” is also disclosed. It should also be understood that each unit between two particular units is also disclosed. For example, if 10 and 15 are disclosed, 11, 12, 13, and 14 are also disclosed.

[0016] As used herein, the terms “about” and “at or about” mean that the quantity or value discussed may be a specific value, an approximate specific value, or about the same as the specific value. It should generally be understood that, as used herein, nominal values ​​indicate a variation of ±10%, unless otherwise indicated or inferred. These terms are intended to convey that similar values ​​result in equivalent results or effects as described in the claims. That is, it should be understood that quantities, sizes, formulations, parameters, and other quantities and characteristics are not and need not be precise, but may be approximate and / or larger or smaller as needed, reflecting tolerances, conversion factors, rounding, measurement errors, and other factors known to those skilled in the art. Generally, quantities, sizes, formulations, parameters, or other quantities or characteristics are “about” or “approximate,” whether explicitly stated or not. It should be understood that where “about” is used before a quantifiable value, the parameter also includes the specific quantifiable value itself, unless otherwise specifically stated.

[0017] The components used to prepare the compositions of this disclosure and the compositions themselves used in the methods disclosed herein are disclosed. These and other materials are disclosed herein, and it should be understood that while specific references to various individual and collective combinations and arrangements of these materials cannot be explicitly disclosed, each is specifically considered and described herein. For example, if a particular compound is disclosed and discussed, and various modifications that may be made to multiple molecules (including the compound) are discussed, then each combination and arrangement of the compound and possible modifications are specifically considered unless specifically indicated to the contrary. Thus, if a class of molecules A, B, and C and a class of molecules D, E, and F are disclosed, and examples of the combination molecule AD are disclosed, then each combination is considered individually and collectively, even if each combination is not described separately; this means that combinations AE, AF, BD, BE, BF, CD, CE, and CF are considered disclosed. Similarly, any subsets or combinations of these are also disclosed. Thus, for example, subgroups AE, BF, and CE would be considered disclosed. This concept applies to all aspects of this application, including but not limited to steps in methods of making and using the compositions of this disclosure. Therefore, if there are various additional steps that can be performed, it should be understood that each of these additional steps can be performed in any specific aspect or combination of aspects of the method disclosed herein.

[0018] References to the weight parts of a particular element or component in the composition or article in the specification and the final claims indicate the weight relationship between the element or component and any other element or component, expressed as parts by weight. Thus, in a compound containing 2 parts by weight of component X and 5 parts by weight of component Y, X and Y are present in a weight ratio of 2:5, and are present in such a ratio regardless of whether the compound contains any additional components.

[0019] Unless specifically stated to the contrary, the weight percentage of a component is based on the total weight of the formulation or composition including the component.

[0020] As used herein, the interchangeable terms “BisA,” “BPA,” or “bisphenol A” refer to compounds having a structure represented by the following formula:

[0021]

[0022] BisA can also be referred to by the names 4,4'-(propane-2,2-diyl)diol; p,p'-isopropylidene bisphenol; or 2,2-bis(4-hydroxyphenyl)propane. The CAS number for BisA is 80-05-7.

[0023] As used herein, “polycarbonate” means an oligomer or polymer comprising residues of one or more dihydroxy compounds (e.g., dihydroxy aromatic compounds) linked by carbonate bonds; it also encompasses homopolymers, copolymers and (co)polyesters.

[0024] The terms “residue” and “structural unit” used to describe the composition of the polymer are synonymous throughout the specification.

[0025] As used herein, unless otherwise specified, the terms "weight percentage," "wt%," and "wt.%" are used interchangeably to indicate the weight percentage of a given component based on the total weight of the composition. That is, unless otherwise specified, all wt% values ​​are based on the total weight of the composition. It should be understood that the sum of the wt% values ​​of all components in the disclosed composition or formulation is equal to 100.

[0026] Unless otherwise stated herein, all testing standards are current and valid at the time of filing of this application.

[0027] Each raw material used in the exemplary and / or comparative compositions described herein is commercially available and / or its manufacturing method is known to those skilled in the art.

[0028] It should be understood that the compositions disclosed herein have certain functions. This document discloses certain structural requirements for performing the disclosed functions, and it should be understood that various structures exist that can perform the same functions associated with the disclosed structures, and these structures generally achieve the same results.

[0029] thermoplastic composition

[0030] Various aspects of this disclosure relate to thermoplastic compositions comprising: (a) about 10 wt% to about 90 wt% of a polycarbonate component; (b) about 2 wt% to about 40 wt% of a polycarbonate-siloxane (PC-Si) copolymer, wherein the siloxane content of the PC-Si copolymer is at least 25 wt%; (c) about 2 wt% to about 15 wt% of a bisphenol A bis(diphenyl phosphate) (BPADP) flame retardant; and (d) about 0.05 wt% to about 2 wt% of a polytetrafluoroethylene (PTFE) flame retardant. The combined weight percentage of all components does not exceed 100 wt%, and all weight percentages are based on the total weight of the composition.

[0031] The polycarbonate component may include virgin polycarbonate or mechanically recycled polycarbonate, and may include polycarbonate copolymers. In one particular aspect, the polycarbonate component includes mechanically recycled polycarbonate. An exemplary mechanically recycled polycarbonate is post-consumer recycled polycarbonate (PCR-PC). PCR-PC is purchased from, for example, Hongyu.

[0032] In some aspects, the composition comprises about 10 wt% to about 90 wt% of a polycarbonate component. In other aspects, the composition comprises at least 10 wt%, or at least 15 wt%, or at least 20 wt%, or at least 25 wt%, or at least 30 wt%, or at least 35 wt%, or at least 40 wt%, or at least 45 wt%, or at least 50 wt%, or at least 55 wt%, or at least 60 wt%, or at least 65 wt%, or at least 70 wt%, or at least 75 wt%, or at least 80 wt%, or at most 90 wt%, or at most 85 wt%, or at most 80 wt%, or at most 75 wt%, or at most 70 wt%, or at most 65 wt%, or at most 60 wt%, or at most 55 wt%, or at most 50 wt% of a polycarbonate component.

[0033] In a particular aspect, the composition comprises about 50 wt% to about 85, or at least 50 wt%, or at least 55 wt%, or at least 60 wt%, or at least 65 wt%, or at least 70 wt%, or at least 75 wt%, or at least 80 wt%, or at most 85 wt%, or at most 80 wt%, or at most 75 wt%, or at most 70 wt%, or at most 65 wt%, or at most 60 wt% of mechanically recycled polycarbonate.

[0034] In some aspects, the composition comprises more than 0 wt% to about 20 wt%, or at least 1 wt%, or at least 2 wt%, or at least 3 wt%, or at least 4 wt%, or at least 5 wt%, or at least 10 wt%, or at least 15 wt%, or at most 20 wt%, or at most 19 wt%, or at most 18 wt%, or at most 17 wt%, or at most 16 wt%, or at most 15 wt%, or at most 14 wt%, or at most 13 wt%, or at most 12 wt%, or at most 11 wt%, or at most 10 wt% of at least one virgin polycarbonate.

[0035] The compositions according to various aspects of this disclosure comprise about 2 wt% to about 40 wt% of a polycarbonate-siloxane (PC-Si) copolymer. The PC-Si copolymer has a siloxane content of at least 25 wt%. In some aspects, the polycarbonate copolymer component comprises a polycarbonate-siloxane copolymer having a siloxane content of about 25 wt% to about 65 wt%, or at least 25 wt%, or at least 30 wt%, or at least 35 wt%, or at most 65 wt%, or at most 60 wt%, or at most 55 wt%, or at most 50 wt%, or at most 45 wt%, based on the total weight of the polycarbonate-siloxane copolymer component. In other aspects, the polycarbonate-siloxane copolymer has a siloxane content of about 35-45 wt%, or about 38-42 wt%, or about 40 wt% (e.g., a 40 wt% siloxane copolymer purchased from SABIC).

[0036] In other respects, the composition comprises at least 2 wt%, or at least 3 wt%, or at least 4 wt%, or at least 5 wt%, or at least 6 wt%, or at least 7 wt%, or at least 8 wt%, or at least 9 wt%, or at least 10 wt%, or at least 11 wt%, or at least 12 wt%, or at least 13 wt%, or at least 14 wt%, or at least 15 wt%, or up to 40 wt%, or up to 39 wt%, or up to 38 wt%, or up to 37 wt%, or up to 36 wt%, or up to 35 wt%, or up to 34 wt%, or up to 33 wt%, or up to 32 wt%, or up to 31 wt%, or up to 30 wt%, or up to 29 wt%, or up to 28 wt%, or up to 27 wt%, or up to 26 wt%, or up to 25 wt%, or up to 24 wt%, or up to 23 wt%, or up to 22 wt%. The composition comprises, by weight, or at most 21 wt%, or at most 20 wt%, or at most 19 wt%, or at most 18 wt%, or at most 17 wt%, or at most 16 wt%, or at most 15 wt%, or at most 14 wt%, or at most 13 wt%, or at most 12 wt%, or at most 11 wt%, or at most 10 wt%, of a polycarbonate-siloxane copolymer, wherein the siloxane content is at least 25 wt%. In one particular aspect, the composition comprises, by weight, or at most 5 wt% to about 30 wt%, or by weight, or at most 5 wt% to about 10 wt%, of a PC-Si copolymer.

[0037] The compositions according to various aspects of this disclosure comprise about 2 wt% to about 15 wt% of a BPADP flame retardant. BPADP has the structure of Formula 1:

[0038] (1)

[0039] In some aspects, the composition comprises at least 2 wt%, or at least 3 wt%, or at least 4 wt%, or at least 5 wt%, or at least 6 wt%, or at least 7 wt%, or at least 8 wt%, or at least 9 wt%, or at least 10 wt%, or at least 11 wt%, or at least 12 wt%, or at least 13 wt%, or at least 14 wt%, or up to 15 wt%, or up to 14 wt%, or up to 13 wt%, or up to 12 wt%, or up to 11 wt%, or up to 10 wt%, or up to 9 wt%, or up to 8 wt%, or up to 7 wt%, or up to 6 wt% of a BPADP flame retardant. In some aspects, the composition comprises about 5 wt% to about 15 wt%, or about 5 wt% to about 10 wt% of a BPADP flame retardant.

[0040] The composition comprises about 0.05 wt% to about 2 wt% of a polytetrafluoroethylene (PTFE) flame retardant. The PTFE flame retardant provides the composition with anti-dripping properties. An exemplary PTFE flame retardant is styrene-acrylonitrile encapsulated PTFE (SAN-PTFE or TSAN). In a particular aspect, the composition comprises at least 0.05 wt%, or at least 0.1 wt%, or at least 0.2 wt%, or at least 0.3 wt%, or at least 0.4 wt%, or at least 0.5 wt%, or at least 0.6 wt%, or at least 0.7 wt%, or at least 0.8 wt%, or at least 0.9 wt%, or at least 1.0 wt%, or at most 2 wt%, or at most 1.9 wt%, or at most 1.8 wt%, or at most 1.7 wt%, or at most 1.6 wt%, or at most 1.5 wt%, or at most 1.4 wt%, or at most 1.3 wt%, or at most 1.2 wt%, or at most 1.1 wt%, or at most 1.0 wt% of a PTFE flame retardant.

[0041] In other respects, the composition includes at least one additional additive. At least one additional additive may include, but is not limited to, deacidifying agents, anti-dripping agents, antioxidants, antistatic agents, chain extenders, colorants, release agents, flow promoters, lubricants, plasticizers, quenchers, additional flame retardants, UV reflective additives, impact modifiers, foaming agents, reinforcing agents, or combinations thereof.

[0042] In a particular aspect, the composition comprises about 0.1 wt% to about 10 wt%, or at least 0.1 wt%, or at least 0.2 wt%, or at least 0.3 wt%, or at least 0.4 wt%, or at least 0.5 wt%, or at least 0.6 wt%, or at least 0.7 wt%, or at least 0.8 wt%, or at least 0.9 wt%, or at least 1.0 wt%, or at most 10 wt%, or at most 9 wt%, or at most 8 wt%, or at most 7 wt%, or at most 6 wt%, or at most 5 wt%, or at most 4 wt%, or at most 3 wt%, or at most 2 wt%, or at most 1 wt%, or at most 0.9 wt%, or at most 0.8 wt%, or at most 0.7 wt%, or at most 0.6 wt%, or at most 0.5 wt% of at least one additional additive.

[0043] According to UL94 assessment, the compositions according to various aspects of this disclosure can exhibit good flame retardant (FR) properties. In some aspects, according to UL94 assessment, the compositions have a V0 flame retardant rating at thicknesses of 1.0 mm, 0.9 mm, 0.8 mm, or 0.75 mm. According to UL94, the V0 flame retardant rating is achieved both before and after aging.

[0044] In some respects, the compositions according to aspects of this disclosure have a melt flow rate of at least 8 g / 10 min, as tested according to ASTM D1238 at a temperature of 265°C and a load of 2.16 kg. In other respects, the MFR is at least 9 g / 10 min, or at least 10 g / 10 min, or at least 11 g / 10 min, or at least 12 g / 10 min, or at least 13 g / 10 min, or at least 14 g / 10 min, or at least 15 g / 10 min, or at most 25 g / 10 min, or at most 20 g / 10 min, as tested according to ASTM D1238 at a temperature of 265°C and a load of 2.16 kg.

[0045] In other respects, according to ASTM D256 using a pendulum energy of 5 lbf / ft, the compositions according to various aspects of this disclosure have a notched Izod impact (NII) strength of at 23°C of at least 300 joules / meter (J / m), or at least 350 J / m, or at least 400 J / m, or at least 450 J / m, or at least 500 J / m, or at least 550 J / m, or at least 600 J / m, or at least 650 J / m, or at least 700 J / m, or at least 750 J / m, or at least 800 J / m, or at least 850 J / m, or at least 900 J / m.

[0046] In other respects, according to ASTM D256, using a pendulum energy of 5 lbf / ft, the composition has at least 90% NII ductility, or at least 95% ductility, or 100% ductility at 23°C.

[0047] In certain respects, according to ASTM D256 using a pendulum energy of 5 lbf / ft, the composition has a NII strength of at 0°C of at least 300 J / m, or at least 350 J / m, or at least 400 J / m, or at least 450 J / m, or at least 500 J / m, or at least 550 J / m, or at least 600 J / m, or at least 650 J / m, or at least 700 J / m, or at least 750 J / m, or at least 800 J / m.

[0048] In certain aspects, the composition has at least 90% NII ductility, or at least 95% ductility, or 100% ductility at 0°C, as assessed by ASTM D256 using a pendulum energy of 5 lbf / ft.

[0049] In some respects, the composition has an L* value of at least 80, as evaluated using a sample thickness of 3.2 mm in the CIELab color space. In other respects, the composition has an L* value of at least 81, or at least 82, or at least 83, or at least 84, or at least 85, or at least 86, or at least 87, or at least 88, as evaluated using a sample thickness of 3.2 mm in the CIELab color space.

[0050] In a specific aspect, the composition was assessed for chemical resistance after 7 days of exposure to a sunscreen with a sun protection factor (SPF) of 30 (SPF30) under an applied strain of 0.7%.

[0051] Manufacturing method

[0052] One or any of the aforementioned components described herein can be first dry-blended with each other or with any combination of the aforementioned components, and then fed into the extruder from one or more feeders, or fed into the extruder individually from one or more feeders. Alternatively, the fillers used in this disclosure can be first treated into a masterbatch and then fed into the extruder. The components can be fed into the extruder from a throat hopper or any side feeder.

[0053] The extruder used in this disclosure may have a single screw, multiple screws, meshing screws rotating in the same or opposite directions, non-meshing screws rotating in the same or opposite directions, reciprocating screws, pin-driven screws, screen-driven screws, pin-driven barrels, rollers, plungers, helical rotors, co-kneaders, disc extruders, various other types of extrusion equipment, or combinations including at least one of the aforementioned extruders.

[0054] The components can also be mixed together and then melt-blended to form a thermoplastic composition. Melt blending of the components involves the use of shear force, tensile force, compressive force, ultrasonic energy, electromagnetic energy, thermal energy, or a combination of at least one of the foregoing forms of force or energy.

[0055] If the resin is a semi-crystalline organic polymer, the barrel temperature on the extruder during compounding can be set to the temperature at which at least a portion of the polymer has reached a temperature greater than or equal to approximately the melt temperature; or if the resin is an amorphous resin, the barrel temperature can be set to the temperature at which at least a portion of the polymer has reached a temperature greater than or equal to approximately the flow point (e.g., the glass transition temperature).

[0056] If desired, the mixture comprising the foregoing components can undergo multiple blending and forming steps. For example, the thermoplastic composition can first be extruded and formed into granules. The granules can then be fed into a molding machine, where they can be formed into any desired shape or product. Alternatively, the thermoplastic composition produced in a single melt mixer can be formed into sheets or bundles and subjected to post-extrusion processes such as annealing, uniaxial or biaxial orientation.

[0057] In some aspects, the melt temperature in the process of this invention can be kept as low as possible to avoid excessive thermal degradation of the components. In some aspects, the melt temperature is maintained between about 230°C and about 350°C, but higher temperatures can be used provided that the residence time of the resin in the processing equipment remains relatively short. In some aspects, the melt-processed composition exits the processing equipment, such as an extruder, through a small outlet orifice in a die. The bundles produced from the molten resin can be cooled by passing the bundles through a water bath. The cooled bundles can be cut into pellets for packaging and further processing.

[0058] Products

[0059] In some aspects, this disclosure relates to molded articles, formed articles, or molded articles comprising thermoplastic compositions. Thermoplastic compositions can be molded into useful molded articles in a variety of ways, such as injection molding, extrusion, rotational molding, blow molding, and thermoforming, to form articles and structural components, for example, personal or commercial electronic devices, including but not limited to cellular phones, tablet computers, personal computers, laptop computers, and portable computers, as well as other such devices, medical applications, RFID applications, automotive applications, etc. In other aspects, the articles are extruded. In still other aspects, the articles are injection molded.

[0060] In some respects, the product is a component of consumer electronic devices.

[0061] This disclosure covers various combinations of elements of this disclosure, such as combinations of elements from supplementary claims attached to the same independent claim.

[0062] All aspects of this disclosure

[0063] In all respects, this disclosure relates to and includes at least the following aspects.

[0064] Aspect 1. A thermoplastic composition comprising, consisting of, or substantially consisting of the following:

[0065] a. A polycarbonate component of about 10 wt% to about 90 wt%;

[0066] b. About 2 wt% to about 40 wt% of a polycarbonate-siloxane (PC-Si) copolymer, wherein the siloxane content of the PC-Si copolymer is at least 25 wt%;

[0067] c. Approximately 2 wt% to approximately 15 wt% of bisphenol A bis(diphenyl phosphate) (BPADP) flame retardant; and

[0068] d. Approximately 0.05 wt% to approximately 2 wt% of polytetrafluoroethylene (PTFE) flame retardant.

[0069] The combined weight percentage of all components does not exceed 100 wt%, and all weight percentages are based on the total weight of the composition.

[0070] Aspect 2. The thermoplastic composition according to aspect 1, wherein the polycarbonate component comprises virgin polycarbonate or mechanically recycled polycarbonate.

[0071] Aspect 3. The thermoplastic composition according to aspect 2, wherein the polycarbonate component comprises mechanically recycled polycarbonate.

[0072] Aspect 4. The thermoplastic composition according to any one of Aspects 1 to 3, wherein the composition comprises about 50 wt% to about 85 wt% of mechanically recycled polycarbonate.

[0073] Aspect 5. The thermoplastic composition according to aspect 4, wherein the composition further comprises more than 0 wt% to about 20 wt% of at least one virgin polycarbonate.

[0074] Aspect 6. The thermoplastic composition according to any one of Aspects 1 to 5, wherein the siloxane content of the PC-Si copolymer is from 25 wt% to 65 wt%.

[0075] Aspect 7. The thermoplastic composition according to any one of Aspects 1 to 6, wherein the siloxane content of the PC-Si copolymer is 35 wt% to 45 wt%.

[0076] Aspect 8. The thermoplastic composition according to any one of Aspects 1 to 7, wherein the composition comprises about 5 wt% to about 30 wt% of the PC-Si copolymer.

[0077] Aspect 9. The thermoplastic composition according to any one of Aspects 1 to 8, wherein the composition comprises about 5 wt% to about 15 wt% of the BPADP flame retardant.

[0078] Aspect 10. The thermoplastic composition according to any one of Aspects 1 to 9, wherein the composition comprises at least one additional additive.

[0079] Aspect 11. The thermoplastic composition according to aspect 10, wherein the at least one additional additive comprises an acid remover, an anti-dripping agent, an antioxidant, an antistatic agent, a chain extender, a colorant, a release agent, a flow promoter, a lubricant, a plasticizer, a quencher, an additional flame retardant, a UV reflective additive, an impact modifier, a foaming agent, a reinforcing agent, or a combination thereof.

[0080] Aspect 12. The thermoplastic composition according to aspect 10 or 11, wherein the composition comprises about 0.1 wt% to about 10 wt% of the at least one additional additive.

[0081] Aspect 13. The thermoplastic composition according to any one of Aspects 1 to 12, wherein the composition has a V0 flame retardant rating when the thickness is 0.75 mm, as evaluated according to UL94.

[0082] Aspect 14. The thermoplastic composition according to any one of Aspects 1 to 13, wherein the composition has a melt flow rate of at least 15 g / 10 min when tested according to ASTM D1238 at a temperature of 265°C and a load of 2.16 kg.

[0083] Aspect 15. The thermoplastic composition according to any one of aspects 1 to 14, wherein the composition comprises:

[0084] The notched cantilever beam impact (NII) strength at 23°C is at least 300 joules per meter (J / m).

[0085] The NII has a ductility of at least 90% at 23°C;

[0086] The NII strength at 0°C is at least 300 J / m; or

[0087] The NII has a ductility of at least 90% at 0°C.

[0088] The NII strength and NII ductility are evaluated according to ASTM D256 at a specified temperature using a pendulum energy of 5 lbf / ft.

[0089] Aspect 16. The thermoplastic composition according to any one of Aspects 1 to 15, wherein the composition has an L* value of at least 80 when evaluated using a sample thickness of 3.2 mm in the CIELab color space.

[0090] Aspect 17. The thermoplastic composition according to any one of Aspects 1 to 16, wherein the composition is assessed as chemically resistant after exposure to a sunscreen with a sun protection factor (SPF) of 30 (SPF30) for 7 days under an applied strain of 0.7%.

[0091] Aspect 18. An article comprising the thermoplastic composition according to any one of aspects 1 to 17.

[0092] Aspect 19. The article of manufacture according to aspect 18, wherein the article of manufacture is a component of a consumer electronic device.

[0093] Example

[0094] The following examples are provided to provide a complete disclosure and description of how to manufacture and evaluate the compounds, compositions, articles, apparatus, and / or methods claimed herein, and are intended merely as examples and not to limit this disclosure. Efforts have been made to ensure the accuracy of figures (e.g., amounts, temperatures, etc.), but some errors and deviations should be accounted for. Unless otherwise indicated, parts are parts by weight, temperatures are in °C or at ambient temperature, and pressures are at or near atmospheric pressure. Unless otherwise indicated, percentages of compositions refer to wt%.

[0095] There are many variations and combinations of reaction conditions, such as component concentration, desired solvent, solvent mixture, temperature, pressure, and other reaction ranges and conditions that can be used to optimize the purity and yield of the product obtained from the process. Optimizing such process conditions requires only reasonable and routine experiments.

[0096] The compositions described herein include one or more of the components listed in Table 1:

[0097] Table 1 - Components

[0098]

[0099] The compositions described herein were extruded into granules, which were then injection molded into samples for specified testing. The granule compounding process was performed on a Toshiba TEM-37BS twin-screw extruder. The FR component (BPADP) was fed separately before zone 3. Other resins and additives were premixed and fed from the main feed inlet using a separate feeder. The granules were then molded into compositions / samples according to the conditions shown in Table 2.

[0100] Table 2 - Injection Molding Conditions

[0101]

[0102] Evaluate tensile properties at a test speed of 50 mm / min according to ASTM D638. Evaluate notched cantilever beam impact strength (NII) using a pendulum energy of 5 lbf / ft according to ASTM D256. Evaluate flexural properties at a test speed of 1.27 mm / min and a part thickness of 3.2 mm according to ASTM D790. Measure melt flow rate (MFR) using granular samples dried at 90°C for 4 hours according to ASTM D1238. Evaluate HDT at a stress of 1.82 MPa and a part thickness of 3.2 mm according to ASTM D648. Evaluate flame retardancy (Vx) according to UL94. Evaluate color characteristics (L*, a*, b*) using a 3.2 mm thick sample according to the CIELab color space. Evaluate spiral flowability by measuring the injection channel depth / length according to ASTM D3123.

[0103] Chemical resistance is assessed to test the accelerated failure of polymeric materials under the combined effects of environment, temperature, and stress. Failure depends primarily on the material's characteristics, the chemical substances, the exposure conditions, and the magnitude of the stress. To assess chemical resistance, test strips were exposed to sunscreen (Banana Boat® with SPF 30) for 7 days at an applied strain of 0.7%. The surface was then observed to determine the sample's chemical resistance. If the sample showed no surface change, it was rated as best performance ("normal" in the table); samples with this performance were considered "chemically resistant," as the term is used generally herein. If the surface exhibited fine cracks but no major cracks, it was rated as moderate performance. If the surface exhibited large cracks, it was rated as poor / low performance.

[0104] The compositions comprising virgin polycarbonate were prepared and tested as shown in Table 3:

[0105] Table 3 – Comparative Compositions Including Native PC

[0106]

[0107]

[0108] As can be observed from the data in Table 3, the composition of a phosphate-based flame retardant (BPADP) with a suitable loading and a polycarbonate-siloxane copolymer with a siloxane content of 40 wt% exhibits excellent thin-wall FR properties (0.75 mm or less), good elongation properties (NII strength and NII elongation) at room temperature and 0°C, and good flowability (HDT). Even at the same siloxane loading, the BPADP / EXL (20 wt% siloxane) blend cannot achieve this technical effect. Furthermore, compared to the comparative composition including EXL (20 wt% siloxane), the composition including PC-Si (40%) has improved color (L*) properties, thus offering the potential to produce white / whiter-colored articles.

[0109] Table 4 shows a comparison of the preparation and testing of post-consumer recycled polycarbonate (PCR-PC) and exemplary compositions:

[0110] Table 4 – Compositions including PCR-PC

[0111]

[0112] Comparative composition C10 comprises PCR-PC and EXL (20 wt% siloxane). Exemplary composition Ex1 comprises PCR-PC and PC-Si (40 wt% siloxane). The total siloxane content in each composition is 2.6 wt% (C10 contains 13 wt% of PC-Si containing 20 wt% siloxane, and Ex1 contains 6.5 wt% of PC-Si containing 40 wt% siloxane). The data show that when the PCR-PC loading in C10 is high, its impact resistance (NII) remains very low even with the inclusion of the EXL PC-Si copolymer. In contrast, exemplary composition Ex1, with PC-Si (40%), exhibits significantly higher impact resistance (6.5 wt% vs. 13 wt%) even at lower PC-Si loadings. Other mechanical properties of Ex1, such as HDT, tensile properties, and flexural properties, are comparable to those of C10.

[0113] The results lead to the conclusion that incorporating polycarbonate-siloxane copolymers with a high siloxane content (e.g., 40 wt%) into the polymer compositions described herein imparts good FR, impact resistance, and flowability, making them suitable for consumer electronics applications requiring high recyclability / sustainability. The above description is intended to be illustrative and not restrictive. For example, the examples described above (or one or more aspects thereof) may be used in combination with each other. Other aspects may be used as appropriate by one of ordinary skill in the art upon review of the above description. An abstract is provided to conform to 37C.FR §1.72(b), thereby allowing the reader to quickly determine the nature of the technical disclosure. The submission of the abstract should be understood not to be construed as limiting the scope or meaning of the claims. Moreover, in the detailed description above, various features may be grouped together to simplify this disclosure. This should not be construed as expecting unclaimed features to be necessary for any claim. Rather, the subject matter of the invention may comprise fewer features than all of a particular disclosed aspect. Therefore, the following claims are incorporated herein by way of example or aspect, wherein each claim exists as a separate aspect, and it is contemplated that such aspects may be combined with each other in various combinations or arrangements. The scope of this disclosure should be determined by reference to the appended claims and the full scope of the equivalent forms granted by such claims.

Claims

1. A thermoplastic composition comprising: a. A polycarbonate component of about 10 wt% to about 90 wt%; b. About 2 wt% to about 40 wt% of a polycarbonate-siloxane (PC-Si) copolymer, wherein the siloxane content of the PC-Si copolymer is at least 25 wt%; c. Approximately 2 wt% to approximately 15 wt% of bisphenol A bis(diphenyl phosphate) (BPADP) flame retardant; and d. Approximately 0.05 wt% to approximately 2 wt% of polytetrafluoroethylene (PTFE) flame retardant. The combined weight percentage of all components does not exceed 100 wt%, and all weight percentages are based on the total weight of the composition.

2. The thermoplastic composition of claim 1, wherein the polycarbonate component comprises virgin polycarbonate or mechanically recycled polycarbonate.

3. The thermoplastic composition of claim 2, wherein the polycarbonate component comprises mechanically recycled polycarbonate.

4. The thermoplastic composition according to any one of claims 1 to 3, wherein the composition comprises about 50 wt% to about 85 wt% of mechanically recycled polycarbonate.

5. The thermoplastic composition of claim 4, wherein the composition further comprises more than 0 wt% to about 20 wt% of at least one virgin polycarbonate.

6. The thermoplastic composition according to any one of claims 1 to 5, wherein the siloxane content of the PC-Si copolymer is 35 wt% to 45 wt%.

7. The thermoplastic composition according to any one of claims 1 to 6, wherein the composition comprises about 5 wt% to about 15 wt% of the BPADP flame retardant.

8. The thermoplastic composition according to any one of claims 1 to 7, wherein the composition comprises at least one additional additive.

9. The thermoplastic composition of claim 8, wherein the at least one additional additive comprises an acid remover, an anti-dripping agent, an antioxidant, an antistatic agent, a chain extender, a colorant, a release agent, a flow promoter, a lubricant, a plasticizer, a quencher, an additional flame retardant, a UV reflective additive, an impact modifier, a foaming agent, a reinforcing agent, or a combination thereof.

10. The thermoplastic composition according to any one of claims 1 to 9, wherein the composition has a V0 flame retardant rating at a thickness of 0.75 mm as assessed by UL94.

11. The thermoplastic composition according to any one of claims 1 to 10, wherein the composition has a melt flow rate of at least 15 g / 10 min, as tested according to ASTM D1238 at a temperature of 265°C and a load of 2.16 kg.

12. The thermoplastic composition according to any one of claims 1 to 11, wherein the composition comprises: The notched cantilever beam impact (NII) strength at 23°C is at least 300 joules per meter (J / m). The NII has a ductility of at least 90% at 23°C; The NII strength at 0°C is at least 300 J / m; or The NII has a ductility of at least 90% at 0°C. The NII strength and NII ductility are evaluated according to ASTM D256 at a specified temperature using a pendulum energy of 5 lbf / ft.

13. The thermoplastic composition according to any one of claims 1 to 12, wherein the composition has an L* value of at least 80, as evaluated using a sample thickness of 3.2 mm in the CIELab color space.

14. The thermoplastic composition according to any one of claims 1 to 13, wherein the composition is assessed as chemically resistant after exposure to a sunscreen with a sun protection factor (SPF) of 30 (SPF30) for 7 days at an applied strain of 0.7%.

15. An article comprising the thermoplastic composition according to any one of claims 1 to 14, wherein the article is a component of a consumer electronic device.