Materials with surface-treated coatings
By forming a surface treatment film with a specific composition on the material surface, the problems of insufficient antifouling and low-temperature drying properties of materials in the prior art under high and low temperature environments are solved, and the excellent performance of materials under these environments is achieved.
Patent Information
- Application Number
- CN202580028111.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-16
- Filing Date
- 2025-04-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing materials are difficult to simultaneously possess excellent antifouling properties and low-temperature drying properties in industrial products such as medical devices, kitchen equipment, cooking utensils, and food packaging containers under both high and low temperature environments.
By forming a surface-treated film containing organosilicon polymers and specific metal elements on the material surface, the infrared absorption spectrum shows a specific peak intensity ratio and metal element ratio, forming a film with excellent anti-fouling and low-temperature drying properties.
It achieves significant improvements in the anti-fouling properties and low-temperature drying properties of material surfaces under high and low temperature environments, and is suitable for industrial products such as medical equipment, kitchen equipment, cooking utensils and food packaging containers.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to a material having a surface-treated film, which is formed using a surface-treated agent suitable for application to components of industrial products such as medical devices, kitchen equipment, cooking utensils, and food packaging containers. Background Technology
[0002] In industrial products such as medical devices, kitchen equipment, cooking utensils, and food packaging containers, metals, resins, and fibrous materials are used in the components that make up these products. These industrial products are used in various environments, therefore the materials used in them require a variety of properties. Therefore, in order to impart various properties to these materials, techniques have been developed to apply surface treatment films with various properties to the surface of the material. For example, Patent Document 1 discloses a technique relating to a composition for surface treatment of metal materials and a treatment method thereof. The composition for surface treatment of metal materials is prepared by combining a specified phosphoric acid compound, a fluoric acid having at least four fluorine atoms and a specified element, a silane coupling agent having at least one amino group containing active hydrogen, and a silane coupling agent having at least one epoxy group in specified amounts and in a dissolved or dispersed state.
[0003] Existing technical documents
[0004] Patent documents
[0005] Patent document 1: Japanese Patent Application Publication No. 2006-213958. Summary of the Invention
[0006] The problem the invention aims to solve
[0007] In recent years, there have been increasing demands on the performance of materials used in the aforementioned components. The purpose of this invention is to provide a new material for surface treatment films that exhibits excellent anti-fouling properties and low-temperature drying characteristics.
[0008] Solution for solving the problem
[0009] In order to solve the above-mentioned problems, the inventors have repeatedly conducted in-depth research and found that the above-mentioned problems can be solved by using a surface-treated film containing a specified organosilicon polymer and a specified metal element, and whose infrared absorption spectrum shows a specified peak intensity, thereby completing the present invention.
[0010] That is, the present invention is:
[0011] [1] A material having a coating, wherein the coating is present on or on a surface,
[0012] The aforementioned coating comprises an organosilicon polymer (A) and at least one metallic element (B) selected from titanium, zirconium, and aluminum, and satisfies the following (I) and (II):
[0013] (I) The above-mentioned coating exhibits a high absorption rate at 950 cm⁻¹ in the infrared absorption spectrum. -1 ~1080cm -1 The range of peaks (α) and at 720 cm⁻¹ -1 ~830cm -1 The range of peaks (β), and the peak intensity (β) of the aforementioned peak β. A The peak intensity (α) relative to the above peak α A The ratio of (β) A / α A () is above 0.22 and below 0.72;
[0014] (II) The equivalent mass (B) of the aforementioned metal elements in the above-mentioned coating M The Si equivalent mass (A) of the aforementioned organosilicon polymer (A) M The ratio of (B) M / A M () in the range of 0.001 and 0.880;
[0015] [2] The material having a coating according to [1], wherein the material is selected from metal materials, resin materials and fiber materials;
[0016] [3] The material having a coating according to [1] or [2], wherein a base film is provided between the material and the coating, the base film comprising at least one selected from a silane coupling agent having an amino group, a polymer of the silane coupling agent and a copolymer of the polymer, and / or a phosphate.
[0017] [4] A material having a coating according to any one of [1] to [3], wherein the thickness of the coating is 0.3 μm or more and 10 μm or less; etc.
[0018] Invention Effects
[0019] According to the present invention, it is possible to provide a material with excellent antifouling properties and low-temperature drying properties for surface-treated films. Detailed Implementation
[0020] The following describes surface treatment agents, materials with surface treatment films, and methods for manufacturing them. In this specification, the numerical range indicated by "~" refers to the range including the values before and after "~" as the lower and upper limits, and "X~Y" means above X and below Y.
[0021] (Surface treatment agent)
[0022] A surface treatment agent capable of forming a film on the surface of a material to which the surface treatment film is to be formed can also be an embodiment of the present invention. The surface treatment agent of this embodiment contains an organosilicon polymer (A) and a compound containing at least one metallic element (B) selected from titanium, zirconium, and aluminum.
[0023] By using this surface treatment agent, a surface-treated film with excellent antifouling properties (especially suppressing pollution caused by plants and animals under high-temperature environments) and low-temperature drying properties can be formed on the surface of materials. Therefore, it is useful as an antifouling film forming agent. Furthermore, in this embodiment, the high-temperature environment for antifouling refers to an environment of 100°C to 200°C, and the low-temperature drying property refers to 20°C to 80°C. In addition, the surface-treated film with excellent antifouling properties and low-temperature drying properties formed by the surface treatment agent is useful for materials used in mechanical components of industrial products such as medical devices, kitchen equipment, cooking utensils, and food packaging containers.
[0024] <Organosilicon polymer (A)>
[0025] As for the silicone polymer (A), as described later, there are no particular limitations as long as it is an organosilicon polymer capable of forming a film with a specific infrared absorption spectrum absorption peak, having multiple siloxane bonds, and having an organopolysiloxane structure with organic groups bonded to silicon (Si). Preferably, it is an organosilicon polymer with an organopolysiloxane structure having at least one organic group bonded to Si in one molecule. Furthermore, there are no particular limitations on the position of the organic groups; they can be bonded to the main chain, side chain, or end. Additionally, the silicone polymer (A) can be a homopolymer having the aforementioned organopolysiloxane structure, a mixture of a homopolymer having the aforementioned organopolysiloxane structure and a homopolymer having a polysiloxane structure, or a copolymer (block copolymer or graft copolymer) having the aforementioned organopolysiloxane structure and a polysiloxane structure. Furthermore, the silicone polymer (A) can be addition-type or condensation-type. Moreover, the silicone polymer (A) can be any one of thermosetting, room temperature curing (RVT), or UV curing.
[0026] Examples of organic groups bonded to Si in the structure of organopolysiloxanes include, but are not limited to, saturated hydrocarbon groups, unsaturated hydrocarbon groups, haloalkyl groups, and epoxidecycloalkyl groups. Examples of saturated hydrocarbon groups include, for example, linear or branched alkyl groups and cycloalkyl groups. Examples of unsaturated hydrocarbon groups include, for example, linear or branched alkenyl groups, cycloalkenyl groups, cycloalkenylalkyl groups, and aryl groups.
[0027] Examples of haloalkyl groups include chloromethyl, 3-chloropropyl, 1-chloro-2-methylpropyl, and 3,3,3-trifluoropropyl. Examples of linear or branched alkyl groups include methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, sec-pentyl, neopentyl, 3-pentyl, tert-pentyl, hexyl, heptyl, octyl, nonyl, and decyl. Examples of cycloalkyl groups include cyclopentyl and cyclohexyl. Examples of linear or branched alkenyl groups include vinyl, 1-propenyl, allyl, isopropenyl, 1-butenyl, 2-butenyl, pentenyl, and hexenyl. Examples of cycloalkenyl groups include cyclopentenyl and cyclohexenyl. Examples of cycloalkenyl alkyl groups include cyclopentenylethyl, cyclohexenylethyl, and cyclohexenylpropyl. Examples of aryl groups include phenyl, tolyl, and naphthyl.
[0028] As for the polysiloxane structure, there are no particular limitations as long as it differs from the aforementioned organopolysiloxane structures. Examples include polysiloxane structures having at least two oxygen atoms bonded to Si in one molecule, and polysiloxane structures having at least two alkoxy groups bonded to Si in one molecule. Examples of alkoxy groups include methoxy, ethoxy, propoxy, and butoxy. Furthermore, the alkoxy group can be linear or branched.
[0029] In the preparation of surface treatment agents, one or more of the above-mentioned organosilicon polymers (A) may be used.
[0030] In particular, from the viewpoint of forming a film with a specific infrared absorption spectrum as described later, the organosilicon polymer (A) preferably comprises a structure having three reactive functional groups relative to one Si atom. By using such an organosilicon polymer, the infrared absorption spectrum of the formed film exhibits β... A / α A The values tend to be lower than before. This indicates that in the silicone polymer in the coating, there are fewer Si-C bonds and fewer organic groups in the side chains compared to Si-O bonds, thereby endowing the coating with suitable antifouling and low-temperature drying properties.
[0031] From the viewpoint of antifouling properties, the organic groups in the side chains that impart functionality to organosilicon polymers are preferably alkyl groups, and from the viewpoint of low-temperature drying properties, they are preferably alkoxy groups.
[0032] In the surface treatment agent of this embodiment, the content of the organosilicon polymer (A) is not particularly limited as long as it can form the desired film, preferably 5 to 20% by mass, more preferably 7 to 20% by mass, and even more preferably 15 to 20% by mass. When two or more organosilicon polymers are used in the surface treatment agent, the mass percentage of the content refers to their total content.
[0033] <Compounds containing the metallic element (B)>
[0034] The surface treatment agent of this embodiment contains a compound (hereinafter referred to as compound (B)) containing at least one metallic element (B) selected from titanium, zirconium and aluminum.
[0035] The compound containing titanium is not particularly limited as long as it contains titanium as an element, and can be any of inorganic or organic titanium compounds. Examples of inorganic titanium compounds include, but are not limited to, titanium oxysulfate, titanium oxynitrate, titanium nitrate, titanium oxychloride, titanium chloride, titanium dioxide sol, and titanium oxide. Examples of organic titanium compounds include, but are not limited to, potassium titanate oxalate, titanium lactate, tetraisopropyl titanate, tetrabutyl titanate, tetrabutyl titanate dimer, titanium acetylacetonate, diisopropoxydiacetylacetonate, and di(acetylacetonate)diisopropyl titanate. Among these, organic titanium compounds are preferred. One or more of these compounds can be used in the preparation of the surface treatment agent.
[0036] The compound containing zirconium is not particularly limited as long as it contains zirconium as an element, and can be any of inorganic zirconium compounds or organozirconium compounds. Examples of inorganic zirconium compounds include, but are not limited to, zirconium oxysulfate, zirconium oxynitrate, zirconium nitrate, zirconium oxychloride, zirconium chloride, zirconium oxide sol, and zirconium oxide. Examples of organozirconium compounds include, but are not limited to, zirconium lactate, zirconium tetraisopropoxy, zirconium acetylacetonate, zirconium n-propoxide, zirconium n-butoxide, and zirconium tetraacetylacetonate. Among these, organozirconium compounds are preferred. One or more of these compounds can be used in the preparation of the surface treatment agent.
[0037] There are no particular limitations on the type of compound containing aluminum, as long as it contains aluminum as an element; it can be any of inorganic aluminum compounds or organoaluminum compounds. Examples of inorganic aluminum compounds include, but are not limited to, aluminum sulfate, aluminum nitrate, aluminum chloride, alumina sol, and aluminum oxide. Examples of organoaluminum compounds include, but are not limited to, aluminum lactate, aluminum tetraisopropoxy, aluminum acetylacetonate, aluminum n-propoxide, aluminum n-butoxide, and aluminum tetraacetylacetonate. Among these, organoaluminum compounds are preferred. In the preparation of the surface treatment agent, one or more of these compounds may be used.
[0038] In the surface treatment agent of this embodiment, the content of compound (B) is not particularly limited as long as it can form the desired film, preferably 0.02 to 18% by mass, more preferably 0.1 to 15% by mass, and even more preferably 0.2 to 10% by mass. When two or more compounds are used in the surface treatment agent, the mass% of the content refers to their total content.
[0039] In the surface treatment agent of this embodiment, the metal elemental conversion mass (B) of the above-mentioned compound (B) is... M The Si equivalent mass (A) relative to the organosilicon polymer (A) M The ratio of (B) M / A M The value is 0.001 to 0.880, preferably 0.005 to 0.750, more preferably 0.010 to 0.487, and even more preferably 0.010 to 0.265.
[0040] Solvent
[0041] The solvent used in the surface treatment agent of this embodiment is not particularly limited and can be an organic solvent or a mixture of an organic solvent and water. Examples of organic solvents include hydrocarbon solvents, alcohol solvents, ester solvents, nitrile solvents, and ketone solvents. Examples of hydrocarbon solvents include benzene, ethylbenzene, toluene, xylene, and cyclohexane. Examples of alcohol solvents include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, 2-methyl-2-propanol, 1-pentanol, 3-methyl-1-butanol, 2,2-dimethyl-1-propanol, 2-pentanol, 3-methyl-2-butanol, 3-pentanol, 2-methyl-2-butanol, 1-hexanol, 2-hexanol, 3-hexanol, 2-methyl-1-pentanol, 3-methyl-1-pentanol, 4-hexanol, 4-hexanol, 2-methyl-1-pentanol, 3-methyl-1-pentanol, 4-hexanol, 2-hexanol, 3 ...2-hexanol, 3-hexanol, 2-methyl-1-pentanol, 4-hex Examples of ester solvents include methyl-1-pentanol, 2-methyl-2-pentanol, 3-methyl-2-pentanol, 4-methyl-2-pentanol, 2-methyl-3-pentanol, 3-methyl-3-pentanol, 2,2-dimethyl-1-butanol, 2,3-dimethyl-1-butanol, 3,3-dimethyl-1-butanol, 2,3-dimethyl-2-butanol, 3,3-dimethyl-2-butanol, and 2-ethyl-1-butanol. Examples of ester solvents include methyl acetate, ethyl acetate, butyl acetate, and 2-ethoxyethyl acetate. Examples of nitrile solvents include acetonitrile. Examples of ketone solvents include acetone, methyl ethyl ketone, and methyl isobutyl ketone, but these are not limited to these. Furthermore, one or more organic solvents may be used. Additionally, alcohols with 1 to 5 carbon atoms are preferred as alcohol solvents.
[0042] The moisture concentration of the surface treatment agent is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 1% by mass or less, and even more preferably substantially water-free. By setting such a moisture content, the surface treatment agent exhibits excellent stability. Furthermore, the moisture concentration of the surface treatment agent can be measured using, for example, an MKV-710 manufactured by Kyoto Electronics Industry Co., Ltd.
[0043] In this embodiment, when the surface treatment agent contains an alcohol-based solvent as a solvent, the content of the alcohol-based solvent is preferably 65-85% by mass relative to the surface treatment agent, more preferably 70-85% by mass, and even more preferably 75-85% by mass.
[0044] In the surface treatment agent of this embodiment, the concentration of fluoride ions is preferably 1% by mass or less, more preferably 0.5% by mass or less, and even more preferably substantially non-existent. Furthermore, the concentration of fluoride ions can be determined, for example, by using a Primus IV filter manufactured by Rigaku Corporation, through the drop filter paper method, by comparing the fluorescence X-ray intensity of each element with a known standard curve.
[0045] <Other Additives>
[0046] The surface treatment agent of this embodiment may contain various additives as needed. Examples of additives include, but are not limited to, surfactants, defoamers, leveling agents, thickeners, antibacterial and antifungal agents, and colorants. By adding these additives to the surface treatment agent, the storage and drying properties of the surface treatment agent can be improved, or the operability in manufacturing a surface-treated film using the surface treatment agent can be improved, or the appearance (especially the design) of the manufactured surface-treated film can be improved. These additives can be added within a range that does not impair the effects of the present invention, and the content of the additives relative to the mass of the surface treatment agent is at most a fractional mass.
[0047] (Manufacturing method of surface treatment agent)
[0048] The method for manufacturing the surface treatment agent in this embodiment is not particularly limited, and it can be manufactured by mixing an organosilicon polymer (A), a compound containing at least one metal element (B) selected from titanium, zirconium and aluminum, a solvent, additives, etc.
[0049] <Surface Treatment Coating>
[0050] The surface-treated film of this embodiment exhibits a high infrared absorption spectrum at 950 cm⁻¹. -1 ~1060cm -1 The range of peaks (α) and at 720 cm⁻¹ -1 ~830cm -1 The range of peaks (β), the absorbance of the aforementioned peak β (β)A The absorbance relative to the above peak α (α) A The ratio of (β) A / α A The value is 0.22 to 0.72, preferably 0.30 to 0.62, more preferably 0.30 to 0.55, and even more preferably 0.30 to 0.45.
[0051] Peak α indicates, for example, the presence of Si-O stretching vibrations. Furthermore, peak β indicates, for example, the presence of Si-C stretching vibrations.
[0052] The infrared absorption spectrum of a surface-treated film can be measured using reflectance spectroscopy, a type of infrared spectroscopy. Examples of suitable equipment include, for instance, the FT-IR (Spectrum Two) instrument manufactured by Perkin Elmer.
[0053] In addition, the surface-treated film contains an organosilicon polymer (A) and a metal element (B), and the calculus of the metal element (B) is (BA). M The Si equivalent mass (A) relative to the organosilicon polymer (A) M The ratio of (B) M / A M The value is in the range of 0.001 to 0.880. Preferably, it is in the range of 0.005 to 0.750, more preferably in the range of 0.010 to 0.487, and even more preferably in the range of 0.010 to 0.265.
[0054] By (β) A / α A ) and (B M / A M By setting the parameters within the above range, a film with excellent antifouling properties and low-temperature drying properties can be produced.
[0055] (Materials with surface-treated coatings and their manufacturing methods)
[0056] The method for manufacturing a material having a surface-treated film according to this embodiment includes: a contact step in which the surface-treated agent comes into contact with the surface of the material or the surface of the material; and a drying step in which the surface-treated agent in contact with the material is dried to form a surface-treated film. By performing these steps, a material having a surface-treated film can be manufactured.
[0057] Before performing the above-mentioned contact process, the material can be pretreated to remove oil and dirt adhering to its surface. There are no particular limitations on the pretreatment method; examples include hot water washing, solvent cleaning, and alkaline degreasing cleaning.
[0058] As a method for contacting the surface treatment agent in the above-mentioned contact process, various contact methods can be used, and the optimal method is preferably selected according to the shape of the material being treated. Specifically, methods such as immersion treatment, spray treatment, flow coating, brush coating, roller coating, and bar coating can be used, but are not limited to these methods. In addition, one or more coating devices such as spin coaters, slot coaters, die coaters, doctor blade coaters, and dispensing machines can also be used for coating.
[0059] The drying temperature (ambient temperature) in the above-mentioned drying process is not particularly limited and can be above 20℃, above 30℃, above 50℃, below 250℃, below 180℃, below 100℃, or below 80℃. That is, the drying temperature in the drying process can be 20℃~250℃, 30℃~180℃, 50℃~180℃, 50℃~100℃, or 50℃~80℃. The drying method is not particularly limited and can include: natural drying at room temperature and pressure; or drying the surface treatment agent by heating it with hot air, induction heaters, infrared rays, or near-infrared rays. Furthermore, the drying time is not particularly limited; the most suitable conditions can be set appropriately according to the type of material used, the surface of the material, and the amount of surface treatment agent adhering to the surface.
[0060] The method for manufacturing a material having a surface-treated film according to this embodiment may further include, before the step of contacting the surface-treated agent (or after the pretreatment in the case of pretreatment): a step of contacting a substrate treatment agent with the surface of the material or the surface thereof, wherein the substrate treatment agent comprises at least one selected from a silane coupling agent having an amino group, a polymer of the silane coupling agent, and a copolymer of the polymer, and / or phosphoric acid; and a step of washing the substrate treatment agent in contact with the material with water or without washing and drying it to form a substrate film. By performing the surface-treated agent contact step and the drying step after performing these steps, it is possible to manufacture a material having a surface-treated film and a substrate film.
[0061] The substrate treatment agent comprises at least one selected from the group consisting of an amino-containing silane coupling agent, a polymer of the silane coupling agent, and a copolymer of the polymer, and / or phosphate ions. As an amino-containing silane coupling agent, there is no particular limitation as long as it has one or more amino groups; examples include 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane. Furthermore, there is no particular limitation on the phosphate ion supply source; examples include manganese phosphate, iron phosphate, zinc phosphate, zinc calcium phosphate, and phosphoric acid, among which manganese phosphate is preferred.
[0062] The solvent contained in the substrate treatment agent is not particularly limited, and examples of solvents include: alcohols, acetone, acetonitrile, benzene, cyclohexane, methyl acetate, ethyl acetate, methyl ethyl ketone, and other organic solvents; mixtures of these organic solvents with water; etc. Alcohols with 5 or fewer carbon atoms are preferred as organic solvents. Furthermore, the mass percentage of water contained in the substrate treatment agent is preferably less than 5% by mass. In addition, the substrate treatment agent may contain: leveling agents to improve wettability to metallic materials, film-forming aids to improve film-forming properties, organic crosslinking agents and inorganic crosslinking agents to make the substrate film a more robust coating, defoamers to inhibit foaming, thickeners to control viscosity, rust inhibitors, and other additives; these additives can be combined within a range that does not impair the effects of the present invention.
[0063] Various contact methods can be used as the contact method for the substrate treatment agent, and the optimal method is preferably selected appropriately according to the shape of the metal material being treated. Specifically, in addition to the coating method using the coating apparatus described above, methods such as dip coating, spray coating, flow coating, roller coating, bar coating, and electrolytic deposition can be cited, but are not limited to these methods.
[0064] Examples of drying methods after contact with the substrate treatment agent include heating and drying using hot air, induction heaters, infrared radiation, near-infrared radiation, etc., and drying by vacuum distillation, but are not limited to these. The temperature during heating and drying is not particularly limited, but is preferably in the range of 20°C to 250°C (ambient temperature), more preferably in the range of 30°C to 180°C (ambient temperature). Furthermore, the heating time is not particularly limited; the most suitable conditions can be appropriately set according to the type of material used and the amount of substrate treatment agent adhering to the surface of the metal material.
[0065] <Materials>
[0066] The material used to form the film on the surface is not particularly limited, but metallic materials, resin materials, and fiber materials are preferred. Examples of metallic materials include, but are not limited to, ferrous metals, zinc-based metals, aluminum-based metals, magnesium-based metals, nickel-based metals, titanium-based metals, zirconium-based metals, copper-based metals, tin-based metals, tungsten-based metals, chromium-based metals, manganese-based metals, molybdenum-based metals, and cobalt-based metals. In this invention, ferrous metals are preferred, and stainless steel is more preferred. Although metallic materials are described below as examples of materials to which the surface treatment agent is applied, the materials to which the surface treatment agent of this embodiment is applied are not limited to metallic materials; any material that requires an antifouling film can be used.
[0067] Furthermore, the material having a surface-treated coating in this embodiment may also have a base film between the material and the surface-treated coating. This base film comprises at least one selected from: an amino-containing silane coupling agent, a polymer of the silane coupling agent, and a copolymer of the polymer, and / or a phosphate. Additionally, when the above-mentioned additive is incorporated into the substrate treatment agent forming the base film, the base film may also contain the additive.
[0068] The material having the surface-treated film described above can be manufactured using the above-described manufacturing method. The thickness of the surface-treated film is not particularly limited, but is preferably 0.3 μm to 10 μm on each side, more preferably 0.5 μm to 5 μm. Furthermore, the thickness of the substrate film is not particularly limited, but is preferably 0.5 μm to 15 μm on each side.
[0069] The aforementioned metal materials with surface-treated coatings exhibit excellent anti-fouling properties, making them suitable for industrial products such as medical equipment, kitchen equipment, cooking utensils, and food packaging containers.
[0070] Example
[0071] The effects of the present invention are illustrated below through specific examples. However, the following examples do not limit the scope of the present invention.
[0072] Test materials (materials)
[0073] The following commercially available materials were used as test materials.
[0074] (M1) Stainless steel plate SUS304: plate thickness 0.8mm;
[0075] (M2) Cold-rolled steel sheet SPCC-SD: 0.8mm thick;
[0076] (M3) Aluminum plate A1050P: Plate thickness 0.8mm;
[0077] (M4) Copper plate C1020P: Plate thickness 0.8mm.
[0078] Pretreatment (alkaline degreasing and cleaning)
[0079] The surfaces of various test materials were degreased by immersing them in a 2% aqueous solution of an alkaline degreasing agent (Fine Cleaner E6406 manufactured by Pakase Sei Co., Ltd., Japan) at 60°C for 30 seconds to remove oil and dirt from the surfaces. Next, the materials were washed with tap water, then rinsed with pure water, and finally dried at 100°C.
[0080] Preparation of surface treatment agents
[0081] Surface treatment agents X1 to X30 were prepared by mixing the components shown in Table 1 in the prescribed mass ratios. In Table 1, the mass percentages for "organosilicon polymer (A)," "compound containing metal element (B)," and "solvent" represent the proportion of each component's mass relative to their total mass. Furthermore, the mass percentage of organosilicon polymer (A) in Table 1 is not the mass of the product, but rather the mass of the organosilicon polymer. The types of components shown in Table 1 are listed in Tables 2 to 4.
[0082] [Table 1]
[0083]
[0084] [Table 2]
[0085]
[0086] [Table 3]
[0087]
[0088] [Table 4]
[0089]
[0090] Materials with surface-treated coatings
[0091] The various surface treatment agents shown in Table 5 were brought into contact with the surfaces of the various test materials that had undergone pretreatment (alkali degreasing and cleaning). Then, without washing with water, the surface treatment agents in contact with the test materials were dried at the drying temperatures shown in Table 5 to prepare the test materials (test plates) of Examples 1 to 38 and Comparative Examples 1 to 5 with surface treatment films having specified film thicknesses.
[0092] In addition, the substrate treatment (Y) in Table 5 is performed in the following manner.
[0093] Various test materials were immersed for 30 seconds in a surface treatment modifier for manganese phosphate treatment (PREPALENE55 manufactured by PARCASE Co., Ltd., Japan) diluted with tap water to a concentration of 0.3% by mass. Next, a manganese phosphate-based surface treatment reagent (PARPHOS M1A manufactured by PARCASE Co., Ltd., Japan) was diluted with tap water to a concentration of 14% by mass. The total acidity was adjusted to 50, the free acidity to 8.6, the acid ratio (total acidity / free acidity) to 5.8, and the iron concentration to 1.5 g / L. The surface-treated iron-based metal materials were then immersed for 900 seconds in a chemical conversion treatment agent heated to 97°C. Afterward, the materials were washed with tap water, then rinsed with pure water, and the surface of the test materials was dried at 100°C (ambient temperature) for 10 minutes to form a base film (thickness = 3 μm) mainly composed of manganese phosphate and ferric manganese phosphate.
[0094] [Table 5]
[0095]
[0096] membrane analysis
[0097] The positions and absorbance of the peaks in the infrared absorption spectrum of the organosilicon polymer (A) in the dried coating were analyzed by infrared spectroscopy. Similarly, the equivalent metal mass (B) of at least one metal element selected from titanium, zirconium, and aluminum was determined by fluorescence X-ray spectrophotometry. M The Si equivalent mass (A) relative to the organosilicon polymer (A) M The ratio of (B) M / A M ).
[0098] Fluorescence X-ray Spectrophotometry (B) M / A M )>
[0099] Analysis was performed using fluorescence X-ray spectrophotometry. The apparatus used was a Primus IV manufactured by Rigaku Corporation. Quantitative analysis was performed by comparing the fluorescence X-ray intensity of each element with a known standard curve. The converted mass (A) was obtained by subtracting the quantitative analysis result of the test material before surface treatment from the obtained quantitative analysis result. M Or B M Find B. M / A M The obtained values are shown in Table 6.
[0100] Fourier transform infrared spectroscopy (β) A / α A )>
[0101] The analysis was performed using the reflectance method, a type of infrared spectroscopy. A Perkin Elmer FT-IR (Spectrum Two) instrument was used, with the sample surface pressed against the measurement site. After measurement, automatic baseline correction was performed using software. In this study, the absorbance of the aforementioned peak β (β0) was... A The absorbance relative to the above peak α (α) A The ratio of (β) A / α A The value is the average of three measurements. The obtained values are shown in Table 6.
[0102] Evaluation test
[0103] The following evaluation tests were performed on the test plates of Examples 1-38 and Comparative Examples 1-5. The results of each evaluation test are shown in Table 6. In addition, from a practical point of view, test plates that do not have a "D" in any of the evaluation items shown in Table 6 are judged as qualified.
[0104] <Protection against blood contamination>
[0105] Five drops (1 drop: approximately 50 μL) of pig blood (Tokyo Shibaura Organs Co., Ltd.) were added to various test plates and forced to dry in a hot air drying oven at 200°C for 3 minutes to fix it onto the test plate surface. After cooling to room temperature, a 2.5 kg load was placed on a 1.2 cm diameter gauze, and the blood adhering to the coating was wiped back and forth only 5 times. The gauze was replaced after each drop was wiped. For each drop, the ratio of the area of residual blood after wiping to the area of blood after drying and fixing was evaluated according to the following criteria. The average value of the evaluation after excluding the best and worst evaluations of the 5 drops is shown in Table 6. It can be understood that the antifouling performance of the test pieces in the examples is excellent even at a high temperature of 200°C. On the other hand, the antifouling performance of the test pieces in the comparative examples is significantly worse.
[0106] AA: Residual rate less than 5%;
[0107] A: The residue rate is 5% or higher but less than 15%;
[0108] B: The residue rate is 15% or higher but less than 30%;
[0109] C: The residue rate is above 30% and less than 45%;
[0110] D: The residual rate is 45% or more, or there is film peeling.
[0111] <Film-forming properties>
[0112] The hardness of various test pieces was measured according to JIS K 5600-5-4:1999. The test results were evaluated according to the following standards, and the results are shown in Table 6. It can be understood that in the test pieces of the examples, a film was formed even at drying temperatures of 20°C and 30°C. On the other hand, in the comparative examples, there were test pieces that did not form a film even at a drying temperature of 80°C.
[0113] AA: The coating hardness is 4H or higher;
[0114] A: The coating hardness is less than 4H and greater than H;
[0115] B: The coating hardness is less than H and greater than 2B;
[0116] C: The hardness of the coating is less than 2B and a coating has formed;
[0117] D: No film formed.
[0118] [Table 6]
[0119]
[0120] Furthermore, although the present invention has been described in detail with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention.
[0121] According to the present invention, a material with a coating that not only has excellent antifouling properties but also excellent low-temperature drying properties can be obtained, thereby reducing the energy required to dry the coating, which is an invention that contributes to the SDGs (Sustainable Development Goals).
Claims
1. A material having a coating, wherein the coating is present on or on a surface, The coating comprises an organosilicon polymer (A) and at least one metallic element (B) selected from titanium, zirconium, and aluminum, and satisfies the following (I) and (II): (I) The coating exhibits an infrared absorption spectrum with a wavelength at 950 cm⁻¹. -1 ~1080cm -1 The range of peaks (α) and at 720 cm⁻¹ -1 ~830cm -1 The range of peaks (β), and the peak intensity (β) of said peak β. A The peak intensity (α) relative to the peak α A The ratio of (β) A / α A The value ranges from 0.22 to 0.
72. (II) The equivalent mass (B) of the metal element (B) in the film M The Si equivalent mass (A) relative to the organosilicon polymer (A) M The ratio of (B) M / A M It is in the range of 0.001 to 0.
880.
2. The material with a coating according to claim 1, wherein, The material is selected from metal materials, resin materials, and fiber materials.
3. The material with a coating according to claim 1 or 2, wherein, A base film is provided between the material and the coating. The substrate membrane comprises at least one selected from the group consisting of an amino-containing silane coupling agent, a polymer of the silane coupling agent, and a copolymer of the polymer, and / or a phosphate.
4. The material with a coating according to claim 1 or 2, wherein, The thickness of the coating is greater than 0.3 μm and less than 10 μm.
Citation Information
Patent Citations