Electrode and secondary battery including the same

By setting a specific slope at the end of the electrode layer of the lithium secondary battery and removing the sliding part, the problem of capacity balance reversal caused by the sliding phenomenon in the lithium secondary battery is solved, the cycle characteristics and stability of the battery are improved, and more efficient is achieved charging and discharging performance.

CN221861688UActive Publication Date: 2024-10-18LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202290000523.4
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Priority Date
2021-12-24
Filing Date
2022-12-23
Publication Date
2024-10-18
Estimated Expiration
2032-12-23

AI Technical Summary

Technical Problem

The electrodes of existing lithium secondary batteries have sliding phenomena during charging and discharging, which causes the capacity balance between the positive electrode and the negative electrode to be reversed, making it difficult to control and affecting the stability and performance of the battery.

Method used

By setting a slope of 80°-90° at the end of the electrode layer and using laser ablation to remove the sliding part to form an end part of 10mm or smaller, the height difference of the electrode layer is reduced and the sliding phenomenon is prevented.

Benefits of technology

It effectively suppresses Li deposition and overvoltage phenomena, improves the cycle characteristics of the electrode and the stability of the battery, prevents the reversal of the capacity balance between the positive electrode and the negative electrode, and improves the service life and charging efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221861688U_ABST
    Figure CN221861688U_ABST
Patent Text Reader

Abstract

An electrode and a method of manufacturing the same are disclosed. The electrode comprises a current collector; and an electrode layer located on at least one surface of the current collector, and an uncoated portion having no electrode layer, in which a vertical cross-section of the electrode layer is provided with a middle portion of the electrode layer and end portions extending from both side portions of the middle portion of the electrode layer and contacting the current collector while a height of the electrode layer decreases, an end portion of the electrode layer has a gradient of 80 DEG to 90 DEG, and the gradient of the end portion indicates an angle formed between a tangent line at a boundary point at which the end portion of the electrode layer contacts the current collector and one surface of the current collector facing the electrode layer.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims priority to Korean Patent Application No. 10-2021-0187849 filed in Korea on December 24, 2021, the disclosure of which is incorporated herein by reference. Technical Field

[0002] The present disclosure relates to electrodes and methods for making electrodes. In particular, the present disclosure relates to electrodes and methods for making electrodes that facilitate long life and fast charging. Background Art

[0003] As technology develops and the need for mobile instruments increases, the demand for secondary batteries as energy sources has become increasingly greater, and thus active research has been conducted on batteries that can meet various needs.

[0004] This secondary battery can be roughly divided into a positive electrode, a negative electrode, a separator and an electrolyte. Lithium ions move back and forth between the two electrodes while being deintercalated from the positive electrode active material during the first charge, intercalated into the negative electrode active material, and then deintercalated during the subsequent discharge. Lithium secondary batteries can be recharged by converting energy using the above-mentioned process.

[0005] Generally, the electrode of a lithium secondary battery is prepared by dispersing an electrode active material, a binder, etc. to prepare an active material slurry and coating an active material layer on one surface of a current collector. When the active material slurry is coated on one surface of a current collector, a sliding phenomenon occurs in which the active material slurry spreads out. For this reason, a sliding portion having a smaller thickness than the middle portion is formed at the end of the active material layer. Specifically, the sliding portion may refer to a portion extending from each of the two ends of the middle portion and gradually decreasing in thickness toward the end of the active material layer, that is, from the middle portion of the active material layer to the portion of the uncoated portion without the active material layer. Due to this sliding phenomenon, the two ends of the active material layer have a lower load compared to the middle portion. Therefore, there is a problem that the secondary battery achieves a lower capacity compared to its designed capacity.

[0006] In addition, due to the above-mentioned sliding portion generated at the uncoated portion of the electrode end portion, the ratio of the positive electrode to the negative electrode may be reversed at the uncoated portion (joint portion) of the electrode, a physical gap may be generated and the sliding portion may be difficult to control, making it difficult to maintain stable electrode quality. Utility Model Content

[0007] Technical issues

[0008] The present disclosure is designed to solve the problems of the related art, and thus the present disclosure is directed to providing an electrode that is advantageous for long life and fast charging and a method for manufacturing the electrode.

[0009] Technical Solution

[0010] In one aspect of the present disclosure, an electrode and a method for manufacturing the electrode according to the following embodiments are provided.

[0011] According to a first embodiment of the present disclosure, an electrode is provided.

[0012] The electrode comprises: a current collector; an electrode layer, the electrode layer being disposed on at least one surface of the current collector; and an uncoated portion, the uncoated portion not having the electrode layer.

[0013] wherein a vertical cross section of the electrode layer is provided with a middle portion of the electrode layer and an end portion extending from each of two side portions of the middle portion of the electrode layer and contacting the current collector while the height of the electrode layer is reduced,

[0014] The electrode layer exhibits a slope of the end portion of 80°-90°, and

[0015] The slope of the end portion refers to an angle formed between a tangent line at a boundary point where the end portion of the electrode layer contacts the current collector and one surface of the current collector facing the electrode layer.

[0016] According to a second embodiment of the present disclosure, there is provided the electrode defined in the first embodiment,

[0017] Wherein, the electrode layer exhibits a slope of the end portion of 85°-90°.

[0018] According to a third embodiment of the present disclosure, there is provided the electrode defined in the first or second embodiment,

[0019] wherein the electrode layer has a length of the end portion of 10 mm or less,

[0020] The length of the end portion refers to the distance between the vertical downward point of the slope starting point relative to the current collector and the boundary point of the end portion of the electrode layer contacting the current collector,

[0021] And the slope starting point is the position on the end portion where an acute angle of 10° or more is first present when an acute angle formed by an extension line of the middle portion of the electrode layer and a tangent line on the end portion is measured along the end portion extending from the middle portion.

[0022] According to a fourth embodiment of the present disclosure,

[0023] There is provided a method for manufacturing an electrode defined according to the first to third embodiments, the method comprising the steps of: applying a slurry for an electrode layer to at least one surface of a current collector in such a manner that an uncoated portion can be formed adjacent to one end of an electrode current collector at a top end portion, and then drying to form an electrode layer;

[0024] pressing the electrode current collector having the electrode layer formed thereon; and

[0025] After pressing, a sliding portion of the electrode layer formed at the boundary portion is removed as the uncoated portion.

[0026] According to a fifth embodiment of the present disclosure, there is provided the method for manufacturing an electrode defined in the fourth embodiment,

[0027] Wherein, the sliding portion is removed by using laser ablation.

[0028] According to a sixth embodiment of the present disclosure, there is provided the method for manufacturing an electrode defined in the fifth embodiment,

[0029] Wherein, the laser ablation is performed by using a femtosecond laser.

[0030] According to a seventh embodiment of the present disclosure, there is provided the method for manufacturing an electrode defined in any one of the fourth to sixth embodiments,

[0031] Wherein, after pressing, or after pressing and groove forming, the sliding portion of the electrode layer is removed.

[0032] According to an eighth embodiment of the present disclosure, there is provided a method for manufacturing an electrode as defined in any one of the fourth to seventh embodiments,

[0033] wherein the sliding portion of the electrode layer is removed by 10 mm or less from a boundary with the uncoated portion.

[0034] According to a ninth embodiment of the present disclosure,

[0035] There is provided a secondary battery including the electrode defined in any one of the first to third embodiments.

[0036] According to a tenth embodiment of the present disclosure, there is provided the secondary battery defined in the ninth embodiment,

[0037] The secondary battery is a lithium secondary battery.

[0038] Beneficial Effects

[0039] According to an embodiment of the present disclosure, the electrode sliding portion generated at the uncoated portion provided at each of the two end portions of the electrode due to the slurry spreading phenomenon caused by the wet coating of the electrode layer is removed, thereby preventing the reversal phenomenon of the capacity balance (N / P balance) between the positive electrode and the negative electrode. As a result, Li deposition that conventionally occurs in the sliding portion can be suppressed and the cycle characteristics of the secondary battery using the electrode can be improved. In addition, according to an embodiment of the present disclosure, the physical distance between the positive electrode layer and the negative electrode layer is reduced, so that the overvoltage phenomenon can be reduced by preventing the lithium ion concentration gradient between the positive electrode and the negative electrode (i.e., the polarization phenomenon of the electrolyte concentration). BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The accompanying drawings illustrate preferred embodiments of the present disclosure and, together with the above disclosure, are used to provide a further understanding of the technical features of the present disclosure, and thus the present disclosure shall not be construed as being limited to the accompanying drawings.

[0041] Figure 1 is a schematic diagram illustrating an electrode according to the related art.

[0042] Figure 2 This is an example of a method for Figure 1 Graph showing the thickness variation of the electrode before and after pressing depending on the length of the electrode layer.

[0043] Figure 3 is a schematic diagram illustrating an electrode according to an embodiment of the present disclosure.

[0044] Figure 4 It is an example of an embodiment according to the present disclosure. Figure 3 Graph showing the thickness variation of the electrode before and after pressing depending on the length of the electrode layer.

[0045] Figure 5 The definition of the slope of the electrode end portion according to the embodiment of the present disclosure is illustrated.

[0046] Figure 6 The definition of the length of the electrode end portion according to the embodiment of the present disclosure is illustrated.

[0047] Figure 7 is a schematic diagram illustrating a method for manufacturing an electrode according to an embodiment of the present disclosure.

[0048] Figure 8 is a schematic cross-sectional view illustrating an electrode assembly according to the related art.

[0049] Fig. 9 is a schematic cross-sectional view illustrating an electrode assembly according to an embodiment of the present disclosure.

[0050] Fig.10 is a schematic cross-sectional view illustrating an electrode according to an embodiment of the present disclosure.

[0051] Fig.11 is a schematic cross-sectional view illustrating an electrode according to the related art.

[0052] Fig.12 is a graph illustrating the cycle characteristics of Example 1 and Comparative Example 1. DETAILED DESCRIPTION

[0053] Hereinafter, preferred embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. Before the description is made, it should be understood that the terms used in the specification and the appended claims should not be interpreted as limited to the common meanings and dictionary meanings, but are interpreted based on the meanings and concepts corresponding to the technical aspects of the present disclosure on the basis of the principle that allows the inventor to define terms suitable for the best description.

[0054] In the case of an electrode according to the related art, wet coating is performed on a current collector, and thus sliding portions are inevitably generated at both ends of the wet-coated electrode layer due to a slurry spreading phenomenon, which causes a reversal phenomenon of the capacity balance (N / P balance) between the positive electrode and the negative electrode in an electrochemical device using an electrode having such a sliding portion, thereby causing lithium (Li) deposition and degradation of the electrochemical device.

[0055] In order to solve the above-mentioned problems of electrodes according to the related art, the present disclosure provides an electrode,

[0056] The electrode comprises: a current collector; an electrode layer, the electrode layer being disposed on at least one surface of the current collector; and an uncoated portion, the uncoated portion having no electrode layer.

[0057] Herein, a vertical cross-section of the electrode layer is provided with a middle portion of the electrode layer and end portions extending from each of two side portions of the middle portion of the electrode layer and contacting the current collector while the height of the electrode layer is reduced.

[0058] The electrode layer exhibits a slope of 80-90° at the end portion, and

[0059] The slope of the end portion refers to an angle formed between a tangent line at a boundary point where the end portion of the electrode layer contacts the current collector and one surface of the current collector facing the electrode layer.

[0060] In other words, the electrode according to the present disclosure is characterized in that the sliding portion of the electrode (which causes the degradation of secondary battery performance, such as the reversal phenomenon of the capacity balance between the positive electrode and the negative electrode) is removed to minimize the difference between the capacity and height per unit area of ​​the middle portion of the electrode layer and the capacity and height per unit area of ​​the end portion of the electrode layer.

[0061] Figure 1 is a schematic diagram illustrating an electrode according to the related art, and Figure 2 This is an example of a method for Figure 1 Graph showing the thickness variation of the electrode before and after pressing depending on the length of the electrode layer.

[0062] Reference Figure 1 , an electrode 10 according to the related art is provided with an electrode layer 12 having a sliding portion S at an end portion and an uncoated portion 13 in which the electrode layer does not exist on one surface of a current collector 11 and the surface of the current collector is exposed.

[0063] Reference Figure 2 As can be seen from the thickness of the electrode layer depending on the length from the end portion of the electrode layer, before and after pressing, the length A of the electrode layer extending to the end portion of the electrode layer before pressing (while showing a decrease in the height of the middle portion of the electrode layer) is slightly reduced to the length B of the electrode layer extending to the end portion of the electrode layer after pressing (while showing a decrease in the height of the middle portion of the electrode layer). However, the length B is still significantly maintained. The region of the electrode layer corresponding to the length B becomes a sliding portion, which can cause performance degradation of the secondary battery.

[0064] also, Figure 3 is a schematic diagram illustrating an electrode according to an embodiment of the present disclosure, and Figure 4 It is an example of an embodiment according to the present disclosure. Figure 3 Graph showing the thickness variation of the electrode before and after pressing depending on the length of the electrode layer.

[0065] exist Figure 3 In the embodiment, after the sliding portion S of the electrode 10 according to the related art is removed by a method described below, the electrode 20 according to the embodiment of the present disclosure is provided with the electrode layer 22 and the uncoated portion 23 on one surface of the current collector 21 from which the sliding portion is removed.

[0066] Reference Figure 4, the electrode 20 provided with the electrode layer 22 with the sliding portion removed according to the embodiment of the present disclosure has substantially no length of the electrode layer extending to the end portion of the electrode layer compared to the length of the electrode layer before pressing, while showing a decrease in the height of the middle portion of the electrode layer after pressing. In other words, the electrode has an electrode layer extending substantially vertically from the height of the middle portion to its end portion without the sliding portion.

[0067] Figure 5 The definition of the slope of the electrode end portion according to the embodiment of the present disclosure is illustrated.

[0068] Reference Figure 5 According to an embodiment of the present disclosure, the electrode 20 includes: a current collector 21; and an electrode layer 22, which is arranged on at least one surface of the current collector 21; and an uncoated portion 23, which does not have an electrode layer, wherein a vertical cross-section of the electrode layer 22 is provided with a middle portion 22a and end portions 22b, 22c of the electrode layer, and the end portions 22b, 22c extend from each of the two side portions of the middle portion 22a of the electrode layer and contact the current collector while the height of the electrode layer is reduced.

[0069] Herein, the slope θ of the end portion refers to an angle formed between a tangent line L at a boundary point 24 where the end portion of the electrode layer contacts the current collector 21 and one surface of the current collector 21 facing the electrode layer.

[0070] In addition, the slope of the end portion of the electrode layer according to the present disclosure may be 80°-90°. According to an embodiment of the present disclosure, the slope of the end portion may be 85°-90°.

[0071] When the slope of the end portion of the electrode layer satisfies the range defined above, the reversal phenomenon of the capacity balance (N / P balance) between the positive electrode and the negative electrode can be prevented, Li deposition can be suppressed by calculating the electrolyte concentration generated at the sliding portion, the overvoltage and cycle characteristics of the secondary battery using the electrode can be improved, and the adhesion between the separator and the electrode at the end portion can be improved.

[0072] Reference Figure 6 According to an embodiment of the present disclosure, the electrode 20 includes: a current collector 21; and an electrode layer 22, which is arranged on at least one surface of the current collector 21; and an uncoated portion 23, which does not have an electrode layer, wherein a vertical cross-section of the electrode layer 22 is provided with a middle portion 22a and end portions 22b, 22c of the electrode layer, and the end portions 22b, 22c extend from each of the two side portions of the middle portion 22a of the electrode layer and contact the current collector while the height of the electrode layer is reduced.

[0073] Herein, the length d of the end portion of the electrode layer refers to the distance between the vertical downward point B of the slope starting point A relative to the current collector 21 and the boundary point C where the end portion of the electrode layer contacts the current collector, and the slope starting point A may be a position on the end portion where an acute angle α of 10° or more is firstly formed when the acute angle α formed by the extension line X of the middle portion of the electrode layer and the tangent line Y on the end portion is measured along the end portion extending from the middle portion of the electrode layer. In other words, the slope starting point may refer to a position on the end portion where an acute angle α of 10° or more is firstly formed when the acute angle α formed by the extension line X of the middle portion of the electrode layer and the tangent line Y at the optional position on the end portion is measured along the direction from the optional position on the end portion to the boundary point C, wherein the optional position on the end portion refers to a position where the height starts to decrease compared to the height of the electrode layer at the middle portion of the electrode layer. When the outer counter of the vertical cross section of the end portion has a curved shape and contacts the current collector, when the height of the electrode layer is reduced, the position on the end portion where an acute angle α of 10° or more is firstly formed may be determined while the optional point on the end portion is continuously changed. On the other hand, when the outer relative portion of the vertical cross-section of the end portion has a diagonal line or a vertical line shape having a predetermined angle of 10° or greater and is in contact with the current collector, as the height of the electrode layer decreases, the position on the end portion where the acute angle α of 10° or greater is first present may be the point where the diagonal line or vertical line shape starts.

[0074] The length of the end portion of the electrode layer according to the present disclosure may be 10 mm or less. According to an embodiment of the present disclosure, the length of the end portion of the electrode layer may be 4 mm-10 mm, 4 mm-7 mm, or 7 mm-10 mm.

[0075] When the end portion of the electrode layer satisfies the range defined above, the reversal phenomenon of the capacity balance (N / P balance) between the positive electrode and the negative electrode can be prevented, Li deposition can be suppressed by calculating the concentration of the electrolyte generated at the sliding portion, the overvoltage and cycle characteristics of the secondary battery using the electrode can be improved, and the adhesion between the electrode and the separator at the end portion can be improved.

[0076] According to the present disclosure, the electrode may be a positive electrode or a negative electrode, and the electrode layer may be a positive electrode active material layer or a negative electrode active material layer.

[0077] For example, when the electrode is a positive electrode, the active material contained in the positive electrode active material layer is a positive electrode active material such as a lithium-containing oxide, and a lithium-containing transition metal oxide can be preferably used. Specific examples of the lithium-containing transition metal oxide can include x (Ni a Co b Mn c)O2(0.5 < x < 1.3, 0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1), Li x FePO4(0.5 < x < 1.3), Li x CoO2(0.5 < x < 1.3), Li x NiO2(0.5 < x < 1.3), Li x MnO2(0.5 < x < 1.3), Li x Mn2O4(0.5 < x < 1.3), Li x Ni 1-y Co y O2(0.5 < x < 1.3, 0 < y < 1), Li x Co 1-y Mn y O2(0.5 < x < 1.3, 0 ≤ y < 1), Li x Ni 1-y Mn y O2(0.5 < x < 1.3, 0 ≤ y < 1), Li x (Ni a Co b Mn c )O4(0.5 < x < 1.3, 0 < a < 2, 0 < b < 2, 0 < c < 2, a + b + c = 2), Li x Mn 2-z Ni z O4(0.5 < x < 1.3, 0 < z < 2), Li x Mn 2-z Co z O4(0.5 < x < 1.3, 0 < z < 2) and Li x Any one or a mixture of two or more selected from the group consisting of CoPO4(0.5 < x < 1.3). Additionally, the lithium-containing transition metal oxide may be coated with a metal such as aluminum (Al) or a metal oxide. Additionally, sulfides, selenides, and halides may be used in addition to the lithium-containing transition metal oxide.

[0078] For example, when the electrode is the negative electrode, specific examples of the negative electrode active material contained in the active material layer include: carbon such as non-graphitizable carbon or graphite-like carbon; such as Li x Fe2O3(0 ≤ x ≤ 1), Li x WO2(0 ≤ x ≤ 1) and Sn x Me 1- x Me’ y O zMetal composite oxides such as (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, Group I, Group II and Group III elements in the periodic table, halogens; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8); lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; silicon oxides such as SiO, SiO / C and SiO2; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4 and Bi2O5; conductive polymers such as polyacetylene; Li-Co-Ni type materials, etc.

[0079] The electrode according to an embodiment of the present disclosure may include: a current collector; and an active material layer disposed on at least one surface of the current collector and formed by stacking an active material paste containing an active material, a conductive material, and a binder; and an uncoated portion that does not have an active material layer.

[0080] According to an embodiment of the present disclosure, the electrode may be a positive electrode, and the active material may be a positive electrode active material. In this case, the positive electrode current collector may be formed to have a thickness of about 3 μm-50 μm. The positive electrode current collector is not particularly limited as long as it has high conductivity without causing any chemical changes in the corresponding battery. Specific examples of positive electrode current collectors include stainless steel, aluminum, nickel, titanium, carbon electrodes, aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. In addition, fine surface unevenness may be formed on the surface of the current collector to enhance the binding force with the positive electrode active material. The current collector may be used in various shapes including films, sheets, foils, nets, porous bodies, foams, non-woven fabrics, etc. In addition, according to the present disclosure, the conductive material contained in the active material layer is generally added in an amount of 0.2 wt%-5 wt% based on the total weight of the mixture including the positive electrode active material. The conductive material is not particularly limited as long as it has conductivity without causing any chemical changes in the corresponding battery. Specific examples of conductive materials include: graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black or thermal black; conductive fibers such as carbon fibers or metal fibers; fluorocarbons; metal powders such as aluminum powder or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium dioxide; and conductive materials such as polyphenylene derivatives. In addition, the binder contained in the active material layer is a component that helps the active material to bind to the conductive material and to the current collector, and the usual addition amount is 0.2 wt % to 5 wt % based on the total weight of the slurry including the positive active material. Specific examples of binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, various copolymers, etc.

[0081] For example, when the electrode is a negative electrode, the negative electrode current collector is not particularly limited as long as it has high conductivity and does not cause any chemical changes in the corresponding battery. Specific examples of negative electrode current collectors include copper, stainless steel, aluminum, nickel, titanium, carbon electrodes, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. In addition, the negative electrode current collector may generally have a thickness of 3μm-50μm. Similar to the positive electrode current collector, surface roughness may be formed on the surface of the current collector to enhance the binding force with the negative electrode active material. For example, the negative electrode current collector may be used in various shapes including films, sheets, foils, nets, porous bodies, foams, non-woven fabrics, etc. In addition, the conductive material and binder contained in the active material layer are the same as those described above with reference to the positive electrode.

[0082] In another aspect of the present disclosure, there is provided a method for manufacturing an electrode, the method comprising the following steps:

[0083] applying a slurry for an electrode layer to at least one surface of a current collector in such a manner that an uncoated portion may be formed adjacent to one end of the electrode current collector at a top end portion, and then drying to form an electrode layer;

[0084] pressing the electrode current collector having the electrode layer formed thereon; and

[0085] After pressing, the sliding portion of the electrode layer formed at the boundary portion is removed as an uncoated portion.

[0086] In the following, reference will be made to Figure 3 A method for producing an electrode is described in detail.

[0087] First, a slurry for an electrode layer is applied to at least one surface of the current collector 11 in such a manner that the uncoated portion 13 can be formed adjacent to one end of the electrode current collector 11 at the top end portion, and then dried to form the electrode layer 12. The electrode layer 12 is provided with a sliding portion S in a region connected to the uncoated portion 13, and the sliding portion S extends to an end portion of the electrode layer contacting the uncoated portion while the height of the electrode layer 12 is reduced compared to that of the middle portion.

[0088] Next, the electrode current collector having the electrode layer is pressed. Herein, any pressing process may be used as long as it is a pressing process performed for a conventional electrode. The thickness of the electrode layer may be controlled to a desired level through the pressing process.

[0089] Then, after pressing, the sliding portion S of the electrode layer formed at the boundary between the uncoated portion (ie, the portion of the current collector without the electrode layer) and the current collector is removed. The sliding portion extends from each of the two end portions of the middle portion of the electrode layer, and refers to a portion (ie, an inclined portion) whose thickness gradually decreases toward the uncoated portion without the electrode layer.

[0090] The sliding portion may be removed by using various etching processes conventionally used as long as such processes do not cause physical / chemical changes in the remaining electrode layer.

[0091] According to an embodiment of the present disclosure, the sliding portion may be removed by using laser ablation.

[0092] Herein, laser ablation refers to the removal of the portion where the light is concentrated by focusing a laser beam onto a sample using a high-output pulsed laser. Figure 3 , the sliding portion can be removed by performing such laser ablation.

[0093] Laser ablation can be practiced by using a femtosecond laser.

[0094] Femtosecond laser refers to a laser with a power of several hundred femtoseconds (10 -15 When laser processing is performed using such short pulse width and high peak output characteristics of a femtosecond laser, the time of the irradiated laser pulse is shorter than the thermal diffusion time of the material to be processed, thus allowing non-thermal processing without causing thermal degradation of the material. In addition, compared with conventional continuous wave or nanosecond lasers, femtosecond lasers achieve high peak output even with relatively small energy, so the impact applied to the electrode to be processed is small, allowing ultra-precision fine processing, and can remove fine cracks or burr formation in the electrode. In addition, there is no shock wave and surface deformation.

[0095] When laser ablation is performed as mentioned above to prevent the quality and function of the electrode from deteriorating, the output wavelength of the laser beam may be 500nm-1080nm or 800nm-1030nm. In addition, the repetition ratio of the laser beam may be 300kHz-1000kHz, and the output may be 10W-100W. When the processing conditions exceed the range defined above, it is difficult to control the processing, so the electrode collector may dissolve. When the processing conditions are less than the range defined above, there is a problem that the electrode layer at the sliding portion may not be removed.

[0096] According to an embodiment of the present disclosure, the sliding portion of the electrode layer may be removed after pressing or after pressing and notching.

[0097] In other words, after applying the slurry for the electrode layer to the current collector and then drying to form the electrode layer, and then performing a pressing process to obtain the electrode layer of a predetermined height, or after performing a pressing process and then performing a groove step to form the uncoated portion as a joint portion, the sliding portion of the electrode layer can be removed.

[0098] Reference Figure 7 , the electrode 10 according to the present disclosure is obtained by the following steps: a slurry for an electrode layer is applied to at least one surface of a current collector 11 in such a manner that an uncoated portion 13 can be formed adjacent to one end of an electrode current collector 11 at a top portion, and then dried to form an electrode layer 12 having a sliding portion S. Herein, the uncoated portion 13 can be formed as a joint portion by grooving. Then, an etching process such as laser ablation is performed to obtain an electrode 20, which includes an electrode layer 22 from which a sliding portion is removed on one surface of the current collector 11 and an uncoated portion also serving as a joint portion 13 extending from the electrode layer.

[0099] According to an embodiment of the present disclosure, when the sliding portion of the electrode layer is removed, the sliding portion may be removed by 10 mm from a boundary between an uncoated portion before the sliding portion is removed and an end portion of the sliding portion.

[0100] After removing the sliding portion of the electrode layer by 10 mm from the boundary between the uncoated portion before removing the sliding portion and the end of the sliding portion, adhesion between the electrode and the separator at the end portion can be improved.

[0101] After the sliding portion is removed by laser ablation, the thickness difference between the middle portion of the electrode layer and the end portion thereof may be 3 μm or less, or the slope of the end portion of the electrode layer may be 80°-90°, wherein the slope of the end portion refers to the angle formed between the surface of the current collector and a straight line connecting a boundary point where the end portion of the electrode layer contacts the current collector and an inflection point where the height of the middle portion begins to decrease and connects to the end portion.

[0102] According to an embodiment of the present disclosure, when etching residues remain in the end portion of the electrode layer, etc. after laser ablation (laser etching) is performed, a step of removing the etching residues may be further performed after removing the sliding portion by using laser ablation. For example, the etching residues may be removed by blowing air toward the end region of the electrode layer with a compressor, etc.

[0103] In another aspect of the present disclosure, a secondary battery is provided, the secondary battery including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the positive electrode or the negative electrode is the same electrode as defined according to the embodiment of the present disclosure.

[0104] The separator used in combination with the electrode according to the present disclosure is not particularly limited. The separator is between the positive electrode and the negative electrode to separate them from each other, and includes an insulating film with high ion permeability and mechanical strength. Any separator can be used without particular limitation, as long as it is a separator commonly used in secondary batteries. Specific examples of separators include porous polymer films such as porous polymer films made of ethylene homopolymers, propylene homopolymers, ethylene / butene copolymers, ethylene / butene copolymers, ethylene / hexene copolymers, ethylene / methacrylate copolymers, etc., or a laminated structure of two or more layers of such porous polymer films. In addition, conventional porous nonwoven fabrics such as nonwoven fabrics made of high melting point glass fibers, polyethylene terephthalate fibers, etc. can be used.

[0105] In addition, a separator coated with inorganic particles, a binder polymer, or a mixture of inorganic particles and a binder polymer may be used optionally in the form of a single layer structure or a multilayer structure to ensure heat resistance and mechanical strength. In addition, when a solid electrolyte such as a polymer is used as an electrolyte, the solid electrolyte may also be used as a separator.

[0106] Figure 8 is a schematic cross-sectional view illustrating an electrode assembly according to the related art, and Fig. 9 is a schematic cross-sectional view illustrating an electrode assembly according to an embodiment of the present disclosure.

[0107] Reference Figure 8 and Fig. 9 , the electrode assembly 30 according to the related art includes a separator 33 between a positive electrode 31 and a negative electrode 32, the negative electrode 32 being provided with a sliding portion S of an electrode layer. In addition, the electrode assembly 40 according to an embodiment of the present disclosure includes a separator 43 between a negative electrode 42 and a positive electrode 41, the positive electrode 41 including an electrode layer from which a sliding portion is removed and having a slope of an end portion of the electrode layer of 80°-90°.

[0108] and Figure 8 In comparison, Fig. 9 In the electrode assembly shown in , sliding is improved to provide improved adhesion between the separator and the electrode, suppress the reversal phenomenon of the capacity balance (N / P balance) between the positive electrode and the negative electrode, and suppress overvoltage, thereby suppressing deposition and side reactions at the end portion or the top portion.

[0109] Specifically, the suppression of overvoltage is a phenomenon caused by the improvement of close adhesion between the electrode and the separator and the reduction of the physical distance between the positive electrode and the negative electrode. When a lithium ion concentration gradient is generated between the positive and negative electrodes and the lithium ion concentration decreases, the ionic conductivity decreases, thereby causing an increase in resistance and the generation of overvoltage.

[0110] Fig.10 is a schematic cross-sectional view illustrating an electrode according to an embodiment of the present disclosure.

[0111] Reference Fig.10 The electrode 50 according to the embodiment of the present disclosure is provided with an electrode layer 52, which is provided on the current collector 51, and the end portion 52e of the electrode layer has a slope of the end portion of 80°-90°. In addition, the end portion 52e of the electrode layer according to the embodiment of the present disclosure can be basically provided with a flat surface (etched surface) removed by using laser ablation (laser etching).

[0112] also, Fig.11is a schematic cross-sectional view illustrating an electrode according to the related art. According to the related art, the sliding portion of the end portion of the electrode can be removed by applying a mechanical force (for example, by attaching a tape to the sliding portion and tearing it off). In other words, the electrode 60 according to the related art is provided with an electrode layer 62, which is provided on the current collector 61, but it is removed by tearing off the end portion 62e of the electrode layer with the help of the adhesion of the tape. As a result, the shape of the active material remaining in the end portion 62e after tearing off is directly reflected to the end portion, so the end portion basically has surface unevenness.

[0113] According to the present disclosure, the secondary battery may be a lithium secondary battery, including a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.

[0114] Hereinafter, examples will be described more fully so that the present disclosure can be easily understood. However, the following examples can be implemented in many different forms and should not be understood as being limited to the exemplary embodiments set forth herein. Rather, these exemplary embodiments are provided so that the present disclosure will be thorough and complete, and the scope of the present disclosure will be fully conveyed to those skilled in the art.

[0115] Example 1

[0116] LiCoO2, carbon black, and polyvinylidene fluoride (PVDF) as positive electrode active materials were introduced into N-methylpyrrolidone (NMP) at a weight ratio of 98:1:1 and mixed therein to prepare a positive electrode slurry. Then, the positive electrode slurry was heated to 18.7 mg / cm 2 A loading amount is applied to a current collector made of aluminum foil, followed by drying to form a positive electrode layer, and the current collector with the positive electrode layer is pressed to an electrode density of 4.0 g / cc. After pressing, a femtosecond laser device is used to remove the sliding portion of the electrode layer formed at the boundary portion with the uncoated portion under the conditions of a wavelength of 1030 nm, a repetition ratio of 200 kHz, and an output of 3 W. In this way, after removing the sliding portion, a positive electrode having a positive electrode layer end portion slope of 87° is obtained. In this article, the slope of the end portion of the positive electrode layer refers to the angle formed between the tangent at the boundary point where the end portion of the positive electrode layer contacts the current collector and a surface of the current collector facing the positive electrode layer.

[0117] Then, 96 parts by weight of artificial graphite as a negative electrode active material, 0.5 parts by weight of acetylene black as a conductive material, 1.0 parts by weight of carboxymethyl cellulose (CMC) as a thickener, and 2.5 parts by weight of styrene butadiene rubber (SBR) as a binder were added to water and mixed with water to prepare a negative electrode slurry. Next, the negative electrode slurry was stirred at 10.1 mg / cm based on dry weight.2 A loading amount of 1000 g / cm2 was applied to a copper (Cu) current collector, followed by drying to form a negative electrode layer, and the current collector with the negative electrode layer was pressed to an electrode density of 1.7 g / cc. After pressing, a femtosecond laser device was used to remove the sliding portion of the negative electrode layer formed at the boundary portion with the uncoated portion under the conditions of a wavelength of 1070 nm, a repetition ratio of 500 kHz, and an output of 10 W. In this way, after removing the sliding portion, a negative electrode with a negative electrode layer end portion slope of 87° was obtained. Herein, the slope of the end portion of the negative electrode layer refers to the angle formed between the tangent at the boundary point where the end portion of the negative electrode layer contacts the current collector and a surface of the current collector facing the negative electrode layer.

[0118] Thereafter, the electrodes were stacked with the separator, the resulting structure was introduced into a pouch-type battery case, and an electrolyte was injected therein to obtain a battery. The electrolyte was prepared by mixing ethylene carbonate, propylene carbonate, ethyl propionate, and propyl propionate in a weight ratio of 2:1:2.5:4.5 and introducing LiPF6 at a concentration of 1.2 M therein.

[0119] Comparative Example 1

[0120] LiCoO2, carbon black, and PVDF as positive electrode active materials were introduced into NMP at a weight ratio of 98:1:1 and mixed therein to prepare a positive electrode slurry. Then, the positive electrode slurry was heated to 18.7 mg / cm 2 A loading amount of 200 g / cc was applied to a current collector made of aluminum foil, followed by drying to form a positive electrode layer, and the current collector with the positive electrode layer was pressed to an electrode density of 4.0 g / cc to obtain a positive electrode. Here, the slope of the end portion of the positive electrode layer was 60°.

[0121] Then, 96 parts by weight of artificial graphite as a negative electrode active material, 0.5 parts by weight of acetylene black as a conductive material, 1.0 parts by weight of carboxymethyl cellulose (CMC) as a thickener, and 2.5 parts by weight of styrene butadiene rubber (SBR) as a binder were added to water and mixed with water to prepare a negative electrode slurry. Next, the negative electrode slurry was stirred at 10.1 mg / cm 2 A loading amount of 1.7 g / cc was applied to a copper (Cu) current collector, followed by drying to form a negative electrode layer, and the current collector with the negative electrode layer was pressed to an electrode density of 1.7 g / cc to obtain a negative electrode. Herein, the slope of the end portion of the negative electrode layer was 60°.

[0122] Thereafter, the electrodes were stacked with the separator, the resulting structure was introduced into a pouch-type battery case, and an electrolyte was injected therein to obtain a battery. The electrolyte was prepared by mixing ethylene carbonate, propylene carbonate, ethyl propionate, and propyl propionate in a weight ratio of 2:1:2.5:4.5 and introducing LiPF6 at a concentration of 1.2 M therein.

[0123] <Evaluation of Room Temperature Cycle Characteristics>

[0124] The battery according to each of Example 1 and Comparative Example 1 was charged to 4.45 V in a constant current (CC) mode at 2.0 C and to a charge cutoff current of 0.005 C in a constant voltage (CV) mode, and discharged to 3 V in a constant current mode at 1 C. Such a charge / discharge cycle was repeated 500 times (500 cycles), and the capacity retention rate of each cycle was evaluated. The results are shown in FIG. Fig.12 The test was performed at room temperature (25°C).

[0125] The capacity retention rate of each battery was calculated from the results according to the following formula:

[0126] Capacity retention rate after Nth cycle (%) = (capacity at Nth cycle / initial capacity) × 100 (where N is 2-500)

[0127] Reference Fig.12 It can be seen that the battery according to Example 1 exhibits excellent cycle characteristics and maintains a capacity retention rate of about 93% or more compared to the initial capacity even after performing 500 charge / discharge cycles, while the battery according to Comparative Example 1 shows a capacity retention rate reduced to a level of 85% after performing 500 charge / discharge cycles.

Claims

1. An electrode, characterized in that: The electrode comprises: a current collector; an electrode layer, the electrode layer being disposed on at least one surface of the current collector; and an uncoated portion, the uncoated portion not having the electrode layer. wherein a vertical cross section of the electrode layer is provided with a middle portion of the electrode layer and an end portion extending from each of two side portions of the middle portion of the electrode layer and contacting the current collector while the height of the electrode layer is reduced, The electrode layer exhibits a slope of the end portion of 80°-90°, and The slope of the end portion refers to an angle formed between a tangent line at a boundary point where the end portion of the electrode layer contacts the current collector and one surface of the current collector facing the electrode layer. The electrode layer has a length of the end portion of 10 mm or less, The length of the end portion refers to the distance between the vertical downward point of the slope starting point relative to the current collector and the boundary point where the end portion of the electrode layer contacts the current collector, and The slope starting point is the position on the end portion where an acute angle of 10° or more is first present when an acute angle formed by an extension line of the middle portion of the electrode layer and a tangent line on the end portion is measured along the end portion extending from the middle portion.

2. The electrode according to claim 1, characterized in that The electrode layer exhibits a slope of the end portion of 85°-90°.

3. A secondary battery, characterized in that: The secondary battery comprises the electrode according to any one of claims 1 to 2.

4. The secondary battery according to claim 3, characterized in that: The secondary battery is a lithium secondary battery.