Puncture-resistant insulating film

By using a puncture-resistant insulating film prepared by a segmented coating process between cells/cells and cold plates, combined with an acrylic adhesive layer and a polyamide or high-density polyethylene puncture-resistant layer, the existing problem is solved The problem that the insulating film is easily punctured achieves the safety and reliability of high energy density and long endurance power battery packs.

CN221876933UActive Publication Date: 2024-10-22CYBRID TECHNOLOGIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202322901063.1
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-10-27
Publication Date
2024-10-22
Estimated Expiration
2033-10-27

AI Technical Summary

Technical Problem

The existing double-sided tape insulation film used between cells/cells and cold plates is easily pierced by metal particles when squeezed, resulting in insulation failure and unable to meet the safety and reliability of high energy density and long endurance power battery packs. Require.

Method used

A puncture-resistant insulating film is designed, including a first glue layer, a first puncture-resistant layer, a second glue layer, a base material layer, a third glue layer and a fourth glue layer arranged in sequence from top to bottom. The acrylic adhesive layer and the polyamide or high-density polyethylene puncture-resistant layer are prepared through a segmented coating process to ensure the combination of bonding performance and puncture resistance.

Benefits of technology

It effectively improves the reliability and puncture resistance of the insulating film, maintains good insulation under the pressure of aluminum metal particles, and improves the safety and reliability of the battery pack.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221876933U_ABST
    Figure CN221876933U_ABST
Patent Text Reader

Abstract

The utility model relates to a puncture-resistant insulating film, and belongs to the technical field of insulating films. The puncture-resistant insulating film comprises a first adhesive layer, a first puncture-resistant layer, a second adhesive layer, a base material layer, a third adhesive layer, a second puncture-resistant layer and a fourth adhesive layer which are sequentially arranged from top to bottom. Through proper structural design, the puncture-resistant insulating film has a puncture-resistant function while ensuring a bonding effect, and the reliability of the insulating film can be effectively improved. And after a puncture resistance test of the aluminum metal particles, the aluminum alloy still has good insulativity. And when the adhesive is applied to bonding between battery cells / between the battery cells and a cold plate, the safety and reliability of the battery PACK can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model belongs to the technical field of insulating films, and in particular relates to a puncture-resistant insulating film. Background Art

[0002] At present, the demand for new energy power batteries at home and abroad continues to grow, production capacity continues to expand, and the market is huge. With the explosive growth of the market, people have higher and higher requirements for power battery components, requiring a single Pack to have a higher energy density and provide a longer mileage, which requires the Pack to be structurally optimized, thus gradually developing from CMP technology (cell-module-battery pack) to CTP (cell-battery pack), CTC (cell-cell) and CTB (cell-body) and other highly integrated technologies.

[0003] Regarding CTP technology, the optimized structural design involves large-area cold plate bonding, and new requirements are put forward for the structural bonding of the aluminum water-cooled plate and the battery cell interface. In the actual production process, there is a risk of metal particles between the cold plate and the battery cell. The existing insulating film for bonding does not have puncture resistance. When squeezed, metal particles will pierce the insulating film, causing insulation failure. Therefore, it is necessary to have an insulating film with puncture resistance to improve the safety and reliability of the Pack. Utility Model Content

[0004] To this end, the technical problem to be solved by the utility model is to overcome the problem that the double-sided tape insulating film used for bonding between battery cells / between battery cells and cold plates in the existing market only has a bonding function and cannot take into account the puncture resistance function, especially in the presence of foreign matter, when squeezed, it is easy to puncture the insulating film, resulting in insulation failure.

[0005] To solve the above technical problems, the utility model provides a puncture-resistant insulating film, comprising a first adhesive layer, a first puncture-resistant layer, a second adhesive layer, a substrate layer, a third adhesive layer, a second puncture-resistant layer and a fourth adhesive layer arranged in sequence from top to bottom.

[0006] In one embodiment of the present invention, the first adhesive layer, the second adhesive layer, the third adhesive layer and the fourth adhesive layer are independently selected from acrylic adhesive layers to provide bonding properties.

[0007] In one embodiment of the present invention, the raw materials for preparing the acrylic adhesive layer include, by mass, 80-100 parts of main adhesive, 1-20 parts of rosin-modified phenolic resin, 1-20 parts of terpene phenolic resin and 0.1-1 part of curing agent.

[0008] In one embodiment of the present invention, the curing agent is an isocyanate curing agent.

[0009] In one embodiment of the present invention, the thickness of the first adhesive layer, the second adhesive layer, the third adhesive layer and the fourth adhesive layer are independently 10 μm-50 μm.

[0010] Further, the thickness of the first glue layer, the second glue layer, the third glue layer and the fourth glue layer are independently 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 21μm, 22μm, 23μm, 24μm, 25μm, 26μm, 27μm, 28μm, 29μm, 30μm, 31μm, 32μm, 33μm, 34μm, 35μm, 36μm, 37μm, 38μm, 39μm, 40μm, 41μm, 42μm, 43μm, 44μm, 45μm, 46μm, 47μm, 48μm, 49μm, 50μm; or any thickness value between any two values.

[0011] In one embodiment of the present invention, the first puncture-resistant layer and the second puncture-resistant layer are independently selected from polyamide (PA) puncture-resistant layer and / or high-density polyethylene (HDPE) puncture-resistant layer to improve the puncture strength of the puncture-resistant insulating film.

[0012] In one embodiment of the present invention, the thickness of the first puncture-resistant layer and the second puncture-resistant layer are independently 25 μm-100 μm.

[0013] Further, the thickness of the first puncture-resistant layer and the second puncture-resistant layer are independently 25μm, 26μm, 27μm, 28μm, 29μm, 30μm, 31μm, 32μm, 33μm, 34μm, 35μm, 36μm, 37μm, 38μm, 39μm, 40μm, 41μm, 42μm, 43μm, 44μm, 45μm, 46μm, 47μm, 48μm, 49μm, 50μm, 51μm, 52μm, 53μm, 54μm, 55μm, 56μm, 57μm, 58μm, 59μm, 60μm, 61μm, or any thickness value between any two values.

[0014] In one embodiment of the present invention, the substrate layer is selected from a polyethylene terephthalate (PET) substrate layer, a polycarbonate (PC) substrate layer or a polyimide (PI) substrate layer.

[0015] In one embodiment of the present invention, the thickness of the substrate layer is 25 μm-150 μm.

[0016] Furthermore, the thickness of the substrate layer is 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 65μm, 70μm, 75μm, 80μm, 85μm, 90μm, 95μm, 100μm, 105μm, 110μm, 115μm, 120μm, 125μm, 130μm, 135μm, 140μm, 145μm, 150μm; or any thickness value between any two values.

[0017] In one embodiment of the present invention, the puncture-resistant insulating film is prepared by a segmented coating process to prepare a puncture-resistant insulating film with good puncture resistance.

[0018] In one embodiment of the present invention, the preparation of the puncture-resistant insulating film comprises the following steps:

[0019] S1, disposing a second adhesive layer and a third adhesive layer on both sides of the substrate layer to obtain a semi-finished product A;

[0020] A first adhesive layer is provided on the release surface of the release film, and a first puncture-resistant layer is attached thereto after drying to obtain a semi-finished product B;

[0021] A fourth adhesive layer is provided on the release surface of the release film, and the second puncture-resistant layer is laminated thereon after drying to obtain a semi-finished product C;

[0022] S2. Lay the first puncture-resistant layer of the semi-finished product B and the second puncture-resistant layer of the semi-finished product C on the second adhesive layer and the third adhesive layer of the semi-finished product A respectively to obtain a puncture-resistant insulating film.

[0023] In an embodiment of the present invention, the drying temperature is 50°C-130°C.

[0024] Further, the drying temperature is 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C, 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C, 95°C, 96°C, 97°C, 98°C, 99°C, 100°C, 101°C, 102°C, 103°C, 104°C, 105°C ℃, 5℃, 96℃, 97℃, 98℃, 99℃, 100℃, 101℃, 102℃, 103℃, 104℃, 105℃, 106℃, 107℃, 108℃, 109℃, 110℃, 111℃, 112℃, 113℃, 114℃, 115℃, 116℃, 117℃, 118℃, 119℃, 120℃, 121℃, 122℃, 123℃, 124℃, 125℃, 126℃, 127℃, 128℃, 129℃, 130℃; or any temperature value between any two values.

[0025] Compared with the prior art, the technical solution of the utility model has the following advantages:

[0026] The puncture-resistant insulating film of the utility model has a puncture-resistant function while ensuring the bonding effect through appropriate structural design, which can effectively improve the reliability of the insulating film. After the puncture resistance test of aluminum metal particles, it still has good insulation. When used for bonding between battery cells / battery cells and cold plates, it can effectively improve the safety and reliability of battery PACK. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to make the content of the utility model easier to understand, the utility model is further described in detail according to the specific embodiments of the utility model in combination with the accompanying drawings, wherein:

[0028] Figure 1 This is a schematic diagram of the structure of the puncture-resistant insulating film of the utility model;

[0029] Explanation of reference numerals: 1 - first adhesive layer, 2 - first puncture-resistant layer, 3 - second adhesive layer, 4 - substrate layer, 5 - third adhesive layer, 6 - second puncture-resistant layer, 7 - fourth adhesive layer. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0031] In the present utility model, unless otherwise specified, the terms "center", "longitudinal", "lateral", "upper", "lower", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present utility model and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present utility model. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present utility model, unless otherwise specified, "multiple" means two or more.

[0032] In the present invention, unless otherwise specified, the terms "disposed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.

[0033] In the present invention, unless otherwise specified, a thickness gauge is used to measure the thickness of the substrate layer, the puncture-resistant layer and the adhesive layer. The specific test standard refers to GB / T 7125-2014.

[0034] In the present invention, unless otherwise specified, the raw materials for preparing the acrylic adhesive layer in the embodiment are calculated by mass, including 90 parts of main adhesive (purchased from Changxing Chemical, brand 77307), 10 parts of rosin-modified phenolic resin (purchased from Sumitomo Chemical, brand PR-12603), 10 parts of terpene phenolic resin (purchased from Anyuan Chemical, brand TH130) and 0.5 parts of isocyanate curing agent (purchased from Covestro, brand L-75).

[0035] Example 1

[0036] Reference Figure 1 As shown, this embodiment provides a puncture-resistant insulating film, which includes a first adhesive layer 1, a first puncture-resistant layer 2, a second adhesive layer 3, a base material layer 4, a third adhesive layer 5, a second puncture-resistant layer 6 and a fourth adhesive layer 7 arranged in sequence from top to bottom;

[0037] The first adhesive layer 1 , the second adhesive layer 3 , the third adhesive layer 5 and the fourth adhesive layer 7 are all acrylic adhesive layers, which provide bonding performance.

[0038] The first puncture-resistant layer 2 and the second puncture-resistant layer 6 are both PA puncture-resistant layers (purchased from Xiamen Changsu, model OA1), which improve the puncture strength of the puncture-resistant insulating film.

[0039] The substrate layer 4 is a PET substrate layer (purchased from Shaoxing Xiangyu, model number PD-XY).

[0040] The preparation method of the puncture-resistant insulating film in this embodiment is as follows:

[0041] S1, coating acrylic pressure-sensitive adhesive (second adhesive layer 3 and third adhesive layer 5) on both sides of a substrate layer 4 having a thickness of 100 μm, wherein the thickness of the second adhesive layer 3 and the third adhesive layer 5 are both 20 μm, to obtain a semi-finished product A;

[0042] An acrylic pressure-sensitive adhesive (first adhesive layer 1) is coated on the release surface of the release film, and dried in an oven at 90° C. The dry adhesive thickness is 20 μm, and a first puncture-resistant layer 2 with a thickness of 50 μm is laminated to obtain a semi-finished product B;

[0043] An acrylic pressure-sensitive adhesive (fourth adhesive layer 7) is coated on the release surface of the release film, and dried in an oven at 90°C. The dry adhesive thickness is 20 μm, and a second puncture-resistant layer 6 with a thickness of 50 μm is laminated to obtain a semi-finished product C;

[0044] S2. Lay the first puncture-resistant layer 2 of the semi-finished product B and the second puncture-resistant layer 6 of the semi-finished product C on the second adhesive layer 3 and the third adhesive layer 5 of the semi-finished product A respectively to obtain a puncture-resistant insulating film.

[0045] Example 2

[0046] The embodiment is basically the same as the first embodiment, except that the thickness of the substrate layer 4 is 50 μm.

[0047] Example 3

[0048] Basically the same as Example 1, except that: the substrate layer 4 is a PI substrate layer (purchased from Jiangyin Junyou, model HL50); the thickness of the first adhesive layer 1 is 30μm, the thickness of the second adhesive layer 3 is 10μm, the thickness of the third adhesive layer 5 is 10μm, and the thickness of the fourth adhesive layer 7 is 30μm.

[0049] Example 4

[0050] The embodiment is basically the same as Example 1, except that: the first puncture-resistant layer 2 and the second puncture-resistant layer 6 are both HDPE puncture-resistant layers (purchased from Kunshan Zhongsu); the thickness of the first adhesive layer 1 is 30 μm, the thickness of the second adhesive layer 3 is 10 μm, the thickness of the third adhesive layer 5 is 10 μm, and the thickness of the fourth adhesive layer 7 is 30 μm.

[0051] Example 5

[0052] The embodiment is basically the same as Example 1, except that: the substrate layer 4 is a PC substrate layer (purchased from Nantong Huapu, model EFR86); the first puncture-resistant layer 2 and the second puncture-resistant layer 6 are both HDPE puncture-resistant layers with a thickness of 25 μm (purchased from Kunshan Zhongsu); the thickness of the first adhesive layer 1 is 30 μm, the thickness of the second adhesive layer 3 is 10 μm, the thickness of the third adhesive layer 5 is 10 μm, and the thickness of the fourth adhesive layer 7 is 30 μm.

[0053] Example 6

[0054] The embodiment is basically the same as the embodiment 1, except that the thickness of the first puncture-resistant layer 2 and the second puncture-resistant layer 6 are both 30 μm.

[0055] Comparative Example 1

[0056] It is basically the same as Example 1, except that: the first puncture-resistant layer 2, the second puncture-resistant layer 6, the first adhesive layer 1 and the fourth adhesive layer 7 are not provided; the thickness of the second adhesive layer 3 is 50 μm, and the thickness of the third adhesive layer 5 is 50 μm.

[0057] Comparative Example 2

[0058] The embodiment is basically the same as the embodiment 1, except that the thickness of the first puncture-resistant layer 2 and the second puncture-resistant layer 6 are both 15 μm.

[0059] Comparative Example 3

[0060] The embodiment is basically the same as the first embodiment, except that the thickness of the first adhesive layer 1 , the second adhesive layer 3 , the third adhesive layer 5 and the fourth adhesive layer 7 are all 5 μm.

[0061] Test Case

[0062] The peel strength, puncture strength, puncture resistance, etc. of the puncture-resistant insulating films of Examples 1-6 and Comparative Examples 1-3 were tested:

[0063] (1) Peel strength: The insulating film was cut into 24 mm wide strips with a size of 24 mm*125 mm. After being laminated to a mirror steel plate and left to stand for 20 min, the 180° peel strength was tested at room temperature of 25°C. The peel rate was 300 mm / min, and the unit was N / 24 mm. The test instrument was a Shimadzu universal tensile machine AGS-J. The specific test standard was referred to GB / T 2792-2014.

[0064] (2) Puncture strength: Cut the insulating film into 100mm*100mm size, the puncture needle is made of stainless steel, the tip is hemispherical with a radius of (0,50±0.05)mm, the test speed is (100±10)mm / min, and the test instrument is Japan Shimadzu universal tensile machine AGS-J. The specific test standard refers to GB / T 37841-2019;

[0065] (3) Puncture resistance test: Aluminum metal particles with a diameter of 0.7 mm to 1.0 mm are placed on the insulating film and left to stand for 15 min under a pressure of 2.5 MPa to test whether the insulating film meets the insulation withstand voltage performance requirements. The insulation performance test parameters are 60 s at 1000 V DC, insulation resistance ≥ 500 MΩ, and the withstand voltage performance test parameters are 60 s at 3800 V DC, leakage current ≤ 1 mA. For specific test standards, refer to GB / T1408.1-2016.

[0066] Table 1 shows the relevant test results:

[0067] Table 1

[0068]

[0069]

[0070] It can be seen from Table 1 that after adding the puncture-proof layer, the puncture strength and puncture resistance of the insulating film are significantly enhanced, and as the thickness of the puncture-proof layer decreases, the puncture strength and puncture resistance decrease accordingly. It can be seen from Comparative Examples 1 and 2 that when the thickness of the puncture-proof layer is ≤15μm, the insulating film will fail after the puncture resistance test; it can be seen from the comparison between Comparative Example 3 and Example 1 that the puncture resistance of the insulating film is not affected by not changing the thickness of the insulating layer, but only changing the thickness of the adhesive layer, and only affecting the peel strength of the insulating film.

[0071] Obviously, the above embodiments are merely examples for the purpose of clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention of the utility model.

Claims

1. A puncture-resistant insulating film, characterized in that: The invention comprises a first adhesive layer, a first puncture-resistant layer, a second adhesive layer, a base material layer, a third adhesive layer, a second puncture-resistant layer and a fourth adhesive layer which are arranged in sequence from top to bottom.

2. The puncture-resistant insulating film according to claim 1, characterized in that: The first adhesive layer, the second adhesive layer, the third adhesive layer and the fourth adhesive layer are independently selected from acrylic adhesive layers.

3. The puncture-resistant insulating film according to claim 1, characterized in that: The thickness of the first adhesive layer, the second adhesive layer, the third adhesive layer and the fourth adhesive layer are independently 10 μm-50 μm.

4. The puncture-resistant insulating film according to claim 1, characterized in that: The first puncture-resistant layer and the second puncture-resistant layer are independently selected from a polyamide puncture-resistant layer and / or a high-density polyethylene puncture-resistant layer.

5. The puncture-resistant insulating film according to claim 1, characterized in that: The thickness of the first puncture-resistant layer and the second puncture-resistant layer are independently 25 μm-100 μm.

6. The puncture-resistant insulating film according to claim 1, characterized in that: The substrate layer is selected from a polyethylene terephthalate substrate layer, a polycarbonate substrate layer or a polyimide substrate layer.

7. The puncture-resistant insulating film according to claim 1, characterized in that: The thickness of the substrate layer is 25 μm-150 μm.