Electrode binder polymers for non-aqueous electrochemical devices, electrode binder compositions for non-aqueous electrochemical devices, electrode compositions for non-aqueous electrochemical devices, electrodes for non-aqueous electrochemical devices, non-aqueous electrochemical devices, and non-aqueous secondary batteries.

By using a specific monomer copolymer as an electrode binder, the problems of slow dissolution rate and large swelling in the prior art are solved, realizing rapid dissolution and low swelling of electrode binders in non-aqueous electrochemical devices, and improving coating performance.

CN123125699APending Publication Date: 2026-11-17TEIJIN LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202580029267.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-30
Filing Date
2025-04-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the prior art, polyvinylidene fluoride resins used as electrode binders have problems such as slow dissolution rate and high swelling caused by electrolyte, which limit their application in non-aqueous electrochemical devices.

Method used

A copolymer containing acrylonitrile and methacrylonitrile and unsaturated carboxylic acids, unsaturated carboxylic acid alkyl esters or unsaturated carboxylic acid amides is used as an electrode binder. The content and weight-average molecular weight of each monomer in the copolymer are controlled to improve the dissolution rate and reduce the swelling caused by the electrolyte.

Benefits of technology

It achieves rapid dissolution and low swelling in solvents, resulting in excellent coatability, and is suitable for electrode binders and batteries in non-aqueous electrochemical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The electrode binder polymer for non-aqueous electrochemical devices is a copolymer comprising structural units of at least one monomer (1) derived from acrylonitrile and methacrylonitrile, and structural units of at least one monomer (2) selected from the group consisting of unsaturated carboxylic acids, unsaturated carboxylic acid alkyl esters and unsaturated carboxylic acid amides, wherein the content of the structural units derived from the aforementioned monomer (2) is 0.1 mol% to 4.9 mol% relative to the total amount of the structural units derived from the aforementioned monomer (1) and the structural units derived from the aforementioned monomer (2), and the weight average molecular weight of the aforementioned polymer is 10,000 to 450,000.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to electrode binder polymers for non-aqueous electrochemical devices, electrode binder compositions for non-aqueous electrochemical devices, electrode compositions for non-aqueous electrochemical devices, electrodes for non-aqueous electrochemical devices, non-aqueous electrochemical devices, and non-aqueous secondary batteries. Background Technology

[0002] Organofluorine compounds possess useful properties such as heat resistance, chemical resistance, and surface activity, and are therefore widely used in manufacturing and industrial applications. For example, polyvinylidene fluoride resins are known to be used as binders for electrodes.

[0003] However, in recent years, reports have highlighted the ecotoxicity and human toxicity of organofluorine compounds, leading to increasingly stringent restrictions on their manufacture and use worldwide. Therefore, efforts are underway to develop binders for electrodes with low or no polyvinylidene fluoride (PVDF) resin content.

[0004] For example, Patent Documents 1 and 2 disclose the use of polymers having structural units derived from acrylonitrile and specific monomers as binders for electrodes.

[0005] Patent Document 1: Japanese Patent Application Publication No. 2003-132893 Patent Document 2: Japanese Patent Application Publication No. 2004-185826 Summary of the Invention

[0006] The problem that the invention aims to solve However, the polymers disclosed in Patent Documents 1 and 2, which have structural units derived from acrylonitrile and specific monomers, have problems in practical application, such as slow dissolution rate in solvents and high swelling caused by electrolytes.

[0007] This disclosure is made in view of the above circumstances, and relates to the provision of electrode binder polymers for non-aqueous electrochemical devices, electrode binder compositions for non-aqueous electrochemical devices, electrode compositions for non-aqueous electrochemical devices, electrodes for non-aqueous electrochemical devices, non-aqueous electrochemical devices, and non-aqueous secondary batteries, which have fast dissolution rates in solvents, low swelling caused by electrolytes, and excellent coatability.

[0008] Methods for solving problems This public text includes the following methods.

[0009] <1> Electrode binder polymer for non-aqueous electrochemical devices is a copolymer comprising structural units of at least one monomer (1) derived from acrylonitrile and methacrylonitrile, and structural units of at least one monomer (2) derived from the group consisting of unsaturated carboxylic acids, unsaturated alkyl carboxylic esters and unsaturated carboxylic amides. The content of structural units derived from the aforementioned monomer (2) is 0.1 mol% to 4.9 mol% relative to the total amount of structural units derived from the aforementioned monomer (1) and structural units derived from the aforementioned monomer (2). The weight-average molecular weight of the aforementioned polymers ranges from 10,000 to 450,000.

[0010] <2> like <1> The electrode binder polymer of the non-aqueous electrochemical device, wherein the aforementioned unsaturated alkyl carboxylic acid ester is at least one of methyl acrylate and methyl methacrylate.

[0011] <3> like <1> or <2> The electrode binder polymer of the non-aqueous electrochemical device, wherein the aforementioned unsaturated carboxylic acid is at least one selected from the group consisting of acrylic acid, methacrylic acid and itaconic acid.

[0012] <4> like <1> ~ <3> The electrode binder polymer of the non-aqueous electrochemical device described in any one of the above-mentioned monomers (2) has 5 or fewer carbon atoms.

[0013] <5> Electrode binder composition for non-aqueous electrochemical devices, comprising <1> ~ <4> The electrode binder polymer of the non-aqueous electrochemical device described in any one of the following statements.

[0014] <6> like <5> The electrode binder composition for the non-aqueous electrochemical device further comprises a solvent.

[0015] <7> Electrode compositions for non-aqueous electrochemical devices, comprising active materials and <1> ~ <4> The electrode binder polymer of the non-aqueous electrochemical device described in any one of the following statements.

[0016] <8> like <7> The electrode composition of the non-aqueous electrochemical device, wherein the aforementioned active material is a positive electrode active material.

[0017] <9> Electrodes of non-aqueous electrochemical devices, which possess <7> or <8> The electrode composition of the aforementioned non-aqueous electrochemical device.

[0018] <10> Non-aqueous electrochemical devices, which possess <9> The electrodes of the aforementioned non-aqueous electrochemical device.

[0019] <11> Non-aqueous secondary batteries have <9> or <10> The electrodes of the aforementioned non-aqueous electrochemical device.

[0020] Invention Effects According to this disclosure, there are electrode binder polymers for non-aqueous electrochemical devices, electrode binder compositions for non-aqueous electrochemical devices, electrode compositions for non-aqueous electrochemical devices, electrodes for non-aqueous electrochemical devices, non-aqueous electrochemical devices, and non-aqueous secondary batteries, which can be provided with compositions that have fast dissolution in solvents, low swelling caused by electrolytes, and excellent coatability. Detailed Implementation

[0021] The following is a detailed description of one embodiment of this disclosure. However, this disclosure is not limited to the following embodiment. In the following disclosure, the constituent elements (including element steps, etc.) are not essential unless specifically stated otherwise. Similarly, numerical values ​​and their ranges are not limited to this disclosure.

[0022] In this document, the numerical range indicated by “~” includes the values ​​before and after “~” as the lower limit and upper limit, respectively.

[0023] In the numerical ranges described in this disclosure, the upper or lower limit of one numerical range can be replaced with the upper or lower limit of another numerical range described in other periods. Additionally, the upper or lower limit of a numerical range described in this disclosure can also be replaced with the values ​​shown in the embodiments.

[0024] In this disclosure, the percentage of each component in the composition refers to the total percentage of the various substances present in the composition, unless otherwise specified, when multiple substances belonging to each component are present in the composition.

[0025] In this disclosure, when “or” or “or” is used to list multiple elements, unless otherwise explicitly stated, the combination of multiple elements is not excluded as long as it does not create a technical contradiction.

[0026] In this disclosure, even when elements are expressed in a singular form, multiple instances are not excluded unless otherwise explicitly stated, provided that no technical contradiction arises.

[0027] In this public document, multiple examples described separately can be combined to form new methods, provided they do not contradict each other.

[0028] Electrode binder polymers for non-aqueous electrochemical devices The electrode binder polymer of the non-aqueous electrochemical device disclosed herein (hereinafter also referred to as the "binder polymer of this disclosure") is a copolymer comprising structural units of at least one monomer (1) derived from acrylonitrile and methacrylonitrile, and structural units of at least one monomer (2) derived from the group consisting of unsaturated carboxylic acids, unsaturated alkyl carboxylic esters and unsaturated carboxylic amides. The content of structural units derived from the aforementioned monomer (2) is 0.1 mol% to 4.9 mol% relative to the total amount of structural units derived from the aforementioned monomer (1) and structural units derived from the aforementioned monomer (2). The weight-average molecular weight of the aforementioned polymers ranges from 10,000 to 450,000.

[0029] The adhesive polymer according to this disclosure has a fast dissolution rate in solvents, low swelling caused by electrolytes, and yields compositions with excellent coatability.

[0030] The role of the adhesive polymer in this disclosure is presumed to be as follows.

[0031] The adhesive polymer of this disclosure contains structural units derived from monomer (2), which improve the dissolution rate in solvents and, on the other hand, improve the swelling properties in electrolytes. However, the adhesive polymer of this disclosure excels in both fast dissolution rate in solvents and low swelling properties caused by electrolytes by specifying the content of structural units derived from monomer (2) within a certain range.

[0032] Furthermore, if the weight-average molecular weight of the binder polymer is too high, the viscosity of the composition obtained from the aforementioned binder polymer will increase, resulting in low leveling properties and a tendency for uneven film thickness to occur on the coated film when the aforementioned composition is applied. However, the binder polymer of this disclosure specifies a weight-average molecular weight within a certain range, therefore, when the composition obtained from the binder polymer of this disclosure is applied, it exhibits high leveling properties and is less prone to uneven film thickness on the coated film, i.e., excellent coatability.

[0033] It should be noted that this public text is not subject to any of the aforementioned presumptions.

[0034] <Structural unit derived from single unit (1)> The adhesive polymer disclosed herein comprises structural units of at least one monomer (1) derived from acrylonitrile and methacrylonitrile. The monomer (1) may comprise only one monomer or in combination of two or more monomers.

[0035] The monomer (1) is preferably acrylonitrile.

[0036] From the viewpoint of balancing the dissolution rate in the solvent and the swelling caused by the electrolyte, the content of the structural unit derived from monomer (1) is preferably 95.1 mol% to 99.9 mol% relative to the total amount of the structural units derived from monomer (1) and the structural units derived from monomer (2), more preferably 96.0 mol% to 99.5 mol%, and even more preferably 96.5 mol% to 99.0 mol%.

[0037] If the content of structural units derived from monomer (1) is 95.1 mol% or more relative to the total amount of structural units derived from monomer (1) and monomer (2), the binder polymer exhibits excellent low swelling due to electrolyte. If the content of structural units derived from monomer (1) is 99.9 mol% or less relative to the total amount of structural units derived from monomer (1) and monomer (2), the binder polymer exhibits excellent fast dissolution rate in solvent.

[0038] It should be noted that in this disclosure, when multiple monomers (1) are present in the adhesive polymer of this disclosure, "content of structural units derived from monomer (1)" refers to the total content of structural units derived from the multiple monomers (1). Similarly, when multiple monomers (2) are present in the adhesive polymer of this disclosure, "content of structural units derived from monomer (2)" refers to the total content of structural units derived from the multiple monomers (2).

[0039] In this disclosure, the content of structural units derived from specific monomers in the polymer can be determined by NMR.

[0040] <Structural unit derived from single unit (2)> The adhesive polymer disclosed herein comprises structural units derived from at least one monomer (2) selected from the group consisting of unsaturated carboxylic acids, unsaturated carboxylic acid alkyl esters and unsaturated carboxylic acid amides.

[0041] Monomer (2) may contain one type alone or two or more types in combination.

[0042] From the viewpoint of preventing an increase in swelling, the number of carbon atoms in the aforementioned monomer (2) is preferably 10 or less, more preferably 7 or less, and even more preferably 5 or less. The number of carbon atoms in the aforementioned monomer (2) may be 2 or more, or 3 or more.

[0043] From the viewpoint of balancing the dissolution rate in the solvent and the swelling caused by the electrolyte, the monomer (2) is preferably at least one of unsaturated carboxylic acid and unsaturated carboxylic acid alkyl ester, more preferably unsaturated carboxylic acid or unsaturated carboxylic acid alkyl ester, and even more preferably unsaturated carboxylic acid and unsaturated carboxylic acid alkyl ester.

[0044] (Unsaturated carboxylic acids) Examples of unsaturated carboxylic acids include olefinically unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, and isocrotonic acid; and unsaturated dicarboxylic acids such as maleic acid, fumaric acid, citraconic acid, mesoconic acid, pentenediaic acid, and itaconic acid. Unsaturated carboxylic acids can be a single type or a combination of two or more.

[0045] From the viewpoint of dissolution rate in solvent and swelling caused by electrolyte, the aforementioned unsaturated carboxylic acid is preferably at least one selected from the group consisting of acrylic acid, methacrylic acid and itaconic acid, more preferably at least one selected from methacrylic acid and itaconic acid, and even more preferably itaconic acid.

[0046] (Alkyl esters of unsaturated carboxylic acids) Examples of unsaturated carboxylic acid alkyl esters include: Alkyl acrylates such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, tert-butyl acrylate, and isobutyl acrylate; Alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, and isobutyl methacrylate; Crotonic acid alkyl esters such as methyl crotonate, ethyl crotonate, n-propyl crotonate, isopropyl crotonate, n-butyl crotonate, tert-butyl crotonate, and isobutyl crotonate. Amino methacrylates such as dimethylaminoethyl methacrylate and diethylaminoethyl methacrylate; Methoxy polyethylene glycol acrylate, ethoxy polyethylene glycol acrylate, ethoxy diethylene glycol acrylate, methoxy dipropylene glycol acrylate, methoxy ethyl acrylate, 2-ethoxy ethyl acrylate, butoxy ethyl acrylate, phenoxy ethyl acrylate, and other acrylates containing alkoxy groups. Methoxylated polyethylene glycol methacrylate, ethoxylated polyethylene glycol methacrylate, methoxylated diethylene glycol methacrylate, methoxylated dipropylene glycol methacrylate, methoxyethyl methacrylate, 2-ethoxyethyl methacrylate, butoxyethyl methacrylate, phenoxyethyl methacrylate, and other methacrylates containing alkoxy groups; Alkyl acrylates and alkyl methacrylates having phosphate residues, sulfonic acid residues, boric acid residues, etc. on the alkyl group.

[0047] Unsaturated carboxylic acid alkyl esters may contain only one type or in combination of two or more types.

[0048] From the viewpoint of dissolution rate in solvent and swelling caused by electrolyte, the aforementioned unsaturated carboxylic acid alkyl ester is preferably at least one of methyl acrylate and methyl methacrylate, more preferably methyl acrylate or methyl methacrylate.

[0049] (Unsaturated carboxylic acid amide) Examples of unsaturated carboxylic acid amides include acrylamide, methacrylamide, itaconic acid diamide, hydroxymethylacrylamide, and butoxyhydroxymethylacrylamide. Unsaturated carboxylic acid amides can be a single type or a combination of two or more types.

[0050] From the viewpoint of dissolution rate in solvent and swelling caused by electrolyte, the aforementioned unsaturated carboxylic acid amide is preferably at least one selected from the group consisting of acrylamide, methacrylamide and itaconic acid diamide, and more preferably acrylamide or methacrylamide.

[0051] (content) The content of structural units derived from the aforementioned monomer (2) is 0.1 mol% to 4.9 mol% relative to the total amount of structural units derived from the aforementioned monomer (1) and structural units derived from the aforementioned monomer (2).

[0052] If the content of structural units derived from the aforementioned monomer (2) is 0.1 mol% or more relative to the total amount of structural units derived from the aforementioned monomer (1) and structural units derived from the aforementioned monomer (2), the polymer exhibits faster dissolution rate in the solvent and thus becomes superior. If the content of structural units derived from the aforementioned monomer (2) is 4.9 mol% or less relative to the total amount of structural units derived from the aforementioned monomer (1) and structural units derived from the aforementioned monomer (2), the polymer exhibits lower swelling due to electrolyte and thus becomes superior.

[0053] From the viewpoint of balancing the dissolution rate in the solvent and the swelling caused by the electrolyte, the content of the structural units derived from the aforementioned monomer (2) is 0.1 mol% to 4.9 mol% relative to the total amount of structural units derived from the aforementioned monomer (1) and structural units derived from the aforementioned monomer (2), preferably 0.2 mol% to 4.5 mol%, and more preferably 0.3 mol% to 3.5 mol%.

[0054] When the adhesive polymer of this disclosure comprises two or more structural units derived from monomer (2), the ratio of the contents of each structural unit derived from monomer (2) in the adhesive polymer of this disclosure is not particularly limited. For example, the content of structural units derived from alkyl esters of unsaturated carboxylic acids is preferably 20% to 1000% on a mol basis, more preferably 100% to 800%, and even more preferably 200% to 700% of the content of structural units derived from saturated carboxylic acids.

[0055] <Structural units derived from monomers other than monomer (1) and monomer (2)> The adhesive polymer disclosed herein may contain structural units derived from monomers other than monomer (1) and monomer (2).

[0056] There are no particular limitations on the monomers other than monomer (1) and monomer (2), and any known copolymerizable unsaturated compound may be used. Examples of monomers other than monomer (1) and monomer (2) include olefins (e.g., 1-olefins with 2 to 4 carbon atoms, such as ethylene, propylene, 1-butene, etc.), vinyl compounds (e.g., vinyl acetate, vinyl chloride, vinyl sulfonic acid, maleic anhydride, N-vinylpyrrolidone, etc.), aromatic vinyl compounds (e.g., styrene, etc.), and heterocyclic vinyl compounds (e.g., vinylpyridine, vinylimidazole, etc.). Monomers other than monomer (1) and monomer (2) may be included individually or in combination with more than two.

[0057] Regarding the content of structural units derived from monomers other than monomer (1) and monomer (2), there is no particular limitation as long as the effect of this disclosure can be achieved. Relative to all structural units of the adhesive polymer of this disclosure, it can be 0 mol% to 50 mol%, 0 mol% to 25 mol%, or 0 mol% to 5 mol%.

[0058] <Molecular weight of adhesive polymer> The weight-average molecular weight of the adhesive polymers disclosed herein is between 10,000 and 450,000.

[0059] The fact that the weight-average molecular weight of the binder polymer in this disclosure is 10,000 or more means that the binder polymer in this disclosure is a polymer compound. If the weight-average molecular weight of the binder polymer in this disclosure is 450,000 or less, the viscosity of the composition containing the binder polymer in this disclosure will not become too high, and the coatability will be excellent.

[0060] From the viewpoint of obtaining a composition with excellent coatability, the weight-average molecular weight of the adhesive polymer of this disclosure is more preferably 50,000 to 400,000, more preferably 100,000 to 380,000, and even more preferably 200,000 to 370,000.

[0061] It should be noted that, in this disclosure, the weight-average molecular weight of the polymer is determined by gel permeation chromatography (GPC). As an example of the apparatus, a GPC apparatus (Tosoh Corporation HPLC-8320GPCEcoSEC) can be used. In this case, a TSK gel α-M column (Tosoh Corporation) is used, and a differential refractive index detector (Tosoh Corporation HLC-8320 GPC RI detector) is used. For the mobile phase, dimethylformamide is used as the eluent, with lithium bromide and phosphoric acid added at 50 mM and 10 mM, respectively. Polystyrene (Tosoh Corporation Standard Polystyrene Kit PStQuick Kit-C, D) is used as the standard.

[0062] <Manufacturing Methods of Adhesive Polymers> There are no particular limitations on the method for manufacturing the adhesive polymer as disclosed in this document; any known polymerization method may be used, with free radical polymerization being preferred.

[0063] In the case of free radical polymerization, known polymerization methods such as solution polymerization, dispersion polymerization, bulk polymerization, suspension polymerization, and emulsion polymerization can be used. From a productivity perspective, solution polymerization or suspension polymerization is preferred. The polymerization initiators and catalysts used in free radical polymerization are not particularly limited; examples include azo compounds, organic peroxides, or redox catalysts such as persulfate / sulfurous acid, chloric acid / sulfurous acid, or their sodium or ammonium salts. When using a redox initiator, a catalyst and / or pH adjuster can be appropriately added to ensure efficient redox reaction. Examples of catalysts include ferric sulfate (II), and examples of pH adjusters include concentrated sulfuric acid.

[0064] In the case of solution polymerization, known solvents such as aqueous zinc chloride solution, dimethyl sulfoxide, and dimethylformamide can be used as polymerization solvents. In particular, considering the reduction of side reactions, aqueous zinc chloride solution or dimethyl sulfoxide is preferred.

[0065] Electrode binder compositions for non-aqueous electrochemical devices The electrode binder composition of the non-aqueous electrochemical device of this disclosure (hereinafter also referred to as "the binder composition of this disclosure") comprises the binder polymer of this disclosure.

[0066] <Adhesive polymers in this disclosure> The adhesive composition of this disclosure contains the adhesive polymer described above.

[0067] From the viewpoint of achieving a balance between improving the adhesion of the electrode and increasing the presence rate of the active material in the electrode, in the binder composition of this disclosure, the content of the binder polymer of this disclosure is preferably 0.5% to 10% by mass, more preferably 1.0% to 5% by mass, and even more preferably 1.5% to 3% by mass.

[0068] Solvent The adhesive compositions disclosed herein may also contain solvents.

[0069] The solvent is not particularly limited as long as it can dissolve the adhesive polymer of this disclosure. Examples include amides such as N-methyl-2-pyrrolidone (NMP), N,N-dimethylacetamide, and N,N-dimethylformamide, as well as acetone, water, methanol, ethanol, propanol, butanol, butanediol, ethylene glycol, propylene glycol, and tripropylene glycol. From the viewpoint of easily dissolving the adhesive polymer of this disclosure, NMP is preferred as the solvent. The solvent may be a single type or a combination of two or more types.

[0070] From the viewpoint of obtaining a fluidity that allows for application, the solvent content in the adhesive composition of this disclosure is preferably 0% to 99% by mass, more preferably 10% to 70% by mass, and even more preferably 20% to 60% by mass.

[0071] <Ingredients other than the adhesive polymers and solvents disclosed herein> The adhesive composition of this disclosure may contain components other than the adhesive polymer and solvent of this disclosure. Examples of components other than the adhesive polymer and solvent of this disclosure include polymers other than the adhesive polymer of this disclosure, dispersants such as surfactants, wetting agents, defoamers, pH adjusters, viscosity modifiers, flow agents, etc.

[0072] (Polymers other than the adhesive polymers mentioned in this disclosure) Examples of polymers other than the adhesive polymers described in this disclosure include polyvinylidene fluoride (PVDF) resins, fully aromatic polyamides, polyamide-imides, polyimides, polyethersulfones, polysulfones, polyether ketones, polyketides, polyether-imides, poly-N-vinylacetamides, polyacrylamides, copolyether polyamides, fluorinated rubbers, acrylic resins, ethylene / methyl acrylate copolymers, ethylene / vinyl alcohol copolymers, acrylonitrile / butadiene copolymers and their hydrides, styrene / butadiene copolymers, butadiene rubber, ethylene / propylene / non-conjugated diene terpolymers (EPDM), cellulose, polyvinyl alcohol, etc.

[0073] <Method for manufacturing adhesive composition> There are no particular limitations on the method for manufacturing the binder composition of this disclosure. Known dissolution methods can be used, such as manual mixing or mixing using a mixer by adding the binder polymer of this disclosure and optional components such as further solvents. As a mixer, a ball mill, sand mill, pigment disperser, pounder, ultrasonic disperser, homogenizer, planetary mixer, etc. can be used.

[0074] Electrode Compositions for Non-Aqueous Electrochemical Devices The electrode composition of the non-aqueous electrochemical device disclosed herein (hereinafter also referred to as "electrode composition of this disclosure") comprises the binder polymer of this disclosure and the active material.

[0075] <Adhesive polymers in this disclosure> The description of the binder polymer contained in the electrode composition of this disclosure is as described above.

[0076] <Active Substances> The active material is preferably at least one of a positive electrode active material and a negative electrode active material, and from the viewpoint of the reduction resistance of the binder polymer of this disclosure, a positive electrode active material is more preferred.

[0077] Examples of positive electrode active materials include LiCoO2, LiNiO2, and LiMn. 1 / 2 Ni 1 / 2 O2, LiCo 1 / 3 Mn 1 / 3 Ni 1 / 3O2, LiMn2O4, LiFePO4, LiCo 1 / 2 Ni 1 / 2 O2, LiAl 1 / 4 Ni 3 / 4Lithium-containing transition metal oxides such as O2; transition metal sulfides such as TiS2, TiS3, and amorphous MoS3; Cu2V2O3, amorphous V2O-P2O5, MoO3, V2O5, and V6O 13 Transition metal oxides, etc.

[0078] As negative electrode active materials, examples include materials that can electrochemically absorb lithium ions, such as amorphous carbon, graphite, natural graphite, mesophase carbon microspheres (MCMB), pitch-based carbon fibers, activated carbon, and other carbon materials; alloys of silicon, tin, aluminum, etc. with lithium; and Wood's alloy.

[0079] <Composition of the electrode composition described in this disclosure> The electrode composition of this disclosure can be a positive electrode composition or a negative electrode composition. From the viewpoint of the reduction resistance of the binder polymer of this disclosure, a positive electrode composition is preferred.

[0080] <Method for manufacturing the electrode composition of this disclosure> There are no particular limitations on the method of manufacturing the electrode composition of this disclosure; known methods can be applied, and the binder composition of this disclosure can be used to manufacture it.

[0081] For example, it can be manufactured by manually mixing or using a mixer by adding the binder composition, active substance, and further optional conductive additives as described in this disclosure. As a mixer, a ball mill, sand mill, pigment disperser, pounder, ultrasonic disperser, homogenizer, planetary mixer, etc., can be used.

[0082] Electrodes for Non-Aqueous Electrochemical Devices The electrode of the non-aqueous electrochemical device of this disclosure (hereinafter also referred to as "the electrode of this disclosure") comprises the electrode composition of this disclosure. That is, the electrode of this disclosure comprises the binder polymer of this disclosure and the aforementioned active material.

[0083] <Construction of electrodes in this disclosure> The electrode in this disclosure can be either a positive electrode or a negative electrode. From the viewpoint of the reduction resistance of the binder polymer in this disclosure, a positive electrode is preferred.

[0084] Examples of embodiments of the positive electrode include a structure obtained by disposing an active material layer comprising the positive electrode active material and the binder polymer of this disclosure on a current collector. Examples of current collectors include aluminum foil, titanium foil, stainless steel foil, etc., with a thickness of 5 μm to 30 μm.

[0085] The active material layer may also include conductive additives, polymers other than the binder polymers described above in this disclosure, dispersants such as surfactants, wetting agents, defoamers, pH adjusters, viscosity modifiers, flow agents, etc. Examples of conductive additives include acetylene black, Ketjen black, graphite powder, carbon materials such as ultrafine carbon fibers, conductive polymers, and metal powders.

[0086] Examples of embodiments of the negative electrode include a structure obtained by disposing an active material layer comprising the negative electrode active material and the binder polymer of this disclosure on a current collector. Examples of current collectors include copper foil, nickel foil, and stainless steel foil with a thickness of 5 μm to 30 μm. Alternatively, lithium metal foil may be used as the negative electrode instead of the aforementioned negative electrode.

[0087] The active material layer may also include conductive additives, polymers other than the binder polymers described above in this disclosure, dispersants such as surfactants, wetting agents, defoamers, pH adjusters, viscosity modifiers, flow agents, etc. Examples of conductive additives include acetylene black, Ketjen black, graphite powder, carbon materials such as ultrafine carbon fibers, conductive polymers, and metal powders.

[0088] <Method for manufacturing electrodes as disclosed in this disclosure> There are no particular limitations on the method of manufacturing the electrode of this disclosure. Known methods can be applied, and the electrode composition of this disclosure can be used to manufacture it. For example, the electrode composition of this disclosure is coated onto a current collector such as a metal foil and dried and / or rolled (i.e., pressed), thereby forming an electrode in which an active material is dispersed and fixed in a matrix formed on the surface of the current collector.

[0089] There are no particular limitations on the method of coating the electrode composition of this disclosure onto the current collector. For example, coating can be performed by blade coating, dip coating, reverse roller coating, direct roller coating, gravure coating, extrusion coating, brush coating, etc. There are no particular limitations on the amount of coating, and it is usually adjusted so that the thickness of the mixed layer containing the active material formed after drying is 0.005 to 5 mm, preferably 0.01 to 2 mm.

[0090] There are no particular limitations on the drying method. Examples include drying using warm air, hot air, low-humidity air, vacuum drying, and drying using far-infrared rays, infrared rays, electron beams, etc. The drying conditions are adjusted to remove the solvent as quickly as possible within a speed range that will not cause stress concentration leading to cracking in the active material layer or peeling of the active material layer from the current collector.

[0091] There are no particular restrictions on the rolling method; the electrode can be stabilized by rolling the coated or dried current collector. Examples of rolling methods include die pressing and roll pressing.

[0092] Non-aqueous electrochemical devices The non-aqueous electrochemical device disclosed herein has the electrodes of this disclosure.

[0093] The non-aqueous electrochemical device disclosed herein can be a non-aqueous battery or a non-aqueous capacitor. The non-aqueous battery can be a non-aqueous primary battery or a non-aqueous secondary battery, preferably a non-aqueous secondary battery, and more preferably a non-aqueous lithium-ion secondary battery.

[0094] In addition to electrodes, the non-aqueous electrochemical device disclosed herein may also include an electrolyte, outer packaging material, and a separator. The non-aqueous electrochemical device of this disclosure has, for example, a structure in which a battery element, with a negative electrode and a positive electrode facing each other separated by a separator, is encapsulated together with the electrolyte within an outer packaging material.

[0095] (Electrolyte) The electrolyte is preferably a solution obtained by dissolving a lithium salt in a non-aqueous solvent. Examples of lithium salts include LiPF6, LiBF4, and LiClO4. Examples of non-aqueous solvents include cyclic carbonates such as ethylene carbonate, propylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, and vinylene carbonate; chain carbonates such as dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, and their fluorinated derivatives; cyclic esters such as γ-butyrolactone and γ-valerolactone; etc. These can be used alone or in combination.

[0096] As an electrolyte, a solution obtained by mixing cyclic carbonates and chain carbonates at a mass ratio (cyclic carbonate: chain carbonate) of 20:80 to 40:60 and dissolving lithium salts in the range of 0.5 mol / L to 1.5 mol / L is suitable.

[0097] (Outer packaging materials) Examples of packaging materials include aluminum laminate packaging, metal casings, and button batteries.

[0098] (Diaphragm) The diaphragm can be any known diaphragm, for example, a composite membrane having a porous substrate and a porous layer disposed on one or both sides of the porous substrate, or a single-layer membrane of the porous substrate itself.

[0099] -Porous substrate- In this disclosure, a porous substrate refers to a substrate having pores or voids within its structure. Examples of such substrates include microporous membranes; porous sheets such as nonwoven fabrics and paper formed from fibrous materials; and so on. The preferred material for the porous substrate is a material with electrical insulating properties.

[0100] To impart a shut-off function to the porous substrate, the porous substrate preferably comprises a thermoplastic resin. The shut-off function refers to the function that, when the battery temperature rises, the constituent material melts and blocks the pores of the porous substrate, thereby blocking ion migration and preventing thermal runaway of the battery. As a thermoplastic resin, a thermoplastic resin with a melting point of less than 200°C is preferred. Examples of thermoplastic resins include polyesters such as polyethylene terephthalate; polyolefins such as polyethylene and polypropylene; etc., with polyolefins being preferred.

[0101] -Porous layer- A porous layer is a layer disposed on one or both sides of a porous substrate, having numerous gaps or micropores, allowing gas or liquid to pass through from one side to the other. The porous layer preferably contains at least one of inorganic particles and a binder resin. A porous layer can also be a structure composed of multiple porous layers stacked together.

[0102] Examples of inorganic particles include metal oxide particles such as alumina and boehmite, metal hydroxide particles such as aluminum hydroxide and magnesium hydroxide, metal sulfate particles such as barium sulfate, metal carbonate particles such as calcium carbonate, metal nitride particles such as boron nitride, and clay mineral particles such as talc.

[0103] As an adhesive resin, it can be any resin selected from those soluble in polar solvents, soluble in water, and dispersible in water. Examples of adhesive resins include polyamides, polyimides, polyamide-imides, fluorinated resins, acrylic resins, styrene-butadiene copolymers, and butadiene-acrylonitrile resins. These resins can be used alone or in combination of two or more.

[0104] <Method for manufacturing non-aqueous electrochemical devices disclosed herein> There are no particular limitations on the manufacturing method of the non-aqueous electrochemical device disclosed herein, and known methods can be applied. For example, it can be manufactured as follows: a laminate with a diaphragm disposed between the positive and negative electrodes is manufactured, the laminate is then placed in an outer packaging material, an electrolyte is injected, and the outer packaging material is sealed.

[0105] When manufacturing a laminate with a separator disposed between the positive and negative electrodes, the separator can be disposed between the positive and negative electrodes in a manner that involves stacking the positive electrode, separator, and negative electrode at least one layer in sequence (so-called stacking method), or in a manner that involves overlapping the positive electrode, separator, negative electrode, and separator in sequence and winding them in the length direction.

[0106] The non-aqueous electrochemical device disclosed herein can be any shape, such as coin-shaped, button-shaped, sheet-shaped, cylindrical, square, or flat.

[0107] Example The following examples further illustrate the binder polymer, binder composition, electrode composition, electrode, non-aqueous electrochemical device, and non-aqueous secondary battery of this disclosure. The materials, amounts, proportions, and processing steps shown in the following examples may be appropriately modified without departing from the spirit of this disclosure. Therefore, the scope of the binder polymer, binder composition, electrode composition, electrode, non-aqueous electrochemical device, and non-aqueous secondary battery of this disclosure should not be interpreted limitingly based on the specific examples shown below.

[0108] Unless otherwise specified, synthesis, processing, and manufacturing shall be carried out at room temperature (25℃±3℃) in the following instructions.

[0109] <Preparation of Adhesive Polymers> (Example 1) In a 1L separable flask, 449.54 parts by mass of deoxygenated ion-exchanged water (purged with nitrogen), 0.05 parts by mass of concentrated sulfuric acid (as a pH adjuster), and 0.0005 parts by mass of ferric sulfate (II) (as a catalyst) were added. The flask was stirred to create a nitrogen atmosphere, and then immersed in a hot water bath adjusted to 50°C. 49.50 parts by mass of acrylonitrile (monomer 1) and 0.50 parts by mass of itaconic acid (monomer 2) were added. Once the internal temperature of the flask reached 48°C or higher, 0.37 parts by mass of a 50% aqueous solution of ammonium bisulfite and 0.15 parts by mass of ammonium persulfate (as polymerization initiators) were added. The flask was kept at 50°C for 1 hour to carry out the polymerization reaction. After the reaction was complete, white particles were filtered from the reaction mixture, thoroughly washed with ion-exchanged water, and dried overnight at 70°C in an electric drying oven to obtain the binder polymer. The copolymer composition of the obtained binder polymer is 99.6 mol% acrylonitrile and 0.4 mol% itaconic acid, which is the same as the loading ratio when converted by mass.

[0110] (Examples 2 to 5 and Comparative Examples 1 to 5) The composition of monomer (1) and monomer (2) was changed as shown in Table 1. Otherwise, the adhesive polymers of Examples 2 to 5 and Comparative Examples 1 to 5 were obtained by the same method as in Example 1.

[0111] (Comparative Example 6 and Comparative Example 7) As shown in Table 2, the compositions of monomers (1) and (2) were changed, and the polymerization reaction time was changed to a longer time. Otherwise, the binder polymers of Comparative Examples 6 and 7 were obtained by the same method as in Example 1.

[0112] <Evaluation of Adhesive Polymers> [Dissolution rate of binder polymer in solvent] To a bottle containing 85 parts by weight of N-methyl-2-pyrrolidone as a solvent, 15 parts by weight of the binder polymer powders from Examples 1-5 and Comparative Examples 1-5 were added respectively. The sealed bottle was rotated at 25°C to mix, resulting in binder polymer solutions. The time required for mixing until no undissolved residue was visible was defined as the dissolution time, and the dissolution rate was evaluated on a four-level scale according to the following criteria.

[0113] A: Dissolution time is less than 1 day.

[0114] B: The dissolution time is more than 1 day but less than 7 days.

[0115] C: The dissolution time is more than 7 days but less than 14 days.

[0116] D: The dissolution time is more than 14 days.

[0117] The dissolution rates are shown in Table 1. The binder polymers of Examples 1 to 5 exhibited excellent dissolution rates in the solvent.

[0118] [Swelling of binder polymers caused by electrolyte] The above-mentioned binder polymer solution was cast onto glass plates and dried to produce 4 cm square cast films. The mass of the cast films was measured under a drying environment of 25°C. The cast films were then immersed in the electrolyte in a container and the container was sealed. After 72 hours, the cast films were lifted, the adhering liquid was wiped off, and the mass was measured again. The electrolyte used was 1 M (mol / L) LiPF6-ethylene carbonate / methyl ethyl carbonate (=3 / 7 [mass ratio]). The value of (mass after immersion) / (mass before immersion) was used as the swelling degree, and the swelling was evaluated according to the following four-level criteria.

[0119] A: The degree of swelling is less than 1.1.

[0120] B: The degree of swelling is greater than 1.1 and less than 1.2.

[0121] C: The degree of swelling is greater than 1.2 and less than 1.3.

[0122] D: The degree of swelling is 1.3 or higher.

[0123] The swelling results are shown in Table 1. The binder polymers of Examples 1 to 5 exhibit excellent low swelling due to electrolyte.

[0124] [Weight-average molecular weight of the binder polymer] The weight-average molecular weight of the binder polymer was determined by gel permeation chromatography (GPC). A GPC apparatus (Tosoh Corporation HPLC-8320GPC EcoSEC) was used. A TSK gel α-M column (Tosoh Corporation) was used, and a differential refractive index detector (Tosoh Corporation HLC-8320 GPC RI detector) was used. For the mobile phase, dimethylformamide was used as the eluent, with lithium bromide and phosphoric acid added at 50 mM and 10 mM, respectively. Polystyrene (Tosoh Corporation Standard Polystyrene Kit PStQuick Kit-C, D) was used as the standard.

[0125] The results of the weight-average molecular weight determination are shown in Table 2.

[0126] <Preparation of Electrode Composition> 94 parts by weight of lithium cobalt oxide (LiCoO2) powder as the positive electrode active material, 3 parts by weight of acetylene black as the conductive additive, 3 parts by weight of the above-mentioned binder polymer, and an appropriate amount of N-methyl-2-pyrrolidone as the solvent are mixed to prepare positive electrode compositions.

[0127] Evaluation of Electrode Compositions [Coating properties of the electrode composition] The obtained positive electrode composition was coated onto a 20 μm thick aluminum foil using a roller coater and then dried to obtain a positive electrode film. The coating surface of the positive electrode film with a width of 100 mm and a length of 500 mm was visually inspected, and the coating performance was evaluated on a four-level scale according to the following criteria. It should be noted that when the coating performance of the electrode composition is low, uneven film thickness occurs on the coating film, which can be observed as uneven density in appearance.

[0128] A: The coating surface is generally homogeneous, and no unevenness in concentration was detected.

[0129] B: Uneven color distribution was confirmed in an area of ​​less than 1 / 16 of the overall coating surface.

[0130] C: Uneven color distribution was confirmed in an area of ​​more than 1 / 16 but less than 1 / 8 of the overall coating surface.

[0131] D: Uneven color distribution was confirmed in more than 1 / 8 of the overall coating surface area.

[0132] The coating properties are shown in Table 2. When the binder polymers of Examples 1 to 5 of this disclosure with a weight-average molecular weight of 450,000 or less were used in the electrode compositions, the coating properties were good. On the other hand, when polymers with a weight-average molecular weight greater than 450,000 were used in the electrode compositions, the coating properties of Comparative Examples 6 and 7 were poor.

[0133] Fabrication of Non-Aqueous Electrochemical Devices (Examples 6 to 10) The positive electrode films obtained in the above-mentioned "Electrode Composition Evaluation" and which respectively used the binder polymers of Examples 1 to 5 were further pressed to form a positive electrode. Additionally, lithium metal foil was used as the negative electrode. A polyethylene microporous membrane (8 μm thick, 36% porosity) was sandwiched between the positive and negative electrodes as a separator. After placing a button battery as the outer packaging material inside, an electrolyte was injected and the battery was sealed, thereby obtaining a non-aqueous lithium-ion secondary battery (one type of non-aqueous electrochemical device of this disclosure). The electrolyte used was 1 M (mol / L) LiPF6-ethylene carbonate / ethyl methyl carbonate (=3 / 7 [mass ratio]). Furthermore, all these button battery fabrication operations were carried out under an Ar atmosphere.

[0134] [Performance of non-aqueous lithium-ion secondary batteries] The performance of non-aqueous lithium-ion secondary batteries is evaluated using the capacity utilization rate, which is the ratio of the battery's 0.2C constant current discharge capacity to the intrinsic capacity of lithium cobalt oxide (150 mAh / g). The discharge cutoff voltage is set to 2.5V. It should be noted that charging is performed at 0.2C and 4.2V constant current / constant voltage.

[0135] The results are shown in Table 3. The capacity utilization rates of the non-aqueous lithium-ion secondary batteries in Examples 6 to 10 were 95.8%, 95.1%, 96.3%, 96.5%, and 95.9%, respectively. That is, the non-aqueous lithium-ion secondary batteries in Examples 6 to 10 fully utilized the capacity of lithium cobalt oxide and can be used as non-aqueous lithium-ion secondary batteries in practical applications.

[0136] [Table 1] [Table 2] [Table 3] As can be seen from the above, the binder polymers of Examples 1 to 5 are binder polymers that, based on a good standard, balance fast dissolution rate in solvents and low swelling caused by electrolytes, and can produce compositions with excellent coatability. In the non-aqueous electrochemical devices of Examples 6 to 10, the capacity utilization rate is also excellent.

[0137] It should be noted that the entire contents of the publication text of Japanese Patent Application No. 2024-074124, filed on April 30, 2024, are incorporated herein by reference. Furthermore, all documents, patent applications, and technical standards described in this specification are incorporated herein by reference to the same extent as they are specifically and separately described.

Claims

1. An electrode binder polymer for non-aqueous electrochemical devices, comprising a structural unit comprising at least one monomer (1) derived from acrylonitrile and methacrylonitrile, and a structural unit comprising at least one monomer (2) derived from the group consisting of unsaturated carboxylic acids, alkyl esters of unsaturated carboxylic acids, and amides of unsaturated carboxylic acids. The content of structural units derived from the monomer (2) is 0.1 mol% to 4.9 mol% relative to the total amount of structural units derived from the monomer (1) and structural units derived from the monomer (2). The polymer has a weight-average molecular weight of 10,000 to 450,000.

2. The electrode binder polymer for the non-aqueous electrochemical device as described in claim 1, wherein, The unsaturated alkyl carboxylic acid ester is at least one of methyl acrylate and methyl methacrylate.

3. The electrode binder polymer for non-aqueous electrochemical devices as described in claim 1 or 2, wherein, The unsaturated carboxylic acid is at least one selected from the group consisting of acrylic acid, methacrylic acid, and itaconic acid.

4. The electrode binder polymer for non-aqueous electrochemical devices as described in claim 1 or 2, wherein, The monomer (2) has 5 or fewer carbon atoms.

5. An electrode binder composition for a non-aqueous electrochemical device, comprising the electrode binder polymer for a non-aqueous electrochemical device as described in claim 1 or 2.

6. The electrode binder composition for a non-aqueous electrochemical device as described in claim 5, further comprising a solvent.

7. An electrode composition for a non-aqueous electrochemical device, comprising an active material and an electrode binder polymer for a non-aqueous electrochemical device as described in claim 1 or 2.

8. The electrode composition of the non-aqueous electrochemical device as described in claim 7, wherein, The active material is a positive electrode active material.

9. An electrode for a non-aqueous electrochemical device comprising the electrode composition of the non-aqueous electrochemical device according to claim 7.

10. A non-aqueous electrochemical device comprising the electrodes of the non-aqueous electrochemical device of claim 9.

11. A non-aqueous secondary battery comprising the electrodes of the non-aqueous electrochemical device of claim 9.

Citation Information

Patent Citations

  • Slurry composition for electrode, electrode, and lithium ion secondary battery

    JP2003132893A

  • Slurry composition for electrode, electrode and secondary battery

    JP2004185826A

  • Information processing device and program

    JP2024074124A