Prism structure, brightness enhancement film, POP type laminated brightness enhancement film applied to prism structure, and display device
By using the staggered arrangement of first prisms and second prisms and a non-sharp prism structure in the brightness enhancement film, the problem of damage to the brightness enhancement film during transportation and installation is solved, and high brightness and scratch resistance are improved. Avoiding membrane adsorption and cost increase.
Patent Information
- Application Number
- CN202420580211.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2034-03-25
AI Technical Summary
Existing brightness enhancement films are susceptible to scratches and damage during transportation and installation, resulting in damage to the microstructure of the optical film. They cannot effectively protect the microstructure during the assembly of backlight modules and the transportation of finished display products, and existing protection measures such as peeling off the protective film Residual glue left behind or insufficient refractive index limits the brightness.
The first prism and the second prism are arranged in a staggered manner. The height of the second prism is greater than that of the first prism, and the jitter height is preset in its extension direction to form a non-sharp prism structure to improve scratch resistance and brightness.
It achieves high brightness while improving the scratch resistance of the brightness enhancement film, avoiding the risk of adsorption between films, reducing costs, and meeting the gap requirements of the backlight module architecture design.
Smart Images

Figure CN221883934U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of optical films, in particular to a prism structure, a brightness enhancement film and applications thereof to a POP type laminating brightness enhancement film and a display device. Background Art
[0002] At present, brightness enhancement film (BEF) is usually used in backlight modules to converge the light emitted by the light source. In particular, in display devices such as monitors, brightness enhancement film is often used to increase the display brightness to achieve the purpose of reducing the energy consumption of the display. The brightness enhancement film is usually composed of a substrate and a focusing prism structure on the substrate, and the substrate and the focusing prism structure are both made of transparent resin material. Usually, the prism structure layer is composed of a plurality of identical prism strips for converging light, and these prism strips are arranged in parallel in the same direction to form a prism array. The prism array adjusts the light emitted outside the observer's field of view to within the observer's field of view through the refraction and reflection of light, thereby improving the utilization rate of the light energy emitted by the light source.
[0003] However, the brightness enhancement film will be scratched to varying degrees during transportation and installation, causing damage to the optical film microstructure, thereby reducing utilization and yield, and thus increasing costs.
[0004] To solve the above problems, patent number CN206594325U proposes a high-transmittance, scratch-resistant, and brightening film, comprising a substrate, a brightening layer arranged on one side of the substrate, and an anti-sticking layer arranged on the other side of the substrate, the brightening layer comprising a first prism and a second prism, the cross-section of the second prism is an isosceles triangle, the cross-section of the first prism is a trapezoid, the top of the trapezoid is provided with diffusion particles, and the height of the first prism is greater than the height of the second prism.
[0005] Patent No. CN101216639A proposes an optical film, comprising a substrate and a microstructure layer located on a surface of the substrate, wherein the microstructure layer comprises one or more first regions, each of the first regions comprises at least one multi-peak columnar structure, the multi-peak columnar structure is a union structure formed by at least two columnar structures overlapping each other, and the maximum height of the multi-peak columnar structure is composed of an arc columnar structure; and the microstructure layer optionally comprises one or more second regions, each of the second regions comprises at least one single-peak prismatic columnar structure.
[0006] An optical film comprises a substrate, a microstructure layer located on one surface of the substrate and an anti-scratch layer located on the other surface of the substrate, wherein the microstructure layer comprises a repeating structure composed of a first region and a second region, wherein the first region comprises at least one multi-peak columnar structure, and the multi-peak columnar structure is composed of a union structure formed by at least two arc columnar structures overlapping each other, wherein adjacent side surfaces of two adjacent columnar structures are connected to form a valley line, and the height of the valley line is 45% to 80% of the height of the lower one of the two adjacent columnar structures; and the second region comprises at least one single-peak prismatic columnar structure; wherein the maximum height of the multi-peak columnar structure in the first region is greater than the maximum height of the single-peak prismatic columnar structure in the second region.
[0007] In the prior art, in order to protect the microstructure of the brightness enhancement film, a protective film is usually applied on the brightness enhancement film, and the protective film is adhered to the prism structure layer of the brightness enhancement film through an adhesive layer to protect the prism structure layer. However, there are risks of residual adhesive and other poor appearance left after the protective film is peeled off, and it will also lead to increased costs. This method can only prevent the damage to the surface microstructure of the optical film product during the transportation stage, but cannot protect the optical film microstructure during the backlight module assembly stage and the transportation stage of the finished display.
[0008] Alternatively, a resilient self-repairing resin is used as the UV resin coating of the microstructure layer to improve the scratch resistance of the brightness enhancement film. However, the refractive index of the resin with excellent high resilience and scratch resistance is usually not more than 1.56, which limits the brightness of the brightness enhancement film.
[0009] Or use a non-pointed prism structure to make a brightness enhancement film. The disadvantage of this method is that after the prism tip is replaced by a rounded corner, the brightness is significantly attenuated, and the rounded corner has a certain risk of adsorption between films due to the large contact area. The use of it has strict requirements on the gap of the backlight module structure design and is very restrictive. There is no effective solution to the above problems. Utility Model Content
[0010] Purpose of the utility model: To provide a prism structure, a brightness enhancement film and its application in a POP type laminated brightness enhancement film and a display device, so as to solve the above-mentioned problems existing in the prior art.
[0011] Technical solution: A prism structure, comprising: a plurality of first prisms and a plurality of second prisms arranged in an array, and the height of the second prisms is greater than the height of the first prisms; wherein the second prism is arranged as a non-pointed prism structure, and a jitter height along its height direction is preset in its extension direction.
[0012] Preferably, the shaking height of the second prism includes: the highest shaking height is H and the lowest shaking height is H'; wherein, the highest height H-the lowest height H'≦5um, and>0.
[0013] Preferably, the cross section of the second prism is an isosceles right triangle, and the top angle thereof is set to a rounded corner or a flat-top structure.
[0014] Preferably, when the vertex angle of the second prism is rounded, the center of the arc is located on the perpendicular bisector of the second prism, and the fillet radius r is 0.25-10 um.
[0015] Preferably, when the vertex of the second prism is a flat-top structure, its vertex width W is 0.5-10 um.
[0016] Preferably, the first prism and the second prism are staggered with each other at a preset angle so that the prism structure has high brightness.
[0017] Preferably, an included angle a between an extending direction of the first extension axis of the first prism and an extending direction of the second extension axis of the second prism is 10° to 170°.
[0018] Preferably, the height h of the first prism is 10-40 um.
[0019] Preferably, the distance d between adjacent second prisms is 0-20h.
[0020] Preferably, the height H of the second prism is greater than the height h of the first prism, and H≧h+1um.
[0021] Preferably, the cross section of the first prism is an isosceles right triangle.
[0022] Preferably, the first prism and the second prism are made of light-cured hard resin, and the refractive index range of the resin is 1.5 to 1.7.
[0023] In order to achieve the above objective, according to another aspect of the present application, a brightness enhancement film is also provided.
[0024] The brightness enhancement film according to the present application is characterized by comprising the prism structure as described above;
[0025] It also includes: the first prisms and the second prisms are arranged alternately with each other at a preset angle to form a transparent structure layer; and a substrate layer is arranged on the bottom side of the transparent structure layer.
[0026] In order to achieve the above-mentioned purpose, according to another aspect of the present application, a POP-type laminating brightness enhancement film is also provided.
[0027] According to the POP type laminated brightness enhancement film of the present application, the upper prism layer includes the brightness enhancement film as described above.
[0028] In order to achieve the above objective, according to another aspect of the present application, a display device is also provided.
[0029] The display device according to the present application includes the brightness enhancement film as described above.
[0030] Beneficial effect: In the embodiment of the present application, the first prism and the second prism are staggered, and the second prism is higher than the first prism, and the non-sharp-angled second prism is preset with a jitter height along its height direction in its extension direction, so that the compound prism structure has high brightness and anti-adsorption and scratch resistance functions, thereby solving the problem in the prior art that in order to protect the microstructure of the brightness enhancement film, a protective film is usually applied to the brightness enhancement film, and the protective film is adhered to the prism structure layer of the brightness enhancement film through an adhesive layer to protect the prism structure layer, but there will be residual glue left after the protective film is peeled off and other poor appearance phenomena. Risk, which will also lead to an increase in cost; or use a resin with good self-rebound and scratch-resistant performance as the upper UV resin coating to improve the scratch resistance of the brightness enhancing film, but the refractive index of the resin with excellent high rebound and scratch resistance is usually not more than 1.56, which limits the brightness of the brightness enhancing film; or use a non-sharp prism structure to make a brightness enhancing film. The disadvantage of this method is that after the tip of the prism is replaced by a rounded corner, the brightness is significantly attenuated, and the rounded corner has a certain risk of inter-film adsorption due to the large contact area. The use of the backlight module structure design has strict requirements on the gap, which is a major technical problem. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the prism structure of the utility model;
[0032] Figure 2 It is a schematic diagram of a first prism of the utility model;
[0033] Figure 3 is a cross-sectional schematic diagram of a first prism structure of the utility model;
[0034] Figure 4 is a schematic diagram of a second prism of the utility model;
[0035] Figure 5 is a cross-sectional schematic diagram of the second prism structure of the utility model;
[0036] Figure 6 is a cross-sectional schematic diagram of another second prism structure of the utility model; and
[0037] Figure 7 It is a schematic diagram of the up and down shaking height of the utility model.
[0038] The accompanying drawings are marked as follows:
[0039] 1. first prism; 1', first extension axis;
[0040] 2. second prism; 2' second extension axis;
[0041] 3. Base material layer. DETAILED DESCRIPTION
[0042] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present application.
[0043] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequential order. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present application described here. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0044] In addition, the terms "installed", "set", "provided with", "connected", "connected", and "socketed" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral structure; it can be a mechanical connection, or an electrical connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be an internal connection between two devices, elements, or components. For those of ordinary skill in the art, the specific meanings of the above terms in this utility model can be understood according to specific circumstances.
[0045] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0046] The present application relates to a prism structure, a brightness enhancement film and its application in a POP-type laminated brightness enhancement film and a display device.
[0047] like Figure 1As shown, the prism structure includes: a plurality of first prisms 1 and a plurality of second prisms 2 arranged in an array, wherein the height of the second prisms 2 is greater than the height of the first prisms 1, and the two are arranged in a staggered manner;
[0048] The second prism 2 is configured as a non-pointed prism structure, and a shaking height along its height direction is preset in its extension direction, so that the prism structure has anti-adsorption and scratch-resistant functions.
[0049] Specifically, by setting the height of the second prism 2 to be greater than the height of the first prism 1 and setting the second prism 2 to a non-pointed prism structure, the second prism 2 can be scratch-resistant and at the same time, the first prism 1 can be protected.
[0050] At the same time, by pre-setting a shaking height in the height direction of the second prism 2 so that the top height of the second prism 2 is different, the second prism 2 can have an effect of shaking up and down along the height direction, thereby avoiding the situation where adsorption occurs due to no gap or too small gap between the film layers;
[0051] The first extension axis of the first prism and the second extension axis of the second prism are in different extension directions and are arranged in a staggered manner, so that the second prism 2 can protect the first prism 1 while retaining the high brightness of the sharp-angled first prism 1.
[0052] Furthermore, the second prism 2 itself can also provide further optical gain, thereby obtaining a better optical gain effect than a conventional single-axis prism.
[0053] The first prism 1 and the second prism 2 are formed by methods including but not limited to sputtering, evaporation, spraying, coating or mold imprinting, so as to obtain the desired compound prism structure.
[0054] The prism structure may be a conventional prism structure in the field of optical films, and can be used for various optical applications such as light splitting, focusing, and beam splitting; at the same time, these prisms can be arranged into various geometric shapes to achieve different optical functions.
[0055] Among them, Figure 2-3 As shown, the first prism 1 is the same as a conventional brightness enhancement film, and is an isosceles triangle structure with equal heights and right angles arranged in close proximity.
[0056] The rounded or flat-top prism height of the second prism 2 is H, which is further defined as the highest height of the vertical shaking of the Z axis; at the same time, the lowest height of the vertical shaking is set as H'.
[0057] The brightness enhancement film of the present application can improve the scratch resistance of the brightness enhancement film while ensuring high brightness due to the special design of the compound prism; at the same time, it can also avoid the risk of adsorption between films.
[0058] From the above description, it can be seen that the present application achieves the following technical effects:
[0059] In the embodiment of the present application, the first prism and the second prism are staggered, and the second prism is higher than the first prism, and the non-sharp-angled second prism is preset with a jitter height along its height direction in its extension direction, so that the compound prism structure has high brightness and anti-adsorption and scratch-resistant functions, thereby solving the problem in the prior art that in order to protect the microstructure of the brightness enhancement film, a protective film is usually applied to the brightness enhancement film, and the protective film is adhered to the prism structure layer of the brightness enhancement film through an adhesive layer to protect the prism structure layer, but there will be a risk of residual glue left after the protective film is peeled off and other phenomena of poor appearance, and at the same time This will lead to an increase in cost; or use a resin with good self-rebound and scratch-resistant performance as the upper UV resin coating to improve the scratch resistance of the brightness enhancing film. However, the refractive index of the resin with excellent high rebound and scratch resistance performance is usually not more than 1.56, which limits the brightness of the brightness enhancing film; or use a non-sharp prism structure to make a brightness enhancing film. The disadvantage of this method is that after the tip of the prism is replaced by a rounded corner, the brightness is significantly attenuated, and the rounded corner has a certain risk of inter-film adsorption due to the large contact area. The use of the backlight module structure design has strict requirements on the gap, which is a major technical problem.
[0060] Furthermore, the shaking height of the second prism 2 includes: the highest shaking height is H and the lowest shaking height is H'; wherein the highest height H-the lowest height H'≦5um, and>0. It can be understood that by setting the upper and lower shaking heights along the Z-axis direction within a preset range, it can ensure that the second prism is easy to process and form, and at the same time, it can also avoid the situation where the optical performance of the film layer is affected by the excessive shaking height difference.
[0061] Furthermore, the first extension axis 1' of the first prism 1 and the second extension axis 2' of the second prism 2 are in different extension directions and are arranged in a staggered manner. It can be understood that a is the angle between 1' and 2'.
[0062] Furthermore, the angle a between the extension direction of the first prism 1 and the extension direction of the second prism 2 is 10° to 170°. It is understandable that by setting the angle a between the extension directions of the first prism 1 and the second prism 2 in the range of 10° to 170°, it is possible to ensure that the prism structure has good optical performance, thereby avoiding the situation where the angle is too large or too small and causes poor effects.
[0063] Furthermore, the height h of the first prism 1 is 10-40 um. It is understandable that by setting the height range of the first prism 1 to 10-40 um, a variety of sizes can be selected, thereby meeting diverse usage requirements; at the same time, setting the height of the first prism 1 within the above range can ensure that the first prism 1 has good optical performance.
[0064] Further, such as Figure 4 As shown, the spacing between adjacent second prisms 2 is d, and d is 0 to 20h. It can be understood that by setting the spacing between two adjacent second prisms 2 to 0 to 20h, a good brightness effect can be ensured, while avoiding the situation where the protection effect is poor and the scratch resistance strength is reduced due to too large a spacing.
[0065] Furthermore, the height H of the second prism 2 is greater than the height h of the first prism 1, and H≧h+1um. It is understandable that, because the height of the second prism 2 is greater than the height of the first prism 1, a good protection effect is achieved for the first prism 1, thereby achieving an effect of improving the optical performance; at the same time, the compound prism can also achieve an effect of having a variety of materials to choose from.
[0066] like Figure 5-6 As shown, the cross section of the second prism 2 is an isosceles triangle, and its top angle is set to a rounded corner or a flat top structure. It can be understood that by setting the cross section of the second prism 2 to an isosceles right triangle, the effect of further improving the brightness can be achieved; at the same time, setting its top angle to a rounded corner or a flat top structure can have good scratch resistance. Preferably, the cross section of the second prism 2 is an isosceles right triangle.
[0067] like Figure 5 As shown, when the vertex of the second prism 2 is rounded, the center of the arc is located on the perpendicular bisector of the second prism 2, and the fillet radius r is 0.25 to 10 um. It can be understood that by setting the fillet radius r to 0.25 to 10 um, a variety of sizes can be selected, thereby meeting a variety of usage requirements.
[0068] It should be noted that when the r angle of the tip of the second prism 2 is too small, sufficient scratch resistance cannot be provided. When the r angle of the tip of the second prism 2 is too large, the contact area is too large to cause inter-film adsorption, and obvious streaks will appear on the screen. Therefore, setting the fillet radius within the above range can ensure good optical performance.
[0069] like Figure 6As shown, when the vertex angle of the second prism 2 is a flat-top structure, its vertex angle width W is 0.5-10 um. It is understandable that setting the vertex angle width W to 0.5-10 um can achieve the effect of multiple sizes being available, thereby being able to meet the effect of multiple usage requirements.
[0070] It should be noted that when the flat top width W at the tip of the second prism 2 is too small, it cannot provide sufficient scratch resistance. If it is too large, there will be adsorption between films due to excessive contact area, and obvious stripes will appear on the screen. Therefore, setting the W value within the above range can ensure good optical performance.
[0071] Furthermore, the cross section of the first prism 1 is an isosceles right triangle. It can be understood that by adopting an isosceles right triangle, good optical performance can be ensured.
[0072] Furthermore, the first prism 1 and the second prism 2 are light-cured hard resins with a refractive index range of 1.5-1.7. It is understandable that due to the difference in structural height, the second prism 2 protects the first prism 1, so that the product can choose a light-cured hard resin with a higher refractive index, thereby improving the brightness of the brightness enhancement film and taking into account the scratch resistance.
[0073] The specific examples are further described below:
[0074] The testing items of the brightness enhancement film provided by the utility model include but are not limited to: scratch resistance test and brightness test.
[0075] Scratch test: The brightness enhancement film of the following examples is subjected to a scratch test using a scratch test machine with a load of 200g and the back of the diffusion film for scratch testing; the scratch test may be performed using, but is not limited to: steel wool
[0076] Brightness test: The brightness enhancement film of the following example was installed in the backlight module, and the brightness was measured using a BM-7AC brightness meter, and the picture condition was observed.
[0077] Example 1
[0078] like Figure 1 As shown, the substrate layer 3 is PET, and a UV resin with a refractive index of 1.6 is selected; the height h of the first prism 1 is 20um; the height H of the second prism 2 is 24um, H' is 22um, the spacing d between adjacent second prisms 2 is 20um, and the fillet radius r is 2.5um; the angle a between the extension direction of the first prism 1 and the extension direction of the second prism 2 is 90°.
[0079] At this time, after testing, the performance parameters of the brightness enhancement film are: scratch resistance is 10 times OK, brightness is 7132cd / m 2 , the picture condition is normal.
[0080] Example 2
[0081] The difference between Example 2 and Example 1 is that the angle a between the extension direction of the first prism 1 and the extension direction of the second prism 2 is 10°.
[0082] At this time, after testing, the performance parameters of the brightness enhancement film are: scratch resistance is 10 times OK, brightness is 6515cd / m 2 , the picture condition is normal.
[0083] Example 3
[0084] The difference between Example 3 and Example 1 is that the included angle a between the extension direction of the first prism 1 and the extension direction of the second prism 2 is 50°.
[0085] At this time, after testing, the performance parameters of the brightness enhancement film are: scratch resistance is 10 times OK, brightness is 6851cd / m 2 , the picture condition is normal.
[0086] Example 4
[0087] The difference between Example 4 and Example 1 is that the included angle a between the extension direction of the first prism 1 and the extension direction of the second prism 2 is 130°.
[0088] At this time, after testing, the performance parameters of the brightness enhancement film are: scratch resistance is 10 times OK, brightness is 6859cd / m 2 , the picture condition is normal.
[0089] Example 5
[0090] The difference between Example 5 and Example 1 is that the distance d between adjacent second prisms 2 is 0.
[0091] At this time, after testing, the performance parameters of the brightness enhancement film are: scratch resistance is 10 times OK, brightness is 7545cd / m 2 , the picture condition is normal.
[0092] Example 6
[0093] The difference between Example 6 and Example 1 is that the distance d between adjacent second prisms 2 is 50 um.
[0094] At this time, after testing, the performance parameters of the brightness enhancement film are: scratch resistance is 10 times OK, brightness is 6945cd / m 2 , the picture condition is normal.
[0095] Example 7
[0096] The difference between Example 7 and Example 1 is that the distance d between adjacent second prisms 2 is 100 um.
[0097] At this time, after testing, the performance parameters of the brightness enhancement film are: scratch resistance is 10 times OK, brightness is 6711cd / m 2 , the picture condition is normal.
[0098] Example 8
[0099] The difference between Example 8 and Example 1 is that the distance d between adjacent second prisms 2 is 200 um.
[0100] At this time, after testing, the performance parameters of the brightness enhancement film are: scratch resistance is 10 times OK, brightness is 6429cd / m 2 , the picture condition is normal.
[0101] Example 9
[0102] The difference between Example 9 and Example 1 is that the distance d between adjacent second prisms 2 is 400 um.
[0103] At this time, after testing, the performance parameters of the brightness enhancement film are: scratch resistance is 10 times OK, brightness is 6240cd / m 2 , the picture condition is normal.
[0104] Example 10
[0105] The difference between Example 10 and Example 1 is that the fillet radius r is 0.25 um.
[0106] At this time, after testing, the performance parameters of the brightness enhancement film are: scratch resistance is 5 times OK, brightness is 7390cd / m 2 , the picture condition is normal.
[0107] Embodiment 11
[0108] The difference between Example 11 and Example 1 is that the fillet radius r is 5 um.
[0109] At this time, after testing, the performance parameters of the brightness enhancement film are: scratch resistance is 10 times OK, brightness is 6957cd / m 2 , the picture condition is normal.
[0110] Example 12
[0111] The difference between Example 12 and Example 1 is that the fillet radius r is 10 um.
[0112] At this time, after testing, the performance parameters of the brightness enhancement film are: scratch resistance is 15 times OK, brightness is 6328cd / m 2 , the picture condition is normal.
[0113] Embodiment 13
[0114] The difference between Example 13 and Example 1 is that the second prism 2 is a flat-top structure, and its top angle width W is 0.5 um.
[0115] At this time, after testing, the performance parameters of the brightness enhancement film are: scratch resistance is 5 times OK, brightness is 7160cd / m 2 , the picture condition is normal.
[0116] Embodiment 14
[0117] The difference between Example 14 and Example 1 is that the second prism 2 is a flat-top structure, and its top angle width W is 5 um.
[0118] At this time, after testing, the performance parameters of the brightness enhancement film are: scratch resistance is 10 times OK, brightness is 6793cd / m 2 , the picture condition is normal.
[0119] Embodiment 15
[0120] The difference between Example 15 and Example 1 is that the second prism 2 is a flat-top structure, and its top angle width W is 10 um.
[0121] At this time, after testing, the performance parameters of the brightness enhancement film are: scratch resistance is 15 times OK, brightness is 6127cd / m 2 , the picture condition is normal.
[0122] Comparative Example 1
[0123] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 does not have the second prism structure.
[0124] At this time, after testing, the performance parameters of the film are: scratch resistance is 1 NG, brightness is 5981cd / m 2 , the picture condition is normal.
[0125] Comparative Example 2
[0126] The difference between Comparative Example 2 and Example 1 is that the angle a between the extension direction of the first prism 1 and the extension direction of the second prism 2 is 175°.
[0127] At this time, after testing, the performance parameters of the film are: scratch resistance is 10 times OK, brightness is 6288cd / m 2 , the picture condition shows interference fringes.
[0128] Comparative Example 3
[0129] The difference between Comparative Example 3 and Example 1 is that the distance d between adjacent second prisms 2 is 450 um.
[0130] At this time, after testing, the performance parameters of the film are: scratch resistance is 4 times NG, brightness is 6121cd / m2, and the picture condition is normal.
[0131] Comparative Example 4
[0132] The difference between Comparative Example 4 and Example 1 is that the fillet radius r is 0.1 um.
[0133] At this time, after testing, the performance parameters of the film are: scratch resistance is 2 times NG, brightness is 7459cd / m 2 , the picture condition is normal.
[0134] Comparative Example 5
[0135] The difference between Comparative Example 5 and Example 1 is that the fillet radius r is 15 um.
[0136] At this time, after testing, the performance parameters of the film are: scratch resistance is 20 times OK, brightness is 5763cd / m 2 , the screen condition is striped.
[0137] Comparative Example 6
[0138] The difference between Comparative Example 6 and Example 1 is that the top angle width W is 0.4 um.
[0139] At this time, after testing, the performance parameters of the film are: scratch resistance is 4 times NG, brightness is 7197cd / m 2 , the picture condition is normal.
[0140] Comparative Example 7
[0141] The difference between Comparative Example 7 and Example 1 is that the vertex width W is 11 um.
[0142] At this time, after testing, the performance parameters of the film are: scratch resistance is 15 times OK, brightness is 5933cd / m 2 , the screen condition is striped.
[0143] Comparative Example 8
[0144] The difference between Comparative Example 8 and Example 1 is that Comparative Example 8 has a second prism structure but does not have a jitter height.
[0145] At this time, after testing, the performance parameters of the film are: scratch resistance is sub-10ok, brightness is 7147cd / m2, and the picture condition is normal.
[0146] Comparative Example 9
[0147] The difference between Comparative Example 9 and Example 1 is that it has a second prism structure but does not have a jitter height, and the fillet radius r is 0.1 um.
[0148] At this time, after testing, the performance parameters of the film are: scratch resistance is 2 times NG, brightness is 7291cd / m 2, the picture condition is normal.
[0149] Comparative Example 10
[0150] The difference between Comparative Example 10 and Example 1 is that it has a second prism structure but does not have a jitter height, and the fillet radius r is 0.25 um.
[0151] At this time, after testing, the performance parameters of the film are: scratch resistance is 5 times OK, brightness is 7215cd / m 2 , the picture condition is normal.
[0152] Comparative Example 11
[0153] The difference between Comparative Example 11 and Example 1 is that it has a second prism structure but does not have a jitter height, and the fillet radius r is 5 um.
[0154] At this time, after testing, the performance parameters of the film are: scratch resistance is 10 times OK, brightness is 6988cd / m 2 , the picture condition is normal.
[0155] Comparative Example 12
[0156] The difference between Comparative Example 12 and Example 1 is that it has a second prism structure but does not have a jitter height, and the fillet radius r is 10 um.
[0157] At this time, after testing, the performance parameters of the film are: scratch resistance is 15 times OK, brightness is 6335cd / m 2 , the screen status is adsorption.
[0158] Comparative Example 13
[0159] The difference between Comparative Example 13 and Example 1 is that it has a second prism structure but does not have a jitter height, and the fillet radius r is 15 um.
[0160] At this time, after testing, the performance parameters of the film are: scratch resistance is 20 times OK, brightness is 5781cd / m 2 , the screen status is adsorption.
[0161] The results of various embodiments and comparative examples are shown in Table 1:
[0162]
[0163]
[0164] From the above test results we can see that:
[0165] 1. It can be seen from Examples 1 to 4 that the brightness enhancement film of the present invention adds a second prism 2, and the top angle of the second prism 2 is rounded, which can not only improve the brightness gain effect of the brightness enhancement film, but also have good scratch resistance.
[0166] 2. It can be seen from Example 1 and Comparative Example 1 that when the second prism structure 2 is not provided, the scratch resistance effect is very poor.
[0167] 3. It can be seen from Examples 1 to 4 and Comparative Example 2 that when the angle a between the second prism 2 and the first prism 1 is too small, interference fringes begin to appear on the screen.
[0168] 4. It can be seen from Examples 1 and 5-9 that the brightness enhancement film of the present invention adds a second prism 2, and the top angle of the second prism 2 is rounded, which can improve the brightness gain effect of the brightness enhancement film and provide good scratch resistance.
[0169] 5. It can be seen from Examples 1, 5-9 and Comparative Example 3 that when the spacing between the second prisms 2 increases, the brightness will gradually decrease. When the spacing between the second prisms 2 is too large, the protection effect will be poor and the scratch resistance will decrease.
[0170] 6. It can be seen from Examples 1 and 10-12 that, after adding the second prism 2, the brightness enhancement film of the utility model can improve the brightness gain effect of the brightness enhancement film and provide good scratch resistance.
[0171] 7. It can be seen from Examples 1, 10-12 and Comparative Examples 4-5 that when the r angle of the second prism tip 2 is too small, it cannot provide sufficient scratch resistance; when the r angle of the second prism tip is too large, inter-film adsorption will occur due to excessive contact area.
[0172] 8. It can be seen from Examples 1 and 13-15 that the brightness enhancement film of the utility model adds a second prism 2, and the top angle of the second prism 2 is a flat-top structure, which can improve the brightness gain effect of the brightness enhancement film and provide good scratch resistance. As the top angle size of the second prism 2 increases, the number of scratch resistance of the film tends to increase, and the brightness tends to decrease.
[0173] 9. It can be seen from Examples 1, 13-15 and Comparative Examples 6-7 that when the W value of the second prism 2 is too small, the scratch resistance will be reduced. When the W value of the second prism 2 is too large, interference fringes will appear on the screen.
[0174] 10. It can be seen from Example 1 and Comparative Example 8 that both solutions can meet the use requirements, and Comparative Example 8 is protected as a key feature in another application.
[0175] 11. It can be seen from Example 1 and Comparative Examples 9-13 that if the second prism 2 does not have an up-and-down shaking shape and other parameters remain unchanged, as the r value increases, the number of scratch resistance increases significantly, but the brightness also decreases accordingly;
[0176] When the r value is above 5 μm, adsorption occurs and the method is not applicable, for example, Comparative Examples 12-13.
[0177] It should be noted that 5 scratch resistance times is the bottom line for passing.
[0178] In summary, it can be seen from the embodiments and comparison results that the composite staggered dithering prism structure of the brightness enhancement film of the present invention has high brightness and good scratch resistance and anti-adsorption properties.
[0179] The present application also relates to a brightness enhancement film, comprising the prism structure as described above;
[0180] It also includes: the first prism 1 and the second prism 2 are arranged alternately with each other at a preset angle to form a transparent structure layer; and
[0181] A substrate layer 3 is disposed on the side of the transparent structure layer away from the extension axis.
[0182] Specifically, the substrate layer 3 refers to the base material or substrate to which the optical film or coating is attached, which can achieve good fixing and supporting effects; at the same time, it can also cooperate with other film layer structures to achieve multiple functional effects. Preferably, the substrate layer is PET, PC, PMMA, PE, PVC or PS. It can achieve the effect of multiple materials to choose from, so that the effect can be easily achieved.
[0183] By staggering the first prism 1 and the second prism 2 on the substrate layer 3 at a preset angle, a single brightness enhancement film with a stable structure can be formed, while also having high brightness and scratch resistance.
[0184] The present application also relates to a POP-type laminating brightness enhancement film, including the brightness enhancement film as described above.
[0185] The scratch-resistant compound interlaced prism structure of the utility model can be applied to not only a single brightness enhancement film, but also a POP type laminated brightness enhancement film as an upper prism structure to improve the surface scratch resistance of the POP product.
[0186] The present application also relates to a display device, comprising the brightness enhancement film as described above.
[0187] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings; however, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, various equivalent transformations can be made to the technical scheme of the present invention, and these equivalent transformations all belong to the protection scope of the present invention.
Claims
1. A prismatic structure, characterized in that: include: A plurality of first prisms (1) and a plurality of second prisms (2) are arranged in an array, and the height of the second prisms (2) is greater than the height of the first prisms (1); The second prism (2) is configured as a non-pointed prism structure, and a shaking height along its height direction is preset in its extension direction.
2. The prism structure according to claim 1, characterized in that: The shaking height of the second prism (2) includes: the highest shaking height is H and the lowest shaking height is H'; wherein the highest height (H)-the lowest height (H') ≤ 5um, and > 0.
3. The prism structure according to claim 1, characterized in that: The cross section of the second prism (2) is an isosceles triangle, and the top angle thereof is set to be a rounded corner or a flat top structure.
4. The prism structure according to claim 3, characterized in that: When the vertex angle of the second prism (2) is rounded, the center of the arc is located on the perpendicular bisector of the second prism (2), and the rounded radius r is 0.25 to 10 um.
5. The prism structure according to claim 3, characterized in that: When the vertex of the second prism (2) is a flat-top structure, its vertex width W is 0.5-10 um.
6. The prism structure according to claim 1, characterized in that: The first prism (1) and the second prism (2) are arranged alternately with each other at a preset angle, so that the prism structure has high brightness.
7. The prism structure according to claim 1, characterized in that: The first extension axis (1') of the first prism (1) and the second extension axis (2') of the second prism (2) are in different extension directions and are arranged in a staggered manner.
8. The prism structure according to claim 1, characterized in that: The included angle a between the extension direction of the first prism (1) and the extension direction of the second prism (2) is 10° to 170°.
9. The prism structure according to claim 1, characterized in that: The height h of the first prism (1) is 10-40 um.
10. The prism structure according to claim 1, characterized in that: The distance d between adjacent second prisms (2) is 0 to 20h.
11. The prism structure according to claim 1, characterized in that: The height H of the second prism (2) is greater than the height h of the first prism (1), and H≧h+1um.
12. The prism structure according to claim 1, characterized in that: The cross section of the first prism (1) is an isosceles right triangle.
13. The prism structure according to claim 1, characterized in that: The first prism (1) and the second prism (2) are photocurable hard resins, and the refractive index range is 1.5 to 1.
7.
14. Brightness enhancement film, characterized in that: comprising a prismatic structure as claimed in any one of claims 1 to 13; It also includes: the first prism (1) and the second prism (2) are arranged alternately with each other at a preset angle to form a transparent structure layer; and A substrate layer (3) is arranged on the bottom side of the transparent structural layer.
15. Applied to POP type bonding brightening film, characterized in that: The upper prism layer includes the brightness enhancement film as claimed in claim 14.
16. A display device, characterized in that The method comprises the brightness enhancement film as claimed in any one of claims 14 to 15.