Interference Filter and its Manufacturing Method
By using a silver-doped metal layer in the automatic dimming filter, the challenges of metal layer uniformity and thinness were solved, improving optical performance and infrared radiation attenuation, and enabling a more efficient manufacturing process.
Patent Information
- Application Number
- CN202580029492.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-22
- Filing Date
- 2025-04-17
- Publication Date
- 2026-11-17
AI Technical Summary
The metal layer in existing automatic dimming filters is difficult to achieve a uniform and thin interference filter, which affects its optical performance and attenuation effect on infrared, blue and ultraviolet radiation.
A metal layer made of silver-doped material is alternately deposited on a dielectric layer using physical vapor deposition to form a metal layer with a thickness of less than 40 nanometers and discrete clusters and voids, ensuring uniformity and thinness, with an average maximum cluster size of less than 70 nm and a total void area of less than 1% of the stacked area.
The optical performance of the interference filter was improved, light transmittance was increased, light scattering was reduced, and the attenuation effect on near-infrared radiation was enhanced, while the deposition rate and manufacturing efficiency were also improved.
Smart Images

Figure CN123125520A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates in its entirety to an interference filter for an automatic dimming filter and a method for manufacturing the interference filter. Background Technology
[0002] Automatic dimming filters are typically mounted on protective helmets to provide protection against high-intensity light. Automatic dimming filters generally include switchable filters and interference filters. Interference filters may comprise multiple dielectric layers and multiple metal layers alternating with the dielectric layers. Interference filters attenuate infrared, blue, and ultraviolet radiation. For the desired performance of the interference filter, each of the multiple metal layers may need to be uniform and thin (e.g., less than 15 nanometers thick). However, producing uniform and thin metal layers can be challenging. Summary of the Invention
[0003] In a first aspect, this disclosure provides an interference filter for an automatic dimming filter. The interference filter includes an optically transparent substrate. The interference filter also includes an optical stack disposed on the substrate. The optical stack includes a plurality of first layers and a plurality of second layers alternating with the plurality of first layers. The optical stack defines a plane and a total stack area in the plane of the optical stack. Each of the plurality of first layers is dielectric. Each of the plurality of second layers is metallic. Each second layer defines a thickness perpendicular to the plane. The thickness of each second layer is less than 40 nanometers (nm). Each second layer includes a plurality of discrete clusters extending along the thickness of the second layer in the plane of the optical stack. The plurality of discrete clusters are spaced apart from each other such that each second layer also includes a plurality of voids extending through the thickness of the second layer and having a total void area in the plane of the optical stack. The average maximum cluster size of the plurality of discrete clusters in each second layer, measured along the plane of the optical stack, is less than 70 nm. The total void area of each second layer is less than 1% of the total stack area of the optical stack.
[0004] In a second aspect, this disclosure provides an automatic dimming filter. The automatic dimming filter includes a switchable filter that changes from a bright transmission state to a dark transmission state in response to an activation signal. The automatic dimming filter also includes an interference filter as described in the first aspect. The interference filter is disposed on the switchable filter.
[0005] In a third aspect, this disclosure provides a protective helmet. The protective helmet includes the automatic dimming filter of the second aspect.
[0006] In a fourth aspect, this disclosure provides a method for manufacturing an interference filter for an automatic dimming filter. The method includes providing an optically transparent substrate. The method further includes forming an optical stack on the substrate by depositing a plurality of second layers on a plurality of first layers, such that the plurality of second layers alternate with the plurality of first layers to form the optical stack on the substrate.
[0007] The optical stack defines a plane and a total stack area in the plane of the optical stack. Each of the plurality of first layers is dielectric. Each of the plurality of second layers is metallic. Each second layer defines a thickness perpendicular to the plane. The thickness of each second layer is less than 40 nanometers (nm). Each second layer includes a plurality of discrete clusters extending along the thickness of the second layer in the plane of the optical stack. The plurality of discrete clusters are spaced apart from each other such that each second layer also includes a plurality of voids extending through the thickness of the second layer and having a total void area in the plane of the optical stack. The average maximum cluster size of the plurality of discrete clusters in each second layer, measured along the plane of the optical stack, is less than 70 nm. The total void area of each second layer is less than 1% of the total stack area of the optical stack.
[0008] Details of one or more examples of this disclosure are set forth in the accompanying drawings and the following description. Other features, objects, and advantages of this disclosure will become apparent from the description, the drawings, and the claims. Attached Figure Description
[0009] A more complete understanding of the exemplary embodiments disclosed herein will be gained from the following detailed description in conjunction with the figures below. The figures are not necessarily drawn to scale. Similar numbers used in the figures refer to similar parts. However, it should be understood that the use of numbers to refer to parts in a given figure is not intended to limit parts labeled with the same numbers in another figure.
[0010] Figure 1 This is a schematic cross-sectional view of an interference filter for an automatic dimming filter according to one embodiment of the present disclosure;
[0011] Figure 2A It is based on one implementation scheme of this disclosure. Figure 1 A schematic top view of the separate second layer of the interference filter;
[0012] Figure 2B It is based on one implementation scheme of this disclosure. Figure 1 The interference filter is depicted with schematic partial cross-sectional views of the individual first layer and the adjacent second layer;
[0013] Figure 3 This is a schematic exploded perspective view of an automatic darkening filter according to one embodiment of the present disclosure;
[0014] Figure 4It includes one embodiment of this disclosure. Figure 3 A schematic perspective view of a protective face shield with an automatic dimming filter;
[0015] Figure 5 It is a flowchart depicting various steps of a method for manufacturing an interference filter according to one embodiment of the present disclosure;
[0016] Figure 6A This is a photograph of the first sample produced by depositing pure silver on a substrate layer;
[0017] Figure 6B This is a photograph of the second sample produced by depositing copper-doped silver on a substrate layer;
[0018] Figure 7A An example is obtained using a scanning electron microscope. Figure 6A The SEM image of the first sample;
[0019] Figure 7B An example is obtained using a scanning electron microscope. Figure 6B The SEM image of the second sample;
[0020] Figure 8 It is a graph depicting the relationship between the transmittance and wavelength of various first and second samples.
[0021] Figure 9 It is a graph depicting the relationship between visible transmittance and deposition rate;
[0022] Figure 10A It is a graph depicting the relationship between the transmittance and wavelength of various first samples after heat treatment; and
[0023] Figure 10B It is a graph depicting the relationship between the transmittance and wavelength of various second samples after heat treatment. Detailed Implementation
[0024] In the following description, reference is made to the accompanying drawings, which form a part thereof, and various embodiments are illustrated therein. It should be understood that other embodiments may be conceived and made without departing from the scope or spirit of this disclosure. Therefore, the following detailed description should not be considered limiting.
[0025] In the following disclosure, the following definitions are used.
[0026] As used herein, “a,” “an,” “the,” “at least one,” and “one or more” are used interchangeably.
[0027] As used herein, as a modifier of a characteristic or attribute, unless otherwise specifically defined, the term “approximately” means that the characteristic or attribute will be easily identifiable by a person skilled in the art without requiring absolute precision or a perfect match (e.g., within + / - 20% for quantifiable characteristics).
[0028] Unless otherwise specifically defined, the term “substantially” means a high degree of approximation (e.g., within + / -10% for quantifiable properties), but also does not require absolute precision or a perfect match.
[0029] As used in this article, all figures should be considered as being modified by the term “approximately”. Unless otherwise specifically defined, the term “approximately” means a high degree of approximation (e.g., within + / -5% for quantifiable properties), but also does not require absolute precision or a perfect match.
[0030] As used herein, the terms “first” and “second” are used as identifiers. Therefore, such terms should not be construed as limiting the scope of this disclosure. Throughout the embodiments of this disclosure, the terms “first” and “second” are used interchangeably when used in conjunction with a feature or element.
[0031] As used herein, when a first material is referred to as “similar” to a second material, at least 90% by weight of the first material and the second material are identical, and any variation between the first material and the second material accounts for less than about 10% by weight of each of the first material and the second material. As used herein, “at least one of A and B” should be understood to mean “only A, only B, or both A and B”.
[0032] As used herein, the term “transmittance” broadly refers to the percentage of energy in a given region of the electromagnetic spectrum transmitted across a surface (e.g., the visible range, the infrared range, or any other range).
[0033] As used herein, the term "optically transparent" refers to the ability of light to pass through a material. Optically transparent elements have high light transmittance (e.g., greater than 80%) over at least a portion of the visible spectrum (from about 400 nm to about 700 nm).
[0034] As used herein, the terms “light transmittance” and “visual transmittance” refer to the weighted average of transmittance over the visible wavelength range (i.e., from about 380 nm to about 780 nm).
[0035] As used herein, the term "dielectric" refers to a non-metallic and non-conductive material. A dielectric layer is made of one or more dielectric materials.
[0036] As used herein, the term "refractive index" refers broadly to the absolute refractive index of a material, that is, it should be understood as the ratio of the velocity of electromagnetic radiation in free space to the velocity of electromagnetic radiation in that material. This refractive index can be measured using known methods and is typically measured in the visible light region using an Abbe refractometer.
[0037] As used herein, unless otherwise specifically defined, the term "between about..." generally refers to a range of inclusion or closure. For example, if parameter X is between about A and B, then A ≤ X ≤ B.
[0038] This disclosure relates to an interference filter for an automatic dimming filter. The interference filter includes an optically transparent substrate. The interference filter also includes an optical stack disposed on the substrate. The optical stack includes a plurality of first layers and a plurality of second layers alternating with the plurality of first layers. The optical stack defines a plane and a total stack area in the plane of the optical stack. Each of the plurality of first layers is dielectric. Each of the plurality of second layers is metallic. Each second layer defines a thickness perpendicular to the plane. The thickness of each second layer is less than 40 nanometers (nm). Each second layer includes a plurality of discrete clusters extending along the thickness of the second layer in the plane of the optical stack. The plurality of discrete clusters are spaced apart from each other such that each second layer also includes a plurality of voids extending through the thickness of the second layer and having a total void area in the plane of the optical stack. The average maximum cluster size of the plurality of discrete clusters of each second layer, measured along the plane of the optical stack, is less than 70 nm. The total void area of each second layer is less than 1% of the total stack area of the optical stack.
[0039] Each second layer, having an average maximum cluster size of less than 70 nm and a total void area of less than 1% of the total stack area, can be highly uniform (i.e., having a substantially uniform thickness with reduced defects such as discrete clusters and void area). The high uniformity of each second layer improves the optical performance of the interference filter (i.e., improved light transmittance, reduced light scattering, and improved near-infrared radiation attenuation).
[0040] In some examples, each second layer may be made of silver doped (i.e., silver and a dopant). The dopant may contain copper (Cu), aluminum (Al), zinc (Zn), silicon carbide (SiC), or a combination thereof.
[0041] Fabricating each second layer with silver doping improves its uniformity. Specifically, fabricating each second layer with silver doping reduces both the average maximum cluster size of the multiple discrete clusters and the total void area of the multiple voids in the second layer. As discussed above, the high uniformity of each second layer improves the optical performance of the interference filter.
[0042] Furthermore, fabricating each second layer with silver doping allows for a reduction in the second layer's thickness while maintaining high uniformity. For example, the thickness of each second layer can range from 6 nm to 12 nm. Therefore, silver doping allows for the formation of ultrathin and uniform second layers.
[0043] Furthermore, compared to pure silver, a mixture of silver and dopant can be deposited at a higher deposition rate without compromising the uniformity of the resulting second layer. Therefore, a mixture of silver and dopant offers greater flexibility in deposition rate compared to pure silver, and in some cases, can accelerate the fabrication of interference filters.
[0044] Now refer to the attached diagram, Figure 1 A schematic cross-sectional view of an interference filter 100 for an automatic darkening filter according to one embodiment of the present disclosure is shown. Figure 1 The interference filter 100 shown may alternatively be referred to as an "inductive transmission filter".
[0045] The interference filter 100 includes an optically transparent substrate 102. In some embodiments, the substrate 102 comprises glass or alumina (Al2O3). In some embodiments, depending on the desired application properties, the substrate 102 may comprise soda-lime glass, borosilicate glass, aluminosilicate glass, or any other suitable glass. Depending on the desired application properties, the substrate 102 may have any suitable thickness.
[0046] The interference filter 100 also includes an optical stack 104 disposed on the substrate 102. The optical stack 104 defines a plane 110 (by...). Figure 1 (The lines in the diagram are schematically depicted) and the total stacked area in plane 110 of optical stack 104. Optical stack 104 includes a plurality of first layers 106 and a plurality of second layers 108 alternating with the plurality of first layers 106.
[0047] Each of the plurality of first layers 106 is dielectric. In some embodiments, each first layer 106 comprises silicon dioxide (SiO2), titanium dioxide (TiO2), tantalum pentoxide (Ta2O5), aluminum oxide (Al2O3), hafnium oxide (HfO2), zinc sulfide (ZnS), or combinations thereof.
[0048] Each first layer 106 may define a thickness 106T perpendicular to the plane 110. The thickness 106T of each first layer 106 may be selected based on desired application properties. The thickness 106T of the plurality of first layers 106 may be the same or different. Furthermore, the plurality of first layers 106 may have the same or different refractive indices. In some embodiments, one or more of the plurality of first layers 106 may be multilayered. In other words, in some embodiments, one or more first layers 106 may consist of a plurality of dielectric layers.
[0049] Each of the plurality of second layers 108 is metallic. Each second layer 108 defines a thickness 108T perpendicular to the plane 110. The thickness 108T of each second layer 108 is less than 40 nanometers (nm).
[0050] Figure 2A A schematic top view of a single second layer 108 among a plurality of second layers 108 according to one embodiment of the present disclosure is shown. Figure 2B An embodiment according to this disclosure is illustrated. Figure 1 The interference filter 100 is depicted in a schematic partial cross-sectional view of a single second layer 108 and a first layer 106 adjacent to the second layer 108. Optical stack 104 ( Figure 1 Plane 110 (as shown in the diagram) is also... Figure 2A and Figure 2B Described in the text.
[0051] refer to Figure 1 , Figure 2A and Figure 2B Each second layer 108 comprises a plurality of discrete clusters 112 extending along the thickness 108T of the second layer 108 on the plane 110 of the optical stack 104. Figure 2A (Schematally depicted as circles). Each of the plurality of discrete clusters 112 may include a maximum cluster size 112L in plane 110 of optical stack 104. The plurality of discrete clusters 112 in each second layer 108 may define an average maximum cluster size. The average maximum cluster size may be the mean or average of the maximum cluster sizes 112L of the plurality of discrete clusters 112 in the respective second layer 108.
[0052] Multiple discrete clusters 112 are spaced apart from each other, such that each second layer 108 also includes multiple gaps 114 (in Figure 2A (Schematably depicted as a dashed ellipse), the plurality of voids extend through the thickness 108T of the second layer 108 and have a total void area in the plane 110 of the optical stack 104. The total void area can be the sum of the areas of the plurality of voids 114 of the corresponding second layer 108 in plane 110. In other words, the total void area of each second layer 108 can be the sum of the areas of the plurality of voids 114 of the second layer 108. The total void area can correspond to the area of the adjacent first layer 106 that is not covered by the second layer 108. The average maximum cluster size and the total void area can be determined using scanning electron microscopy (SEM).
[0053] The average maximum cluster size of the plurality of discrete clusters 112 in each second layer 108, measured along plane 110 of optical stack 104, is less than 70 nm. Furthermore, the total void area of each second layer 108 is less than 1% of the total stack area of optical stack 104.
[0054] Each second layer 108, having an average maximum cluster size of less than 70 nm and a total void area of less than 1% of the total stack area, can be highly uniform (i.e., having a substantially uniform thickness with reduced defects such as discrete clusters and void areas). The high uniformity of each second layer 108 improves the optical performance of the interference filter 100 (i.e., improved light transmittance, reduced light scattering, and improved near-infrared radiation attenuation).
[0055] In some embodiments, each second layer 108 contains 95% to 99.5% silver by weight. Each second layer 108 also contains 0.5% to 5% dopant by weight. In some embodiments, the dopant contains copper (Cu), aluminum (Al), zinc (Zn), silicon carbide (SiC), or combinations thereof.
[0056] The aforementioned composition of silver and a dopant (also referred to herein as "doped silver") is used to fabricate each second layer 108, thereby improving the uniformity of the second layer 108. Specifically, fabricating each second layer 108 with doped silver reduces both the average maximum cluster size of the plurality of discrete clusters 112 and the total void area of the plurality of voids 114 in the second layer 108. As discussed above, the high uniformity of each second layer 108 improves the optical performance of the interference filter 100.
[0057] Furthermore, fabricating each second layer 108 with silver doping allows for a reduction in the thickness 108T of the second layer 108 while maintaining high uniformity. In some embodiments, the thickness 108T of each second layer 108 can be less than 12 nm. In some embodiments, the thickness 108T of each second layer 108 can be in the range of 6 nm to 12 nm. Silver doping thus allows for the formation of ultrathin and uniform second layers 108. In some embodiments, the average maximum cluster size can be from 48 nm to 68 nm.
[0058] In some implementations, the total void area of each second layer 108 may be less than 0.1% of the total stack area of the optical stack 104, such that the second layer 108 substantially covers adjacent first layers 106 among the plurality of first layers 106. This configuration of the plurality of second layers 108 may also improve the optical characteristics of the interference filter 100.
[0059] In some embodiments, the interference filter 100 may further include a dielectric stack (not shown). In some embodiments, the dielectric stack may be disposed on an optical stack 104 such that the optical stack 104 is disposed between the dielectric stack and the substrate 102. In some other embodiments, the dielectric stack may be disposed between the optical stack 104 and the substrate 102. In some other embodiments, the dielectric stack may be disposed between two layers of the optical stack 104. The dielectric stack may include multiple dielectric layers stacked on top of each other. The multiple dielectric layers may have the same or different refractive indices. In some cases, alternating dielectric layers from the multiple dielectric layers may have alternating high and low refractive indices. For example, a first dielectric layer from the multiple dielectric layers may have a high refractive index, and a second dielectric layer adjacent to the first dielectric layer may have a low refractive index. Therefore, the interference filter 100 may employ a combination of dielectric stack and optical stack 104 based on desired application properties.
[0060] Interference filter 100 can be configured to attenuate infrared (IR), blue, and ultraviolet (UV) wavelength components from high-intensity light. In some embodiments, interference filter 100 can eliminate harmful IR, blue, and UV wavelength components from high-intensity light.
[0061] Figure 3 A schematic exploded perspective view of an automatic darkening filter 10 according to one embodiment of the present disclosure is shown.
[0062] The auto-darkening filter 10 includes a switchable filter 40 that changes from a bright transmission state to a dark transmission state in response to an activation signal. The auto-darkening filter 10 also includes an interference filter 100. The interference filter 100 is disposed on the switchable filter 40. In some embodiments, the interference filter 100 may be removably disposed on the switchable filter 40, making the interference filter 100 replaceable. Figure 3 In the illustrated embodiment, the switchable filter 40 includes a first polarizing filter 14, a first optically rotating liquid crystal unit 16, a second polarizing filter 18, a second optically rotating liquid crystal unit 20, a third polarizing filter 22, and a fourth polarizing filter 26. The polarizing filters 14, 18, and 22 may have substantially perpendicular polarization directions. In other words, the polarization direction of the second polarizing filter 18 may be substantially perpendicular to the polarization direction of the first polarizing filter 14, and the third polarizing filter 22 may have substantially the same polarization direction as the first polarizing filter 14. Furthermore, the third polarizing filter 22 and the fourth polarizing filter 26 may have substantially parallel polarization directions.
[0063] exist Figure 3In the illustrated embodiment, the switchable filter 40 also includes a low-twist color-tunable liquid crystal cell 24 disposed between the third polarizing filter 22 and the fourth polarizing filter 26. The low-twist color-tunable liquid crystal cell 24 may be similar in design to the liquid crystal cells 16 and 20, but its operation is different because it is sandwiched between the parallel polarizers 22 and 26 relative to the cross polarizer.
[0064] Liquid crystal cells 16, 20, and 24 may be provided with connectors 30, 32, and 34, respectively, through which control voltages can be applied. Each liquid crystal cell in liquid crystal cells 16 and 20 may include a liquid crystal defining surface. Nematic crystal molecules may adopt specific angular positions such that the nematic crystal molecules are twisted by corresponding twist angles between them on the defining surface.
[0065] Applying a voltage to connectors 30 and 32 creates an electric field between the defined surfaces. Nematic liquid crystal molecules align with this electric field, which is perpendicular to the defined surfaces rather than parallel to them, and the cells darken. Therefore, a filter effect is achieved when a control voltage is applied to the low-twist cells 16 and 20. The rotation angle of the nematic crystal molecules can be controlled by changing the control voltage, and thus the corresponding filter effect can also be controlled. As a result, liquid crystal cells 16 and 20 can be in a bright transmission state when no voltage is applied, and in a dark transmission state when a voltage is applied. The voltage level can vary for different cell designs, depending on the liquid crystal material used, different cell gap geometries, etc. Furthermore, when no voltage is applied to connector 34, the low-twist color-tunable liquid crystal cell 24 can be dark and exhibit a certain color, primarily blue to the user. When a voltage greater than approximately 4.0 V is applied via connector 34, the low-twist color-tunable liquid crystal cell 24 can become optically transparent.
[0066] Figure 4 A schematic perspective view of a protective helmet 50 according to one embodiment of the present disclosure is shown.
[0067] The protective helmet 50 includes an automatic dimming filter 10. Figure 4 In the illustrated embodiments, the protective helmet 50 is a face shield 60 (e.g., a safety mask, also known as a protective helmet). The face shield 60 includes a face shield body 62. An auto-darkening filter 10 may be positioned within the face shield body 62 such that when a user wears the face shield 60, the auto-darkening filter 10 is directly in front of the user's eyes. The auto-darkening filter 10 blocks electromagnetic radiation (e.g., visible light, UV light, IR, etc.). In some embodiments, the auto-darkening filter 10 may be removably attached to the face shield body 62.
[0068] In some embodiments, the auto-darkening filter 10 may be provided in any other suitable equipment or article and for other applications. For example, the auto-darkening filter 10 may be provided as part of protective eyewear (e.g., goggles) instead of the full-coverage face shield 60. Alternatively, the auto-darkening filter 10 may be provided in a handheld device or in a window or aperture that allows viewing of a room, cabinet, cabin, etc., where high-intensity light may be present. The auto-darkening filter 10 may be used in conjunction with industrial operations such as welding (e.g., arc welding, blow welding, acetylene welding), cutting (e.g., laser cutting, acetylene cutting), brazing, soldering, etc. The auto-darkening filter 10 may also be used in conjunction with medical procedures involving high-intensity light, such as laser surgery, hair removal, tattoo removal, and photocuring of dental resins.
[0069] Figure 5 An example is illustrated of the manufacture of an automatic dimming filter (e.g., according to one embodiment of the present disclosure). Figure 3 The automatic dimming filter 10) is an interference filter (e.g., Figure 1 The flowchart of method 200 for interference filter 100 is shown below. (Refer to...) Figures 1 to 4 Method 200 is described further.
[0070] At step 202, method 200 includes providing an optically transparent substrate. (Reference) Figure 1 For example, method 200 may include providing a substrate 102.
[0071] At step 204, method 200 further includes forming an optical stack on the substrate by depositing a plurality of second layers on a plurality of first layers, such that the plurality of second layers alternate with the plurality of first layers to form the optical stack on the substrate. The optical stack defines a plane and a total stack area in the plane of the optical stack. Each of the plurality of first layers is dielectric. Each of the plurality of second layers is metallic. Each second layer defines a thickness perpendicular to the plane. The thickness of each second layer is less than 40 nm. Each second layer includes a plurality of discrete clusters extending along the thickness of the second layer in the plane of the optical stack. The plurality of discrete clusters are spaced apart from each other such that each second layer also includes a plurality of voids extending through the thickness of the second layer and having a total void area in the plane of the optical stack. The average maximum cluster size of the plurality of discrete clusters of each second layer, measured along the plane of the optical stack, is less than 70 nm. The total void area of each second layer is less than 1% of the total stack area of the optical stack.
[0072] refer to Figure 1 , Figure 2A and Figure 2BFor example, method 200 may include forming an optical stack 104 on a substrate 102 by depositing a plurality of second layers 108 on a plurality of first layers 106, such that the plurality of second layers 108 alternate with the plurality of first layers 106 to form the optical stack 104 on the substrate 102.
[0073] In some implementations, the average maximum cluster size is 48 nm to 68 nm. In some implementations, the total void area of each second layer is less than 0.1% of the total stack area of the optical stack, such that the second layer substantially covers the adjacent first layers among the plurality of first layers.
[0074] In some implementations, each second layer contains 95% to 99.5% silver by weight. Each second layer also contains 0.5% to 5% dopant by weight.
[0075] In some embodiments, the dopant comprises copper (Cu), aluminum (Al), zinc (Zn), silicon carbide (SiC), or combinations thereof. In some embodiments, the thickness of each second layer is less than 12 nm.
[0076] In some embodiments, each first layer comprises silicon dioxide (SiO2), titanium dioxide (TiO2), tantalum pentoxide (Ta2O5), aluminum oxide (Al2O3), hafnium oxide (HfO2), zinc sulfide (ZnS), or combinations thereof.
[0077] In some implementations, the substrate comprises glass or aluminum oxide (Al2O3).
[0078] In some implementations, each second layer is deposited on top of an adjacent first layer via physical vapor deposition (PVD) using a thermal resistance source or electron gun evaporation. (Reference) Figure 1 and Figure 2B For example, each second layer 108 can be deposited on the adjacent first layer 106 by physical vapor deposition (PVD) using a thermal resistance source or electron gun evaporation. PVD may be a suitable and preferred process for depositing each second layer 108.
[0079] In some implementations, each second layer is deposited by evaporating a mixture of silver and dopant. (Reference) Figure 1 and Figure 2B For example, each second layer 108 can be deposited by evaporating a mixture of silver and dopant.
[0080] In some implementations, the deposition rate of each second layer on adjacent first layers is greater than 8 angstroms / second. (Reference) Figure 1 For example, the deposition rate of each second layer 108 on the adjacent first layer 106 can be greater than 8 angstroms / second.
[0081] Compared to pure silver, a mixture of silver and dopant can be deposited at a higher deposition rate without compromising the uniformity of the resulting second layer 108. Therefore, a mixture of silver and dopant offers greater flexibility in deposition rate compared to pure silver, and in some cases, can accelerate the fabrication of interference filters.
[0082] Experimental results
[0083] Various samples were prepared by coating an 11 nm metal layer onto an 80 nm substrate on a glass substrate using physical vapor deposition (PVD), resulting in each sample having the following structure: {metal layer / substrate / glass substrate}. PVD was performed in a vacuum chamber (often referred to as a "box coater"), where the {substrate / glass substrate} structure underwent planetary rotation.
[0084] Multiple first samples were prepared by coating a substrate with pure silver. Multiple second samples were also prepared by coating a substrate with a mixture of 98.5% silver and 1.5% Cu (referred to herein as “copper-doped silver”). The mixture (copper-doped silver) was deposited on the substrate using particles ranging in size from 2 mm to 5 mm.
[0085] Various experiments were conducted on the samples to test their optical properties, uniformity, and thermal robustness.
[0086] Figure 6A This is a photograph of a first sample. Figure 6B This is a photograph of a second sample. (Reference) Figure 6A and Figure 6B It was observed that the first sample with a pure silver coating ( Figure 6A Compared to the sample shown), the second sample with a copper-doped silver coating (as shown) Figure 6B The first sample (as shown in the diagram) exhibited reduced light scattering. Specifically, the second sample showed reduced "wide-angle forward scattering," which was visually observable. The first and second samples were then tested according to ISO 18526-2:2020, 14.2 (Test methods for eye and face protection). An improvement of approximately 2% to 4% was observed in the second sample relative to the first sample.
[0087] Figure 7A SEM images of different cross sections of the first sample obtained using a scanning electron microscope are shown. Figure 7B SEM images of different segments of the second sample obtained using scanning electron microscopy are shown.
[0088] refer to Figure 7AThe average maximum cluster size of the discrete clusters formed by the three segments in the pure silver layer was calculated to be between 84 nm and 99 nm. The uncovered area of the three segments (i.e., the area of the substrate not covered by the pure silver layer) was calculated to be between 1.7% and 4.5% of the total area of the substrate.
[0089] Now for reference Figure 7B The average maximum cluster size of the discrete clusters formed by three segments in the copper-doped silver layer was calculated to be 48 nm to 68 nm. Furthermore, the copper-doped silver layer essentially covers the substrate layer. That is, the uncovered area of the substrate layer is zero. Compared with the first sample (e.g....), Figure 7A Compared to the example shown, the copper-doped silver layer is smoother, more uniform, and has much smaller discrete clusters.
[0090] Figure 8 Graph 300 illustrates the relationship between transmittance (y-axis, in %) and wavelength (x-axis, in nm) for some first samples and some second samples.
[0091] Graph 300 includes a calculated curve 301 (dashed line) depicting the ideal or desired relationship between transmittance and wavelength for a sample produced for experimental purposes, and having the following structure: {metal layer / substrate / glass substrate}. Graph 300 also includes a first curve 302 (long dash, short dash) depicting the transmittance of a first sample (with a pure silver layer) as a function of wavelength, and a second curve 304 (long dash, double dash) depicting the transmittance of a second sample (with a copper-doped silver layer) as a function of wavelength. Graph 300 also includes other curves depicting the transmittance as a function of wavelength for other samples, but for clarity, they are not indicated by reference numerals. The best-performing first and second samples (relative to the calculated curve 301) correspond to the first curve 302 and the second curve 304, respectively. Note that the second curve 304 is closer to the calculated curve 301 than the first curve 304.
[0092] For each wavelength in the visible wavelength range extending from approximately 400 nm to approximately 520 nm, the second sample corresponding to the second curve 304 transmits more than 60% of substantially perpendicular incident light. Compared to the first sample corresponding to the first curve 304, the second sample exhibits higher transmittance in the visible wavelength range extending from approximately 400 nm to approximately 520 nm. The second sample demonstrates better light transmittance than the first sample.
[0093] Furthermore, for each wavelength in the infrared wavelength range extending from approximately 960 nm to approximately 1000 nm, the second sample corresponding to the second curve 304 transmits less than 30% of substantially perpendicular incident light. Compared to the first sample corresponding to the first curve 302, the second sample exhibits lower transmittance (or higher reflectance) in the infrared wavelength range extending from approximately 960 nm to approximately 1000 nm. In other words, the second sample exhibits better infrared reflectance (or infrared attenuation) than the first sample. It was also observed that the second sample corresponding to the second curve 304 exhibits a higher ratio of light transmittance (in the range of 400 nm to 700 nm) to near-infrared transmittance (greater than 780 nm) than the first sample corresponding to the first curve 302, which is desirable for interference filters.
[0094] Figure 9 A graph 350 illustrates the relationship between visible transmittance (y-axis, in %) and deposition rate (x-axis, in Å / s) for samples prepared from pure silver and copper-doped silver. Graph 350 includes a first curve 352, which depicts the variation of visible transmittance of the first sample relative to the deposition rate of pure silver on the substrate. Graph 350 also includes a second curve 354, which depicts the variation of visible transmittance of the second sample relative to the deposition rate of the copper-doped silver layer on the substrate. As depicted by the first curve 352, the visible transmittance of the first sample is highly sensitive to the deposition rate of pure silver. On the other hand, as depicted by the second curve 354, the visible transmittance of the second sample is less sensitive to the deposition rate of copper-doped silver. The conclusion is that copper-doped silver offers greater flexibility in terms of deposition rate compared to pure silver. Moreover, copper-doped silver can be deposited at higher deposition rates (e.g., greater than 8 Å / s) without negatively impacting the resulting visible transmittance of the second sample.
[0095] The thermal robustness of the first and second samples was also tested. Some of the first samples and some of the second samples were heat-treated at 100 degrees Celsius for 10 minutes. In addition, some of the first samples and some of the second samples were heat-treated at 290 degrees Celsius for 10 seconds.
[0096] The first sample, heat-treated at 100 degrees Celsius for 10 minutes, showed minimal visual degradation. On the other hand, the second sample, heat-treated at 100 degrees Celsius for 10 minutes, showed no visual change.
[0097] The first sample, heat-treated at 290 degrees Celsius for 10 seconds, also showed minimal visual degradation. On the other hand, the second sample, heat-treated at 290 degrees Celsius for 10 seconds, showed no visual change.
[0098] It is noted that the pure silver layer of the first sample deteriorated after both heat treatments, while the copper-doped silver layer of the second sample did not show any visible deterioration after both heat treatments. Then, the relationship between transmittance and wavelength characteristics was tested on the first and second samples that underwent the aforementioned heat treatments.
[0099] Figure 10A The graph illustrates the relationship between transmittance (y-axis, in %) and wavelength (x-axis, in nm) for a heat-treated first sample and an untreated first sample.
[0100] Graph 400 includes reference curves 401A, 401B, 401C, and 401D (solid lines), which depict the transmittance of four untreated first samples relative to wavelength. Graph 400 also includes first curves 402A and 402B (long dashed line followed by two short dashed lines), which depict the transmittance of two first samples heat-treated at 100 degrees Celsius for 10 minutes relative to wavelength. Graph 400 further includes second curves 404A and 404B (dashed lines), which depict the transmittance of two first samples heat-treated at 290 degrees Celsius for 10 seconds relative to wavelength.
[0101] As depicted by curves 402A and 402B, the first samples heat-treated at 100 degrees Celsius for 10 minutes exhibited significantly degraded phototransmittance compared to the untreated first samples (corresponding to reference curves 401A, 401B, 401C, and 401D). Furthermore, as depicted by curves 404A and 404B, the first samples heat-treated at 290 degrees Celsius for 10 seconds also exhibited substantially degraded phototransmittance compared to the untreated first samples (corresponding to reference curves 401A, 401B, 401C, and 401D). It is noted that the pure silver layer degrades significantly upon exposure to high temperatures, which adversely affects the phototransmittance of the first samples.
[0102] Figure 10B Graph 450 illustrates the relationship between transmittance (y-axis, in %) and wavelength (x-axis, in nm) for a heat-treated second sample and an untreated second sample.
[0103] Graph 450 includes reference curves 451A and 451B (solid lines), which depict the transmittance of two untreated second samples relative to wavelength. Graph 400 also includes a first curve 452 (long dashed line followed by two short dashed lines), which depicts the transmittance of a second sample heat-treated at 100 degrees Celsius for 10 minutes relative to wavelength. Graph 400 also includes second curves 454A and 454B (dashed lines), which depict the transmittance of two second samples heat-treated at 290 degrees Celsius for 10 seconds relative to wavelength.
[0104] As depicted by the first curve 452, the second sample heat-treated at 100 degrees Celsius for 10 minutes exhibited similar visible transmittance compared to the untreated second samples (corresponding to reference curves 451A and 451B). Furthermore, as depicted by the second curves 454A and 454B, the second sample heat-treated at 290 degrees Celsius for 10 seconds also exhibited similar visible transmittance compared to the untreated second samples (corresponding to reference curves 451A and 451B). It is noted that the copper-doped silver layer is robust to high temperatures, and therefore, the visible transmittance of the second samples exposed to high temperatures was not negatively affected.
[0105] Unless otherwise stated, all figures used in the specification and claims to indicate feature dimensions, quantities, and physical properties should be understood to be modified by the term "about". Therefore, unless stated to the contrary, the numerical parameters listed in the foregoing specification and appended claims are approximations and can vary according to the desired properties sought by those skilled in the art using the teachings disclosed herein.
[0106] While specific embodiments have been illustrated and described herein, those skilled in the art will recognize that various alternative and / or equivalent embodiments may be used in place of the illustrated and described embodiments without departing from the scope of this disclosure. This application is intended to cover any modifications or variations of the specific embodiments discussed herein. Therefore, this disclosure is intended to be limited only by the claims and their equivalents.
Claims
1. An interference filter for an automatic dimming filter, the interference filter comprising: Optically transparent substrate; and An optical stack disposed on the substrate, the optical stack comprising a plurality of first layers and a plurality of second layers alternating with the plurality of first layers, the optical stack defining a plane and a total stack area in the plane of the optical stack; Each of the plurality of first layers is dielectric; Each of the plurality of second layers is metallic, and each second layer defines a thickness perpendicular to the plane, wherein the thickness of each second layer is less than 40 nanometers (nm). Each second layer includes a plurality of discrete clusters extending along the thickness of the second layer on the plane of the optical stack, the plurality of discrete clusters being spaced apart from each other such that each second layer also includes a plurality of voids extending through the thickness of the second layer and having a total void area in the plane of the optical stack, wherein the average maximum cluster size of the plurality of discrete clusters of each second layer, measured along the plane of the optical stack, is less than 70 nm, and wherein the total void area of each second layer is less than 1% of the total stack area of the optical stack.
2. The interference filter according to claim 1, wherein the average maximum cluster size is 48 nm to 68 nm.
3. The interference filter of claim 1, wherein the total void area of each second layer is less than 0.1% of the total stack area of the optical stack, such that the second layer substantially covers the adjacent first layer among the plurality of first layers.
4. The interference filter of claim 1, wherein each second layer comprises: 95% to 99.5% silver by weight; and 0.5% to 5% dopant by weight.
5. The interference filter according to claim 4, wherein the dopant comprises copper (Cu), aluminum (Al), zinc (Zn), silicon carbide (SiC), or a combination thereof.
6. The interference filter of claim 1, wherein the thickness of each second layer is less than 12 nm.
7. The interference filter according to claim 1, wherein each first layer comprises silicon dioxide (SiO2), titanium dioxide (TiO2), tantalum pentoxide (Ta2O5), aluminum oxide (Al2O3), hafnium oxide (HfO2), zinc sulfide (ZnS), or combinations thereof.
8. The interference filter according to claim 1, wherein the substrate comprises glass or aluminum oxide (Al2O3).
9. An automatic dimming filter, the automatic dimming filter comprising: A switchable filter that responds to an activation signal to change from a bright transmission state to a dark transmission state; and The interference filter according to claim 1, wherein the interference filter is disposed on the switchable filter.
10. A protective helmet comprising the automatic dimming filter according to claim 9.
11. A method for manufacturing an interference filter for an automatic dimming filter, the method comprising: Provides optically transparent substrates; as well as An optical stack is formed on the substrate by depositing a plurality of second layers on a plurality of first layers, such that the plurality of second layers alternate with the plurality of first layers to form the optical stack on the substrate, the optical stack defining a plane and a total stack area in the plane of the optical stack; Each of the plurality of first layers is dielectric; Each of the plurality of second layers is metallic, and each second layer defines a thickness perpendicular to the plane, wherein the thickness of each second layer is less than 40 nanometers (nm). Each second layer includes a plurality of discrete clusters extending along the thickness of the second layer on the plane of the optical stack, the plurality of discrete clusters being spaced apart from each other such that each second layer also includes a plurality of voids extending through the thickness of the second layer and having a total void area in the plane of the optical stack, wherein the average maximum cluster size of the plurality of discrete clusters of each second layer, measured along the plane of the optical stack, is less than 70 nm, and wherein the total void area of each second layer is less than 1% of the total stack area of the optical stack.
12. The method of claim 11, wherein the average maximum cluster size is 48 nm to 68 nm.
13. The method of claim 11, wherein the total void area of each second layer is less than 0.1% of the total stack area of the optical stack, such that the second layer substantially covers the adjacent first layer among the plurality of first layers.
14. The method of claim 11, wherein each second layer comprises: Silver content of 95% to 99.5% by weight; and dopant content of 0.5% to 5% by weight.
15. The method of claim 14, wherein the dopant comprises copper (Cu), aluminum (Al), zinc (Zn), silicon carbide (SiC), or a combination thereof.
16. The method of claim 11, wherein the thickness of each second layer is less than 12 nm.
17. The method of claim 11, wherein each first layer comprises silicon dioxide (SiO2), titanium dioxide (TiO2), tantalum pentoxide (Ta2O5), aluminum oxide (Al2O3), hafnium oxide (HfO2), zinc sulfide (ZnS), or combinations thereof.
18. The method of claim 11, wherein the substrate comprises glass or aluminum oxide (Al2O3).
19. The method of claim 11, wherein each second layer is deposited on the adjacent first layer by physical vapor deposition (PVD) using a thermal resistance source or electron gun evaporation.
20. The method of claim 11, wherein each second layer is deposited by evaporating a mixture of silver and dopant.
21. The method of claim 11, wherein the deposition rate of each second layer on the adjacent first layer is greater than 8 angstroms / second.